Ink for forming low-reflection layer, laminate, and method for forming low-reflection layer
The low-reflection ink formulation addresses the limitations of existing coatings by using a balanced binder resin content, specific particle sizes, and organic solvents to enhance adhesion, scratch resistance, and moisture resistance, ensuring effective light-shielding and low reflectivity.
Patent Information
- Application Number
- JP2023212037
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing low-reflection coatings lack sufficient light-shielding properties, adhesion to substrates, scratch resistance, and durability due to the use of carbon black with small particle diameters and low binder resin content, leading to potential deterioration over time and uneven application.
A low-reflection ink formulation with a binder resin content of 30-55% by mass, average colorant particle size of 50-250 nm, and inclusion of extender pigments and/or resin fine particles, along with specific organic solvents, to enhance substrate adhesion, scratch resistance, and moisture resistance while maintaining low reflectivity.
The ink achieves improved light-shielding, low reflectivity, and durability through enhanced substrate adhesion, scratch resistance, and moisture resistance, effectively suppressing phenomena like ghosts and flares in camera modules.
Smart Images

Figure 2024167039000001 
Figure 2024167039000002 
Figure 2024167039000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink for forming a low reflective layer, and a low reflective laminate.
[0002] More specifically, the present invention relates to an ink for forming a low reflection layer, and a low reflection laminate having a low reflection layer on a substrate and having excellent low reflectivity and light blocking properties on the surface of the low reflection layer. [Background technology]
[0003] In the field of imaging, in camera modules of single-lens reflex cameras, smartphones, etc., low-reflective black ink is applied to the sides and edges of lenses to remove unnecessary incident light and reflected light and suppress the occurrence of flare and ghosting, which are factors that cause deterioration of image quality. Meanwhile, in the field of sensing, there is an increasing demand for ToF (Time of Flight) sensors that use laser light to measure distance for the purpose of object recognition and three-dimensional measurement. For these ToF sensors, low-reflective paint is applied around the light source to suppress internal reflection of the light source laser.
[0004] Outside of the fields of imaging and sensing, low-reflectivity colored inks are expected to be used to add design features in the field of packaging for consumer goods. In addition, with the increased demand for web video shooting amid the COVID-19 pandemic, there is a demand for low reflectivity in green screens used as backgrounds for subjects to improve image quality.
[0005] In the above-mentioned optical applications such as imaging and sensing, there is an example of a surface anti-reflective coating film that uses a surface anti-reflective coating material for atomization application containing a binder resin, carbon black, hydrophobized dry silica, roughening particles, dyes and solvents (Patent Document 1). However, this method imparts blackness by using carbon black and dyes in combination, but since dyes have low light resistance, there is a concern that low reflectivity will deteriorate over time. In addition, this composition is for atomization application, and even if it is applied to, for example, screen printing ink rather than printing ink, it is considered that the effect of forming unevenness is small and low reflectivity is difficult to obtain. In addition, the amount of silica as a matting agent is excessive, and there is a possibility that it may be inferior in scratch resistance and reverse gloss.
[0006] Patent Documents 2 and 3 describe a low-reflection film using carbon black, and an optical sensing kit and a low-reflection molded body using the same. However, the average particle diameter (D50) of the colorant carbon black is as small as 25 nm, and the transparency in the visible light region is high, so there is a concern that the light blocking properties will be insufficient. In addition, the content of the acrylic resin, which is the binder resin, is low, so there are problems with the adhesion to the substrate, etc. Therefore, a technology that satisfies the characteristics of a low-reflection laminate has not yet been obtained. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2020-97730 A [Patent Document 2] WO2020 / 195693 publication [Patent Document 3] JP 2021-140072 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention provides an ink for forming a low-reflection layer having excellent light-shielding properties and low reflectivity, as well as excellent adhesion to a substrate, scratch resistance, and moist heat resistance, a low-reflection laminate, and a method for forming a low-reflection layer. The purpose is to: [Means for solving the problem]
[0009] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by the following invention, and have completed the present invention.
[0010] The present invention provides an ink for forming a low reflection layer, comprising a binder resin, a colorant, fine particles (except when the fine particles are the colorant), and an organic solvent, The content of the binder resin is more than 30% by mass and not more than 55% by mass of the total mass of the ink solids, The average particle size of the colorant is 50 to 250 nm, The present invention relates to an ink for forming a low reflection layer, wherein the fine particles include a body pigment and / or resin fine particles.
[0011] The present invention also relates to the ink for forming a low reflection layer, wherein the binder resin comprises at least one resin selected from the group consisting of an acrylic resin, a polyester resin, and a urethane resin.
[0012] The present invention also relates to the ink for forming a low reflective layer, wherein the colorant contains at least carbon black.
[0013] The present invention also relates to the above ink for forming a low reflective layer, wherein the binder resin has a hydroxyl value of 10 to 50 mgKOH / g.
[0014] The present invention also relates to the above ink for forming a low reflective layer, wherein the total mass of the colorant and the fine particles is 40 to 55% by mass based on the total mass of the ink solids.
[0015] The present invention also relates to the above ink for forming a low reflective layer, wherein the fine particles have an average particle size of 0.5 to 15 μm.
[0016] The present invention also relates to the ink for forming a low reflection layer, wherein the fine particles are resin fine particles, and the resin fine particles contain at least one kind selected from the group consisting of polyester resin fine particles and acrylic resin fine particles.
