Physical quantity evaluation device, physical quantity evaluation method

The physical quantity evaluation device addresses the limitations of conventional stress measurement in glass by using a confocal Raman spectroscopic microscope to simultaneously measure surface reflection and Raman spectra, achieving high spatial resolution and precise surface detection for accurate stress and crystallinity assessment.

JP2024167587APending Publication Date: 2024-12-04AGC INC +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023083766
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

Smart Images

  • Figure 2024167587000001_ABST
    Figure 2024167587000001_ABST
Patent Text Reader

Abstract

To provide a physical quantity evaluation device capable of accurately measuring a physical quantity of a transparent measuring medium in a short time.SOLUTION: A physical quantity evaluation device evaluating a physical quantity of a transparent measuring medium includes: a laser beam source; a semitransparent mirror which converts an optical path of light from the laser beam source to a direction of the measuring medium; an objective lens condensing light from the semitransparent mirror to a surface or to an interior of the measuring medium; an imaging lens forming an image of an objective lens focus; a pinhole allowing passage of light of at least a part of the image of the objective lens; a spectroscope which spectrally diffracting light having passed through the pinhole; an imaging device which detects an intensity of a spectrum spectrally diffracted by the spectroscope, and converts the detected intensity to an electric signal; and a calculation unit processing the electric signal. The objective lens, the imaging lens, and the pinhole constitute a confocal Raman spectroscopic microscope measuring a Raman spectrum which is a spectrum of Raman scattered light from a part of the measuring medium. The imaging device simultaneously measures an intensity of a surface reflection spectrum of the light, and an intensity of the Raman spectrum.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a physical quantity evaluation device and a physical quantity evaluation method. [Background technology]

[0002] In electronic devices such as mobile phones and smartphones, glass is often used for the display unit and the housing body. For such glass, so-called chemically strengthened glass is used, which is strengthened by forming a surface layer (ion exchange layer) on the glass surface by ion exchange in order to increase the strength of the glass.

[0003] The surface layer of chemically strengthened glass includes at least a compressive stress layer present on the glass surface side in which compressive stress due to ion exchange occurs, and may include a tensile stress layer present on the glass inner side adjacent to the compressive stress layer in which tensile stress occurs. Sodium-containing aluminosilicate glass is often used for chemically strengthened glass, as it is easy to carry out ion exchange, has a high surface stress value, and can form a deep stress layer in a short time in the chemical strengthening process.

[0004] This aluminosilicate glass is immersed in high-temperature potassium nitrate molten salt to perform chemical strengthening. Because the concentration of potassium ions in the molten salt is high, sodium ions in the glass are exchanged with potassium ions in the molten salt. Because potassium ions are larger than sodium ions, large compressive stress is generated on the glass surface, increasing the strength of the glass. The glass that has been chemically strengthened has the highest potassium ion concentration at the glass surface in contact with the potassium nitrate solution, and the concentration decreases from the glass surface toward the depth direction.

[0005] Here, the refractive index of glass becomes higher when sodium ions are exchanged for potassium ions. In other words, the refractive index is highest at the glass surface, and decreases with depth from the glass surface.

[0006] As a technique for measuring the stress of the surface layer of such chemically strengthened glass, for example, when the refractive index of the surface layer of the chemically strengthened glass is higher than the refractive index inside, a technique for non-destructively measuring the compressive stress of the surface layer by utilizing the optical waveguiding effect and the photoelastic effect (hereinafter referred to as non-destructive measurement technique) can be mentioned. In this non-destructive measurement technique, monochromatic light is incident on the surface layer of the chemically strengthened glass to generate multiple modes by the optical waveguiding effect, and light with a fixed ray trajectory is extracted in each mode and imaged into a bright line corresponding to each mode by a convex lens. Note that there are as many imaged bright lines as there are modes.

[0007] Furthermore, in this nondestructive measurement technique, the light extracted from the surface layer is configured so that bright lines of two types of light components, the vibration directions of which are horizontal and vertical to the exit surface, can be observed. Utilizing the property that the light of the lowest order, mode 1, passes through the side of the surface layer closest to the surface, the refractive index of each of the two types of light components is calculated from the position of the bright line corresponding to mode 1 of the two types of light components, and the stress near the surface of the chemically strengthened glass is found from the difference between the two types of refractive index and the photoelastic constant of the glass (see, for example, Patent Document 1).

[0008] Furthermore, with regard to measuring the stress distribution in the surface layer of chemically strengthened glass, a method has been proposed that, based on the principles of the above-mentioned nondestructive measurement technology, determines the refractive index distribution from the surface of the glass based on the positions of emission lines corresponding to all modes, and further determines the stress distribution based on the photoelastic effect (see, for example, Patent Document 2 and Non-Patent Document 1).

[0009] However, chemically strengthened glass has become more diverse in order to improve its strength and performance, and conventional stress measurement methods are no longer sufficient for its evaluation.

[0010] For example, there is tempered glass in which lithium-containing glass is exchanged for two types of ions: potassium in the region near the surface and sodium in the region deeper than the surface, thereby controlling the stress distribution.

[0011] In this lithium-containing chemically strengthened glass, a conventional stress measurement device using optical waveguide light can evaluate the stress layer near the surface where lithium is exchanged with potassium because the refractive index increases when lithium is exchanged with potassium, but cannot evaluate the stress layer inside the glass where lithium is exchanged with sodium because the refractive index decreases when lithium is exchanged with sodium. Therefore, the stress distribution of the entire chemically strengthened layer cannot be measured.

[0012] In order to measure the stress distribution in such chemically strengthened glass, a stress measuring device has been proposed that utilizes the change in intensity of scattered laser light due to the photoelastic effect (see, for example, Patent Document 3). This stress measuring device can measure the stress inside the chemically strengthened glass regardless of the refractive index distribution.

[0013] However, the spatial resolution of this stress measurement device is determined by the laser spot diameter, which is about 10 μm. Therefore, the accuracy of the stress value is low in the region from the outermost surface of the glass to a depth of about 10 μm, and in particular, in chemically strengthened glass in which lithium ions are replaced with potassium ions near the surface, the stress value changes significantly in the region about 10 μm deep near the surface. This results in a large error in the outermost surface stress value CS, which is an important value for predicting the strength of glass.

[0014] In order to compensate for this drawback, it has been proposed to measure the area near the surface with a stress measurement device that uses guided light, and to measure deeper areas with a stress measurement device that uses scattered laser light, and to combine the two stress distribution data to obtain the overall stress distribution.

[0015] In recent years, a new method for measuring stress in glass has been developed that uses Raman spectroscopy (see, for example, Patent Document 4 and Non-Patent Document 2). This stress measurement method is said to be able to calculate stress from the D1, D2, and A1 peaks of the Raman spectrum at a certain depth in the glass. The generation of compressive stress due to chemical strengthening is determined by the ion exchange rate (positive effect) and structural relaxation (negative effect). Conventional methods that use the photoelastic effect could not separate and evaluate them. For example, even if the stress values ​​at two points are equal, it is not possible to determine whether this is due to a high ion exchange rate or the result of effectively suppressing structural relaxation. The Raman evaluation method is said to be able to distinguish between their contributions by focusing on D1, D2 (structural relaxation), and A1 (structural relaxation + ion exchange).

[0016] Furthermore, in the method using Raman spectrum described in Patent Document 4 and Non-Patent Document 2, the use of a confocal microscope is proposed as a method for measuring the distribution of stress in the depth direction. Patent Document 5 is an example of a confocal Raman microscope. Since a confocal Raman microscope can measure a Raman spectrum at a specific depth, the spectral data of this confocal Raman microscope can be analyzed by the method described in Patent Document 4 to measure the stress distribution in the depth direction of the strengthened glass.

[0017] In addition, confocal Raman microscopes can increase the resolution in the depth direction to about 1 μm, enabling them to accurately measure rapidly changing stress near the surface while also enabling simultaneous measurements in deep areas.

[0018] Meanwhile, stronger crystallized glass is beginning to be used instead of glass in the displays and housings of electronic devices such as mobile phones and smartphones.

[0019] Since crystallized glass must be transparent, particularly for use in displays, the crystallized glass used here is crystallized glass whose crystal grains are sufficiently smaller than the wavelength of visible light and is transparent in the visible range. Therefore, the surface stress formed in the chemical strengthening process can be measured with a conventional optical surface stress measuring device (see, for example, Patent Document 6). On the other hand, such crystallized glass is usually subjected to a crystallization process. The properties of the crystallized glass, such as transparency and strength, are greatly influenced by the degree of crystallization in this crystallization process. Therefore, it is necessary to measure the degree of crystallization after the crystallization process.

[0020] In the above-mentioned stress measurement by Raman spectroscopy, it is also possible to measure the crystallinity of this glass-ceramic at the same time. [Prior art documents] [Patent documents]

[0021] [Patent Document 1] Japanese Patent Application Publication No. 53-136886 [Patent Document 2] JP 2016-142600 A [Patent Document 3] WO2018 / 056121 [Patent Document 4] JP 2020-139940 A [Patent Document 5] Patent No. 6203355 [Patent Document 6] JP 2022-103233 A [Patent Document 7] Japanese Patent Application Publication No. 6-347343 [Non-patent literature]

[0022] [Non-Patent Document 1] Yogyo-Kyokai-Shi (Ceramics Association Journal) 87{3}1979 [Non-Patent Document 2] "Development of an equation for evaluating local stress in chemically strengthened glass based on Raman spectroscopy" Nobuaki Terakado, Yoshihiro Takahashi, Takumi Fujiwara, Shuji Orihara, Yoshio Orihara, Monthly Functional Materials 4027-35 December 2020 Summary of the Invention [Problem to be solved by the invention]

[0023] The stress of chemically strengthened glass is distributed in a layer of several tens of micrometers on the surface. Therefore, to measure the stress distribution, high spatial resolution in the depth direction is required, and high accuracy is also required for detecting the position of the glass surface, and an accuracy of 1 μm or less is required. In stress measurement from Raman spectrum using a confocal Raman microscope, if a high-magnification objective lens is used, a spatial resolution in the depth direction of about 1 μm can be obtained. This advantage is highly anticipated, since conventional stress measurement devices using the photoelastic effect cannot accurately measure the stress distribution in the area near the surface. However, to ensure absolute accuracy of the depth from the surface, it is necessary to accurately detect the position of the surface of the measurement medium, but conventional confocal Raman microscopes cannot accurately detect the position of the surface of the measurement medium.

[0024] Conventionally, for example, a method of detecting the glass surface is used by taking an image of a laser spot reflected on the glass surface with a camera and finding the point where the laser spot image is smallest. However, although this method can detect the surface with an accuracy of 1 μm or less, the confocal pinhole and the camera are separate optical paths, and it is necessary to align the focal positions of the pinhole and the camera in advance. The deviation between the focal position of the camera and the position of the pinhole directly results in an error in the detection of the surface point. And, since this positional relationship is a mechanically set positional relationship, it is difficult to always align it with an accuracy of 1 μm or less. In other words, in the measurement of the stress distribution in the depth direction from the surface of chemically strengthened glass, the absolute positional accuracy in the depth direction cannot be obtained.

[0025] In addition, recent chemically strengthened glass can form a very strong compressive stress layer near a very shallow surface, for example, a compressive stress layer of 1000 MPa can form at a depth of about 5 μm. In such chemically strengthened glass, a deviation in the detection accuracy of the surface point by just 1 μm can cause a large error in the measured stress distribution.

[0026] On the other hand, in the case of crystallized glass, in addition to measuring the stress due to chemical strengthening, it is also necessary to measure the degree of crystallization at a certain depth from the surface in controlling the crystallization process.

[0027] The surface is polished and removed, and then a chemical strengthening process is carried out to give the final glass shape, but in the crystallization process, the temperature conditions near the surface are different and the glass does not reach the desired crystalline state. For this reason, the surface layer is polished and removed.

