Semiconductor device and manufacturing method of the same

By structuring the drift region of silicon carbide-based IGBTs with low and high carbon vacancy density zones positioned deeper than the depletion layer edge, the device achieves reduced on-resistance and turn-off loss, addressing the trade-off challenge in silicon carbide-based IGBTs.

JP2024166743APending Publication Date: 2024-11-29HITACHI LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023083061
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

Smart Images

  • Figure 2024166743000001_ABST
    Figure 2024166743000001_ABST
Patent Text Reader

Abstract

To provide a technique capable of improving a trade-off relation between a reduction of ON-resistance and a reduction of turn off loss.SOLUTION: It is assumed that a low-carbon pore density region 20 of which a carbon pore density is small is formed on an upper surface side of a drift region 4, and a high-carbon pore density region 30 of which the carbon pore density is large is formed on a lower surface side of the drift region 4. A position of an equivalent density line 100 that is an equivalent density line contained in a boundary region 40 between the low-carbon pore density region 20 and the high-carbon pore density region 30, and of which a carbon pore concentration corresponds to 1 / 2 of the carbon pore density of the high-carbon pore density region 30, is at a position that is deeper than an end part 200 of a depletion layer extending to the drift region 4 when an IGBT is turned off.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a manufacturing method thereof, and more particularly to a technique that is effective when applied to a semiconductor device having an insulated gate bipolar transistor and a manufacturing method thereof. [Background technology]

[0002] To reduce the energy consumption of power electronics devices, low-loss power semiconductor elements using wide-gap semiconductor materials such as silicon carbide (SiC), gallium nitride (GaN), and diamond are being researched. Silicon carbide and gallium nitride have a dielectric breakdown field strength about 10 times higher than that of silicon (Si), so for a power semiconductor element with the same breakdown voltage, the film thickness of the drift region can be reduced to one-tenth that of silicon. By thinning the drift region in this way, the resistance value in the drift region can be significantly reduced, and therefore the on-resistance of the entire element can be reduced.

[0003] Applications of wide-gap semiconductor materials include unipolar elements such as Schottky barrier diodes (SBDs) and power metal oxide field effect transistors (MOSFETs), as well as bipolar elements such as pn junction diodes and insulated gate bipolar transistors (IGBTs). In particular, bipolar elements using silicon carbide are expected to achieve low conduction losses in ultra-high voltage applications exceeding 6.5 kV.

[0004] In silicon carbide, the minority carrier lifetime in the material in the final growth state of the epitaxial crystal layer (as-grown state, as-grown means as-grown) is significantly shorter than that of silicon. Therefore, in order to improve the conductivity modulation effect in bipolar elements and reduce the resistance during on-operation, a process for increasing the minority carrier lifetime in the drift region is carried out during element manufacturing. On the other hand, if the minority carrier lifetime in the entire drift region is long, more residual carriers are discharged during the turn-off operation when the element switches from the on state to the off state, resulting in large turn-off losses. Therefore, by using a "local lifetime control structure" in which only the minority carrier lifetime on the collector side of the drift region is locally short, it is possible to reduce the on-voltage and turn-off losses.

[0005] Patent Document 1 describes an element in which the edge of a depletion layer formed in a drift region upon application of an operating voltage is located within a region with a short minority carrier lifetime.

[0006] Furthermore, Patent Document 2 describes a method for forming a region for extending the minority carrier lifetime inside a silicon carbide epitaxial layer, in which the depth to which the carrier lifetime extension region reaches from the injection surface of the silicon carbide epitaxial layer is arbitrarily changed by changing the annealing temperature or annealing time of annealing for diffusing and activating carbon atoms ion-implanted into the silicon carbide epitaxial layer, thereby making the thickness of the region thicker than other regions of the epitaxial layer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 3622405 [Patent Document 2] Patent Publication No. 2021-19157 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the above-mentioned Patent Document 1, there is a region in the depletion layer where the minority carrier lifetime is short. Since there are no residual carriers in the depletion layer, even if the minority carrier lifetime of the depletion layer is short, it does not affect the suppression of turn-on loss, but on the other hand, it causes an increase in on-resistance, which causes a deterioration of the trade-off relationship between on-resistance and turn-off loss.

[0009] Furthermore, since the above-mentioned Patent Document 2 does not disclose anything about the relationship between the carrier lifetime extension region and the depletion layer, there is a possibility that this will cause a deterioration in the trade-off relationship between on-resistance and turn-off loss, similar to the above-mentioned Patent Document 1.

[0010] In view of the above problems, an object of the present invention is to provide a technique capable of improving the trade-off relationship between reduced on-resistance and reduced turn-off loss. [Means for solving the problem]

[0011] A semiconductor device according to an embodiment includes an insulated gate bipolar transistor having a drift region of a first conductivity type, the drift region including silicon carbide as a constituent material. Here, the drift region includes a first region having a first carbon vacancy density, a second region having a second carbon vacancy density higher than the first density, and a boundary region sandwiched between the first region and the second region and having a higher carbon vacancy density than the first region and a lower carbon vacancy density than the second region. In this case, a position of an isopycnic line included in the boundary region, where the isopycnic line corresponds to a carbon vacancy concentration that is half the second density, is located deeper than an end of a depletion layer extending to the drift region when the insulated gate bipolar transistor is turned off.

[0012] In one embodiment, a method for manufacturing a semiconductor device includes an insulated gate bipolar transistor in which an end of a depletion layer that extends when the transistor is turned off remains inside a drift region. Here, the method for manufacturing a semiconductor device includes the steps of: (a) forming a drift region of a first conductivity type containing silicon carbide as a constituent material; (b) introducing carbon atoms into an upper surface of the drift region; and (c) diffusing the carbon atoms into the drift region.

