Black pigment dispersion for forming cured film and method for producing the same
Coating lactam black with a resin having acidic groups addresses dispersibility and surface roughness issues, resulting in a cured film with enhanced dispersibility and reduced roughness for improved display quality.
Patent Information
- Application Number
- JP2023082870
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
AI Technical Summary
Lactam black pigments suffer from poor dispersibility and high surface roughness when used in forming cured films, leading to issues like gelling during storage and display unevenness on organic electroluminescence (EL) displays.
Coating lactam black with a resin having acidic groups, specifically acrylic acid, methacrylic acid, or maleic acid resin with an acid value between 30 mgKOH/g and 100 mgKOH/g, to create a black pigment dispersion with improved dispersibility and low surface roughness.
The resulting cured film exhibits reduced surface roughness and improved dispersibility, minimizing development residues and enhancing display quality.
Smart Images

Figure 2024166648000001 
Figure 2024166648000002 
Figure 2024166648000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a black pigment dispersion which contains lactam black coated with a resin, has excellent dispersibility, and is suitable for forming a cured film, and a method for producing the same. [Background technology]
[0002] In recent years, many products using organic electroluminescence (EL) displays have been developed for display devices having thin displays, such as smartphones, tablet PCs, and televisions. In general, an organic EL display has a first electrode having translucency such as a silver / magnesium alloy on the light extraction side of a light-emitting element, a second electrode such as tin indium oxide (ITO) and a metal reflective layer such as a silver / copper alloy on the non-light extraction side of the light-emitting element, and a patterned pixel division layer having the function of an insulating layer between the first and second electrodes to divide the pixels of each of the red / blue / green light-emitting elements. The first and second electrodes are generally formed by sputtering, and the pixel division layer is required to have a low taper pattern shape to prevent disconnection of the first electrode.
[0003] An organic EL display is a self-luminous display device that emits light using the energy generated by the recombination of electrons injected from a cathode and holes injected from an anode. Therefore, when external light such as sunlight is incident, the visibility and contrast are reduced due to the reflection of the external light, and therefore a technique for reducing the reflection of the external light is required. As a technique for reducing the reflection of the external light, for example, a method of forming a pixel division layer having a light-shielding property using a photosensitive composition can be mentioned. As a coloring material for imparting light-shielding properties, an organic black pigment having excellent insulating properties and high coloring power can be mentioned, and as a specific example thereof, bis-oxodihydroindolylene-benzodifuranone, which is a benzodifuranone-based pigment, is disclosed in Patent Document 1. As other organic black pigments, perylene-based black pigments (Patent Document 2) and azo-based black pigments (Patent Document 3) are known.
[0004] However, when the organic black pigments disclosed in Patent Documents 1 to 3 are incorporated into a photosensitive composition and a pixel division layer of an organic EL display is formed by photolithography, there is a problem that development residues are generated on the substrate. Such development residues cause a decrease in the yield of the development process and a decrease in visibility due to the occurrence of non-light-emitting areas in pixels called dark spots caused by the development residues.
[0005] Patent Document 4 discloses a black pigment having (a) a core containing at least one organic black pigment selected from the group consisting of benzodifuranone-based black pigments, perylene-based black pigments, azo-based black pigments, and isomers thereof, and (b) a coating layer containing silica, metal oxides, and / or metal hydroxides. Benzodifuranone-based black pigments have very low alkali resistance compared to inorganic black pigments such as carbon black and titanium black, or many non-black organic pigments such as blue and red. Therefore, when patterning is performed in the development process, the crystal structure of the benzodifuranone-based black pigment is destroyed and dissolved or semi-dissolved upon contact with an alkaline developer that has penetrated through a binder component, and decomposed components are generated and fixed on the substrate, resulting in the generation of residues at the openings of the pixel division layer. In Patent Document 4, the particle surface of lactam black is coated with silica, metal oxides, and metal hydroxides to improve the alkali resistance of the benzodifuranone-based black pigment. According to the black pigment of Patent Document 4, it is possible to form a pixel division layer in a pattern while suppressing the generation of development residues, and it is possible to improve the light-emitting properties of an organic EL display. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2009 / 010521 [Patent Document 2] International Publication No. 2005 / 078023 [Patent Document 3] US Patent Application Publication No. 2002-121228 [Patent Document 4] International Publication No. 2018 / 038083 Summary of the Invention [Problem to be solved by the invention]
[0007] Lactam black is a black pigment that has the advantages of high infrared and ultraviolet transmittance, high insulating properties, low dielectric constant, etc., but has the disadvantage of poor dispersibility when made into a pigment dispersion. That is, when preparing a pigment dispersion containing lactam black, there are problems in that the dispersion gels or the viscosity of the dispersion changes during storage.