[0028] In order to measure the degree of crystallinity or the state of crystallinity by Raman spectroscopy immediately after this crystallization step, it is necessary to perform Raman spectroscopy measurement at a depth that will become the final thickness.

[0029] In addition, the thickness of such reinforced glass and crystallized glass is wide, ranging from several tens of μm to several tens of mm. Conventional Raman microscopes measure the upper surface of the reinforced glass by placing the reinforced glass with the surface to be measured facing up on a stage that can move up and down. However, if the thickness of the reinforced glass differs, the distance between the top surface of the glass to be measured and the objective lens changes, so the stage must be moved up and down to change the distance between the stage and the microscope part and focus the objective lens on the top surface of the glass. In addition, with high-magnification objective lenses, the WD (Working Distance: the distance from the tip of the objective lens to the focus) is several mm to less than 1 mm, so there is a risk of hitting the objective lens when adjusting the up and down position. Furthermore, the stage needs to be changed up and down with a positional accuracy of 1 μm or less and a range of movement of several tens of mm, so the up and down movement mechanism of the stage is large and not practical.

[0030] As described above, it has been difficult to measure a physical quantity such as stress accurately in a short time in a transparent measurement medium such as glass.

[0031] The present invention has been made in consideration of the above-mentioned points, and has an object to provide a physical quantity evaluation device capable of measuring the physical quantity of a transparent measurement medium with high accuracy in a short period of time. [Means for solving the problem]

[0032] This physical quantity evaluation device is a physical quantity evaluation device that evaluates the physical quantity of a transparent measurement medium, and includes a laser light source, a semi-transparent mirror that converts the optical path of light from the laser light source in the direction of the measurement medium, an objective lens that focuses the light from the semi-transparent mirror on the surface or inside of the measurement medium, an imaging lens that forms an image of the focal point of the objective lens, a pinhole that passes at least a part of the light of the focal point image of the objective lens, a spectroscope that disperses the light that has passed through the pinhole, an imaging element that detects the intensity of the spectrum dispersed by the spectroscope and converts it into an electrical signal, and a calculation unit that processes the electrical signal, wherein the objective lens, the imaging lens, and the pinhole constitute a confocal Raman spectroscopic microscope that measures a Raman spectrum, which is the spectrum of Raman scattered light from a portion of the measurement medium, and the imaging element simultaneously measures the intensity of the surface reflection spectrum of the light and the intensity of the Raman spectrum. Effect of the Invention

[0033] According to the disclosed technique, it is possible to provide a physical quantity evaluation device capable of measuring the physical quantity of a transparent measurement medium in a short period of time with high accuracy. [Brief description of the drawings]

[0034] [Figure 1] 1 is a diagram illustrating a physical quantity evaluation device according to a first embodiment. [Diagram 2] FIG. 1 is a diagram illustrating a spectrometer of a physical quantity evaluation device 1. [Diagram 3] 2 is a diagram illustrating a spectrum measured by the physical quantity evaluation device 1. FIG. [Figure 4]FIG. 13 is a diagram illustrating the relationship between the intensity of a surface reflectance spectrum and depth. [Diagram 5] FIG. 1 is a diagram illustrating an example of the intensity of a surface reflection spectrum and the intensity of a Raman spectrum. [Figure 6] FIG. 2 is a diagram illustrating a Raman spectrum of chemically strengthened glass. [Figure 7] FIG. 7 is a diagram showing the position of the C peak in the spectrum of FIG. 6 measured in the depth direction. [Figure 8] FIG. 2 is a diagram illustrating a stress distribution of chemically strengthened glass whose surface is saturated. [Figure 9] FIG. 2 is a diagram illustrating a Raman spectrum of crystallized glass. [Figure 10] FIG. 1 compares Raman spectra at different depths in unstrengthened glass. [Figure 11] FIG. 13 is a diagram illustrating correction of a spectral shape. [Figure 12] FIG. 1 is a diagram (part 1) illustrating a measurement flow in the physical quantity evaluation device 1. [Figure 13] 2 is a diagram illustrating an example of functional blocks of a calculation unit 110 of the physical quantity evaluation device 1. FIG. [Figure 14] 2 is a diagram (part 2) illustrating a measurement flow in the physical quantity evaluation device 1. FIG. [Figure 15] FIG. 3 is a diagram (part 3) illustrating a measurement flow in the physical quantity evaluation device 1. [Figure 16] FIG. 11 is a diagram illustrating a physical quantity evaluation device according to a second embodiment. [Figure 17] FIG. 13 is a diagram illustrating a physical quantity evaluation device according to a modified example of the second embodiment. [Figure 18] 11 is a diagram illustrating an example of the relationship between the voltage applied to a liquid crystal element and the polarization phase difference. [Figure 19] 1A to 1C are diagrams illustrating a method of driving a liquid crystal element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and duplicated explanations may be omitted.

[0036] First embodiment Fig. 1 is a diagram illustrating a physical quantity evaluation device according to a first embodiment. As shown in Fig. 1, the physical quantity evaluation device 1 includes a laser light source 10, an optical member 20, a semitransparent mirror 30, an objective lens 40, an imaging lens 50, a wavelength selection member 60, a pass region limiting member 70, a light conversion member 80, a spectroscope 90, an image sensor 100, a calculation unit 110, and a fixing member 180. The physical quantity evaluation device 1 does not need to include all of these components.

[0037] The physical quantity evaluation device 1 is capable of evaluating the physical quantity of a transparent measurement medium such as glass, resin, plastic, etc. Here, a transparent measurement medium refers to a measurement medium having a transmittance of 30% or more at the measurement depth for the wavelength of the laser light emitted by the laser light source 10.

[0038] Here, the following description will be given taking the case where the transparent measurement medium is tempered glass as an example. The tempered glass 200 shown in Fig. 1 is a transparent measurement medium. The tempered glass 200 is glass that has been subjected to a tempering process, for example, by a chemical tempering method or an air-cooling tempering method.

[0039] (Overall configuration of physical quantity evaluation device 1) Fixing member 180 is a portion that fixes the measurement medium. Fixing member 180 has a first surface 181 and a second surface 182 that faces first surface 181. First surface 181 and second surface 182 are, for example, parallel to each other. Fixing member 180 has an opening 183 that allows light to pass through.

[0040] The strengthened glass 200 is fixed to the fixing member 180 with the surface 201 to be measured pressed against the first surface 181 of the fixing member 180. The surface 201 of the strengthened glass 200 is in contact with the first surface 181 of the fixing member 180. Note that the strengthened glass 200 is not a component of the physical quantity evaluation device 1.

[0041] The laser light source 10, the optical member 20, the semi-transparent mirror 30, and the objective lens 40 are located on the second surface 182 side of the fixed member 180. The laser light emitted by the laser light source 10 passes through the optical member 20 and enters the semi-transparent mirror 30. The semi-transparent mirror 30 changes the optical path of the light from the laser light source 10 toward the measurement medium, and the light whose optical path has been changed enters the objective lens 40.

[0042] The objective lens 40 collects the light from the semi-transparent mirror 30 and forms a focal point on the first surface 181 side rather than the second surface 182. The focal point of the objective lens 40 is located on the surface 201 of the strengthened glass 200 or near the surface 201. In other words, the objective lens 40 collects the light from the semi-transparent mirror 30 on the surface or inside of the strengthened glass 200. The light collected by the objective lens 40 passes through the opening 183 and reaches the strengthened glass 200.

[0043] The fixed member 180 is configured to be able to change the distance from the objective lens 40. Specifically, the fixed member 180 is configured to be able to mechanically move the distance L between the objective lens 40 and a first surface 181 of the fixed member 180 in a direction perpendicular to the surface 201 with the surface 201 as the center, relative to the focal position of the objective lens 40. The fixed member 180 may be moved manually, but is desirably driven by a stepping motor or a piezoelectric motor controlled with an accuracy of several μm or 1 μm or less by a fixed member moving means 114 of the calculation unit 110 described later.

[0044] Reflected light and scattered light from the reinforced glass 200 pass through the opening 183, the objective lens 40, and the semi-transparent mirror 30 and enter the imaging lens 50. The imaging lens 50 is located on the opposite side of the objective lens 40 from the fixed member 180, and forms an image at the focal point of the objective lens 40. The objective lens 40 and the imaging lens 50 can form a magnifying microscope that magnifies and forms an image of a measurement medium, which is the subject of the focal point of the objective lens 40, at the focal point of the imaging lens 50. The light between the objective lens 40 and the imaging lens 50 is parallel. In other words, the magnifying microscope including the objective lens 40 and the imaging lens 50 is configured as a so-called infinity corrected optical system.

[0045] A passing area limiting member 70 is disposed at the position where the image is formed by the magnifying microscope. The passing area limiting member 70 is located on the opposite side of the fixed member 180 with respect to the imaging lens 50, and has a pinhole 70x that passes at least a part of the image of the focal point of the objective lens 40. The laser light, which is a parallel light having a predetermined beam diameter emitted from the laser light source 10, is incident on the optical axis of the objective lens 40 and the imaging lens 50 toward the objective lens 40 via the semi-transparent mirror 30, and is focused on the surface 201 or inside of the reinforced glass 200 by the objective lens 40. The focal point for forming an image on the pinhole 70x of the objective lens 40 and the focal point at which the laser light is most converged are the same.

[0046] The spectroscope 90 is located on the opposite side of the pinhole 70x from the fixed member 180, and separates the light that has passed through the pinhole 70x. That is, of the image formed on the pass-area limiting member 70, only the light from the pinhole 70x passes through and is guided to the spectroscope 90, and only the light that has passed through the pinhole 70x is separated.

[0047] Furthermore, in order to efficiently guide the light from the pinhole 70x to the spectroscope 90, a light conversion member 80 for converging the light may be inserted between the pinhole 70x and the spectroscope 90. As will be described later, since the entrance portion of the spectroscope 90 is slit-shaped, the light conversion member 80 can also have a function of converting the circular light that has passed through the pinhole 70x into a slit-shaped light. Specifically, a lens made of optical glass, a cylindrical lens, or the like can be used.

[0048] Furthermore, since the diameter of the pinhole 70x and the slit width of the spectroscope 90 are small, at several tens of μm, even a slight deviation in the optical axis prevents the light from the pinhole 70x from entering the spectroscope 90. For this reason, the optical axis may be adjusted by the light conversion member 80. Specifically, by making it possible to move a lens or cylindrical lens as the light conversion member 80 in the narrower direction of the slit of the spectroscope 90, slight deviations in the optical axis can be corrected.

[0049] The light dispersed by the spectroscope 90 enters the image sensor 100. The image sensor 100 detects the intensity of the spectrum dispersed by the spectroscope 90 and converts it into an electrical signal. The electrical signal converted by the image sensor 100 is sent to the calculation unit 110 as image data and processed by the calculation unit 110. The calculation unit 110 calculates spectral data from the image data obtained from the image sensor 100, for example.

[0050] A wavelength selection member 60 that selectively attenuates the intensity of the wavelength of the laser light incident on the image sensor 100 may be inserted between the semi-transparent mirror 30 and the image sensor 100. The wavelength selection member 60 selectively attenuates only the intensity of the wavelength of the laser light in the vicinity of the wavelength. The wavelength selection member 60 can be inserted at any position between the semi-transparent mirror 30 and the image sensor 100.

[0051] (laser light source) A DPSS laser with a wavelength of 405 nm, 532 nm, 785 nm, etc. can be used as the laser light source 10. Other lasers may also be used as the laser light source 10. Examples of other lasers include solid-state lasers, gas lasers, and semiconductor lasers.

[0052] (Configuration of confocal optical system) The laser light from the laser light source 10 passes through the semi-transparent mirror 30 and the objective lens 40, and is focused on the surface 201 of the tempered glass 200 or in the tempered glass 200 near the surface 201, forming an extremely small spot. The diameter of this spot is determined by the wavelength λ0 of the laser light, the focal length fob of the lens, and the beam diameter d0 of the laser light incident on the objective lens 40.

