Transparent conductive film
The transparent conductive film with a roughened surface and rare gas-containing layer addresses adhesion issues in foldable displays by enhancing bonding strength and peeling resistance through higher energy deposition using krypton as the sputtering gas.
Patent Information
- Application Number
- JP2023082973
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
AI Technical Summary
Transparent conductive films used in foldable display panels face challenges with the adhesion of the transparent conductive layer to the transparent base material, necessitating improved bonding to withstand bending and folding without peeling.
A transparent conductive film with a transparent base material having a surface roughness of 1.50 nm or more and a transparent conductive layer containing rare gas atoms with an atomic number greater than argon, formed using a sputtering method with a rare gas as the sputtering gas, enhances adhesion by increasing the anchoring effect.
The configuration ensures high adhesion of the transparent conductive layer to the base material, suitable for foldable displays by improving bonding strength and resistance to peeling, particularly through the use of krypton as the sputtering gas for higher energy deposition.
Smart Images

Figure 2024166688000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent conductive film. [Background technology]
[0002] Conventionally, a transparent conductive film is known which includes a resin transparent substrate and a transparent conductive layer in that order in the thickness direction. The transparent conductive layer is used as a conductive film for forming a transparent electrode in various devices such as a display panel, a touch panel, and a solar cell. The transparent conductive layer is formed, for example, by forming a film of a transparent conductive material on a transparent substrate by a sputtering method (sputtering film formation). In sputtering film formation, argon is conventionally used as a sputtering gas (inert gas). Technology relating to such a transparent conductive film is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-213990 A Summary of the Invention [Problem to be solved by the invention]
[0004] Transparent conductive films require good adhesion of the transparent conductive layer to the transparent substrate so that the transparent conductive layer does not peel off from the transparent substrate. Meanwhile, development of display panels that can be repeatedly folded (foldable) for smartphones and tablet terminals is progressing. For example, transparent conductive films for foldable display panels strongly require high adhesion of the transparent conductive layer to the transparent substrate.
[0005] The present invention provides a transparent conductive film suitable for achieving high adhesion of a transparent conductive layer to a transparent substrate. [Means for solving the problem]
[0006] The present invention [1] includes a transparent conductive film comprising a transparent substrate having a first surface and a second surface opposite to the first surface, and a transparent conductive layer on the first surface, wherein the first surface has a surface roughness Ra of 1.50 nm or more, and the transparent conductive layer contains rare gas atoms having an atomic number greater than that of argon.
[0007] The present invention [2] includes the transparent conductive film according to the above [1], in which the rare gas atom is krypton.
[0008] The present invention [3] includes the transparent conductive film according to the above [1] or [2], in which the transparent conductive layer is a crystalline film.
[0009] The present invention [4] includes the transparent conductive film according to any one of the above [1] to [3], wherein the surface roughness Ra is 2.50 nm or less.
[0010] The present invention [5] includes the transparent conductive film according to any one of the above [1] to [4], wherein the transparent substrate has an easy-adhesion layer forming the first surface, and the easy-adhesion layer has an average thickness of 50 nm or less. Effect of the Invention
[0011] In the transparent conductive film of the present invention, as described above, the surface roughness Ra of the first surface of the transparent substrate is 1.50 nm or more, and a transparent conductive layer is formed on the first surface. Such a configuration is suitable for ensuring a high anchoring effect of the first surface to the transparent conductive layer, and is useful for improving the adhesion of the transparent conductive layer to the transparent substrate. In addition, in the transparent conductive film of the present invention, as described above, the transparent conductive layer contains rare gas atoms having an atomic number larger than that of argon. Such a transparent conductive layer can be formed by sputtering film formation of a transparent conductive material on the first surface. In the sputtering film formation, rare gas atoms having an atomic number larger than that of argon are used as a sputtering gas. In such sputtering film formation, the transparent conductive material can be collided with the transparent substrate with higher energy and deposited on the substrate than in the sputtering film formation using argon as the sputtering gas. This is useful for improving the adhesion of the transparent conductive layer to the transparent substrate. Therefore, the transparent conductive film of the present invention is suitable for realizing high adhesion of the transparent conductive layer to the transparent substrate. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of a transparent conductive film of the present invention. [Diagram 2] FIG 2 shows an example of a method for producing the transparent conductive film shown in FIG 1. FIG 2A shows a step of preparing a resin film, FIG 2B shows a step of forming an easy-adhesion layer on the resin film, and FIG 2C shows a step of forming a transparent conductive layer on the easy-adhesion layer. [Diagram 3] This illustrates a case where the transparent conductive layer in the transparent conductive film shown in FIG. 1 is patterned. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A transparent conductive film X according to an embodiment of the present invention includes a transparent substrate 10 and a transparent conductive layer 20 in this order in a thickness direction D. The transparent substrate 10 has a first surface 10a and a second surface 10b opposite to the first surface 10a. The transparent conductive layer 20 is disposed on the first surface 10a. That is, the transparent conductive layer 20 is in contact with the first surface 10a. The transparent conductive film X has a sheet shape that spreads in a direction (plane direction) perpendicular to the thickness direction D. Such a transparent conductive film X is an element included in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device (display panel), and the like.