[0008] In addition, when a black cured film is produced using a pigment dispersion containing lactam black coated with a resin, the surface roughness after development is large, which may cause uneven display on a display device. In this regard, Patent Document 4 evaluates the alkali resistance of the black pigment by checking whether it dissolves in an aqueous trimethylammonium hydroxide solution, but does not check the surface roughness of the cured film after development.
[0009] An object of the present invention is to provide a black pigment dispersion which has excellent dispersibility, has small surface roughness of the cured film formed after development, and is suitable for forming a cured film, and a method for producing the same. [Means for solving the problem]
[0010] The present inventors have found that by using lactam black which has an acidic group and is coated with a resin having a specific acid value, it is possible to prepare a black pigment dispersion which has excellent dispersibility and is capable of producing a cured film having small surface roughness, and have thus completed the present invention.
[0011] Specifically, the present invention relates to a lactam black coated with a resin having an acidic group; A dispersant; A black pigment dispersion comprising: The resin is at least one selected from the group consisting of acrylic acid resins, methacrylic acid resins, and maleic acid resins, and has an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less. The present invention relates to a black pigment dispersion for forming a cured film.
[0012] Lactam black coated with an acrylic acid resin, methacrylic acid resin, or maleic acid resin which has an acidic group and has an acid value within a specific range has excellent dispersibility compared to lactam black coated with a resin whose acid value is outside the specific range, and it is possible to obtain a black pigment dispersion which can produce a cured film with small surface roughness after development.
[0013] The content of the lactam black coated with the resin having an acidic group in the black pigment dispersion is preferably 5% by mass to 25% by mass relative to the mass of the black pigment dispersion. If it is less than 5% by mass, the pigment concentration is low and coloring may be insufficient, while if it exceeds 25% by mass, the viscosity becomes high and the handleability is easily deteriorated.
[0014] The viscosity of the black pigment dispersion during preparation is preferably 20 mPa·s or less.
[0015] The present invention also provides A step A of wet-grinding lactam black; A method for producing a black pigment dispersion, comprising: a step B of mixing the lactam black finely divided by the step A, a dispersant, and a solvent, In the step A, a resin which is one or more selected from the group consisting of an acrylic acid resin, a methacrylic acid resin, and a maleic acid resin and has an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less is added to finely pulverize the lactam black. The present invention relates to a method for producing a black pigment dispersion for forming a cured film. Effect of the Invention
[0016] According to the present invention, it is possible to produce a cured film having a smaller surface roughness after development than in the past. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Lactam Black) As the lactam black, for example, Irgaphor (registered trademark) Black S0100CF manufactured by DIC Corporation can be used. One type of lactam black may be used, or two or more types may be used in combination.
[0018] The lactam black may be subjected to a milling treatment in advance from the viewpoint of adjusting the average particle size, and from the viewpoint of the surface smoothness of the coating film when used as a column spacer, black matrix or black bank. The milling treatment can be performed according to a standard method depending on the type of black pigment, etc. Examples of such milling treatment include a solvent salt milling method.
[0019] The average particle size of the lactam black coated with the resin having an acidic group in the black pigment dispersion is preferably 100 nm or less, and more preferably 80 nm or less.
[0020] (resin) The resin used in the present invention is an acrylic acid resin, a methacrylic acid resin, or a maleic acid resin having an acidic group in its chemical structure and an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less. Commercially available products can be used as such resins. The molecular weight of these resins is preferably 1,000 or more and 50,000 or less in terms of weight average molecular weight. By adjusting the molecular weight within this range, excellent alkali solubility, anti-aggregation effect during drying, and dispersibility can be achieved in the lactam black coated with the resin.
[0021] Here, the acid value refers to the acid value per 1 g of resin solid content, and can be determined by potentiometric titration in accordance with JIS K 0070 (1992) (unit: mgKOH / g).
[0022] (Step A / Method of covering lactam black with resin) Lactam black coated with a resin (hereinafter, sometimes referred to as resin-coated lactam black) can be prepared by making a resin present when lactam black is pulverized in wet pulverization step A. There are no particular limitations on step A as long as it is wet pulverization, and examples of this include solvent salt milling.
