Block copolymer, dispersant, and, coloring composition

A block copolymer with A, B, and C blocks addresses the challenges of high pigment concentrations by enhancing dispersibility and stability in coloring compositions, ensuring effective colorant dispersion and alkaline developability.

JP2024167056APending Publication Date: 2024-11-29OTSUKA CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024072456
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-04-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing dispersants face challenges in achieving high colorant dispersion performance and viscosity stability in coloring compositions due to the increasing concentration of pigments, which affects dispersibility and alkali developability.

Method used

A block copolymer with a specific arrangement of A, B, and C blocks, where A contains structural units with hydroxy and/or ether groups, B contains nitrogen-containing functional groups, and C contains hydroxy groups, with a controlled molar volume ratio of (c-1)/(b-1) between 0.1 to 1.5, ensuring high affinity with the dispersion medium and colorant, thereby suppressing desorption.

Benefits of technology

The block copolymer exhibits excellent colorant dispersion performance, resulting in a colored composition with improved viscosity stability and alkaline developability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167056000001
    Figure 2024167056000001
  • Figure 2024167056000002
    Figure 2024167056000002
  • Figure 2024167056000003
    Figure 2024167056000003
Patent Text Reader

Abstract

To provide a block copolymer having high dispersibility of a coloring material, when used as a dispersant of a coloring composition.SOLUTION: A block copolymer contains an A block, a B block, and a C block, and the arrangement of each block is in the order of A block-B block-C block, wherein the A block is a structural unit (a-1) having a hydroxy group and / or an ether group, the B block is a structural unit (b-1) having a nitrogen-containing functional group, and the C block each contains a structural unit (c-1) having a hydroxy group, respectively, and a molar volume ratio ((c-1) / (b-1)) of the structural unit (c-1) to the structural unit (b-1) is 0.1-1.5, and a content ratio of the structural unit (b-1) in the 100 mol% of the structural unit constituting the A block is 3 mol% or less, and the content ratio of the structural unit (b-1) in the 100 mol% of the structural unit constituting the C block is 3 mol% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a block copolymer, and more particularly to a block copolymer which can be used as a dispersant for a colorant in a coloring composition. [Background technology]

[0002] Conventionally, in the manufacture of color filters used in liquid crystal displays and the like, dyeing methods, printing methods, inkjet methods, electrodeposition methods, pigment dispersion methods, and the like are known as methods for applying colorants to substrates. Among these, the pigment dispersion method is mainstream from the viewpoints of spectral characteristics, durability, pattern shape, and accuracy. In this pigment dispersion method, a coating film made of a coloring composition in which a pigment, a dispersant, a dispersion medium (solvent), a binder resin, and the like are mixed is formed on a substrate, and the coating film is cured by irradiating radiation through a photomask having a desired pattern shape, and then alkali development is performed.

[0003] In recent years, in order to obtain good color reproducibility and high contrast of color filters, it has been considered to increase the concentration of pigment in a coloring composition. When the pigment is increased in concentration, the proportion of the dispersant is relatively decreased, so the dispersant is required to have high dispersibility (for example, see Patent Document 1 (paragraph 0004)). In addition, in alkaline development, a binder resin having alkali solubility plays a major role. However, in the case of a pigment dispersion composition with a high pigment concentration, the proportion of the binder resin, which is a developing component, decreases, and the alkali developability decreases. Therefore, the alkali developability that was originally required of the binder resin is also required of the dispersant. As such a dispersant, Patent Document 2 describes the use of an AB block copolymer consisting of an A block having a polylactone chain in the side chain and a B block having a tertiary amino group in the side chain as a pigment dispersion (see Patent Document 2 (paragraphs 0023 to 0045)). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-265515 A [Patent Document 2] JP 2013-119568 A Summary of the Invention [Problem to be solved by the invention]

[0005] In a resin-type dispersant, it has been proposed to introduce a tertiary amino group into the side chain in order to improve the dispersibility of the colorant (see Patent Document 2). However, due to the recent trend toward higher concentrations of colorants in colored compositions, further improvement in dispersibility is required.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a block copolymer which has high dispersibility of a colorant when used as a dispersant for a coloring composition. [Means for solving the problem]

[0007] The block copolymer of the present invention, which has been able to solve the above problems, is a block copolymer containing an A block, a B block, and a C block, and the arrangement of the blocks is in the order of A block-B block-C block, the A block contains a structural unit (a-1) having a hydroxy group and / or an ether group, the B block contains a structural unit (b-1) having a nitrogen-containing functional group, and the C block contains a structural unit (c-1) having a hydroxy group, the molar volume ratio of the structural unit (c-1) to the structural unit (b-1) ((c-1) / (b-1)) being 0.1 to 1.5, the content of the structural unit (b-1) in 100 mol % of the structural units constituting the A block is 3 mol % or less, and the content of the structural unit (b-1) in 100 mol % of the structural units constituting the C block is 3 mol % or less.

[0008] In the block copolymer of the present invention, the A block contains the structural unit (a-1), the B block contains the structural unit (b-1), and the C block contains the structural unit (c-1), and the content of the structural unit (b-1) in the A block and the C block is 3 mol% or less. The structural unit (a-1) and the structural unit (c-1) have high affinity with the dispersion medium, and the structural unit (b-1) has high affinity with the colorant, so that the structural unit (b-1) is adsorbed to the colorant. By controlling the molar volume ratio ((c-1) / (b-1)) of the structural unit (c-1) to the structural unit (b-1) within a predetermined range, it is possible to suppress detachment of the dispersant from the colorant. Effect of the Invention

[0009] The block copolymer of the present invention has excellent dispersibility for coloring materials, and when used as a dispersant for coloring materials, a colored composition having excellent viscosity stability can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example, and the present invention is not limited to the following embodiment.

[0011] <Definition> In this specification, "(meth)acrylic" means "at least one of acrylic and methacrylic". "(meth)acrylate" means "at least one of acrylate and methacrylate", and is an ester compound in which the hydrogen atom of the carboxyl group of (meth)acrylic acid is substituted with an organic group. "(meth)acryloyl" means "at least one of acryloyl and methacryloyl". "(meth)acrylic monomer" means "monomer having a (meth)acryloyl group in the molecule", including "(meth)acrylate". "Vinyl monomer" means "monomer having a carbon-carbon double bond capable of radical polymerization in the molecule", including "(meth)acrylate" and "(meth)acrylic monomer".

[0012] In this specification, "structural unit derived from (meth)acrylate" means "structural unit in which a radically polymerizable carbon-carbon double bond of (meth)acrylate is polymerized to form a carbon-carbon single bond". "Structural unit derived from (meth)acrylic monomer" means "structural unit in which a radically polymerizable carbon-carbon double bond of (meth)acrylic monomer is polymerized to form a carbon-carbon single bond". "Structural unit derived from vinyl monomer" means "structural unit in which a radically polymerizable carbon-carbon double bond of vinyl monomer is polymerized to form a carbon-carbon single bond".

[0013] In this specification, when it is written "X~Y" (X and Y are any numbers), it means "X or more, Y or less". Furthermore, when it is written "X or more" (X is any number), it also means "X or more than X", and when it is written "Y or less" (Y is any number), it also means "Y or less than Y". Furthermore, "X and / or Y (X and Y are any configuration)" means "at least one of X and Y", and can mean three things: "X only", "Y only", and "X and Y".

[0014] <Block copolymer> The block copolymer of the present invention is a block copolymer containing an A block, a B block, and a C block.

[0015] In this specification, an "A block" can be alternatively referred to as an "A segment", a "B block" can be alternatively referred to as a "B segment", and a "C block" can be alternatively referred to as a "C segment".

[0016] (A Block) The A block contains a structural unit (a-1) having a hydroxy group and / or an ether group. The structural unit (a-1) may be used alone or in combination of two or more types. The A block has high affinity with the dispersion medium and acts as a compatible site. In addition, the A block can suppress aggregation between colorant particles due to changes over time due to a steric repulsion effect.

[0017] The content of the structural unit (a-1) in 100 mol% of the structural units constituting the A block is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 20 mol% or more, and is preferably 95 mol% or less, more preferably 70 mol% or less, even more preferably 50 mol% or less, and particularly preferably 40 mol% or less. If the content of the structural unit (a-1) is 5 mol% or more, the affinity to the dispersion medium is further increased, and the solubility in an alkaline developer is further increased, and the alkaline developability of the colored composition can be further improved, and if it is 95 mol% or less, the affinity to the dispersion medium is increased, and the dispersibility can be further improved.

[0018] The molar volume ratio ((a-1) / (b-1)) of the structural unit (a-1) to the structural unit (b-1) in the B block is preferably 0.1 or more, more preferably 0.5 or more, even more preferably 3.0 or more, and is preferably 10.0 or less, more preferably 9.0 or less, even more preferably 7.0 or less, and particularly preferably 6.0 or less. When the molar volume ratio ((a-1) / (b-1)) is within the above range, aggregation between colorant particles due to steric repulsion can be more effectively suppressed. When the B block contains multiple types of structural units (b-1), the molar volume ratio is calculated as the ratio to the molar volume of the structural unit (b-1) with the highest content.

[0019] The molar volume (V) of a structural unit is the sum of the molar volumes Vi of the atomic groups i that compose the structural unit. The molar volumes Vi of representative atomic groups are shown in Table 1. The combination of the structural unit (a-1) and the structural unit (b-1) described below, and the combination of the structural unit (c-1) and the structural unit (b-1) described below can also be examined using a method called materials informatics that utilizes computational science / information science.

[0020] [Table 1]

[0021] The A block may contain a structural unit (a-1) having a molar volume ratio ((a-1) / (b-1)) outside the above range. The content of structural units having a molar volume ratio ((a-1) / (b-1)) within the above range in 100 mol% of structural units (a-1) contained in the A block is preferably 20 mol% or more, more preferably 50 mol% or more, and even more preferably 100 mol%.

[0022] (Structural unit (a-1)) The structural unit (a-1) is preferably a structural unit represented by formula (1).

[0023] [ka] [In formula (1), R 11 represents a hydrogen atom or a methyl group. A 11 represents an ester group, an amide group, or a single bond. R 12 is a divalent hydrocarbon group, -R 14 -(O-CO-R 15 ) m1 -group or -R 16 -(OR 17 ) n1 - represents a group. R 13 represents a hydrogen atom or a monovalent hydrocarbon group. 12 is a divalent hydrocarbon group, or -R 14 -(O-CO-R 15 ) m1 - group, R 13 is a hydrogen atom. m1 represents an integer of 1 to 10. R 14 represents a divalent hydrocarbon group. R 15 represents a divalent hydrocarbon group, and when m1 is 2 or more, a plurality of R 15 may be the same or different. n1 represents an integer from 1 to 30. R 16 represents a divalent hydrocarbon group. R17 represents a divalent hydrocarbon group, and when n1 is 2 or more, multiple R 17 may be the same or different.]

[0024] The above A 11 represents an ester group (-CO-O-), an amide group (-CO-NH-) or a single bond, and an ester group or an amide group is preferable. The bonding direction of the ester group or the amide group is not particularly limited. The bonding mode of the ester group is C-CO-OR. 12 or CO-CO-R 12 C-CO-OR 12 The bonding form of the amide group is preferably C-CO-NH-R. 12 or C-NH-CO-R 12 C-CO-NH-R 12 is preferred.

[0025] R 12 Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 20 carbon atoms, an alkenylene group having 2 to 20 carbon atoms, and an arenediyl group having 6 to 20 carbon atoms. Among these, an alkylene group having 1 to 20 carbon atoms is preferred. The alkylene group may be either linear or branched, but linear is preferred. The number of carbon atoms in the alkylene group is more preferably 1 to 4. Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0026] R 12 Represented by -R 14 -(O-CO-R 15 ) m1 -group or -R 16 -(OR 17 ) n1 In the -group, R 14 , R 15 , R 16 or R 17Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 20 carbon atoms, an alkenylene group having 2 to 20 carbon atoms, and an arenediyl group having 6 to 20 carbon atoms. 14 , R 15 , R 16 or R 17 The divalent hydrocarbon group represented by the following formula is preferably an alkylene group having 1 to 20 carbon atoms.

[0027] The structural unit (a-1) is preferably at least one selected from the group consisting of a structural unit (a-11) represented by formula (2), a structural unit (a-12) represented by formula (3), and a structural unit (a-13) represented by formula (4).

[0028] (Structural unit (a-11)) The structural unit (a-11) is a structural unit derived from a (meth)acrylate having a hydroxy group.