[0053] The optical member 20 is an optical member for laser beam processing, such as a beam expander, for adjusting the beam diameter and parallelism of the laser light, and is disposed between the laser light source 10 and the semitransparent mirror 30 as necessary.

[0054] Scattered light is generated from the trajectory of the laser light incident on the strengthened glass 200. This scattered light includes Rayleigh scattered light and Raman scattered light. The Rayleigh scattered light has the same wavelength as the wavelength λ0 of the laser light, and the Raman scattered light has a wavelength slightly shifted from the wavelength λ0 of the laser light. The physical quantity evaluation device 1 separates the Raman scattered light and evaluates the physical quantity of the strengthened glass 200, which is the measurement medium.

[0055] An image of light scattered in the strengthened glass 200 by the laser light is formed on a pinhole 70x by the objective lens 40 and the imaging lens 50. The diameter of the pinhole 70x is approximately the same as the diameter of an image obtained by enlarging the spot diameter of the laser light focused near the surface 201 of the strengthened glass 200 by the magnification of the microscope.

[0056] For example, when the wavelength λ0 of the laser light source 10 is 532 nm, the focal length fob of the objective lens 40 is 2 mm, NA=0.9, and the focal length fim of the imaging lens 50 is 200 mm, the magnification as a magnifying microscope is 100 times. In this case, the laser spot diameter at the focal position of the objective lens 40 is 0.9 μm, and the scattered light image on the pinhole 70x is 0.9 μm × 100 times = 90 μm. In such a case, the diameter of the pinhole 70x is preferably 60 μm or more and 120 μm or less. Such a microscope is usually called a confocal microscope.

[0057] In this manner, the objective lens 40, the imaging lens 50, and the pinhole 70x constitute a confocal Raman spectroscopic microscope that measures a Raman spectrum, which is the spectrum of Raman scattered light from a portion of the reinforced glass 200.

[0058] (Principle of confocal optical system) As described above, the physical quantity evaluation device 1 has a confocal microscope configuration and has resolution in the depth direction. In a confocal microscope, a scattered light image by the laser light at the focal position of the objective lens 40 becomes an image with a diameter substantially equal to the diameter of the pinhole 70x, and almost all of the light can pass through the pinhole 70x. However, a scattered light image at a position shifted from the focal position in the depth direction first has a wider laser spot diameter, and furthermore, the image at the position of the pinhole 70x becomes out of focus and becomes an image larger than the diameter of the pinhole 70x, and almost no light can pass through the pinhole 70x.

[0059] In this way, in the confocal microscope, only scattered light from the spot of the laser light at the focal position of the objective lens 40 can pass through the pinhole 70x, providing resolution in the depth direction. For example, in the previous example, when the wavelength λ0 of the laser light source 10 is 532 nm, the focal length fob of the objective lens 40 is 2 mm, NA=0.9, the focal length fim of the imaging lens 50 is 200 mm, and the diameter of the pinhole 70x is 90 μm, the resolution in the depth direction is about 1.5 μm, and the in-plane spatial resolution is φ0.9 μm, which is the diameter of the laser beam at the focal point.

[0060] Then, the scattered light in the strengthened glass 200 that has passed through the pinhole 70x is introduced into the spectroscope 90. This makes it possible to measure the spectrum of the scattered light only in the vicinity of the focal position of the objective lens 40, and therefore the Raman spectrum of an extremely small region in the strengthened glass 200 can be measured.

[0061] (spectroscope) 2 is a diagram for explaining the spectroscope of the physical quantity evaluation device 1. The spectroscope 90 can be composed of, for example, a pass-area limiting member 91 having a slit 91x, an optical member 92 for collimating the light from the slit 91x, a diffraction grating 93 for dispersing the collimated light, and an optical member 94 for forming an image of the light Ld dispersed by the diffraction grating 93 on the image sensor 100. The optical members 92 and 94 are, for example, lenses, concave mirrors, or parabolic mirrors made of optical glass. The diffraction grating 93 is, for example, a reflective or transmissive diffraction grating with 300 to 2000 lines / mm. The resolution can be set to, for example, 3 nm or less.

[0062] An image of the dispersed slit 91x is formed on the image sensor 100. The image sensor 100 has a function of converting the imaged light into an electric signal, and has pixels arranged one-dimensionally or two-dimensionally. In detail, the image sensor 100 can convert received light into an electric signal, and output the luminance value of each of a plurality of pixels constituting a one-dimensional or two-dimensional image as image data to the calculation unit 110. As the image sensor 100, it is preferable to use an element such as a CMOS (Complementary Metal Oxide Semiconductor) image sensor, which is free from smear caused by oversaturation of photodiodes and has very little blooming. Other elements having similar functions may also be used.

[0063] (calculation section) The calculation unit 110 has a function of taking in image data from the image sensor 100 and performing image processing and numerical calculations. The calculation unit 110 may have other functions. Examples of other functions include a function of controlling the distance L between the fixing member 180 and the objective lens 40.

[0064] The calculation unit 110 converts the electrical signal obtained from the imaging element 100 into spectrum data, and determines the physical quantity at a predetermined depth from the surface 201 of the strengthened glass 200 and the distribution of the physical quantity in the depth direction based on the converted spectrum data.

[0065] The calculation unit 110 can be configured to include, for example, a CPU (Central Processing Unit), a ROM (Read Only Memory), a RAM (Random Access Memory), a main memory, and the like. In this case, various functions of the calculation unit 110 can be realized by reading a program recorded in the ROM or the like into the main memory and executing it by the CPU. The CPU of the calculation unit 110 can read data from the RAM and store it as necessary. However, a part or the whole of the calculation unit 110 may be realized only by hardware. Furthermore, the calculation unit 110 may be physically configured by multiple devices, etc. A personal computer, for example, can be used as the calculation unit 110.

[0066] (Spectrum to be measured) The above-mentioned spectrometer 90, image sensor 100, and calculation unit 110 can measure the spectrum in the range of wavelengths about 100 nm longer than the wavelength λ0 of the laser light source 10, that is, λ0 to λ0+100 nm, with a resolution of 3 nm or less.

[0067] The wavelength range of λ0 to λ0+100 nm includes the spectrum of the laser light and the Raman scattered light (sometimes simply referred to as the Raman spectrum). By analyzing the spectrum data of the Raman scattered light by the calculation unit 110, it is possible to know the composition, molecular structure (glass structure), and / or stress of the strengthened glass 200 as physical quantities. Furthermore, in the physical quantity evaluation device 1, by changing the distance L between the objective lens 40 and the fixing member 180 and acquiring the spectrum data, it is possible to measure the difference in the Raman spectrum in the depth direction from the surface 201 of the strengthened glass 200, i.e., the distribution of the Raman spectrum.

[0068] Furthermore, the physical quantity evaluation device 1 can measure the intensity of the surface reflection spectrum of the laser light of the strengthened glass 200, which has the same wavelength λ0 as the laser light, simultaneously with the Raman spectrum. Here, the surface reflection spectrum includes the laser light reflected by the surface 201 of the strengthened glass 200 and the laser light reflected in the vicinity of the surface 201 in the strengthened glass 200. The intensity of the surface reflection spectrum of the laser light reflected by the surface 201 of the strengthened glass 200 is strongest. That is, when the focal point of the objective lens 40 is located on the surface 201 of the strengthened glass 200, the intensity of the surface reflection spectrum is strongest.

[0069] Therefore, by measuring the intensity of the surface reflection spectrum while changing the distance L between the objective lens 40 and the first surface 181 of the fixing member 180 and searching for the position where the intensity is strongest, it is possible to detect with great accuracy that the focal point of the objective lens 40 is located on the surface 201 of the strengthened glass 200. This makes it possible to know with high accuracy physical quantities such as the stress and molecular structure (glass structure) of the strengthened glass 200, and the distribution of the physical quantities in the depth direction of the strengthened glass 200.

[0070] (Surface point detection method) In a conventional confocal Raman microscope, only the Raman scattered light at the focal point of the laser light is measured. In contrast, in the physical quantity evaluation device 1, when the focal point of the objective lens 40 is located near the surface 201, the image sensor 100 can simultaneously measure the intensity of the surface reflection spectrum and the intensity of the Raman spectrum.

[0071] Usually, the reflected light of laser light from the glass surface has the same wavelength λ0 as the laser light, which is different from the wavelength of Raman scattered light. Furthermore, the intensity of the reflected light from the surface is much greater than that of the Raman scattered light, ranging from 10,000 times (10 to the power of 4) to 10,000,000 times (10 to the power of 7). Therefore, if the reflected light from the surface is measured with the sensitivity required to measure the Raman spectrum when the focal point of the objective lens is located near the glass surface, the image sensor becomes saturated and the intensity cannot be measured. Furthermore, the Raman spectrum is covered by the components of the surface reflection spectrum, making it impossible to measure the Raman spectrum.

[0072] Therefore, the physical quantity evaluation device 1 preferably has a wavelength selection member 60 between the semi-transparent mirror 30 and the image pickup element 100, which attenuates light of the wavelength of the laser light incident on the image pickup element 100 and transmits light of the wavelength of the Raman spectrum. In this case, the peak intensity of the Raman spectrum measured by the image pickup element 100 is preferably 1 / 10 to 10 times the peak intensity of the surface reflection spectrum measured by the image pickup element 100 when the focal point of the objective lens 40 is located on the surface 201 of the strengthened glass 200. That is, in the wavelength selection member 60, the attenuation rate at the wavelength λ0 of the laser light is preferably 1 / 1000 (1 / 10 to the power of 3) to 1 / 1000000 (1 / 10 to the power of 6).

[0073] On the other hand, the wavelength of the laser light can also be attenuated in the semi-transparent mirror 30 without providing the wavelength selection member 60 or together with the wavelength selection member 60. For example, by making the semi-transparent mirror 30 a dichroic mirror that transmits light in a specific wavelength range and reflects the remaining wavelength range, it is possible to attenuate the light of the wavelength of the laser light contained in the light from the strengthened glass 200. The dichroic mirror efficiently reflects the laser light when the laser light is incident on the strengthened glass 200, and also transmits the light scattered in the glass from the objective lens 40 without attenuation, thereby obtaining an optically efficient semi-transparent mirror 30.

[0074] When a dichroic mirror is used, the light having the wavelength of the laser light is attenuated by the dichroic mirror among the light traveling from the objective lens 40 to the imaging lens 50. When a dichroic mirror is used together with the wavelength selecting member 60, the attenuation rate combined with the wavelength selecting member 60 is preferably such that the intensity of the surface reflection spectrum when the focal point is located on the glass surface is 1 / 10 to 10 times the intensity of the Raman spectrum.

[0075] The wavelength selection member 60 may be, for example, a short-cut filter, a band-pass filter, or a notch filter made of a multi-layered dielectric film. A combination of these filters may also be used. In the case of a combination of multiple filters, the filters may be combined at different positions between the semitransparent mirror 30 and the image sensor 100.

[0076] Fig. 3 is a diagram illustrating a spectrum measured by the physical quantity evaluation device 1. Fig. 3(a) is a spectrum at a depth of 30 μm from the surface 201 of the strengthened glass 200, and part A is the Raman spectrum. Since the strengthened glass 200 is amorphous, the Raman spectrum is broad and weak in intensity, and contains information such as stress and crystallinity. The physical quantity evaluation device 1 can measure physical quantities such as stress and crystallinity.

[0077] On the other hand, Fig. 3(b) shows a spectrum when the focal point of the objective lens 40 is located on the surface 201 of the strengthened glass 200. In Fig. 3(b), part A is the Raman spectrum as in Fig. 3(a). Also, in Fig. 3(b), part B is the surface reflection spectrum of the laser light from the surface 201 of the strengthened glass 200.

[0078] When the focal point of the objective lens 40 is on the surface 201 of the strengthened glass 200, half of the resolution in the depth direction as a confocal microscope is inside the strengthened glass 200 and the other half is outside the strengthened glass 200. Therefore, the intensity of the Raman spectrum of part A on the surface 201 of the strengthened glass 200 in Fig. 3(b) is about 50% of the intensity of the Raman spectrum of part A at a deep point (depth 30 µm) in Fig. 3(a).

