Hydrogen gas barrier coated body

The laminated ZnO/AlO structure in the hydrogen gas barrier coating addresses the stress-related cracking and peeling issues of metal nitride films, providing superior hydrogen gas barrier performance and cost efficiency.

JP2024166692APending Publication Date: 2024-11-29DENSO CORP +2

Patent Information

Application Number
JP2023082980
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

Smart Images

  • Figure 2024166692000001_ABST
    Figure 2024166692000001_ABST
Patent Text Reader

Abstract

To provide a hydrogen gas barrier coated body that is coated with a hydrogen gas barrier film capable of suppressing detachment and obtaining a hydrogen gas barrier function.SOLUTION: A hydrogen gas barrier coated body includes: a substrate 10; and a hydrogen gas barrier film 20 arranged at one surface 10a of the substrate 10 and constituted of a laminate structure deposited with a ZnO film and an AlO film.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a hydrogen gas barrier coated article, which is an article coated with a hydrogen gas barrier film. [Background technology]

[0002] Patent Document 1 proposes a hydrogen gas barrier film having a total thickness of 0.5 to 2 μm, in which 10 to 1000 crystalline nano-thin films made of different types of metal nitride films are laminated multiple times. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-139009 Summary of the Invention [Problem to be solved by the invention]

[0004] However, metal nitride films have high stress due to their material properties, and the stress increases as the film thickness increases. High stress makes the film more susceptible to cracks and peeling. In addition, in crystalline films, cracks occur at grain boundaries, which become hydrogen permeation paths, reducing the hydrogen gas barrier function.

[0005] An object of the present disclosure is to provide a hydrogen gas barrier coated body that is coated with a hydrogen gas barrier film that can suppress peeling and provides hydrogen gas barrier function. [Means for solving the problem]

[0006] In order to achieve the above object, the invention described in claim 1 is a hydrogen gas barrier coating, comprising a substrate (10) and a hydrogen gas barrier film (20) disposed on one surface (10a) of the substrate and consisting of a laminated structure including a ZnO film (21) and an AlO film (22).

[0007] In this way, by forming a hydrogen gas barrier film with a laminated structure of a ZnO film and an AlO film, it is possible to obtain a hydrogen gas barrier function. Furthermore, since the hydrogen gas barrier film is formed not of a metal nitride film but of a ZnO film and an AlO film, the stress of the hydrogen gas barrier film can be reduced, and the occurrence of cracks in the film and peeling due to cracks can be suppressed. Therefore, it is possible to obtain a hydrogen gas barrier coating covered with a hydrogen gas barrier film that can suppress peeling and obtain a hydrogen gas barrier function.

[0008] The reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]

[0009] [Figure 1A] 1 is a cross-sectional view of a hydrogen gas barrier covering according to a first embodiment. [Figure 1B] FIG. 1B is a cross-sectional view showing a detailed structure of the hydrogen gas barrier film in FIG. 1A. [Diagram 2] 1 is a table showing the relationship between the film thickness, the number of layers, and the hydrogen permeability coefficient in Examples 1 to 5 and Comparative Examples 1 and 2. [Diagram 3] 1 is a table showing the relationship between the film thickness, the number of layers, and the hydrogen permeability coefficient in Examples 6 to 9 and Comparative Examples 3 and 4. [Figure 4] 1 is a graph summarizing the relationship between the number of layers and the hydrogen permeability coefficient in Examples 1 to 5. [Diagram 5] 1 is a graph summarizing the relationship between the number of layers and the hydrogen permeability coefficient in Examples 6 to 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.

[0011] (First embodiment) A hydrogen gas barrier coating according to the first embodiment will be described. As shown in Fig. 1, a hydrogen gas barrier film 20 is formed on one surface 10a of a substrate 10, and the one surface 10a of the substrate 10 is coated with the hydrogen gas barrier film 20 to form a hydrogen gas barrier coating.