[0029] [ka] [In formula (2), R 21 represents a hydrogen atom or a methyl group. R 22 represents an alkylene group having 1 to 20 carbon atoms, an alkenylene group having 2 to 20 carbon atoms, or an arenediyl group having 6 to 20 carbon atoms.]

[0030] R 22 is preferably an alkylene group having a carbon number of 1 to 12, and more preferably an alkylene group having a carbon number of 1 to 5. The alkylene group may be either linear or branched, but is preferably linear.

[0031] Specific examples of vinyl monomers forming the structural unit represented by the formula (2) include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 4-hydroxyphenyl (meth)acrylate, etc. Among these, (meth)acrylates having a hydroxyalkyl group having 1 to 5 carbon atoms are more preferred.

[0032] (Structural unit (a-12)) The structural unit (a-12) is a structural unit derived from a (meth)acrylate having a lactone-modified hydroxy group.

[0033] [ka] [In formula (3), R 31 represents an alkylene group having 1 to 10 carbon atoms. R 32 represents an alkylene group having 1 to 10 carbon atoms. R 33 represents a hydrogen atom or a methyl group. m3 represents an integer of 1 to 10. When m3 is 2 or more, a plurality of R 31 may be the same or different.

[0034] R 31 , R 32 The alkylene group having 1 to 10 carbon atoms represented by the following formula (1) may be either linear or branched, but is preferably linear. R 31 is preferably an alkylene group having 1 to 8 carbon atoms, and more preferably an alkylene group having 3 to 8 carbon atoms. R 32 is preferably an alkylene group having 1 to 5 carbon atoms. The above m3 is preferably an integer of 1 to 7, and more preferably an integer of 1 to 5.

[0035] Specific examples of the vinyl monomer that forms the structural unit represented by the formula (3) include caprolactone adducts of hydroxyalkyl (meth)acrylates (in the formula (3), R 31 The hydroxyalkyl (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, a caprolactone adduct of 2-hydroxyethyl (meth)acrylate (in formula (3), R 33 is a hydrogen atom or a methyl group, R 32 is an ethylene group, R 31 is a pentamethylene group, and m3 is 1 to 10).

[0036] Examples of the caprolactone adduct of 2-hydroxyethyl (meth)acrylate include an adduct of 1 mol of 2-hydroxyethyl (meth)acrylate with caprolactone, an adduct of 2-hydroxyethyl (meth)acrylate with 2 mol of caprolactone, an adduct of 3 mol of 2-hydroxyethyl (meth)acrylate with caprolactone, an adduct of 4 mol of 2-hydroxyethyl (meth)acrylate with caprolactone, and an adduct of 5 mol of 2-hydroxyethyl (meth)acrylate with caprolactone.

[0037] (Structural unit (a-13)) The structural unit (a-13) is a structural unit derived from a (meth)acrylate having a polyalkylene glycol structure.

[0038] [ka] [In formula (4), R 41 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. R 42 represents an alkylene group having 1 to 3 carbon atoms. R 43 represents an alkylene group having 1 to 3 carbon atoms. R 44 represents a hydrogen atom or a methyl group. m4 represents an integer of 1 to 30. When m4 is 2 or more, a plurality of R 42 may be the same or different.

[0039] R 41 The alkyl group having 1 to 3 carbon atoms represented by the formula (I) may be either linear or branched, but is preferably linear. 41 Specific examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. R 42 , R 43 The alkylene group having 1 to 3 carbon atoms represented by the formula (I) may be either linear or branched, but is preferably linear. R 42 The alkylene group having 1 to 3 carbon atoms represented by the formula (I) is preferably an ethylene group or a trimethylene group. R 43 The alkylene group having 1 to 3 carbon atoms represented by the formula (I) is preferably an ethylene group or a trimethylene group. The m4 is 2 or more, preferably 5 or more, and 30 or less, preferably 20 or less, and more preferably 15 or less.

[0040] Examples of the monomer constituting the structural unit represented by the formula (4) include (meth)acrylates having a polyalkylene glycol structure. The polyalkylene glycol portion may be, for example, a mixture of ethylene oxide and propylene oxide. Examples of the (meth)acrylate having a polyalkylene glycol structure include (meth)acrylates having a polyethylene glycol structure such as polyethylene glycol (degree of polymerization = 2 to 30) methyl ether (meth)acrylate, polyethylene glycol (degree of polymerization = 2 to 30) ethyl ether (meth)acrylate, polyethylene glycol (degree of polymerization = 2 to 30) propyl ether (meth)acrylate, and polyethylene glycol (degree of polymerization = 2 to 30) mono(meth)acrylate; and (meth)acrylates having a polypropylene glycol structural unit such as polypropylene glycol (degree of polymerization = 2 to 30) methyl ether (meth)acrylate, polypropylene glycol (degree of polymerization = 2 to 30) ethyl ether (meth)acrylate, polypropylene glycol (degree of polymerization = 2 to 30) propyl ether (meth)acrylate, and polypropylene glycol (degree of polymerization = 2 to 30) mono(meth)acrylate.

[0041] The A block may be composed only of the structural unit (a-1), or may contain other structural units.

[0042] Examples of the vinyl monomer constituting the other structural unit include (meth)acrylic vinyl monomers, α-olefins, aromatic vinyl monomers, vinyl monomers containing a heterocycle, vinyl amides, vinyl carboxylates, dienes, and the like. One or a combination of two or more of these can be used.

[0043] Examples of the (meth)acrylic vinyl monomer include (meth)acrylates having a chain alkyl group, (meth)acrylates having a cyclic alkyl group, (meth)acrylates having an aromatic group, (meth)acrylates having an alkoxy group, (meth)acrylates having a cyclic ether group, (meth)acrylates having an acidic group, and (meth)acrylic acid.

[0044] Examples of the (meth)acrylate having a chain alkyl group include (meth)acrylates having a straight-chain alkyl group and (meth)acrylates having a branched-chain alkyl group.

[0045] The (meth)acrylate having a linear alkyl group is preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 20, more preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 10, and even more preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 5. Examples of the (meth)acrylate having a linear alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-lauryl (meth)acrylate, and n-stearyl (meth)acrylate.

[0046] The (meth)acrylate having a branched alkyl group is preferably a (meth)acrylate having a branched alkyl group with a carbon number of 3 to 20, and more preferably a (meth)acrylate having a branched alkyl group with a carbon number of 3 to 10. Examples of the (meth)acrylate having a branched alkyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate.

[0047] The (meth)acrylate having a cyclic alkyl group is preferably a (meth)acrylate having a cyclic alkyl group with a carbon number of 6 to 12. Examples of the cyclic alkyl group include a cyclic alkyl group having a monocyclic structure (e.g., a cycloalkyl group) and a cyclic alkyl group having a bridged ring structure (e.g., an adamantyl group, a norbornyl group, an isobornyl group).

[0048] Specific examples of the (meth)acrylate having a cyclic alkyl group with a monocyclic structure include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, and cyclododecyl (meth)acrylate. Specific examples of the (meth)acrylate having a cyclic alkyl group having a bridged ring structure include isobornyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0049] The (meth)acrylate having an aromatic group is preferably a (meth)acrylate having an aromatic group with 6 to 12 carbon atoms, and more preferably a (meth)acrylate having an aromatic group with 6 to 9 carbon atoms. Examples of the aromatic group include an aryl group, and may have a chain portion such as an alkylaryl group, an aralkyl group, or an aryloxyalkyl group. Specific examples of the (meth)acrylate having an aromatic group include benzyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate.

[0050] Examples of the (meth)acrylate having an alkoxy group include methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate.

[0051] Examples of the (meth)acrylate having a cyclic ether group include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, tetrahydrofuranyl methoxyethyl (meth)acrylate, tetrahydrofuranyl methoxypropyl (meth)acrylate, tetrahydrofuranyl methoxyisopropyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, 2-[(2-tetrahydropyranyl)oxy]ethyl (meth)acrylate, and (1,3-dioxolan-4-yl)methyl (meth)acrylate.

[0052] The acidic group includes a carboxy group (-COOH), a sulfonic acid group (-SO 3 H), phosphate group (-OPO 3 H 2 ), phosphonic acid group (-PO 3 H 2 ), phosphinic acid group (-PO 2 H 2Examples of the (meth)acrylate having an acidic group include a (meth)acrylate having a carboxy group, a (meth)acrylate having a phosphoric acid group, and a (meth)acrylate having a sulfonic acid group.

[0053] Examples of the (meth)acrylate having a carboxy group include monomers obtained by reacting (meth)acrylates having a hydroxy group, such as carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate, and 2-(meth)acryloyloxyethyl phthalate, with acid anhydrides, such as maleic anhydride, succinic anhydride, and phthalic anhydride. Examples of the (meth)acrylate having a phosphoric acid group include 2-(phosphonooxy)ethyl (meth)acrylate. Examples of the (meth)acrylate having a sulfonic acid group include ethyl sulfonate (meth)acrylate.

[0054] Examples of the α-olefin include 1-hexene, 1-octene, and 1-decene. Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, 4-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methoxystyrene, 2-hydroxymethylstyrene, and 1-vinylnaphthalene. The vinyl monomer containing a heterocycle includes 2-vinylthiophene and the like. Examples of the vinyl amide include N-vinylformamide and N-vinylacetamide. Examples of the vinyl carboxylate include vinyl acetate, vinyl pivalate, and vinyl benzoate. Examples of dienes include butadiene, isoprene, 4-methyl-1,4-hexadiene, and 7-methyl-1,6-octadiene.

[0055] (Structural unit (a-2)) The A block preferably has, as the structural unit (a-2), a structural unit derived from one or more vinyl monomers selected from the group consisting of (meth)acrylates having a chain alkyl group, (meth)acrylates having a cyclic alkyl group, and (meth)acrylates having an aromatic group.

[0056] The structural unit (a-2) is preferably a structural unit represented by the formula (5).

[0057] [ka] [In formula (5), R 51 represents an alkyl group having 1 to 20 carbon atoms or an aromatic hydrocarbon group having 6 to 20 carbon atoms. R 52 represents a hydrogen atom or a methyl group.

[0058] R 51 The alkyl group having 1 to 20 carbon atoms represented by the formula (I) may be either a chain alkyl group or an alkyl group having a cyclic structure. R 51 The chain alkyl group represented by the formula: preferably has 1 to 10 carbon atoms, and more preferably has 1 to 5 carbon atoms. R 51 The alkyl group having a cyclic structure represented by the following formula (I) preferably has 4 to 18 carbon atoms, more preferably 6 to 12 carbon atoms, and further preferably 6 to 10 carbon atoms.

[0059] R 51 Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms represented by the formula (I) include an aryl group which may have a substituent and an aralkyl group which may have a substituent. R 51 The number of carbon atoms in the aryl group which may have a substituent represented by the following formula (I) is preferably 6 to 12, and more preferably 6 to 8. Examples of the substituent in the aryl group include an alkyl group having 1 to 5 carbon atoms. R 51The number of carbon atoms in the aralkyl group which may have a substituent represented by the following formula (I) is preferably 6 to 12, and more preferably 6 to 8. Examples of the substituent in the aralkyl group include an alkyl group having 1 to 5 carbon atoms.

[0060] When the A block contains the structural unit (a-2), the content of the structural unit (a-2) in 100 mol% of the structural units constituting the A block is preferably 5 mol% or more, more preferably 30 mol% or more, even more preferably 50 mol% or more, particularly preferably 60 mol% or more, and is preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 80 mol% or less. If the content of the structural unit (a-2) is 5 mol% or more, the affinity to the dispersion medium is further increased, and the solubility in an alkaline developer is further increased, and the alkaline developability of the colored composition can be further improved. If the content is 95 mol% or less, the affinity to the dispersion medium is further increased, and the dispersibility can be further improved.

[0061] When the A block contains the structural unit (a-2), the total content of the structural unit (a-1) and the structural unit (a-2) in 100 mol % of the structural units constituting the A block is preferably 80 mol % or more, more preferably 90 mol % or more, and even more preferably 98 mol % or more. If the total content is 80 mol % or more, the affinity to the dispersion medium is further increased, and the dispersibility can be further improved.

[0062] The A block may have a structural unit derived from a vinyl monomer having an acidic group (preferably a (meth)acrylate or (meth)acrylic acid having an acidic group). By having a structural unit derived from a vinyl monomer having an acidic group, the solubility in an alkaline developer is increased, and the alkaline developability of the colored composition can be improved.

[0063] When a structural unit derived from a vinyl monomer having an acidic group is contained, the content thereof is preferably 2 mol % or more and preferably 20 mol % or less in 100 mol % of the structural units constituting the A block. If the content of the structural unit derived from a vinyl monomer having an acidic group is 2 mol % or more, the dissolution rate when neutralized with alkali in alkaline development becomes high, and if it is 20 mol % or less, the hydrophilicity is not too high, and it is possible to prevent the formed pixels from becoming disordered.