[0079] The surface reflection spectrum of part B in Fig. 3(b) is not observed in Fig. 3(a). This is because the focal point of the objective lens 40 deviates from the confocal point of the confocal microscope at a point sufficiently deep from the surface 201 of the strengthened glass 200. In other words, the components of the surface reflection spectrum are observed only when the focal point is located near the range of the resolution in the depth direction of the confocal microscope, and the intensity is strongest when the focal point is located on the surface 201 of the strengthened glass 200.

[0080] FIG. 4 is a diagram illustrating the relationship between the intensity and depth of the surface reflection spectrum. In FIG. 4, the point with the maximum intensity is the surface 201 of the reinforced glass 200. The width of the peak corresponds to the spatial resolution in the depth direction as a confocal microscope. The surface reflection spectrum in FIG. 4 was measured with a laser light wavelength of 532 nm, a focal length f0 of the objective lens 40 of 3.3 mm, NA=0.7, a focal length fim of the imaging lens 50 of 200 mm, and a diameter of the pinhole 70x of 60 μm. In this case, the resolution in the depth direction is calculated to be about 3 μm, and it can be seen from FIG. 4 that it is almost as calculated. In addition, since the peak is sharp, the position of the peak can be identified with an accuracy of 1 μm or less.

[0081] However, the surface reflection spectrum can only be measured within a range of the depth resolution of a confocal microscope, which is a depth range of about ± several μm in front of and behind the surface 201 of the strengthened glass 200. Therefore, unless a relatively wide depth range is checked in units of several μm, it is not possible to capture the surface reflection spectrum and to identify the surface 201 of the strengthened glass 200. On the other hand, the depth range in which the Raman spectrum can be measured is about 1 mm from the surface 201 of the strengthened glass 200, which is a relatively wide range.

[0082] Fig. 5 is a diagram illustrating the intensity of the surface reflection spectrum and the intensity of the Raman spectrum. That is, Fig. 5 shows an example of the intensity of the surface reflection spectrum and the intensity of the Raman spectrum with respect to the depth from the surface of the strengthened glass. As shown in Fig. 5, the intensity of the Raman spectrum decreases as it approaches the surface 201 of the strengthened glass 200, becomes about 1 / 2 at the surface 201 of the strengthened glass 200, and becomes 0 away from the surface 201 of the strengthened glass 200.

[0083] That is, the depth at which the Raman spectrum can be measured is easily found, and using that point as a reference, the depth is changed toward the surface 201 of the strengthened glass 200 to find the point at which the Raman spectrum cannot be measured. This point is located close to the surface 201 of the strengthened glass 200. By measuring the intensity of the surface reflection spectrum while successively shortening the distance L from that point and searching for the point at which the intensity of the surface reflection spectrum is maximum, it is possible to accurately identify the position of the surface 201 of the strengthened glass 200 in a short time.

[0084] In this way, the physical quantity evaluation device 1 simultaneously measures the surface reflection spectrum and the Raman spectrum, and thereby makes it possible to detect the position of a surface point of the tempered glass, i.e., the surface 201 of the tempered glass 200, with high accuracy in a short period of time based on the intensities of the surface reflection spectrum and the Raman spectrum.

[0085] (CMOS image sensor) The intensity of the Raman spectrum and the intensity of the surface reflection spectrum differ depending on the type of glass, and therefore the ratio of the intensity of the Raman spectrum to the intensity of the surface reflection spectrum also differs greatly depending on the type of glass. Even if the wavelength selection member 60 for attenuating the intensity of the surface reflection spectrum of a certain type of glass is set to an attenuation rate or sensitivity that does not saturate the surface reflection spectrum and allows the Raman spectrum to be measured sufficiently, it may saturate the surface reflection spectrum of another reinforced glass. As a result, the surface reflection spectrum may be covered by other spectral signals, making it impossible to measure the Raman spectrum.

[0086] A CCD (Charge Coupled Device) is sometimes used as a component to convert light dispersed by a conventional spectrometer into an electrical signal. A CCD image sensor accumulates electric charges generated by light received by a photodiode, and the CCD transfers the electric charges to convert the amount of electric charge into a voltage. Therefore, when the photodiode of a pixel becomes saturated, the electric charge immediately overflows into the surrounding CCD and other pixels, causing blooming (image bleeding) and smear (vertical lines), and as a result, the saturated spectral signal overlaps with the surrounding spectral signals.

[0087] Furthermore, because the spectral image split by the spectrometer is an image of a slit, it is long and narrow, measuring several tens of microns wide and several mm long. For this reason, the pixels of the image sensor are either long and narrow to match the shape of the slit, or multiple pixels are electrically added in the length direction to obtain the entire spectral signal. However, the brightness of the split spectral image is not necessarily uniform along the length of the slit, and the center is usually brighter. Even if the photodiode signal as the image of the entire slit does not appear to be saturated at first glance, the center of the photodiode may be saturated, causing charge to leak out to the surrounding pixels.

[0088] On the other hand, in a CMOS image sensor, the charge stored in the photodiode is transferred via metal wiring, or the charge amount is converted into a voltage within the pixel and then the signal is transferred. Therefore, in principle, there is no smear and blooming is very small. Furthermore, since there is no limit to the maximum charge transfer amount as in the case of a CCD, and the saturation charge amount of the photodiode can be made large, there is almost no risk of a pixel becoming saturated and leaking charge to the surrounding area, causing it to overlap with other spectral signals.

[0089] Furthermore, because CMOS image sensors are capable of high-speed transfer, the dynamic range can be expanded by adding up the data obtained by exposing the image sensor multiple times in a calculation unit.

[0090] Thus, a CMOS image sensor is preferably used as the imaging element 100. By using a CMOS image sensor as the imaging element 100, even a surface reflection spectrum that has an extremely higher intensity than the Raman spectrum can be measured without the signal being overlapped with the Raman spectrum.

[0091] (Surface reflectance spectrum intensity) In some cases, the attenuation of the intensity at the laser wavelength λ0 of the wavelength selection member 60 is insufficient, and the surface reflection spectrum is extremely stronger than the Raman spectrum, resulting in saturation of the surface reflection spectrum. In this case, the CMOS image sensor does not have the components of the surface reflection spectrum overlapping the Raman spectrum as in the case of a CCD, but the intensity peak of the surface reflection spectrum cannot be measured accurately, and the detection accuracy of the surface point decreases. In such a case, when acquiring the spectrum data, imaging with a short exposure after exposure in a normal measurement allows measurement of the data of the strong surface reflection spectrum without saturation. Since the short exposure requires less than 1 / 10 of the time required for normal exposure, the overall measurement time is almost the same.

[0092] (Glass thickness compatible) The thickness of the chemically strengthened glass, which is the measurement target of the physical quantity evaluation device 1, is very wide, ranging from several tens of μm to several tens of mm. In a normal confocal Raman microscope, the stage position needs to be located at a position that is farther away than the glass thickness in addition to the WD of the objective lens. In particular, when measuring thick glass, the stage position needs to be located much farther away from the objective lens. Therefore, the stage position needs to be adjusted for each glass thickness, and it is impossible to measure glass with a thickness outside the operating area of ​​the stage. In the physical quantity evaluation device 1, the position of the surface 201 of the strengthened glass 200 is always fixed near the first surface 181 by the fixing member 180. The accuracy is about ± several tens of μm to ± 100 μm, even when considering the undulations and bending of the surface 201 of the strengthened glass 200, and does not depend on the thickness of the strengthened glass 200.

[0093] (Real-time depth measurement) Usually, the spectral data in the depth direction is acquired by identifying the surface position of the tempered glass and moving from that position to deeper positions in the glass. However, with the physical quantity evaluation device 1, if the spectrum is measured sequentially from a position slightly outside the tempered glass from the surface, the spectral data at each depth includes the Raman spectrum and the surface reflection spectrum. Therefore, it is possible to know which depth data is the spectral data of the surface point from the spectral data of each depth, and the spectral data at the surface point can be determined simultaneously from the spectral data of each depth, and highly reliable spectral data in the depth direction from the surface point can be obtained.

[0094] (Stress calculation method 1) Generally, in crystalline materials, the peak of the Raman spectrum shifts slightly due to stress, and the stress can be measured from the amount of peak shift (see, for example, Patent Document 7). The Raman spectrum reflects the bond energy between atoms and molecules, and the bond energy changes due to stress, causing the wavelength of the spectrum to change slightly. Although the spectrum of reinforced glass is broader than that of crystals, it reflects the bonds between atoms and molecules, so the internal stress can be measured from the amount of shift in the spectrum peak.

[0095] FIG. 6 is a diagram illustrating the Raman spectrum of chemically strengthened glass, and shows the Raman spectrum of a sodium-containing aluminosilicate glass that has been chemically strengthened by replacing sodium ions with potassium ions. FIG. 7 is a diagram showing the position of the C peak in the spectrum of FIG. 6 measured in the depth direction from the glass surface. From FIG. 7, it can be seen that the C peak position shifts with depth and changes along with the stress due to chemical strengthening. If the shift amount of the peak position and the conversion coefficient of the stress value are obtained in advance using glass with a known stress value, the stress distribution in the depth direction of the chemically strengthened glass can be measured based on the shift amount of the peak position. The stress distribution can also be measured in crystallized glass using a similar method.

[0096] The tempered glass for which the conversion coefficient is calculated preferably has an absolute value of stress of 100 MPa or more. In addition, more accurate stress measurement is possible by using multiple tempered glasses with different tempering conditions for correction. For example, when using two or more pieces of glass for correction, one piece of glass is used with a small absolute value of stress value, and the other piece is used with a large absolute value of stress value, and the relationship between the difference in peak positions and the difference in stress values ​​and the difference in peak position ratios and the difference in stress values ​​for each depth is obtained. This allows the relationship between the peak positions and the peak position ratios at the depth to be obtained.

[0097] Furthermore, when two or more sheets of glass are used, the absolute value of the stress value of one of the sheets of tempered glass is preferably 100 MPa or more, while the absolute value of the stress value of the other sheet of tempered glass is preferably less than 100 MPa.

[0098] (Stress calculation method 2) In stress calculation method 1, the effect of stress relaxation inside the glass is not taken into account. However, in chemically strengthened glass, which undergoes a long tempering process to maximize the surface compressive stress, stress relaxation cannot be ignored, and the measurement accuracy of the stress value decreases in such chemically strengthened glass. In such cases, more accurate stress measurement is possible by calculating the amount of relaxation from the Raman spectrum of the strengthened glass.

[0099] A method for determining stress taking into account the amount of relaxation from Raman spectra will be described. For example, Figure 2 in Non-Patent Document 2 shows the Raman spectrum of a typical aluminosilicate-based chemically strengthened glass, and is a spectrum of a non-ion-exchanged region and a region where compressive stress occurs due to ion exchange.

[0100] According to Patent Document 4 and Non-Patent Document 2, in the Raman spectrum of the aluminosilicate-based chemically strengthened glass shown in FIG. 2 in Non-Patent Document 2, characteristic peaks are Boson, D1, D2, and A1 at 60, 480, 580, and 1100 cm, respectively. -1The Boson peak position, the peak intensity ratio of D1 and D2, and the A1 peak position affect the compressive stress due to chemical strengthening, and it is said that the stress can be calculated by measuring these peaks by spectroscopically analyzing Raman scattered light.

