Mixed paper having low linear expansion and manufacturing method thereof

A mixed paper with expanded graphite, aramid pulp, and carbon fiber, impregnated with a binder resin, addresses the challenge of achieving both high thermal conductivity and low linear expansion, ensuring dimensional stability for semiconductor components.

JP2024166867APending Publication Date: 2024-11-29AWA PAPER MFG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023083255
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing materials with high thermal conductivity often have a large coefficient of linear expansion, leading to potential issues with semiconductor components shifting due to thermal expansion, making it difficult to achieve both properties simultaneously.

Method used

A low linear expansion mixed paper composed of expanded graphite, aramid pulp, and carbon fiber, impregnated with a binder resin, which maintains thermal conductivity while suppressing linear expansion coefficients to 5 ppm/K or less and reducing directional differences.

Benefits of technology

The mixed paper achieves both high thermal conductivity (34 W/m·K or more) and low linear expansion (5 ppm/K or less) with minimal anisotropy, suitable for applications requiring dimensional stability during thermal cycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166867000001_ABST
    Figure 2024166867000001_ABST
Patent Text Reader

Abstract

To provide a mixed paper having low linear expansion with a suppressed linear expansion coefficient while maintaining thermal conductivity.SOLUTION: A mixed paper having low linear expansion includes an expanded graphite, an aramid pulp, a carbon fiber, and a binder resin. The mixed paper having low linear expansion has a linear expansion coefficient in its longitudinal direction and transverse direction at 30-200°C of 5 ppm / K or under, respectively, and a thermal conductivity of 34 W / m K or over. By this, a mixed paper having low linear expansion with a suppressed linear expansion coefficient can be achieved.SELECTED DRAWING: Figure 10
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a low linear expansion mixed paper and a manufacturing method thereof that can be used, for example, for heat dissipation sheets, and the like, and a manufacturing method thereof. [Background technology]

[0002] The power consumption of semiconductor components used in various electrical products has increased in recent years due to the demand for higher output, and the amount of heat generated is also increasing. Therefore, the boards on which semiconductor components are mounted and the sheet materials to which they are attached are required to have high thermal conductivity so as to quickly dissipate the generated heat and prevent the temperature of the board from rising.

[0003] On the other hand, if such sheet materials expand due to heat, it is possible that the mounted semiconductor components may become misaligned, causing malfunctions. For this reason, materials with a low linear expansion coefficient are required to prevent thermal expansion. However, many materials with high thermal conductivity, such as metals, have a high linear expansion coefficient, so it is not easy to achieve both. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7070819 [Patent Document 2] JP 2021-106202 A [Patent Document 3] JP 2020-12194 A [Patent Document 4] JP 2011-25297 A [Patent Document 5] JP 2011-21303 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present disclosure is to provide a low linear expansion mixed paper having a reduced linear expansion coefficient while maintaining thermal conductivity, and a method for producing the same.

[0006] A first embodiment of the low linear expansion mixed paper comprises expanded graphite, aramid pulp, carbon fiber, and a binder resin, and has a linear expansion coefficient of 5 ppm / K or less from 30°C to 200°C in both the longitudinal and transverse directions, and a thermal conductivity of 34 W / m K or more. With the above configuration, a low linear expansion mixed paper with a suppressed linear expansion coefficient can be realized.

[0007] In addition, according to the second embodiment of the low linear expansion mixed paper, the difference between the linear expansion coefficients of the low linear expansion mixed paper in the longitudinal and transverse directions from 30°C to 200°C is 0.5 ppm / K or less. With the above configuration, a low linear expansion mixed paper with a small difference in the linear expansion coefficients in the longitudinal and transverse directions can be obtained.

[0008] Further, according to the third embodiment of the low linear expansion mixed paper, in any of the above embodiments, the linear expansion coefficients of the low linear expansion mixed paper at 30°C to 200°C in both the longitudinal and transverse directions are 4 ppm / K or less, and the difference between the two is 0.2 ppm / K or less. With the above configuration, a low linear expansion mixed paper with a small difference in the longitudinal and transverse linear expansion coefficients can be obtained.

[0009] Furthermore, in the low linear expansion mixed paper according to a fourth embodiment, in any one of the above embodiments, the expanded graphite is in the form of powder.

