Polyamide resin composition, molding, and method for producing polyamide resin composition

The polyamide resin composition, with a fatty acid metal salt and specific spatial distribution, addresses the instability of existing compositions in high-cycle molding by enhancing rigidity, surface appearance, and bleed-out resistance, ensuring stable molded products.

JP2024167063APending Publication Date: 2024-11-29ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024076814
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing polyamide resin compositions are inadequate for high-cycle molding due to issues with surface appearance and mechanical properties, particularly when subjected to high-temperature molding conditions, leading to decomposition and instability in molded products.

Method used

A polyamide resin composition containing a polyamide resin and a fatty acid metal salt with specific spatial distribution characteristics, including a shape parameter k of 1.0 or more, which enhances rigidity, surface appearance, and bleed-out resistance, suitable for high-cycle molding.

Benefits of technology

The composition provides molded articles with improved rigidity upon water absorption, excellent surface appearance, and resistance to bleed-out, making it suitable for high-cycle molding processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167063000001
    Figure 2024167063000001
  • Figure 2024167063000002
    Figure 2024167063000002
  • Figure 2024167063000003
    Figure 2024167063000003
Patent Text Reader

Abstract

To provide a polyamide resin composition excellent in toughness, surface appearance, and bleed-out resistance during water absorption when molded, and suitable for high cycle molding, a producing method thereof and a molding containing the polyamide resin composition.SOLUTION: A polyamide resin composition containing a polyamide resin (A) and a fatty acid metal salt (B) of a metal containing an alkali metal and / or an alkaline earth metal, is characterized in that the polyamide resin composition contains 0.05 to 5.00 pts.mass inclusive of the fatty acid metal salt (B) relative to 100 pts.mass of the polyamide resin (A), and that In an area distribution with respect to the space area per one metal ion of the fatty acid metal salt (B) on a surface of the polyamide resin composition, a shape parameter k of gamma distribution is 1.0 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide resin composition, a molded article, and a method for producing a polyamide resin composition. [Background technology]

[0002] Generally, polyamide resins have excellent mechanical properties as well as heat resistance, impact resistance, and chemical resistance, and are therefore widely used in automobile parts, electrical parts, electronic parts, household goods, and the like.

[0003] In recent years, from the standpoint of economic efficiency and environmental issues, there has been a strong demand for polyamide resins that have better moldability and can be used in a wider range of environments. In particular, there is a demand for polyamide resin materials that have improved rigidity after absorbing water (water-absorbed rigidity) and rigidity under high temperature use (hot rigidity) and that exhibit minimal change in physical properties when used in any environment.

[0004] In addition, molded products using polyamide resins may be molded under high-cycle molding conditions in which the molding temperature is increased and the mold temperature is decreased in order to improve productivity. On the other hand, molding under high-temperature conditions may cause decomposition of the polyamide resin or changes in flowability, making it difficult to obtain molded products stably. Therefore, there is a demand for polyamide resins that are excellent in the stability of the surface appearance of molded products even under the above-mentioned harsh molding conditions and are suitable for high-cycle molding.

[0005] In response to such demands, there have been disclosed, as materials capable of improving the surface appearance and mechanical properties of molded articles, polyamides consisting of polyamide 66 / 6I into which an isophthalic acid component has been introduced (see, for example, Patent Document 1), and polyamide resin compositions containing polycapramide resin, semi-aromatic amorphous polyamide resin 6T / 6I, and an inorganic reinforcing material (see, for example, Patent Document 2). In addition, a polyamide resin composition containing polyamide 6T / 6I, which contains a terephthalic acid component and an isophthalic acid component, has been disclosed as a material that can improve mechanical properties, fluidity, surface appearance, etc. (see, for example, Patent Document 3). Furthermore, materials that combine a polyamide resin composition with a release agent for the purpose of improving releasability have been disclosed (see, for example, Patent Documents 4 and 5), and it has been reported that the adhesion between the molded product and the wall surface of the mold is reduced by combining a stearic acid-based aliphatic metal salt with an ester compound, an amide compound, or the like as a release agent. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-032980 [Patent Document 2] JP 2000-154316 A [Patent Document 3] Japanese Patent Application Publication No. 11-349806 [Patent Document 4] Japanese Patent Application Publication No. 11-42666 [Patent Document 5] JP 2013-147641 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the techniques disclosed in Patent Documents 1 to 5 are insufficient in terms of compatibility between suitability for high-cycle molding in consideration of productivity and surface appearance of molded articles. In particular, the polyamide resin composition containing polycapramide resin and semi-aromatic amorphous polyamide resin 6T / 6I described in Patent Document 2 has a slow crystallization rate, poor suitability for high-cycle molding, and room for improvement in production processability. Therefore, it is difficult to achieve both surface appearance of molded articles and suitability for high-cycle molding.

[0008] The present invention has been made in consideration of the above circumstances, and provides a polyamide resin composition which, when formed into a molded article, has excellent rigidity, surface appearance and bleed-out resistance when absorbing water and is suitable for high-cycle molding; a molded article containing the polyamide resin composition; and a method for producing the polyamide resin composition. [Means for solving the problem]

[0009] That is, the present invention is as follows. (1) A polyamide resin composition comprising a polyamide resin (A) and a fatty acid metal salt (B) of a metal including an alkali metal and / or an alkaline earth metal, The fatty acid metal salt (B) is contained in an amount of 0.05 parts by mass or more and 5.00 parts by mass or less relative to 100 parts by mass of the polyamide resin (A), A polyamide resin composition, characterized in that in an area distribution relating to a spatial area per metal ion of the fatty acid metal salt (B), which is calculated by subjecting a surface of the polyamide resin composition to the following measurement, a shape parameter k of a gamma distribution is 1.0 or more. [measurement] In a distribution image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition or an intensity information image of the metal ion image, a Voronoi division is performed with the center of the metal ion as a generating point to calculate the spatial area per metal ion on the surface. The spatial area of ​​each region obtained by the Voronoi division is calculated and classified according to spatial area, and a shape parameter k is calculated from a gamma distribution represented by the following formula. [ka] (wherein k is a shape parameter, θ is a scale parameter, and x is a spatial area) (2) The polyamide resin composition according to (1), wherein the fatty acid metal salt (B) is a fatty acid metal salt having a terminal hydrocarbon group having 19 or more carbon atoms. (3) The polyamide resin composition according to (1) or (2), wherein the polyamide resin (A) is an aliphatic polyamide (Aa), a semi-aromatic polyamide (Ab) containing a diamine unit and a dicarboxylic acid unit, or a mixture thereof. (4) The polyamide resin (A) is 100 parts by mass. 50 parts by mass or more and 99 parts by mass or less of the aliphatic polyamide (Aa); 1 part by mass or more and 50 parts by mass or less of the semi-aromatic polyamide (Ab); 0.05 parts by mass or more and 5.00 parts by mass or less of the fatty acid metal salt (B); Furthermore, 0.01 parts by mass or more and 3.00 parts by mass or less of a fatty acid amide compound (C); The polyamide resin composition according to (3), (5) The polyamide resin composition according to (4), wherein the ratio Bw / Cw of the mass Bw of the fatty acid metal salt (B) to the mass Cw of the fatty acid amide compound (C) is 0.6 or more and 4.0 or less. (6) The polyamide resin composition according to (4) or (5), wherein the ratio Bn / Cn of the number of carbon atoms Bn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the number of carbon atoms Cn of the terminal hydrocarbon group of the fatty acid amide compound (C) is more than 1.00 and not more than 2.00. (7) The polyamide resin composition according to any one of (3) to (6), wherein the aliphatic polyamide (Aa) is polyamide 6 or polyamide 66. (8) The polyamide resin composition according to any one of (3) to (7), wherein the semi-aromatic polyamide (Ab) contains 50 mol % or more of isophthalic acid units relative to all dicarboxylic acid units constituting the semi-aromatic polyamide (Ab), and contains, as the diamine units, diamine units having 4 to 10 carbon atoms. (9) The polyamide resin composition according to any one of (3) to (7), wherein the semi-aromatic polyamide (Ab) contains 75 mol % or more of isophthalic acid units relative to all dicarboxylic acid units constituting the semi-aromatic polyamide (Ab), and contains, as the diamine units, diamine units having 4 to 10 carbon atoms. (10) The polyamide resin composition according to any one of (1) to (9), wherein the polyamide resin (A) has a weight average molecular weight Mw of 10,000 or more and 50,000 or less. (11) The polyamide resin composition according to any one of (1) to (10), wherein the polyamide resin (A) has a molecular weight distribution Mw / Mn of 2.4 or less. (12) The polyamide resin composition according to any one of (1) to (11), wherein the fatty acid metal salt (B) is at least one selected from the group consisting of sodium montanate and calcium montanate. (13) The polyamide resin composition according to any one of (4) to (12), wherein the fatty acid amide compound (C) is at least one selected from the group consisting of fatty acid amide compounds and fatty acid bisamide compounds having a hydrocarbon group having from 9 to 30 carbon atoms. (14) The polyamide resin composition according to any one of (4) to (13), wherein the fatty acid amide compound (C) is at least one member selected from the group consisting of N,N'-ethylenebisstearamide and N-stearylerucamide. (15) Further containing an inorganic filler (D), The polyamide resin composition according to any one of (1) to (14), wherein the content of the inorganic filler (D) is 5 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the polyamide resin (A). (16) Further containing nigrosine (E), The polyamide resin composition according to any one of (1) to (15), wherein the content of the nigrosine (E) is more than 0 part by mass and not more than 0.5 parts by mass per 100 parts by mass of the polyamide resin (A). (17) The polyamide resin composition according to any one of (1) to (16), having a chloride ion content of 5 ppm or less by mass. (18) A molded article comprising the polyamide resin composition according to any one of (1) to (17). (19) A method for producing a polyamide resin composition according to any one of (1) to (17), comprising the steps of: A production method comprising the step of melt-kneading the polyamide resin (A) and the fatty acid metal salt (B). Effect of the Invention

[0010] According to the present invention, it is possible to provide a polyamide resin composition which, when made into a molded article, has excellent rigidity, surface appearance and bleed-out resistance when absorbing water and is suitable for high-cycle molding, and a production method thereof, as well as a molded article which contains the polyamide resin composition and has excellent rigidity, surface appearance and bleed-out resistance when absorbing water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0012] In this specification, the term "polyamide" refers to a polymer having an amide group (-NHCO-) ​​in the main chain.

[0013] <Polyamide resin composition> The polyamide resin composition of the present embodiment is a polyamide resin composition containing a polyamide resin (A) and a fatty acid metal salt (B) of a metal containing an alkali metal and / or an alkaline earth metal, and is characterized in that, in an area distribution relating to the spatial area per metal ion of the fatty acid metal salt (B), which is calculated by subjecting a surface of the polyamide resin composition to the following measurement, a shape parameter k of a gamma distribution is 1.0 or more. [measurement] In a distribution image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition or an intensity information image of the metal ion image, a Voronoi division is performed with the center of the metal ion as a generating point to calculate the spatial area per metal ion on the surface. The spatial area of ​​each region obtained by the Voronoi division is calculated and classified according to spatial area, and a shape parameter k is calculated from a gamma distribution represented by the following formula. [ka] (wherein k is a shape parameter, θ is a scale parameter, and x is a spatial area)

[0014] The polyamide resin composition of the present embodiment, having the above-described configuration, can give a molded article that is excellent in rigidity, surface appearance, and bleed-out resistance when absorbing water, and is also suitable for high-cycle molding.

[0015] Hereinafter, each of the components of the polyamide resin composition of the present embodiment will be described in detail.

[0016] <Polyamide resin (A)> The polyamide resin (A) is not particularly limited, but examples thereof include aliphatic polyamides (Aa), semi-aromatic polyamides (Ab) containing diamine units and dicarboxylic acid units, and mixtures thereof. The polyamide resin (A) may be one type alone or two or more types in combination.

[0017] <Aliphatic polyamide (Aa)> The aliphatic polyamide (Aa) preferably contains one or more units (Aa-1) selected from the group consisting of lactam units and aminocarboxylic acid units, or contains aliphatic dicarboxylic acid units (Aa-2) and aliphatic diamine units (Aa-3).

[0018] [One or more units (Aa-1) selected from the group consisting of lactam units and aminocarboxylic acid units] The aliphatic polyamide (Aa) may contain one or more units (Aa-1) selected from the group consisting of lactam units and aminocarboxylic acid units. By containing such units, the polyamide tends to have excellent toughness. The term "lactam unit and aminocarboxylic acid unit" used herein means a (condensed) polymerized lactam and aminocarboxylic acid.