[0017] The present invention also relates to the ink for forming a low reflective layer, wherein a mass ratio of the colorant to the fine particles (fine particles / colorant) is in the range of 3-5.
[0018] The present invention also relates to the above-mentioned ink for forming a low-reflection layer, wherein the organic solvent contains an organic solvent (A) consisting of a ketone-based organic solvent, and at least one organic solvent (B) selected from glycol ether-based organic solvents, ester-based organic solvents, aliphatic organic solvents, and aromatic organic solvents.
[0019] The present invention also relates to the above low reflection ink for forming a low reflection layer, wherein the difference in boiling point between the organic solvent (A) and the organic solvent (B) is 35 to 80°C.
[0020] The present invention also relates to a low reflective laminate having a low reflective layer made of the above-mentioned ink for forming a low reflective layer on a substrate.
[0021] The present invention also provides a method for forming a low reflection layer, which comprises printing an ink for forming a low reflection layer on a substrate to form a low reflection layer, the method comprising the steps of: The ink for forming a low reflection layer is the ink for forming a low reflection layer described above, The present invention relates to a method for forming a low reflective layer, which includes a drying step of volatilizing the organic solvent. Effect of the Invention
[0022] The present invention makes it possible to provide an ink for forming a low-reflection layer having excellent light-shielding properties and low reflectivity, as well as excellent adhesion to a substrate, scratch resistance, and moist heat resistance, a low-reflection laminate, and a method for forming a low-reflection layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The following describes in detail the embodiments of the present invention. However, the description of the components described below is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents as long as it does not go beyond the gist of the present invention.
[0024] In the present invention, "low reflection" has the same meaning as "anti-reflection" described in the prior art, and means that the reflectance is lower than that of the layer before improvement. In the following description, the "low-reflectivity laminate" may be referred to simply as the "laminate," and the "ink for forming a low-reflectivity layer" may be referred to as the "printing ink" or "ink," but they have the same meaning.
[0025] The present invention will be described in detail below. The present invention relates to an ink for forming a low-reflection layer, which contains a binder resin, a colorant, fine particles and an organic solvent, wherein the content of the binder resin is more than 30% by mass and not more than 55% by mass based on the total mass of the ink solids, the average particle diameter of the colorant is 50 to 250 nm, and the fine particles contain an extender pigment and / or resin fine particles. By setting the binder resin content in the ink within the above range, the ink layer formed after drying has good substrate adhesion, scratch resistance, and moist heat resistance. Furthermore, by setting the average particle size of the colorant within the above range, the ink fluidity is maintained good while the light shielding property and low reflectivity are improved, so that the ink layer formed has low reflection and can satisfy the light shielding property, substrate adhesion, scratch resistance, and moist heat resistance. By using a low-reflection laminate including a low-reflection layer made of the ink for forming a low-reflection layer of the present invention inside the lens barrel of a camera module for a smartphone or an in-vehicle sensor or around an image sensor, it can contribute to suppressing phenomena such as ghosts and flares. However, this function is based on consideration and does not particularly limit the present invention.
[0026] <Ink for low reflection formation> The low reflection forming ink of the present invention contains a binder resin, a colorant, fine particles and an organic solvent. A low reflection layer can be formed by printing the low reflection forming ink on a substrate and drying it, and the obtained print becomes a low reflection laminate.
[0027] (binder resin) In the present invention, the binder resin refers to a resin that can function as a binding agent in the ink, and is preferably a thermoplastic resin. Examples of the thermoplastic resin include acrylic resin, polyester resin, urethane resin, vinyl chloride-vinyl acetate copolymer resin, epoxy resin, styrene-based resin, rosin-based resin, styrene-maleic acid resin, dammar resin, polycarbonate resin, rosin-modified maleic acid resin, rosin ester resin, and terpene resin. These resins may be used in combination within a range that does not impair the effects of the present invention. From the viewpoint of substrate adhesion and moist heat resistance, it is preferable that the thermoplastic resin contains at least one selected from the group consisting of acrylic resin, polyester resin, and urethane resin, and it is more preferable that the thermoplastic resin contains acrylic resin.
[0028] The binder resin content is in the range of more than 30% by mass and less than 55% by mass of the total ink solids. The content is within the range of 32 to 55% by mass, more preferably 32 to 55% by mass, and further preferably 35 to 50% by mass. By making it more than 30% by mass, the adhesion to the substrate, scratch resistance, and moist heat resistance become good, and by making it 55% by mass or less, the light blocking property and low reflectance become good.
[0029] The hydroxyl value of the binder resin is preferably in the range of 10 to 50 mgKOH / g, and more preferably in the range of 20 to 40 mgKOH / g. By making it 10 mgKOH / g or more, the adhesion to the substrate is good, and by making it 50 mgKOH / g or less, the resistance to moist heat is good.
[0030] The weight average molecular weight (Mw) of the binder resin is preferably in the range of 5,000 to 120,000, and more preferably in the range of 20,000 to 100,000. By making the weight average molecular weight 5,000 or more, printability becomes good, and by making it 120,000 or less, scratch resistance becomes good. The weight average molecular weight is a value measured by GPC (gel permeation chromatography) in terms of polystyrene.