[0064] The content of the structural unit (b-1) described below in 100 mol % of the structural units constituting the A block is 3 mol % or less, more preferably 2 mol % or less, and further preferably 1 mol % or less. If the content of the structural unit (b-1) in the A block is 3 mol % or less, it acts as an efficient compatible site that does not contribute to adsorption to the colorant.

[0065] When two or more types of structural units are contained in the A block, the various structural units contained in the A block may be contained in the A block in any form such as random copolymerization, block copolymerization, etc., and from the viewpoint of uniformity, it is preferable that they are contained in the A block in the form of random copolymerization. For example, the A block may be formed of a copolymer of structural units consisting of the a1 block and structural units consisting of the a2 block.

[0066] (Block B) The B block contains a structural unit (b-1) having a nitrogen-containing functional group. The structural unit (b-1) may be used alone or in combination of two or more kinds. The B block has a high affinity with the functional groups present on the surface of the colorant, and can impart good dispersibility.

[0067] The content of the structural unit (b-1) in 100 mol% of the structural units constituting the B block is preferably 5 mol% or more, more preferably 40 mol% or more, even more preferably 60 mol% or more, and is preferably 100 mol% or less, more preferably 95 mol% or less, even more preferably 90 mol% or less. If the content of the structural unit (b-1) is within the above range, the colorant is easily adsorbed by the B block.

[0068] The nitrogen-containing functional group includes an amino group, a nitrogen-containing heterocyclic group, an amide group, a cyano group, and the like. Among these, an amino group or a nitrogen-containing heterocyclic group is preferable. In this specification, an amino group means a general amino group (-NH 2 ) plus -NHR, where H is replaced by a hydrocarbon group. a , -NR a R b (R a , R b each independently represents a linear or cyclic hydrocarbon group.) The nitrogen-containing heterocyclic group includes aromatic heterocyclic groups such as a 4-pyridyl group, a 1-imidazole group, a 2-pyridyl group, and a 9-carbazole group; and non-aromatic heterocyclic groups such as a 1-piperidyl group, a 4-morpholino group, a 1-pyrrolidyl group, a pyrrolidone group, a methylpyrrolidone group, an ethylpyrrolidone group, a propylpyrrolidone group, and a butylpyrrolidone group.

[0069] The structural unit (b-1) may be, for example, a structure derived from a vinyl monomer having a nitrogen-containing functional group. The structural unit (b-1) is preferably a structural unit represented by formula (6) and / or a structural unit represented by formula (7).

[0070] [ka] [In formula (6), R 61 represents a hydrogen atom or a methyl group. A 61 represents an ester group, an amide group, or a single bond. R 62represents a divalent hydrocarbon group. R 63 and R 64 each independently represents a hydrogen atom or a linear or cyclic hydrocarbon group which may have a substituent.

[0071] The above A 61 represents an ester group (-CO-O-), an amide group (-CO-NH-) or a single bond, and an ester group or an amide group is preferable. The bonding direction of the ester group or the amide group is not particularly limited. The bonding mode of the ester group is C-CO-OR. 62 or CO-CO-R 62 C-CO-OR 62 The bonding form of the amide group is preferably C-CO-NH-R. 62 or C-NH-CO-R 62 C-CO-NH-R 62 is preferred.

[0072] R 62 Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 10 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, and an arenediyl group having 6 to 10 carbon atoms. Among these, an alkylene group having 1 to 10 carbon atoms is preferred. The alkylene group may be either linear or branched, but linear is preferred. The number of carbon atoms in the alkylene group is more preferably 1 to 4. Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0073] R 63 and R 64Examples of the chain-like hydrocarbon group represented by the formula (I) include linear alkyl groups and branched alkyl groups. The linear alkyl group preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 1 to 5 carbon atoms. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-hexyl, n-octyl, n-nonyl, n-decyl, and n-lauryl groups. The branched alkyl group preferably has 3 to 20 carbon atoms, more preferably 3 to 10 carbon atoms, and even more preferably 3 to 5 carbon atoms. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, 2-ethylhexyl, neopentyl, and isooctyl groups.

[0074] R 63 and R 64 The substituents of the chain hydrocarbon group represented by the formula (I) include halogen groups, alkoxy groups, and benzoyl groups (-COC 6 H 5 ), hydroxyl groups, etc.

[0075] R 63 and R 64 Examples of the cyclic hydrocarbon group represented by the formula (I) include a cyclic alkyl group and an aromatic group, and the cyclic alkyl group and the aromatic group may have a chain portion. The number of carbon atoms of the cyclic alkyl group is preferably 4 to 18, more preferably 6 to 12, and even more preferably 6 to 10. Examples of the cyclic alkyl group include a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. The number of carbon atoms of the aromatic group is preferably 6 to 18, more preferably 6 to 12, and even more preferably 6 to 8. Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a mesityl group. Examples of the cyclic alkyl group having a chain portion and the chain portion of the aromatic group having a chain portion include an alkylene group having 1 to 12 carbon atoms, preferably an alkylene group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms.

[0076] R63 and R 64 Examples of the substituent that the cyclic hydrocarbon group represented by the formula (I) has include a halogen group, an alkoxy group, a chain alkyl group, and a hydroxy group.

[0077] Specific examples of vinyl monomers that form the structural unit represented by formula (6) include 2-(dimethylamino)ethyl (meth)acrylate, 3-(dimethylamino)propyl (meth)acrylate, 4-(dimethylamino)butyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, 3-(diethylamino)propyl (meth)acrylate, 4-(diethylamino)butyl (meth)acrylate, 2-(ethylamino)ethyl (meth)acrylate, 3-(ethylamino)propyl (meth)acrylate, 4-(ethylamino)butyl (meth)acrylate, 2-(propylamino)ethyl (meth)acrylate, 3-(propylamino)propyl (meth)acrylate, 4-(propylamino)butyl (meth)acrylate, and (meth)acrylamide.

[0078] In the structural unit represented by formula (6), a part of the amino group may form a salt. Examples of the salt of the amino group include inorganic salts such as halide salts (F, Cl, Br, I, etc.) and sulfate salts of the amino group; and sulfonate, sulfate, phosphate, or carboxylate salts of organic compounds. In this specification, examples of the salt of the amino group include quaternary ammonium groups (-NH 4 + , -NR 4 + etc.) salts (e.g., halides, etc.) of the above-mentioned compounds are also included.

[0079] [ka] [In formula (7), R 71 , R 72 , R 73 and R 74 are the same or different and represent a hydrogen atom or an optionally substituted alkyl group having 1 to 10 carbon atoms. m7 represents an integer of 0 to 4. n7 represents an integer from 1 to 3.

[0080] R 71 ~R 74 The number of carbon atoms in the alkyl group in R is preferably 1 to 6, and more preferably 1 to 4. The alkyl group is further preferably a methyl group or an ethyl group, and particularly preferably a methyl group. 71 ~R 74 The substituent in is not particularly limited, but examples thereof include a carboxy group, a sulfonic acid group, and esters and salts thereof; an amino group; and a hydroxy group.

[0081] R 71 is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. R 72 ~R 74 is preferably a hydrogen atom. The above m7 is preferably an integer of 0 to 2, more preferably an integer of 0 to 1, and further preferably 0. The n7 is preferably 1 or 2, and more preferably 1.

[0082] Examples of the vinyl monomer forming the structural unit represented by the formula (7) include vinyl monomers having a 5-membered ring lactam group such as N-vinylpyrrolidone, N-vinyl-5-methylpyrrolidone, N-vinyl-5-ethylpyrrolidone, N-vinyl-5-propylpyrrolidone, N-vinyl-5-butylpyrrolidone, and 1-(2-propenyl)-2-pyrrolidone; vinyl monomers having a 6-membered ring lactam group such as N-vinylpiperidone; and vinyl monomers having a 7-membered ring lactam group such as N-vinylcaprolactam. The vinyl monomer forming the structural unit represented by the formula (7) can be one or more. Among these, vinyl monomers having a 5-membered ring lactam group are preferred, and N-vinylpyrrolidone is more preferred.

[0083] The molar volume of the structural unit (b-1) is 60 cm 3 / mol or more is preferable, and 80cm is more preferable. 3 / mol or more, preferably 100cm 3 / mol or more, 200cm 3 / mol or less is preferable, and 180cm 3 / mol or less, more preferably 150cm 3 When the molar volume of the structural unit (b-1) is within the above range, efficient adsorption to the colorant is achieved.

[0084] The B block may contain other structural units than the structural unit (b-1). Specific examples of vinyl monomers capable of forming the other structural units of the B block include the same as those exemplified as specific examples of monomers capable of forming the A block. As the other structural units, structural units derived from (meth)acrylic vinyl monomers are preferred.

[0085] The content of structural units having a hydroxy group and / or an ether group in 100 mol % of structural units constituting the B block is 4 mol % or less, more preferably 2 mol % or less, and further preferably 1 mol % or less.

[0086] When two or more types of structural units are contained in the B block, the various structural units contained in the B block may be contained in the B block in any form such as random copolymerization, block copolymerization, etc., and from the viewpoint of uniformity, it is preferable that they are contained in the B block in the form of random copolymerization. For example, the B block may be formed of a copolymer of structural units consisting of the b1 block and structural units consisting of the b2 block.

[0087] (C Block) The C block contains a structural unit (c-1) having a hydroxyl group. The structural unit (c-1) may be used alone or in combination of two or more. The C block has a high affinity with the dispersion medium and acts as a compatible site.

[0088] The content of the structural unit (c-1) in 100 mol% of the structural units constituting the C block is preferably 40 mol% or more, more preferably 50 mol% or more, and even more preferably 90 mol% or more. If the content of the structural unit (c-1) is 40 mol% or more, it is easily compatible with the dispersion medium and effectively functions as a compatible portion.

[0089] The molar volume ratio ((c-1) / (b-1)) of the structural unit (c-1) to the structural unit (b-1) in the B block is 0.1 or more, preferably 0.2 or more, more preferably 0.4 or more, and 1.5 or less, preferably 1.2 or less, more preferably 0.9 or less, and more preferably 0.7 or less. If the molar volume ratio ((c-1) / (b-1)) is within the above range, the C block does not interfere with the adsorption of the B block, and effectively blends with the solvent and acts as a compatible site, thereby suppressing aggregation between colorant particles. When the B block contains multiple types of structural units (b-1), the molar volume ratio is calculated as the ratio to the molar volume of the structural unit (b-1) with the highest content.

[0090] The C block may contain a structural unit (c-1) having a molar volume ratio ((c-1) / (b-1)) outside the above range. The content of structural units having a molar volume ratio ((c-1) / (b-1)) within the above range in 100 mol% of structural units (c-1) contained in the C block is preferably 50 mol% or more, more preferably 90 mol% or more, and even more preferably 100 mol%.

[0091] (Structural unit (c-1)) The structural unit (c-1) is preferably a structural unit represented by the formula (8).

[0092] [ka] [In formula (8), R 81 represents a hydrogen atom or a methyl group. A 81 represents an ester group, an amide group, or a single bond. R 82is a divalent hydrocarbon group, -R 83 -(O-CO-R 84 ) m8 -group or -R 85 -(OR 86 ) n8 - represents a group. m8 represents an integer from 1 to 10. R 83 represents a divalent hydrocarbon group. R 84 represents a divalent hydrocarbon group, and when m8 is 2 or more, a plurality of R 84 may be the same or different. n8 represents an integer from 1 to 30. R 85 represents a divalent hydrocarbon group. R 86 represents a divalent hydrocarbon group, and when n8 is 2 or more, multiple R 86 may be the same or different.]

[0093] The above A 81 represents an ester group (-CO-O-), an amide group (-CO-NH-) or a single bond, and is preferably an ester group or an amide group, more preferably an ester group. The bonding direction of the ester group or the amide group is not particularly limited. The bonding mode of the ester group is C-CO-OR 82 or CO-CO-R 82 C-CO-OR 82 The bonding form of the amide group is preferably C-CO-NH-R. 82 or C-NH-CO-R 82 C-CO-NH-R 82 is preferred.