[0014] In this embodiment, the transparent substrate 10 includes a resin film 11 and an easy-adhesion layer 12 in this order in a thickness direction D. The easy-adhesion layer 12 is in contact with the resin film 11. The easy-adhesion layer 12 forms a first surface 10a.
[0015] The surface roughness Ra of the first surface 10a is 1.50 nm or more, preferably 1.60 nm or more, and more preferably 1.65 nm or more, from the viewpoint of ensuring a high anchoring effect of the first surface 10a to the transparent conductive layer 20. From the viewpoint of ease of forming the crystalline transparent conductive layer 20, the surface roughness Ra is preferably 2.50 nm or less, more preferably 2.20 nm or less, and even more preferably 2.00 nm or less. The surface roughness Ra is the arithmetic mean surface roughness based on JIS B 0601-2001. The method of measuring the surface roughness Ra is specifically as described below in the examples.
[0016] The resin film 11 is a base material that ensures the strength of the transparent conductive film X. The resin film 11 is a transparent resin film having flexibility. Examples of the material of the resin film 11 include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyolefin resin include polyethylene, polypropylene, and cycloolefin polymer. Examples of the acrylic resin include polymethacrylate. As the material of the resin film 11, for example, from the viewpoint of transparency and strength, a polyester resin is preferably used, and more preferably PET is used.
[0017] The surface of the resin film 11 on the side of the easy-adhesion layer 12 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.
[0018] The thickness of the resin film 11 is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, from the viewpoint of ensuring the strength of the transparent conductive film X. The thickness of the resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of ensuring the handleability of the resin film 11 in the roll-to-roll system.
[0019] The total light transmittance (JIS K 7375-2008) of the resin film 11 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The total light transmittance of the resin film 11 is, for example, 100% or less.
[0020] The easy-adhesion layer 12 improves the adhesion of the transparent conductive layer 20 to the transparent substrate 10. In this embodiment, the easy-adhesion layer 12 is a cured product of a curable resin composition containing a curable resin and particles. Examples of the curable resin include polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, epoxy resin, and melamine resin. These curable resins may be used alone or in combination of two or more kinds.
[0021] Examples of the curable resin include ultraviolet-curable resins and thermosetting resins. The ultraviolet-curable resin is preferred as the curable resin because it can be cured without high temperature heating and therefore helps improve the production efficiency of the transparent conductive film X.
[0022] Examples of the particles include inorganic oxide particles and organic particles. Examples of the inorganic oxide particle material include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of the organic particle material include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate. The particles are preferably inorganic oxide particles, and more preferably silica particles and / or zirconia particles.