[0031] (Coloring agent) As the colorant for use in the present invention, various organic pigments, inorganic pigments, dyes, etc. can be mentioned, and they can be used in combination within a range that does not impair the effects of the present invention. From the viewpoint of light blocking properties and low reflectivity, it is preferable to use carbon black. The average particle size of the colorant used in the present invention is in the range of 50 to 250 nm, and more preferably in the range of 100 to 200 nm. By making it 50 nm or more, the fluidity of the ink becomes good, and by making it 250 nm or less, the light blocking property and low reflectance are good.
[0032] In the present invention, the average particle size refers to the D50 particle size measured by dynamic light scattering, and can be measured, for example, by Microtrack (manufactured by Microtrack-Bell, product name "MT3300EXII").
[0033] (Carbon Black) The carbon black used in the present invention may be any known one, and an example thereof is CI Pigment Black 7, as indicated by the CI number of the Colour Index International (abbreviated as CI).
[0034] The oil absorption of the above carbon black is 10 to 150 cm 3 / 100g, and 20 to 100cm 3It is more preferable that the oil absorption is in the range of 100 g / 100 g. By setting the oil absorption in this range, sufficient density of the printed matter can be obtained and the light blocking properties are good. The oil absorption is measured according to JIS K6221, and is the amount of DBP (dibutyl phthalate) absorbed by 100 g of carbon black.
[0035] The specific surface area of carbon black (nitrogen adsorption method) is 5 to 200 m 2 / g, and 10 to 150 m 2 By setting the specific surface area in this range, printability becomes good.
[0036] Specific examples of carbon black that satisfy the above requirements include Mitsubishi Carbon #10, Mitsubishi Carbon #20, Mitsubishi Carbon MA220 (manufactured by Mitsubishi Chemical Corporation), Seast S, Seast SP, Seast TA (manufactured by Tokai Carbon Co., Ltd.), SUNBLACK 235, Asahi #8, and Asahi #15 (manufactured by Asahi Carbon Co., Ltd.).
[0037] Specific examples of organic pigments other than the above carbon black that can be preferably used as colorants are shown below with their color index numbers.
[0038] Yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 20, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 86, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 1 No. 6, 127, 128, 129, 137, 138, 139, 147, 148, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 193, 194, 198, 199, 213, 214, 218, 219, 220, 221, 231, etc. can be suitably used.
[0039] Red pigments include CI Pigment Red 7, 9, 14, 41, 48:1, 48:2, 48:3, 48:4, 57:1, 81, 81:1, 81:2, 81:3, 81:4, 97, 122, 123, 146, 149, 150, 168, 169, 176, 177, 178, 180, 184, 185, 187, 192, 200, 202, 208, 209, 210, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, 242, 246, 254, 255, 264, 268, 270, 272, 273, 274, 276, 277, 278, 279, 280, 281, 282, 283, 284, 285, 286, 287, etc. can be suitably used.
[0040] As the indigo pigment, CI Pigment Blue 1, 1:2, 1:3, 2, 2:1, 2:2, 3, 8, 9, 10, 10:1, 11, 12, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 18, 19, 22, 24, 24:1, 53, 56, 56:1, 57, 58, 59, 60, 61, 62, 64, etc. can be suitably used.
[0041] As the orange pigment, CI Pigment Orange 36, 38, 43, 51, 55, 59, 61, 71, 73, etc. can be suitably used.
[0042] As the green pigment, CI Pigment Green 7, 10, 36, 37, 58, 62, 63, etc. can be suitably used.
[0043] As the purple pigment, CI Pigment Violet 1, 19, 27, 29, 30, 32, 37, 40, 42, 50, etc. can be suitably used.
[0044] Examples of inorganic pigments include titanium oxide, aluminum paste, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, iron oxide red, yellow iron oxide, iron black, etc. In order to ensure good coatability, sensitivity, developability, etc. while maintaining a balance between saturation and brightness, inorganic pigments are also preferably used in combination with organic pigments.
[0045] The content of the colorant is preferably in the range of 5 to 15 mass % of the total mass of the ink solids, and more preferably in the range of 7 to 12 mass %. When the content is 5 mass % or more, the light blocking property is good, and when the content is 15 mass % or less, the adhesion to the substrate and the scratch resistance are good.
[0046] (fine particles) The low reflection ink of the present invention contains a body pigment and / or resin fine particles as the fine particles. From the viewpoint of low reflectivity and printability, it is preferable to use resin fine particles as the fine particles. Note that the fine particles do not include so-called color pigments or colored resin fine particles, which are colorants. However, this does not exclude the case where the body pigment and / or resin fine particles are slightly colored.
[0047] The average particle size of the fine particles is preferably in the range of 0.5 to 15 μm, more preferably in the range of 2 to 10 μm. By making the average particle size 0.5 μm or more, fine irregularities can be formed on the surface of the low reflection layer, resulting in good low reflectivity, and by making the average particle size 15 μm or less, the scratch resistance of the surface of the low reflection layer can be good.
[0048] The refractive index of the fine particles used in the present invention is preferably in the range of 1.4 to 1.6, and more preferably in the range of 1.45 to 1.5. By setting the refractive index within the above range, good low reflectance can be achieved.
[0049] The content of the fine particles is preferably in the range of 25 to 50% by mass, more preferably 35 to 45% by mass, based on the total mass of the ink solids. By making the content ratio 25% by mass or more, low reflectivity is improved, and by making the content ratio 50% by mass or less, scratch resistance is improved.
[0050] As the extender pigment, for example, one or more of silica fine particles, alumina fine particles, talc fine particles, calcium carbonate fine particles, kaolin fine particles, precipitated barium sulfate fine particles, etc. can be used, but is not limited thereto.