[0023] When solvent salt milling is performed as step A, for example, lactam black, a water-soluble inorganic salt, a water-soluble solvent, and a resin (acrylic acid resin, methacrylic acid resin, or maleic acid resin) are mixed, and the resulting mixture is mechanically kneaded using a kneader or the like, thereby simultaneously grinding the lactam black with the water-soluble inorganic salt and coating the lactam black with the resin. Known conditions can be used for such a solvent salt milling method.
[0024] After the solvent salt milling, the mixture is washed with water to remove the water-soluble inorganic salt and the water-soluble solvent, and the resin-coated lactam black is obtained. The mixture is preferably washed with water until the water-soluble inorganic salt and the water-soluble solvent are completely removed. After washing with water, it is preferable to carry out a drying treatment to remove the moisture in the resin-coated lactam black.
[0025] The water-soluble inorganic salt is not particularly limited as long as it dissolves in water, and known salts such as sodium chloride, barium chloride, potassium chloride, sodium sulfate (mirabite), and anhydrous sodium sulfate (anhydrous mirabite) can be used.
[0026] The water-soluble solvent is not particularly limited as long as it dissolves (is miscible with) water and does not substantially dissolve the water-soluble inorganic salt used, and a known water-soluble solvent can be used. However, since the temperature rises during kneading and the solvent becomes easily evaporated, it is preferable to use a high-boiling point solvent with a boiling point of 120°C or more from the viewpoint of safety. For example, it is preferable to use 2-methoxyethanol, 2-butoxyethanol, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, ethylene glycol, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, liquid polyethylene glycol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, liquid polypropylene glycol, etc.
[0027] When resin coating of lactam black is also performed during solvent salt milling, the method of adding the resin is not particularly limited, and the entire amount may be added at the start of kneading, or the resin may be added in several portions after the start of kneading. In the present invention, a pigment derivative may be added in step A in order to promote microparticulation of lactam black.
[0028] Preferred skeletons of the pigment derivative include skeletons of quinacridone pigments, phthalocyanine pigments, azo pigments, quinophthalone pigments, isoindoline pigments, isoindolinone pigments, diketopyrrolopyrrole pigments, benzimidazolone pigments, etc. In addition, pale yellow aromatic polycyclic compounds such as naphthalene, anthraquinone, triazine, and quinoline are also included in the preferred skeletons of the pigment derivative.
[0029] Examples of pigment derivatives that can be added include pigment derivatives described in JP-A-11-49974, JP-A-11-189732, JP-A-10-245501, JP-A-2006-265528, JP-A-8-295810, JP-A-11-199796, JP-A-2005-234478, JP-A-2003-240938, JP-A-2001-356210, JP-A-2001-220520, JP-A-2007-186681, and the like.
[0030] In the present invention, when a pigment derivative is added during the solvent salt milling, the pigment derivative is preferably added in a ratio of 0.1 to 20 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of lactam black.
[0031] In the present invention, when the pigment derivative is added during the solvent salt milling, the pigment derivative may be added to the lactam black before kneading, or may be added during kneading. The pigment derivative may be added in its entirety at once, or may be added in several portions.
[0032] From the viewpoint of dispersion stability, the amount of resin coated on the lactam black is preferably 5% by mass or more and 30% by mass or less, and more preferably 10% by mass or more and 20% by mass or less, based on the mass of the lactam black.
[0033] (Dispersant) The dispersant used in the present invention is not particularly limited, but for example, a urethane-based resin dispersant, an acrylic-based resin dispersant, a polyester-based resin dispersant, and a resin dispersant containing an amide bond in the side chain can be used.
[0034] Examples of the urethane resin dispersant include the base-type urethane resin dispersant disclosed in JP 2011-057823 A. From the viewpoint of dispersibility, the urethane resin dispersant preferably has an amine value of 2 mgKOH / g or more and 60 mgKOH / g or less, more preferably 5 mgKOH / g or more and 40 mgKOH / g or less.