[0094] R 82Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 20 carbon atoms, an alkenylene group having 2 to 20 carbon atoms, and an arenediyl group having 6 to 20 carbon atoms. Among these, an alkylene group having 1 to 20 carbon atoms is preferred. The alkylene group may be either linear or branched, but linear is preferred. The number of carbon atoms in the alkylene group is more preferably 1 to 4. Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0095] R 82 Represented by -R 83 -(O-CO-R 84 ) m8 -group or -R 85 -(OR 86 ) n8 In the -group, R 83 , R 84 , R 85 or R 86 Examples of the divalent hydrocarbon group represented by the formula (I) include an alkylene group having 1 to 20 carbon atoms, an alkenylene group having 2 to 20 carbon atoms, and an arenediyl group having 6 to 20 carbon atoms. 83 , R 84 , R 85 or R 86 The divalent hydrocarbon group represented by the following formula is preferably an alkylene group having 1 to 20 carbon atoms.

[0096] The C block may contain a structural unit other than the structural unit (c-1). Specific examples of vinyl monomers capable of forming the other structural units of the C block include the same monomers as those exemplified as specific examples of monomers capable of forming the A block and the B block. As the other structural units, structural units derived from (meth)acrylic vinyl monomers are preferred.

[0097] The content of the structural unit (b-1) in 100 mol % of the structural units constituting the C block is 3 mol % or less, more preferably 2 mol % or less, and further preferably 1 mol % or less. If the content of the structural unit (b-1) in the C block is 3 mol % or less, it acts as an efficient compatible site that does not contribute to adsorption to the colorant.

[0098] When two or more types of structural units are contained in the C block, the various structural units contained in the C block may be contained in the C block in any form such as random copolymerization or block copolymerization, and from the viewpoint of uniformity, it is preferable that they are contained in the C block in the form of random copolymerization. For example, the C block may be formed of a copolymer of a structural unit consisting of a c1 block and a structural unit consisting of a c2 block.

[0099] (Block Copolymer) The structure of the block copolymer is a linear block copolymer, and the arrangement of the blocks is A block-B block-C block in this order. It is believed that the presence of the A block and the B block allows the structural unit (a-1) of the A block and the structural unit (b-1) of the B block to be localized, and thus allows them to effectively interact with the colorant, the dispersion medium, and the binder resin. Furthermore, the presence of the C block enhances the effect of the compatible portion without interfering with the action of the B block, improving the viscosity stability of the coloring composition.

[0100] The block copolymer may have other blocks than the A block, the B block, and the C block, so long as the effects of the present invention are not impaired. In addition, another block may be present between the A block and the B block, or another block may be present between the B block and the C block. The block copolymer is preferably a triblock copolymer in which the block is arranged in the order of the A block, the B block, and the C block.

[0101] In all structural units constituting the block copolymer, the total molar content of the structural units constituting the A block is preferably 15 mol% or more, more preferably 20 mol% or more, even more preferably 25 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, even more preferably 60 mol% or less. If the total molar content of the structural units constituting the A block is 15 mol% or more, the structural units will be more compatible with the dispersion medium, and if it is 80 mol% or less, the structural units will be more likely to act as a compatible moiety.

[0102] In all structural units constituting the block copolymer, the total molar content of the structural units constituting the B block is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 15 mol% or more, and is preferably 70 mol% or less, more preferably 60 mol% or less, even more preferably 50 mol% or less. If the total molar content of the structural units constituting the B block is 5 mol% or more, multipoint adsorption to the colorant can be achieved, and if it is 70 mol% or less, bridging adsorption between colorant particles can be prevented.

[0103] In all structural units constituting the block copolymer, the total molar content of the structural units constituting the C block is preferably 15 mol% or more, more preferably 20 mol% or more, even more preferably 25 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, even more preferably 60 mol% or less. If the total molar content of the structural units constituting the C block is 15 mol% or more, the structural units will be more compatible with the dispersion medium, and if it is 80 mol% or less, they will more easily function as a compatible site.

[0104] In the block copolymer, the molar ratio of the total molar amount of the structural units constituting the A block to the total molar amount of the structural units constituting the B block (A block / B block) is preferably 10 / 90 or more, more preferably 20 / 80 or more, and even more preferably 40 / 60 or more, and is preferably 95 / 5 or less, more preferably 90 / 10 or less, and even more preferably 80 / 20 or less. If the molar ratio (A block / B block) is 10 / 90 or more, the A block is more likely to function as a compatible site, and aggregation between colorant particles can be more effectively suppressed, while if it is 95 / 5 or less, the B block is more likely to be adsorbed to the colorant, and dispersibility can be further improved.

[0105] In the block copolymer, the molar ratio of the total molar amount of the structural units constituting the C block to the total molar amount of the structural units constituting the B block (C block / B block) is preferably 10 / 90 or more, more preferably 20 / 80 or more, and even more preferably 40 / 60 or more, and is preferably 95 / 5 or less, more preferably 90 / 10 or less, and even more preferably 80 / 20 or less. If the molar ratio (C block / B block) is 10 / 90 or more, the C block can easily act as a compatible site, and aggregation between colorant particles can be further suppressed, and if it is 20 / 80 or less, the B block can be adsorbed to the colorant and dispersibility can be improved.

[0106] The weight average molecular weight (Mw) of the block copolymer is preferably 5,000 or more, more preferably 8,000 or more, even more preferably 10,000 or more, and is preferably 40,000 or less, more preferably 30,000 or less, even more preferably 20,000 or less. If the weight average molecular weight is within the above range, the dispersion performance when used as a dispersant is improved. The molecular weight of the block copolymer is measured by gel permeation chromatography (hereinafter referred to as "GPC") method.

[0107] The molecular weight distribution (Mw / Mn) of the block copolymer is preferably less than 3.0, more preferably 2.0 or less, and even more preferably 1.5 or less. If the molecular weight distribution (Mw / Mn) is less than 3.0, the dispersion performance when used as a dispersant will be better. The molecular weight distribution is calculated by (weight average molecular weight (Mw) of the block copolymer) / (number average molecular weight (Mn) of the block copolymer). The smaller the value of the molecular weight distribution, the narrower the width of the molecular weight distribution, which means the copolymer has a uniform molecular weight, and when the value is 1.0, the width of the molecular weight distribution is the narrowest. In other words, the lower limit of the molecular weight distribution is 1.0.

[0108] From the viewpoint of adsorption to a colorant and dispersibility of a colorant, the amine value of the block copolymer is preferably 10 mgKOH / g or more, more preferably 25 mgKOH / g or more, and even more preferably 55 mgKOH / g or more, and is preferably 150 mgKOH / g or less, more preferably 120 mgKOH / g or less, and even more preferably 100 mgKOH / g or less.

[0109] When the block copolymer contains a structural unit having an acidic group, the block copolymer preferably has an acid value of 5 mgKOH / g or more and 50 mgKOH / g or less. By setting the acid value within this range, the block copolymer can act favorably with the binder resin (alkali-soluble resin) without impairing the affinity of the block copolymer with the colorant.

[0110] (Method of Producing Block Copolymer) Examples of the method for producing the block copolymer include a method in which an A block is first produced by a polymerization reaction of a vinyl monomer, a monomer for a B block is polymerized onto the A block, and a monomer for a C block is polymerized onto the B block; a method in which a C block is first produced, a monomer for a B block is polymerized onto the C block, and a monomer for an A block is polymerized onto the B block, etc. When the structural unit (b-1) is a structural unit represented by formula (6), the method may include a step of quaternizing a part of the tertiary amine structures of the structural unit (b-1) in the obtained polymer.

[0111] Although the polymerization method is not particularly limited, living polymerization is preferred, that is, the block copolymer is preferably one polymerized by living polymerization. Among the four elementary reactions in chain polymerization, namely, initiation reaction, propagation reaction, termination reaction, and chain transfer reaction, living polymerization is substantially free of side reactions such as termination reaction and chain transfer reaction, and the vinyl monomer reacts and the polymer chain grows without deactivating the reaction point (polymerization growth end), so that it is easy to produce a polymer with a narrow molecular weight distribution and uniform composition. Living polymerization includes living radical polymerization, living anionic polymerization, living cationic polymerization, and the like. Among these, living radical polymerization is preferable from the viewpoint of the simplicity of polymerization. In addition, living radical polymerization is preferable in that it is difficult to cause termination reaction or chain transfer reaction, and the growth end grows without being deactivated, while maintaining the simplicity and versatility of conventional radical polymerization, so that it is easy to precisely control the molecular weight distribution and produce a polymer with a uniform composition.

[0112] Living radical polymerization includes a method using a compound capable of generating a nitroxide radical (nitroxide method; NMP method) depending on the method of stabilizing the polymer growth terminal; a method using a metal complex such as copper or ruthenium to polymerize a halogenated compound as a polymerization initiator compound in a living manner from the polymerization initiator compound (ATRP method); a method using a dithiocarboxylate or xanthate compound (RAFT method); a method using an organic tellurium compound (TERP method); a method using an organic iodine compound (ITP method); a method using an iodine compound as a polymerization initiator compound and an organic compound such as a phosphorus compound, a nitrogen compound, an oxygen compound, or a hydrocarbon as a catalyst (reversible transfer catalyst polymerization; RTCP method, reversible catalyst-mediated polymerization; RCMP method), etc. Among these methods, the TERP method is preferable from the viewpoint of the diversity of monomers that can be used, molecular weight control in the polymer region, uniform composition, or coloring.

[0113] The TERP method is a method in which an organic tellurium compound is used as a chain transfer agent to polymerize a radically polymerizable compound (vinyl monomer), and is described, for example, in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, WO 2004 / 096870, and WO 2020 / 116144.

[0114] Specific polymerization methods of the TERP method include the following (a) to (d). (a) A method of polymerizing a vinyl monomer using an organotellurium compound represented by formula (T1). (b) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (T1) and an azo-based polymerization initiator. (c) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (T1) and an organoditelluride compound represented by formula (T2). (d) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (T1), an azo-based polymerization initiator, and an organoditelluride compound represented by formula (T2).

[0115] [ka] [In formula (T1), R a R represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group. b and R c R each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. d represents an alkyl group having 1 to 8 carbon atoms, an aryl group, a substituted aryl group, an aromatic heterocyclic group, an alkoxy group, an acyl group, an amido group, an oxycarbonyl group, a cyano group, an allyl group, or a propargyl group. In formula (T2), R a represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group.]

[0116] Specific examples of the organic tellurium compound represented by formula (T1) include ethyl 2-methyl-2-n-butyltellanyl-propionate, ethyl 2-n-butyltellanyl-propionate, (2-hydroxyethyl) 2-methyl-methyltellanyl-propionate, and the organic tellurium compounds described in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, WO 2004 / 096870, and WO 2020 / 116144. Specific examples of the organic ditelluride compound represented by formula (T2) include dimethyl ditelluride, dibutyl ditelluride, and the like. The azo polymerization initiator can be any azo polymerization initiator used in normal radical polymerization without any particular limitation. Examples of the azo polymerization initiator include 2,2'-azobis(isobutyronitrile) (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1'-azobis(1-cyclohexanecarbonitrile) (ACHN), dimethyl-2,2'-azobisisobutyrate (MAIB), 4,4'-azobis(4-cyanovaleric acid) (ACVA), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (V-70), and 2,2'-azobis(N-butyl-2-methylpropionamide) (VAm-110).

[0117] In the polymerization step, a vinyl monomer and an organic tellurium compound of formula (T1) are mixed in a vessel purged with an inert gas, and for the purpose of promoting the reaction and controlling the molecular weight and molecular weight distribution according to the type of vinyl monomer, an azo-based polymerization initiator and / or an organic ditelluride compound of formula (T2) are further mixed. Examples of the inert gas include nitrogen, argon, and helium. Argon and nitrogen are preferable. The amount of the vinyl monomer used in the above (a), (b), (c), and (d) may be appropriately adjusted depending on the physical properties of the desired copolymer.

[0118] The polymerization reaction can be carried out without a solvent, but may be carried out by stirring the mixture using an aprotic solvent or a protic solvent generally used in radical polymerization. Examples of aprotic solvents that can be used include acetonitrile, methyl ethyl ketone, anisole, benzene, toluene, propylene glycol monomethyl ether acetate, ethyl acetate, tetrahydrofuran (THF), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP), acetone, dioxane, chloroform, and carbon tetrachloride. Examples of protic solvents include water, methanol, ethanol, isopropanol, n-butanol, ethyl cellosolve, butyl cellosolve, 1-methoxy-2-propanol, hexafluoroisopropanol, and diacetone alcohol. The solvent may be used alone or in combination of two or more kinds. The amount of the solvent used may be appropriately adjusted, and is preferably 0.01 ml to 50 ml per 1 g of vinyl monomer, for example. In the polymerization reaction, a surfactant and / or a dispersant may be used in addition to the solvent. The reaction temperature and reaction time may be appropriately adjusted depending on the molecular weight or molecular weight distribution of the copolymer to be obtained, but the reaction is usually performed at 0°C to 150°C for 1 minute to 100 hours with stirring. The pressure is usually normal pressure, but it may be increased or decreased. The polymerization reaction may be performed by irradiating light. After the polymerization reaction is completed, the solvent used and the remaining vinyl monomer are removed from the reaction mixture obtained by a conventional separation and purification means, and the target copolymer can be separated.

