Ethylene-vinyl alcoholic copolymer composition, melt-molding material, and melt-molded product

JP2024166853APending Publication Date: 2024-11-29MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023083236
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Benefits of technology

【0011】 本発明のEVOH樹脂組成物は、溶融成形加工性に優れ、高湿度下でのガスバリア性に優れる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166853000001
    Figure 2024166853000001
Patent Text Reader

Abstract

To provide an EVOH resin composition with superior melting moldability and superior gas barrier properties under high humidity.SOLUTION: An ethylene-vinyl alcoholic copolymer composition contains an ethylene-vinyl alcoholic copolymer (A) with an ethylene structural unit content of 20-60 mol% and a hydrotalcite thermal decomposition product (B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ethylene-vinyl alcohol copolymer (hereinafter, sometimes referred to as "EVOH resin") composition, a melt-molding material, and a melt-molded product. [Background technology]

[0002] Ethylene-vinyl alcohol copolymers (hereinafter sometimes referred to as "EVOH resins") are excellent in transparency, gas barrier properties such as oxygen and other gases, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and are formed into films, sheets, bottles, etc., and are widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and agricultural chemical packaging materials.

[0003] However, because EVOH resin has relatively active hydroxyl groups in its molecules, its gas barrier properties tend to deteriorate in high humidity environments, and there is a demand for improvements in its thermal stability, such as by increasing the decomposition temperature when heated during melt molding.

[0004] In response to the above problems, for example, Patent Document 1 discloses a resin composition containing EVOH resin and polyolefin and hydrotalcite as a halogen scavenger, for the purpose of improving gas barrier properties, chemical resistance, and flexibility.

[0005] Furthermore, Patent Document 2 discloses a gas barrier composition obtained by coating or immersing a composition in which a compound having two or more hydroxyl groups in the molecule and a portion of a polyvalent carboxylic acid are crosslinked with an aqueous dispersion of a hydrotalcite compound in order to improve hot water resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-88666 A [Patent Document 2] JP 2005-146267 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in Patent Document 1, hydrotalcite has a problem in melt molding processability because foaming occurs due to dehydration of interlayer water caused by the relatively high processing temperatures of EVOH resin and polyolefin. Furthermore, Patent Document 2 discloses a coating treatment or immersion treatment using an aqueous dispersion, but it is known that the pyrolyzed hydrotalcite reverts to hydrotalcite when it is made into an aqueous dispersion, and in addition, the film is formed using an aqueous dispersion, which results in poor productivity.

[0008] Under such circumstances, an object of the present invention is to provide an EVOH resin composition which has excellent melt moldability and excellent gas barrier properties under high humidity conditions. [Means for solving the problem]

[0009] In view of these circumstances, the present inventors have discovered that by incorporating a hydrotalcite pyrolysate (B) into an EVOH resin (A), the film-forming properties during melt molding are excellent and the gas barrier properties under high humidity conditions can be improved.

[0010] That is, the present invention has the following aspects. [1] An ethylene-vinyl alcohol copolymer composition comprising (A) an ethylene-vinyl alcohol copolymer having an ethylene structural unit content of 20 to 60 mol % and (B) a thermally decomposed product of hydrotalcite. [2] The ethylene-vinyl alcohol copolymer composition according to [1], wherein the content of the thermal decomposition product of hydrotalcite (B) is 0.7 to 12 mass % based on the ethylene-vinyl alcohol copolymer composition. [3] A melt molding material comprising the ethylene-vinyl alcohol copolymer composition according to [1] or [2]. [4] The melt-molded material described in [3], which was allowed to stand in an environment of 20°C and 90% RH for 2 weeks and had a peak derived from hydrotalcite at 2θ = 9 to 13° when measured by wide-angle X-ray diffraction using CuKα radiation. [5] A melt-molded article comprising the melt-molded material described in [3]. [Advantages of the Invention]

[0011] The EVOH resin composition of the present invention is excellent in melt-molding processability and gas barrier properties under high humidity conditions.