[0013] Then, after the step (c), the drift region has a first region having a carbon vacancy density of a first density, a second region having a carbon vacancy density of a second density higher than the first density, and a boundary region sandwiched between the first region and the second region and having a carbon vacancy density higher than that of the first region and lower than that of the second region. At this time, the position of the isopycnal included in the boundary region, which corresponds to a carbon vacancy concentration that is half the second density, is deeper than the end of the depletion layer that extends when the semiconductor device is turned off. Effect of the Invention

[0014] According to one embodiment, it is possible to achieve an improvement in achieving both a reduction in the on-voltage and a reduction in the turn-off loss, which are in a trade-off relationship with each other. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 illustrates an active cell of an IGBT according to an embodiment. [Diagram 2] 1A to 1C are diagrams illustrating a manufacturing process of a semiconductor device according to an embodiment. [Diagram 3] 3 is a diagram showing a manufacturing process of the semiconductor device subsequent to FIG. 2; [Figure 4] 4 is a diagram showing a manufacturing process of the semiconductor device subsequent to FIG. 3. [Diagram 5] 5 is a diagram showing a manufacturing process of the semiconductor device subsequent to FIG. 4. [Figure 6] 6 is a diagram showing a manufacturing process of the semiconductor device subsequent to FIG. 5. [Figure 7]7 is a diagram showing a manufacturing process of the semiconductor device subsequent to FIG. 6. [Figure 8] FIG. 13 is a diagram showing a modified example of the manufacturing method. [Figure 9] 13 is a graph showing the results of a simulation of the changes in current and voltage over time at turn-off when the lifetime of minority carriers in a high carbon vacancy density region, which is a "localized lifetime control structure," is changed. [Figure 10] FIG. 13 is a diagram showing a first structural modification example. [Figure 11] FIG. 13 is a diagram showing a second structural modification example. [Figure 12] FIG. 13 is a diagram showing a third structural modification example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In all the drawings for explaining the embodiments, the same members are generally designated by the same reference numerals, and the repeated explanations thereof will be omitted. In addition, hatching may be applied even to plan views in order to make the drawings easier to understand.

[0017] In this embodiment, a semiconductor device including an insulated gate bipolar transistor having an n-type channel structure in which the drift region and the emitter region are composed of n-type semiconductor regions and the body region is composed of a p-type semiconductor region will be described as an example. However, it goes without saying that the technical idea of ​​this embodiment can also be applied to an insulated gate bipolar transistor having a p-type channel structure with the conductivity type reversed.

[0018] <Study by the present inventor> In an insulated gate bipolar transistor (hereinafter sometimes referred to as IGBT), when a gate voltage equal to or higher than the threshold voltage is applied to the gate electrode to turn on the IGBT, holes, which are minority carriers, are injected from the collector region to the drift region. As a result, electrons, which are majority carriers, are injected from the emitter region to the drift region, as if they are attracted to the injected holes. As a result, a conductivity modulation phenomenon occurs in the drift region, reducing the on-resistance of the IGBT.

[0019] On the other hand, when an IGBT is turned from on to off by applying a gate voltage smaller than the threshold voltage to the gate electrode, the IGBT turns off after all the electrons and holes injected into the drift region are swept out of the drift region. In other words, when an IGBT turns off, all the electrons and holes injected into the drift region must be swept out of the drift region, and the tail current caused by this sweeping flows before the IGBT turns off.

[0020] In an IGBT that operates in this way, the longer the lifetime of the minority carrier holes, the lower the on-resistance can be. This is because if the lifetime of the holes injected into the drift region is long, the number of holes that can attract electrons can be increased, and as a result, the number of electrons attracted to the drift region increases, thereby reducing the on-resistance. Therefore, in order to reduce the on-resistance of the IGBT, it is desirable to extend the lifetime of the holes.

[0021] On the other hand, when the IGBT is turned off, turn-off loss occurs. The cause of this turn-off loss is the tail current. Therefore, in order to reduce the turn-off loss, it is necessary to reduce the tail current. This tail current is a current that occurs when all the electrons and holes injected into the drift region are swept out of the drift region, and the shorter the hole lifetime, the more the tail current can be reduced. This is because if the hole lifetime is short, more holes will disappear before being swept out of the drift region, and as a result, the number of holes swept out of the drift region will decrease, which means that the tail current will be reduced.

[0022] From the above, in an IGBT, the longer the lifetime of holes, the more the on-resistance can be reduced, while the shorter the lifetime of holes, the more the turn-off loss can be reduced. That is, in an IGBT, the reduction in on-resistance and the reduction in turn-off loss are in a trade-off relationship. Therefore, the present inventor is studying an improvement to achieve both the reduction in on-resistance and the reduction in turn-off loss, which are in a trade-off relationship.

[0023] For example, the drift region can be formed by using an epitaxial growth method, but it is known that in IGBTs that use silicon carbide as a constituent material, the lifetime of holes in the "as-grown" drift region is significantly shorter than in IGBTs that use silicon as a constituent material. Therefore, if the "as-grown" drift region is used as is, the short lifetime of the holes reduces turn-off loss, but increases on-resistance. For this reason, it is not desirable to use the "as-grown" drift region as is in IGBTs that use silicon carbide as a constituent material.

[0024] In this regard, carbon vacancies exist in drift regions that use silicon carbide as a constituent material. These carbon vacancies function as trap levels that capture holes. For this reason, in drift regions with a high carbon vacancy density, the number of trap levels that capture holes increases, and the lifetime of holes becomes shorter. In other words, in drift regions with a low carbon vacancy density, the number of trap levels that capture holes decreases, and the lifetime of holes becomes longer.