[0019] The lactam constituting the lactam unit is not particularly limited, but is preferably a lactam having 4 to 14 carbon atoms, and more preferably a lactam having 6 to 12 carbon atoms. Specific examples of lactams include, but are not limited to, butyrolactam, pivalolactam, ε-caprolactam, caprylolactam, enantholactam, undecanolactam, laurolactam (dodecanolactam), and the like. Among them, the lactam is preferably ε-caprolactam or laurolactam, and more preferably ε-caprolactam. By including lactam units derived from such lactams, the polyamide resin composition tends to have better toughness. In addition, the term "lactam constituting a lactam unit" used herein means a lactam capable of being polymerized (condensed).

[0020] The amino carboxylic acid constituting the amino carboxylic acid unit is not particularly limited, but is preferably an amino carboxylic acid having 4 to 14 carbon atoms, and more preferably an amino carboxylic acid having 6 to 12 carbon atoms. Specific examples of aminocarboxylic acids include, but are not limited to, ω-aminocarboxylic acids, which are compounds formed by ring-opening of lactams, and α,ω-amino acids. In addition, the aminocarboxylic acid is preferably a linear or branched saturated aliphatic carboxylic acid having 4 to 14 carbon atoms and substituted with an amino group at the ω-position. Examples of such aminocarboxylic acids include, but are not limited to, 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. In addition, examples of aminocarboxylic acids include paraaminomethylbenzoic acid. The term "amino carboxylic acid constituting the amino carboxylic acid unit" used herein means an amino carboxylic acid capable of being polymerized (condensed).

[0021] The lactam and aminocarboxylic acid constituting the lactam unit and the aminocarboxylic acid unit may each be used alone or in combination of two or more kinds.

[0022] [Aliphatic dicarboxylic acid unit (Aa-2)] Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit (Aa-2) include, but are not limited to, linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms, such as malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and diglycolic acid.

[0023] The aliphatic dicarboxylic acid preferably contains an aliphatic dicarboxylic acid having 6 or more carbon atoms, since the polyamide resin composition tends to have better heat resistance, fluidity, toughness, low water absorption, rigidity, etc. The aliphatic dicarboxylic acid having 6 or more carbon atoms is not particularly limited, and examples thereof include adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, etc. Among these, adipic acid, sebacic acid, or dodecanedioic acid is more preferable from the viewpoint of the heat resistance, etc., of the polyamide resin composition.

[0024] The aliphatic dicarboxylic acids constituting the aliphatic dicarboxylic acid unit (Aa-2) may be used alone or in combination of two or more.

[0025] In addition, the aliphatic polyamide (Aa) may further contain units derived from a polyvalent carboxylic acid having three or more valences, such as trimellitic acid, trimesic acid, and pyromellitic acid, as necessary, within a range that does not impair the effects of the polyamide resin composition of the present embodiment. The trivalent or higher polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0026] [Aliphatic diamine unit (Aa-3)] The aliphatic diamine constituting the aliphatic diamine unit (Aa-3) may be linear or branched.

[0027] Examples of the linear aliphatic diamine constituting the aliphatic diamine unit (Aa-3) include, but are not limited to, linear saturated aliphatic diamines having 2 to 20 carbon atoms, such as ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine.

[0028] Examples of branched aliphatic diamines (diamines constituting a diamine unit having a substituent branched from the main chain) constituting the aliphatic diamine unit (Aa-3) include, but are not limited to, branched saturated aliphatic diamines having 3 to 20 carbon atoms, such as 2-methylpentamethylenediamine (also referred to as 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also referred to as 2-methyloctamethylenediamine), and 2,4-dimethyloctamethylenediamine. Among these, 2-methylpentamethylenediamine or 2-methyl-1,8-octanediamine is preferred, and 2-methylpentamethylenediamine is more preferred. By including the aliphatic diamine unit (Aa-3) derived from such an aliphatic diamine, the polyamide resin composition tends to have better heat resistance, rigidity, and the like.

[0029] The number of carbon atoms in the aliphatic diamine unit (Aa-3) is more preferably 6 to 12, and even more preferably 6 to 10. When the number of carbon atoms is equal to or more than the lower limit, the heat resistance tends to be better, while when the number of carbon atoms is equal to or less than the upper limit, the crystallinity and releasability tend to be better.

[0030] The aliphatic diamine constituting the aliphatic diamine unit may be used alone or in combination of two or more kinds.

[0031] The aliphatic polyamide (Aa) may further contain units derived from a polyvalent aliphatic amine having three or more valences, such as bishexamethylenetriamine, as necessary, within a range that does not impair the effects of the polyamide resin composition of the present embodiment. The trivalent or higher polyvalent aliphatic amines may be used alone or in combination of two or more kinds.

[0032] Specific examples of the aliphatic polyamide (Aa) include polyamide 6 (PA6) and polyamide 66 (PA66). PA6 is considered to be a suitable material for automotive parts because of its excellent mechanical properties, appearance, moldability, and toughness. PA66 has excellent heat resistance, especially mechanical properties at high temperatures.

[0033] [Aliphatic polyamide (Aa) content] When the polyamide resin (A) is a mixture of aliphatic polyamide (A-a) and semi-aromatic polyamide (Ab), the content of the aliphatic polyamide (Aa) is preferably 50 parts by mass or more and 99 parts by mass or less, more preferably 50 parts by mass or more and 90 parts by mass or less, even more preferably 60 parts by mass or more and 85 parts by mass or less, even more preferably 65 parts by mass or more and 82 parts by mass or less, particularly preferably 70 parts by mass or more and 80 parts by mass or less, and most preferably 75 parts by mass or more and 80 parts by mass or less. When the content of the aliphatic polyamide (Aa) is within the above range, a polyamide resin composition that is excellent in mechanical properties, moldability, bleed-out resistance, and laser printability and is suitable for high-cycle molding tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) typified by glass fiber described later tends to have a more excellent surface appearance.

[0034] <Semi-aromatic polyamide (Ab)> The semi-aromatic polyamide (Ab) is a polyamide containing a diamine unit (Abb) and a dicarboxylic acid unit (Aba). When the aliphatic polyamide (Aa) and the semi-aromatic polyamide (Ab) are combined in the polyamide resin (A) of the present embodiment, the fatty acid metal salt (B) tends to be well dispersed on the surface of the molded article during molding.

[0035] The semi-aromatic polyamide (Ab) preferably contains 20 mol % or more and 80 mol % or less of aromatic structural units, more preferably 30 mol % or more and 70 mol % or less of aromatic structural units, and even more preferably 40 mol % or more and 60 mol % or less of aromatic structural units, based on all structural units of the semi-aromatic polyamide (Ab). The term "aromatic structural unit" used herein means an aromatic diamine unit and an aromatic dicarboxylic acid unit.

[0036] [Dicarboxylic acid unit (Aba)] The dicarboxylic acid unit (Aba) may contain, for example, an aromatic dicarboxylic acid unit, an aliphatic dicarboxylic acid unit, an alicyclic dicarboxylic acid unit, etc., but is not particularly limited thereto. Among these, it is preferable that the dicarboxylic acid unit contains an isophthalic acid unit. The content of isophthalic acid units is preferably 50 mol% or more, more preferably 65 mol% or more, even more preferably 70 mol% or more, even more preferably 75 mol% or more, particularly preferably 80% or more and 100 mol% or less, and most preferably 100 mol%, based on 100 mol% of all dicarboxylic acid units (Aba) constituting the semi-aromatic polyamide (Ab). When the ratio of isophthalic acid units in the dicarboxylic acid units (Aba) is equal to or more than the above lower limit, a polyamide resin composition tends to be obtained which is improved in all of mechanical properties, particularly water absorption rigidity, hot rigidity, fluidity, surface appearance, and the like. The ratio of a predetermined monomer unit constituting the semi-aromatic polyamide (Ab) can be measured by nuclear magnetic resonance spectroscopy (NMR) or the like.

[0037] (aromatic dicarboxylic acid unit) Examples of the aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit include, but are not limited to, dicarboxylic acids having a phenyl group, a naphthyl group, etc., in addition to the above-mentioned isophthalic acid. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent. The substituent is not particularly limited, but examples thereof include alkyl groups having 1 to 4 carbon atoms, aryl groups having 6 to 10 carbon atoms, arylalkyl groups having 7 to 10 carbon atoms, halogen groups such as chloro and bromo groups, silyl groups having 1 to 6 carbon atoms, sulfonic acid groups and salts thereof (sodium salts, etc.).

[0038] In addition to the above-mentioned isophthalic acid, specific examples of the aromatic dicarboxylic acid include, but are not limited to, aromatic dicarboxylic acids having 8 to 20 carbon atoms, which are unsubstituted or substituted with a specific substituent, such as terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodiumsulfoisophthalic acid. The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more kinds.

[0039] (Aliphatic dicarboxylic acid unit) Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit include, but are not limited to, linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms, such as malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and diglycolic acid.

[0040] (alicyclic dicarboxylic acid unit) Examples of alicyclic dicarboxylic acids constituting an alicyclic dicarboxylic acid unit (hereinafter also referred to as an "alicyclic dicarboxylic acid unit") include, but are not limited to, alicyclic dicarboxylic acids having an alicyclic structure with 3 to 10 carbon atoms, and alicyclic dicarboxylic acids having an alicyclic structure with 5 to 10 carbon atoms are preferred. Examples of such alicyclic dicarboxylic acids include, but are not limited to, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. Among these, 1,4-cyclohexanedicarboxylic acid is preferred. The alicyclic dicarboxylic acid constituting the alicyclic dicarboxylic acid unit may be used alone or in combination of two or more kinds.

[0041] The alicyclic group of the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent, which may include, but is not limited to, an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, or a tert-butyl group.

[0042] In the semi-aromatic polyamide (Ab), preferred dicarboxylic acid units (Aba) other than isophthalic acid units include aromatic dicarboxylic acid units other than isophthalic acid units, and aromatic dicarboxylic acid units other than isophthalic acid units having 8 or more carbon atoms are more preferred. When such a dicarboxylic acid unit (Aba) is contained, the mechanical properties of the polyamide resin composition, in particular, water absorption rigidity, hot rigidity, fluidity, surface appearance, and the like tend to be more excellent.

[0043] In this specification, the dicarboxylic acid constituting the dicarboxylic acid unit (Aba) is not limited to the compounds described above as the dicarboxylic acid, and may be a compound equivalent to the above dicarboxylic acid. The term "compound equivalent to a dicarboxylic acid" used herein means a compound that can have a dicarboxylic acid structure similar to the dicarboxylic acid structure derived from the dicarboxylic acid. Examples of such compounds include, but are not limited to, anhydrides and halides of dicarboxylic acids.

[0044] In addition, the semi-aromatic polyamide (Ab) may further contain units derived from a polyvalent carboxylic acid having three or more valences, such as trimellitic acid, trimesic acid, and pyromellitic acid, as necessary, within a range that does not impair the effects of the polyamide resin composition of this embodiment. The trivalent or higher polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0045] [Diamine unit (Abb)] The diamine unit (Abb) constituting the semi-aromatic polyamide (Ab) may contain, for example, an aromatic diamine acid unit, an aliphatic diamine unit, an alicyclic diamine unit, etc., but is not particularly limited thereto. Among them, it is preferable to contain a diamine unit having 4 to 10 carbon atoms. The content of the diamine units having 4 to 10 carbon atoms is preferably 50 mol% or more, more preferably 80 mol% or more and 100 mol% or less, even more preferably 90 mol% or more and 100 mol% or less, and particularly preferably 100 mol%, relative to 100 mol% of all diamine units (Abb) constituting the semi-aromatic polyamide (Ab). When the content of diamine units having 4 to 10 carbon atoms in the diamine units (Abb) is equal to or more than the above lower limit, a polyamide resin composition tends to be obtained which is improved in all of the mechanical properties, particularly water absorption rigidity, hot rigidity, fluidity, surface appearance, bleed-out resistance, and the like.

[0046] (Aliphatic diamine unit) Examples of aliphatic diamines constituting the aliphatic diamine unit include, but are not limited to, linear saturated aliphatic diamines having 4 to 20 carbon atoms, such as ethylene diamine, propylene diamine, tetramethylene diamine, pentamethylene diamine, hexamethylene diamine, heptamethylene diamine, octamethylene diamine, nonamethylene diamine, decamethylene diamine, undecamethylene diamine, dodecamethylene diamine, and tridecamethylene diamine.

[0047] (alicyclic diamine unit) Examples of alicyclic diamines (hereinafter also referred to as "alicyclic diamines") constituting the alicyclic diamine unit include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-cyclopentanediamine, and the like.