[0010] Furthermore, in a fifth aspect of the low linear expansion mixed paper, in any one of the above aspects, the ratio of the aramid pulp to the expanded graphite is 0.10 to 0.30.

[0011] Furthermore, according to the sixth embodiment of the low linear expansion mixed paper, in any of the above embodiments, the thickness is 100 μm or more. With the above configuration, the low linear expansion mixed paper can be easily handled in the manufacturing process of products using the low linear expansion mixed paper.

[0012] Furthermore, in the low linear expansion mixed paper according to a seventh embodiment, in any one of the above embodiments, the resin coating amount of the binder resin is 14% to 33%.

[0013] Furthermore, according to the eighth embodiment of the low linear expansion mixed paper, in any of the above embodiments, the size is 1 m x 1 m or more. With the above configuration, it is possible to make the paper larger by utilizing a papermaking process that allows continuous production.

[0014] Furthermore, according to the ninth embodiment of the low linear expansion mixed paper, in any one of the above embodiments, the density is 1.5 g / cm 3 The following is the result.

[0015] Furthermore, according to a tenth embodiment of the low linear expansion mixed paper, in any one of the above embodiments, the binder resin is impregnated into a sheet material containing the expanded graphite, the aramid pulp, the carbon fiber, and the binder resin fiber.

[0016] Furthermore, according to the eleventh embodiment, the method for producing a low linear expansion mixed paper includes the steps of: mixing expanded graphite, aramid pulp, and carbon fiber to obtain a sheet material; impregnating the sheet material with a thermosetting resin as a binder resin; and hot-pressing the sheet material impregnated with the thermosetting resin to obtain a low linear expansion mixed paper having a linear expansion coefficient of 5 ppm / K or less in both the longitudinal and transverse directions at 30°C to 200°C and a thermal conductivity of 34 W / m·K or more. This makes it possible to obtain a low linear expansion mixed paper having dimensional stability and thermal conductivity by papermaking. In addition, it is possible to enjoy the advantage that a low linear expansion mixed paper having increased strength in multiple directions can be obtained by papermaking using carbon fiber scraps without using expensive carbon fiber cross material to compensate for the shortcomings of UD materials. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing how a display is constructed by arranging multiple substrates with LEDs attached thereto. [Diagram 2] FIG. 2A is a graph showing the amount of deformation in MD of the low linear expansion mixed paper according to Comparative Example 2, and FIG. 2B is a graph showing the amount of deformation in CD. [Diagram 3] FIG. 3A is a graph showing the amount of deformation in MD of the low linear expansion mixed paper according to Example 1, and FIG. 3B is a graph showing the amount of deformation in CD. [Figure 4] FIG. 4A is a graph showing the amount of deformation in MD of the low linear expansion mixed paper according to Example 2, and FIG. 4B is a graph showing the amount of deformation in CD. [Diagram 5] FIG. 5A is a graph showing the amount of deformation in MD of the low linear expansion mixed paper according to Example 3, and FIG. 5B is a graph showing the amount of deformation in CD. [Figure 6] FIG. 6A is a graph showing the amount of deformation in MD of the low linear expansion mixed paper according to Example 4, and FIG. 6B is a graph showing the amount of deformation in CD. [Figure 7] 1 is a graph showing the linear expansion coefficients at 30° C. to 50° C. of low linear expansion mixed papers according to Comparative Examples 1-2 and Examples 1-4. [Figure 8] 1 is a graph showing the linear expansion coefficients at 30° C. to 100° C. of low linear expansion mixed papers according to Comparative Examples 1-2 and Examples 1-4. [Figure 9] 1 is a graph showing the linear expansion coefficients at 30° C. to 150° C. of low linear expansion mixed papers according to Comparative Examples 1-2 and Examples 1-4. [Figure 10] 1 is a graph showing the linear expansion coefficients at 30° C. to 200° C. of low linear expansion mixed papers according to Comparative Examples 1-2 and Examples 1-4. [Figure 11] 1 is a graph showing the thermal conductivity of low linear expansion mixed papers according to Comparative Examples 1-2 and Examples 1-4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present disclosure will be described based on the drawings. However, the embodiments shown below are examples for embodying the technical ideas of the present disclosure, and the present disclosure is not limited to the following. In addition, this specification never specifies the members shown in the claims as the members of the embodiments. In particular, the dimensions, materials, shapes, and relative positions of the components described in the embodiments are not intended to limit the scope of the present disclosure to those, and are merely explanatory examples, unless otherwise specified. Note that the size and positional relationship of the members shown in each drawing may be exaggerated to clarify the explanation. Furthermore, in the following explanation, the same name and symbol indicate the same or similar members, and detailed explanation will be omitted as appropriate. Furthermore, each element constituting the present disclosure may be configured as a form in which multiple elements are composed of the same member and one member serves multiple elements, or conversely, the function of one member can be shared among multiple members.