[0101] As a specific method, the Young's modulus and Poisson's ratio are measured in advance for the tempered glass to be measured. Then, Raman spectra are obtained for the ion-unexchanged portion in the deep portion and the ion-exchanged portion near the outermost surface, and the Boson peak position, the peak intensity ratio of D1 and D2, and the A1 peak position are determined. Next, the composition of the ion-exchanged portion near the outermost surface is determined using an electron beam probe microanalyzer or X-ray photoelectron spectroscopy. Then, a melt-quenched glass that matches the composition is prepared, a Raman spectrum is obtained, and the Boson peak position, the peak intensity ratio of D1 and D2, and the A1 peak position are determined. From these data, the constant term related to the right-hand side compressive stress in formula (8) of Non-Patent Document 2 can be determined. As a result, the stress at each depth can be calculated from the peak intensity ratio of D1 and D2 at each depth, the A1 peak position, and the stress balance condition of formula (3) of Non-Patent Document 2.

[0102] (Stress calculation method 3) In the above stress calculation method 2, more accurate stress can be calculated by the peak shift of A1 in the Raman spectrum and the peak intensity ratio of D2 and D1. However, to determine the coefficients determined by the glass in the calculation formula, it is necessary to measure the composition analysis, BOSON peak, Young's modulus, and Poisson's ratio.

[0103] On the other hand, industrially, it is more practical to measure a pre-prepared tempered glass by a conventional stress measurement method, and obtain a formula for calculating the stress value from the Raman spectrum based on the stress value. In the stress measurement device using scattered light photoelasticity described as a conventional stress measurement device, the laser beam diameter is finite, so the spatial resolution in the depth direction is usually about 10 μm of the laser beam diameter. Therefore, there is a possibility of many errors in the stress distribution between the surface and about 10 μm, but the stress distribution can be measured accurately in deeper regions.

[0104] Such measuring instruments that utilize the scattered light photoelastic effect have already been commercialized, for example, Orihara Manufacturing Co., Ltd. has commercialized the SLP-2000, which has a proven track record in the market. On the other hand, looking at equation (8) for calculating stress in Reference 2, there are as many as four coefficients to be determined for each glass type, and in order to accurately determine these four coefficients, multiple glasses with significantly different strengthening conditions are required.

[0105] So, ΔK A1 is related to the local stress, Δ(S D2 / S D1 ) is related to the relaxation in the medium range structure of glass, and the sum of these is the final stress, so we came up with the idea of ​​using the following general formula (1).

[0106]

number

[0107] For example, Pk,n other than n=10 is fixed to zero, Ps,m other than m=10 is fixed to zero, and Pk,10 and Ps,10 are used as fitting parameters to obtain the following formula (2). The calculation unit 110 can calculate the stress in the depth direction of the measurement medium based on, for example, formula (2).

[0108]

number

[0109] P in Equation (2) 3 can be calculated from the stress balance using formula (3). In formula (3), z is the depth from the glass surface, z0 is the surface, and zh is the point at a depth of 1 / 2 the glass thickness.

[0110]

number

[0111] On the other hand, in tempered glass samples where the ions exchanged during the tempering process are not saturated on the surface, the amount of ion exchange and the amount of relaxation are almost proportional. 1 and P 2 However, if strengthening treatment is performed for a long period of time, the amount of ion exchange near the surface becomes saturated, the compressive stress does not increase any more, and relaxation only proceeds, and conversely, the compressive stress decreases, and the stress on the surface becomes smaller than that inside.

[0112] FIG. 8 is a diagram illustrating the stress distribution of chemically strengthened glass with a saturated surface, which is a stress distribution measured by a stress measuring device using scattered light photoelasticity. The strengthened glass used in the measurement of FIG. 8 is one in which the ions exchanged during the strengthening process are not saturated on the surface. In this strengthened glass, the ion exchange is already saturated in a portion shallower than 50 μm, and the concentration of exchanged potassium ions is constant. However, further stress relaxation occurs near the surface, and as a result, the compressive stress on the surface becomes smaller, and the stress peaks at a depth of about 50 μm.

[0113] In such tempered glass, the amount of ion exchange and the amount of relaxation are almost proportional in the region deeper than the peak depth, but they differ in the region shallower than the peak depth. In other words, such a sample was prepared, and the stress values ​​at the point near the surface where relaxation is large and at the deep point where relaxation is small, and the ΔK at that depth were measured. A1 and Δ(S D2 / S D1 ) to measure P 1 and P 2 can be determined.

[0114] For example, in the case of the tempered glass shown in Figure 8, the stress values ​​at depths of 10 μm and 100 μm, which are highly accurate even with a conventional stress measurement device that uses the scattered light photoelastic effect, and the Raman spectrum show that P 1 and P 2 can be determined.

[0115] In this way, the parameters of formula (2) can be determined by measuring a measurement medium having a known stress in advance. The same applies to the parameters of formula (4) described later. The measurement medium having a known stress is, for example, tempered glass. There may be a plurality of measurement media having a known stress. The measurement medium having a known stress may also include untempered glass having an absolute value of the stress value of 10 MPa or less in the entire plate thickness. The plurality of measurement media having a known stress may further include tempered glass having an absolute value of the stress value of 100 MPa or more in the surface layer. The plurality of measurement media having a known stress may include a plurality of tempered glasses having an absolute value of the stress value of 100 MPa or more in the surface layer, and the difference between the maximum compressive stresses of each may be 100 MPa or more. The measurement medium having a known stress may include crystallized glass having a known degree of crystallization.

[0116] In addition, multiple pieces of tempered glass with different degrees of saturation can be used. For example, two pieces of tempered glass, one with a saturated surface and one without, are used, and the stress and Raman spectrum at the same point of 10 μm depth are used to determine P 1 and P 2 In this way, by preparing a sample of the same glass type with a saturated surface, the P 1 and P 2 can be determined, and P 3 Since can be calculated from the stress balance, it is possible to calculate the stress from D2 / D1 and the A1 shift amount. Furthermore, within the condition range where the surface is not saturated, it is possible to make the formula (2) into an even simpler formula such as the following formula (4).

[0117]

number

[0118] This is the same method as Stress Calculation Method 1, but within the range of strengthening conditions where the surface is not saturated, accurate stress can be calculated using formula (4). In industry, strengthening conditions are often set within a range where the surface is not saturated, so for production management, etc., measuring stress using this method is preferable. In this way, efficient stress measurement is possible by using different formulas depending on the strengthening conditions.

[0119] (Method of measuring peak intensity and peak position) In order to determine the intensities of the D1 and D2 peaks and the position of the A1 peak, it is preferable to perform least-squares fitting of the spectrum using at least three Gaussian waveforms centered on the D1, D2, and A1 peaks. Since the physical quantity evaluation device 1 can obtain a Raman spectrum at a certain depth of the tempered glass, the stress distribution in the depth direction can be measured from the D1, D2, and A1 peaks.

[0120] In this way, the stress at a certain depth can be calculated from the distribution of the Raman spectrum in the physical quantity evaluation device 1. Furthermore, the physical quantity evaluation device 1 can continuously measure the Raman spectrum of the strengthened glass for each depth at one time in a certain depth range without mechanical movement, and can measure the stress distribution in the depth direction.

[0121] (Measurement of crystallinity) FIG. 9 is a diagram illustrating the Raman spectrum of crystallized glass, where (a) is before the crystallization process, and (b) and (c) are after the crystallization process. FIG. 9(b) shows the target crystal state, where the peak E1 of the crystal phase is sharp, and it can be seen that crystals have been generated in some places. On the other hand, FIG. 9(c) shows the state after the crystallization process in which not enough crystals have been generated, and it can be seen that the peak E2 of the crystal phase is smaller than the peak E1 in FIG. 9(b). In this way, the crystallinity of the crystallized glass can be detected based on the Raman spectrum.

[0122] The degree of crystallinity (Rc) is calculated by the ratio of the area (Ap) forming the peak of the crystalline phase to the total area (Ao) and the correction coefficient C (Rc = C × Ap / Ao). The correction coefficient is obtained by using glass with a known degree of crystallinity in advance. In addition, more accurate stress can be obtained by correcting with multiple tempered glasses with different degrees of crystallinity.

[0123] For example, when using two or more pieces of tempered glass for correction, one piece of tempered glass with a low degree of crystallinity and the other piece of tempered glass with a high degree of crystallinity are used to obtain a correction coefficient C for each ratio (Ap / Ao). By approximating the relationship between this ratio (Ap / Ao) and the correction coefficient C with an approximation function, correction can be made even more accurately. Note that the approximation function is preferably an n-th order function (n is an integer less than the number of pieces of glass used for correction), but other approximation functions are also acceptable.

[0124] (High-precision wavelength measurement) In a Raman spectrum, the wavelength difference from the excitation wavelength is important, and while the wavelength span (the wavelength difference per unit distance of the dispersed light on the image sensor 100) hardly shifts due to the structure of the spectrometer, the absolute value of the wavelength is easily affected by slight shifts in the optical axis, etc. In the physical quantity evaluation device 1, the wave number of the measured Raman spectrum is calculated from the difference with the wavelength of the surface reflection spectrum measured at the same time. Here, the wavelength of the surface reflection spectrum is the wavelength of the excitation light, and since the Raman spectrum and the surface reflection spectrum can be measured at the same time, the Raman spectrum wavelength can always be measured stably by taking the difference from the wavelength of the surface reflection spectrum.

[0125] (Correction for non-tempered glass) In a confocal microscope, the optical conditions are different near the surface of the tempered glass and at a deep point. This is because the objective lens of the microscope is designed on the assumption that there is air from the lens to the focal point, or that there is glass of a fixed thickness. For example, in an objective lens designed on the assumption that there is air from the lens to the focal point, when the focal point is on the glass surface, the laser spot diameter will be as designed with the smallest aberration. However, when measuring the inside of tempered glass, the laser passes through a space with a different refractive index by the depth of the tempered glass between the lens and the focal point, and aberration occurs. Therefore, while the spot diameter is ideal as designed near the surface of the tempered glass, the aberration increases at deep points, causing the spot diameter to widen.

[0126] As a result, at deep points in the tempered glass, scattered light and fluorescent light from outside the minute area that should be measured are mixed in. In other words, the spectrum is measured from different areas near the surface and at deep points in the tempered glass. In this case, the spectral shape is exactly the same even if the depth changes in glass that is not chemically tempered, but the measured spectral shape also changes due to the difference in aberration caused by the objective lens's depth in the glass.

[0127] On the other hand, in order to measure stress from differences in Raman spectra in the depth direction, it is necessary to measure slight differences in the spectrum shape. Therefore, changes in the spectrum shape due to the aberration of the objective lens at deep points affect stress measurement, causing errors. Therefore, in the physical quantity evaluation device 1, it is preferable to measure the Raman spectrum in the depth direction in advance for unstrengthened glass and record the differences in the spectrum shape at each depth. Then, when measuring the Raman spectrum of strengthened glass, correction is made using the differences in the Raman spectrum shapes at depth for unstrengthened glass, making it possible to accurately measure even minute differences in the Raman spectrum shapes due to stress.

[0128] FIG. 10 is a diagram comparing Raman spectra at different depths in unstrengthened glass, comparing the Raman spectra at a depth of 10 μm and a depth of 100 μm in unstrengthened glass. In FIG. 10, the solid line is the spectrum at a depth of 10 μm, and the dotted line is the spectrum at a depth of 100 μm. In FIG. 10, the solid line and the dotted line are adjusted so that the level is the same at peak F, where the intensity of the Raman spectrum is the greatest. There is a slight difference between the two spectral shapes.

[0129] When measuring the Raman spectrum at each depth of the strengthened glass, the calculation unit 110 measures the Raman spectrum at each depth of the unstrengthened glass in advance, and corrects the spectrum shape at each depth measured on the strengthened glass from the difference in the spectrum shape at each depth. This makes it possible to correct the difference in spectrum shape that is not related to stress due to the difference in depth, and to measure the stress distribution with high accuracy. It is preferable that the calculation unit 110 corrects the Raman spectrum shape at each depth using the Raman spectrum of the unstrengthened glass with an absolute value of the stress value of 10 MPa or less.