[0012] In addition, the melt-molded material comprising the resin composition of the present invention is excellent in molding processability because foaming due to dehydration of the interlayer water of hydrotalcite does not occur during heating such as during melt-kneading or melt-molding. Therefore, it can be suitably used, for example, as a molding material for various molded articles obtained via melt-molding, such as packaging materials for foods, pharmaceuticals, agricultural chemicals, etc., particularly liquid packaging materials. [Modes for Carrying Out the Invention]

[0013] Hereinafter, the present invention will be described in more detail based on embodiments of the present invention, but the present invention is not limited to these embodiments. In the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it means "X or more and Y or less", and also includes the meaning of "preferably greater than X" or "preferably less than Y". In addition, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably less than Y". In the present invention, "x and / or y" (x and y are arbitrary configurations or components) means three combinations: only x, only y, and x and y.

[0014] [EVOH Resin Composition] An EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains an EVOH resin (A) and a specific hydrotalcite pyrolysate (B). Each component will be described below.

[0015] [EVOH resin (A)] The EVOH resin (A) used in the present invention is usually a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.

[0016] As the vinyl ester monomer, vinyl acetate is typically used because of its good market availability and efficiency in treating impurities during production. Examples of vinyl ester monomers other than vinyl acetate include aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate, and generally, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms are used. These are generally used alone, but multiple types may be used simultaneously as necessary.

[0017] The polymerization method for copolymerizing the ethylene and the vinyl ester monomer can be any known polymerization method, such as solution polymerization, suspension polymerization, emulsion polymerization, etc., but solution polymerization using methanol as a solvent is generally used. The saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method. The EVOH resin (A) thus produced is composed mainly of structural units derived from ethylene and vinyl alcohol structural units, and also contains a small amount of vinyl ester structural units which remain unsaponified.

[0018] The content of the ethylene structural unit in the EVOH resin (A) is 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. The content of the ethylene structural unit can be controlled by the ethylene pressure when the vinyl ester monomer and ethylene are copolymerized. If the content is too low, the gas barrier property and melt moldability under high humidity tend to decrease, and conversely, if the content is too high, the gas barrier property tends to decrease. The content of the ethylene structural unit can be measured based on ISO14663.

[0019] The saponification degree of the EVOH resin (A) is usually 90 to 100 mol%, preferably 95 to 100 mol%, particularly preferably 99 to 100 mol%. The saponification degree can be controlled by the amount, temperature, time, etc. of a saponification catalyst (usually an alkaline catalyst such as sodium hydroxide is used) used when saponifying an ethylene-vinyl ester copolymer, and if the saponification degree is too low, the gas barrier property, heat stability, moisture resistance, etc. tend to decrease. The degree of saponification of the EVOH resin (A) can be measured based on JIS K6726 (wherein the EVOH resin is used as a solution uniformly dissolved in a water / methanol solvent).

[0020] The melt flow rate (MFR) (210°C, load 2160g) of the EVOH resin (A) is usually 0.5 to 100g / 10min, preferably 1 to 50g / 10min, and particularly preferably 3 to 35g / 10min. If the MFR is too high, the stability during film formation tends to be impaired, whereas if it is too low, the viscosity tends to be too high, making melt extrusion difficult. The MFR is an index of the polymerization degree of the EVOH resin (A), and can be adjusted by the amount of the polymerization initiator and the amount of the solvent used when copolymerizing ethylene with a vinyl ester monomer.

[0021] The melting point of the EVOH resin (A) is usually 240° C. or lower, preferably 170 to 230° C., and particularly preferably 180 to 220° C. If the melting point is too high, the EVOH resin tends to be easily decomposed during molding, whereas if the melting point is too low, extrusion moldability tends to be unstable. The melting point of the EVOH resin (A) can be measured, for example, using a differential scanning calorimeter, based on the melting peak temperature determined in accordance with the method of measuring the melting temperature after a certain heat treatment as specified in JIS K7121.