[0023] The average particle diameter (D50) of the particles is preferably 20 nm or more, more preferably 25 nm or more, and even more preferably 30 nm or more, from the viewpoint of forming sufficient surface unevenness on the first surface 10a. The average particle diameter of the particles is preferably 200 nm or less, more preferably 150 nm or less, even more preferably 120 nm or less, and particularly preferably 100 nm or less, from the viewpoint of appropriately forming a crystalline transparent conductive layer 20 (from the viewpoint of suppressing inhibition of crystallization of the transparent conductive layer 20). The average particle diameter (D50) of the particles is the median diameter in a volume-based particle size distribution (the particle diameter at which the volume cumulative frequency reaches 50% from the small diameter side), and is determined, for example, based on a particle size distribution obtained by a laser diffraction / scattering method (the same applies to the average particle diameters of other particles).
[0024] The content of the particles in the easy-adhesion layer 12 is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 8 parts by mass or more per 100 parts by mass of the curable resin from the viewpoint of ensuring the surface irregularities of the first surface 10a. The content of the particles in the easy-adhesion layer 12 is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 12 parts by mass or less per 100 parts by mass of the curable resin.
[0025] The average thickness of the easy-adhesion layer 12 is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 7 nm or more, and particularly preferably 9 nm or more, from the viewpoint of ensuring adhesion with the transparent conductive layer 20. The average thickness of the easy-adhesion layer 12 is preferably 50 nm or less, more preferably 30 nm or less, and even more preferably 20 nm or less, from the viewpoint of thinning the transparent conductive film X. The method for measuring the average thickness of the easy-adhesion layer 12 is specifically as described below in the examples.
[0026] The surface of the adhesive layer 12 on the transparent conductive layer 20 side may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.
[0027] The thickness of the transparent substrate 10 is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. The thickness of the transparent substrate 10 is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less. These configurations regarding the thickness of the transparent substrate 10 are suitable for ensuring the handleability of the transparent conductive film X.
[0028] The total light transmittance (JIS K 7375-2008) of the transparent substrate 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The total light transmittance of the transparent substrate 10 is, for example, 100% or less.
[0029] The transparent conductive layer 20 is a film having both optical transparency and electrical conductivity. Such a transparent conductive layer 20 is formed from a transparent conductive material. An example of the transparent conductive material is a transparent conductive oxide. The transparent conductive layer 20 is preferably a crystalline film. The transparent conductive layer 20 being a crystalline film is suitable for suppressing a large fluctuation in the resistance value of the transparent conductive layer 20 due to subsequent heating.
[0030] The fact that the transparent conductive layer (the transparent conductive layer 20 on the transparent substrate 10 in the transparent conductive film X) is a crystalline film can be determined, for example, by the following method. First, the transparent conductive layer is immersed in hydrochloric acid with a concentration of 5% by mass at 20° C. for 15 minutes. Next, the transparent conductive layer is washed with water and then dried. Next, the resistance (inter-terminal resistance) between a pair of terminals separated by a distance of 15 mm is measured on the exposed plane of the transparent conductive layer (the surface 21 of the transparent conductive layer 20 on the opposite side to the transparent substrate 10 in the transparent conductive film X). In this measurement, if the inter-terminal resistance is 10 kΩ or less, it can be determined that the transparent conductive layer is a crystalline film. In addition, it can also be determined that the transparent conductive layer is a crystalline film by observing the presence of crystal grains in the transparent conductive layer with a transmission electron microscope.
[0031] Examples of the conductive oxide include indium-containing conductive oxide and antimony-containing conductive oxide. Examples of the indium-containing conductive oxide include indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), and indium gallium zinc composite oxide (IGZO). Examples of the antimony-containing conductive oxide include antimony tin composite oxide (ATO). From the viewpoint of realizing high transparency and good electrical conductivity, the conductive oxide is preferably an indium-containing conductive oxide, and more preferably ITO. This ITO may contain a metal or semimetal other than In and Sn in an amount less than the respective contents of In and Sn.