[0119] The growing end of the copolymer obtained by the polymerization reaction is -TeR derived from the tellurium compound. a (In the formula, R ais the same as above), and is deactivated by handling in air after the polymerization reaction is completed, but tellurium atoms may remain. Since copolymers with tellurium atoms remaining at the terminals are colored and have poor thermal stability, it is preferable to remove the tellurium atoms. Methods for removing tellurium atoms include radical reduction methods, adsorption methods using activated carbon, and adsorption of metals using ion exchange resins, and these methods can also be used in combination. The other end of the copolymer obtained by the polymerization reaction (the end opposite to the growing end) is formed of -CR derived from the tellurium compound. b R c R d (In the formula, R b , R c and R d is R in formula (T1). b , R c and R d ) Therefore, the copolymer obtained by the TERP method does not have a substituent containing a sulfur atom at the end.

[0120] When the tertiary amine group of the structural unit (b-1) is quaternized, examples of the quaternizing agent include alkyl halides such as methyl chloride, ethyl chloride, methyl bromide, and methyl iodide; aralkyl halides such as benzyl chloride, benzyl bromide, and benzyl iodide; diaryl sulfates such as diphenyl sulfate; dialkyl sulfates such as dimethyl sulfate, diethyl sulfate, and di-n-propyl sulfate; and aromatic alkyl sulfonates such as methyl p-toluenesulfonate and ethyl p-toluenesulfonate. Among these, preferred are aralkyl halides such as benzyl chloride, benzyl bromide, and benzyl iodide, dialkyl sulfates such as dimethyl sulfate, diethyl sulfate, and di-n-propyl sulfate, and aromatic alkyl sulfonates such as methyl p-toluenesulfonate and ethyl p-toluenesulfonate, and more preferred are benzyl chloride, dimethyl sulfate, and methyl p-toluenesulfonate. Into the structure after quaternization, an alkyl group or aralkyl group derived from the quaternizing agent is introduced.

[0121] As a method for quaternizing a part of the tertiary amine structures of the structural units having a basic group in the polymer, a method of contacting the polymer with a quaternizing agent can be mentioned. Specifically, a method of polymerizing a monomer composition containing a vinyl monomer capable of forming a structural unit having a basic group, adding a quaternizing agent to the reaction liquid, and stirring the reaction liquid can be mentioned. The temperature of the reaction liquid to which the quaternizing agent is added is preferably 55°C to 65°C, and the stirring time is preferably 5 hours to 20 hours.

[0122] <Dispersant> The dispersant of the present invention contains the block copolymer. The dispersant preferably contains the block copolymer as a main component (50% by mass or more). The block copolymer exerts an effect of enhancing the dispersibility of the colorant by adsorbing the nitrogen-containing functional group in the structure (B block) to the colorant. In other words, the dispersant of the present invention is a component that disperses the colorant well by this effect, so there is no particular limitation on the type of colorant to be dispersed. The dispersant of the present invention has high dispersibility for coloring materials and can be suitably used as a dispersant for colored compositions for color filters. In addition, since the dispersant of the present invention has high dispersibility for colorants, it can also be used in inkjet inks, printing inks, inks for writing instruments, paints, etc. By appropriately changing the composition of the block copolymer, it can be used not only in coloring compositions using organic solvents, but also in coloring compositions using aqueous solvents.

[0123] The content of the block copolymer in the dispersant is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more. The dispersant may be composed of only the block copolymer.

[0124] <Coloring composition> The coloring composition of the present invention contains the dispersant, a colorant, and a dispersion medium. The coloring composition is suitable for use in forming a color layer of a color filter.

[0125] (Coloring material) The type and particle size of the coloring material may be appropriately selected according to the application, and are not particularly limited. The coloring composition preferably contains a pigment as a coloring material. The pigment may be either an organic pigment or an inorganic pigment, but an organic pigment mainly composed of an organic compound is particularly preferred. Examples of the pigment include red pigments, yellow pigments, orange pigments, blue pigments, green pigments, purple pigments, and other pigments of various colors. The structure of the pigment may include azo pigments such as monoazo pigments, diazo pigments, and condensed diazo pigments, diketopyrrolopyrrole pigments, phthalocyanine pigments, isoindolinone pigments, isoindoline pigments, quinacridone pigments, indigo pigments, thioindigo pigments, quinophthalone pigments, dioxazine pigments, anthraquinone pigments, perylene pigments, and polycyclic pigments such as perinone pigments. The pigment contained in the coloring composition may be only one type or multiple types.

[0126] Specific examples of pigments include red pigments such as CI Pigment Red 7, 9, 14, 41, 48:1, 48:2, 48:3, 48:4, 81:1, 81:2, 81:3, 122, 123, 146, 149, 168, 177, 178, 179, 187, 200, 202, 208, 210, 215, 224, 254, 255, 264, and 291; and CI Pigment Yellow Yellow pigments such as 1, 3, 5, 6, 14, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 93, 97, 98, 104, 108, 110, 138, 139, 147, 150, 151, 154, 155, 166, 167, 168, 170, 180, 185, 188, 193, 194, 213; orange pigments such as CI Pigment Orange 36, 38, 43; blue pigments such as CI Pigment Blue 15, 15:2, 15:3, 15:4, 15:6, 16, 22, 60; CI Pigment Green green pigments such as 7, 36, 58, 59, 62, 63, aluminum phthalocyanine, polyhalogenated aluminum phthalocyanine, aluminum phthalocyanine hydroxide, diphenoxyphosphinyloxyaluminum phthalocyanine, diphenylphosphinyloxyaluminum phthalocyanine, polyhalogenated diphenoxyphosphinyloxyaluminum phthalocyanine, and polyhalogenated diphenylphosphinyloxyaluminum phthalocyanine; purple pigments such as CI Pigment Violet 23, 32, and 50.Of these, preferred pigments are CI Pigment Red 177, CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 264, CI Pigment Red 291, CI Pigment Blue 15, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6, CI Pigment Blue 16, CI Pigment Green 7, CI Pigment Green 36, CI Pigment Green 58, CI Pigment Green 59, CI Pigment Green 62, Pigment Green 63, and the like.

[0127] The colorant may contain a dye derivative (synergist) as a dispersing aid. This improves the dispersibility of the colorant. The dye derivative is a dye skeleton into which an acidic group, a basic group, or a neutral group has been introduced, and preferably an acidic group or a neutral group has been introduced. Examples of the dye derivative include compounds having an acidic group such as a sulfonic acid group, a carboxy group, or a phosphoric acid group, and / or their amine salts; compounds having a basic substituent such as a sulfonic acid amide group or a tertiary amino group at the end; and compounds having a neutral substituent such as a phenyl group or a phthalimidoalkyl group. The dye skeleton is preferably the same or similar to the colorant constituting the coloring composition, or the same or similar to the compound serving as the raw material of the colorant. Specific examples of the dye skeleton include an azo-based dye skeleton, a phthalocyanine-based dye skeleton, an anthraquinone-based dye skeleton, a triazine-based dye skeleton, an acridine-based dye skeleton, and a perylene-based dye skeleton. The amount of the dye derivative used is not particularly limited, but is preferably 4 parts by mass to 17 parts by mass with respect to 100 parts by mass of the colorant, for example.

[0128] The upper limit of the content of the coloring material in the coloring composition is usually 80 mass%, preferably 70 mass%, more preferably 60 mass%, based on the total solid content of the coloring composition, from the viewpoint of brightness. The lower limit of the content of the coloring material in the coloring composition is usually 10 mass%, preferably 20 mass%, more preferably 30 mass%, based on the total solid content of the coloring composition. Here, the solid content refers to components other than the dispersion medium described below. The content of the dispersant relative to the colorant in the coloring composition is preferably 5 parts by mass to 200 parts by mass, more preferably 10 parts by mass to 100 parts by mass, and even more preferably 10 parts by mass to 80 parts by mass, relative to 100 parts by mass of the colorant. If the content of the dispersant is within the above range, the viscosity of the coloring composition becomes good.

[0129] (dispersion medium) The dispersion medium used in the present invention can be appropriately selected and used as long as it disperses or dissolves the other components constituting the coloring composition, does not react with these components, and has appropriate volatility. For example, a conventionally known organic solvent can be used, for example, a conventionally known organic solvent can be used, for example, glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-butyl ether, propylene glycol-t-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, methoxymethyl pentanol, dipropylene glycol monoethyl ether, dipropylene glycol monomethyl ether, 3-methyl-3-methoxybutanol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and tripropylene glycol methyl ether; glycol dialkyl ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, and dipropylene glycol dimethyl ether;Glycol alkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-butyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, methoxybutyl acetate, 3-methoxybutyl acetate, methoxypentyl acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol mono-n-butyl ether acetate, dipropylene glycol monomethyl ether acetate, triethylene glycol monomethyl ether acetate, triethylene glycol monoethyl ether acetate, 3-methyl-3-methoxybutyl acetate; glycol diacetates such as ethylene glycol diacetate, 1,3-butylene glycol diacetate, 1,6-hexanol diacetate; cyclohexanol diacetates; alkyl acetates such as xanol acetate; ethers such as amyl ether, propyl ether, diethyl ether, dipropyl ether, diisopropyl ether, butyl ether, diamyl ether, ethyl isobutyl ether, and dihexyl ether; acetone, methyl ethyl ketone, methyl amyl ketone, methyl isopropyl ketone, methyl isoamyl ketone, diisopropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclohexanone, ethyl amyl ketone, methyl butyl ketone, methyl hexyl ketone, methyl Ketones such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, propylene glycol, butanediol, diethylene glycol, dipropylene glycol, triethylene glycol, methoxypropanol, methoxymethylpentanol, glycerin, benzyl alcohol, and other monohydric or polyhydric alcohols; aliphatic hydrocarbons such as n-pentane, n-octane, diisobutylene, n-hexane, hexene, isoprene, dipentene, dodecane, and other aliphatic hydrocarbons;Alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, methylcyclohexene, and bicyclohexyl; aromatic hydrocarbons such as benzene, toluene, xylene, and cumene; amyl formate, ethyl formate, ethyl acetate, butyl acetate, propyl acetate, amyl acetate, methyl isobutyrate, ethylene glycol acetate, ethyl propionate, propyl propionate, butyl butyrate, isobutyl butyrate, methyl isobutyrate, ethyl caprylate, butyl stearate, ethyl benzoate, and 3-ethoxypropionate. Examples of the organic solvent include linear or cyclic esters such as methyl ester, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, and γ-butyrolactone; alkoxycarboxylic acids such as 3-methoxypropionic acid and 3-ethoxypropionic acid; halogenated hydrocarbons such as butyl chloride and amyl chloride; ether ketones such as methoxymethylpentanone; and nitriles such as acetonitrile and benzonitrile. From the viewpoints of dispersibility of colorants, solubility of dispersants, and coatability of the coloring composition, the organic solvent is preferably glycol alkyl ether acetates, glycol monoalkyl ethers, and monohydric or polyhydric alcohols. The dispersion medium contained in the coloring composition may be one type only or may be a plurality of types.

[0130] When forming pixels of a color filter by photolithography, the boiling point of the dispersion medium is preferably 100°C to 200°C (under a pressure condition of 1013.25 hPa. The same applies to all boiling points below), and more preferably 120°C to 170°C. Among the above dispersion media, glycol alkyl ether acetates are preferred because they have a good balance of application properties, surface tension, and the like, and the solubility of the components in the coloring composition is relatively high. The glycol alkyl ether acetates may be used alone or in combination with other dispersion media. It is also preferred to use a dispersion medium having a boiling point of 150°C or higher in combination. By using a dispersion medium having a high boiling point in combination, the destruction of the interrelationship of the coloring composition due to the rapid drying of the coloring composition can be suppressed. The dispersion medium having a boiling point of 150°C or higher may be a glycol alkyl ether acetate.

[0131] The content of the dispersion medium in the coloring composition is not particularly limited and can be adjusted appropriately. The upper limit of the content of the dispersion medium in the coloring composition is usually 99% by mass. The lower limit of the content of the dispersion medium in the coloring composition is usually 70% by mass, preferably 80% by mass, in consideration of the viscosity suitable for application of the coloring composition. The dispersion medium can be used as a solvent for dissolving and removing precipitates formed from the coloring composition.