[0012] The substrate 10 is a component that does not allow hydrogen gas to pass through, or a component that suppresses the movement of hydrogen gas to a component located on the opposite side of the substrate 10 across a space containing hydrogen gas. An example of the former is a tank wall in which hydrogen gas is stored in a hydrogen gas tank. An example of the latter is a film material in a hydrogen gas barrier film. The material of the substrate 10 may be any material that can form a hydrogen gas barrier film 20, and is, for example, a resin material such as PA (polyamide). The shape of the substrate 10 is arbitrary, and may be a three-dimensional structure or a film-like structure. The thickness of the substrate 10 is arbitrary, and may be, for example, 1 mm, and if it is 0.3 mm or less, it can be applied to a film-like structure.

[0013] The hydrogen gas barrier film 20 is composed of a laminated structure of a ZnO (zinc oxide) film 21 and an AlO (aluminum oxide) film 22. If the number of layers is defined as the number of layers when the ZnO film 21 and the AlO film 22 are formed one by one, the number of layers can be any number, but as described later, a number of layers of 40 or more is preferable since it provides a particularly good hydrogen gas barrier function. The overall thickness of the hydrogen gas barrier film 20 (hereinafter referred to as the total thickness) can be any number, but if the total thickness is too large, the stress in the entire film increases, so it is preferably 100 nm or less.

[0014] The ZnO film 21 is a crystalline film having a hydrogen gas barrier function. The thickness of the ZnO film 21 is arbitrary. However, if the thickness of the ZnO film 21 is too large, the stress becomes too large, and if the thickness is too small, the hydrogen gas barrier function is impaired, so the thickness of the ZnO film 21 in each layer is set to 1 nm to 40 nm. The thickness of the ZnO film 21 in each layer may be determined according to the total thickness of the hydrogen gas barrier film 20 and the number of layers of the ZnO film 21 and the AlO film 22. For example, the thickness of the ZnO film 21 may be determined according to the number of layers while keeping the total thickness 100 nm or less so that the stress does not become too large. Also, the thickness of the ZnO film 21 in each layer does not need to be the same, and may be different.

[0015] The AlO film 22 is an amorphous film, and by covering the ZnO film 21 of each layer, it ensures the hydrogen gas barrier function of the ZnO film 21, and also has a hydrogen gas barrier function itself. Incidentally, amorphous refers to a state of a substance that does not have a crystal structure, and is also called non-crystalline. The ZnO film 21 has a high hydrogen gas barrier function, but is a crystalline film in which grain boundaries may occur, so there is a possibility that hydrogen gas may permeate through the grain boundaries. For this reason, the AlO film 22, which is composed of an amorphous film alternately with the ZnO film 21, is formed to cover the grain boundaries of the ZnO film 21 and protect the gaps, thereby ensuring the hydrogen gas barrier function of the ZnO film 21 of each layer. In addition, it becomes possible to follow the deformation of the substrate 10, and the hydrogen gas barrier function can be obtained even if the substrate 10 is a thin film.

[0016] The thickness of the AlO film 22 is arbitrary. However, if the thickness of the AlO film 22 is too large, the stress becomes too large, and if the thickness is too small, the function of covering the grain boundaries of the ZnO film 21 is impaired, so the thickness of the AlO film 22 in each layer is set to 1 nm to 40 nm. The thickness of the AlO film 22 in each layer may be determined according to the total thickness of the hydrogen gas barrier film 20 and the number of layers of the ZnO film 21 and the AlO film 22. For example, the thickness of the AlO film 22 may be determined depending on the number of layers while keeping the total thickness at 100 nm or less so that the stress does not become too large. Also, the thickness of the AlO film 22 in each layer does not need to be the same, and may be different.

[0017] The order of lamination of the ZnO film 21 and the AlO film 22 on one surface 10a of the substrate 10 is arbitrary, and the ZnO film 21 or the AlO film 22 may be formed on one surface 10a. However, it is preferable that the outermost surface of the hydrogen gas barrier film 20 is not the ZnO film 21 in which grain boundaries may exist, but the AlO film 22 which covers it.