[0130] FIG. 11 is a diagram for explaining the correction of the spectral shape. In FIG. 11, the A1 shift amount measured on tempered glass is compared with that without correction using the spectrum of untempered glass at each depth. In FIG. 11, the solid line indicates the case of correction, and the dotted line indicates the case of no correction. Normally, at deep points where tempering does not reach, the characteristics are constant, but when no correction is made, for example, at 50 μm or more, the deeper the point, the larger the characteristic becomes. On the other hand, when correction is made, it can be seen that the characteristics are constant.

[0131] (Measurement flow 1) Fig. 12 is a diagram (part 1) illustrating a measurement flow in the physical quantity evaluation device 1. Also, Fig. 13 is a diagram illustrating functional blocks of the calculation unit 110 of the physical quantity evaluation device 1. In measurement flow 1, a flow for measuring a surface reflection spectrum and a Raman spectrum at a certain depth will be described with reference to Figs. 12 and 13.

[0132] [Laser light irradiation process] In step S401, light from the laser light source 10 is focused via the semitransparent mirror 30 and the objective lens 40 onto the surface 201 or inside of the strengthened glass 200 into a small beam spot.

[0133] [Scattered light image formation process] In step S402, an image of the focal point of the objective lens 40 is formed by the imaging lens 50, and at least a part of the light of the image of the focal point of the objective lens 40 is passed through the pinhole 70x. That is, scattered light from a portion of the laser light irradiated in a spot shape in the strengthened glass 200 passes through the objective lens 40 again and is magnified on the pinhole 70x by the imaging lens 50, and is imaged as a scattered light image. At this time, it is preferable that the wavelength selection member 60 suppresses the intensity of only the same wavelength of the laser light.

[0134] [Spectroscopy process] In step S403, the light scattered in the strengthened glass that has passed through the pinhole 70x is split by the spectroscope 90, and a slit image of the split light by the spectroscope 90 is formed on the surface of the image sensor 100.

[0135] [Imaging process] In step S404, the image sensor 100 detects the intensity of the spectrum dispersed in the spectroscopic process, converts it into an electrical signal (digital data), and sends it to the calculation unit 110. In the imaging process, the intensity of the surface reflection spectrum and the intensity of the Raman spectrum can be measured simultaneously. The image sensor 100 may perform exposure multiple times. The image sensor 100 can capture an image when the focal point of the objective lens 40 is at any one depth of the measurement medium. The image sensor 100 may also capture an image multiple times when the focal point of the objective lens 40 is at different positions in the depth direction of the measurement medium. The focal position of the objective lens 40 in the depth direction of the measurement medium can be changed by moving the fixing member 180.

[0136] [Spectral data creation process] In step S405, the spectral data generating means 111 of the calculation unit 110 is used to generate spectral data from the image data from the image sensor 100. The spectral data includes surface reflection spectrum data and Raman spectrum data.

[0137] When the image sensor 100 is exposed multiple times, the spectral data creation means 111 of the calculation unit 110 may add up the data obtained from the multiple exposures. When the image sensor 100 is exposed multiple times with different exposure times, the spectral data creation means 111 of the calculation unit 110 may add up the data with different weights for creating the surface reflection spectrum and the Raman spectrum for each exposure.

[0138] [Spectral intensity measurement process] In step S406, the spectrum intensity measuring means 112 of the calculation unit 110 measures the intensity of the surface reflection spectrum, which is the wavelength of the laser light, and the intensities of D1 and D2 and the peak position of A1 of the Raman spectrum.

[0139] The spectral intensity measuring means 112 of the calculation unit 110 can measure the intensity of the surface reflection spectrum and / or the intensity of the Raman spectrum based on data captured by the imaging element 100 when the focus of the objective lens 40 is at any one depth of the measurement medium, or based on multiple data captured when the focus of the objective lens 40 is at different positions in the depth direction of the measurement medium.

[0140] (Measurement flow 2) FIG. 14 is a diagram (part 2) illustrating a measurement flow in the physical quantity evaluation device 1. FIG. 15 is a diagram (part 3) illustrating a measurement flow in the physical quantity evaluation device 1. In measurement flow 2, a flow for detecting a surface point of strengthened glass and measuring a spectrum up to a predetermined depth will be described with reference to FIGS. 13 to 15. Note that the flow in FIG. 12 is used for measuring the spectrum and the spectrum intensity. In this example, the prerequisites are that the accuracy in the depth direction is 1 μm and that the difference between the surface 201 of the strengthened glass 200 and the first surface 181 of the fixing member 180 is within ±100 μm.

[0141] In step S501, the fixed member moving means 114 moves the first surface 181 of the fixed member 180 to a position 130 μm away from the focal position of the objective lens 40. Note that 130 μm is just an example and is not limiting.

[0142] In step S502, the fixed member moving means 114 moves the first surface 181 of the fixed member 180 30 μm closer to the focal position of the objective lens 40. Note that 30 μm is an example and is not limiting. However, this is a smaller value than in step S501.

[0143] In step S503, the spectrum intensity measuring means 112 measures the intensity of the Raman spectrum and the intensity of the surface reflection spectrum according to the flow of Fig. 12. Note that the measurement target here is the Raman spectrum, but the measured spectrum data may also include the surface reflection spectrum.

[0144] In step S504, the spectrum intensity measuring means 112 checks whether the intensity of the Raman spectrum in the spectrum measured in step S503 is equal to or greater than a certain level.

[0145] If the intensity of the Raman spectrum is less than a certain level in step S504 (if NO), the process returns to step S502 and repeats the same processes as described above. If the intensity of the Raman spectrum is equal to or greater than a certain level in step S504 (if YES), the process proceeds to step S505.

[0146] In step S505, the fixed member moving means 114 moves the first surface 181 of the fixed member 180 5 μm away from the objective lens 40. Note that 5 μm is an example and is not limiting. However, this is a smaller value than in step S502.

[0147] In step S506, the spectrum intensity measuring means 112 measures the intensity of the Raman spectrum and the intensity of the surface reflection spectrum according to the flow of Fig. 12. Note that the measurement target here is the Raman spectrum, but the measured spectrum data may also include the surface reflection spectrum.

[0148] In step S507, the spectrum intensity measuring means 112 checks whether the intensity of the Raman spectrum in the spectrum measured in step S506 is equal to or lower than a certain level.

[0149] If the intensity of the Raman spectrum is greater than a certain level in step S507 (if NO), the process returns to step S505 and repeats the same process as above. If the intensity of the Raman spectrum is less than a certain level in step S507 (if YES), the process proceeds to step S508.

[0150] In step S508, the fixed member moving means 114 moves the first surface 181 of the fixed member 180 away from the objective lens 40 by 2 μm. Note that 2 μm is an example and is not limiting. However, this is a smaller value than in step S505.

[0151] In step S509, the spectrum intensity measuring means 112 measures the intensity of the Raman spectrum and the intensity of the surface reflection spectrum according to the flow of Fig. 12. Note that the measurement target here is the surface reflection spectrum, but the measured spectrum data may include the Raman spectrum.

[0152] In step S510, the fixed member moving means 114 moves the first surface 181 of the fixed member 180 1 μm closer to the objective lens 40. Note that 1 μm is an example and is not limiting. However, the value is smaller than that in step S508.

[0153] In step S511, the spectrum intensity measuring means 112 measures and records the intensity of the Raman spectrum and the intensity of the surface reflection spectrum according to the flow of Fig. 12. Note that the measurement target here is the surface reflection spectrum, but the measured spectrum data may include the Raman spectrum.

[0154] In step S512, the spectrum intensity measurement means 112 examines whether the intensity of the surface reflection spectrum is appropriate. Specifically, the spectrum intensity measurement means 112 examines whether the intensity of the surface reflection spectrum measured in step S509 is equal to or higher than a certain level, and whether the intensity of the surface reflection spectrum measured in step S511 is lower than that level. If it is lower, it is appropriate.

[0155] If the intensity of the surface reflection spectrum is not appropriate in step S512 (if NO), the process returns to step S510 and repeats the same process as above. If the intensity of the surface reflection spectrum is appropriate in step S512 (if YES), the process proceeds to step S513 in FIG. 15. If the result is YES, the surface reflection spectrum measured in step S509 is the desired surface reflection spectrum. The desired surface reflection spectrum is the surface reflection spectrum with the strongest intensity when the focal point of the objective lens 40 is located on the surface 201 of the strengthened glass 200.

[0156] In step S513, the fixed member moving means 114 moves the first surface 181 of the fixed member 180 a predetermined distance closer to the objective lens 40. Since the desired surface reflection spectrum has been found, that is, the position of the surface 201 of the strengthened glass 200 has been specified, the distance to be moved is then varied depending on the depth from the surface 201 of the strengthened glass 200. As an example, if the depth is 0 μm or more and less than 10 μm, the moving distance is 1 μm increments; if the depth is 10 μm or more and less than 20 μm, the moving distance is 5 μm increments; if the depth is 20 μm or more and less than 100 μm, the moving distance is 20 μm increments; and if the depth is 100 μm or more and less than 1000 μm, the moving distance is 50 μm increments.

[0157] In step S514, the spectrum intensity measuring means 112 measures and records the intensity of the Raman spectrum and the intensity of the surface reflection spectrum according to the flow of Fig. 12. Note that since the position of the surface 201 of the strengthened glass 200 has already been identified, the measurement target here is the Raman spectrum. However, since the recorded spectrum data also includes the surface reflection spectrum, it is also possible to use the data of the surface reflection spectrum as appropriate.

[0158] In step S515, the spectrum intensity measuring means 112 checks whether or not the measurement has been completed up to a predetermined depth.

[0159] If the measurement has not been completed to the predetermined depth in step S515 (if NO), the process returns to step S513 and repeats the same process as above. If the measurement has been completed to the predetermined depth in step S515 (if YES), the process proceeds to step S516.

[0160] In step S516, the spectrum intensity measuring means 112 calculates the level ratio of D2 to D1 of the Raman spectrum and the A1 peak position based on the recorded spectrum data at each depth. In addition, since the recorded spectrum data also includes the surface reflection spectrum, the position of the surface 201 of the strengthened glass 200 can be reconfirmed.

[0161] In step S517, the physical quantity calculation means 113 calculates stress at a certain depth of the strengthened glass 200 or in the depth direction, using the intensity of the Raman spectrum in the depth direction of the strengthened glass 200. Specifically, the physical quantity calculation means 113 calculates stress based on the level ratio between D2 and D1 of the Raman spectrum calculated in step S516 and the data of the A1 peak position. The physical quantity calculation means 113 may calculate the stress in the depth direction of the measurement medium based on the above-mentioned formula (2).

[0162] The physical quantity calculation means 113 may calculate a physical quantity other than the stress of the strengthened glass 200 based on each peak of the Raman spectrum at each depth in the strengthened glass 200. Of course, the physical quantity calculation means 113 may calculate both the stress and a physical quantity other than the stress. The calculated stress distribution and physical quantity may be displayed on a display device (such as a liquid crystal display).

[0163] For example, the physical quantity calculation means 113 may calculate the crystallinity at a certain depth of the strengthened glass or in the depth direction by using the intensity of the Raman spectrum in the depth direction of the strengthened glass 200. Alternatively, the physical quantity calculation means 113 may use a plurality of crystallized glasses having different crystallinity degrees and calculate the crystallinity degree by correlating the shape of the peak of the Raman spectrum with the crystallinity degree.

[0164] In this way, the physical quantity evaluation device 1 can measure the physical quantity of a transparent measurement medium in a short time with high accuracy. For example, the physical quantity evaluation device 1 can measure a physical quantity such as stress in a depth direction from an exact surface position of the transparent measurement medium in a short time with high accuracy.

[0165] Second Embodiment In the second embodiment, an example of a physical quantity evaluation device that can continuously change the polarization of laser light over time to obtain a Raman spectrum with a high S / N ratio will be described. Note that in the second embodiment, the description of the same components as those in the already described embodiments may be omitted.