[0132] (binder resin) The coloring composition may contain a binder resin (excluding the block copolymer). Examples of the binder resin include an alkali-soluble resin, a polymerizable compound (polymerizable resin, a monomer having one polymerizable unsaturated bond in the molecule, a monomer having two or more polymerizable unsaturated bonds in the molecule, an oligomer, etc.), a thermosetting resin, a thermoplastic resin, etc. These may be used alone or in a mixture of two or more kinds. Among these, an alkali-soluble resin and / or a polymerizable compound is preferable.

[0133] The content of the binder resin in the coloring composition is, in terms of the total amount of the binder resin used, preferably 1 mass% or more, more preferably 2 mass% or more, and even more preferably 5 mass% or more, of the total solid content of the coloring composition, and is preferably 70 mass% or less, more preferably 60 mass% or less, and even more preferably 50 mass% or less.

[0134] (alkali soluble resin) The alkali-soluble resin is not particularly limited as long as it acts as a binder for a colorant and is soluble in a developer, preferably an alkaline developer, used in the development process when producing a color filter. However, it is preferable that the resin is a resin having an acidic group such as a carboxy group or a phenolic hydroxy group.

[0135] Examples of the alkali-soluble resin include a resin obtained by adding an unsaturated monobasic acid to at least a portion of the epoxy groups in a copolymer of an epoxy group-containing (meth)acrylate and another radically polymerizable monomer, or a resin obtained by adding a polybasic acid anhydride to at least a portion of the hydroxyl groups produced by the addition reaction; a linear resin containing a carboxy group in the main chain; a resin in which an epoxy group-containing unsaturated compound is added to the carboxy group portion of a carboxy group-containing resin; a (meth)acrylic resin; and an epoxy (meth)acrylate resin having a carboxy group. These can be used alone or in combination of two or more kinds.

[0136] The alkali-soluble resin is preferably a random copolymer containing a structural unit derived from a carboxyl group-containing vinyl monomer, a structural unit derived from a (meth)acrylate, and styrene, a synthetic resin in which a (meth)acrylic group is introduced into an epoxy resin, or a random copolymer containing a structural unit derived from a carboxyl group-containing vinyl monomer and a structural unit derived from a (meth)acrylate. The carboxyl group-containing vinyl monomer is preferably (meth)acrylic acid. Examples of the (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycerol mono(meth)acrylate, glycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.

[0137] The alkali-soluble resin preferably has a total content of structural units derived from a carboxyl group-containing vinyl monomer and structural units derived from a (meth)acrylate of 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The alkali-soluble resin preferably has a total content of structures derived from a carboxyl group-containing vinyl monomer of 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, and preferably 90% by mass or less, and more preferably 70% by mass or less.

[0138] Among the above-mentioned alkali-soluble resins, a random copolymer of a carboxyl group-containing vinyl monomer and a (meth)acrylate is preferred. Specific examples of such copolymers include a random copolymer of (meth)acrylic acid and butyl (meth)acrylate, a random copolymer of (meth)acrylic acid and benzyl (meth)acrylate, and a random copolymer of (meth)acrylic acid, butyl (meth)acrylate, and benzyl (meth)acrylate. From the viewpoint of the affinity between the alkali-soluble resin and the colorant, the alkali-soluble resin is particularly preferably a random copolymer of (meth)acrylic acid and benzyl (meth)acrylate. In the copolymer of a carboxyl group-containing vinyl monomer and a (meth)acrylate, the content of (meth)acrylic acid is usually 5% by mass to 90% by mass, preferably 10% by mass to 70% by mass, and more preferably 20% by mass to 70% by mass, in the total monomer components. The polymerization method of these random copolymers is not particularly limited, but living polymerization is preferred from the viewpoint of alkali solubility.

[0139] The alkali-soluble resin may have a radically polymerizable carbon-carbon double bond in the side chain. By having a double bond in the side chain, the photocurability of the coloring composition according to the present invention is increased, so that the resolution and adhesion can be further improved. As a method for introducing a radically polymerizable carbon-carbon double bond in the side chain, for example, a method of reacting a compound such as glycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, or o-(or m-, or p-)vinylbenzyl glycidyl ether with the acidic group of the binder resin can be mentioned.

[0140] The Mw of the alkali-soluble resin is preferably 3,000 to 100,000, more preferably 5,000 to 50,000, and even more preferably 5,000 to 20,000. When the Mw of the alkali-soluble resin is 3,000 or more, the heat resistance, film strength, etc. of the colored layer formed from the colored composition become good, and when the Mw is 100,000 or less, the alkali developability of this coating film becomes even better.

[0141] The acid value of the alkali-soluble resin is preferably 20 mgKOH / g to 170 mgKOH / g, more preferably 50 mgKOH / g to 150 mgKOH / g, and even more preferably 90 mgKOH / g to 150 mgKOH / g. When the acid value of the alkali-soluble resin is 20 mgKOH / g or more, the alkali developability when the colored composition is used as a colored layer becomes even better, and when the acid value is 170 mgKOH / g or less, the heat resistance becomes good.

[0142] The coloring composition may contain only one type of alkali-soluble resin, or may contain multiple types. In the coloring composition, the content of the alkali-soluble resin is preferably 5 parts by mass to 200 parts by mass, more preferably 10 parts by mass to 100 parts by mass, and even more preferably 20 parts by mass to 80 parts by mass, relative to 100 parts by mass of the coloring material.

[0143] (polymerizable compound) Examples of the polymerizable compound include polymerizable resins (for example, resins in which a crosslinkable group such as a (meth)acrylic compound or cinnamic acid is introduced into a linear polymer having a reactive substituent such as a hydroxyl group, a carboxyl group, or an amino group via an isocyanate group, an aldehyde group, or an epoxy group), compounds having one polymerizable unsaturated bond in the molecule (for example, monofunctional (meth)acrylic monomers (alkyl (meth)acrylates, aralkyl (meth)acrylates, etc.)), and compounds having two or more polymerizable unsaturated bonds in the molecule (for example, polyfunctional (meth)acrylic monomers (di(meth)acrylates of dihydric alcohols, poly(meth)acrylates of trihydric or higher polyhydric alcohols, etc.)). Examples of the polymerizable unsaturated bond include carbon-carbon double bonds and carbon-carbon triple bonds. These can be used alone or in a mixture of two or more. Among these, compounds having two or more polymerizable unsaturated bonds in the molecule are preferred.

[0144] Examples of the monomer having two or more polymerizable unsaturated bonds in the molecule as the polymerizable compound include bisphenol A di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, glycerol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0145] The content of the polymerizable compound in the coloring composition is preferably 10 parts by mass to 1,000 parts by mass, more preferably 20 parts by mass to 500 parts by mass, based on 100 parts by mass of the coloring material. If the content of the polymerizable compound is within the above range, sufficient curability is obtained, and the alkali developability is also good. It is also preferable to use an alkali-soluble resin and a polymerizable compound in combination as the binder resin.

[0146] (thermosetting resin, thermoplastic resin) Examples of the thermosetting resin and thermoplastic resin include butyral resin, styrene-maleic acid copolymer, chlorinated polyethylene, chlorinated polypropylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, polyvinyl acetate, polyurethane resin, phenol resin, polyester resin, acrylic resin, alkyd resin, styrene resin, polyamide resin, rubber resin, cyclized rubber, epoxy resin, cellulose, polybutadiene, polyimide resin, benzoguanamine resin, melamine resin, and urea resin.

[0147] (Photopolymerization initiator) The coloring composition of the present invention may contain a photopolymerization initiator as necessary. This can impart radiation sensitivity to the coloring composition. The photopolymerization initiator is a compound that generates an active species that can initiate polymerization of a polymerizable compound by exposure to radiation such as visible light, ultraviolet light, far infrared light, electron beams, and X-rays.

[0148] Examples of the photopolymerization initiator include thioxanthone compounds, acetophenone compounds, biimidazole compounds, triazine compounds, O-acyloxime compounds, onium salt compounds, benzoin compounds, benzophenone compounds, α-diketone compounds, polynuclear quinone compounds, diazo compounds, imide sulfonate compounds, etc. The photopolymerization initiator can be used alone or in combination of two or more kinds.

[0149] In the coloring composition of the present invention, the content of the photopolymerization initiator is preferably 0.01 to 120 parts by mass, more preferably 1 to 100 parts by mass, relative to 100 parts by mass of the polymerizable compound. In this case, if the content of the photopolymerization initiator is too small, curing by exposure may be insufficient, while if it is too large, the formed coloring layer tends to easily fall off from the substrate during development.

[0150] (Other combination agents) In the coloring composition of the present invention, other additives can be added in addition to the above-mentioned additives, so long as the preferable physical properties of the present invention are not impaired. Examples of other additives include dispersants other than the block copolymers (urethane-based dispersants, polyethyleneimine-based dispersants, polyoxyethylene alkyl ether-based dispersants, polyoxyethylene glycol diester-based dispersants, sorbitan aliphatic ester-based dispersants, aliphatic modified polyester-based dispersants, etc.), sensitizing dyes, thermal polymerization inhibitors, surfactants (nonionic surfactants, anionic surfactants, cationic surfactants, amphoteric surfactants), plasticizers, organic carboxylic acid compounds, organic carboxylic anhydrides, antioxidants, ultraviolet absorbers, light stabilizers, pH adjusters, preservatives, antifungal agents, aggregation inhibitors, adhesion improvers, development improvers, storage stabilizers, etc.

[0151] Sensitizing dyes include 4,4'-dimethylaminobenzophenone, 4,4'-diethylaminobenzophenone, 2-aminobenzophenone, 4-aminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 3,4-diaminobenzophenone, 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-diethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzo[4,5]benzoxazole, 2-(p-dimethylaminophenyl)benzo[6,7]benzoxazole, 2,5-bis(p-diethylaminophenyl)1,3,4- Examples of the aryl group include oxazole, 2-(p-dimethylaminophenyl)benzothiazole, 2-(p-diethylaminophenyl)benzothiazole, 2-(p-dimethylaminophenyl)benzimidazole, 2-(p-diethylaminophenyl)benzimidazole, 2,5-bis(p-diethylaminophenyl)1,3,4-thiadiazole, (p-dimethylaminophenyl)pyridine, (p-diethylaminophenyl)pyridine, (p-dimethylaminophenyl)quinoline, (p-diethylaminophenyl)quinoline, (p-dimethylaminophenyl)pyrimidine, and (p-diethylaminophenyl)pyrimidine.

[0152] Examples of the thermal polymerization inhibitor include hydroquinone, p-methoxyphenol, pyrogallol, catechol, 2,6-t-butyl-p-cresol, and β-naphthol.

[0153] Nonionic surfactants include fluorine-based surfactants (1,1,2,2-tetrafluorooctyl (1,1,2,2-tetrafluoropropyl) ether, 1,1,2,2-tetrafluorooctylhexyl ether, octaethylene glycol di(1,1,2,2-tetrafluorobutyl) ether, hexaethylene glycol di(1,1,2,2,3,3-hexafluoropentyl) ether, octapropylene glycol di(1,1,2,2-tetrafluorobutyl) ether, hexapropylene glycol di(1,1,2,2,3,3-hexafluoropentyl) ether, sodium perfluorododecyl sulfonate, 1,1,2,2,8,8,9,9,10,10-decafluorododecane, 1,1,2,2,3 ,3-hexafluorodecane, etc.), silicone-based surfactants, polyoxyethylene-based surfactants (polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, pentaerythritol fatty acid esters, polyoxyethylene pentaerythritol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, sorbitol fatty acid esters, polyoxyethylene sorbitol fatty acid esters, etc.).

[0154] Examples of anionic surfactants include alkyl sulfonates, alkyl benzene sulfonates, alkyl naphthalene sulfonates, polyoxyethylene alkyl ether sulfonates, alkyl sulfates, alkyl sulfate ester salts, higher alcohol sulfate ester salts, aliphatic alcohol sulfate ester salts, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkyl phenyl ether sulfates, alkyl phosphate ester salts, polyoxyethylene alkyl ether phosphates, polyoxyethylene alkyl phenyl ether phosphates, and special polymer surfactants.

[0155] Examples of the cationic surfactant include quaternary ammonium salts, imidazoline derivatives, and alkylamine salts.

[0156] Examples of the amphoteric surfactant include betaine-type compounds, imidazolium salts, imidazolines, and amino acids.

[0157] Examples of the plasticizer include dioctyl phthalate, didodecyl phthalate, triethylene glycol dicaprylate, dimethyl glycol phthalate, tricresyl phosphate, dioctyl adipate, dibutyl sebacate, and triacetyl glycerin.