[0032] Indium oxide (In) in ITO 2 O 3 ) and tin oxide (SnO 2The ratio of the content of tin oxide to the total content of indium atoms (tin atoms / indium atoms) in ITO is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, and particularly preferably 7% by mass or more. The ratio of the number of tin atoms to the number of indium atoms in ITO (tin atoms / indium atoms) is preferably 0.01 or more, more preferably 0.03 or more, even more preferably 0.05 or more, and particularly preferably 0.07 or more. These configurations are suitable for ensuring the durability of the transparent conductive layer 20. In addition, the ratio of the content of tin oxide to the total content of indium oxide and tin oxide in ITO is preferably 15% by mass or less, more preferably 13% by mass or less, and even more preferably 12% by mass or less. The ratio of the number of tin atoms to the number of indium atoms in ITO (tin atoms / indium atoms) is preferably 0.15 or less, more preferably 0.13 or less, and even more preferably 0.12 or less. These configurations are preferable from the viewpoint of reducing the resistance of the transparent conductive layer 20.
[0033] The tin oxide ratio in ITO can be identified, for example, as follows. First, the abundance ratio of indium atoms (In) and tin atoms (Sn) in ITO, which is the object to be measured, is determined by X-ray photoelectron spectroscopy. From the abundance ratios of In and Sn in ITO, the ratio of the number of Sn atoms to the number of In atoms in ITO is determined. This gives the tin oxide ratio in ITO. The tin oxide ratio in ITO can also be determined by the tin oxide (SnO 2 ) content ratio can also be identified.
[0034] The transparent conductive layer 20 contains a rare gas atom (atom E) having an atomic number larger than that of argon. Examples of such rare gas atoms include krypton (Kr) and xenon (Xe), and preferably Kr is used. The transparent conductive layer 20 may also contain argon (Ar). In this embodiment, the rare gas atoms in the transparent conductive layer 20 are derived from rare gas atoms used as a sputtering gas in a sputtering method described later for forming the transparent conductive layer 20. In this embodiment, the transparent conductive layer 20 is a film (sputtered film) formed by a sputtering method. The transparent conductive layer 20 containing atom E is useful for improving the adhesion of the transparent conductive layer 20 to the transparent substrate 10, as described later. Methods for determining whether the transparent conductive layer 20 contains atom E include, for example, fluorescent X-ray analysis and Rutherford Backscattering Spectrometry (RBS).
[0035] The content of atom E in the transparent conductive layer 20 is preferably 0.0001 atomic % or more, and preferably 1 atomic % or less, more preferably 0.5 atomic % or less, further preferably 0.3 atomic % or less, and particularly preferably 0.2 atomic % or less, in the entire region in the thickness direction D. Examples of a method for identifying the content of rare gas atoms in the transparent conductive layer 20 include fluorescent X-ray analysis and Rutherford backscattering spectrometry (RBS). Even if the content of atom E is below the detection limit in the method for identifying the content of rare gas atoms, if the presence of atom E is confirmed by the above-mentioned method for identifying atom E in the transparent conductive layer 20, the transparent conductive layer 20 contains atom E.
[0036] The thickness of the transparent conductive layer 20 is preferably 10 nm or more, more preferably 20 nm or more, and even more preferably 30 nm or more, from the viewpoint of reducing the resistance of the transparent conductive layer 20. Moreover, the thickness of the transparent conductive layer 20 is preferably 300 nm or less, more preferably 150 nm or less, even more preferably 120 nm or less, even more preferably 100 nm or less, and particularly preferably 80 nm or less, from the viewpoint of ensuring flexibility (resistance to cracking when bent).
[0037] The total light transmittance (JIS K 7375-2008) of the transparent conductive layer 20 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency of the transparent conductive layer 20. The total light transmittance of the transparent conductive layer 20 is, for example, 100% or less.
[0038] The total light transmittance (JIS K 7375-2008) of the transparent conductive film X is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The total light transmittance of the base film 10 is, for example, 100% or less.
[0039] The transparent conductive film X is produced, for example, as follows.
[0040] First, as shown in FIG. 2A, a resin film 11 is prepared.
[0041] 2B, an adhesive layer 12 is formed on one surface of the resin film 11 in the thickness direction D. By forming the adhesive layer 12 on the resin film 11, a transparent substrate 10 is produced.
[0042] The adhesive layer 12 can be formed by applying the above-mentioned curable resin composition onto the resin film 11 to form a coating film, and then curing the coating film. When the curable resin composition contains an ultraviolet-curable resin, the coating film is cured by ultraviolet irradiation. When the curable resin composition contains a thermosetting resin, the coating film is cured by heating.