[0048] (aromatic diamine unit) The aromatic diamine constituting the aromatic diamine unit is not limited to the following, so long as it is a diamine containing an aromatic group, and examples thereof include metaxylylenediamine.

[0049] The diamines constituting the diamine unit (Abb) may be used alone or in combination of two or more.

[0050] Among the diamine units (Abb), an aliphatic diamine unit is preferred, a diamine unit having a linear saturated aliphatic group having 4 to 10 carbon atoms is more preferred, a diamine unit having a linear saturated aliphatic group having 6 to 10 carbon atoms is even more preferred, and a hexamethylenediamine unit is particularly preferred. By including such a diamine unit, the polyamide resin composition tends to have better mechanical properties, particularly better rigidity when absorbing water, better rigidity when hot, better fluidity, and better surface appearance.

[0051] In addition, the semi-aromatic polyamide (Ab) may further contain units derived from a polyvalent aliphatic amine having three or more valences, such as bishexamethylenetriamine, as necessary, within a range that does not impair the effects of the polyamide resin composition of this embodiment. The trivalent or higher polyvalent aliphatic amines may be used alone or in combination of two or more kinds.

[0052] As the semi-aromatic polyamide (Ab), polyamide 6I (polyhexamethylene isophthalamide), polyamide 6I / 6T, polyamide MXD6, polyamide 9I, or polyamide 10I is preferred, and polyamide 6I is more preferred. Polyamide 6I is considered to be a suitable material for automobile parts because of its excellent heat resistance, moldability, and flame retardancy.

[0053] [Semi-aromatic polyamide (Ab) content] When the polyamide resin (A) is a mixture of aliphatic polyamide (A-a) and semi-aromatic polyamide (Ab), the content of the semi-aromatic polyamide (Ab) is preferably 1 part by mass or more and 50 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, even more preferably 15 parts by mass or more and 40 parts by mass or less, even more preferably 18 parts by mass or more and 35 parts by mass or less, particularly preferably 20 parts by mass or more and 30 parts by mass or less, and most preferably 20 parts by mass or more and 25 parts by mass or less, relative to 100 parts by mass of the polyamide resin (A) (total of the aliphatic polyamide (Aa) and the semi-aromatic polyamide (Ab)). When the content of the semi-aromatic polyamide (Ab) is within the above range, a polyamide resin composition that is excellent in mechanical properties, moldability, bleed-out resistance, and laser printability and is suitable for high-cycle molding tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber described later tends to have a more excellent surface appearance.

[0054] <End-capping agent> The ends of the polyamide resin (A) may be capped with a known end-capping agent. Such an end-capping agent can also be added as a molecular weight regulator when producing the polyamide resin (A) from the above-mentioned dicarboxylic acid and diamine, and one or more selected from the group consisting of lactam and aminocarboxylic acid, which are used as necessary.

[0055] Examples of the end-capping agent include, but are not limited to, monocarboxylic acids, monoamines, acid anhydrides such as phthalic anhydride, monoisocyanates, monoacid halides, monoesters, and monoalcohols. Among these, monocarboxylic acids and monoamines are preferred. By capping the terminals of the polyamide resin (A) with an end-capping agent, the polyamide resin composition tends to have better thermal stability.

[0056] The end-capping agent may be used alone or in combination of two or more kinds.

[0057] The monocarboxylic acid that can be used as the end-capping agent may be any one that is reactive with amino groups that may be present at the ends of the polyamide resin (A), and includes, but is not limited to, aliphatic monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; and aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid. In particular, it is preferable that the terminals of the semi-aromatic polyamide (Ab) are blocked with acetic acid from the viewpoints of fluidity and mechanical strength. The monocarboxylic acid may be used alone or in combination of two or more kinds.

[0058] The monoamine that can be used as the end-capping agent may be any monoamine that is reactive with a carboxy group that may be present at the end of the polyamide resin (A), and includes, but is not limited to, aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; and aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine. The monoamines may be used alone or in combination of two or more kinds.

[0059] A polyamide resin composition containing a polyamide resin (A) end-capped with an end-capping agent tends to be superior in heat resistance, flowability, toughness, low water absorbency, and rigidity.

[0060] <Production method of polyamide resin (A)> The method for producing the polyamide resin (A) will be described. In producing the polyamide resin (A), the amount of dicarboxylic acid added and the amount of diamine added are preferably approximately the same molar amount. Taking into consideration the amount of diamine that escapes to the outside of the reaction system during the polymerization reaction, the molar amount of the total diamine relative to the total molar amount of dicarboxylic acid is preferably 0.9 to 1.2, more preferably 0.95 to 1.1, and even more preferably 0.98 to 1.05.

[0061] The method for producing the polyamide resin (A) can include, but is not limited to, the following polymerization step (1) or (2). (1) A step of polymerizing one or more members selected from the group consisting of lactams constituting lactam units and aminocarboxylic acids constituting aminocarboxylic acid units to obtain a polymer. (2) A step of polymerizing a combination of a dicarboxylic acid constituting the dicarboxylic acid unit and a diamine constituting the diamine unit to obtain a polymer.

[0062] The method for producing the polyamide resin (A) preferably further comprises, after the polymerization step, an increasing step of increasing the degree of polymerization of the polyamide, and may further comprise, as necessary, a capping step of capping the ends of the resulting polymer with a terminal capping agent after the polymerization step and the increasing step.

[0063] Specific examples of the method for producing the polyamide resin (A) include various methods as exemplified by the following 1) to 4). 1) A method in which an aqueous solution or suspension of one or more selected from the group consisting of lactams, aminocarboxylic acids, dicarboxylic acid-diamine salts, and mixtures of dicarboxylic acids and diamines is heated and polymerized while maintaining the molten state (hereinafter, sometimes referred to as the "thermal melt polymerization method"). 2) A method in which the degree of polymerization of polyamide obtained by hot melt polymerization is increased while maintaining the polyamide in a solid state at a temperature below the melting point (hereinafter sometimes referred to as "hot melt polymerization / solid-state polymerization method"). 3) A method in which one or more members selected from the group consisting of dicarboxylic acid-diamine salts, mixtures of dicarboxylic acids and diamines, lactams, and aminocarboxylic acids are polymerized while maintaining the solid state (hereinafter, sometimes referred to as the "solid-state polymerization method"). 4) A method of polymerization using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method").

[0064] Among them, as a specific method for producing the polyamide resin (A), a production method including a hot melt polymerization method is preferable. When producing the polyamide resin (A) by the hot melt polymerization method, it is preferable to maintain the molten state until the polymerization is completed. In order to maintain the molten state, it is necessary to produce the polyamide resin under polymerization conditions suitable for the polyamide resin. Examples of the polymerization conditions include the following conditions. First, the polymerization pressure in the hot melt polymerization method is set to 14 kg / cm. 2 More than 25kg / cm 2 Heating is continued while controlling the pressure in the vessel to below atmospheric pressure (gauge pressure is 0 kg / cm 2) over 30 minutes or more until the blood pressure drops to 0.

[0065] In the method for producing the polyamide resin (A), the polymerization form is not particularly limited, and may be a batch type or a continuous type. The polymerization apparatus used for producing the polyamide resin (A) is not particularly limited, and known apparatuses can be used. Specific examples of the polymerization apparatus include an autoclave type reactor, a tumbler type reactor, and an extruder type reactor (such as a kneader).

[0066] Hereinafter, as a method for producing polyamide resin (A), a method for producing polyamide resin (A) by a batch-type hot melt polymerization method will be specifically described, but the method for producing polyamide resin (A) is not limited thereto. First, an aqueous solution containing about 40% to 60% by mass of raw material components of polyamide resin (A) (lactam, aminocarboxylic acid, or mixture of dicarboxylic acid and diamine) is prepared. Then, the aqueous solution is concentrated to about 65% to 90% by mass in a concentration tank operated at a temperature of 110°C to 180°C and a pressure of about 0.035 MPa to 0.6 MPa (gauge pressure) to obtain a concentrated solution. The concentrated solution obtained is then transferred to an autoclave, and heating is continued until the pressure in the autoclave reaches about 1.2 MPa or more and 2.2 MPa or less (gauge pressure). Next, in the autoclave, the pressure is maintained at about 1.2 MPa to 2.2 MPa (gauge pressure) while removing at least one of water and gas components. Next, when the temperature reaches about 220° C. to 260° C., the pressure is reduced to atmospheric pressure (gauge pressure: 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure can be reduced as necessary to effectively remove the by-product water. The autoclave is then pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave as a strand. The extruded strand is cooled and cut to obtain pellets of the polyamide resin (A).

[0067] <Polymer end of polyamide resin (A)> The polymer terminals of the polyamide resin (A) are not particularly limited, but can be classified and defined as follows: 1) to 4). That is, 1) amino terminus, 2) carboxyl terminus, 3) terminus with a capping agent, and 4) other terminus. 1) The amino terminal is a polymer end having an amino group (-NH2 group) and originates from the diamine raw material. 2) The carboxyl terminal is a polymer terminal having a carboxyl group (-COOH group) and originates from the dicarboxylic acid used as the raw material. 3) The term "terminals formed by a capping agent" refers to terminals formed when a capping agent is added during polymerization. Examples of the capping agent include the above-mentioned terminal capping agents. 4) Other terminals are polymer terminals not classified into the above 1) to 3), and examples of such terminals include terminals generated by deammonia reaction of amino terminals and terminals generated by decarboxylation of carboxyl terminals.

[0068] <Characteristics of polyamide resin (A)> [Weight average molecular weight Mw] The weight average molecular weight Mw can be used as an index of the molecular weight of the polyamide resin (A). The weight average molecular weight Mw of the polyamide resin (A) is preferably 10,000 to 50,000, more preferably 17,000 to 40,000, even more preferably 20,000 to 34,000, even more preferably 23,000 to 33,500, particularly preferably 25,000 to 33,000, and most preferably 26,000 to 32,000. When the weight average molecular weight Mw is within the above range, a polyamide resin composition having excellent mechanical properties, particularly water absorption rigidity, hot rigidity, fluidity, releasability, etc., can be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber, which will be described later, tends to have a more excellent surface appearance. As a method for controlling the Mw of the polyamide resin (A) within the above range, for example, an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab) each having an Mw within the above range may be used. The weight average molecular weight (Mw) can be measured by using GPC (gel permeation chromatography) as described in the Examples below.

[0069] [Molecular weight distribution Mw / Mn] The molecular weight distribution of the polyamide resin (A) is indicated by the weight average molecular weight Mw / number average molecular weight Mn. The Mw / Mn of the polyamide resin (A) is 1.0 or more and preferably 2.4 or less, more preferably 1.7 to 2.3, more preferably 1.8 to 2.2, and more preferably 1.9 to 2.1. When the Mw / Mn is within the above range, a polyamide resin composition having better fluidity and the like tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) such as glass fiber, which will be described later, tends to have better surface appearance. As a method for controlling the Mw / Mn of the polyamide resin (A) within the above range, when the semi-aromatic polyamide (Ab) is contained, the molecular weight distribution Mw of the semi-aromatic polyamide (Ab) may be adjusted. (A-b) / Mn (A-b) It is important that the Mw / Mn ratio is within the above-mentioned range. When the molecular structure of the polyamide resin (A) contains many aromatic compound units, the molecular weight distribution (Mw / Mn) tends to increase with increasing molecular weight. A high molecular weight distribution indicates a high proportion of polyamide molecules having a three-dimensional molecular structure, and the three-dimensional molecular structure tends to progress further during high-temperature processing, resulting in a decrease in fluidity. For this reason, in polyamide resin compositions further containing an inorganic filler (D) such as glass fiber (described later), there is a risk of the surface appearance being deteriorated, so the molecular weight distribution Mw / Mn of the semi-aromatic polyamide (Ab) is set to 100%. (A-b) / Mn (A-b) By controlling the value to be equal to or less than the upper limit, the surface appearance can be improved. The Mw / Mn of the polyamide resin (A) can be calculated using the weight average molecular weight Mw and the number average molecular weight Mn obtained by GPC, as described in the Examples below.

[0070] <Characteristics of Aliphatic Polyamide (Aa)> [Weight average molecular weight Mw (A-a) ] The weight average molecular weight Mw is an index of the molecular weight of the aliphatic polyamide (Aa). (A-a) The Mw of aliphatic polyamide (Aa) can be used. (A-a) is preferably 10,000 or more and 50,000 or less, more preferably 15,000 or more and 45,000 or less, even more preferably 20,000 or more and 40,000 or less, and particularly preferably 25,000 or more and 37,000 or less. Mw (A-a) Within the above range, a polyamide resin composition having excellent mechanical properties, particularly water absorption rigidity, hot rigidity, flowability, etc., tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) such as glass fiber, which will be described later, tends to have excellent surface appearance. The weight average molecular weight Mw(Aa) can be measured using GPC.