[0025] In view of the above, it is conceivable to introduce carbon into the drift region in the "as-grown state" to fill the carbon vacancies with the introduced carbon. In this case, it is possible to reduce the carbon vacancies that function as trap levels that capture holes, and as a result, it is possible to extend the lifetime of the holes. That is, the present inventor is considering extending the lifetime of the holes by introducing carbon into the drift region. This is because if the lifetime of the holes can be extended, the on-resistance of the IGBT can be reduced.

[0026] However, doping carbon throughout the entire drift region increases the lifetime of holes throughout the drift region, leading to increased turn-off loss. Therefore, in order to balance the trade-off between reduced on-resistance and reduced turn-off loss, it is important to determine the depth to which carbon is doped into the drift region.

[0027] In other words, on the premise that a low carbon vacancy density region in which the carbon vacancy density is reduced by introducing carbon and a high carbon vacancy density region in which the carbon vacancy density is increased by maintaining the “as-grown state” without introducing carbon are provided in the drift region, it is important to determine the position (depth) of the boundary region between the low carbon vacancy density region and the high carbon vacancy density region.

[0028] In this regard, the present inventors have discovered, as a novel finding, that in specifying the depth of the above-mentioned boundary region, in order to achieve an improvement toward achieving both a reduction in on-resistance and a reduction in turn-off loss, which are in a trade-off relationship with each other, it is important to specify the relationship with the end of the depletion layer that extends into the drift region when the IGBT is turned off.

[0029] For example, consider a case where the depth of the above-mentioned boundary region is shallower than the end of the depletion layer that extends to the drift region when the IGBT is turned off. In this case, the low carbon vacancy density region becomes narrow, which is disadvantageous in terms of reducing the on-resistance. On the other hand, inside the depletion layer, the residual carriers are swept out by the electric field in the depletion layer and do not exist. For this reason, even if there is a high carbon vacancy density region in the depletion layer where the hole lifetime is short, the presence of this high carbon vacancy density region in the depletion layer does not affect the improvement of the turn-off loss.

[0030] In other words, from the viewpoint of achieving improvements toward achieving both reduced on-resistance and reduced turn-off loss, which are in a trade-off relationship with each other, a configuration in which the depth of the boundary region is located at a position shallower than the edge of the depletion layer cannot be said to be appropriate.

[0031] In this embodiment, therefore, in order to improve the balance between the reduction in on-resistance and the reduction in turn-off loss, which are in a trade-off relationship, a device is devised to appropriately define the depth of the boundary region between the low carbon vacancy density region and the high carbon vacancy density region in relation to the edge of the depletion layer. The technical concept of this device in the present embodiment is described below.

[0032] <Basic Concept of the Embodiment> The basic idea of ​​the present embodiment is based on the premise that, in an IGBT using silicon carbide as a constituent material, a low carbon vacancy density region in which carbon is introduced to reduce the carbon vacancy density and a high carbon vacancy density region in which carbon is not introduced and the "as-grown state" is maintained to increase the carbon vacancy density are provided in the drift region. The basic idea is that the position of the boundary region between the low carbon vacancy density region and the high carbon vacancy density region is located deeper than the end of the depletion layer that extends to the drift region when the IGBT is turned off.

[0033] According to this basic concept, the thickness of the low carbon vacancy density region where holes have a long lifetime can be increased, thereby reducing the on-resistance of the IGBT. On the other hand, according to the basic concept, the high carbon vacancy density region where holes have a short lifetime is provided below the depletion layer, so that the turn-off loss caused by the tail current can be reduced by adjusting the thickness of the high carbon vacancy density region. That is, according to the basic concept, by providing the boundary region at a position deeper than the edge of the depletion layer, it is possible to improve both the on-resistance and the turn-off loss, which are in a trade-off relationship with each other. The following describes an embodiment that embodies the basic concept.

[0034] <Embodiment> <<Configuration of Semiconductor Device>> FIG. 1 is a cross-sectional view that illustrates a schematic diagram of an active cell of an "n-channel SiC-IGBT" (hereinafter sometimes abbreviated as IGBT) included in a semiconductor device in an embodiment.

[0035] In FIG. 1, the IGBT has an n-type drift region 4 containing n-type impurities (donors) such as nitrogen and phosphorus, and the drift region 4 contains silicon carbide as a main component material. This drift region 4 has, for example, a buffer region 3a and a low-concentration drift region 3b, and the buffer region 3a is formed below the low-concentration drift region 3b. That is, the drift region 4 has the low-concentration drift region 3b and the buffer region 3a located below the low-concentration drift region 3b, in contact with the low-concentration drift region 3b, and having a higher impurity concentration than the low-concentration drift region 3b. The buffer region 3a is not necessarily required, but is provided to improve the withstand voltage of the IGBT and suppress conduction loss (reduce the on-resistance of the IGBT).

[0036] The lower layer of the buffer region 3a is p + A p-type collector region 2 is provided. + A collector electrode 1 is provided under the collector region 2. + The collector region 2 is made of a p-type semiconductor region containing p-type impurities such as aluminum or boron.

[0037] Next, a body region 5, which is a p-type semiconductor region containing aluminum, boron, etc., is formed inside the low-concentration drift region 3b, and an n-type semiconductor region containing nitrogen, phosphorus, etc. is formed inside the body region 5. + A type emitter region 6 is formed in the body region 5. In the contact opening of the body region 5, a body contact region 7 having an impurity concentration higher than that of the body region 5 is formed.

[0038] Next, n + A gate insulating film 8 is formed so as to cover the n-type emitter region 6, the body region 5 and the low-concentration drift region 3b, and a gate electrode 9 is provided so as to cover the gate insulating film 8. + An emitter electrode 10 is provided so as to cover the type emitter region 6 and the body contact region 7, and an interlayer insulating film 11 is formed to insulate the gate electrode 9 from the emitter electrode 10.

