Tube for covered electric wire
By using high molecular weight rubber with carbon and white carbon, the coated electric wire tubes achieve both high flame retardancy and flexibility, addressing the trade-off issue in existing technologies.
Patent Information
- Application Number
- JP2023083552
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-21
- Publication Date
- 2024-12-03
AI Technical Summary
Existing coated electric wire tubes face a trade-off between flame retardancy and flexibility, as adding large amounts of magnesium hydroxide for flame retardancy reduces flexibility.
Using high molecular weight rubber as a base resin, combined with carbon and white carbon as auxiliary agents and reinforcing materials, reduces the amount of magnesium hydroxide needed while maintaining or improving flame retardancy and flexibility.
The solution achieves an oxygen index of 32.0 or more and an elongation of 600% or more, meeting the requirements for high flame retardancy and flexibility, essential for applications like railway vehicles.
Smart Images

Figure 2024167154000002 
Figure 2024167154000003 
Figure 2024167154000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a tube for a covered electric wire, and more particularly to a tube for a covered electric wire having improved flame retardancy and flexibility. [Background technology]
[0002] A tube for coated electric wires (heat shrink tube) is a resin tube that shrinks in the radial direction when heated. When an object to be coated is coated with a tube for coated electric wires and heated, the tube shrinks to fit the shape of the part to be coated, forming a resin layer that adheres closely to the part. Thus, tubes for coated electric wires are used to form the coating layer (insulating layer) of coated electric wires, and to protect, insulate, and waterproof the bundling parts of electric wires and the terminals of wiring. In particular, insulated electric wire tubes for insulating and protecting insulated electric wires used in the internal wiring of railway cars, automobiles, etc., are required to be halogen-free, have high flame retardancy, and have excellent mechanical strength such as tensile strength and tensile elongation. For example, insulated electric wire tubes used in railway cars are required to have an oxygen index, which is an index of flame retardancy, of a predetermined value or more. In addition, from the viewpoint of ease of wiring work when using a tube for covered electric wires, a certain degree of flexibility is required.
[0003] Examples of halogen-free flame-retardant resin compositions having high flame retardancy include the techniques described in Patent Document 1 and Patent Document 2. Patent Document 1 discloses a tube for covered electric wires made of a halogen-free flame-retardant resin composition in which magnesium hydroxide is blended with a polyolefin resin. Patent Document 2 also discloses a tube for covered electric wires made of a polyolefin in which magnesium hydroxide is blended. Patent Document 2 also discloses a technique in which carbon black is used as a flame retardant. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 63-77958 [Patent Document 2] JP 2020-184469 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, both Patent Document 1 and Patent Document 2 are premised on the addition of a large amount of magnesium hydroxide. Therefore, there is a trade-off between flame retardancy and flexibility, and the problem is how to resolve the trade-off.
[0006] In order to solve this problem, the inventors focused on the type of base resin and the compounding ratio of the flame retardant and reinforcing agent, and discovered that the problem could be solved by using a high molecular weight rubber, reducing the amount of flame retardant, and adding carbon and white carbon together to function as a flame retardant assistant and reinforcing agent, thereby completing the present invention.
[0007] An object of the present invention is to provide a tube for a covered electric wire having flame retardancy, specifically an oxygen index, of a predetermined value or more, and improved flexibility. [Means for solving the problem]
[0008] The invention described in claim 1 is a tube for covered electric wires in which metal hydroxide, carbon, and white carbon are added to high molecular weight rubber, and the elongation in a test to evaluate the amount of plastic deformation is 600% or more, and the oxygen index measured based on JIS K 7201 is 32.0 or more, and the test to evaluate the amount of plastic deformation is performed by setting a test piece with a gauge length of 20 mm in an autograph, pulling the test piece at 100 mm / min, holding the test piece when the tensile length reaches 60 mm for 10 seconds, and then returning the test piece to the state at the start of the evaluation at 100 mm / min, and then removing the test piece from the autograph and measuring the length between the gauge lines to calculate the elongation.
[0009] According to the invention described in claim 1, a high molecular weight rubber is used as the base resin, without using low molecular weight rubber or low density resin. Generally, it is said that low molecular weight rubber and low density resin are easily combusted, and a large amount of metal hydroxide is required to obtain a certain level of flame retardancy with the metal hydroxide. If a high molecular weight rubber is used, the amount of metal hydroxide can be reduced.
[0010] In addition, in the invention described in claim 1, the combined use of carbon and white carbon not only serves as a flame retardant auxiliary that enhances the flame retardancy of the metal hydroxide, but also serves to enhance the rubber strength and elasticity of the polymer rubber. Therefore, in order to increase flexibility, the amount of metal hydroxide added can be reduced, and the amount of plastic deformation can be improved while maintaining the necessary flame retardancy.