[0071] [Molecular weight distribution Mw (A-a) / Mn (A-a) ] The molecular weight distribution of aliphatic polyamide (Aa) is the weight average molecular weight Mw (A-a) / number average molecular weight Mn (A-a) is used as an indicator. Molecular weight distribution Mw of aliphatic polyamide (Aa) (A-a) / Mn (A-a) The molecular weight distribution Mw can be 1.0 or more, preferably 1.8 to 2.5, and more preferably 1.9 to 2.4. (A-a) / Mn (A-a) Within the above range, a polyamide resin composition having better flowability tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) typified by glass fiber described below tends to have better surface appearance. Molecular weight distribution Mw (A-a) / Mn (A-a)Examples of the method for controlling the above range include a method of adding a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite as an additive during the hot melt polymerization of the aliphatic polyamide (Aa), and a method of controlling polymerization conditions such as heating conditions and reduced pressure conditions. Molecular weight distribution Mw (A-a) / Mn (A-a) The weight average molecular weight Mw was measured using GPC. (A-a) , number average molecular weight Mn (A-a) It can be calculated using:

[0072] <Characteristics of semi-aromatic polyamide (Ab)> [Weight average molecular weight Mw (A-b) ] The weight average molecular weight Mw is an index of the molecular weight of the semi-aromatic polyamide (Ab). (A-b) Weight average molecular weight Mw (A-b) is preferably 10,000 or more and 50,000 or less, more preferably 13,000 or more and 40,000 or less, even more preferably 15,000 or more and 35,000 or less, particularly preferably 18,000 or more and 30,000 or less, and most preferably 19,000 or more and 29,000 or less. Weight average molecular weight Mw (A-b) Within the above range, the polyamide resin composition tends to have better mechanical properties, particularly better water absorption rigidity, hot rigidity, flowability, etc. Furthermore, in a polyamide resin composition further containing an inorganic filler (D) typified by glass fiber described below, the surface appearance tends to be better. The weight average molecular weight Mw (A-b) The measurement can be performed using GPC.

[0073] [Molecular weight distribution Мw (A-b) / Mn (A-b) ] The molecular weight distribution of the semi-aromatic polyamide (Ab) is the weight average molecular weight Mw (A-b) / number average molecular weight Mn (A-b) is used as an indicator. Molecular weight distribution Mw of semi-aromatic polyamide (Ab) (A-b) / Mn (A-b)can be 1.0 or more, preferably 2.4 or less, more preferably 1.7 or more and 2.4 or less, even more preferably 1.8 or more and 2.3 or less, particularly preferably 1.9 or more and 2.2 or less, and most preferably 1.9 or more and 2.1 or less. Molecular weight distribution Mw (A-b) / Mn (A-b) Within the above range, a polyamide resin composition having better flowability tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) typified by glass fiber described below tends to have better surface appearance. Molecular weight distribution Mw (A-b) / Mn (A-b) As a method for controlling within the above range, for example, a method of adding a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite as an additive during the thermal melt polymerization of the semi-aromatic polyamide (Ab) can be mentioned. In addition, a method of controlling the polymerization conditions such as heating conditions and reduced pressure conditions can be mentioned, and it is important to complete the polycondensation reaction at the lowest possible temperature and in the shortest possible time. In particular, when the semi-aromatic polyamide (Ab) is an amorphous polyamide, the reaction temperature can be lowered since it does not have a melting point. If the molecular structure of polyamide (A) contains a large number of aromatic compound units, the molecular weight distribution Mw (A-b) / Mn (A-b) A high molecular weight distribution indicates that the proportion of polyamide molecules having a three-dimensional molecular structure is high, and the three-dimensional molecular structure tends to progress further during high-temperature processing, resulting in a decrease in fluidity. Therefore, in polyamide resin compositions further containing an inorganic filler (D) such as glass fiber, which will be described later, there is a risk of the surface appearance being deteriorated, so the molecular weight distribution Mw (A-b) / Mn (A-b) By controlling the value to be equal to or less than the upper limit, the surface appearance can be improved. The molecular weight distribution Mw (A-b) / Mn (A-b) The weight average molecular weight Mw was measured using GPC. (A-b) , number average molecular weight Mn (A-b) It can be calculated using:

[0074] <Fatty acid metal salt (B)> The fatty acid metal salt (B) is a fatty acid metal salt of a metal containing an alkali metal ion and / or an alkaline earth metal ion. That is, the metal element constituting the fatty acid metal salt (B) is not particularly limited as long as it contains an alkali metal and / or an alkaline earth metal, and may also contain, for example, zinc, aluminum, etc. Examples of the alkali metal include sodium and potassium. Examples of alkaline earth metals include calcium and magnesium. Of these, sodium, potassium, calcium, magnesium, or aluminum is more preferable.

[0075] The fatty acid constituting the fatty acid metal salt (B) may be either chain-like or cyclic, but is preferably chain-like. In addition, when it is chain-like, it may be either linear or branched, but is preferably linear. Examples of linear fatty acids include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, and melissic acid.

[0076] The fatty acid metal salt (B) is not particularly limited as long as it is a combination of a metal element, including an alkali metal and / or an alkaline earth metal, and a fatty acid. From the viewpoints of nucleation effect and flowability, however, metal salts of higher fatty acids having a terminal hydrocarbon group with 12 or more carbon atoms are preferred, and metal salts of higher fatty acids having a terminal hydrocarbon group with 19 or more carbon atoms are more preferred. Moreover, such fatty acid metal salt (B) is preferably a montanate salt, and more preferably sodium montanate or calcium montanate. These fatty acid metal salts (B) may be used alone or in combination of two or more.

[0077] [Content of fatty acid metal salt (B)] The content of the fatty acid metal salt (B) is from 0.05 to 5.00 parts by mass, preferably from 0.05 to 1.00 parts by mass, and more preferably from 0.10 to 0.50 parts by mass, per 100 parts by mass of the polyamide resin (A). When the content of the fatty acid metal salt (B) is equal to or more than the lower limit, a polyamide resin composition suitable for high cycle molding can be obtained. On the other hand, when the content of the fatty acid metal salt (B) is equal to or less than the upper limit, a polyamide resin composition having excellent mechanical properties such as toughness and rigidity, particularly excellent water absorption properties, can be obtained without impairing the properties of the polyamide resin (A).

[0078] <Fatty acid amide compounds (C)> The polyamide resin composition of the present embodiment can contain a fatty acid amide compound (C). When the polyamide resin composition of the present embodiment contains the fatty acid amide compound (C), the dispersibility of the fatty acid metal salt (B) is improved, and a polyamide resin composition having excellent molding cycle properties and excellent bleed-out resistance and laser printability when formed into a molded product can be obtained.

[0079] The fatty acid amide compound (C) is preferably one or more selected from the group consisting of amide compounds and bisamide compounds of an aliphatic carboxylic acid (fatty acid) having a terminal hydrocarbon group having from 9 to 30 carbon atoms. That is, the fatty acid amide compound (C) is preferably one or more selected from the group consisting of fatty acid amide compounds having a terminal hydrocarbon group having from 9 to 30 carbon atoms, and fatty acid bisamide compounds having a hydrocarbon group having from 9 to 30 carbon atoms at one or both terminals. The terminal hydrocarbon group of the fatty acid amide compound (C) more preferably has from 12 to 27 carbon atoms, and even more preferably has from 17 to 21 carbon atoms.

[0080] Examples of the fatty acid amide compound (C) include, but are not limited to, capric acid amide, lauric acid amide, palmitic acid amide, stearic acid amide, oleic acid amide, erucic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, N-oleyl oleic acid amide, N-methylol stearic acid amide, N,N'-methylene bisstearic acid amide, N,N'-ethylene biscapric acid amide, N,N'-ethylene bislauric acid amide, N,N'-ethylene bisstearic acid amide, N,N'-ethylene bisbehenic acid amide, N,N'-hexamethylene bisstearic acid amide, N,N'-hexamethylene bisbehenic acid amide, N,N'-ethylene bisoleic acid amide, N,N'-ethylene biserucic acid amide, N,N'-hexamethylene bisoleic acid amide, and the like. Among these, bisamide compounds are preferred, and N,N'-ethylenebisstearic acid amide or N-stearyl erucic acid amide is more preferred. These fatty acid amide compounds (C) may be used alone or in combination of two or more.

[0081] [Fatty acid amide compound (C) content] The content of the fatty acid amide compound (C) is preferably 0.01 parts by mass or more and 3.00 parts by mass or less, more preferably 0.05 parts by mass or more and 2.00 parts by mass or less, and even more preferably 0.10 parts by mass or more and 1.00 parts by mass or less, relative to 100 parts by mass of the polyamide resin (A). When the content of the fatty acid amide compound (C) is equal to or more than the lower limit, a polyamide resin composition having excellent processability can be obtained. On the other hand, when the content of the fatty acid amide compound (C) is equal to or less than the upper limit, a polyamide resin composition having excellent mechanical properties such as toughness and rigidity, particularly excellent water absorption properties can be obtained without impairing the properties of the polyamide resin (A).

[0082] In the polyamide resin composition, the ratio Bw / Cw of the mass Bw of the fatty acid metal salt (B) to the mass Cw of the fatty acid amide compound (C) is preferably 0.6 or more and 4.0 or less, more preferably 0.8 or more and 3.8 or less, even more preferably 1.0 or more and 3.5 or less, even more preferably 1.5 or more and 3.4 or less, and particularly preferably 2.0 or more and 3.0 or less. When the mass ratio Bw / Cw is equal to or more than the lower limit, the polyamide resin composition is more suitable for high cycle molding. When the mass ratio Bw / Cw is equal to or less than the upper limit, the polyamide resin composition is more excellent in surface appearance and mechanical properties.

[0083] The ratio Bn / Cn of the carbon number Bn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the carbon number Cn of the terminal hydrocarbon group of the fatty acid amide compound (C) is preferably more than 1.00 and not more than 2.00, more preferably 1.01 or more and not more than 2.00, even more preferably 1.10 or more and not more than 1.80, and even more preferably 1.35 or more and not more than 1.60. By having the carbon number ratio Bn / Cn exceeding or not less than the above lower limit, a polyamide resin composition that is more suitable for high-cycle molding and has excellent bleed-out resistance and laser printability after molding can be obtained. In addition, by having the carbon number ratio Bn / Cn not more than the upper limit, a polyamide resin composition that is excellent in surface appearance and mechanical properties can be obtained.

[0084] When the carbon number ratio Bn / Cn is within the above range, the fatty acid amide compound (C) acts as an emulsifier between the polyamide matrix and the fatty acid metal salt (B), so that the dispersibility of the fatty acid metal salt (B) in the polyamide resin composition can be dramatically improved. When the carbon number ratio Bn / Cn exceeds the above upper limit, the fatty acid amide compound (C) has low compatibility with the fatty acid metal salt (B), so that there is little interaction, and the dispersion diameter of the fatty acid metal salt (B) tends not to change. In addition, when the carbon number ratio Bn / Cn is equal to or less than the above lower limit, the compatibility between the fatty acid amide compound (C) and the fatty acid metal salt (B) becomes high, so that the fatty acid metal salt (B) is taken into the micelles of the fatty acid amide compound (C), which tends to prevent the bleeding of the fatty acid metal salt (B) during molding. Therefore, by controlling the carbon number ratio Bn / Cn within the above range, the fatty acid metal salt (B) does not become unevenly distributed on the surface of the molded article during molding, and is dispersed more uniformly. This makes it possible to obtain a polyamide resin composition that is more suitable for high-cycle molding without impairing the appearance, and that has excellent bleed-out resistance and laser printability after molding.

[0085] <Inorganic filler (D)> The polyamide resin composition of the present embodiment preferably further contains an inorganic filler (D). By containing the inorganic filler (D), the polyamide resin composition can be made more excellent in mechanical properties such as toughness and rigidity, and more suitable for high-cycle molding.

[0086] The inorganic filler (D) is not particularly limited, and examples thereof include glass fibers, carbon fibers, calcium silicate fibers, potassium titanate fibers, aluminum borate fibers, glass flakes, talc, kaolin, mica, hydrotalcite, zinc carbonate, calcium hydrogen phosphate, wollastonite, zeolite, boehmite, magnesium oxide, calcium silicate, sodium aluminosilicate, magnesium silicate, ketjen black, acetylene black, furnace black, carbon nanotubes, graphite, brass, copper, silver, aluminum, nickel, iron, calcium fluoride, montmorillonite, swellable fluoromica, and apatite. These inorganic fillers (D) may be used alone or in combination of two or more kinds. Among these, the inorganic filler (D) is preferably glass fiber, carbon fiber, glass flake, talc, kaolin, mica, calcium hydrogen phosphate, wollastonite, carbon nanotube, graphite, calcium fluoride, montmorillonite, expandable fluoromica, or apatite from the viewpoint of rigidity, strength, etc. Furthermore, the inorganic filler (D) is more preferably glass fiber or carbon fiber, and further preferably glass fiber.