[0039] In the IGBT configured in this manner, the drift region 4 contains silicon carbide as a main constituent material, and as a result, carbon vacancies are inevitably present. In the drift region 4 in the embodied embodiment, the above-mentioned carbon vacancy density has an intentional distribution.

[0040] In other words, the drift region 4 in the embodied embodiment has a low carbon vacancy density region 20 having a first carbon vacancy density, a high carbon vacancy density region 30 having a second carbon vacancy density higher than the first density, and a boundary region 40 sandwiched between the low carbon vacancy density region 20 and the high carbon vacancy density region 30, and having a carbon vacancy density higher than that of the low carbon vacancy density region 20 and a carbon vacancy density lower than that of the high carbon vacancy density region 30. For example, the first density is 1×10 13 / cm 3 The second density is smaller than 1×10 13 / cm 3 That's all.

[0041] In this embodiment, the low carbon vacancy density region 20 is provided in the low concentration drift region 3b. Meanwhile, the high carbon vacancy density region 30 is provided in a part of the low concentration drift region 3b and in the buffer region 3a. The position of the isopycnal 100, which is included in the boundary region 40 and corresponds to a carbon vacancy concentration that is half the second density, is located deeper than the end 200 of the depletion layer that extends to the drift region 4 when the IGBT is turned off. In this embodiment, the isopycnal 100 exists in the low concentration drift region 3b, and the end 200 of the depletion layer also exists in the low concentration drift region 3b.

[0042] For example, the graph on the right side of FIG. 1 shows the distribution of the carbon vacancy density in the depth direction (dotted line) contained in the drift region 4 and the distribution of the electric field in the depth direction (dashed line) generated in the drift region 4 when the IGBT is turned off with a power supply voltage applied between the collector electrode 1 and the emitter electrode 10. From the graph on the right side of FIG. 1, a low carbon vacancy density region 20 having a low carbon vacancy density extends from the upper surface side of the drift region 4. A high carbon vacancy density region 30 having a high carbon vacancy density is formed below the low carbon vacancy density region 20 with a boundary region 40 sandwiched therebetween. At this time, in the boundary region 40, an isodenescence line 100 where the carbon vacancy density is half the carbon vacancy density of the high carbon vacancy density region 30 exists at a position deeper than an end 200 of the depletion layer where the electric field generated in the drift region 4 becomes "0".

[0043] The carbon vacancies function as trap levels that capture minority carriers (holes). Therefore, the lifetime of minority carriers in the low carbon vacancy density region 20, where the carbon vacancy density is low, is longer than the lifetime of minority carriers in the high carbon vacancy density region 30, where the carbon vacancy density is high. Thus, the semiconductor device in the embodied mode has an IGBT in which the drift region 4 is configured to include regions with different minority carrier lifetimes.

[0044] <<Method of manufacturing semiconductor device>> Next, a method for manufacturing a semiconductor device according to an embodiment will be described. First, as shown in FIG 2, an n-type bulk substrate 12 made of silicon carbide is prepared. Then, p + A collector region 2, a buffer region 3a and a low concentration drift region 3b are grown in this order.

[0045] Here, p + The impurity concentration of the collector region 2 is, for example, 1×10 18 / cm 3 The impurity concentration of the buffer region 3a is higher than that of the low-concentration drift region 3b. The impurity concentration of the low-concentration drift region 3b is, for example, 5×1015 / cm 3 The temperature in the epitaxial growth method is, for example, 1700° C. or higher, and p + The carbon vacancy density in each of the collector region 2, the buffer region 3a, and the low-concentration drift region 3b is 1×10 13 / cm 3 The epitaxial growth is performed so that the thickness of the low-concentration drift region 3b is about 50 μm to 100 μm when the withstand voltage of the IGBT is 6.5 kV class, for example. Also, when the withstand voltage of the IGBT is 20 kV class, for example, the thickness of the low-concentration drift region 3b is about 180 μm to 250 μm.

[0046] 3, carbon atoms are ion-implanted from the upper surface of the low-concentration drift region 3b. The implantation amount of carbon atoms is, for example, 1×10 15 / cm 2 That is all. Thereafter, as shown in Fig. 4, the carbon atoms are diffused into the low-concentration drift region 3b by heat treatment. This allows carbon atoms to fill the carbon vacancies present in the region from the top surface of the low-concentration drift region 3b to a predetermined depth, thereby reducing the carbon vacancy density in that region. The temperature of the heat treatment (annealing temperature) at this time is, for example, 1300°C or higher, and the heat treatment time is, for example, 60 minutes or longer.

[0047] In this manner, as shown in Fig. 4, in the embodied embodiment, a low carbon vacancy density region 20 having a carbon vacancy density of a first density, a high carbon vacancy density region 30 having a carbon vacancy density of a second density higher than the first density, and a boundary region 40 sandwiched between the low carbon vacancy density region 20 and the high carbon vacancy density region 30 and having a carbon vacancy density higher than that of the low carbon vacancy density region 20 and a carbon vacancy density lower than that of the high carbon vacancy density region 30 are formed. Note that Fig. 4 illustrates, for example, an isopycnic line 100 included in the boundary region 40, in which the carbon vacancy concentration corresponds to a density half the second density.

[0048] Next, as shown in FIG. 5, the body region 5 and n + The emitter region 6 and the body contact region 7 are formed by, for example, an ion implantation method using a photoresist as a patterning mask. The impurity concentration of the body region 5 is, for example, 2×10 16 / cm 3 From 2 × 10 18 / cm 3 n + The dopant concentration of each of the emitter region 6 and the body contact region 7 is, for example, 1×10 19 / cm 3 The conductive impurities are implanted at a high concentration so as to satisfy the above conditions. After a protective film made of, for example, carbon is formed on the surface, heat treatment is performed at, for example, 1700° C. to 1900° C. to activate the conductive impurities introduced by ion implantation.