[0011] The insulated electric wire tube of the present invention is required to have an elongation of 600% or more in a room temperature tensile test using a tensile tester, and an oxygen index of 32.0 or more measured according to JIS K 7201. These can be obtained by adding metal hydroxide, carbon, and white carbon to a high molecular weight rubber, and the high flame retardant performance and high elongation make it possible to achieve both a high oxygen index (high flame retardancy) and high flexibility. If the oxygen index is less than 32.0, it will not be possible to meet the hazard level 3 specified in EN45545-2, which is the regulation on fire safety requirements for European railway vehicles. Also, if the elongation rate is less than 600%, the coated wire tube will be too hard, which is not appropriate in terms of the efficiency of wiring work.
[0012] The invention described in claim 2 is the tube for covered electric wire according to claim 1, in which the metal hydroxide is magnesium hydroxide, and 80 PHR or more of the magnesium hydroxide is added.
[0013] According to the invention described in claim 2, magnesium hydroxide is used as the metal hydroxide. In this case, the magnesium hydroxide is added in an amount of 80 parts by weight (80 PHR) or more per 100 parts by weight of resin solids. If the magnesium hydroxide is less than 80 PHR, the oxygen index will not be 32.0 or more, and the required flame retardancy cannot be obtained. There is no particular upper limit on the amount of magnesium hydroxide added, but from the viewpoint of flexibility, the upper limit of the amount of magnesium hydroxide added is about 160 PHR.
[0014] The invention described in claim 3 is the tube for covered electric wire according to claim 1 or 2, in which the carbon is added in an amount of 5 PHR or more.
[0015] According to the invention described in claim 3, 5 PHR or more of carbon is added. This not only improves flame retardancy but also enhances rubber strength and elasticity, even if the amount of magnesium hydroxide added is reduced to increase flexibility.
[0016] The invention described in claim 4 is the tube for covered electric wire according to claim 1 or 2, to which 1 PHR or more of a glycerin fatty acid ester is added. The invention described in claim 5 is the tube for covered electric wire according to claim 3, in which 1 PHR or more of a glycerin fatty acid ester is added.
[0017] According to the inventions described in claims 4 and 5, 1 PHR or more of a glycerin fatty acid ester is added, which makes it possible to lower the viscosity of the master batch and to increase the dispersibility. Effect of the Invention
[0018] Generally, when a large amount of flame retardant is added, the flame retardancy improves, but the tensile deformation amount, which is a characteristic of rubber, decreases. On the other hand, it is known that low molecular weight rubber has a higher tensile deformation amount than high molecular weight rubber. According to the present invention, a high molecular weight rubber is used as a base resin without using a low molecular weight rubber or a low density resin, and carbon and white carbon are used in combination, which not only acts as a flame retardant auxiliary to enhance the flame retardancy of the metal hydroxide, but also enhances the rubber strength and elasticity of the polymer rubber. Therefore, by reducing the amount of metal hydroxide added, it is possible to increase flexibility and improve the amount of plastic deformation while maintaining the necessary flame retardancy. In the present invention, the advantages of the high molecular weight rubber cover the disadvantages of the flame retardant, so that even if the amount of metal hydroxide added is reduced to increase flexibility, the amount of plastic deformation can be improved while maintaining the necessary flame retardancy.
[0019] Furthermore, if the insulated electric wire tube of the present invention has an elongation of 600% or more in a room temperature tensile test using a tensile tester and an oxygen index of 32.0 or more measured in accordance with JIS K 7201, then it is possible to achieve both a high oxygen index (high flame retardancy) and high flexibility.
[0020] In particular, according to the invention described in claim 2, the oxygen index is 32.0 or more, the necessary flame retardant properties can be obtained, and the necessary amount of plastic deformation can be obtained.
[0021] Furthermore, according to the invention described in claim 3, even if the amount of magnesium hydroxide added is reduced in order to increase flexibility, the flame retardancy is not lowered more than necessary, and the rubber strength and elasticity can be enhanced.
[0022] Furthermore, according to the inventions described in claims 4 and 5, it is possible to reduce the viscosity of the masterbatch and to increase the dispersibility. [Brief description of the drawings]
[0023] [Figure 1] 1 is a graph showing the relationship between the amount of flame retardant added and the oxygen index when the basic resin composition is not changed and the amount of carbon black added is fixed at 25 parts by weight in an example according to the present invention. [Diagram 2]1 is a graph showing the relationship between the amount of carbon black added and the oxygen index when the basic resin composition is not changed and the amount of flame retardant (magnesium hydroxide) added is fixed at 120 parts by weight in an example according to the present invention. [Diagram 3] 1 is a graph showing the relationship between the amount of flame retardant added and the amount of plastic deformation in an example according to the present invention, where the basic resin composition is not changed and the amount of carbon black added is fixed at 25 parts by weight. [Figure 4] 1 is a graph showing the relationship between the amount of carbon black added and the amount of plastic deformation when the basic resin composition is not changed and the amount of flame retardant (magnesium hydroxide) added is fixed at 120 parts by weight in an example according to the present invention. [Diagram 5] 1 is a graph showing the relationship between the amount of white carbon added and the amount of plastic deformation when the basic resin composition is not changed and the amount of flame retardant (magnesium hydroxide) added is fixed at 120 parts by weight in an example according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments.