[0043] The exposed surface of the adhesive layer 12 formed on the resin film 11 is subjected to a surface modification treatment as necessary. When a plasma treatment is performed as the surface modification treatment, for example, argon gas is used as an inert gas. The discharge power in the plasma treatment is, for example, 10 W or more and, for example, 5000 W or less.
[0044] 2C, a transparent conductive layer 20 is formed on the transparent substrate 10 (transparent conductive layer forming step). Specifically, a transparent conductive material is deposited on the easy-adhesion layer 12 of the transparent substrate 10 by a sputtering method to form the transparent conductive layer 20.
[0045] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a film formation process by a roll-to-roll method. When using a sputtering deposition apparatus of the roll-to-roll method in the manufacture of the transparent conductive film X, a material is deposited on the transparent substrate 10 while the long transparent substrate 10 is traveling from a pay-out roll to a take-up roll provided in the apparatus, thereby forming the transparent conductive layer 20. In addition, in the sputtering method, a sputtering deposition apparatus having one deposition chamber may be used, or a sputtering deposition apparatus having multiple deposition chambers arranged in order along the traveling path of the transparent substrate 10 may be used.
[0046] In the sputtering method, specifically, a sputtering gas (inert gas) is introduced under vacuum conditions into a film-forming chamber equipped with a sputtering film-forming apparatus, while a negative voltage is applied to a target placed on a cathode in the film-forming chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed to eject target material from the target surface, and the ejected target material is deposited on the transparent substrate 10. For example, the sintered body of the conductive oxide described above for the transparent conductive layer 20 is used as the target material. As the sputtering gas, a rare gas atom (atom E) having an atomic number larger than that of argon is used. The atom E has a larger mass than argon. Therefore, the atom E is suitable for colliding with the target with higher energy than argon, and therefore is suitable for ejecting the target material from the target surface with high energy. As the atom E, Kr is preferably used. As the sputtering gas, a mixed gas containing the atom E and argon may be used.
[0047] The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, for example, oxygen as a reactive gas is introduced into the film formation chamber in addition to the sputtering gas. In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of the sputtering gas and oxygen introduced into the film formation chamber is, for example, 0.01 flow % or more, and, for example, 15 flow % or less.
[0048] The air pressure in the film formation chamber during film formation by sputtering (sputter film formation) is, for example, 0.02 Pa or more and, for example, 1 Pa or less.
[0049] The temperature of the transparent substrate 10 during sputtering deposition is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher, from the viewpoint of promoting crystal growth of the material to be deposited and forming the transparent conductive layer 20 as a good crystalline film. The temperature of the transparent substrate 10 during sputtering deposition is preferably 100° C. or lower, more preferably 70° C. or lower, and even more preferably 50° C. or lower, from the viewpoint of suppressing outgassing from the transparent substrate 10 during sputtering deposition and forming the transparent conductive layer 20 as a good crystalline film.
[0050] Examples of power sources for applying voltage to the target include DC power sources, AC power sources, MF power sources, and RF power sources. A DC power source and an RF power source may be used in combination as the power source. The absolute value of the discharge voltage during sputtering deposition is, for example, 50 V or more, and, for example, 500 V or less. The horizontal magnetic field strength on the target is, for example, 10 mT or more, and, for example, 100 mT or less.
[0051] In this manner, the transparent conductive film X can be produced.
[0052] The transparent conductive layer 20 in the transparent conductive film X may be patterned as shown in Fig. 3. The transparent conductive layer 20 can be patterned by etching the transparent conductive layer 20 through a predetermined etching mask. The patterned transparent conductive layer 20 functions as, for example, a wiring pattern.
[0053] In the transparent conductive film X, as described above, the surface roughness Ra of the first surface 10a of the transparent substrate 10 is 1.50 nm or more, preferably 1.60 nm or more, and more preferably 1.65 nm or more, and the transparent conductive layer 20 is formed on the first surface 10a. Such a configuration is suitable for ensuring a high anchoring effect of the first surface 10a to the transparent conductive layer 20, and is useful for improving the adhesion of the transparent conductive layer 20 to the transparent substrate 10.