[0035] As the urethane-based resin dispersant, commercially available products can be used. Suitable commercially available urethane-based resin dispersants include: Manufactured by BYK Japan Co., Ltd. DISPERBYK®-161 (amine value 37 mg KOH / g, acid value 0 mg KOH / g), DISPERBYK®-162 (amine value 34 mg KOH / g, acid value 0 mg KOH / g), DISPERBYK®-167 (amine value 25 mg KOH / g, acid value 0 mg KOH / g), DISPERBYK®-182 (amine value 30 mg KOH / g, acid value 0 mg KOH / g), DISPERBYK®-2150 (amine value 110 mg KOH / g, acid value 0 mg KOH / g), DISPERBYK®-2163 (amine value 22 mg KOH / g, acid value 0 mg KOH / g), DISPERBYK®-2164 (amine value 23 mg KOH / g, acid value 0 mg KOH / g), BYK-9077 (amine value 46 mg KOH / g, acid value 0 mg KOH / g), Manufactured by Lubrizol Japan, Ltd. Examples include Solsperse 24000 (amine value 42 mg KOH / g, acid value 25 mg KOH / g).
[0036] Here, the amine value refers to the amine value per 1 g of dispersant solid content, and is the value (unit: mgKOH / g) calculated as the potassium hydroxide equivalent after determining it by potentiometric titration using a 0.1 N hydrochloric acid aqueous solution. Also, the acid value refers to the acid value per 1 g of dispersant solid content, and can be determined by the same method as the acid value of the resin.
[0037] As the acrylic resin dispersant, for example, the dispersants disclosed in JP-A-2022-065931 and JP-A-2023-004245 can be used. From the viewpoint of dispersibility, the acrylic resin dispersant preferably has an amine value of 50 mgKOH / g or more and 200 mgKOH / g or less, more preferably 120 mgKOH / g or more and 180 mgKOH / g or less.
[0038] The acrylic resin dispersant may be a commercially available product. Suitable commercially available acrylic resin dispersants include DISPERBYK (registered trademark)-2001 (amine value 63 mg KOH / g, acid value 41 mg KOH / g) manufactured by BYK Japan Co., Ltd.
[0039] As the polyester-based resin dispersant, the amine-containing polyester-based dispersant disclosed in JP 2015-068914 A can be used.
[0040] The polyester resin dispersant may be a commercially available product. Suitable commercially available polyester resin dispersants include: Manufactured by Ajinomoto Fine-Techno Co., Ltd. AJISPER PB-711 (amine value 112.5 mg KOH / g, acid value 0 mg KOH / g), AJISPER PB-821 (amine value 9.5 mg KOH / g, acid value 18 mg KOH / g) etc. can be used.
[0041] As a resin dispersant having an amide bond in a side chain, the dispersant disclosed in JP 2019-002005 can be used.
[0042] From the viewpoint of optical properties such as dispersion stability, OD value, and color purity, the content of the dispersant is preferably 5% by mass or more and 80% by mass or less, and more preferably 20% by mass or more and 60% by mass or less, relative to the mass of the resin-coated lactam black (if a pigment derivative is also included, the total mass of the resin-coated lactam black and the pigment derivative).
[0043] (solvent) As the solvent, various organic solvents such as aromatic, ketone, ester, glycol ether, alcohol, aliphatic, etc. may be used. The organic solvent may be used alone or in combination of two or more kinds.
[0044] Examples of aromatic organic solvents include aromatic hydrocarbons such as toluene, xylene, and ethylbenzene.
[0045] Examples of the ketone-based organic solvent include methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, acetylacetone, isophorone, acetophenone, and cyclohexanone.
[0046] Examples of ester-based organic solvents include ethyl acetate, n-butyl acetate, isobutyl acetate, isopropyl acetate, methyl propionate, 3-methoxybutyl acetate, ethyl glycol acetate, propylene glycol monomethyl ether acetate (PMA), propylene glycol monoethyl ether acetate, propylene glycol methyl ether propionate, 3-methyl-3-methoxybutyl acetate, methyl monochloroacetate, ethyl monochloroacetate, butyl monochloroacetate, methyl acetoacetate, ethyl acetoacetate, butyl carbitol acetate, butyl lactate, ethyl 3-ethoxypropionate, ethylene glycol monobutyl ether acetate, ethylene glycol monomethyl ether acetate, propyl acetate, and 1,3-butylene glycol diacetate.
[0047] Examples of glycol ether-based organic solvents include water-soluble glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, ethylene glycol mono-iso-propyl ether, diethylene glycol mono-iso-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol mono-n-butyl ether, ethylene glycol mono-t-butyl ether, diethylene glycol mono-t-butyl ether, 1-methyl-1-methoxybutanol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-iso-propyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and dipropylene glycol monopropyl ether; Examples of the glycol ethers include water-insoluble glycol ethers such as ethylene glycol monohexyl ether, ethylene glycol-2-ethylhexyl ether, ethylene glycol phenyl ether, diethylene glycol-n-hexyl ether, diethylene glycol-2-ethylhexyl ether, and dipropylene glycol monobutyl ether.