[0022] In addition, the EVOH resin (A) may further contain structural units derived from the comonomers shown below (for example, 10 mol % or less of the EVOH resin (A)) within a range that does not impair the effects of the present invention. Examples of the comonomer include olefins such as propylene, 1-butene, and isobutene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 3-butene-1,2-diol, 4-penten-1-ol, and 5-hexene-1,2-diol, and derivatives thereof such as esters and acylation products; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyloxy-2-methylenepropane; hydroxyalkylvinylidene diacetates such as hydroxyalkyl-2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, or their salts or mono- or dialkyl esters having an alkyl group with 1 to 18 carbon atoms; acrylamide, N-alkylacrylamide having an alkyl group with 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its acid salts or its quaternary salts. acrylamides such as methacrylamide, N-alkyl methacrylamides having an alkyl group with 1 to 18 carbon atoms, N,N-dimethyl methacrylamide, 2-methacrylamidopropanesulfonic acid or its salt, methacrylamidepropyldimethylamine or its acid salt or its quaternary salt; N-vinyl amides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; alkyl vinyl ethers having an alkyl group with 1 to 18 carbon atoms, hydrochloride, etc. vinyl ethers such as alkoxyalkyl vinyl ether and alkoxyalkyl vinyl ether; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; and comonomers such as trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride and acrylamido-2-methylpropanesulfonic acid.These can be used alone or in combination of two or more.

[0023] Among them, hydroxyl group-containing α-olefins are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the hydroxyl group-containing α-olefins are copolymerized, the resulting EVOH resin has a primary hydroxyl group in the side chain. Such an EVOH resin having a primary hydroxyl group in the side chain, particularly an EVOH resin having a 1,2-diol structure in the side chain, is preferred in that it has good secondary moldability while maintaining gas barrier properties.

[0024] When the EVOH resin (A) used in the present invention has a primary hydroxyl group in a side chain, the content of the structural unit derived from the monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, particularly preferably 1 to 10 mol % of the EVOH resin (A).

[0025] As the EVOH resin (A), there can also be used an EVOH resin that has been "post-modified" by esterification, urethanization, acetalization, cyanoethylation, oxyalkylenation, or the like.

[0026] When the post-modified EVOH resin is used, the modification rate is usually 10 mol% or less, and preferably 4 mol% or less. If the modification rate of the EVOH resin used is too high, the resin tends to be easily thermally deteriorated and the long-run property tends to be reduced.

[0027] Furthermore, the EVOH resin (A) may be a mixture of EVOH resins having different contents of ethylene structural units, degrees of saponification, degrees of polymerization, copolymerization components, and the like.

[0028] [Hydrotalcite pyrolysate (B)] Hydrotalcite pyrolysis product (B) is Mg 1-x Al x O 1+x / 2 and is obtained by calcining hydrotalcite (for example, at 500 to 700° C. for 1 to 3 hours).

[0029] Such hydrotalcite is a compound represented by the following general formula (1), and these can be used alone or in combination of two or more kinds. [Formula] 〔M 2+ 1-x M 3+ x (OH)2〕 x+ 〔A n- x / n ·mH2O〕 x ···(1)

[0030] In the above formula (1), M 2+ : Mg 2+ , Mn 2+ , Fe 2+ , Co 2+ , Ni 2+ , Cu 2+ , Zn 2+ and other divalent metals. M 3+ : Al 3+ , Fe 3+ , Cr 3+ , Co 3+ , In 3+ and other trivalent metals. A n- : OH - , F - , Cl - , Br - , NO3 - , CO3 2- , SO4 2- , Fe(CN)6 3- , CH3COO - and n-valent anions such as oxalate ion and salicylate ion. x is in the range of 0 < x ≦ 0.33.

[0031] Specific hydrotalcite represented by the above formula (1) includes Mg4Al2(OH) 12 CO3·3H2O (x = 0.33), Mg 4.5 Al2(OH) 13 CO3·3.5H2O (x = 0.3), Mg6Al2(OH) 16CO3·4H2O(x=0.25), etc.

[0032] Specifically, when the hydrotalcite pyrolysate (B) is measured by wide-angle X-ray diffraction (XRD) using CuKα radiation, peaks derived from the hydrotalcite pyrolysate (B) are observed at around 43° (e.g., 40 to 46°) and around 64° (e.g., 60 to 67°). The wide-angle X-ray diffraction of the hydrotalcite pyrolysate (B) can be measured under the measurement conditions described below.