[0025] The tube for covered electric wire according to the present invention is produced by preparing a master batch and then molding the master batch into the tube for covered electric wire by extrusion molding. Master batches are made by adding magnesium hydroxide, which is a metal hydroxide, carbon, white carbon, and various additives to a base resin made of high molecular weight rubber, and kneading the resulting mixture in an air atmosphere.
[0026] As the high molecular weight rubber, any of various rubbers such as ethylene propylene rubber and ethylene acrylic rubber can be used.
[0027] Examples of metal hydroxides include magnesium hydroxide, aluminum hydroxide, calcium hydroxide, etc. Among them, magnesium hydroxide and aluminum hydroxide are preferred, and magnesium hydroxide is more preferred. As the metal hydroxide, those having a particle size in the range of 0.1 μm to 5.0 μm are preferred, and those having a particle size in the range of 0.5 μm to 2.0 μm are preferably used from the viewpoints of dispersibility in the resin, flame retardancy when dispersed, and mechanical strength. If the particle size is larger than the above range, the tensile elongation of the resin tends to decrease, and if it is smaller than the above range, the metal hydroxide is likely to aggregate. In addition, metal hydroxides surface-treated with a silane coupling agent or metal hydroxides surface-treated with an anionic surfactant can also be used.
[0028] The carbon is known as carbon black, and functions as a colorant and a flame retardant assistant. By adding carbon, it is possible to reduce the amount of metal hydroxide added.
[0029] White carbon is a white oxide of silicon, and is used as a rubber reinforcing agent and to improve adhesion, tear resistance, heat resistance, etc. Depending on the manufacturing method, white carbon is classified into wet silica (hydrated silicic acid) and dry silica (anhydrous silicic acid), and either can be used in the present invention.
[0030] As various additives, various additives such as antioxidants, lubricants, processing stabilizers, colorants (color pigments), foaming agents, reinforcing agents, fillers such as calcium carbonate, polyfunctional monomers (crosslinking assistants), etc. can be blended as long as they do not impair the spirit of the invention. Among the various additives, it is preferable to add glycerin fatty acid esters, because they lower the viscosity of the master batch during preparation and molding, making molding easier, and they improve the dispersibility of the base resin and various inorganic additives (fillers), making it possible to uniform the quality.
[0031] (Example) Examples of the present invention will now be described.
[0032] (Main material of master batch) The main materials used for the masterbatch were as follows: High molecular weight rubber: Ethylene propylene rubber (hereinafter referred to as "EPT") was used. Carbon: Made with SRF carbon. Magnesium hydroxide: Magnesium hydroxide with an average particle size of 0.83 μm was used. In addition, white carbon and glycerin fatty acid ester were used.
[0033] The main materials used above were mixed in the composition (mass ratio, PHR) shown in Table 1 in an internal mixer with a discharge temperature set to about 160°C, and then formed into a sheet using an open roll. When the crosslinking agent was added, the rubber temperature during mixing was lowered to 100°C or less. After that, the mixture was crosslinked using a press molding machine to obtain a sheet-like molded product of about A4 size and the thickness required for evaluating each property.
[0034] The following tests were carried out on the obtained molded body. The test results are shown in Table 1.
[0035] (Oxygen Index) The oxygen index indicates the minimum oxygen concentration (volume %, the minimum concentration of oxygen in a mixture of oxygen and nitrogen that can sustain the combustion of a material) required to sustain the combustion of a material, and is standardized in JIS K 7201:2007, and is an index of the flammability of a material. In the examples and comparative examples, the oxygen index was measured in accordance with JIS K 7201:2007 (a flammability test method for polymeric materials using the oxygen index method). Generally, a highly flame-retardant material is desired to have an oxygen index of 30 or more, and in particular, for fire requirements for European railway vehicles, the flammability behavior requirements for materials and components EN45545-2 require that hazard level 3 be satisfied, that is, that the oxygen index is 32 or more, so that materials with an oxygen index of 32 or more are judged to pass.