[0048] Examples of the alcohol-based organic solvent include alkyl alcohols having 1 to 4 carbon atoms, such as ethanol, methanol, butanol, propanol, and isopropanol; Examples of the glycol include ethylene glycol, propylene glycol, diethylene glycol, pentamethylene glycol, trimethylene glycol, 2-butene-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, tripropylene glycol, polyethylene glycols with a molecular weight of 2000 or less, isopropylene glycol, isobutylene glycol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, glycerin, mesoerythritol, and pentaerythritol.
[0049] Examples of the aliphatic organic solvent include aliphatic hydrocarbons such as n-pentane, n-hexane, and n-heptane.
[0050] From the viewpoint of ease of handling, the content of the solvent is preferably adjusted so that the solid content concentration including the pigment etc. is 6 to 40 mass %.
[0051] The black pigment dispersion of the present invention may contain other additives in addition to the above-mentioned components, as necessary. Examples of the other additives include an antioxidant, an anti-aggregation agent, a surface conditioner (leveling agent), etc.
[0052] (Step B: Mixing finely divided lactam black with a dispersant and a solvent) The black pigment dispersion of the present invention can be obtained by step B, which involves mixing the resin-coated lactam black, a dispersant, and a solvent. Step B is a step of dispersing the above-mentioned components, and for example, a known dispersing machine such as a bead mill, a sand mill, a disperser, or a paint shaker can be used. There is no particular limitation on the way in which the components are mixed, and the components may be added to the dispersing machine at the same time, or may be added one by one.
[0053] <Production Example of Black Pigment Composition> A black pigment dispersion was produced using the following raw materials and production method.
[0054] (Preparation Example 1 of Lactam Black / Resin-Coated Micronized Lactam Black) Irgaphor (registered trademark) Black S0100CF (manufactured by DIC Corporation) was used as the lactam black. 100 parts by mass of this lactam black, 700 parts by mass of neutral anhydrous Glauber's salt (manufactured by Mitajiri Chemical Industry Co., Ltd., average particle size 20 μm) as a water-soluble inorganic salt, and 155 parts by mass of ethylene glycol as a water-soluble solvent were charged into a twin-arm kneader (manufactured by Nihon Spindle Manufacturing Co., Ltd., 5L kneader Σ type) and kneaded at 50 ° C for 7 hours. Next, acrylic resin A (acid value 92.3 mg KOH / g) was charged so that the solid content was 15 parts by mass, and kneaded at 50 ° C for 1 hour. The obtained kneaded product was stirred and dispersed in 12 L of hot water at 60 ° C, and further adjusted to pH 2.4 with hydrochloric acid, and then stirred for about 1 hour to form a slurry. Thereafter, it was filtered and washed with water to remove the Glauber's salt and the solvent, and dried in a thermostatic bath at 60 ° C to obtain the fine lactam black of Preparation Example 1.
[0055] (Preparation Example 2 of Lactam Black / Resin-Coated Micronized Lactam Black) The same procedure as in Preparation Example 1 was repeated except that acrylic resin C (acid value 33.0 mgKOH / g) was used instead of acrylic resin A, to obtain finely divided lactam black of Preparation Example 2.
[0056] (Lactam Black Preparation Example 3 / Resin-Coated Micronized Lactam Black) The same procedure as in Preparation Example 1 was repeated except that acrylic resin D (acid value 10.0 mgKOH / g) was used instead of acrylic resin A, to obtain finely divided lactam black of Preparation Example 3.
[0057] (Lactam Black Preparation Example 4 / Non-resin-coated fine lactam black) The same procedures as in Preparation Example 1 were carried out except that acrylic resin A was not used and kneading was not carried out after the addition of acrylic resin A, to obtain a finely divided lactam black of Preparation Example 4.
[0058] The conditions for Preparation Examples 1 to 4 are shown in Table 1. The numbers in Table 1 represent parts by mass.