[0018] In this way, by forming a hydrogen gas barrier coating in which one surface 10a of the substrate 10 is coated with the hydrogen gas barrier film 20, a high hydrogen gas barrier function can be provided. Since the hydrogen gas barrier film 20 is formed of the ZnO film 21 and the AlO film 22 that do not contain a metal nitride film, the stress can be reduced compared to when the hydrogen gas barrier film 20 is formed of a metal nitride film. Therefore, cracks occurring in the film with high stress can be suppressed, and peeling can be suppressed. Even if grain boundaries exist in the crystalline ZnO film 21, since the film is covered with the AlO film 22, cracks occurring from the grain boundaries and deterioration of the hydrogen gas barrier function can be suppressed. Therefore, it is possible to obtain a hydrogen gas barrier coating that can suppress peeling and deterioration of the hydrogen gas barrier function.

[0019] Next, examples of the hydrogen gas barrier coating having the above-mentioned configuration will be described in comparison with comparative examples.

[0020] First, a plate-shaped PA was prepared as the substrate 10, and a ZnO film 21 and an AlO film 22 were alternately and repeatedly formed on one surface 10a of the substrate 10 made of this PA. Specifically, using an ALD (atomic layer deposition) apparatus, raw material gases of TMA (trimethylaluminum) as the raw material of the AlO film 22 and DEZn (diethylzinc) as the raw material of the ZnO film 21 were alternately introduced and exhausted at a temperature of 80°C. Then, atomic layers were deposited one by one to control the AlO film 22 and the ZnO film 21 to have the desired thicknesses, and the desired number of films were formed by repeating the alternating process.

[0021] FIG. 2 shows the measurement results of the hydrogen permeability coefficient when the AlO film 22 is formed on one surface 10a of a plate-shaped PA having a thickness of about 1 mm as the substrate 10, and then the ZnO film 21 is formed alternately, and finally the AlO film 22 is formed on the outermost surface. The total thickness of the AlO film 22 and the ZnO film 21 is about 85 nm. FIG. 3 shows the same measurement as in FIG. 2, performed using a film-shaped PA having a thickness of about 0.3 mm as the substrate 10. In the formula showing the film thickness of each example and each comparative example shown in the figure, the first term shows the film thickness of the outermost AlO film 22, and the second term shows the film thickness of each of the ZnO film 21 and the AlO film 22, and the repetition of laminating these two layers. In addition, the number of layers in each example and each comparative example shown in the figure shows the total number of layers, with each layer being one ZnO film 21 or one AlO film 22. The hydrogen permeability coefficient is evaluated by a measurement method based on the JIS standard (JIS K 7126-1). Specifically, a device capable of controlling the pressure of the spaces above and below the sample to be evaluated is used to introduce hydrogen gas into the upper space while controlling the space pressure, placing the lower space in a reduced pressure state close to a vacuum, and measuring the amount of hydrogen permeated from the upper space to the lower space. Under these conditions, the hydrogen permeability coefficient is calculated by multiplying the amount of hydrogen permeated by the thicknesses of the substrate 10 and the hydrogen gas barrier film 20. Since the thickness of the hydrogen gas barrier film 20 is sufficiently small compared to the thickness of the substrate 10, the hydrogen permeability coefficient is generally expressed as the amount of hydrogen permeated multiplied by the thickness of the substrate 10. For this reason, the thinner the substrate 10, the smaller the hydrogen permeability coefficient, but the hydrogen gas barrier function of the hydrogen gas barrier film 20 is generally the same if the film quality is the same.

[0022] 2, the hydrogen permeability coefficient was measured for Comparative Example 1, in which only the AlO film 22 was formed in a single layer with a thickness of 80 nm, and for Comparative Example 2, in which only the ZnO film 21 was formed in a single layer with a thickness of 80 nm. -16 (mol / msPa), and 1.4 × 10 -15 (mol / msPa).