[0087] When the inorganic filler (D) is glass fiber or carbon fiber, the number average fiber diameter (d) is preferably 3 μm or more and 30 μm or less, more preferably 5 μm or more and 17 μm or less. The weight average fiber length (L) is preferably 100 μm or more and 750 μm or less. Furthermore, the aspect ratio ((L) / (d)) of the number average fiber diameter (d) to the weight average fiber length (L) is preferably 3 or more and 100 or less, more preferably 10 or more and 100 or less. By using the glass fiber or carbon fiber having the above configuration, higher properties can be exhibited.

[0088] In particular, when the inorganic filler (D) is glass fiber, the number average fiber diameter (d) is preferably 3 μm to 30 μm, more preferably 5 μm to 17 μm, and particularly preferably 7 μm to 13 μm. The weight average fiber length (L) is more preferably 103 μm to 500 μm. Furthermore, the aspect ratio ((L) / (d)) is preferably 3 to 100.

[0089] The number average fiber diameter (d) and weight average fiber length (L) of the inorganic filler (D) can be measured by the following method. First, the polyamide resin composition is placed in an electric furnace, and the organic matter contained therein is incinerated. From the residue after the treatment, 100 or more inorganic fillers (D) are arbitrarily selected, and observed with a scanning electron microscope (SEM) to measure the fiber diameter (long diameter) of these inorganic fillers (D), thereby obtaining the number average fiber diameter (d). In addition, the fiber length is measured using an SEM photograph of the 100 or more inorganic fillers (D) taken at a magnification of 1000 times, thereby obtaining the weight average fiber length (L).

[0090] The content of the inorganic filler (D) in the polyamide resin composition is preferably 5 parts by mass or more and 200 parts by mass or less, more preferably 10 parts by mass or more and 200 parts by mass or less, even more preferably 20 parts by mass or more and 150 parts by mass or less, particularly preferably 30 parts by mass or more and 120 parts by mass or less, and most preferably 40 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of the polyamide resin (A). When the content of the inorganic filler (D) is equal to or more than the lower limit, the mechanical properties such as strength and rigidity of the polyamide resin composition are improved and the composition is more suitable for high cycle molding. On the other hand, when the content of the inorganic filler (D) is equal to or less than the upper limit, the polyamide resin composition can have a better surface appearance.

[0091] <Nigrosine (E)> The polyamide resin composition of the present embodiment may contain nigrosine (E). The polyamide resin composition of the present embodiment contains nigrosine (E), which has the effect of improving the dispersibility of the fatty acid metal salt (B) through interaction with the fatty acid metal salt (B), and therefore can be a polyamide resin composition that is excellent in molding cycle property, surface glossiness, and laser printability when formed into a molded product.

[0092] The content of nigrosine (E) in the polyamide resin composition is preferably more than 0 parts by mass and not more than 0.5 parts by mass, more preferably from 0.01 parts by mass to 0.3 parts by mass, and even more preferably from 0.05 parts by mass to 0.1 parts by mass, per 100 parts by mass of polyamide resin (A). When the content of nigrosine (E) is equal to or more than the lower limit, a polyamide resin composition having excellent molding cycle properties, surface glossiness, and laser markability when molded into a molded product can be obtained. On the other hand, when the content of nigrosine (E) is equal to or less than the upper limit, a polyamide resin composition having excellent laser markability can be obtained.

[0093] The nigrosine (E) contained in the polyamide resin composition of the present embodiment is a chloride ion (Cl - ) may be included. The chloride ion content in nigrosine (E) is preferably 5000 ppm or less by mass, more preferably 2500 ppm or less, and even more preferably 1000 ppm or less. By having the chloride ion content be 5000 ppm or less by mass, the interaction with the fatty acid metal salt (B) is appropriately adjusted, the dispersibility of the fatty acid metal salt (B) is improved, and the shape parameter k tends to be high.

[0094] The chloride ion content in the polyamide resin composition of the present embodiment is not particularly limited, but is preferably 5 ppm or less by mass in the polyamide resin composition, more preferably 2.5 ppm or less, and even more preferably 1 ppm or less. By making the chloride ion content 5 ppm or less by mass, the interaction with the fatty acid metal salt (B) is appropriately adjusted, the dispersibility of the fatty acid metal salt (B) becomes good, and the shape parameter k tends to be high. The chloride ion content in the polyamide resin composition can be adjusted by adjusting the chloride ion content of each component constituting the polyamide resin composition and the content ratio of each component.

[0095] <Other ingredients (F)> The polyamide resin composition of the present embodiment may contain other components (F) within the scope of not impairing the effects of the polyamide resin composition of the present embodiment. Examples of the other components (F) include heat stabilizers, other polymers, metal phosphites, metal hypophosphites, phosphite compounds, and other additives. The other component (F) may be used alone or in combination of two or more kinds.

[0096] [Heat stabilizer] Examples of the heat stabilizer include, but are not limited to, phenol-based heat stabilizers, phosphorus-based heat stabilizers, amine-based heat stabilizers, metal salts of elements in groups 3, 4, and 11 to 14 of the periodic table, and halides of alkali metals or alkaline earth metals.

[0097] Examples of the phenol-based heat stabilizer include, but are not limited to, hindered phenol compounds, etc. Hindered phenol compounds have the property of imparting excellent heat resistance and light resistance to resins such as polyamides and fibers.

[0098] Examples of the hindered phenol compound include, but are not limited to, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), pentaerythrityl-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], and the like. ester], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, 3,5-di-tert-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid. These hindered phenol compounds may be used alone or in combination of two or more. In particular, from the viewpoint of improving heat aging resistance, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] is preferred as the hindered phenol compound.

[0099] When a phenolic heat stabilizer is used, the content of the phenolic heat stabilizer in the polyamide resin composition is preferably 0.01% by mass or more and 1% by mass or less, more preferably 0.1% by mass or more and 1% by mass or less, based on the total mass of the polyamide resin composition. When the content of the phenolic heat stabilizer is within the above range, the extrusion processability and molding process stability of the polyamide resin composition can be further improved, and the amount of gas generation can be further reduced.

[0100] Examples of phosphorus-based heat stabilizers include, but are not limited to, pentaerythritol-type phosphite compounds, trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, octyl diphenyl phosphite, trisisodecyl phosphite, phenyl diisodecyl phosphite, phenyl di(tridecyl) phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl (tridecyl) phosphite, triphenyl phosphite, tris(nonyl) phosphite, phenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,4-di-tert-butyl-5-methylphenyl)phosphite, tris(butoxyethyl)phosphite, 4,4'-butylidene-bis(3-methyl-6-tert-butylphenyl-tetra-tridecyl)diphosphite, tetra(C12-C15 mixed alkyl)-4,4'-isopropylidene diphenyl diphosphite, 4,4'-isopropylidenebis(2-tert-butylphenyl)-di(no nylphenyl)phosphite, tris(biphenyl)phosphite, tetra(tridecyl)-1,1,3-tris(2-methyl-5-tert-butyl-4-hydroxyphenyl)butane diphosphite, tetra(tridecyl)-4,4'-butylidenebis(3-methyl-6-tert-butylphenyl)diphosphite, tetra(C1-C15 mixed alkyl)-4,4'-isopropylidene diphenyl diphosphite, tris(mono, dimixed nonylphenyl)phosphite, 4,4'-isopropylidenebis(2 -tert-butylphenyl)-di(nonylphenyl)phosphite, 9,10-di-hydro-9-oxa-9-oxa-10-phosphaphenanthrene-10-oxide, tris(3,5-di-tert-butyl-4-hydroxyphenyl)phosphite, hydrogenated-4,4'-isopropylidene diphenyl polyphosphite, bis(octylphenyl)-bis(4,4'-butylidenebis(3-methyl-6-tert-butylphenyl))-1,6-hexanol diphosphite, hexatridecyl-1,1,Examples of such phosphite include 3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)diphosphite, tris(4,4'-isopropylidenebis(2-tert-butylphenyl))phosphite, tris(1,3-stearoyloxyisopropyl)phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octylphosphite, 2,2-methylenebis(3-methyl-4,6-di-tert-butylphenyl)2-ethylhexylphosphite, tetrakis(2,4-di-tert-butyl-5-methylphenyl)-4,4'-biphenylene diphosphite, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite. These phosphorus-based heat stabilizers may be used alone or in combination of two or more. Among them, from the viewpoint of further improving the extrusion processability and molding process stability of the polyamide resin composition and reducing the amount of gas generated, the phosphorus-based heat stabilizer is preferably at least one selected from the group consisting of pentaerythritol-type phosphite compounds and tris(2,4-di-tert-butylphenyl)phosphite.

[0101] Examples of the pentaerythritol type phosphite compound include, but are not limited to, 2,6-di-tert-butyl-4-methylphenyl-phenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-methyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2-ethylhexyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-isodecyl-pentaerythritol diphosphite, 2, 6-di-tert-butyl-4-methylphenyl-lauryl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-isotridecyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-stearyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-cyclohexyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-benzyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl ethyl cellosolve-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-butylcarbitol-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-octylphenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-nonylphenyl-pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2,6-di-tert-butylphenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2,4-di-tert-butylphenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2,4-di-tert-octylphenyl-pentaerythritol diphosphite, 2,Examples of such diphosphite include 6-di-tert-butyl-4-methylphenyl-2-cyclohexylphenyl-pentaerythritol diphosphite, 2,6-di-tert-amyl-4-methylphenyl-phenyl pentaerythritol diphosphite, bis(2,6-di-tert-amyl-4-methylphenyl)pentaerythritol diphosphite, and bis(2,6-di-tert-octyl-4-methylphenyl)pentaerythritol diphosphite. These pentaerythritol-type phosphite compounds may be used alone or in combination of two or more.

[0102] Among them, from the viewpoint of reducing the amount of gas generated from the polyamide resin composition, the pentaerythritol-type phosphite compound is preferably one or more selected from the group consisting of bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-amyl-4-methylphenyl)pentaerythritol diphosphite, and bis(2,6-di-tert-octyl-4-methylphenyl)pentaerythritol diphosphite, and more preferably bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite.

[0103] When a phosphorus-based heat stabilizer is used, the content of the phosphorus-based heat stabilizer in the polyamide resin composition is preferably 0.01% by mass or more and 1% by mass or less, more preferably 0.1% by mass or more and 1% by mass or less, based on the total mass of the polyamide resin composition. When the content of the phosphorus-based heat stabilizer is within the above range, the extrusion processability and molding process stability of the polyamide resin composition can be further improved, and the amount of gas generation can be further reduced.

[0104] Examples of the amine-based heat stabilizer include, but are not limited to, 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(phenylacetoxy)-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, and 4-stearyloxy-2,2,6,6-tetramethylpiperidine. , 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-(ethylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(cyclohexylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(phenylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, bis(2,2,6,6-tetramethyl-4-piperidyl)-carbonate, bis( 2,2,6,6-tetramethyl-4-piperidyl)-oxalate, bis(2,2,6,6-tetramethyl-4-piperidyl)-malonate, bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)-adipate, bis(2,2,6,6-tetramethyl-4-piperidyl)-terephthalate, 1,2-bis(2,2,6,6-tetramethyl-4-piperidyloxy)-ethane, α,α'-bis(2,2,6,6-tetramethyl-4-piperidyloxy)-p-xylene, biphenyl Bis(2,2,6,6-tetramethyl-4-piperidyl)tolylene-2,4-dicarbamate, bis(2,2,6,6-tetramethyl-4-piperidyl)-hexamethylene-1,6-dicarbamate, tris(2,2,6,6-tetramethyl-4-piperidyl)-benzene-1,3,5-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)-benzene-1,3,4-tricarboxylate, 1-[2-{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy}butyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]2,2,6,6-tetramethylpiperidine, a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5,5)undecane]diethanol, and the like. These amine-based heat stabilizers may be used alone or in combination of two or more.

[0105] When an amine-based heat stabilizer is used, the content of the amine-based heat stabilizer in the polyamide resin composition is preferably 0.01% by mass or more and 1% by mass or less, more preferably 0.1% by mass or more and 1% by mass or less, based on the total mass of the polyamide resin composition. When the content of the amine-based heat stabilizer is within the above range, the extrusion processability and molding process stability of the polyamide resin composition can be further improved, and the amount of gas generation can be further reduced.