[0019] Substrates and sheet materials with excellent heat dissipation and dimensional stability are required for applications such as fixing semiconductor components. For example, the substrate to which the LED elements of a micro LED display are attached is required to have dimensional stability with little fluctuation during thermal expansion in addition to thermal conductivity for heat dissipation. When constructing a micro LED display by laying out multiple substrates with micro LED elements 1 attached as shown in Figure 1, the substrate 10 expands and contracts due to heat generation during use, and gaps GP may occur between the substrates, resulting in a poor appearance.

[0020] Therefore, carbon fiber reinforced plastics (CFRP) using carbon fibers with negative linear expansion are mainly used. However, CFRP is generally a UD (Unidirectional) material, with carbon fibers aligned in one direction, so while it has excellent dimensional stability in the direction in which the carbon fibers are aligned, in the direction crossing this, the linear expansion of the binder resin becomes dominant, resulting in poor dimensional stability. As a result, it is necessary to use multiple sheets by changing the direction to the orthogonal direction, etc., and stacking them, which results in a problem of increased thickness.

[0021] In view of the above background, the present inventors have conducted extensive research into a substrate that combines dimensional stability and thermal conductivity, and have discovered that the use of expanded graphite makes it possible to achieve dimensional stability without directionality, thereby completing the present invention. [Embodiment 1]

[0022] The low linear expansion mixed paper according to the first embodiment is a sheet material made of expanded graphite, aramid pulp, and carbon fiber impregnated with a binder resin. The linear expansion coefficient can be suppressed by using aramid having negative linear expansion characteristics. Specifically, the linear expansion coefficients of the low linear expansion mixed paper at 30°C to 200°C in both the longitudinal and transverse directions are 5 ppm / K or less, preferably 4 ppm / K or less. In addition, the difference between the linear expansion coefficients at 30°C to 200°C in the longitudinal and transverse directions is preferably 0.5 ppm / K or less, more preferably 0.2 ppm / K or less. This makes it possible to obtain a low linear expansion mixed paper with reduced anisotropy.

[0023] In addition, by blending expanded graphite into the low linear expansion mixed paper, the thermal conductivity is increased to 34 W / m K or more, and preferably 40 W / m K or more.

[0024] The expanded graphite is preferably in the form of a powder or powder, which reduces the directional property of the expanded graphite and reduces the difference between the linear expansion coefficient in the longitudinal direction and the transverse direction, compared to fibrous or rod-like graphite.

[0025] The powdered expanded graphite has a larger particle size as long as a uniform mixed paper can be obtained, and the average particle size is preferably 100 to 500 μm, which provides the effect of achieving both thermal conductivity and a low linear expansion coefficient.

[0026] Furthermore, in addition to the expanded graphite, aramid pulp, and carbon fiber, the sheet material may contain binder resin fibers (one type or two or more types). Thermoplastic resins are preferably used as the binder resin fibers. Specifically, the binder resin fibers may be selected from the following: polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), and liquid crystal polyester; polyolefins such as polyethylene (PE), polypropylene (PP), and polybutylene; polyarylene sulfides such as polyoxymethylene (POM), polyamide (PA), and polyphenylene sulfide (PPS); fluorine-based resins such as polyketone (PK), polyether ketone (PEK), polyether ether ketone (PEEK), polyether ketone ketone (PEKK), polyether nitrile (PEN), and polytetrafluoroethylene; and liquid crystal polymers (LCP). "; amorphous resins such as "styrene-based resins, polycarbonate (PC), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyphenylene ether (PPE), polyimide (PI), polyamide-imide (PAI), polyetherimide (PEI), polysulfone (PSU), polyethersulfone, and polyarylate (PAR)"; and thermoplastic resins selected from phenol-based resins, phenoxy resins, polystyrene-based, polyolefin-based, polyurethane-based, polyester-based, polyamide-based, polybutadiene-based, polyisoprene-based, fluorine-based resins, and acrylonitrile-based thermoplastic elastomers, as well as copolymers and modified products thereof.