[0054] Additionally, in the transparent conductive film X, the transparent conductive layer 20 contains rare gas atoms having an atomic number greater than that of argon. Such a transparent conductive layer 20 can be formed by sputtering a transparent conductive material onto the first surface 10a of the transparent substrate 10, as described above. In the sputtering deposition, the atom E (a rare gas atom having an atomic number greater than that of argon) is used as a sputtering gas. In such sputtering deposition, the transparent conductive material can be collided with and deposited on the transparent substrate 10 with higher energy than in sputtering deposition using argon as the sputtering gas. This helps to improve the adhesion of the transparent conductive layer 20 to the transparent substrate 10.
[0055] The transparent conductive film X as described above is suitable for achieving high adhesion of the transparent conductive layer 20 to the transparent substrate 10. Specific examples are as shown below in Examples and Comparative Examples. EXAMPLES
[0056] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".
[0057] Example 1 First, a roll of a long transparent substrate S (product name: "Diafoil T910E125", thickness 125 μm, manufactured by Mitsubishi Chemical Corporation) was prepared. The transparent substrate S consisted of a polyethylene terephthalate (PET) film (thickness 125 μm) as a resin film and an easy-adhesion layer formed on one side of the PET film. The easy-adhesion layer contained silica particles (average particle diameter 30 nm) as particles. The average thickness of the easy-adhesion layer was 10 nm.
[0058] Next, a 125 nm thick transparent conductive layer was formed on the easy-adhesion layer of the transparent substrate by reactive sputtering (transparent conductive layer formation process). In this process, a roll-to-roll sputter deposition device (DC magnetron sputter deposition device) was used. The device is equipped with a deposition chamber that can perform the deposition process while running the work film by the roll-to-roll method. The conditions for sputter deposition in this process are as follows:
[0059] In sputtering, the ultimate vacuum in the deposition chamber is 0.9×10 -4 After the sputtering deposition apparatus was evacuated to a pressure of 0.2 Pa, krypton (Kr) as a sputtering gas (inert gas) and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was set to 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of sputtering gas (Kr) and oxygen introduced into the deposition chamber was set to about 3.1 flow rate %. In addition, a sintered body of indium oxide and tin oxide (ITO with a tin oxide concentration of 10 mass %) was used as the target. A DC power supply was used as the power source for applying a voltage to the target. The horizontal magnetic field strength above the target was 90 mT. The deposition temperature (the temperature of the transparent substrate on which the transparent conductive layer is laminated) was set to 30°C.
[0060] In this manner, a transparent conductive film of Example 1 was produced. The transparent conductive film of Example 1 includes a transparent substrate S with an easy-adhesion layer and a transparent conductive layer on the easy-adhesion layer. The transparent conductive layer is an ITO layer (thickness 125 nm) containing Kr.
[0061] Example 2 The transparent conductive film of Example 2 was produced in the same manner as the transparent conductive film of Example 1, except for the following. In the transparent conductive layer forming step, a first layer having a thickness of 62.5 nm and a second layer having a thickness of 62.5 nm (second sputtering film formation) were sequentially formed on the easy-adhesion layer side of the transparent substrate S to form a transparent conductive layer (thickness 125 nm). The conditions of the first sputtering film formation for forming the first layer were the same as the conditions of the sputtering film formation described above for Example 1. In the second sputtering film formation for forming the second layer, argon (Ar) was used as the sputtering gas, and the ratio of the amount of oxygen introduced to the total amount of sputtering gas (Ar) and oxygen introduced into the film formation chamber was about 3.1 flow rate %. The other conditions of the second sputtering film formation were the same as the conditions of the sputtering film formation described above for Example 1.
[0062] The transparent conductive film of Example 2 includes a transparent substrate S and a transparent conductive layer on an easy-adhesion layer (the easy-adhesion layer is located directly below the transparent conductive layer). The transparent conductive layer includes an ITO layer (first layer) containing Kr and an ITO layer (second layer) containing Ar, in that order from the transparent substrate side.