[0051] Examples of resin particles include polyester resin particles, acrylic resin particles, melamine resin particles, melamine-benzoguanamine resin particles, benzoguanamine-formaldehyde condensed resin particles, fluororesin particles, urethane resin particles, and cellulose resin particles, among which polyester resin particles and / or acrylic particles are preferred, and polyester resin particles are more preferred, although one or more types may be used, and the resin particles applicable to the present invention are not limited to these.
[0052] The polyester resin microparticles include polyester resin microparticles made of polyhydroxyalkanoic acid, polyester resin microparticles made of condensation product of dibasic acid and diol, and polylactic acid resin microparticles. Among them, polyester resin microparticles made of polyhydroxyalkanoic acid and polyester resin microparticles made of condensation product of dibasic acid and diol are preferred, and polyester resin microparticles made of polyhydroxyalkanoic acid are more preferred. In addition, as the polyester resin microparticles, it is also preferred to use polyester resin microparticles formed of biodegradable resin.
[0053] Specific examples of polyester resin fine particles include Techpolymer TP-MG series (manufactured by Sekisui Plastics Co., Ltd.) Furthermore, examples of methods for producing polyester fine particles include the techniques described in JP-A Nos. 2007-191617 and 5-194141.
[0054] Specific examples of acrylic resin microparticles include Eposter MA1002, Eposter MA1004, Eposter MA1006, Eposter MA1010 (manufactured by Nippon Shokubai Co., Ltd.), Tuftic FH-S005, Tuftic FH-S008, Tuftic FH-S010, Tuftic FH-S015, Tuftic FH-S020 (manufactured by Toyobo Co., Ltd.), Chemisnow MX-80H3wT, MX-150, MX-180TA, MX-300, MX-500, MX-1000, MX-1500H, MX-2000, MX-3000 (manufactured by Soken Chemical & Engineering Co., Ltd.), and the like.
[0055] Specific examples of melamine resin fine particles include Eposter SS, Eposter S, Eposter FS, Eposter S6, and Eposter S12 (manufactured by Nippon Shokubai Co., Ltd.). A specific example of melamine-benzoguanamine resin microparticles is Eposta M30 (manufactured by Nippon Shokubai Co., Ltd.).
[0056] Specific examples of benzoguanamine-formaldehyde condensation resin microparticles include Eposter MS and Eposter L15 (manufactured by Nippon Shokubai Co., Ltd.).
[0057] Specific examples of melamine resin fine particles include Eposter SS, Eposter S, Eposter FS, Eposter S6, and Eposter S12 (manufactured by Nippon Shokubai Co., Ltd.). A specific example of melamine-benzoguanamine resin microparticles is Eposta M30 (manufactured by Nippon Shokubai Co., Ltd.).
[0058] Specific examples of benzoguanamine-formaldehyde condensation resin microparticles include Eposter MS and Eposter L15 (manufactured by Nippon Shokubai Co., Ltd.).
[0059] Specific examples of fluororesin fine particles include KTL-1N, KTL-2N, KTL-8N (manufactured by Kitamura Co., Ltd.), Shamrock SST-3D, Shamrock SST-4MG (manufactured by Shamrock Technologies Co., Ltd.), and the like.
[0060] Specific examples of urethane microparticles include crosslinked urethane beads such as Art Pearl C-1000 transparent, Art Pearl C-600 transparent, Art Pearl C-400 transparent, Art Pearl C-800, Art Pearl MM-120T, Art Pearl JB-800T, Art Pearl JB-600T, Art Pearl P-800T, and Art Pearl P-400T (manufactured by Negami Chemical Industries Co., Ltd.).
[0061] In the present invention, the total amount of the colorant and the fine particles is preferably in the range of 40 to 55% by mass, more preferably in the range of 45 to 50% by mass, based on the total mass of the ink solids. By making it 40% by mass or more, the light blocking property and low reflectance are improved, and by making it 55% by mass or less, the adhesion to the substrate, scratch resistance, and moist heat resistance are improved.
[0062] In the present invention, the ratio of colorant to fine particles (fine particles / colorant) in the low reflection layer is preferably in the range of 3 to 5, more preferably in the range of 3.5 to 5, and even more preferably in the range of 4 to 4.8. By making the ratio 3 or more, good low reflectance is obtained, and by making it 5 or less, good light blocking properties are obtained.
[0063] (Organic solvent) The printing ink preferably contains an organic solvent. Examples of the organic solvent include glycol ether-based organic solvents, ester-based organic solvents, aliphatic organic solvents, aromatic organic solvents, alcohol-based organic solvents, and ketone-based organic solvents. Among them, it is preferable to contain an organic solvent (A) consisting of a ketone-based organic solvent and at least one organic solvent (B) selected from glycol ether-based organic solvents, ester-based organic solvents, aliphatic organic solvents, and aromatic organic solvents. More preferably, it is preferable to use a ketone-based organic solvent that has good solubility for the binder resin, and a glycol ether-based organic solvent or an ester-based organic solvent that has good printability.
[0064] (Organic solvent (A)) The organic solvent (A) is a ketone-based organic solvent. Ketone-based organic solvents can be classified into cyclic ketone-based organic solvents having a cyclic skeleton and ketone-based organic solvents not having a cyclic skeleton. Among them, it is preferable to use a cyclic ketone-based organic solvent from the viewpoint of printability.