[0033] The content of the hydrotalcite pyrolysate (B) is preferably 0.7 to 12 mass% based on the EVOH resin composition, more preferably 0.9 to 11.5 mass%, further preferably 1.2 to 11 mass%, particularly preferably 2 to 10.5 mass%, and particularly preferably 2.5 to 10 mass%. If the content is too low, the effect of improving the gas barrier property under high humidity tends to be poor, and if the content is too high, the EVOH resin tends to decompose.

[0034] [Other thermoplastic resins] In addition to the EVOH resin (A) and the hydrotalcite pyrolysate (B), the present EVOH resin composition may further contain other thermoplastic resins as resin components within a range that does not impair the effects of the present invention (for example, usually 30 mass % or less of the present EVOH resin composition, preferably 20 mass % or less, and particularly preferably 10 mass % or less).

[0035] As the other thermoplastic resin, known thermoplastic resins can be used, such as polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more kinds.

[0036] [Other compounding agents] The EVOH resin composition may contain additives that are generally added to EVOH resins, provided that the effects of the present invention are not impaired. Examples of the additives include plasticizers (e.g., aliphatic polyhydric alcohols such as ethylene glycol, glycerin, and hexanediol), oxygen absorbers (e.g., inorganic oxygen absorbers such as aluminum powder and potassium sulfite; polyhydric phenols such as ascorbic acid, its fatty acid esters and metal salts, gallic acid, and hydroxyl-containing phenol aldehyde resins; terpene compounds; blends of tertiary hydrogen-containing resins and transition metals (e.g., a combination of polypropylene and cobalt); blends of carbon-carbon unsaturated bond-containing resins and transition metals. Polymer-based oxygen absorbers such as compounds (e.g., a combination of polybutadiene and cobalt), photooxidative decomposition resins (e.g., polyketones), anthraquinone polymers (e.g., polyvinyl anthraquinone), and compounds of these to which photoinitiators (e.g., benzophenone) or antioxidants or deodorants (e.g., activated carbon) other than those mentioned above have been added, heat stabilizers, light stabilizers, ultraviolet absorbers, colorants, antistatic agents, surfactants (excluding those used as lubricants), antibacterial agents, antiblocking agents, and fillers (e.g., inorganic fillers) may also be added. These compounds may be used alone or in combination of two or more.

[0037] [Method of manufacturing EVOH resin composition] The EVOH resin composition is produced using the essential components EVOH resin (A) and hydrotalcite pyrolysate (B), and the optional components as required. Examples of the production method include known methods such as a dry blend method, a melt mixing method, and a master batch method. Among these, it is preferable to produce the composition by including a step of melt mixing the composition raw material containing the EVOH resin (A) and the hydrotalcite pyrolysate (B). These production methods can also be arbitrarily combined.

[0038] The dry blending method may, for example, be (I) a method in which pellets containing an EVOH resin (A) and a thermally decomposed product of hydrotalcite (B) are dry blended using a tumbler or the like.

[0039] Examples of the melt mixing method include (II) a method in which a dry blend of pellets containing an EVOH resin (A) and a hydrotalcite pyrolysate (B) is melt-kneaded to obtain pellets or other molded products, and (III) a method in which a hydrotalcite pyrolysate (B) is added to a molten EVOH resin (A) using a powder microfeeder or the like, and the mixture is melt-kneaded to obtain pellets or other molded products.

[0040] In addition, in each of the above-mentioned methods, it is also possible to obtain a resin composition of the desired concentration by first blending the EVOH resin (A) and the hydrotalcite pyrolysate (B) in a predetermined ratio to prepare a composition (master batch) having a high concentration of the hydrotalcite pyrolysate (B), and then blending this composition (master batch) with the EVOH resin (A).

[0041] In addition, since the thermally decomposed hydrotalcite (B) easily reacts with water and / or anions and acids to return to the original hydrotalcite, it is preferable to avoid blending using an aqueous dispersion of the thermally decomposed hydrotalcite (B).

[0042] Furthermore, in the present invention, it is possible to combine the above-mentioned different methods. Among them, the melt mixing method is preferred, and method (III) is particularly preferred, in terms of productivity and the fact that a resin composition having the effect of the present invention is obtained.