[0049] Next, for example, the protective film is removed by oxygen plasma treatment or the like, and then the gate insulating film 8 is formed on the low-concentration drift region 3b by, for example, forming a silicon oxide film by wet oxidation, dry oxidation, or CVD (Chemical Vapor Deposition).

[0050] Next, the gate electrode 9 is formed by forming a gate insulating film 8, and then forming a polysilicon film directly thereon by the CVD method, or by forming an amorphous silicon film by the CVD method and then modifying the amorphous silicon film into a polysilicon film by heat treatment. Then, an interlayer insulating film 11 made of a silicon oxide film is formed by the CVD method, and then a contact portion is opened in the interlayer insulating film 11 by using, for example, a dry etching method. As a result, at the bottom of the contact portion, n + The type emitter region 6 and the body contact region 7 are exposed from the interlayer insulating film 11 .

[0051] Thereafter, the emitter electrode 10 made of a metal film such as aluminum, titanium, or nickel is formed by using, for example, a sputtering method or a metal vapor deposition method. A part of the emitter electrode 10 is embedded in the contact portion. The emitter electrode 10 is an n + The gate electrode 1 is electrically connected to the gate emitter region 6 and the body contact region 7 .

[0052] Before forming the emitter electrode 10, the n-type semiconductor layer exposed at the bottom of the contact portion + A silicide layer may be formed to cover the upper surfaces of the type emitter region 6 and the body contact region 7. The silicide layer can be formed by using, for example, a salicide technique.

[0053] Next, as shown in FIG. 6, the bulk substrate 12 is removed by a grinding process, so that p + The bottom surface of the p-type collector region 2 is exposed. + A semiconductor substrate consisting of a type collector region 2, a buffer region 3a and a low-concentration drift region 3b can be obtained.

[0054] Note that, although an example has been described here in which device structures such as gate electrode 9 on a semiconductor substrate are formed and then bulk substrate 12 is removed, if drift region 4 (epitaxial growth layer) on bulk substrate 12 has sufficient strength, bulk substrate 12 may be removed after drift region 4 is formed as shown in FIG. 2, and then device structures such as body region 5 and gate electrode 9 may be formed.

[0055] Next, as shown in Figure 7, + A collector electrode 1 is formed on the lower surface of the p-type collector region 2. The collector electrode 1 can be formed from a metal film such as aluminum, titanium, nickel, or gold by using, for example, a sputtering method or a metal vapor deposition method. + A silicide layer may be formed to cover the lower surface of the mold collector region 2. The silicide layer can be formed by, for example, a laser annealing technique. In this manner, the semiconductor device according to the embodied embodiment can be manufactured.

[0056] The manufacturing method of the semiconductor device in the embodied embodiment can be summarized as follows. That is, the manufacturing method of the semiconductor device in the embodied embodiment is a manufacturing method of a semiconductor device including an IGBT in which the end of the depletion layer that extends when turned off remains inside the drift region 4. In this case, the manufacturing method of the semiconductor device includes the steps of (a) forming an n-type drift region 4 containing silicon carbide as a constituent material, (b) introducing carbon atoms into the upper surface of the drift region 4, and (c) diffusing the carbon atoms into the drift region 4.

[0057] In a completed state of the semiconductor device after the step (c), the drift region 4 has a low carbon vacancy density region having a first carbon vacancy density, a high carbon vacancy density region having a second carbon vacancy density higher than the first density, and a boundary region sandwiched between the low carbon vacancy density region and the high carbon vacancy density region and having a higher carbon vacancy density than the low carbon vacancy density region and a lower carbon vacancy density than the high carbon vacancy density region. The position of the isopycnal included in the boundary region, which corresponds to a carbon vacancy concentration half the second density, is deeper than the end of the depletion layer extending when turned off.

[0058] <<Manufacturing variations>> Next, modified examples of the manufacturing method will be described. In this modification, as shown in FIG. + After the type collector region 2, the buffer region 3a, and the low-concentration drift region 3b are grown in order, a silicon oxide film 50 is formed by thermal oxidation as shown in Fig. 8. In this case, the silicon carbide on the upper surface side of the low-concentration drift region 3b is decomposed by the thermal oxidation process. As a result, the silicon generated by the decomposition forms the silicon oxide film 50 as silicon dioxide, while the carbon generated by the decomposition exists as atoms on the upper surface side of the low-concentration drift region 3b, as in Fig. 3 showing the embodiment.

[0059] At the same time, the carbon atoms are diffused by thermal oxidation, so that the carbon vacancies present in the region from the top surface of the low-concentration drift region 3b to a predetermined depth are filled with the carbon atoms. As a result, the carbon vacancy density in the region is reduced. The temperature of the thermal oxidation is, for example, 1300° C. or higher, and the time of the thermal oxidation is, for example, 60 minutes or longer.

[0060] Thereafter, the silicon oxide film 50 is removed using, for example, hydrofluoric acid, and then a device structure (element structure) is formed in the same manner as in the above-described embodiment.

[0061] In the method for manufacturing a semiconductor device according to this modification, the generation of carbon atoms and the filling of carbon vacancies by the diffusion of the carbon atoms can be performed in the same thermal oxidation step. Furthermore, since the step of removing the silicon oxide film 50 is performed as a step of cleaning the substrate surface in the embodied embodiment, the semiconductor device can be manufactured with a reduced number of steps according to this modification.