[0065] As the cyclic ketone organic solvent, an organic solvent containing a 5- to 7-membered cyclic ketone structure in the molecule is preferable. Examples of the 5-membered cyclic ketone organic solvent include cyclopentanone, 2-methyl-2-cyclopenten-1-one, 2-methylcyclopentanone, 3-methylcyclopentanone, and 4-methylcyclopentanone. Examples of cyclopentanone include cyclopentanone, 2-ethylcyclopentanone, 3-ethylcyclopentanone, 2,2-dimethylcyclopentanone, and 2,4,4-trimethylcyclopentanone. Examples of the 6-membered cyclic ketone organic solvent include cyclohexanone, isophorone, 2-cyclohexen-1-one, 2-methylcyclohexanone, 3-methylcyclohexanone, 4-methylcyclohexanone, 4-ethylcyclohexanone, 2,6-dimethylcyclohexanone, and 2,2-dimethylcyclohexanone. Examples of the seven-membered cyclic ketone organic solvent include cycloheptanone and 2-cycloheptan-1-one.
[0066] Examples of the ketone solvent not having a cyclic skeleton include acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone.
[0067] (Organic solvent (B)) In the present invention, the organic solvent (B) contains at least one selected from glycol ether-based organic solvents, ester-based organic solvents, aliphatic organic solvents, and aromatic organic solvents. Among them, from the viewpoint of printability, it is preferable to contain a glycol ether-based organic solvent or an ester-based organic solvent. However, the organic solvent (B) does not contain the organic solvent (A).
[0068] Examples of glycol ether organic solvents include ethylene glycol dibutyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monomethoxymethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monomethyl ether, triethylene glycol dimethyl ether, triethylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monobutyl ether.
[0069] Examples of the ester-based organic solvent include gamma-butyrolactone, cellosolve acetate, propylene glycol monomethyl ether acetate, ethylene glycol diacetate, ethylene glycol monoacetate, ethylene glycol monobutyl ether acetate, diethylene glycol diacetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, and propylene carbonate.
[0070] Examples of the aliphatic organic solvent include normal paraffin solvents, isoparaffin solvents, and cycloparaffin solvents.
[0071] Examples of aromatic organic solvents include toluene, xylene, ethylbenzene, naphthalene, tetralin, and solvent naphtha, as well as aromatic-rich solvents such as Swazol (manufactured by Cosmo Oil Co., Ltd. and Maruzen Petrochemical Co., Ltd.), Solvesso (manufactured by Exxon Mobil Corp.), and Cactus Fine (manufactured by Japan Energy Corporation).
[0072] In the present invention, the difference in boiling point between the organic solvent (A) and the organic solvent (B) is preferably 35 to 80°C, more preferably in the range of 40 to 70°C. By using a plurality of organic solvents whose boiling point difference is in the above range, the fine particles are likely to segregate to the surface of the low reflection layer due to the gradual evaporation of the organic solvents in the drying process. As a result, an uneven shape can be more effectively formed on the surface of the low reflection layer, and low reflectivity is improved. Furthermore, when printing the ink for forming the low reflection layer, it is preferable to dry at a temperature of 80°C or higher. The shorter the drying time, the easier it is to dry the ink. In this way, the above-mentioned uneven shape can be efficiently formed.
[0073] The content of the organic solvent is preferably in the range of 35 to 80% by mass, and more preferably in the range of 40 to 70% by mass, based on the total mass of the low reflective ink, because this improves the solubility of the resin. The organic solvent (A) and the organic solvent (B) can be mixed in any ratio, but the mass ratio of organic solvent (A) / organic solvent (B) is preferably in the range of 90 / 10 to 50 / 50, and more preferably in the range of 80 / 20 to 55 / 45.
[0074] (hardening agent) If necessary, the low reflection layer-forming ink may contain a polyisocyanate-type curing agent in an amount that does not impair the object of the present invention.
[0075] The content of the curing agent is preferably such that the ratio NCO / OH of the amount of effective isocyanate in the curing agent to the amount of hydroxyl groups in the binder resin in the ink solids is in the range of 0.5 to 1.5, more preferably in the range of 0.75 to 1.25. By making the NCO / OH ratio 0.5 or more, the adhesion to the substrate and scratch resistance are improved, and by making it 1.5 or less, the moist heat resistance is improved.
[0076] (Additives) The ink for forming the low reflection layer may contain additives such as dispersants, defoamers, leveling agents, wetting and penetrating agents, antiskinning agents, UV absorbers, antioxidants, crosslinking agents, preservatives, antifungal agents, viscosity adjusters, and pH adjusters, as necessary, within the scope that does not impair the object of the present invention.
[0077] <Production of ink for forming low reflection layer> The ink for forming a low reflection layer used in the present invention can be produced by mixing the required amounts of binder resin, colorant, fine particles, organic solvent, and, if necessary, curing agent and / or additives, and thoroughly stirring the mixture with a stirrer or the like, or by first preparing a dispersion containing colorant, dispersant, and organic solvent, and then mixing the required amounts of binder resin, organic solvent, curing agent, and / or additives, and thoroughly stirring the mixture with a stirrer or the like.
[0078] <Formation of low reflection layer> In the present invention, printing methods for forming a low reflection layer on a substrate include screen printing, roll coater, dispenser coating, dip coating, brush coating, etc., among which screen printing is preferred. As the printing machine, a cylinder press printing machine or a semi-automatic printing machine is preferably used, and as the printing plate, a resin material such as nylon or polyester, or a resin material such as stainless steel is preferably used.