[0063] Comparative Example 1 A transparent conductive film of Comparative Example 1 was produced in the same manner as the transparent conductive film of Example 1, except for the following. In the transparent conductive layer forming step, a transparent conductive layer was formed on the surface of the long transparent substrate S on the side on which the easy-adhesion layer was not formed. In addition, Ar was used as the sputtering gas, and the ratio of the amount of oxygen introduced to the total amount of sputtering gas (Ar) and oxygen introduced into the film formation chamber was set to about 3.1 flow rate %.
[0064] The transparent conductive film of Comparative Example 1 includes a transparent substrate S and a transparent conductive layer (there is no easy-adhesion layer directly below the transparent conductive layer). The transparent conductive layer is an ITO layer (thickness 125 nm) containing Ar.
[0065] Comparative Example 2 A transparent conductive film of Comparative Example 2 was produced in the same manner as the transparent conductive film of Example 1, except for the following: In the transparent conductive layer forming step, a transparent conductive layer was formed on the surface of the long transparent substrate S on the side on which the easy-adhesion layer was not formed.
[0066] The transparent conductive film of Comparative Example 2 includes a transparent substrate S and a transparent conductive layer (no easy-adhesion layer directly below the transparent conductive layer). The transparent conductive layer is an ITO layer (thickness 125 nm) containing Kr.
[0067] Comparative Example 3 A transparent conductive film of Comparative Example 3 was produced in the same manner as the transparent conductive film of Example 1, except for the following: In the transparent conductive layer forming step, Ar was used as the sputtering gas, and the ratio of the amount of oxygen introduced to the total amount of sputtering gas (Ar) and oxygen introduced into the film formation chamber was set to about 3.1 flow %.
[0068] The transparent conductive film of Comparative Example 3 includes a transparent substrate S and a transparent conductive layer (with an easy-adhesion layer directly below the transparent conductive layer). The transparent conductive layer is an ITO layer (thickness 125 nm) containing Ar.
[0069] <Thickness of Transparent Conductive Layer> The thickness of the transparent conductive layer of each of the transparent conductive films in Examples 1 and 2 and Comparative Examples 1 to 3 was measured by observation with a field emission transmission electron microscope (FE-TEM). Specifically, first, a cross-sectional observation sample of each of the transparent conductive layers in Examples 1 and 2 and Comparative Examples 1 to 3 was prepared by FIB microsampling. In the FIB microsampling method, an FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the cross-section of the transparent conductive layer in the cross-sectional observation sample was observed by FE-TEM, and the thickness of the transparent conductive layer was measured in the observed image. In the observation, an FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.
[0070] <Crystalline> The crystallinity of each of the transparent conductive layers in Examples 1 and 2 and Comparative Examples 1 to 3 was examined as follows. Each of the transparent conductive layers in Examples 1 and 2 and Comparative Examples 1 and 2 was a crystalline film. The transparent conductive layer in Comparative Example 3 was not a crystalline film.
[0071] First, the transparent conductive layer on the transparent substrate S was immersed in hydrochloric acid with a concentration of 5% by mass at 20°C for 15 minutes. Next, the transparent conductive layer was washed with water and then dried. Next, the resistance between a pair of terminals separated by a distance of 15 mm (inter-terminal resistance) was measured on the exposed surface of the transparent conductive layer. In this measurement, if the inter-terminal resistance was 10 kΩ or less, the transparent conductive layer was determined to be a crystalline film.
[0072] <Surface roughness> The roughness of the first surface (the surface on the transparent conductive layer side) of the transparent substrate was examined for each of the transparent conductive films of Examples 1 and 2 and Comparative Examples 1 to 3. Specifically, in the manufacturing process of the transparent conductive film, the surface roughness Ra (arithmetic mean surface roughness based on JIS B 0601-2001) of the first surface of the transparent substrate before the transparent conductive layer formation step was determined from an observation image of 1 μm square using an atomic force microscope (product name "Dimention-Edge SPM SYSTEM", manufactured by Bruker). The surface roughness Ra (nm) of the transparent conductive layer is shown in Table 1.