[0062] <<Features of the Realization>> Next, features of the embodiment will be described. A feature of the embodiment is that, for example, as shown in FIG. 1 , a low carbon vacancy density region 20 with a low carbon vacancy density is formed on the upper surface of the drift region 4, while a high carbon vacancy density region 30 with a high carbon vacancy density is formed on the lower surface of the drift region 4. The characteristic feature of the embodiment is that, assuming that a low carbon vacancy density region 20 with a low carbon vacancy density is formed on the upper surface of the drift region 4, a isopycnal 100 included in a boundary region 40 between the low carbon vacancy density region 20 and the high carbon vacancy density region 30, the isopycnal 100 having a carbon vacancy concentration that is half the carbon vacancy density of the high carbon vacancy density region 30, is located deeper than an end 200 of a depletion layer that extends into the drift region 4 when the IGBT is turned off.

[0063] Here, since carbon vacancies act as a factor shortening the lifetime of minority carriers in silicon carbide, the lifetime of minority carriers in low carbon vacancy density region 20, where the carbon vacancy density is low, is longer than that in high carbon vacancy density region 30, where the carbon vacancy density is high.

[0064] Therefore, the presence of the low-carbon vacancy density region 20 can reduce the on-resistance during IGBT operation. On the other hand, when the IGBT is turned off, there are no residual carriers in the depletion layer extending into the drift region 4, so as long as the low-carbon vacancy density region 20 is within the depletion layer, it does not affect the turn-off loss. As a result, according to the characteristic points in the embodiment, the trade-off relationship between the on-resistance (on-voltage) during IGBT operation and the turn-off loss during IGBT turn-off can be improved.

[0065] For example, the depth Wd (cm) of the depletion layer formed in the IGBT when a voltage is applied can be expressed by the following formula because the impurity concentration difference between the low-concentration drift region 3b and the body region 5 is large, and the built-in voltage generated in the pn junction of silicon carbide is much smaller than the power supply voltage. Wd = {(2·εs·Vcc) / (q·Nd)} 0.5

[0066] Here, the power supply voltage is Vcc (V), the impurity concentration of the low-concentration drift region 3b is Nd (1 / cm 3 ), the charge amount of electrons is q (C), and the dielectric constant of silicon carbide is εs (F / cm).

[0067] Therefore, when the thickness of the low-carbon vacancy density region 20 is W (cm) and the characteristic point (Wd < W) in the embodiment is combined with the above relational formula, the power supply voltage Vcc that realizes the characteristic point will satisfy the following conditions. Vcc < {(q·Nd) / (2·εs)}·W 2

[0068] In addition, the high-carbon vacancy density region 30 acts as a region with a short minority carrier lifetime called a "local lifetime control structure". That is, in the embodiment, the high-carbon vacancy density region 30 constitutes a "local lifetime control structure".

[0069] FIG. 9 is a graph showing the simulation results of the time variations in current and voltage at turn-off in each case where the lifetime of minority carriers in high carbon vacancy density region 30, which is the "local lifetime control structure", is changed.

[0070] When the lifetime of the minority carriers in the high carbon vacancy density region 30 is set to be the same as that in the low carbon vacancy density region 20, that is, when there is no “local lifetime control structure”, the collector current decreases with time, but the slope of the decrease becomes gentle midway, and a tail current is generated.

[0071] In contrast, when the lifetime of the minority carriers in the high carbon vacancy density region 30 is reduced, in the case of 5 μs shown by the dashed line, the waveform is almost the same as that in the case where the “local lifetime control structure” is not present. However, in the case of 2 μs shown by the dashed line and 0.5 μs shown by the dashed double-dotted line, it can be seen that the tail current is reduced.

[0072] In other words, by making the lifetime of minority carriers in the high carbon vacancy density region 30 about 2 μs or less, it is possible to obtain the effect of reducing the turn-off loss by the "local lifetime control structure". 13 / cm 3 In this regard, since the carbon vacancy density of the high carbon vacancy density region 30 is the same as the carbon vacancy density of the epitaxial growth layer in the as-grown state, the carbon vacancy density during epitaxial growth is 1×10 13 / cm 3 By growing in the above manner, a "localized lifetime controlled structure" in the embodied embodiment can be realized.

[0073] In the embodiment, silicon carbide is used as the semiconductor material. In this case, carbon vacancies, which act as a factor in reducing the lifetime of minority carriers, form a "deep level" of 0.63 eV from the conduction band of silicon carbide. This is deeper than the level formed by crystal defects, which act as a factor in reducing the lifetime of minority carriers in silicon. Therefore, according to the embodiment, the "local lifetime control structure" can be maintained even at higher temperatures to reduce turn-off loss. IGBTs are power switching elements, and are used by passing large currents through them. Therefore, the IGBTs become hot when they are in operation. Therefore, by using silicon carbide as the semiconductor material, the effect of the "local lifetime control structure" can be obtained even at high temperatures, and an IGBT with a wider operating range can be obtained.

[0074] As described above, according to the features of the embodiment, it is possible to improve the trade-off between the reduction in on-resistance and the reduction in turn-off loss. In particular, by using silicon carbide as the semiconductor material, the effect of improving the trade-off can be obtained even at high temperatures.

[0075] <<Structural variation 1>> Next, the first modified example will be described. FIG. 10 is a cross-sectional view showing an active cell of an IGBT in the first modification. The IGBT in this modified example 1 differs from the IGBT in the above-described embodiment in that, as shown in FIG. 10 , in this modified example 1, the position of an isopycnal 100, which corresponds to a carbon vacancy concentration that is half the carbon vacancy density of the high carbon vacancy density region 30, is located inside the buffer region 3a, and an end 200 of the depletion layer is also located inside the buffer region 3a.

[0076] Such a device structure is realized by diffusing the carbon atoms deeper in the heat treatment (annealing) performed after implanting carbon atoms as shown in FIG. 4 during the manufacturing process of the IGBT in the embodied embodiment by increasing the heat treatment temperature and heat treatment time compared to the embodied embodiment.