[0158] Examples of organic carboxylic acid compounds include aliphatic monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, pivalic acid, caproic acid, glycolic acid, acrylic acid, and methacrylic acid; aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, cyclohexanedicarboxylic acid, cyclohexenedicarboxylic acid, itaconic acid, citraconic acid, maleic acid, and fumaric acid; aliphatic tricarboxylic acids such as tricarballylic acid and aconitic acid; aromatic carboxylic acids in which a carboxyl group is directly bonded to a phenyl group such as benzoic acid, phthalic acid, trimesic acid, pyropetoic acid, and mellophanic acid; aromatic carboxylic acids in which a carboxyl group is bonded to a phenyl group via a carbon bond such as phenylacetic acid, hydroatropic acid, hydrocinnamic acid, phenylsuccinic acid, and cinnamylindeneacetic acid. By containing an organic carboxylic acid compound, it is possible to improve alkaline developability and background scumming.

[0159] Examples of organic carboxylic acid anhydrides include acetic anhydride, trichloroacetic anhydride, trifluoroacetic anhydride, tetrahydrophthalic anhydride, succinic anhydride, maleic anhydride, citraconic anhydride, itaconic anhydride, glutaric anhydride, 1,2-cyclohexene dicarboxylic anhydride, n-octadecylsuccinic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, naphthalic anhydride, etc. By containing an organic carboxylic acid anhydride, it is possible to improve alkali developability and background scumming.

[0160] <Method of producing colored composition> The coloring composition can be prepared by mixing a coloring material, a dispersant (or a dispersant solution), a dispersion medium, and, if necessary, a binder resin, a photopolymerization initiator, and other compounding agents. For mixing, a mixer / disperser such as a paint shaker, a bead mill, a ball mill, a dissolver, or a kneader can be used. It is preferable to filter the coloring composition after mixing. When the coloring composition has alkaline developability, it can be suitably used for color filters. As the alkaline developer, an aqueous solution containing an organic solvent or a surfactant and an alkaline compound such as potassium hydroxide, sodium hydrogen carbonate, sodium carbonate, or tetramethylammonium hydroxide can be used.

[0161] <Color filters> The color filter of the present invention comprises a colored layer formed using the colored composition.

[0162] The method for producing a color filter may be, for example, the following method. First, a coloring composition in which, for example, a red pigment is dispersed is applied onto a transparent substrate such as a thermoplastic resin sheet such as a polyester resin, a polyolefin resin, a polycarbonate resin, or a polymethyl methacrylate resin, a thermosetting resin sheet such as an epoxy resin, an unsaturated polyester resin, or a poly(meth)acrylic resin, or various types of glass, and then pre-baked to evaporate the solvent (dispersion medium) to form a coating film. Next, the coating film is exposed through a photomask, and then developed using an alkaline developer (an aqueous solution containing an organic solvent or a surfactant and an alkaline compound such as potassium hydroxide, sodium bicarbonate, sodium carbonate, or tetramethylammonium hydroxide) to dissolve and remove the unexposed portion of the coating film. Then, post-baking is performed to form a pixel array in which a red pixel pattern is arranged in a predetermined arrangement. Next, using a green coloring composition or a blue coloring composition, coating, pre-baking, exposure, development, and post-baking of each coloring composition are performed in the same manner as above to sequentially form a green pixel array and a blue pixel array on the same substrate. This results in a color filter having a pixel array of the three primary colors of red, green, and blue arranged on the substrate. However, in the present invention, the order of forming the pixels of each color is not limited to the above. In addition, a black matrix may be provided on the transparent substrate used to form the pixel array of the three primary colors of red, green, and blue.

[0163] When applying the coloring composition to a substrate, a suitable application method such as a spray method, a roll coating method, a rotary coating method (spin coating method), a slit die coating method, or a bar coating method can be used. In particular, it is preferable to use a spin coating method or a slit die coating method.

[0164] On the pixel pattern thus obtained, a protective film is formed as necessary, and then a transparent conductive film (ITO, etc.) is formed by sputtering. After the transparent conductive film is formed, a spacer can be further formed to form a color filter.

[0165] The color filter of the present invention has high brightness, dimensional accuracy, and the like, and can be suitably used in color liquid crystal display elements, color image pickup tube elements, color sensors, organic EL display elements, electronic paper, and the like. EXAMPLES

[0166] The present invention will be described in more detail below based on specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention. The polymerization rate, weight average molecular weight (Mw), molecular weight distribution (Mw / Mn), and amine value of the block copolymer, as well as the physical properties of the colored composition and coating film, were evaluated according to the following methods.

[0167] The meanings of the abbreviations are as follows: BTEE: Ethyl 2-methyl-2-n-butyltellanyl propionate DBDT: Dibutyl ditelluride AIBN: 2,2'-azobis(isobutyronitrile) CL5MA: 5 mol caprolactone adduct of 2-hydroxyethyl methacrylate CL2MA: 2-hydroxyethyl methacrylate adduct with 2 mol of caprolactone CL5A: 5 mol caprolactone adduct of 2-hydroxyethyl acrylate (Green, KOMERATE-C050) BA: n-butyl acrylate HEA: 2-hydroxyethyl acrylate HEMA: 2-hydroxyethyl methacrylate MMA: Methyl methacrylate BMA: n-butyl methacrylate CHMA: Cyclohexyl methacrylate BzMA: benzyl methacrylate MAA: Methacrylic acid DMAEMA: Dimethylaminoethyl methacrylate VP: N-vinyl-2-pyrrolidone PMA: Propylene glycol monomethyl ether acetate MeOH: Methanol

[0168] [Evaluation method] (Polymerization rate) Using a nuclear magnetic resonance (NMR) measuring device (Bruker Biospin, model: AVANCE500 (frequency 500 MHz)), 1 H-NMR measurement (solvent: CDCl 3 (Internal standard: tetramethylsilane) For the obtained NMR spectrum, the integral ratio of the peak derived from the monomer to the peak derived from the polymer was obtained, and the polymerization rate of the monomer was calculated.

[0169] (Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)) The molecular weight was determined by gel permeation chromatography (GPC) using a high performance liquid chromatograph (Tosoh, model HLC-8320). A column of TOSOH TSKgel (registered trademark) SuperMultiporeHZ-H (4.6 mm I.D. × 150 mm, 6 μm), THF as the mobile phase, and a differential refractometer as the detector were used. The measurement conditions were a column temperature of 40°C, a sample concentration of 20 mg / mL, a sample injection amount of 10 μL, and a flow rate of 0.2 mL / min. A calibration curve was created using polystyrene (molecular weights 70,500, 37,900, 19,920, 10,200, 4,290, 2,630, and 1,150) as a standard substance, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured. The molecular weight distribution (Mw / Mn) was calculated from the measured values.

[0170] (amine value) The amine value represents the mass of potassium hydroxide equivalent to the basic component per 1 g of solid content. The measurement sample was dissolved in tetrahydrofuran, and the resulting solution was neutralized with hydrochloric acid (0.1 mol / L)-propanol solution using a potentiometric titrator (product name: GT-06, manufactured by Mitsubishi Chemical). The inflection point of the titration pH curve was used as the titration end point, and the amine value (B) was calculated using the following formula. B=56.11×Vs×0.1×f / w B: Amine value (mgKOH / g) Vs: Amount of hydrochloric acid (0.1 mol / L)-propanol solution required for titration (mL) f: Potency of hydrochloric acid (0.1 mol / L)-propanol solution w: Mass of the measurement sample (g) (solid content equivalent)

[0171] (Acid value) The acid value represents the mass of potassium hydroxide required to neutralize the acidic components per 1 g of solid content. The measurement sample was dissolved in tetrahydrofuran, and a few drops of 1.0 w / v% phenolphthalein ethanol (90) solution were added to the resulting solution as an indicator, and neutralization titration was performed with potassium hydroxide (0.1 mol / L)-ethanol solution. The point where a slight redness remained was set as the titration end point, and the acid value was calculated using the following formula. A=56.11×Vs×0.1×f / w A: Acid value (mgKOH / g) Vs: Amount of potassium hydroxide (0.1 mol / L)-ethanol solution required for titration (mL) f: Potassium hydroxide (0.1 mol / L)-ethanol solution w: Measurement sample mass (g) (solid content equivalent)

[0172] (Initial viscosity, viscosity over time) The viscosity (mPa·s) was measured using an E-type viscometer (product name: RE-80L, manufactured by Toki Sangyo) with a cone rotor (0.8° × R24) at 25°C and a rotor rotation speed of 50 rpm. The initial viscosity of the colored composition immediately after preparation and the viscosity over time after storage at 40° C. for one week were measured.

[0173] <Synthesis of block copolymer> (Block Copolymer No. 1) In a flask equipped with an argon gas inlet tube and a stirrer, 44.21g of BMA, 120.25g of CL5MA, 0.789g of AIBN, and 109.55g of PMA were charged, and after replacing with nitrogen, 7.19g of BTEE and 4.50g of DBDT were added, and the reaction was carried out at 60°C for 17.5 hours to polymerize the A block. The polymerization rate was 98.8%.

[0174] To the reaction solution, a mixed solution of 55.65 g of DMAEMA, 13.92 g of CHMA, 0.398 g of AIBN, and 46.42 g of PMA, which had been previously purged with argon, was added, and the reaction was carried out at 60° C. for 23.5 hours to polymerize block B. The polymerization rate was 99.2%.

[0175] To the reaction solution, a mixed solution of 66.32 g of HEMA, 0.394 g of AIBN, and 44.14 g of PMA, which had been previously purged with argon, was added, and the mixture was reacted at 60° C. for 23.0 hours to polymerize the C block. The polymerization rate was 99.8%.

[0176] After the reaction was completed, the reaction solution was poured into stirred n-heptane. The precipitated polymer was filtered by suction and dried to obtain block copolymer No. 1. The obtained block copolymer No. 1 had Mw of 17,540, Mw / Mn of 1.73, and amine value of 65 mgKOH / g.

[0177] (Block copolymer No. 2-9) Block copolymers No. 2 to 9 were prepared in the same manner as in the preparation of block copolymer No. 1. Tables 2 and 3 show the monomers, organotellurium compounds, azo-based polymerization initiators, solvents, reaction conditions, and polymerization rates used. Tables 4 and 5 show the composition, Mw, Mw / Mn, and amine value of each block copolymer. The content of each structural unit in the copolymer was calculated from the charge ratio and polymerization rate of the monomers used in the polymerization reaction.

[0178] [Table 2]

[0179] [Table 3]

[0180] <Synthesis of alkali-soluble resin (binder resin)> A flask equipped with an argon gas inlet tube and a stirrer was charged with 20.0 g of MAA, 80.0 g of BzMA, and 290.0 g of PMA, and after replacing with argon, 1.5 g of AIBN, 2.0 g of n-dodecanethiol, and 10.0 g of PMA were added and heated to 90° C. While maintaining the solution at 90° C., 40.0 g of MAA, 160.0 g of BzMA, 3.0 g of AIBN, 4.0 g of n-dodecanethiol, and 25.0 g of PMA were added dropwise to the solution over 1.5 hours. 60 minutes after the dropwise addition was completed, the temperature was raised to 110°C, 0.3 g of AIBN and 5.0 g of PMA were added and reacted for 1 hour, 0.3 g of AIBN and 5.0 g of PMA were further added and reacted for 1 hour, and 0.3 g of AIBN and 5.0 g of PMA were further added and reacted for 1 hour.

[0181] The reaction solution was cooled to room temperature, and 120.0 g of PMA was added to obtain an alkali-soluble resin solution with a non-volatile content of 39.9%. The alkali-soluble resin had an Mw of 11,873, an Mw / Mn of 1.77, and an acid value of 127 mgKOH / g.

[0182] <Preparation of Coloring Composition> (Coloring composition No.1) In order to obtain a pigment concentration of 10% by mass, 1.8 g of pigment (CI Pigment Red 254), a solution of block copolymer No. 1 as a dispersant (40 parts by mass of block copolymer per 100 parts by mass of pigment), a solution of alkali-soluble resin (40 parts by mass of alkali-soluble resin per 100 parts by mass of pigment), and PMA were added to a bead mill (trade name: DISPERMAT CA, manufactured by VMA-GETZMANN GmbH), and 50 g of zirconia beads (φ0.3 mm) were added and stirred for 2 hours. After stirring, the beads were filtered to prepare colored composition No. 1. The dispersion performance of the obtained colored composition was evaluated, and the results are shown in Table 4.