[0059] [Table 1]
[0060] [Example 1] Into a polyethylene container, 115 parts by mass of the finely divided lactam black of Preparation Example 1, 35 parts by mass of DISPERBYK (registered trademark)-167 (manufactured by BYK Japan Co., Ltd.) as a dispersant in terms of solid content, 350 parts by mass of PMA (propylene glycol monomethyl ether acetate) as a solvent, and 2000 parts by mass of zirconia beads (φ0.5 mm) were added. Dispersion treatment was carried out for 60 minutes using a paint shaker (manufactured by Asada Iron Works Co., Ltd.), and then 214 parts by mass of PMA was added to adjust the solid content concentration to 21% by mass, thereby obtaining a black pigment dispersion of Example 1.
[0061] [Example 2] A black pigment dispersion of Example 2 was obtained in the same manner as in Example 1, except that 115 parts by mass of the finely divided lactam black of Preparation Example 2 was used instead of the finely divided lactam black of Preparation Example 1.
[0062] [Comparative Example 1] A black pigment dispersion of Comparative Example 1 was obtained in the same manner as in Example 1, except that 115 parts by mass of the finely divided lactam black of Preparation Example 3 was used instead of the finely divided lactam black of Preparation Example 1.
[0063] [Comparative Example 2] A black pigment dispersion of Comparative Example 2 was obtained by the same procedure as in Example 1, except that 100 parts by mass of the finely divided lactam black of Preparation Example 4 was used instead of the finely divided lactam black of Preparation Example 1, and 15 parts by mass of acrylic resin A was added as the dispersing resin in a polyethylene container in terms of solid content to perform a dispersion treatment.
[0064] [Comparative Example 3] A black pigment dispersion of Comparative Example 3 was obtained in the same manner as in Comparative Example 2, except that acrylic resin B (acid value 94.9 mgKOH / g) was used instead of acrylic resin A as the dispersing resin.
[0065] [Comparative Example 4] A black pigment dispersion of Comparative Example 4 was obtained in the same manner as in Comparative Example 2, except that acrylic resin C was used instead of acrylic resin A as the dispersing resin.
[0066] [Comparative Example 5] A black pigment dispersion of Comparative Example 5 was obtained by the same procedure as in Comparative Example 3, except that Irgaphor (registered trademark) Black S0100CF was used as it was without being micronized instead of the micronized lactam black of Preparation Example 4.
[0067] <Viscosity measurement> The viscosities of the black pigment dispersions of Examples 1 and 2 and Comparative Examples 1 to 5 immediately after preparation were measured using an E-type viscometer (TV-25, manufactured by Toki Sangyo Co., Ltd.).
[0068] The compositions and viscosities of the black pigment dispersions of Examples 1 and 2 and Comparative Examples 1 to 5 are shown in Table 2. Each black pigment dispersion contains 100 parts by mass of lactam black, (1) 15 parts by mass of acrylic resin, and (2) 35 parts by mass of DISPERBYK-167 as a dispersant. The final composition of each black pigment dispersion is lactam black / acrylic resin / dispersant / solvent=1 / 0.15 / 0.35 / 5.64 by mass.
[0069] [Table 2]
[0070] <Preparation of a cured film-forming composition for measuring optical density (OD value)> A cured film-forming composition was prepared by mixing 100 parts by mass of the black pigment dispersion of Examples 1 to 2 and Comparative Examples 1 to 5, 7 parts by mass of acrylic resin B (resin for forming coating film) converted into solid content, and 4.5 parts by mass of PMA.
[0071] <Preparation Conditions of Hard Film for OD Value Measurement> Using the prepared composition for forming a hard film for OD value measurement, spin-coat it on a glass plate, heat it at 90 °C for 2.5 minutes as pre-baking and at 230 °C for 30 minutes as post-baking to form a hard film. The rotation speed of spin-coating was adjusted according to the desired film thickness.
[0072] <Measurement of OD Value of Hard Film> Using the formed hard film, the OD value was measured with an OD measuring device (manufactured by X-Rite, X-Rite 361T). The OD values of three hard films with different film thicknesses centered on 1 μm were measured, and the value at a film thickness of 1 μm was calculated as the OD value from the slope and intercept.
[0073] <Preparation of Composition for Forming Hard Film for Development Test> 62.1 parts by weight of the above-mentioned composition for forming a hard film for OD measurement, 30.7 parts by mass of a photosensitive solution (a liquid formulated with a mass ratio of resin / photopolymerizable monomer / photoinitiator / adhesion promoter / crosslinking agent / solvent = 4.3 / 7.4 / 5.4 / 0.2 / 2.7 / 80), and 7.2 parts by mass of PMA (solid content concentration 19.8% by mass) were mixed to prepare a composition for forming a hard film for development test.