[0079] <Screen printing> Screen printing is a technique that uses a screen made of chemical fibers such as polyester or nylon, or stainless steel, and uses a photosensitive emulsion on the screen to pattern areas where the ink passes through and areas where it does not pass through, then the ink is transferred to the substrate by pressing and moving the ink on the inner surface of the screen with a spatula-shaped rubber plate called a squeegee. The angle of the weave direction of the mesh with respect to the screen frame is called the bias angle. The thickness of the printed ink can be adjusted by the thickness of the photosensitive emulsion applied to the substrate surface. During printing, the angle between the substrate and the squeegee, and the angle in the printing direction, is called the attack angle. After printing, the ink can be fixed to the substrate by evaporating the solvent in the ink using a hot air oven.
[0080] <Low reflective layer formation method> The present invention relates to a method for forming a low-reflection layer, which forms a low-reflection layer by printing an ink for forming a low-reflection layer on a substrate, the ink containing a binder resin, a colorant, fine particles and an organic solvent, the content of the binder resin being 30-55% by mass based on the total mass of the ink solids, the average particle diameter of the colorant being 50-250 nm, and the method for forming a low-reflection layer including a drying step for volatilizing the organic solvent. By setting the binder resin content and the average particle diameter of the colorant in the ink within the above ranges, the dispersion stability of the colorant is improved, so that it becomes possible to effectively segregate only the fine particles in the drying step. As a result, an uneven shape is formed by the fine particles segregated on the surface of the low-reflection layer, and a low-reflection layer can be formed. Furthermore, the above-mentioned drying mechanism of the organic solvent makes it possible to more effectively segregate the fine particles.
[0081] In the low-reflectivity laminate of the present invention, the low-reflectivity layer is preferably formed by printing the ink for forming the low-reflectivity layer on the substrate by a screen printing method. The printing speed is preferably in the range of 50 to 300 mm / sec, more preferably in the range of 100 to 250 mm / sec. The drying temperature after printing is preferably 40 to 120°C, more preferably 60 to 120°C, and even more preferably 80 to 100°C. This improves low reflectivity. Furthermore, the viscosity of the ink during printing is preferably in the range of 700 to 12,000 cps, and more preferably in the range of 1,000 to 8,000 cps.
[0082] In the present invention, the low reflection layer preferably has a thickness of 5 μm or more, more preferably 7 μm or more, and particularly preferably 10 μm or more. When the thickness is 5 μm or more, the transmission density is 3 or more, and the light blocking property is good. The transmission density here is a value measured using an optical densitometer, and is expressed in logarithm as the ratio of a vertical transmitted light beam irradiated onto the laminate to a state in which the laminate is not present.
[0083] <Base material> In the present invention, the substrate used to form the laminate is not particularly limited, and examples thereof include various glasses such as soda glass, alkali-free glass, borosilicate glass, white plate glass, AR-coated glass, and UVIR-coated glass, inorganic material substrates such as quartz, polyester substrates such as polyethylene terephthalate, polyethylene, polypropylene, ethylene-vinyl acetate, and other polyolefin substrates, nylon substrates such as polyamide, acrylic substrates, polyvinyl chloride substrates, polycarbonate substrates, urethane substrates, and resin substrates such as epoxy substrates. A laminate using such substrates may also be used. A deposition substrate in which an inorganic compound such as silica, alumina, or aluminum is deposited on the substrate may also be used, and the deposition surface may be further coated with polyvinyl alcohol or the like. Corona treatment, frame treatment, and stretching treatment may also be performed. Among the above, inorganic material substrates such as glass are preferable. EXAMPLES
[0084] Hereinafter, the present invention will be specifically described as examples, but the present invention is not limited by the following examples. In the present invention, unless otherwise specified, "parts" represents "parts by mass" and "%" represents "% by mass".
[0085] <Dry film thickness> The dry film thickness of the low-reflection layer after drying was measured using a contact-type film thickness meter DigiMicro (manufactured by Nikon Corporation).
[0086] <OD value> The transmittance concentration (OD value) was measured using a transmission densitometer Gretag Macbeth TD-931.
[0087] <Reflectance> Using an ultraviolet-visible spectrophotometer V-760 (manufactured by JASCO Corporation), the reflectance was measured in an integrating sphere mode with a barium sulfate white plate as a reference, and evaluated with the average value in the wavelength range of 430 nm to 620 nm.
[0088] <Example 1: Adjustment of Ink for Forming Low-Reflection Layer> Into a 0.3 L glass flask equipped with a stirrer and a thermometer, 22.4 parts of the following acrylic resin 1, 30.0 parts of isophorone (boiling point 215.2 °C), and 16.0 parts of propylene glycol monomethyl ether acetate (boiling point 146.0 °C) were charged, and stirred at 80 °C for 2 hours to obtain an acrylic resin varnish having a solid content of 32.7% by mass. Next, 68.4 parts of the obtained acrylic resin varnish, 4.7 parts of the following carbon black 1, and 1.9 parts of the following dispersant were placed in a metal sealed container, and bead mill dispersion was performed using glass beads. To 75.0 parts of the obtained carbon black dispersion liquid, 22.0 parts of the following polyester resin fine particles 1, 0.5 part of the following antifoaming agent, and 2.5 parts of a polyisocyanate curing agent were charged, and dispersion stirring was performed to obtain the ink for forming a low-reflection layer of Example 1.