[0183] (Coloring composition No.2, 4~10) Except for changing the dispersant (block copolymer), colored compositions Nos. 2, 4 to 10 were prepared in the same manner as in the preparation of colored composition No. 1. The obtained colored compositions were evaluated, and the results are shown in Tables 4 and 5.

[0184] (Coloring composition No.3) Colored composition No. 3 was prepared in the same manner as in preparation of colored composition No. 2, except that the pigment was changed to CI Pigment Green 58. The obtained colored composition was evaluated, and the results are shown in Table 4.

[0185] (Coloring composition No.11) Colored composition No. 11 was prepared in the same manner as in preparation of colored composition No. 10, except that the pigment was changed to CI Pigment Green 58. The obtained colored composition was evaluated, and the results are shown in Table 5.

[0186] [Table 4]

[0187] [Table 5]

[0188] Block copolymers Nos. 1 to 5 are triblocks having an A block-B block-C block structure, in which the A block contains the structural unit (a-1), the B block contains the structural unit (b-1), and the C block contains the structural unit (c-1) having a molar volume ratio ((c-1) / (b-1)) of 0.1 to 1.5, in which the content of the structural unit (b-1) in 100 mol % of the structural units constituting the A block is 3 mol % or less, and the content of the structural unit (b-1) in 100 mol % of the structural units constituting the C block is 3 mol % or less. Colored compositions Nos. 1 to 6 using these block copolymers Nos. 1 to 5 as dispersants all had low initial viscosities, and the difference in viscosity over time was small, so that the dispersibility of the colorant was high.

[0189] Block copolymer No. 6 is a triblock copolymer having an A block-B block-C block structure, in which the A block contains the structural unit (a-1), the B block contains the structural unit (b-1), and the C block does not contain the structural unit (c-1) having a molar volume ratio ((c-1) / (b-1)) of 0.1 to 1.5. Colored composition No. 7 using this block copolymer No. 6 had a low initial viscosity, but its viscosity increased over time and its storage stability was poor.

[0190] Block copolymer No. 7 is a triblock copolymer having an A block-B block-C block structure, in which the A block contains the structural unit (a-1), the B block contains the structural unit (b-1), and the C block does not contain the structural unit (c-1). Colored composition No. 8 using this block copolymer No. 7 had a high initial viscosity and poor dispersibility of the colorant.

[0191] Block copolymers No. 8 and 9 are diblock copolymers having a block A-block B structure. Colored compositions Nos. 9 to 11 using these block copolymers No. 8 and 9 showed a very large change in viscosity over time relative to the initial viscosity, and were poor in storage stability.

[0192] The present invention includes the following aspects.

[0193] (Aspect 1) A block copolymer containing an A block, a B block, and a C block, The arrangement of the blocks is in the order of A block-B block-C block, the A block contains a structural unit (a-1) having a hydroxy group and / or an ether group, the B block contains a structural unit (b-1) having a nitrogen-containing functional group, the C block contains a structural unit (c-1) having a hydroxy group, the molar volume ratio of the structural unit (c-1) to the structural unit (b-1), ((c-1) / (b-1)), is 0.1 to 1.5; the content of the structural unit (b-1) in 100 mol % of the structural units constituting the A block is 3 mol % or less, A block copolymer, characterized in that the content of the structural unit (b-1) in 100 mol % of the structural units constituting the C block is 3 mol % or less.

[0194] (Aspect 2) 2. The block copolymer according to aspect 1, wherein the molar volume ratio of the structural unit (a-1) to the structural unit (b-1), ((a-1) / (b-1)), is 0.1 to 10.0.

[0195] (Aspect 3) The block copolymer according to embodiment 1 or 2, wherein the structural unit (a-1) is a structural unit represented by formula (1).

[0196] [ka] [In formula (1), R 11 represents a hydrogen atom or a methyl group. A 11 represents an ester group, an amide group, or a single bond. R 12 is a divalent hydrocarbon group, -R 14 -(O-CO-R 15 ) m1 -group or -R 16 -(OR 17 ) n1 - represents a group. R 13 represents a hydrogen atom or a monovalent hydrocarbon group. 12 is a divalent hydrocarbon group, or -R 14 -(O-CO-R 15 ) m1 - group, R 13 is a hydrogen atom. m1 represents an integer of 1 to 10. R 14 represents a divalent hydrocarbon group. R 15 represents a divalent hydrocarbon group, and when m1 is 2 or more, a plurality of R 15 may be the same or different. n1 represents an integer from 1 to 30. R 16 represents a divalent hydrocarbon group. R 17 represents a divalent hydrocarbon group, and when n1 is 2 or more, multiple R 17 may be the same or different.]

[0197] (Aspect 4) The block copolymer according to any one of aspects 1 to 3, wherein the structural unit (b-1) is a structural unit represented by formula (6) and / or a structural unit represented by formula (7).

[0198] [ka] [In formula (6), R 61 represents a hydrogen atom or a methyl group. A 61 represents an ester group, an amide group, or a single bond. R 62 represents a divalent hydrocarbon group. R 63 and R 64 each independently represents a hydrogen atom or a linear or cyclic hydrocarbon group which may have a substituent.

[0199] [ka] [In formula (7), R 71 , R 72 , R 73 and R 74 are the same or different and represent a hydrogen atom or an optionally substituted alkyl group having 1 to 10 carbon atoms. m7 represents an integer of 0 to 4. n7 represents an integer from 1 to 3.

[0200] (Aspect 5) The block copolymer according to any one of aspects 1 to 4, wherein the structural unit (c-1) is a structural unit represented by formula (8).

[0201] [ka] [In formula (8), R 81 represents a hydrogen atom or a methyl group. A 81 represents an ester group, an amide group, or a single bond. R 82 is a divalent hydrocarbon group, -R 83 -(O-CO-R 84 ) m8 -group or -R 85 -(OR 86 ) n8 - represents a group. m8 represents an integer from 1 to 10. R 83 represents a divalent hydrocarbon group. R 84 represents a divalent hydrocarbon group, and when m8 is 2 or more, a plurality of R 84 may be the same or different. n8 represents an integer from 1 to 30. R 85 represents a divalent hydrocarbon group. R 86 represents a divalent hydrocarbon group, and when n8 is 2 or more, multiple R 86 may be the same or different.]

[0202] (Aspect 6) 6. The block copolymer according to any one of aspects 1 to 5, wherein the block copolymer has an amine value of 10 mg KOH / g to 150 mg KOH / g.

[0203] (Aspect 7) A block copolymer according to any one of aspects 1 to 6, wherein a content of the structural unit (b-1) in 100 mol % of the structural units constituting the B block is 5 mol % to 100 mol %.

[0204] (Aspect 8) The block copolymer according to any one of aspects 1 to 7, wherein a molar ratio of the total molar amount of structural units constituting the A block to the structure constituting the B block (A block / B block) is 10 / 90 to 95 / 5, and a molar ratio of the total molar amount of structural units constituting the C block to the structure constituting the B block (C block / B block) is 10 / 90 to 95 / 5.

[0205] (Aspect 9) The block copolymer according to any one of Aspects 1 to 8, wherein the block copolymer has a weight average molecular weight of 5,000 to 40,000.

[0206] (Aspect 10) The block copolymer according to any one of aspects 1 to 9, wherein the block copolymer is obtained by living polymerization and has a molecular weight distribution (Mw / Mn) of less than 3.0.

[0207] (Aspect 11) A dispersant comprising the block copolymer according to any one of aspects 1 to 10.

[0208] (Aspect 12) A coloring composition comprising a colorant, a dispersion medium, and the dispersant according to aspect 11.

[0209] (Aspect 13) The coloring composition according to aspect 12, which is for use in a color filter.

[0210] (Aspect 14) A color filter comprising a colored layer formed using the colored composition according to aspect 12 or 13.

Claims

1. A block copolymer containing an A block, a B block, and a C block, The arrangement of the blocks is in the order of A block - B block - C block, the A block contains a structural unit (a-1) having a hydroxy group and / or an ether group, the B block contains a structural unit (b-1) having a nitrogen-containing functional group, the C block contains a structural unit (c-1) having a hydroxy group, the molar volume ratio ((c-1) / (b-1)) of the structural unit (c-1) to the structural unit (b-1) is 0.1 to 1.5; the content of the structural unit (b-1) in 100 mol % of the structural units constituting the A block is 3 mol % or less, A block copolymer, characterized in that the content of the structural unit (b-1) in 100 mol % of the structural units constituting the C block is 3 mol % or less.

2. 2. The block copolymer according to claim 1, wherein the molar volume ratio ((a-1) / (b-1)) of the structural unit (a-1) to the structural unit (b-1) is 0.1 to 10.

0.

3. The block copolymer according to claim 1 or 2, wherein the structural unit (a-1) is a structural unit represented by formula (1). [Case 1] [In formula (1), R 11 represents a hydrogen atom or a methyl group. A 11 represents an ester group, an amide group, or a single bond. R 12 is a divalent hydrocarbon group, -R 14 -(O-CO-R 15 ) m1 - group or -R 16 - (OR 17 ) n1 - represents a group. R 13represents a hydrogen atom or a monovalent hydrocarbon group. 12 is a divalent hydrocarbon group, or -R 14 -(O-CO-R 15 ) m1 In the case of a - group, R 13 is a hydrogen atom. m1 represents an integer of 1 to 10. R 14 represents a divalent hydrocarbon group. R 15 represents a divalent hydrocarbon group, and when m1 is 2 or more, a plurality of R 15 may be the same or different. n1 represents an integer of 1 to 30. R 16 represents a divalent hydrocarbon group. R 17 represents a divalent hydrocarbon group, and when n1 is 2 or more, a plurality of R 17 may be the same or different.

4. The block copolymer according to claim 1 or 2, wherein the structural unit (b-1) is a structural unit represented by formula (6) and / or a structural unit represented by formula (7). [Case 2] [In formula (6), R 61 represents a hydrogen atom or a methyl group. A 61 represents an ester group, an amide group, or a single bond. R 62 represents a divalent hydrocarbon group. R 63 and R 64 each independently represents a hydrogen atom or a linear or cyclic hydrocarbon group which may have a substituent. [C3] [In formula (7), R 71 , R 72 , R 73 and R 74 are the same or different and represent a hydrogen atom or an optionally substituted alkyl group having 1 to 10 carbon atoms. m7 represents an integer of 0 to 4. n7 represents an integer of 1 to 3.

5. The block copolymer according to claim 1 or 2, wherein the structural unit (c-1) is a structural unit represented by formula (8): [C4] [In formula (8), R 81 represents a hydrogen atom or a methyl group. A 81 represents an ester group, an amide group, or a single bond. R 82 is a divalent hydrocarbon group, -R 83 -(O-CO-R 84 ) m8 - group or -R 85 - (OR 86 ) n8 - represents a group. m8 represents an integer of 1 to 10. R 83 represents a divalent hydrocarbon group. R 84 represents a divalent hydrocarbon group, and when m8 is 2 or more, a plurality of R 84 may be the same or different. n8 represents an integer of 1 to 30. R 85 represents a divalent hydrocarbon group. R 86 represents a divalent hydrocarbon group, and when n8 is 2 or more, a plurality of R 86 may be the same or different.

6. 3. The block copolymer according to claim 1, wherein the amine value of the block copolymer is from 10 mg KOH / g to 150 mg KOH / g.

7. 3. The block copolymer according to claim 1, wherein the content of the structural unit (b-1) in 100 mol % of the structural units constituting the B block is 5 mol % to 100 mol %.

8. 3. The block copolymer according to claim 1, wherein a molar ratio of a total molar amount of structural units constituting the A block to a total molar amount of structural units constituting the B block (A block / B block) is 10 / 90 to 95 / 5, and a molar ratio of a total molar amount of structural units constituting the C block to a total molar amount of structural units constituting the B block (C block / B block) is 10 / 90 to 95 / 5.

9. 3. The block copolymer according to claim 1, wherein the weight average molecular weight of the block copolymer is 5,000 to 40,000.

10. 3. The block copolymer according to claim 1, wherein the block copolymer is obtained by living polymerization and has a molecular weight distribution (Mw / Mn) of less than 3.

0.

11. A dispersant comprising the block copolymer according to claim 1 or 2.

12. A coloring composition comprising a colorant, a dispersion medium, and the dispersant according to claim 11.

13. The coloring composition according to claim 12, which is for use in a color filter.

14. A color filter comprising a colored layer formed using the colored composition according to claim 12.

Citation Information

Patent Citations

  • Colored photosensitive composition for color filter

    JP2009265515A

  • Block copolymer, dispersant, and pigment dispersion composition

    JP2013119568A