[0043] The pellets of the resin composition obtained by each of the above methods and the pellets containing the EVOH resin (A) and the hydrotalcite pyrolysate (B) used in each of the above methods may have any shape, and may be any shape, such as a sphere, an oval, a cylinder, a cube, or a rectangular parallelepiped. The shape of the pellets is usually oval or cylindrical, and the size of the pellets is usually 1 to 6 mm, preferably 2 to 5 mm, in the case of a cylinder, from the viewpoint of convenience when used later as a molding material, and the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm. In the case of an oval shape, the major axis is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. The minor axis is usually 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm. A method for measuring the major and minor axes includes, for example, picking up a pellet, observing it, measuring the major axis using a measuring instrument such as a vernier caliper, and then visually and tactilely determining the position of the cross section perpendicular to the major axis that has the largest area, and measuring the minor axis of this cross section in the same manner.

[0044] When the present EVOH resin composition is in the form of pellets, it is preferable to attach a known lubricant to the surface of the pellets in order to stabilize the feedability during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, etc.; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, etc.; bis-higher fatty acid amides such as ethylene bis-stearic acid amide, ethylene bis-oleic acid amide, ethylene bis-erucic acid amide, ethylene bis-lauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylenes having a molecular weight of about 500 to 10,000, low molecular weight polypropylenes, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated ethylene resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the EVOH resin composition. The lower limit is usually 0% by mass.

[0045] The present EVOH resin composition thus obtained has improved gas barrier properties under high humidity conditions, and when the system not containing the hydrotalcite pyrolyzate (B) is taken as 1 (standard), the improvement is preferably 1% or more, more preferably 1.5% or more, even more preferably 5% or more, and particularly preferably 10% or more. The upper limit is usually 12%. The improvement rate of the gas barrier property can be measured using, for example, the method described in the Examples below.

[0046] The EVOH resin composition is prepared in various forms, such as pellets, powder, liquid, etc., and is provided as a molding material for various molded products. In particular, in the present invention, when it is provided as a melt molding material, the effects of the present invention tend to be more efficiently obtained, which is preferable. The present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin (A) and the hydrotalcite pyrolysate (B) used in the present EVOH resin composition.

[0047] Examples of the molded product include melt molded products and single layer films molded from the present EVOH resin composition, as well as multilayer structures having a layer made of the present EVOH resin composition.

[0048] A melt molding material according to one embodiment of the present invention contains the EVOH resin composition, and the melt molding material and a melt molded product made of the melt molding material have excellent gas barrier properties, particularly oxygen barrier properties, under high humidity. The melt molding material and the melt molded product are preferably left to stand for 2 weeks in an environment of 20°C and 90% RH, and when measured by wide-angle X-ray diffraction using CuKα radiation, they have a peak derived from hydrotalcite at 2θ=9 to 13°.

[0049] In the present invention, the moisture of a molten molding material containing an EVOH resin (A) and a hydrotalcite pyrolysate (B) and a molten molded product (e.g., a film) is adjusted, whereby the hydrotalcite pyrolysate (B) changes in the EVOH resin (A) to form hydrotalcite. Further aging causes an interaction between the EVOH resin (A) and the hydrotalcite. It is presumed that the gas barrier properties (particularly the oxygen barrier properties) under high humidity conditions are improved due to the interaction between the EVOH resin (A) and the hydrotalcite and the oxygen labyrinth effect inherent to the hydrotalcite.

[0050] The wide-angle X-ray diffraction is measured under the following conditions. [Measurement conditions] Equipment used: D8 DISCOVER (manufactured by Bruker Japan) Detector: 2D detector VANTEC-500 (manufactured by Bruker Japan) Voltage: 50kV ·Current: 100mA Camera length: 100mm ·Measurement method: Reflection method Accumulation time: 20 minutes Wavelength: CuKα radiation (Kα1 and Kα2 are not separated) Detector position: 2θ=0, 35, 60° ·X-ray incident angle: θ=0.3° · Conditions for one-dimensionalization in the 2θ direction: 2θ=0~59° or 0~84°, azimuth angle (chi)=-110~-70°

[0051] As a sample to be used for the wide-angle X-ray diffraction, the EVOH resin composition in the form of a film described below may be used as it is. When the film of the EVOH resin composition is laminated with another substrate, if the EVOH resin composition layer can be peeled off, the EVOH resin composition layer is peeled off and measurement is performed, and if the EVOH resin composition layer cannot be peeled off, the measurement may be performed while the film is laminated with the other substrate. At the time of measurement, the thickness of the peeled EVOH resin composition layer (film) is preferably 30 μm or more, and if the film is not thick enough, a film may be laminated.