[0166] Fig. 16 is a diagram illustrating a physical quantity evaluation device according to a second embodiment. As shown in Fig. 16, the physical quantity evaluation device 2 differs from the physical quantity evaluation device 1 (see Fig. 1) in that a polarization state varying member 120 is inserted on the optical axis between the laser light source 10 and the semi-transparent mirror 30, and that a polarizing member 130 is inserted between the semi-transparent mirror 30 and the spectrometer 90.

[0167] The polarization state varying member 120 is a member that varies the polarization state of the laser light over time. The polarization state varying member 120 is, for example, a rotating polarization element that varies the polarization state of the laser light over time. The rotating polarization element is a linear polarization element that can rotate the deflection angle at a constant speed over time, and rotates the polarization angle one or more revolutions within the measurement time of the Raman spectrum at a certain depth. The polarization member 130 is a linear polarization element and is fixed.

[0168] Furthermore, when the laser light from the laser light source 10 is linearly polarized like a semiconductor laser, the polarization state varying member 120 may be a rotating polarization phase difference element that rotates a polarization phase difference element (so-called ¼ wavelength plate) that shifts the polarization phase difference at the wavelength λ0 of the laser light. By inserting a fixed ¼ wavelength plate between the rotating polarization phase difference element and the laser light source 10 to convert the laser light into a circularly polarized light, the same effect as when the polarization state varying member 120 is a rotating polarization element can be obtained.

[0169] Raman scattered light has the property of maintaining the polarization of the incident light. Therefore, when the laser light incident on the reinforced glass is linearly polarized, the Raman scattered light also has linear polarization in the same polarization direction. When this linearly polarized scattered light passes through the polarizing member 130, the amount of light passing through changes depending on the difference in the polarization angle between the scattered light and the polarizing member 130, and the intensity of the Raman spectrum obtained by the spectroscope 90 also changes. Since the polarization direction of the laser light changes over time by the polarization state changing member 120, the Raman spectrum also changes in the same way, and the intensity changes with a period every time the polarization state changing member 120 rotates once, that is, every time the polarization direction rotates 360 degrees.

[0170] On the other hand, the fluorescence from the strengthened glass is not polarized regardless of the polarization of the incident laser light. That is, in the spectrum measured by the spectrometer 90, the intensity of the Raman spectrum changes periodically with the rotation of the polarization state varying member 120, but the fluorescence light does not change. In addition, external light and noise from the imaging element, amplifier circuit, etc. are not related to the polarization of the laser light.

[0171] The period and phase of the periodic change in the Raman spectrum are determined by the rotation period and phase of the polarization state varying member 120. Therefore, the polarization state varying member 120 is rotated at a constant speed, and the Raman spectrum is measured at the same depth at constant intervals multiple times for a period of one period or more. The number of times is one or more, and is preferably 2 to 10 times.

[0172] The intensity of the Raman spectrum changes periodically among the spectra acquired at fixed time intervals while the polarization state varying member 120 makes multiple rotations. Then, the amplitude value of the rotation periodic component of the polarization state varying member 120 is calculated by performing a Fourier transform, sine function fitting, or the like on the data of the spectral intensity for each time period of a certain wavelength, and the same processing is performed for all required wavelength bands to calculate the spectral data of the amplitude value of the rotation periodic component.

[0173] This spectrum contains only the Raman spectrum that changes with the rotation of the polarization state varying member 120 and does not contain noise from fluorescent light, external light, the imaging element, the amplifier circuit, etc., so a Raman spectrum with a high S / N ratio is obtained.

[0174] <Modification of the second embodiment> In the modified example of the second embodiment, an example is shown in which a polarization phase difference variable member is used as the polarization state varying member. The polarization phase difference variable member is an element that can electrically vary the polarization phase difference (retardation).

[0175] Fig. 17 is a diagram illustrating a physical quantity evaluation device according to a modified example of the second embodiment. As shown in Fig. 17, the physical quantity evaluation device 2A differs from the physical quantity evaluation device 2 (see Fig. 16) in that the polarization state varying member 120 is replaced with a polarization state varying member 150, and a polarizing member 140 is inserted between the laser light source 10 and the polarization state varying member 150.

[0176] The laser light from the laser light source 10 becomes linearly polarized light by the polarizing member 140. However, when the laser light source 10 emits linearly polarized laser light such as a semiconductor laser, the polarizing member 140 is not necessary.

[0177] Immediately after the polarizing member 140, a polarization phase difference variable member is provided as the polarization state varying member 150. The polarization phase difference variable member varies the polarization state of the laser light over time. More specifically, the polarization phase difference variable member is a variable retarder that varies the polarization phase difference of the laser light over time. The polarization phase difference that is varied is equal to or greater than the wavelength λ0 of the laser light, and is preferably 2 to 10 times the wavelength λ0 of the laser light.

[0178] An example of a variable retarder that can electrically vary the polarization phase difference by 1λ or more uniformly on the wavefront of the laser light is a liquid crystal retarder that uses a liquid crystal element. The liquid crystal element can vary the polarization phase difference by the voltage applied to the element, and for example, when the wavelength of the laser light is 532 nm, it can vary the wavelength by a maximum of 3 to 6. In the liquid crystal element, the maximum value of the polarization phase difference that can be varied by the applied voltage is determined by the size of the cell gap.

[0179] In a typical liquid crystal element, the cell gap is several μm, and therefore the maximum polarization phase difference is approximately 1 / 2λ (several hundreds of nm). Furthermore, in displays using liquid crystal, any change beyond this is not required. In contrast, in the liquid crystal element usable in this embodiment, when the wavelength of the laser light is, for example, 532 nm, it is necessary to vary the polarization phase difference of approximately 1600 nm, which is approximately three times 532 nm, and a cell gap of 20 to 50 μm is required.

[0180] The voltage applied to the liquid crystal element is not proportional to the polarization phase difference. As an example, the relationship between the applied voltage and the polarization phase difference for a liquid crystal element with a cell gap of 30 μm is shown in Figure 18. In Figure 18, the vertical axis is the polarization phase difference (the number of wavelengths relative to a wavelength of 630 nm), and the horizontal axis is the voltage applied to the liquid crystal element (plotted in logarithm).

[0181] When the voltage applied to the liquid crystal element is between 0V and 10V, the polarization phase difference can be varied by 8λ (5000nm) at 630nm. However, in liquid crystal elements, the alignment of the liquid crystal is generally not stable at low voltages between 0V and 1V, and the polarization phase difference varies with temperature changes, etc. Also, when the voltage applied to the liquid crystal element is 5V or more, there is little change in the polarization phase difference with respect to changes in voltage. In the case of this liquid crystal element, by using an applied voltage of 1.5V to 5V, the polarization phase difference can be stably varied from 4λ to 1λ, that is, about 3λ.

[0182] FIG. 19 is a diagram illustrating a method of driving a liquid crystal element, and illustrates a circuit that generates a drive voltage in the liquid crystal element such that the polarization phase difference changes linearly with time.

[0183] 19, in digital data storage circuit 301, voltage values ​​corresponding to the polarization phase difference for changing the polarization phase difference at regular intervals based on data obtained by measuring in advance the applied voltage and the polarization phase difference of the liquid crystal element to be used are recorded in address order as digital data within a required range of polarization phase difference change. Table 1 shows an example of some of the digital data recorded in digital data storage circuit 301. The voltage column in Table 1 is the digital data to be recorded, which is the voltage value for each 10 nm change in the polarization phase difference.

[0184] [Table 1] The clock signal generating circuit 302 generates a clock signal with a constant frequency using a quartz crystal oscillator, etc. The clock signal generated by the clock signal generating circuit 302 is input to the digital data storage circuit 301 and the DA converter 303.

[0185] The DA converter 303 is a circuit that converts the digital data from the digital data storage circuit 301 into an analog signal. Digital data of voltage values ​​stored in the digital data storage circuit 301 are read out in sequence in accordance with the clock signal generated by the clock signal generation circuit 302, and sent to the DA converter 303.

[0186] The DA converter 303 converts the digital data of the voltage value read out at regular time intervals into an analog voltage. The analog voltage output from the DA converter 303 is applied to a polarization phase difference variable member (liquid crystal element) used as the polarization state varying member 150 through a voltage amplifier circuit 304.

[0187] Although not shown in Figure 19, the drive circuit for this liquid crystal element is synchronized with the circuit that controls the image sensor 100, and when application of the drive voltage to the liquid crystal element begins, the image sensor 100 begins capturing images continuously over time.

[0188] The polarization axis of the polarization phase difference variable member used as the polarization state varying member 150 is installed at an angle of 45 degrees to the axis of the polarizing member 140. In this case, the linearly polarized laser light incident on the polarization phase difference variable member is emitted as is when the polarization phase difference of the polarization phase difference variable member is 0 degrees, is circularly polarized when it is 90 degrees, and is linearly polarized when it is 180 degrees, with the polarization direction shifted by 90 degrees from the incident direction. Furthermore, when it is 270 degrees, it becomes circularly polarized again, and when it is 360 degrees, it is emitted as is in the same manner as when it was 0 degrees. That is, it repeatedly changes from linear to circularly polarized to linear (perpendicular direction) to circularly polarized to linear.

[0189] On the other hand, the polarizing member 130 on the side for splitting the scattered light is installed in the same direction as or at right angles to the direction of polarization when the scattered light is linearly polarized. The Raman scattered light by the laser light undergoes a change in polarization similar to that of the laser light. Therefore, when the scattered light passes through the polarizing member 130, the intensity of the Raman scattered light repeats strong and weak in accordance with the period of the polarization phase, as the polarization phase difference of the polarization phase difference variable member changes from maximum to 1 / 2 to 0 to 1 / 2 to maximum, as the polarization phase difference of the polarization phase difference variable member changes. As with the physical quantity evaluation device 2, only the Raman scattered light that maintains its polarization changes in intensity, and this does not occur due to noise of the fluorescent light, external light, image sensor, amplifier circuit, etc. Therefore, by extracting the component that changes in the same period as the period of the polarization phase difference, a Raman spectrum with a high S / N ratio can be obtained without noise of the fluorescent light, external light, image sensor, amplifier circuit, etc.

[0190] In addition, the polarization direction of the laser light, or the polarizing member 140 and the polarizing member 130 that linearly polarize the laser light, are preferably set at 45 degrees to the tilt axis of the semi-transparent mirror 30, and the slit of the spectrometer 90 is also preferably set horizontally or vertically to the tilt axis of the semi-transparent mirror 30. The reflectance, transmittance, and spectral efficiency may differ slightly depending on whether the polarization direction is vertical or horizontal to the semi-transparent mirror 30, the slit of the spectrometer 90, and the tilt axis of the semi-transparent mirror 30. By setting the polarization axis of the laser light and the polarization axis of the polarizing member 130 at 45 degrees to the slit of the spectrometer 90 and the tilt axis of the semi-transparent mirror 30, the polarization phase difference is changed by the polarization phase difference variable member, and when the spectral intensity changes periodically, the phase of the intensity change caused by the difference due to polarization in the reflectance and transmittance of the semi-transparent mirror 30 and the spectral efficiency of the spectrometer 90 is shifted by 90 degrees from the periodic change of the original Raman scattered light. By incorporating the phase as well as the time-varying polarization axis or the period of the polarization phase difference into the extraction conditions based on the change in spectral intensity, a Raman spectrum with a better S / N ratio can be obtained.

[0191] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0192] For example, the wavelength of Raman scattered light is generated not only on the longer wavelength side than the wavelength of the laser light, but also on the shorter wavelength side than the wavelength of the laser light. In each of the above embodiments and modified examples, a Raman spectrum on the longer wavelength side than the wavelength of the laser light is used, but a Raman spectrum on the shorter wavelength side than the wavelength of the laser light may also be used.

[0193] 1 is an example in which the tempered glass 200 is placed on the fixing member 180, the vertical orientation of the tempered glass 200 and the physical quantity evaluation device 1 is not limited to this. For example, in the case of a large piece of glass having a length of 1 m or more, the same measurement is possible even if the physical quantity evaluation device 1 in FIG. 1 is turned upside down and placed on the tempered glass.