[0106] There are no particular limitations on the metal salts of elements in Groups 3, 4, and 11 to 14 of the periodic table, so long as they are salts of metals belonging to these groups. Among them, copper salts are preferred from the viewpoint of further improving the extrusion processability and molding process stability of the polyamide resin composition. Examples of such copper salts include, but are not limited to, copper halides, copper acetate, copper propionate, copper benzoate, copper adipate, copper terephthalate, copper isophthalate, copper salicylate, copper nicotinate, copper stearate, and copper complex salts in which copper is coordinated with a chelating agent.

[0107] Examples of copper halides include copper iodide, copper (I) bromide, copper (II) bromide, and copper (I) chloride. Examples of the chelating agent include ethylenediamine and ethylenediaminetetraacetic acid. These copper salts may be used alone or in combination of two or more. Among them, the copper salt is preferably at least one selected from the group consisting of copper iodide, copper (I) bromide, copper (II) bromide, copper (I) chloride, and copper acetate, and more preferably at least one selected from the group consisting of copper iodide and copper acetate. When the above-mentioned preferred copper salts are used, a polyamide resin composition is obtained which is more excellent in heat aging resistance and can more effectively suppress metal corrosion of the screw and cylinder during extrusion (hereinafter, may be simply referred to as "metal corrosion").

[0108] When a copper salt is used as a heat stabilizer, the content of the copper salt in the polyamide resin composition is preferably 0.01 to 0.60 parts by mass, more preferably 0.02 to 0.40 parts by mass, based on 100 parts by mass of the polyamide resin (A). When the content of the copper salt is within the above range, the extrusion processability and molding process stability of the polyamide resin composition can be further improved, and copper precipitation and metal corrosion can be more effectively suppressed.

[0109] In addition, the content of copper element derived from the above copper salt is set to 100% by mass of polyamide resin (A) from the viewpoint of improving the heat aging resistance of the polyamide resin composition. 6 The amount is preferably from 10 to 2000 parts by mass, more preferably from 30 to 1500 parts by mass, and even more preferably from 50 to 500 parts by mass, based on parts by mass (1 million parts by mass).

[0110] Examples of the alkali metal or alkaline earth metal halide include, but are not limited to, potassium iodide, potassium bromide, potassium chloride, sodium iodide, sodium chloride, and the like. These alkali metal or alkaline earth metal halides may be used alone or in combination of two or more. Among these, from the viewpoints of improving heat aging resistance and suppressing metal corrosion, the alkali metal or alkaline earth metal halide is preferably at least one selected from the group consisting of potassium iodide and potassium bromide, and more preferably potassium iodide.

[0111] When an alkali metal or alkaline earth metal halide is used, the content of the alkali metal or alkaline earth metal halide in the polyamide resin composition is preferably 0.05 to 20 parts by mass, more preferably 0.2 to 10 parts by mass, per 100 parts by mass of the polyamide resin (A). When the content of the alkali metal or alkaline earth metal halide is within the above range, the extrusion processability and molding process stability of the polyamide resin composition are further improved, and copper precipitation and metal corrosion can be more effectively suppressed.

[0112] The heat stabilizer components explained above may be used alone or in combination of two or more.

[0113] Among these, from the viewpoint of further improving the extrusion processability and molding process stability of the polyamide resin composition, a mixture of a copper salt and an alkali metal or alkaline earth metal halide is preferred as the heat stabilizer.

[0114] The content ratio of the copper salt and the alkali metal or alkaline earth metal halide is preferably 2 / 1 or more and 40 / 1 or less, more preferably 5 / 1 or more and 30 / 1 or less, in terms of the molar ratio of halogen to copper (halogen / copper).When the molar ratio of halogen to copper (halogen / copper) is within the above range, the extrusion processability and molding process stability of the polyamide resin composition can be further improved. In addition, when the molar ratio of halogen to copper (halogen / copper) is equal to or greater than the lower limit, copper precipitation and metal corrosion can be more effectively suppressed. On the other hand, when the molar ratio of halogen to copper (halogen / copper) is equal to or less than the upper limit, corrosion of the screw of the molding machine and the like can be more effectively prevented without substantially impairing mechanical properties (e.g., toughness).

[0115] [Other polymers] Other polymers may be added within a range that does not impair the effect of the polyamide resin composition of the present embodiment. The other polymers are not particularly limited as long as they are not polyamides, and examples thereof include polyesters, liquid crystal polyesters, polyphenylene sulfides, polyphenylene ethers, polycarbonates, polyarylates, phenolic resins, epoxy resins, acrylic resins, and styrene resins. The polyesters are not limited to the following, and examples thereof include polybutylene terephthalate, polytrimethylene terephthalate, polyethylene terephthalate, and polyethylene naphthalate.

[0116] The content of the other polymer is preferably 1 part by mass or more and 200 parts by mass or less, more preferably 5 parts by mass or more and 100 parts by mass or less, and even more preferably 5 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the polyamide (A). By having the content of the other polymer within the above range, a polyamide resin composition having excellent heat resistance and releasability can be obtained.

[0117] [Metal phosphites, metal hypophosphites] The polyamide resin composition of the present embodiment may contain at least one metal salt selected from the group consisting of metal phosphites and metal hypophosphites. Examples of the metal phosphites and metal hypophosphites include salts of phosphorous acid, hypophosphorous acid, pyrophosphorous acid, or diphosphorous acid with elements of Groups 1 and 2 of the Periodic Table, manganese, zinc, aluminum, ammonia, alkylamines, cycloalkylamines, or diamines. Among these, as the metal phosphite and metal hypophosphite, sodium hypophosphite, calcium hypophosphite, or magnesium hypophosphite is preferred. When the polyamide resin composition contains at least one selected from the group consisting of metal phosphites and metal hypophosphites, it is possible to obtain a polyamide resin composition having superior extrusion processability and molding process stability.

[0118] The content of at least one metal salt selected from the group consisting of metal phosphites and metal hypophosphites is preferably 0.001 part by mass or more and 1.0 part by mass or less, and more preferably 0.01 part by mass or more and 0.5 part by mass or less, per 100 parts by mass of the polyamide resin (A).

[0119] [Phosphite ester compounds] Specific examples of the phosphite ester compound include trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, octyl-diphenyl phosphite, trisisodecyl phosphite, phenyl diisodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl tridecyl phosphite, triphenyl phosphite, tributyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol-di-phosphite, bis( 2,6-di-tert-butyl-4-methylphenyl)pentaerythritol-di-phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, 4,4'-butylidene-bis(3-methyl-6-tert-butylphenyl-di-tridecyl)phosphite, 1,1,3-tris(2-methyl-4-ditridecylphosphite-5-tert-butyl-phenyl)butane, 4,4'-isopropylidenebis(phenyl-dialkyl phosphite), tris(2,4-di-tert-butylphenyl)phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol-di-phosphite, and the like. These phosphite compounds may be used alone or in combination of two or more. By adding a phosphite compound, it is possible to obtain a polyamide resin composition which is more excellent in extrusion processability and molding process stability.

[0120] The content of the phosphite compound is preferably from 0.01 to 1.0 part by mass, and more preferably from 0.05 to 0.5 part by mass, based on 100 parts by mass of the polyamide resin (A).

[0121] [Other additives] The polyamide resin composition of the present embodiment may contain other additives commonly used in polyamide resin compositions, provided that the effects of the polyamide resin composition of the present embodiment are not impaired. Examples of the other additives include colorants such as pigments and dyes (including colored masterbatches), flame retardants, fibrillating agents, fluorescent bleaching agents, plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, flow improvers, spreading agents, elastomers, etc.

[0122] When the polyamide resin composition of the present embodiment contains other additives, the content of the other additives varies depending on the type and use of the polyamide resin composition, and is not particularly limited as long as it is within a range that does not impair the effects of the polyamide resin composition of the present embodiment. For example, the content may be 0% by mass or more and 5% by mass or less, or 0.01% by mass or more and 1.5% by mass or less, relative to 100% by mass of the polyamide resin composition.

[0123] <Method of producing polyamide resin composition> The method for producing the polyamide resin composition is not particularly limited as long as it is a production method including a step of melt-kneading a polyamide resin (A) and a fatty acid metal salt (B), and, as necessary, a fatty acid amide compound (C), an inorganic filler (D), Nigrosine (E), and other components (F).

[0124] Examples of a method for mixing the above components (A) and (B), and, if necessary, each of the components (C) to (F), include the following method (1) or (2). (1) The above components (A) and (B), and, if necessary, each of the components (C) to (F), are mixed using a Henschel mixer or the like, and the mixture is fed into a melt kneader and kneaded. (2) A method in which the above-mentioned components (A) and (B), and, if necessary, components (C), (E), and (F), are mixed in advance using a Henschel mixer or the like to prepare a mixture containing these components, and the mixture is fed into a melt kneader and kneaded, and then, if necessary, component (D) is added from a side feeder and kneaded.

[0125] The components constituting the polyamide resin composition may be supplied to the melt kneader by supplying all of the components to the same supply port at once, or by supplying each of the components from a different supply port.

[0126] The melt-kneading temperature is preferably about 1° C. to 100° C. higher than the melting point of the polyamide resin (A), and more preferably about 10° C. to 60° C. higher than the melting point of the polyamide resin (A).

[0127] The shear rate in the mixer is 100 sec -1 The average residence time during kneading is preferably about 0.5 minutes or more and 5 minutes or less.

[0128] The melt kneader may be any known device, and for example, a single-screw or twin-screw extruder, a Banbury mixer, a mixing roll, or the like is preferably used.

[0129] The blending amount of each component when producing the polyamide resin composition of the present embodiment is the same as the content of each component in the polyamide resin composition described above.

[0130] <Characteristics of polyamide resin composition> [Dispersion of metal ions in fatty acid metal salts (B) (shape parameter k)] In the area distribution relating to the spatial area per metal ion of the fatty acid metal salt (B), which is calculated by subjecting the surface of the above-mentioned polyamide resin composition to the following measurement, the shape parameter k of the gamma distribution is 1.0 or more, preferably 1.3 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. When the dispersibility (shape parameter k) of the metal ions in the fatty acid metal salt (B) is equal to or higher than the above lower limit, a polyamide resin composition having excellent bleed-out resistance and suitable for high-cycle molding can be obtained. [measurement] In a distribution image obtained by mapping metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition or an intensity information image of the metal ion image, Voronoi division is performed with the center of the metal ion as a kernel point in order to calculate the spatial area per metal ion on the surface of the polyamide resin composition. The spatial area of ​​each region obtained by Voronoi division is calculated and classified by spatial area to create a histogram, and a shape parameter k of the gamma distribution represented by the following formula is calculated from the distribution state of the histogram. [ka] (wherein k is a shape parameter, θ is a scale parameter, and x is a spatial area)

[0131] Examples of the method for controlling the dispersibility of metal ions (shape parameter k) include a method for adjusting the outlet resin temperature of a melt kneader during the production of a polyamide resin composition, a method for adjusting the mass ratio Bw / Cw of the fatty acid metal salt (B) to the fatty acid amide compound (C) or the carbon number ratio Bn / Cn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the fatty acid amide compound (C) when the polyamide resin composition contains a fatty acid amide compound (C), and a method for adjusting the content of chloride ions in the polyamide resin composition when the polyamide resin composition contains chloride ions due to the inclusion of nigrosine (E). In order to obtain the dispersibility of metal ions (shape parameter k) within the above range, it is preferable to set the outlet resin temperature in the melt kneader to 290°C or higher during the production of the polyamide resin composition. It is also preferable that the mass ratio Bw / Cw of the fatty acid metal salt (B) to the fatty acid amide compound (C) and the carbon number ratio Bn / Cn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the fatty acid amide compound (C) satisfy the above range. In addition, it is preferable that the content of chloride ions in the polyamide resin composition satisfies the above-mentioned range.

[0132] The method for calculating the shape parameter k is not particularly limited, as long as it is a method in which the spatial area of ​​each metal ion is calculated by Voronoi division from a distribution image in which metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition are mapped, or from an intensity information image of the metal ion image, and the spatial area is calculated from the distribution state of a histogram created by classifying the spatial area, and the shape parameter k is obtained from a density function. The analysis method used to calculate the shape parameter k is not particularly limited as long as it can map the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition, and a known observation method can be used. The known observation method is not limited to the following, but examples include commonly known surface molecular and elemental analysis methods such as scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) and time-of-flight secondary ion mass spectrometry (TOF-SIMS). The measurement can also be performed on a molded product as necessary, and it is preferable to measure on the smooth surface of a molded product such as a plate-shaped product. The distribution image obtained by the above observation method tends to obtain an accurate ion distribution by binarizing the image using the Otsu method. Alternatively, when using an intensity information image of a metal ion image, analysis can be performed by depicting the data without binarization.