[0052] [Multilayer structure] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the multilayer structure") includes a layer made of the present EVOH resin composition. The layer made of the present EVOH resin composition (hereinafter simply referred to as "the present EVOH resin composition layer") can be laminated with another substrate (hereinafter, the resin used in the substrate may be abbreviated as "substrate resin") mainly composed of a thermoplastic resin other than the present EVOH resin composition to impart further strength, protect the present EVOH resin composition layer from the effects of moisture, etc., or impart other functions.

[0053] Examples of the base resin include polyethylene-based resins such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-propylene (block and random) copolymers, and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; polypropylene-based resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; (unmodified) polyolefin-based resins such as polybutene, polypentene, and polycyclic olefin-based resins (polymers having a cyclic olefin structure in at least one of the main chain and side chain); and polyolefins obtained by treating with unsaturated carboxylic acids or Examples of the polyolefin resin include a broad definition of modified olefin resin, such as unsaturated carboxylic acid modified polyolefin resin graft-modified with the ester, ionomer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, polyester resin, polyamide resin (including copolymerized polyamide), polyvinyl chloride, polyvinylidene chloride, acrylic resin, polystyrene resin, vinyl ester resin, polyester elastomer, polyurethane elastomer, polystyrene elastomer, halogenated polyolefin such as chlorinated polyethylene and chlorinated polypropylene, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0054] Of these, hydrophobic resins such as polyamide-based resins, polyolefin-based resins, polyester-based resins, and polystyrene-based resins are preferred, and more preferred are polyolefin-based resins such as polyethylene-based resins, polypropylene-based resins, polycyclic olefin-based resins, and unsaturated carboxylic acid-modified polyolefin-based resins thereof. In particular, polycyclic olefin-based resins are preferably used as hydrophobic resins.

[0055] The layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc., where a is the EVOH resin composition layer and b is the base resin layer. In addition, when R is a recycled layer containing a mixture of the EVOH resin composition and a thermoplastic resin other than the EVOH resin composition, obtained by remelting and molding the ends or defective products generated in the process of manufacturing the multilayer structure, b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The total number of layers of the multilayer structure is usually 2 to 15, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the respective layers, if necessary.

[0056] The adhesive resin may be a known one, and may be appropriately selected according to the type of thermoplastic resin used in the base resin layer "b". A representative example is a modified polyolefin polymer containing a carboxy group obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin by addition reaction, graft reaction, or the like. Examples of the modified polyolefin polymer containing a carboxy group include maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted ethylene-propylene (block and random) copolymer, maleic anhydride grafted ethylene-ethyl acrylate copolymer, maleic anhydride grafted ethylene-vinyl acetate copolymer, maleic anhydride modified polycyclic olefin resin, maleic anhydride grafted polyolefin resin, etc. These may be used alone or in combination of two or more.

[0057] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layers are located on both sides of the present EVOH resin composition layer, it is preferable to use an adhesive resin with excellent hydrophobicity.

[0058] The base resin and adhesive resin may contain conventionally known plasticizers, fillers, clays (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, waxes, etc., within the range that does not impair the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less, based on the total resin). These may be used alone or in combination of two or more kinds.

[0059] The lamination of the present EVOH resin composition layer and the substrate resin layer (including the case where an adhesive resin layer is interposed) can be performed by a known method. For example, a method of melt extrusion laminating a substrate resin to a film, sheet, etc. of the present EVOH resin composition, a method of melt extrusion laminating the present EVOH resin composition to a substrate resin layer, a method of co-extruding the present EVOH resin composition and a substrate resin, a method of dry laminating the present EVOH resin composition (layer) and a substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on a substrate resin and then removing the solvent, etc. Among these, in consideration of cost and environmental aspects, the present EVOH resin composition can be produced by providing a step of melt molding the present EVOH resin composition layer. Specifically, the co-extrusion method is preferred.