[0027] The thickness of the low linear expansion mixed paper is preferably 100 μm or more, more preferably 150 μm or more, even more preferably 150 μm to 10 mm, and most preferably 150 μm to 3 mm. This is advantageous in terms of handling, such as ease of gripping and transporting the low linear expansion mixed paper in the manufacturing process of products using the low linear expansion mixed paper.

[0028] The size of the low linear expansion mixed paper can be 1 m x 1 m or more, preferably 1 m x 2 m or more. If a papermaking process that allows continuous production is used, it becomes possible to make the paper larger.

[0029] Furthermore, the density of the low linear expansion mixed paper is set at 1.5 g / cm 3 It is preferable that the weight of the low linear expansion mixed paper is less than 100g. This makes it possible to obtain a lightweight low linear expansion mixed paper. Therefore, when the paper is made larger, the weight does not become too large. (binder resin)

[0030] The low linear expansion mixed sheet is obtained by impregnating a sheet material containing expanded graphite, aramid pulp, and carbon fiber with a binder resin. The optimum amount of binder resin is preferably 14% to 33%, more preferably 22% to 26%. More specifically, when the linear expansion coefficient is 5 ppm / K or less, the optimum amount of binder resin is 14% to 32% per 100 g of the sheet material, and when the linear expansion coefficient is 4 ppm / K or less, the optimum amount is 22% to 26%. If the amount of resin is too small, the adhesion between the fillers becomes insufficient. Conversely, if the amount of resin is too large, the linear expansion coefficient of the obtained low linear expansion mixed paper depends on the linear expansion coefficient of the binder resin. Therefore, in order to achieve dimensional stability, the amount of binder resin is adjusted to the above-mentioned range.

[0031] The binder resin may be a thermosetting resin, such as phenol, unsaturated polyester, epoxy, vinyl ester, bismaleimide, cyanate, polyimide, or the like.

[0032] The ratio of aramid pulp to expanded graphite is preferably 0.10 to 0.30. This prevents the expanded graphite from being detached from the mixed paper and also provides the effect of low linear expansion. Specifically, the ratio of expanded graphite is preferably 60 to 90 wt%, aramid pulp is 5 wt% to 30 wt%, and carbon fiber is 0 wt% to 10 wt%. The binder resin is preferably 14% to 33%, more preferably 22 to 26%. [Manufacturing method of low linear expansion mixed paper]

[0033] The manufacturing method of such low linear expansion mixed paper is as follows. First, expanded graphite, aramid pulp, and carbon fiber are mixed to obtain a sheet material. By utilizing the papermaking process, continuous production is possible, and large-sized sheet materials can be obtained. In addition, a sheet material with increased strength in multiple directions can be obtained by papermaking, without stacking multiple sheets in orthogonal directions to compensate for the shortcomings of conventional CFRP UD materials.

[0034] Furthermore, by using scraps as the carbon fibers, there is an advantage that production can be carried out at a lower cost than when long carbon fibers are used. The fiber length of the carbon fibers can be set to 3 mm to 13 mm.

[0035] Next, the sheet material obtained by mixing is impregnated with a thermosetting resin. For the resin impregnation, an impregnation method, a curtain coater, a blade coater, a kiss coater, a roll coater, a gravure coater, a fountain coater, a screen coater, etc. can be used. Among them, the impregnation method is preferably used from the viewpoint of permeating the resin into the inside of the sheet.

[0036] The resin-impregnated sheet material is then subjected to heat and pressure processing (heat pressing). Heat pressing is performed at 100°C to 300°C under an environment of pressure of 1MPa to 20MPa. This allows for the production of low linear expansion mixed paper with high thermal conductivity and a thermal conductivity of 34 W / m·K or more. In addition, since the sheet material is obtained during the papermaking process, it is easy to make the paper larger and there are fewer dimensional restrictions. Furthermore, the anisotropy of the linear expansion coefficient is suppressed, resulting in a low linear expansion mixed paper with a linear expansion coefficient of 4 ppm / K or less at 30°C to 200°C. Another advantage is that the manufacturing process requires only papermaking, resin impregnation, and heat and pressure processing, making it easy to manufacture. [Examples and Comparative Examples]

[0037] The low linear expansion mixed papers according to Examples 1 to 3 and Comparative Examples 1 to 3 were prepared and their properties were examined. Here, expanded graphite powder, aramid pulp, binder resin fiber, and carbon fiber were mixed in a ratio of 70:15:13:2 to obtain base paper for sheet material. The base paper for sheet material had a basis weight of 200 g / m2.2 , and had a thickness of 0.4 mm.