[0077] In this first modification, as shown in FIG. 10, the drift region 4 has a low-concentration drift region 3b and a buffer region 3a that is located below the low-concentration drift region 3b, is in contact with the low-concentration drift region 3b, and has a higher impurity concentration than the low-concentration drift region 3b.

[0078] In this case, in this modified example 1, the low carbon vacancy density region 20 is provided in a part of the buffer region 3a and the low concentration drift region 3b, the high carbon vacancy density region 30 is provided in the buffer region 3a, the isodensity line 100 exists in the buffer region 3a, and the end 200 of the depletion layer also exists in the buffer region 3a.

[0079] In the IGBT configured in this manner, when the IGBT is turned off, the gradient of the electric field in the depth direction generated in the drift region 4 between the collector electrode 1 and the emitter electrode 10 becomes steep in the buffer region 3a having a high impurity concentration, and the spread of the depletion layer can be suppressed even if the power supply voltage is increased. Therefore, even if the power supply voltage is increased, the position of the isodensity line 100 can be made greater than the depth of the end 200 of the depletion layer. Therefore, according to this modification 1, the trade-off between reduced on-resistance and reduced turn-off loss can be improved in a power supply voltage range greater than the power supply voltage range in the embodiment.

[0080] <<Structural variation 2>> Next, the second modified example will be described. FIG. 11 is a cross-sectional view showing an active cell of an IGBT in the second modification. The IGBT in this modification 2 differs from the IGBT in the above-mentioned embodiment in that a high-concentration drift region 3c having a higher impurity concentration than the low-concentration drift region 3b and a lower impurity concentration than the buffer region 3a is provided between the low-concentration drift region 3b and the buffer region 3a. Another difference is that, as shown in Fig. 11, in this modification 2, the position of an isopycnal 100 corresponding to a carbon vacancy concentration that is half the carbon vacancy density of the high carbon vacancy density region 30 is located inside the high-concentration drift region 3c, and an end 200 of the depletion layer is also located inside the high-concentration drift region 3c.

[0081] Such a device structure can be realized by increasing the amount of impurity doping source gas supplied for a predetermined initial period when forming the low-concentration drift region 3b using the epitaxial growth method shown in Fig. 2 during the manufacturing process of the IGBT in the embodied embodiment. Alternatively, the high-concentration drift region 3c may be grown after the buffer region 3a is formed, and then the low-concentration drift region 3b may be formed. Furthermore, if the drift region 4 on the bulk substrate 12 has sufficient strength, it is possible to form the p + After the collector region 2, the buffer region 3a, and the low-concentration drift region 3b are formed in this order, the bulk substrate 12 is removed, and then the p + Alternatively, high-concentration drift region 3c may be formed by ion-implanting n-type impurities (donors) such as nitrogen or phosphorus from the lower surface side (rear surface side) of collector region 2.

[0082] In this second modification, as shown in FIG. 11 , the drift region 4 has a low-concentration drift region 3b, a high-concentration drift region 3c located below the low-concentration drift region 3b, in contact with the low-concentration drift region 3b and having a higher impurity concentration than the low-concentration drift region 3b, and a buffer region 3a located below the high-concentration drift region 3c, in contact with the high-concentration drift region 3c, and having a higher impurity concentration than the high-concentration drift region 3c.

[0083] In this case, in this second modification, the low carbon vacancy density region 20 is provided in a part of the high concentration drift region 3c and in the low concentration drift region 3b, the high carbon vacancy density region 30 is provided in a part of the high concentration drift region 3c and in the buffer region 3a, the isodensity line 100 exists in the high concentration drift region 3c, and the end 200 of the depletion layer also exists in the high concentration drift region 3c.

[0084] In the IGBT configured in this way, when the IGBT is turned off, the gradient of the electric field in the depth direction generated in the drift region 4 between the collector electrode 1 and the emitter electrode 10 becomes steep in the high-concentration drift region 3c having a high impurity concentration, and the spread of the depletion layer can be suppressed even if the power supply voltage is increased. Therefore, even if the power supply voltage is increased, the position of the isodensity line 100 can be made greater than the depth of the end 200 of the depletion layer. Therefore, according to the present modification 2, the trade-off between reduced on-resistance and reduced turn-off loss can be improved in a power supply voltage range greater than the power supply voltage range in the embodiment.

[0085] In addition, since the impurity concentration of the high-concentration drift region 3c is smaller than that of the buffer region 3a, the gradient of the electric field in the depletion layer is gentler than that of the IGBT in the above-described modification 1. Therefore, the gradient of the time change in the voltage applied between the collector electrode 1 and the emitter electrode 10 after the depletion layer reaches the high-concentration drift region 3c when the IGBT is turned off can be made gentler than that of the IGBT in modification 1. As a result, modification 2 has the advantage of being able to suppress the generation of noise and the like due to the time change in the voltage.

[0086] <<Structural variation 3>> Next, the third modified example will be described. FIG. 12 is a cross-sectional view showing an active cell in the third modification. The IGBT in this modified example 3 differs from the IGBT in the above-described embodiment in that the gate electrode 9 in this modified example 3 has a trench structure. +A trench 15 is formed penetrating the n-type emitter region 6 and the body region 5. + A gate insulating film 8 is formed so as to cover the type emitter region 6 and the trench 15 , and a gate electrode 9 is provided so as to cover the gate insulating film 8 .

[0087] Such a device structure is realized by the IGBT manufacturing process in the embodiment, in which the body region 5, n + This can be achieved by forming the type emitter region 6 and the body contact region 7, activating the conductive impurities introduced by ion implantation, and then forming the trench 15 by, for example, dry etching.