[0023] In Example 1, the thickness of the AlO film 22 on the outermost surface was set to 5 nm, and the ZnO film 21 and the AlO film 22 were both set to 40 nm and laminated only once. In this case, the number of layers was 3, and the hydrogen permeability coefficient was 1.1×10 -16 In Example 2, the thickness of the AlO film 22 on the outermost surface was set to 5 nm, and the ZnO film 21 and the AlO film 22 were both set to 10 nm, and these were repeatedly stacked four times. In this case, the number of layers was 9, and the hydrogen permeability coefficient was 1.1×10 -16 In Example 3, the thickness of the AlO film 22 on the outermost surface was set to 5 nm, and the ZnO film 21 and the AlO film 22 were both set to 5 nm and repeatedly stacked 8 times. In this case, the number of stacked layers was 17, and the hydrogen permeability coefficient was 1.0×10 -16 (mol / msPa).

[0024] Furthermore, in Example 4, the thickness of the AlO film 22 on the outermost surface was set to 2 nm, and the ZnO film 21 and the AlO film 22 were both set to 2 nm and repeatedly stacked 20 times. In this case, the number of stacked layers was 41, and the hydrogen permeability coefficient was 6.4×10 -17 In Example 5, the thickness of the AlO film 22 on the outermost surface was set to 1 nm, and the ZnO film 21 and the AlO film 22 were both set to 1 nm and repeatedly stacked 40 times. In this case, the number of stacked layers was 81, and the hydrogen permeability coefficient was 8.0×10 -17 (mol / msPa).

[0025] 3, the hydrogen permeability coefficient was measured for Comparative Example 3 in which only the AlO film 22 was formed in a single layer with a thickness of 80 nm, and for Comparative Example 4 in which only the ZnO film 21 was formed in a single layer with a thickness of 80 nm. -16 (mol / msPa), and 5.4 × 10 -16 (mol / msPa).

[0026] In Example 6, the thickness of the AlO film 22 on the outermost surface was set to 5 nm, and the ZnO film 21 and the AlO film 22 were both set to 40 nm and laminated once. In this case, the number of layers was 3, and the hydrogen permeability coefficient was 6.6×10 -17In Example 7, the thickness of the AlO film 22 on the outermost surface was set to 5 nm, and the ZnO film 21 and the AlO film 22 were both set to 10 nm, and these were repeatedly stacked four times. In this case, the number of layers was 9, and the hydrogen permeability coefficient was 7.3×10 -17 In Example 8, the thickness of the AlO film 22 on the outermost surface was set to 5 nm, and the ZnO film 21 and the AlO film 22 were both set to 5 nm and repeatedly stacked eight times. In this case, the number of stacked layers was 17, and the hydrogen permeability coefficient was 6.8×10 -17 In Example 9, the thickness of the AlO film 22 on the outermost surface was set to 2 nm, and the ZnO film 21 and the AlO film 22 were both set to 2 nm and repeatedly stacked 20 times. In this case, the number of stacked layers was 41, and the hydrogen permeability coefficient was 4.7×10 -17 (mol / msPa).

[0027] Comparative Example 1 and Examples 1 to 3 all have a hydrogen permeability coefficient of 1.0 × 10 -16 (mol / msPa). In addition, in Comparative Example 2, the hydrogen permeability coefficient is 1.4×10 -15 (mol / msPa), which is a relatively high value.

[0028] The hydrogen permeability coefficient is a coefficient that indicates how much hydrogen permeates, and the lower the coefficient, the higher the hydrogen gas barrier function. Compared to Comparative Example 1, Examples 1 to 3 exhibit the same hydrogen gas barrier function. Also, compared to Comparative Example 2, Examples 1 to 3 exhibit higher hydrogen gas barrier function.

[0029] Moreover, in both Comparative Examples 4 and 5, the hydrogen permeability coefficient was smaller than that in Comparative Examples 1 and 2, and it can be said that they exhibited a high hydrogen gas barrier function.