[0038] This sheet material was impregnated with phenol resin as a binder resin. Here, the amount of resin applied to the binder resin was varied in each of the examples and comparative examples. That is, the amount of resin applied was 0% in comparative example 1 and 7% in comparative example 2. On the other hand, it was 14% in example 1, 23% in example 2, 29% in example 3, and 37% in example 4. Specifically, DIC Corporation's J-325 phenol resin was used, diluted with methanol to each applied amount, impregnated, and dried at 60°C for 15 minutes.

[0039] Further, the low linear expansion mixed paper samples were obtained by heat and pressure processing at 7 MPa and 180°C for 10 minutes.

[0040] The linear expansion coefficient of each sample of the low linear expansion mixed paper thus obtained was measured in the machine direction (MD) or longitudinal direction and the cross direction (CD) or transverse direction at temperatures of 30°C to 50°C, 30°C to 100°C, 30°C to 150°C, and 30°C to 200°C. To measure the average linear expansion coefficient, thermomechanical analysis (TMA method) was used with reference to JIS K 7197. The size of the test piece was 5 mm wide x 30 mm. The measurement device used was a super-high temperature compatible thermomechanical analyzer TMA402 F1 Hyperion manufactured by Netsch Japan Co., Ltd. The measurement conditions are: Test mode: Tensile mode ·Measurement direction: MD, CD Sample length: 20mm ·Measurement temperature: Room temperature ~ 200℃ Heating rate: 5℃ / min. Test load: 49mN Measurement atmosphere: Nitrogen flow (150mL / min.) It was decided.

[0041] The thermal conductivity of each sample was also measured. The thermal conductivity was measured at a measurement temperature of 23°C using a xenon flash analyzer LFA447 Nanoflash manufactured by Netz Japan Co., Ltd. The data of each sample is shown in Table 1. The thermal expansion coefficients of the MD and CD of Comparative Example 2 are shown in Figures 2A and 2B, the thermal expansion coefficients of the MD and CD of Example 1 are shown in Figures 3A and 3B, the thermal expansion coefficients of the MD and CD of Example 2 are shown in Figures 4A and 4B, the thermal expansion coefficients of the MD and CD of Example 3 are shown in Figures 5A and 5B, and the thermal expansion coefficients of the MD and CD of Example 4 are shown in Figures 6A and 6B. Furthermore, the linear expansion coefficients at 30°C to 50°C, 30°C to 100°C, 30°C to 150°C, and 30°C to 200°C converted into ppm are shown in Figures 7 to 10. In addition, the thermal conductivity of each sample is shown in Figure 11.

[0042] [Table 1]

[0043] As shown in these tables and figures, the samples according to the comparative examples had a relatively large deviation in the linear expansion coefficients in the MD and CD, whereas the samples according to the examples were able to suppress the difference. In particular, in the range of 30°C to 200°C, the difference in the linear expansion coefficients in the MD and CD was 2.8 ppm in Comparative Example 1 and 4.7 ppm in Comparative Example 2, but in both examples it was suppressed to 1 ppm or less, and in Example 2 it was reduced to 0.2 ppm, confirming that the anisotropy of the linear expansion coefficient was extremely reduced. On the other hand, a thermal conductivity of 34 W / m·K or more was achieved. In this way, a low linear expansion mixed paper was obtained that maintained thermal conductivity by reducing the difference in the length and width while suppressing the linear expansion coefficient. [Industrial Applicability]

[0044] The low linear expansion mixed paper and its manufacturing method according to the present disclosure can be suitably used as a substrate or sheet material for mounting semiconductor components such as micro LED displays, etc. In particular, it can be suitably used in electrical equipment that requires a low linear expansion coefficient and suppresses dimensional changes due to temperature.