[0089] <Example 1: Preparation of Laminate> Using the ink for forming the low-reflection layer obtained by the above procedure, a 5 cm x 5 cm print was created by screen printing on a 1.1 mm thick soda glass substrate under the following screen printing conditions: After screen printing, the substrate was placed in an oven at 80°C for 1 hour to dry the ink, forming a low-reflection layer on the substrate and creating a laminate.
[0090] (Screen printing conditions) A 20 μm-thick emulsion layer made of photosensitive emulsion was formed on a polyester mesh with a mesh count of 250 mesh / inch, and the plate was made so that the bias angle was 22.5°. A urethane squeegee with a durometer A hardness of 80 was used. Screen printing was performed with an attack angle of 75° and a squeegee speed of 100 mm / sec.
[0091] <Examples 2 to 29 and Comparative Examples 1 to 5: Preparation of ink for forming low reflection layer> Using the raw materials and compositions shown in Tables 1 and 2, the same procedure as in Example 1 was carried out to obtain inks for forming low reflective layers of Examples 2 to 29 and Comparative Examples 1 to 5. In the tables, values without unit notation indicate parts, and blanks indicate that no compound was added.
[0092] <Examples 2 to 29 and Comparative Examples 1 to 5: Preparation of Laminates> Using the inks for forming a low reflective layer obtained by the above procedure, laminates were produced in the same manner as in Example 1 using the inks for forming a low reflective layer of Examples 2 to 29 and Comparative Examples 1 to 5.
[0093] [Table 1]
[0094] [Table 1]
[0095] [Table 2]
[0096] Acrylic resin 1: Hydroxyl value 30mgKOH / g, weight average molecular weight Mw42000 Polyester resin 1: hydroxyl value 30mgKOH / g, weight average molecular weight Mw12000 Acrylic resin 2: Hydroxyl value 48mgKOH / g, weight average molecular weight Mw43000 Vinyl chloride-vinyl acetate copolymer resin 1: hydroxyl value 30 mgKOH / g, weight average molecular weight Mw 24000 · Urethane resin 1: Hydroxyl value 30mgKOH / g, weight average molecular weight Mw80000 Acrylic resin 3: hydroxyl value 5mgKOH / g, weight average molecular weight Mw40000 Acrylic resin 4: Hydroxyl value 70mgKOH / g, weight average molecular weight Mw48000 Carbon black 1: Average particle size 150 nm, oil absorption 40 cm 3 / 100g, specific surface area 15m 2 / g Carbon black 2: Average particle size 75 nm, oil absorption 78 cm 3 / 100g, specific surface area 25m 2 / g Carbon black 3: average particle size 220 nm, oil absorption 32 cm 3 / 100g, specific surface area 15m 2 / g Carbon black 4: Average particle size 30 nm, oil absorption 113 cm 3 / 100g, specific surface area 76m 2 / g Carbon black 5: average particle size 350 nm, oil absorption 21 cm 3 / 100g, specific surface area 8m 2 / g CI Pigment Green 7: Average particle size 220nm Polyester resin particles 1: average particle diameter 5μm, refractive index 1.48 Polyester resin particles 2: average particle diameter 1 μm, refractive index 1.48 Polyester resin particles 3: average particle size 12 μm, refractive index 1.48 Acrylic resin particles 1: average particle diameter 6μm, refractive index 1.49 Benzoguanamine-formaldehyde condensation resin microparticles 1: average particle size 5μm, refractive index 1.66 Polyester resin particles 4: average particle size 0.3 μm, refractive index 1.48 Polyester resin particles 5: average particle size 18 μm, refractive index 1.48 Spherical silica 1: average particle size 4μm, refractive index 1.46 Isophorone: boiling point 215.2℃ Cyclohexanone: boiling point 155.6℃ Propylene glycol monomethyl ether acetate: boiling point 146.0℃ Toluene: boiling point 110.6℃ Dispersant: SOLSPERSE 24000 GR, Lubrizol, 100% solids Antifoaming agent: DOWIL SH5500 Antifoam Compound, Dow Chemical Japan, 100% solids Polyisocyanate hardener: Coronate HX, manufactured by Tosoh Corporation, NCO ratio 20.5%, solids content 100%
[0097] <Evaluation> The laminates obtained in the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Tables 1 and 2.
[0098] <Light blocking property> The evaluation was based on the transmission density (OD value) measured by the above method. The evaluation criteria were as follows: 5 (Excellent): OD value 4.5 or higher 4 (Good): OD value 3.8 or more, less than 4.5 3 (Acceptable): OD value 3.0 or more, less than 3.8 2 (Not acceptable): OD value is 2.2 or more and less than 3.0 1 (poor): OD value less than 2.2 Usable practical ratings are 3, 4 and 5.
[0099] <Low reflectivity> The evaluation was based on the reflectance measured by the above method, and the evaluation criteria were as follows. 5 (Excellent): Less than 2.4% 4 (Good): 2.4% or more, less than 2.8% 3 (Acceptable): 2.8% or more, less than 3.2% 2 (Not acceptable): 3.2% or more, less than 3.6% 1 (poor): 3.6% or more Usable practical ratings are 3, 4 and 5.