[0073] <Sliding test> For each of the transparent conductive films of Examples 1 and 2 and Comparative Examples 1 to 3, the adhesion of the transparent conductive layer to the transparent substrate was examined as follows.
[0074] First, a sample film (MD 10cm x TD 5cm) was cut out from a transparent conductive film (transparent substrate / transparent conductive layer). Next, the transparent substrate side of the sample film was bonded to a glass plate using a double-sided strong adhesive tape. Next, the glass plate with the sample film was set on the stage of a sliding tester (product name "10-pen tester", manufactured by MTM Corporation). Next, a sliding test was performed on the transparent conductive layer of the sample film on the glass plate using the sliding tester. Specifically, after ethanol was dropped on the transparent conductive layer of the sample film, a wipe as a sliding material was pressed against the dropped area with a load of 2 kg, and the wipe was moved back and forth in the MD direction 400 times (alcohol sliding test). Then, during and after this sliding test, the transparent conductive layer of the sample film was observed with a laser microscope (product name "VK-X1000", manufactured by Keyence Corporation) to confirm the presence or absence of peeling in the transparent conductive layer. Regarding the adhesion of the transparent conductive layer to the transparent substrate, the case where no peeling of the transparent conductive layer was observed after the sliding test was rated as "excellent," the case where only a small amount of peeling of the transparent conductive layer was observed after the sliding test was rated as "good," the case where no peeling of the transparent conductive layer was observed after 50 reciprocating movements but peeling of the transparent conductive layer was observed over the entire surface after the sliding test (400 reciprocating movements) was rated as "poor," and the case where peeling of the transparent conductive layer was observed over the entire surface after 50 reciprocating movements was rated as "very poor." The evaluation results are shown in Table 1.
[0075] Confirmation of Kr atoms in the transparent conductive layer The presence or absence of Kr atoms in each transparent conductive layer in Examples 1 and 2 and Comparative Examples 1 to 3 was confirmed as follows. First, using a scanning X-ray fluorescence analyzer (product name "ZSX PrimusIV", manufactured by Rigaku Corporation), fluorescent X-ray analysis was repeated five times under the following measurement conditions, and the average value of each scanning angle was calculated to create an X-ray spectrum. Then, by confirming that a peak appeared near a scanning angle of 28.2° in the created X-ray spectrum, it was confirmed that Kr atoms were contained in the transparent conductive layer. In this way, it was confirmed that each transparent conductive layer in Examples 1 and 2 and Comparative Example 2 contained Kr atoms, and that each transparent conductive layer in Comparative Examples 1 and 3 did not contain Kr.
[0076] <Measurement conditions> Spectrum;Kr-KA Measurement diameter: 30mm Atmosphere: Vacuum Target: Rh Tube voltage: 50kV Tube current: 60mA Primary filter: Ni40 Scanning angle (deg): 27.0~29.5 Step(deg):0.020 Speed (deg / min): 0.75 Attenuator: 1 / 1 Slit: S2 Spectroscopic crystal: LiF(200) Detector: SC PHA: 100~300
[0077] [Table 1] [Explanation of symbols]
[0078] X Transparent conductive film D Thickness direction 10 Transparent base material 10a 1st page 10b 2nd side 11 Resin film 12 Easy adhesive layer 20 Transparent conductive layer 21 Surface
Claims
1. a transparent substrate having a first surface and a second surface opposite to the first surface; a transparent conductive layer on the first surface, the first surface has a surface roughness Ra of 1.50 nm or more; A transparent conductive film, wherein the transparent conductive layer contains rare gas atoms having an atomic number greater than that of argon.
2. The transparent conductive film according to claim 1 , wherein the rare gas atoms are krypton.
3. The transparent conductive film according to claim 1 , wherein the transparent conductive layer is a crystalline film.
4. The transparent conductive film according to claim 1 , wherein the surface roughness Ra is 2.50 nm or less.
5. The transparent conductive film according to claim 1 , wherein the transparent substrate has an easy-adhesion layer that forms the first surface, and the easy-adhesion layer has an average thickness of 50 nm or less.
Citation Information
Patent Citations
Transparent conductive film and touch panel
JP2004213990A