[0060] The multilayer structure may be subjected to a (heat) stretching treatment as necessary. The stretching treatment may be either uniaxial stretching or biaxial stretching, and in the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. As the stretching method, a method with a high stretch ratio among roll stretching, tenter stretching, tubular stretching, stretch blowing, vacuum pressure molding, etc. may be used. The stretching temperature is a temperature near the melting point of the multilayer structure, and is usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. If the stretching temperature is too low, the stretchability becomes poor, and if it is too high, it becomes difficult to maintain a stable stretched state.

[0061] The multilayer structure after the stretching treatment may be heat-set for the purpose of imparting dimensional stability. Heat setting can be performed by a known means, for example, the multilayer structure after the stretching treatment is heat-treated usually at 80 to 180°C, preferably 100 to 165°C, for usually about 2 to 600 seconds while being kept in a tensioned state.

[0062] When the stretched multilayer structure is to be used as a shrink film, in order to impart heat shrinkability, the above-mentioned heat setting may be omitted, and instead, a treatment such as cooling and setting the multilayer structure after stretching by applying cold air thereto may be carried out.

[0063] The thickness of the present multilayer structure (including the stretched one), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, cannot be generally stated depending on the layer structure, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., but the thickness of the present multilayer structure (including the stretched one) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0064] Furthermore, the thickness ratio of the present EVOH resin composition layer to the base resin layer in the present multilayer structure (present EVOH resin composition layer / base resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, when there are multiple layers of each, and the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, when there are multiple layers of each ...

[0065] It is also possible to obtain cup- or tray-shaped multilayer containers using this multilayer structure. In this case, a squeeze molding method is usually used, specifically vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. Furthermore, when a tube- or bottle-shaped multilayer container (laminate structure) is obtained from a multilayer parison (a hollow tubular preform before blowing), a blow molding method is used. Specifically, extrusion blow molding (double-head type, mold moving type, parison shift type, rotary type, accumulator type, horizontal parison type, etc.), cold parison type blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding in-line type biaxial stretch blow molding, etc.) are mentioned. The resulting laminate may be subjected to processes such as heat treatment, cooling, rolling, printing, dry lamination, solution or melt coating, bag making, deep drawing, box processing, tube processing, and splitting, as required.

[0066] Bags made of films, sheets, and stretched films obtained using this multilayer structure, as well as containers and lids made of cups, trays, tubes, bottles, etc., are useful as various packaging materials and containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, medicines, etc. In particular, since a layer made of this EVOH resin composition has flexibility and is inhibited from discoloring, this EVOH resin composition and this multilayer structure are particularly useful as liquid packaging materials for water, foods, medicines, agricultural chemicals, etc. (for example, bags for bag-in-boxes and inner bags for pouch dispensers, etc.). EXAMPLES

[0067] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples in any way.

[0068] Prior to the examples, the following components were prepared:

[0069] [EVOH] EVOH (A1): Ethylene content 25 mol%, melting point 195°C, saponification degree 99.7 mol%, MFR 4.0 [g / 10 min] (210°C, load 2160 g) EVOH (A2): Ethylene content 9 mol%, melting point 213°C, saponification degree 98.0 mol%, MFR 130 [g / 10 min] (210°C, load 2160 g)

[0070] [Hydrotalcite pyrolysate] Hydrotalcite pyrolysis product (B1): Mg6Al2(OH) 16 CO3·4H2O was heated in a muffle furnace at 500℃ for 2 hours to produce the pyrolysis product Mg6Al2O9. (In addition, in the XRD measurement, the peak at around 2θ=11° originating from between the layers of hydrotalcite disappeared upon heating, and peaks originating from the thermal decomposition product of hydrotalcite at around 2θ=43° and 63° were observed, confirming the generation of the thermal decomposition product of hydrotalcite.)

[0071] <Example 1> EVOH (A1) with an ethylene content of 25 mol% and hydrotalcite pyrolyzate (B1) were dry-blended so that (B1) was 1 mass% relative to the total resin composition to obtain a mixture. The mixture was then fed to a twin-screw extruder (20 mmφ) equipped with a two-hole die, extruded under the following extrusion conditions, and the strands were solidified by blowing air onto them, and cut to obtain pellets of the EVOH resin composition.