[0100] <Adhesion to substrate> A checkerboard peel test tool was used on the low reflection layer to measure 1 mm 2 A total of 100 cross-cuts were made. Thereafter, adhesive tape (LP24, manufactured by Nichiban Co., Ltd.) was applied onto the cross-cut area and peeled off at a 90-degree angle, and the number of remaining squares in the cured film was counted. The evaluation criteria were as follows: 5 (excellent): 96~100 pieces 4 (good): 91~95 pieces 3 (acceptable): 86~90 pieces 2 (not allowed): 81~85 pieces 1 (poor): 80 pieces or less Usable practical ratings are 3, 4 and 5.
[0101] <Scratch resistance> Evaluation was performed using a Gakushin-type friction fastness tester at 25°C and 50% humidity. A white cotton cloth was attached to the tip of a friction element (20mm x 20mm, R45mm), and the friction element was placed on the low-reflective layer under a load of 200gf and moved back and forth 10 times at a speed of 30 strokes / min. After 10 strokes, the degree of rubbing off of the low-reflective ink was evaluated as coloring on the white cotton cloth. The degree of coloring of the white cotton cloth was evaluated based on JIS L 0805 using a staining gray scale. The evaluation criteria are as follows: 5 (Excellent): Grayscale level 5 4 (Good): Between grayscale level 4 and 5 3 (OK): Grayscale Level 4 2 (Not acceptable): Between grayscale level 3 and 4 1 (Poor): Grayscale level 3 or below Usable practical ratings are 3, 4 and 5.
[0102] <Moisture and heat resistance> The laminate was boiled in boiling water for 60 minutes, then removed from the hot water and allowed to stand at room temperature for 10 minutes, after which the adhesion to the substrate was evaluated by the above method. The evaluation criteria are as follows: 5 (excellent): 96~100 pieces 4 (good): 91~95 pieces 3 (acceptable): 86~90 pieces 2 (not allowed): 81~85 pieces 1 (poor): 80 pieces or less Usable practical ratings are 3, 4 and 5.
[0103] Comparative Example 1, which did not contain any extender pigment and / or resin fine particles, Comparative Examples 2 and 3, in which the binder resin was not in the range of 30 to 55 mass% of the total mass of the ink solids, and Comparative Examples 4 and 5, in which a colorant with an average particle size outside the range of 50 to 250 nm was used, showed poor results in any one of light blocking properties, low reflectivity, adhesion to substrates, scratch resistance, and moist heat resistance.
[0104] According to the present invention, it is possible to provide a low-reflectivity laminate that is excellent in light-shielding properties, low reflectivity, adhesion to a substrate, scratch resistance, and moist heat resistance.
Claims
1. An ink for forming a low reflection layer, comprising a binder resin, a colorant, fine particles (except when the fine particles are the colorant), and an organic solvent, The content of the binder resin is more than 30% by mass and not more than 55% by mass based on the total mass of the ink solids, The average particle size of the colorant is 50 to 250 nm; The ink for forming a low reflection layer, wherein the fine particles include a body pigment and / or a resin fine particle.
2. 2. The ink for forming a low reflection layer according to claim 1, wherein the binder resin comprises at least one resin selected from the group consisting of an acrylic resin, a polyester resin, and a urethane resin.
3. 3. The ink for forming a low reflection layer according to claim 1, wherein the colorant comprises at least carbon black.
4. 3. The ink for forming a low reflective layer according to claim 1, wherein the binder resin has a hydroxyl value of 10 to 50 mgKOH / g.
5. 3. The ink for forming a low reflection layer according to claim 1, wherein the total mass of the colorant and the fine particles is 40 to 55% by mass based on the total mass of the ink solids.
6. 3. The ink for forming a low reflection layer according to claim 1, wherein the fine particles have an average particle size of 0.5 to 15 μm.
7. 3. The ink for forming a low reflection layer according to claim 1, wherein the fine particles are resin fine particles, and the resin fine particles include at least one kind selected from the group consisting of polyester resin fine particles and acrylic resin fine particles.
8. 3. The ink for forming a low reflection layer according to claim 1, wherein a mass ratio of the colorant to the fine particles (fine particles / colorant) is in the range of 3 to 5.
9. 3. The ink for forming a low-reflection layer according to claim 1 or 2, wherein the organic solvent comprises an organic solvent (A) consisting of a ketone-based organic solvent, and at least one organic solvent (B) selected from glycol ether-based organic solvents, ester-based organic solvents, aliphatic organic solvents, and aromatic organic solvents.
10. 10. The low reflection ink for forming a low reflection layer according to claim 9, wherein the difference in boiling point between the organic solvent (A) and the organic solvent (B) is 35 to 80°C.
11. A low-reflection laminate comprising a substrate and a low-reflection layer formed from the ink for forming a low-reflection layer according to claim 1 or 2.
12. A method for forming a low reflection layer, comprising the steps of: printing an ink for forming a low reflection layer on a substrate to form a low reflection layer, The ink for forming a low reflection layer is the ink for forming a low reflection layer according to 1 or 2, A method for forming a low reflective layer, comprising a drying step of volatilizing the organic solvent.
Citation Information
Patent Citations
Surface antireflection coating for atomization coating, and surface antireflection coated film
JP2020097730A
Resin composition for low reflection light-shielding layer, and low reflection light-shielding layer and low reflection light-shielding layer laminate using the same
JP2021140072A
Low reflection film, optical sensing kit using same, and low reflection molded body
WO2020195693A1