[0045] In addition, by using papermaking technology, it is possible to use carbon fiber scraps, which leads to the effective use of waste materials that cannot be used as long carbon fiber. This contributes to the utilization of waste and the expansion of recycling, and reduces the burden on the environment. As a result, it is possible to achieve the following of the 17 goals and 169 targets set out in the international goals SDGs (Sustainable Development Goals) adopted at the United Nations Summit in September 2015: "8. Decent work and economic growth", "8.4 By 2030, improve progressively global resource efficiency in consumption and production and endeavour to decouple economic growth from environmental degradation, in accordance with the 10-year framework of programmes on sustainable consumption and production, with developed countries taking the lead." "9. Build inclusive and sustainable industrial and technological infrastructure", "9.4 By 2030, improve infrastructure and industry to ensure sustainability, including by increasing resource efficiency and expanding the adoption of clean and environmentally friendly technologies and industrial processes. All countries will take action in accordance with their respective capabilities", "11. Sustainable cities and towns", "11.6 By 2030, reduce the adverse per capita environmental impact of cities, including by paying special attention to air quality and municipal and other waste management", This technology contributes to goals such as "12. Responsible Consumption and Production" and "12.4 By 2020, achieve the environmentally sound management of chemicals and all wastes throughout their life cycle, in accordance with agreed international frameworks, and significantly reduce release of chemicals and wastes to air, water and soil in order to minimize their adverse impacts on human health and the environment." [Explanation of symbols]

[0046] 1. Micro LED element 10...Base material

Claims

1. Expanded graphite; Aramid pulp; Carbon fiber, A binder resin; A low linear expansion mixed paper comprising: The linear expansion coefficient of the low linear expansion mixed paper in the longitudinal and transverse directions from 30°C to 200°C is 5 ppm / K or less in both directions, A low linear expansion mixed paper having a thermal conductivity of 34 W / m·K or more.

2. The low linear expansion mixed paper according to claim 1, The difference between the linear expansion coefficients of the low linear expansion mixed paper at 30° C. to 200° C. in the longitudinal and transverse directions is 0.5 ppm / K or less.

3. The low linear expansion mixed paper according to claim 1, The linear expansion coefficient of the low linear expansion mixed paper in the longitudinal and transverse directions from 30 ° C. to 200 ° C. is All of them are 4 ppm / K or less. The difference between the two is 0.2 ppm / K or less.

4. The low linear expansion mixed paper according to claim 1, The low linear expansion mixed paper, wherein the expanded graphite is in the form of powder.

5. The low linear expansion mixed paper according to claim 1, The ratio of the aramid pulp to the expanded graphite is 0.10 to 0.

30.

6. The low linear expansion mixed paper according to any one of claims 1 to 5, A low linear expansion mixed paper having a thickness of 100 μm or more.

7. The low linear expansion mixed paper according to any one of claims 1 to 5, The low linear expansion mixed paper has a resin content of 14% to 33% of the binder resin.

8. The low linear expansion mixed paper according to any one of claims 1 to 5, A low linear expansion mixed paper having a size of 1m x 1m or more.

9. The low linear expansion mixed paper according to any one of claims 1 to 5, Density is 1.5 g / cm 3 A low linear expansion mixed paper having the following properties:

10. The low linear expansion mixed paper according to any one of claims 1 to 5, A low linear expansion mixed paper is obtained by impregnating a sheet material containing the expanded graphite, the aramid pulp, the carbon fiber, and binder resin fibers with the binder resin.

11. A step of obtaining a sheet material by blending expanded graphite, aramid pulp, and carbon fibers; impregnating the sheet material with a thermosetting resin as a binder resin; The sheet material impregnated with the thermosetting resin is subjected to a heat and pressure process, The linear expansion coefficient of the sheet material in the longitudinal and transverse directions from 30°C to 200°C is 5 ppm / K or less in both directions, A step of obtaining a low linear expansion mixed paper having a thermal conductivity of 34 W / m K or more; A method for producing a low linear expansion mixed paper comprising the steps of:

Citation Information

Patent Citations

  • Carbon fiber nonwoven fabric, carbon fiber-reinforced resin sheet, and carbon fiber-reinforced resin molded form

    JP2011021303A

  • Method for producing composite material and composite material

    JP2011025297A

  • Metal-silicon carbide composite and production method of the same

    JP2020012194A

  • Plate material, heat dissipation material, and manufacturing method of plate material

    JP2021106202A

  • Glass fiber reinforced resin molded products

    JP7070819B1