[0036] (Evaluation of the amount of plastic deformation) A test piece with a gauge length of 20 mm is placed on the autograph and pulled at 100 mm / min. When the tensile length reaches 60 mm, this state is held for 10 seconds, and then returned to the state at the start of the evaluation at 100 mm / min. The amount of elongation can be calculated by pulling the test piece on the autograph, removing the test piece from the autograph, measuring the length between the gauge lines, and then calculating the amount of elongation. The elongation in Table 1 was calculated using the above method.
[0037] [Table 1]
[0038] The evaluation results shown in Table 1 show that by using carbon and white carbon in combination, it is possible to obtain a tube for insulated electric wires with an elongation of 600% or more in the plastic deformation evaluation and an oxygen index of 32.0 or more as measured based on JIS K 7201, even when 80 PHR of magnesium hydroxide is added. Moreover, the mechanical strength has been shown to be excellent.
[0039] Based on the evaluation results shown in Table 1, the relationship between the amount of flame retardant added and the oxygen index was plotted in Figure 1, with the basic resin composition unchanged and the amount of carbon black added fixed at 25 parts by weight. The oxygen index was 32.0 when the amount of flame retardant (magnesium hydroxide) added was 80 parts by weight, and it was found that the oxygen index increased as the amount of flame retardant increased. Also, Figure 2 shows a graph of the relationship between the amount of carbon black added and the oxygen index when the basic resin composition was left unchanged and the amount of flame retardant (magnesium hydroxide) added was fixed at 120 parts by weight. The oxygen index was 34.2 when the amount of carbon black added was 5 parts by weight, and there was almost no change in the oxygen index even when the amount added was increased. This shows that there is no problem in terms of the oxygen index if the amount of carbon black added is 5 parts by weight or more.
[0040] Furthermore, without changing the basic resin composition, the amount of carbon black added was fixed at 25 parts by weight, and the relationship between the amount of flame retardant added and the amount of plastic deformation was investigated. The results are shown in a graph in Figure 3. Note that 100%, 200%, and 300% are the percentages of the tensile length when pulled on an autograph and held for 10 seconds in a room temperature tensile test. It can be seen that the relationship between the amount of flame retardant and the amount of plastic deformation is roughly proportional. In addition, the relationship between the amount of carbon black added and the amount of plastic deformation was plotted in a graph shown in Figure 4, where the basic resin composition was left unchanged and the amount of flame retardant (magnesium hydroxide) added was fixed at 120 parts by weight. It was found that the amount of plastic deformation did not change significantly even if the amount of carbon black added was increased.
[0041] Furthermore, without changing the basic resin composition, the amount of flame retardant added was fixed at 120 parts by weight, and the amount of carbon black added was fixed at 25 parts by weight, and the relationship between the amount of white carbon added and the amount of plastic deformation was investigated. The results are shown in a graph in Figure 5. It was found that the tensile strength did not change significantly even if the amount of white carbon added was increased.
[0042] From the above, when the amount of magnesium hydroxide added is 80 parts by weight or more and the amount of carbon black added is 5 parts by weight or more, the elongation in a room temperature tensile test using a tensile tester is 600% or more, the oxygen index measured in accordance with JIS K 7201 is 32.0 or more, and a highly flexible tube for coated electric wires can be produced.
Claims
1. A tube for coated electric wires in which metal hydroxide, carbon, and white carbon are added to a high molecular weight rubber, The elongation in the plastic deformation evaluation test is 600% or more, The oxygen index measured based on JIS K 7201 is 32.0 or more, In the evaluation test of the amount of plastic deformation, a test piece having a gauge length of 20 mm is set in an autograph, the test piece is pulled at 100 mm / min, and when the tensile length reaches 60 mm, the state is held for 10 seconds, and then the test piece is returned to the state at the start of the evaluation at 100 mm / min. Thereafter, the test piece is removed from the autograph, and the length between the gauge lines is measured to calculate the elongation of the insulated electric wire tube.
2. The metal hydroxide is magnesium hydroxide, 2. The tube for coated electric wires according to claim 1, wherein said magnesium hydroxide is added in an amount of 80 PHR or more.
3. 3. The tube for coated electric wires according to claim 1, wherein the carbon is added in an amount of 5 PHR or more.
4. 3. The tube for coated electric wires according to claim 1, further comprising 1 PHR or more of a glycerin fatty acid ester.
5. 4. The tube for coated electric wires according to claim 3, further comprising 1 PHR or more of a glycerin fatty acid ester.
Citation Information
Patent Citations
Method for producing resin composition and resin product using resin composition produced by the production method
JP2006111703A
Flame-retardant resin composition, electric wire-coating material containing the same, and electric wire coated with it
JP2008063562A
Radiation-resistant electric wire / cable
JP2013012326A
Halogen-free fire-resistant rubber composition and hose
JP2019500460A
Flame-retardant and heat-shrinkable tube
JP1988077958A