[0030] On the other hand, when Comparative Examples 3 and 4 are compared with Examples 6 to 9, the hydrogen permeability coefficients of Examples 6 to 9 were smaller, and they demonstrated a high hydrogen gas barrier function.

[0031] When these results were analyzed, the relationship between the number of layers and the hydrogen permeability coefficient when the thickness of the substrate 10 was set to 1 mm and 0.3 mm was shown in Figures 4 and 5. For reference, the hydrogen permeability coefficient of Comparative Example 1 is also shown in Figure 4.

[0032] As shown in FIG. 4, in Comparative Example 1 in which a single layer of an AlO film 22 was formed on a substrate 10 having a thickness of 1 mm, the hydrogen permeability coefficient was 1.0×10 -16 (mol / msPa), but Examples 1 to 5 also had hydrogen permeability coefficients equal to or lower than that. In other words, when a single layer of the AlO film 22 was formed thickly on one surface 10a of the thick substrate 10, a relatively high hydrogen gas barrier function was obtained, but even when a laminated structure of the ZnO film 21 and the AlO film 22 was used, a hydrogen gas barrier function equal to or higher was obtained. Moreover, when a single layer of the ZnO film 21 was used as in Comparative Example 2, the hydrogen permeability coefficient was 1.4×10 -15 (mol / msPa), and Examples 1 to 5 had lower hydrogen permeability coefficients.

[0033] From these, it can be seen that the laminated structure of the ZnO film 21 and the AlO film 22 provides a hydrogen gas barrier function equal to or greater than that of the single layer of the AlO film 22, and higher than that of the single layer of the ZnO film 21. The ZnO film 21 and the AlO film 22 have a hydrogen gas barrier function, but a single layer cannot provide sufficient function if it is thin, so it is necessary to make the film thick, which requires a long manufacturing time. On the other hand, if the manufacturing time is shortened and the film thickness of the ZnO film 21 or the AlO film 22 becomes thin, a sufficient hydrogen gas barrier function cannot be obtained. In contrast, if the laminated structure of the ZnO film 21 and the AlO film 22 is used, it is possible to obtain a high hydrogen gas barrier function while making each layer thin.

[0034] In particular, when the number of layers was 41 or more, the hydrogen permeability coefficient could be further reduced compared to the case of a single layer of the AlO film 22, and a higher hydrogen gas barrier function could be obtained. It is considered that the thickness of each layer becomes thinner and the labyrinth effect becomes stronger, resulting in a higher hydrogen gas barrier function. However, although a high hydrogen gas barrier function can be obtained when the number of layers is 81, the thickness of each layer becomes thinner and the crystallinity of the ZnO film 21 begins to decrease, so in this experiment, the hydrogen permeability coefficient was smaller when the number of layers was 41.

[0035] 5, compared to Comparative Examples 3 and 4 in which a single layer of an AlO film 22 or a ZnO film 21 was formed on one surface 10a of a 0.3 mm film-like substrate 10, Examples 6 to 9 all had smaller hydrogen permeability coefficients. In particular, when the number of layers was 41, the hydrogen permeability coefficient could be reduced by one order of magnitude or more compared to the case in which a single layer of an AlO film 22 or a ZnO film 21 was formed, and a higher hydrogen gas barrier function could be obtained.

[0036] In this way, regardless of the thickness of the base material 10, the laminated structure of the ZnO film 21 and the AlO film 22 can provide a hydrogen gas barrier function that is equal to or better than that of a single layer of the AlO film 22 and is superior to that of a single layer of the ZnO film 21.