[0133] ≪Molded products≫ The molded article of the present embodiment contains the polyamide resin composition of the present embodiment described above, and is obtained by molding the polyamide resin composition of the present embodiment described above. The method for producing the molded product is not particularly limited, and any known molding method can be used. Known molding methods include, but are not limited to, commonly known plastic molding methods such as press molding, injection molding, gas-assisted injection molding, welding molding, extrusion molding, blow molding, film molding, blow molding, multi-layer molding, and melt spinning.

[0134] In addition, since the above-mentioned polyamide resin composition is suitable for high-cycle molding, the molded article of the present embodiment is suitably produced by high-cycle molding.

[0135] The molded article of the present embodiment has a high surface gloss value. The surface gloss value of the molded article of the present embodiment is preferably 50 or more, more preferably 70 or more, and even more preferably 80 or more. When the surface gloss value of the molded article is equal to or more than the above lower limit, the obtained molded article can be suitably used as various parts such as automobile parts, electric and electronic parts, industrial material parts, industrial material parts, and daily necessities and household goods.

[0136] The molded article of the present embodiment is obtained from the polyamide resin composition, and therefore has excellent mechanical properties, particularly water absorption rigidity, hot rigidity, fluidity, surface appearance, and corrosion resistance. Therefore, the molded article can be suitably used as various parts such as automobile parts, electric and electronic parts, home appliance parts, OA (Office Automation) equipment parts, mobile equipment parts, industrial equipment parts, daily necessities and household goods, and for extrusion applications. Among them, the molded article is suitably used as automobile parts, electric and electronic parts, home appliance parts, OA equipment parts, or mobile equipment parts.

[0137] Examples of automobile parts include, but are not limited to, intake system parts, cooling system parts, fuel system parts, interior parts, exterior parts, and electrical parts. EXAMPLES

[0138] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0139] Each of the components of the polyamide resin composition used in the examples and comparative examples will be described.

[0140] <Components> [Aliphatic polyamide (Aa)] Aa-1: Polyamide 6 (manufactured by Ube Industries, product name: "SF1013A", Mw (A-a) :31500, Mw (A-a) / Mn (A-a) :2.2) Aa-2: Polyamide 66 (synthesized by the method described below)

[0141] [Semi-aromatic polyamide (Ab)] Ab-1: Polyamide 6I (synthesized by the method described below) Ab-2: Polyamide 6I / 6T (manufactured by EMS Co., Ltd., product name: "G21", Mw (A-b) :27000, Mw (A-b) / Mn (A-b) :2.4) Ab-3: Polyamide MXD6 (Toyobo nylon manufactured by Toyobo Co., Ltd., product name "T-600", Mw (A-b) :45000, Mw (A-b) / Mw (A-b) :2.2)

[0142] [Fatty acid metal salts (B)] B-1: Sodium montanate (manufactured by Clariant, product name: "LICOMONT NAV101") B-2: Calcium montanate (manufactured by Clariant, product name: LICOMONT CAV102) B-3: Calcium stearate (manufactured by NOF Corporation, product name: "Calcium Stearate G")

[0143] [Fatty acid amide compounds (C)] C-1: N,N'-ethylenebisstearic acid amide (Kao Corporation, product name: "Kaowax EB-P") C-2: N-stearyl erucamide (manufactured by Nippon Fine Chemicals, trade name: "SNT-P")

[0144] [Inorganic filler (D)] D-1: Glass fiber (GF) (manufactured by Nippon Electric Glass, product name: "ECS03T275H", number average fiber diameter 10 μm, cut length (weight average fiber length) 3 mm)

[0145] [(E) Nigrosine] E-1: Nigrosine (manufactured by Orient Chemical Co., Ltd., TH807) (chloride ion concentration: 0.06% by mass) E-2: Nigrosine (manufactured by Orient Chemical Co., Ltd., TH870) (chloride ion concentration: 1.6% by mass)

[0146] [(F) Other ingredients] F-1: Carbon black (CB) (manufactured by Mitsubishi Chemical Corporation, product name: "#45")

[0147] <Production of polyamide> The production methods of the aliphatic polyamide (Aa-2) and the semi-aromatic polyamide (Ab-1) are described in detail below. The aliphatic polyamide (Aa-2) and the semi-aromatic polyamide (Ab-1) obtained by the production methods described below were dried in a nitrogen stream to adjust the moisture content to about 0.2 mass%, and then used as raw materials for the polyamide resin compositions in the examples and comparative examples described later.

[0148] [Synthesis of aliphatic polyamide (Aa-2) (polyamide 66)] The polymerization reaction of polyamide was carried out by the "thermal melt polymerization method" as follows. 1500g of an equimolar salt of adipic acid and hexamethylenediamine was dissolved in 1500g of distilled water to prepare a homogeneous aqueous solution of 50% by mass of the raw material monomer. This aqueous solution was charged into an autoclave with an internal volume of 5.4L and substituted with nitrogen. The solution was concentrated by gradually removing steam to a solution concentration of 70% by mass while stirring at a temperature of 110°C to 150°C. The internal temperature was then raised to 220°C. At this time, the autoclave was pressurized to 1.8MPa. The reaction was continued for 1 hour while gradually removing steam to maintain the pressure at 1.8MPa until the internal temperature reached 245°C. Next, the pressure was lowered over 1 hour. After that, the inside of the autoclave was maintained under a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265°C. The mixture was then pressurized with nitrogen and formed into strands from the lower spinneret (nozzle), water-cooled, cut, and discharged in pellet form. The pellets were then dried at 100°C in a nitrogen atmosphere for 12 hours to obtain a crystalline aliphatic polyamide (Aa-2) (polyamide 66). The resulting crystalline aliphatic polyamide (Aa-2) (polyamide 66) had a molecular weight of Mw (A-a) is 35,000, Mw (A-a) / Mn (A-a) was 2.0.

[0149] [Synthesis of semi-aromatic polyamide (Ab-1) (polyamide 6I)] The polymerization reaction of polyamide was carried out by the "thermal melt polymerization method" as follows. First, 1500 g of an equimolar salt of isophthalic acid and hexamethylenediamine, as well as 1.5 mol % excess adipic acid and 0.5 mol % acetic acid relative to the total equimolar salt components, were dissolved in 1500 g of distilled water to prepare a 50 mass % equimolar homogeneous aqueous solution of raw material monomers. Next, the solution was concentrated by gradually removing steam to a solution concentration of 70 mass % while stirring at a temperature of 110 ° C or higher and 150 ° C or lower. Next, the internal temperature was raised to 220 ° C. At this time, the autoclave was pressurized to 1.8 MPa. The reaction was continued for 1 hour while gradually removing steam and maintaining the pressure at 1.8 MPa until the internal temperature reached 245 ° C. Next, the pressure was reduced over 30 minutes. Next, the inside of the autoclave was maintained under a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265 ° C. The mixture was then pressurized with nitrogen to form a strand from the lower spinneret (nozzle), cooled with water, cut, and discharged in pellet form. The pellets were then dried at 100°C in a nitrogen atmosphere for 12 hours to obtain a semi-aromatic polyamide (Ab-1) (polyamide 6I). The resulting semi-aromatic polyamide (Ab-1) (polyamide 6I) had a content of isophthalic acid units in the dicarboxylic acid units of 100 mol %. (A-b) is 20,000, Mw (A-b) / Mn (A-b) was 2.0.

[0150] <Methods for measuring and evaluating physical properties> The polyamide resin composition pellets obtained in the Examples and Comparative Examples were dried in a nitrogen gas flow to adjust the moisture content in the polyamide resin composition to 500 mass ppm or less. Next, various physical properties and various evaluations were carried out by the following methods using the pellets of each polyamide resin composition with the adjusted moisture content.

[0151] [Molecular weight (Mw) and molecular weight distribution (Mw / Mn) of polyamide resin composition] The weight average molecular weight Mw and number average molecular weight Mn of each polyamide resin composition were measured by GPC (Tosoh Corporation, HLC-8020, hexafluoroisopropanol solvent, PMMA (polymethyl methacrylate) standard sample (Polymer Laboratory Co., Ltd.) conversion). Next, the molecular weight distribution (Mw / Mn) was calculated using the obtained Mw and Mn. The GPC columns used were TSK-GEL GMHHR-M and G1000HHR.

[0152] [Measurement of the dispersibility (shape parameter k) of metal ions in fatty acid metal salts (B)] For each polyamide resin composition, a flat plate molded piece (6 cm x 9 cm x 3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.) The cooling time was set to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90°C, and the cylinder temperature to 280°C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 1.6 ± 0.1 seconds. The surface of an arbitrary position of the molded piece was observed and measured using TOF-SIMS under the following observation conditions to obtain an intensity information image of the metal ion image. From the obtained intensity information image of the metal ion image, the spatial area per metal ion was calculated. For the calculation, metal ions with high intensity were selected so that the number of plots in the intensity information image was 200 to 2000, and Voronoi division was performed with the center of each metal ion as the generating point to obtain the spatial area of ​​each metal ion. Note that polygons protruding outside were deleted. After classifying the spatial area of ​​each region obtained by Voronoi division by area, a histogram was created, and the shape parameter k of the gamma distribution, expressed by the following formula, was calculated from the distribution state of the obtained histogram. [ka] (wherein k is a shape parameter, θ is a scale parameter, and x is a spatial area) (Observation conditions) Equipment used: nano TOF (ULVAC-PHI) Primary ion: Bi3++ Acceleration voltage: 30 kV Ion current: 0.1nA (as DC) Analysis area: 600μm x 600μm Analysis time: 15min Detected ions: Positive ions Neutralization: Electron gun Oxygen introduction: Yes 5.0 x 10 -5 Pa

[0153] [Chloride ion content] The chloride ions (Cl) contained in the pellets of the polyamide resin composition - The content of ) was quantified by combustion ion chromatography. Specifically, a Mitsubishi Chemical Analytech automatic sample combustion device AQF-2100H was used to prepare samples by the combustion tube combustion method using ultrapure water (containing hydrogen peroxide and hydrazine hydrate) as the absorption liquid. The ion chromatography (IC) device used was a Thermo Fisher Scientific Integrion RFIC, the column was a Thermo Fisher Scientific IonPac AS18-4μm (4mmφ×150mm), the eluent was a KOH aqueous solution, and the detector was a UV detector. From the measurement results, the chloride ion (Cl - ) content was calculated. "Cl - Content (ppm by mass) = [(IC measurement value (mg / L)) × (dilution rate) – (blank IC measurement value (mg / L))] × [(amount of absorption solution (mL)) / 1000] × [1000000 / (mass of sample (mg))]

[0154] [Flexural modulus retention after water absorption] For each polyamide resin composition, an ISO dumbbell with a thickness of 4 mm was prepared as a test specimen. The obtained test specimen was used to measure the flexural modulus before water absorption in accordance with ISO178. Next, the ISO dumbbell was left in a constant temperature and humidity atmosphere (temperature: 23°C, relative humidity: 50%), and after reaching water absorption equilibrium, the flexural modulus after water absorption was measured in accordance with ISO178. The flexural modulus retention rate (%) after water absorption was calculated using the following formula. "Flexural modulus retention rate after water absorption (%)" = (flexural modulus after water absorption) / (flexural modulus before water absorption) x 100 The rigidity upon water absorption was evaluated as follows: if the flexural modulus retention rate after water absorption was 90% or more, it was rated A (excellent); if it was 80% or more but less than 90%, it was rated B (good); if it was 70% or more but less than 80%, it was rated C (passable); and if it was less than 70%, it was rated D (poor).

[0155] [Low Speed ​​Appearance] For each polyamide resin composition, a flat plate molded piece (6 cm × 9 cm × 3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.) The cooling time was set to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90°C, and the cylinder temperature to 280°C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 4.5 ± 0.1 seconds. The surface appearance of the flat plate pieces thus produced was evaluated according to the following criteria. (Evaluation Criteria) A (Good): No glass fibers are found in the flat plate molding piece. B (Acceptable): Glass fibers are found in some parts of the flat plate molding piece. C (Poor): Glass fibers are found throughout the flat plate molding piece.

[0156] [Surface gloss] For each polyamide resin composition, a flat plate molded piece (6 cm x 9 cm x 3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.) The cooling time was set to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90°C, and the cylinder temperature to 280°C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 1.6 ± 0.1 seconds. The 60 degree gloss of the central portion of the main surface of the flat plate molded piece thus produced was measured using a glossmeter (HORIBA IG320) in accordance with JIS-K7150. It was determined that the larger the measured value, the better the surface appearance.