[0074] <Development Property Evaluation> The prepared composition for forming a hard film for development test was spin-coated on a glass plate at 480 rpm for 6 seconds, dried at room temperature for 5 minutes, and then dried on a hot plate at 80 °C for 2.5 minutes. Then, it was exposed with an exposure amount of 20 mJ / cm 2 , with a mask gap of 50 μm. Development was carried out using a 0.04% KOH aqueous solution, and the time required for development was measured.
[0075] Subsequently, it was rinsed for 20 seconds, and the obtained development pattern was observed with an optical microscope to evaluate the developability. Specifically, in the exposure process, the presence or absence of residues in the area not irradiated with light (unexposed part) was observed with an optical microscope to evaluate the developability. The evaluation criteria are as follows. - Evaluation Criteria - ○: No residue was confirmed in the unexposed part. ×: Residue was observed in the unexposed area.
[0076] Furthermore, the surface roughness (Ra) of the developed pattern was measured at a magnification of 100 times using a laser microscope (Keyence Corporation, VK-X100).
[0077] Table 3 shows the measurement results of the OD value, the time required for development, the residue evaluation index, and the surface roughness (Ra) of the cured film-forming composition for the development test. The OD value was similar for all cured films, and there was no problem with practical use. As shown in Table 3, cured films No. 1 and No. 2 had no residue and a small surface roughness (Ra) of 0.01. Cured film No. 7 had no residue, but had a large surface roughness (Ra) of 0.04. This means that cured film No. 7 had a lower surface smoothness of the developed pattern. In addition, cured film No. 3 was not developable, and cured films No. 4 to No. 6 had a small surface roughness (Ra) of 0.01, the same as cured films No. 1 and No. 2, but had residue, so it was determined that they were not practical as cured films. As described above, it was confirmed that the cured films No. 1 and No. 2 prepared using the black pigment dispersions of Examples 1 and 2 had no residue after development and had small surface roughness (Ra) of the pattern.
[0078] [Table 3]
[0079] The acrylic resins used in Examples 1 and 2 (acrylic resins A and C) had acid values of 33.0 to 92.3 mgKOH / g, and the acrylic resin used in Comparative Example 1 had an acid value of 10.0 mgKOH / g. Therefore, it was determined that it is preferable to use an acrylic resin having an acidic group and an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less as the acrylic resin.
[0080] In the cured film-forming compositions No. 4 and No. 6 prepared from the black pigment dispersions of Comparative Examples 2 and 4 in which the lactam black was not coated with the acrylic resins A and C but was used as a dispersing resin, residues remained after development. This confirmed that in the present invention, an acrylic resin having an acidic group and an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less needs to be used as a resin for coating the lactam black, rather than as a dispersing resin. [Industrial Applicability]
[0081] The black pigment dispersion for forming a cured film and the method for producing the same of the present invention are useful in technical fields such as displays, solid-state imaging devices, and infrared sensors.
Claims
1. a lactam black coated with a resin having an acidic group; A dispersant; A black pigment dispersion comprising: The resin is at least one selected from the group consisting of acrylic acid resins, methacrylic acid resins, and maleic acid resins, and has an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less. Black pigment dispersion for forming cured films.
2. 2. The black pigment dispersion for forming a cured film according to claim 1, wherein a content of the lactam black coated with the resin having an acidic group in the black pigment dispersion is 5 mass % or more and 25 mass % or less relative to the mass of the black pigment dispersion.
3. A step A of wet-grinding lactam black; A method for producing a black pigment dispersion, comprising: a step B of mixing the lactam black finely divided by the step A, a dispersant, and a solvent, In the step A, a resin which is one or more selected from the group consisting of an acrylic acid resin, a methacrylic acid resin, and a maleic acid resin and has an acid value of 30 mgKOH / g or more and 100 mgKOH / g or less is added to finely disperse the lactam black. A method for producing a black pigment dispersion for forming a cured film.
Citation Information
Patent Citations
Pigment dispersion composition for black matrix, and pigment dispersion resist composition for black matrix
JP2021177204A
Black pigment dispersion and chromatic color pigment dispersion
JP2023004245A
Dispersion for black partition materials
JP2023161757A
Black resin composition for touch panels
WO2014208348A1
Near-infrared transmitting black azo pigments
US20020121228A1