[0037] As described above, a hydrogen gas barrier function can be obtained by forming the hydrogen gas barrier film 20 from a laminated structure of the ZnO film 21 and the AlO film 22. Since the hydrogen gas barrier film 20 is formed not of a metal nitride film but of the ZnO film 21 and the AlO film 22, the stress of the hydrogen gas barrier film 20 can be reduced, and the occurrence of cracks in the film and peeling due to cracks can be suppressed. In particular, in the case of a hydrogen gas barrier film 20 for a thin substrate 10 such as a film having a thickness of 0.3 mm or less, the substrate 10 is largely stretched and deformed, and cracks are likely to occur in the film. However, the laminated structure of the ZnO film 21 and the AlO film 22 can suppress this.

[0038] Furthermore, when the hydrogen gas barrier film 20 is formed of a single layer of the ZnO film 21 or the AlO film 22, the film thickness must be increased, which requires a long manufacturing time and increases the manufacturing cost. In contrast, when the hydrogen gas barrier film 20 is formed as a laminated structure of the ZnO film 21 and the AlO film 22, the film thickness of each layer can be made thin, which shortens the manufacturing time and reduces the manufacturing cost.

[0039] In addition, since the hydrogen gas barrier film 20 is composed of the ZnO film 21 and the AlO film 22, rather than a metal nitride film, it is not necessary to use a high film formation temperature. Therefore, even if the substrate 10 is composed of a resin or the like that is insufficiently resistant to high temperatures, the substrate 10 is not deteriorated.

[0040] Furthermore, the hydrogen gas barrier function can be further improved by increasing the number of layers of the ZnO film 21 and the AlO film 22. In Examples 4, 5, and 9, the cases where the number of layers was 41 and 81 were shown, but according to the experimental results, a higher hydrogen gas barrier function can be obtained by increasing the number of layers to 40 or more.

[0041] (Other embodiments) Although the present disclosure has been described based on the above-described embodiment, it is not limited to the embodiment, and includes various modifications and modifications within the equivalent range. In addition, various combinations and forms, and other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure.

[0042] For example, the number of layers in the laminated structure of the ZnO film 21 and the AlO film 22 described in the first embodiment is merely an example, and other numbers of layers may be used. However, even in that case, it is preferable to set the total thickness of the hydrogen gas barrier film 20 to 100 nm or less, since this can suppress stress.

[0043] In the first embodiment, the ZnO film 21 and the AlO film 22 are repeatedly laminated to have the same thickness, but the ZnO film 21 and the AlO film 22 may have different thicknesses. Furthermore, the thicknesses of the multiple ZnO films 21 included in the laminated structure do not all need to be the same, and they may all have different thicknesses. Similarly, the thicknesses of the multiple AlO films 22 included in the laminated structure do not all need to be the same, and they may all have different thicknesses. [Explanation of symbols]

[0044] 10 Base material 10a one side 20 Hydrogen gas barrier film 21 ZnO film 22 AlO film

Claims

1. A substrate (10); a hydrogen gas barrier film (20) disposed on one surface of the substrate and composed of a laminated structure having a ZnO film (21) and an AlO film (22); The hydrogen gas barrier covering has

2. The hydrogen gas barrier coating according to claim 1 , wherein the ZnO film is a crystalline film.

3. 2. The hydrogen gas barrier coating according to claim 1, wherein the ZnO film and the AlO film are alternately and repeatedly laminated to form a layer count of 40 or more.

4. 2. The hydrogen gas barrier coating according to claim 1, wherein the hydrogen gas barrier film has a thickness of 100 nm or less.

5. The hydrogen gas barrier coating according to claim 1 , wherein the substrate has a thickness of 0.3 mm or less.

6. 6. The hydrogen gas barrier covering according to claim 1, wherein the substrate is made of polyamide.

Citation Information

Patent Citations

  • Thin-film transistor and display device

    JP2010016163A

  • Method for forming a thin film sealing layer

    JP2010541159A

  • Semiconductor device and charge control system

    JP2020087540A

  • Gas barrier polyamide film

    JP2022038958A

  • Method and device for producing metal oxide thin film

    JP2022107413A

Cited By

  • Flow sensor and method of manufacturing a flow sensor