[0157] [Removal time] For each polyamide resin composition, a flat plate molded piece (6 cm x 9 cm x 3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.). The injection time was set to 15 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90 ° C, and the cylinder temperature to 280 ° C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 1.6 ± 0.1 seconds. At that time, the shortest cooling time at which the molded piece naturally fell (automatically fell) from the mold for 10 consecutive shots was defined as the demolding time (seconds). It was determined that the shorter the demolding time, the better the demolding property.

[0158] [Bleed-out test] For each polyamide resin composition, a flat plate molded piece (6 cm x 9 cm x 3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.) The cooling time was set to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90°C, and the cylinder temperature to 280°C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 1.6 ± 0.1 seconds. The flat plate molded piece thus produced was left to stand in a thermo-hygrostat (temperature: 80°C, relative humidity: 95%) for 500 hours. The flat plate molded piece was taken out, and the bleeding matter generated on the surface was observed, and the resistance to bleeding out (bleed-out resistance) was evaluated according to the following criteria. (Evaluation Criteria) A (good): No bleeding was observed on the flat plate molding piece. B (Acceptable): Bleeding is observed in some parts of the flat plate molding piece. C (Poor): Bleeding was observed over the entire flat plate molding piece.

[0159] [Laser printability] For each polyamide resin composition, a flat plate molded piece (6 cm x 9 cm x 3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.) The cooling time was set to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90°C, and the cylinder temperature to 280°C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 1.6 ± 0.1 seconds. Using a laser marker manufactured by Keyence Corporation, product name "MD-V9920," a 3 mm x 3 mm square marking was applied to the flat surface of the molded piece by laser marking to obtain a molded product. The laser marking conditions were wavelength 1064 nm, scanning speed 2000 mm / sec, output 5.2 W or 9.1 W, processing frequency 20 kHz, and processing pitch 50 μm. The laser marking property was visually evaluated according to the following criteria. (Evaluation Criteria) A (Good): The contrast between the laser marked and non-marked areas is very clear, and the characters are not blurred. B (Acceptable): The contrast between the laser marked and non-marked areas is clear, and some of the characters have been blurred. C (Poor): The contrast between the laser marked and non-marked areas is unclear, and the characters are blurred overall.

[0160] [Examples 1 to 12 and Comparative Examples 1 to 9] A TEM58SX twin-screw extruder (set temperature: 280°C, discharge rate: 400 kg / h, screw rotation speed: 300 rpm, resin temperature: 300-340°C), manufactured by Toshiba Machine Co., Ltd., was used. A pre-blended mixture of components (A) to (C) and component (F) was fed from a top feed port provided at the most upstream part of the extruder, and component (D) was fed from a side feed port on the downstream side of the extruder (in a state where the resin fed from the top feed port was fully melted). The molten mixture extruded from the die head was cooled in a strand shape and pelletized to obtain polyamide resin composition pellets. The blending amounts of each polyamide resin composition were as shown in Tables 1 and 2. The measurement and evaluation results of various physical properties are shown in Tables 1 to 3.

[0161] [Comparative Example 10] Using a ZSK-26Mc twin-screw extruder (set temperature: 280°C, discharge rate: 25 kg / h, screw rotation speed: 300 rpm, outlet resin temperature: 280°C) manufactured by Coperion, a pre-blended mixture of components (A) to (C) and component (F) was fed from a top feed port provided at the most upstream part of the extruder, and component (D) was fed from a side feed port on the downstream side of the extruder (in a state where the resin fed from the top feed port was fully melted). The molten mixture extruded from the die head was cooled in a strand shape and pelletized to obtain polyamide resin composition pellets. The blending amounts of the polyamide resin composition were as shown in Table 2. The measurement and evaluation results of various physical properties are shown in Table 2.

[0162] [Examples 13 and 14 and Comparative Examples 11 and 12] A TEM58SX twin-screw extruder (set temperature: 280°C, discharge rate: 400 kg / h, screw rotation speed: 300 rpm, resin temperature: 300-340°C), manufactured by Toshiba Machine Co., Ltd., was used. A pre-blended mixture of components (A) to (C), (E) and (F) was fed from a top feed port provided at the most upstream part of the extruder, and component (D) was fed from a side feed port on the downstream side of the extruder (in a state where the resin fed from the top feed port was fully melted). The molten mixture extruded from the die head was cooled in a strand shape and pelletized to obtain polyamide resin composition pellets. The blending amounts of each polyamide resin composition were as shown in Table 3. The measurement and evaluation results of various physical properties are shown in Table 3.

[0163] [Table 1]

[0164] [Table 2]

[0165] [Table 3]

[0166] As shown in Table 1, the molded articles obtained from the polyamide resin compositions of Examples 1 to 12, which contain the components (A) and (B) and have a shape parameter k of 1.0 or more, had releasability suitable for high-cycle molding, and were excellent in rigidity when absorbing water, surface appearance, and bleed-out resistance when molded into molded articles. They also had excellent laser printability. Furthermore, in a comparison between Example 1 and Example 2, which differ in the presence or absence of component (D), it was found that the inclusion of component (D) tended to result in better releasability and bleed-out resistance. Furthermore, in Examples 2, 6, and 7 in which the carbon number ratio Bn / Cn was the same but the mass ratio Bw / Cw was different, the greater the mass ratio Bw / Cw, the better the release properties tended to be, and the smaller the mass ratio Bw / Cw, the better the surface appearance tended to be. Furthermore, in Examples 2, 3, and 4, which have different ratios of the (Ab) component in the (A) component, the rigidity and surface appearance when absorbing water tended to be better as the ratio of the (Ab) component increased. On the other hand, the release properties tended to be better when the ratio of the (Ab) component in the (A) component was smaller. In addition, in a comparison between Examples 2 and 12, which differ in the type of component (C) and the carbon number ratio Bn / Cn, there was a tendency for the release properties and surface appearance to be more excellent as the fatty acid amide compound (C-1) was added and the carbon number ratio Bn / Cn increased. Furthermore, in a comparison between Examples 2 and 10, which have different types of component (Aa), it was found that the inclusion of the aliphatic polyamide (Aa-1) (PA6) tended to result in better surface appearance.

[0167] The molded article obtained from the polyamide resin composition of Comparative Example 4, which did not contain the component (B), had good rigidity and surface appearance when absorbing water, but had poor releasability. In addition, the molded article using the polyamide resin composition of Comparative Example 10, in which the extrusion conditions were changed, had a shape parameter k lower than those of the Examples, and had good rigidity and surface appearance when absorbing water, but had poor releasability.

[0168] As can be seen from Table 3, the polyamide resin compositions of Examples 13 and 14 containing the component (E) had a higher shape parameter k than Example 2 and tended to be more excellent in releasability and surface appearance. In addition, Comparative Examples 11 and 12, which contained component (E) but had a high chloride ion content, had a lower shape parameter k than the Examples and poor releasability. In addition, the laser marking properties were inferior to those of Examples 13 and 14. [Industrial Applicability]

[0169] The polyamide resin composition of the present invention, when molded into a molded article, is excellent in rigidity, surface appearance, and bleed-out resistance when absorbing water, and is suitable for high-cycle molding, and the molded article obtained by molding the polyamide resin composition of the present invention is excellent in rigidity, surface appearance, and bleed-out resistance when absorbing water. Therefore, the molded article of the present invention can be suitably used as various parts such as automobile parts, electric and electronic parts, industrial material parts, industrial material parts, daily necessities and household goods.

Claims

1. A polyamide resin composition comprising a polyamide resin (A) and a fatty acid metal salt (B) of a metal including an alkali metal and / or an alkaline earth metal, The fatty acid metal salt (B) is contained in an amount of 0.05 parts by mass or more and 5.00 parts by mass or less relative to 100 parts by mass of the polyamide resin (A), A polyamide resin composition, characterized in that in an area distribution relating to a spatial area per metal ion of the fatty acid metal salt (B), which is calculated by subjecting a surface of the polyamide resin composition to the following measurement, a shape parameter k of a gamma distribution is 1.0 or more. [measurement] In a distribution image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition or an intensity information image of the metal ion image, a Voronoi division is performed with the center of the metal ion as a generating point in order to calculate the spatial area per metal ion on the surface. The spatial area of ​​each region obtained by the Voronoi division is calculated and classified according to the spatial area, and a shape parameter k is calculated from a gamma distribution represented by the following formula: 【Chemistry 1】 (where k is a shape parameter, θ is a scale parameter, and x is a spatial area)

2. 2. The polyamide resin composition according to claim 1, wherein the fatty acid metal salt (B) is a fatty acid metal salt having a terminal hydrocarbon group having 19 or more carbon atoms.

3. The polyamide resin composition according to claim 1 or 2, wherein the polyamide resin (A) is an aliphatic polyamide (A-a), a semi-aromatic polyamide (A-b) containing a diamine unit and a dicarboxylic acid unit, or a mixture thereof.

4. The polyamide resin (A) is 100 parts by mass. 50 parts by mass or more and 99 parts by mass or less of the aliphatic polyamide (A-a); 1 part by mass or more and 50 parts by mass or less of the semi-aromatic polyamide (A-b); 0.05 parts by mass or more and 5.00 parts by mass or less of the fatty acid metal salt (B); Furthermore, 0.01 parts by mass or more and 3.00 parts by mass or less of a fatty acid amide compound (C); The polyamide resin composition according to claim 3, comprising:

5. 5. The polyamide resin composition according to claim 4, wherein the ratio Bw / Cw of the mass Bw of the fatty acid metal salt (B) to the mass Cw of the fatty acid amide compound (C) is 0.6 or more and 4.0 or less.

6. 5. The polyamide resin composition according to claim 4, wherein the ratio Bn / Cn of the number of carbon atoms Bn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the number of carbon atoms Cn of the terminal hydrocarbon group of the fatty acid amide compound (C) is more than 1.00 and not more than 2.

00.

7. The polyamide resin composition according to claim 3, wherein the aliphatic polyamide (Aa) is polyamide 6 or polyamide 66.

8. The polyamide resin composition according to claim 3, wherein the semi-aromatic polyamide (A-b) contains 50 mol % or more of isophthalic acid units relative to all dicarboxylic acid units constituting the semi-aromatic polyamide (A-b), and contains, as the diamine units, diamine units having 4 to 10 carbon atoms.

9. The polyamide resin composition according to claim 3, wherein the semi-aromatic polyamide (A-b) contains 75 mol % or more of isophthalic acid units relative to all dicarboxylic acid units constituting the semi-aromatic polyamide (A-b), and contains, as the diamine units, diamine units having 4 to 10 carbon atoms.

10. The polyamide resin composition according to claim 1 or 2, wherein the polyamide resin (A) has a weight average molecular weight Mw of 10,000 or more and 50,000 or less.

11. 3. The polyamide resin composition according to claim 1, wherein the polyamide resin (A) has a molecular weight distribution Mw / Mn of 2.4 or less.

12. 3. The polyamide resin composition according to claim 1, wherein the fatty acid metal salt (B) is at least one selected from the group consisting of sodium montanate and calcium montanate.

13. The polyamide resin composition according to claim 4, wherein the fatty acid amide compound (C) is at least one selected from the group consisting of fatty acid amide compounds and fatty acid bisamide compounds having a hydrocarbon group having 9 to 30 carbon atoms.

14. 5. The polyamide resin composition according to claim 4, wherein the fatty acid amide compound (C) is at least one member selected from the group consisting of N,N'-ethylenebisstearamide and N-stearylerucamide.

15. Further containing an inorganic filler (D), The polyamide resin composition according to claim 1 or 2, wherein the content of the inorganic filler (D) is 5 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the polyamide resin (A).

16. Further containing nigrosine (E), The polyamide resin composition according to claim 1 or 2, wherein the content of the nigrosine (E) is more than 0 part by mass and 0.5 parts by mass or less per 100 parts by mass of the polyamide resin (A).

17. 3. The polyamide resin composition according to claim 1 or 2, wherein the content of chloride ions is 5 ppm or less by mass.

18. A molded article comprising the polyamide resin composition according to claim 1 or 2.

19. A method for producing the polyamide resin composition according to claim 1 or 2, A production method comprising the step of melt-kneading the polyamide resin (A) and the fatty acid metal salt (B).

Citation Information

Patent Citations

  • Crystalline polyamide and composition containing the same

    JP1994032980A

  • Polyamide molded product

    JP1999042666A

  • Polyamide molding composition, preparation thereof and use thereof

    JP1999349806A

  • Polyamide resin composition

    JP2000154316A

  • Combination of mold release agent