[0088] In the IGBT of the present modification 3, the cell pitch can be reduced by the trench gate structure, and as a result, the channel density per unit area can be improved, and the on-resistance of the IGBT can be reduced. In addition, the crystal plane of the side surface of the trench 15 is used as the channel, and since silicon carbide has a large channel mobility on the side surface of the trench, the on-resistance can be further reduced by the synergistic effect with the reduction in the cell pitch.

[0089] The invention made by the inventor has been specifically described above based on the embodiment thereof. However, it goes without saying that the present invention is not limited to the above embodiment, and various modifications can be made without departing from the spirit of the invention. [Explanation of symbols]

[0090] 1 Collector electrode 2 p + Type Collector Region 3a Buffer Area 3b Low concentration drift region 3c High concentration drift region 4. Drift Region 5. Body Region 6n + Type emitter area 7 Body Contact Area 8 Gate insulating film 9 Gate electrode 10 Emitter electrode 11 Interlayer insulating film 12 Bulk Substrate 15. Trench 20 Low carbon vacancy density region 30 High carbon vacancy density region 40 Boundary area 50 Silicon oxide film 100 isopycnal lines 200 End

Claims

1. A semiconductor device including an insulated gate bipolar transistor, the insulated gate bipolar transistor has a drift region of a first conductivity type; the drift region includes silicon carbide as a constituent material; The drift region is a first region having a first density of carbon vacancies; a second region having a carbon vacancy density at a second density higher than the first density; a boundary region between the first region and the second region, the boundary region having a carbon vacancy density higher than that of the first region and a carbon vacancy density lower than that of the second region; having a position of an isopycnal included in the boundary region, the isopycnal corresponding to a carbon vacancy concentration that is half the second density, is located deeper than an end of a depletion layer that extends into the drift region when the insulated gate bipolar transistor is turned off.

2. 2. The semiconductor device according to claim 1, The second density is 1×10 13 / cm 3 That is all about the semiconductor device.

3. 2. The semiconductor device according to claim 1, A semiconductor device, wherein a lifetime of minority carriers in the first region is longer than a lifetime of minority carriers in the second region.

4. 2. The semiconductor device according to claim 1, The voltage applied between the collector and the emitter when the insulated gate bipolar transistor is turned off is Vcc (V), The thickness of the first region is W (cm), The impurity concentration of the first region is set to Nd (1 / cm 3 )year, The charge of the electron is q (C), When the dielectric constant of the first region is ε (F / cm), Vcc<{(q・Nd) / (2・εs)}・W 2 The semiconductor device according to the present invention satisfies the above relationship.

5. 2. The semiconductor device according to claim 1, The drift region is a low concentration drift region; a buffer region located below the low-concentration drift region, in contact with the low-concentration drift region, and having an impurity concentration higher than that of the low-concentration drift region; having the first region is provided in the low concentration drift region, the second region is provided in a part of the low concentration drift region and in the buffer region, the isopycnals are present within the low concentration drift region, an end of the depletion layer is present within the low-concentration drift region.

6. 2. The semiconductor device according to claim 1, The drift region is a low concentration drift region; a buffer region located below the low-concentration drift region, in contact with the low-concentration drift region, and having an impurity concentration higher than that of the low-concentration drift region; having the first region is provided in a part of the buffer region and the low concentration drift region, The second region is provided within the buffer region, the isopycnals lie within the buffer region; An end of the depletion layer is present within the buffer region.

7. 2. The semiconductor device according to claim 1, The drift region is a low concentration drift region; a high-concentration drift region located below the low-concentration drift region, in contact with the low-concentration drift region, and having an impurity concentration higher than that of the low-concentration drift region; a buffer region located below the high-concentration drift region, in contact with the high-concentration drift region, and having an impurity concentration higher than that of the high-concentration drift region; having the first region is provided in a part of the high concentration drift region and in the low concentration drift region, the second region is provided in a part of the high concentration drift region and in the buffer region, the isopycnals are present within the high concentration drift region, an end of the depletion layer is present within the high-concentration drift region.

8. 2. The semiconductor device according to claim 1, The semiconductor device, wherein the insulated gate bipolar transistor is a trench gate insulated gate bipolar transistor.

9. A method for manufacturing a semiconductor device including an insulated gate bipolar transistor in which an end of a depletion layer extending when turned off remains within a drift region, comprising the steps of: (a) forming a drift region of a first conductivity type containing silicon carbide as a constituent material; (b) introducing carbon atoms into an upper surface of the drift region; (c) diffusing the carbon atoms into the drift region; Equipped with After the step (c), The drift region is a first region having a first density of carbon vacancies; a second region having a carbon vacancy density at a second density higher than the first density; a boundary region between the first region and the second region, the boundary region having a carbon vacancy density higher than that of the first region and a carbon vacancy density lower than that of the second region; having a position of an isopycnal included in the boundary region, the isopycnal corresponding to a carbon vacancy concentration that is half the second density, is located deeper than an end of the depletion layer that extends when the semiconductor device is turned off.

10. 10. The method of manufacturing a semiconductor device according to claim 9, In the step (b), the carbon atoms are ion-implanted.

11. 10. The method of manufacturing a semiconductor device according to claim 9, The method for manufacturing a semiconductor device, wherein the steps (b) and (c) are performed by a thermal oxidation step.

12. 10. The method of manufacturing a semiconductor device according to claim 9, The drift region formed in the step (a) has a carbon vacancy density of 1×10 13 (1 / cm 3 ) The method for manufacturing a semiconductor device.

Citation Information

Patent Citations

  • Silicon carbide semiconductor device and manufacturing method of silicon carbide semiconductor device

    JP2021019157A

  • Semiconductor switching elements and igbt modules

    JP3622405B2