[0072] [Extrusion conditions] ·Extruder setting temperature (℃): C1 / C2 / C3 / C4 / C5 / C6 =150 / 200 / 210 / 210 / 210 / 210 Screw speed: 200 rpm

[0073] <Examples 2 to 4> Pellets of an EVOH resin composition were obtained in the same manner as in Example 1, except that the content of the hydrotalcite pyrolysate (B1) in Example 1 was changed as shown in Table 1, and the hydrotalcite pyrolysate (B1) was added using a powder trace feeder.

[0074] <Comparative Example 1> Pellets of an EVOH resin composition were obtained in the same manner as in Example 1, except that the thermal decomposition product of hydrotalcite (B1) was not used.

[0075] <Comparative Example 2> Pellets of an EVOH resin composition were obtained in the same manner as in Example 1, except that EVOH (A2) was used instead of EVOH (A1).

[0076] [Preparation of melt-extruded monolayer film] The pellets of the EVOH resin compositions obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were extruded under the following conditions to obtain melt-extruded monolayer films, which were then left to stand for 2 weeks in an environment of 20°C and 90% RH and then used as gas barrier materials. The film formability and gas barrier property improvement rate of each melt-extruded film were determined by the following measurement methods. The results are shown in Table 1. (Film production conditions) Extruder: Brabender Plastograph EC-plus Screw: Single shaft, 20mmΦ, full flight Cylinder temperature setting: 190~210℃ Cooling roll temperature setting: 80℃ Film thickness: 20μm

[0077] [Film forming property] The appearance of the gas barrier material was visually observed and evaluated according to the following criteria. 〇 No foaming marks or holes ×: Items with foaming marks or holes

[0078] [Gas barrier improvement rate] The oxygen permeability of each of the obtained gas barrier materials (melt-extruded monolayer films) at 20°C and 90% RH was measured using an oxygen permeability measuring device (MOCON's "OXTRAN2 / 21"), and the measured value was converted to a value at a thickness of 20 μm to represent the gas barrier property. The converted oxygen permeability was applied to the following formula to calculate the gas barrier property improvement rate (%). [Formula] Gas barrier property improvement rate (%)=(1-[oxygen permeability of measurement sample (Examples 1 to 4)] / [oxygen permeability of system not containing hydrotalcite pyrolyzate (B) (Comparative Example 1)])×100

[0079] [Table 1]

[0080] As can be seen from Table 1, the EVOH resin compositions of Examples 1 to 4 containing a specific amount of the hydrotalcite pyrolysate (B) had excellent film-forming properties (melt molding processability), and had a higher improvement rate of gas barrier properties under high humidity conditions than the EVOH resin composition of Comparative Example 1 not containing the hydrotalcite pyrolysate (B). Moreover, the EVOH resin composition of Comparative Example 2, in which the content of ethylene structural units in EVOH was lower than the content specified in the present invention, was unable to be formed into a film because the MFR was too high. [Industrial Applicability]

[0081] Since the present EVOH resin composition is inhibited from thermal degradation during melt molding, it is useful as a packaging material for various foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc.

Claims

1. An ethylene-vinyl alcohol copolymer composition comprising (A) an ethylene-vinyl alcohol copolymer having an ethylene structural unit content of 20 to 60 mol % and (B) a thermally decomposed product of hydrotalcite.

2. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein the content of the hydrotalcite pyrolyzate (B) is 0.7 to 12 mass% based on the ethylene-vinyl alcohol copolymer composition.

3. A melt molding material comprising the ethylene-vinyl alcohol copolymer composition according to claim 1 or 2.

4. The melt molding material according to claim 3, wherein the melt molding material is left standing for 2 weeks in an environment of 20 ° C. and 90% RH, and when measured by wide-angle X-ray diffraction using CuKα radiation, the melt molding material has a peak derived from hydrotalcite at 2θ = 9 to 13 °.

5. A melt-molded product comprising the melt-molding material according to claim 3.

Citation Information

Patent Citations

  • Gas barrier composition and laminated material

    JP2005146267A

  • Resin composition containing ethylene-vinyl alcohol copolymer, laminate, and molded article

    JP2017088666A