[0194] In addition to the above-described embodiment, the following supplementary notes are further disclosed. (Appendix 1) A physical quantity evaluation device for evaluating a physical quantity of a transparent measurement medium, comprising: A laser light source; a semi-transparent mirror for redirecting the optical path of the light from the laser light source toward the measurement medium; an objective lens that focuses the light from the semi-transparent mirror onto a surface or inside of the measurement medium; an imaging lens that forms an image at the focal point of the objective lens; a pinhole that transmits at least a part of the light of the image of the focal point of the objective lens; a spectrometer that separates the light that has passed through the pinhole; and an image sensor that detects the intensity of the spectrum generated by the spectrometer and converts the intensity into an electrical signal; A calculation unit for processing the electrical signal; having the objective lens, the imaging lens, and the pinhole constitute a confocal Raman spectroscopic microscope that measures a Raman spectrum, which is a spectrum of Raman scattered light from a portion of the measurement medium; The imaging element simultaneously measures the intensity of the surface reflection spectrum of the light and the intensity of the Raman spectrum. (Appendix 2) 2. The physical quantity evaluation device according to claim 1, further comprising a wavelength selection member between the semi-transparent mirror and the imaging element, the wavelength selection member attenuating light having a wavelength of laser light incident on the imaging element and transmitting light having a wavelength of the Raman spectrum. (Appendix 3) 3. The physical quantity evaluation device according to claim 2, wherein the wavelength selection member has an attenuation rate of 1 / 1000 or more and 1 / 100,000 or less at the wavelength of the laser light. (Appendix 4) 4. The physical quantity evaluation device according to claim 1, wherein a peak intensity of the Raman spectrum is 1 / 10 to 10 times a peak intensity of the surface reflection spectrum. (Appendix 5) 5. The physical quantity evaluation device according to claim 1, wherein the imaging element is a CMOS image sensor. (Appendix 6) 6. The physical quantity evaluation device according to claim 1, wherein the calculation unit has a function of detecting a surface point of the measurement medium based on the intensity of the surface reflection spectrum and the intensity of the Raman spectrum. (Appendix 7) 7. The physical quantity evaluation device according to claim 1, wherein the calculation unit adds up data obtained by exposing the image sensor a plurality of times. (Appendix 8) 8. The physical quantity evaluation device according to claim 7, wherein, when the image sensor is exposed a plurality of times with different exposure times, the calculation unit adds the surface reflection spectrum and the Raman spectrum with different weights for each exposure. (Appendix 9) 9. The physical quantity evaluation device according to claim 1, wherein the wave number of the Raman spectrum is calculated from a difference between the wave number and the wavelength of the surface reflection spectrum measured simultaneously. (Appendix 10) 10. The physical quantity evaluation device according to claim 1, wherein the measurement medium is glass. (Appendix 11) A fixing member for fixing the measurement medium is provided, 11. The physical quantity evaluation device according to claim 10, wherein the fixing member is configured to be able to change a distance between the fixing member and the objective lens. (Appendix 12) The physical quantity evaluation device described in Appendix 11, wherein the calculation unit measures the intensity of the surface reflection spectrum and / or the intensity of the Raman spectrum based on data captured when the focus of the objective lens is at any one depth of the measurement medium, or a plurality of data captured when the focus of the objective lens is at different positions in the depth direction of the measurement medium. (Appendix 13) 13. The physical quantity evaluation device according to claim 12, wherein the calculation unit calculates a certain depth of the measurement medium or stress in the depth direction by using the intensity of the Raman spectrum in the depth direction of the measurement medium. (Appendix 14) 14. The physical quantity evaluation device according to claim 13, wherein the calculation unit calculates the stress in the depth direction of the measurement medium based on the following formula (1):

[0195]

number

[0196] 1,2,2A Physical Quantity Evaluation Device 10 Laser light source 20 Optical Components 30 semi-transparent mirror 40 Objective Lens 50 Imaging Lens 60 Wavelength selection material 70 Passage area restriction member 70x pinhole 80 Light conversion material 90 spectrometer 91 Passage area restriction member 91x Slit 92 Optical Components 93 Diffraction Grating 94 Optical Components 100 Image sensor 110 Arithmetic section 111 Spectral data creation method 112 Spectral Intensity Measurement Means 113 Physical quantity calculation means 114 Fixed member moving means 120,150 Polarization state changing member 130,140 Polarizing element 180 Fixing member 181 Page 1 182 2nd page 183 Opening 200 Tempered Glass 201 Tempered Glass Surface 301 Digital Data Storage Circuit 302 Clock signal generating circuit 303 DA Converter 304 Voltage Amplifier Circuit

Claims

1. A physical quantity evaluation device for evaluating a physical quantity of a transparent measurement medium, comprising: A laser light source; a semi-transparent mirror for redirecting the optical path of the light from the laser light source toward the measurement medium; an objective lens that focuses the light from the semi-transparent mirror onto a surface or inside of the measurement medium; an imaging lens that forms an image at the focal point of the objective lens; a pinhole that transmits at least a part of the light of the image of the focal point of the objective lens; a spectrometer that separates the light that has passed through the pinhole; and an image sensor that detects the intensity of the spectrum generated by the spectrometer and converts the intensity into an electrical signal; A calculation unit for processing the electrical signal; having the objective lens, the imaging lens, and the pinhole constitute a confocal Raman spectroscopic microscope that measures a Raman spectrum, which is a spectrum of Raman scattered light from a portion of the measurement medium; The imaging element simultaneously measures the intensity of the surface reflection spectrum of the light and the intensity of the Raman spectrum.

2. 2. The physical quantity evaluation device according to claim 1, further comprising a wavelength selection member between the semitransparent mirror and the imaging element, the wavelength selection member attenuating light having a wavelength of the laser light incident on the imaging element and transmitting light having a wavelength of the Raman spectrum.

3. The physical quantity evaluation device according to claim 2 , wherein the wavelength selection member has an attenuation rate of 1 / 1000 to 1 / 100,000 at the wavelength of the laser light.

4. The physical quantity evaluation device according to claim 1 , wherein a peak intensity of the Raman spectrum is from 1 / 10 to 10 times a peak intensity of the surface reflection spectrum.

5. The physical quantity evaluation device according to claim 1 , wherein the imaging element is a CMOS image sensor.

6. The physical quantity evaluation device according to claim 1 , wherein the calculation unit has a function of detecting a surface point of the measurement medium based on an intensity of the surface reflection spectrum and an intensity of the Raman spectrum.

7. The physical quantity evaluation device according to claim 1 , wherein the calculation unit adds up data obtained by exposing the image sensor a plurality of times.

8. 8. The physical quantity evaluation device according to claim 7, wherein when the image sensor is exposed a plurality of times with different exposure times, the calculation unit adds the surface reflection spectrum and the Raman spectrum with different weights for each exposure.

9. 2. The physical quantity evaluation device according to claim 1, wherein the wave number of the Raman spectrum is calculated from a difference between the wave number and the wavelength of the surface reflection spectrum measured simultaneously.

10. The physical quantity evaluation device according to claim 1 , wherein the measurement medium is glass.

11. A fixing member for fixing the measurement medium is provided, The physical quantity evaluation device according to claim 10 , wherein the fixing member is configured so that a distance between the fixing member and the objective lens is variable.

12. The physical quantity evaluation device according to claim 11, wherein the calculation unit measures the intensity of the surface reflection spectrum and / or the intensity of the Raman spectrum based on data captured when the focus of the objective lens is at any one depth of the measurement medium, or a plurality of data captured when the focus of the objective lens is at different positions in the depth direction of the measurement medium.

13. The physical quantity evaluation device according to claim 12 , wherein the calculation unit calculates a certain depth of the measurement medium or a stress in the depth direction by using an intensity of the Raman spectrum in the depth direction of the measurement medium.

14. The physical quantity evaluation device according to claim 13 , wherein the calculation unit calculates the stress in the depth direction of the measurement medium based on the following formula (1): [0010] Here, Pk,n are coefficients for calculating the total stress value generated by ion exchange, and Ps,m is a coefficient indicating the amount of relaxation. n and m are each an integer. 0 is the tensile stress at the center of the glass that occurs to balance the overall stress, and z is the depth from the glass surface.

15. The physical quantity evaluation device according to claim 14 , wherein the parameters of the formula (1) are determined by measuring in advance a measurement medium having a known stress.

16. The physical quantity evaluation device according to claim 15 , wherein the measurement medium having a known stress is reinforced glass.

17. The physical quantity evaluation device according to claim 16 , wherein the measurement medium having the known stress is a plurality of measurement media.

18. The physical quantity evaluation device according to claim 17 , wherein the measurement medium having a known stress includes unstrengthened glass having an absolute value of a stress value of 10 MPa or less across the entire plate thickness.

19. 20. The physical quantity evaluation device according to claim 18, wherein the plurality of measurement media having known stresses further include a tempered glass having a surface layer with an absolute value of a stress value of 100 MPa or more.

20. 20. The physical quantity evaluation device according to claim 19, wherein the plurality of measurement media having known stresses include a plurality of tempered glasses having a surface layer with an absolute value of a stress value of 100 MPa or more, and a difference between the respective maximum compressive stresses is 100 MPa or more.

21. 16. The physical quantity evaluation device according to claim 15, wherein the measurement medium having a known stress includes crystallized glass having a known degree of crystallization.

22. 22. The physical quantity evaluation device according to claim 21, wherein the calculation unit calculates the degree of crystallinity at a certain depth of the measurement medium or in the depth direction by using the intensity of the Raman spectrum in the depth direction of the measurement medium.

23. 23. The physical quantity evaluation device according to claim 22, wherein the calculation unit uses a plurality of crystallized glasses having different degrees of crystallinity and calculates the degree of crystallinity by correlating a peak shape of a Raman spectrum with the degree of crystallinity.

24. The physical quantity evaluation device according to claim 11 , wherein the calculation unit corrects the shape of the Raman spectrum at each depth using a Raman spectrum of unstrengthened glass having an absolute value of a stress value of 10 MPa or less.

25. 2. The physical quantity evaluation device according to claim 1, further comprising a polarization state varying member for varying the polarization state of the laser light with time on an optical axis between the laser light source and the semitransparent mirror.

26. The physical quantity evaluation device according to claim 25 , wherein the polarization state varying member is a rotational polarization element.

27. The physical quantity evaluation device according to claim 25 , wherein the polarization state varying member is a variable retarder.

28. The physical quantity evaluation apparatus according to claim 27 , wherein the variable retarder is a liquid crystal retarder.

29. A physical quantity evaluation device for evaluating a physical quantity of a transparent measurement medium, comprising: a fixing member having a first surface that contacts a surface of the measurement medium and a second surface that faces the first surface; A laser light source; a semi-transparent mirror for redirecting the optical path of the light from the laser light source toward the measurement medium; an objective lens located on the second surface side and configured to collect light from the semitransparent mirror and focus the light on the first surface side rather than the second surface; an imaging lens that is located on the opposite side of the objective lens from the fixed member and that forms an image of the focal point; a pinhole located on the opposite side of the imaging lens from the fixed member, the pinhole allowing at least a part of the light of the image of the focal point to pass; a spectroscope located on the opposite side of the pinhole from the fixing member, the spectroscope separating light passing through the pinhole; an image sensor that detects the intensity of the spectrum generated by the spectrometer and converts the intensity into an electrical signal; having The objective lens, the imaging lens, and the pinhole constitute a confocal Raman spectroscopic microscope that measures a Raman spectrum, which is a spectrum of Raman scattered light from a portion of the measurement medium.

30. 30. The physical quantity evaluation device according to claim 29, wherein the imaging element simultaneously measures the intensity of the surface reflection spectrum of the light and the intensity of the Raman spectrum.

31. 31. The physical quantity evaluation device according to claim 29, wherein the measurement medium is glass.

32. A physical quantity evaluation method for evaluating a physical quantity of a transparent measurement medium, comprising: A focusing step of focusing light from a laser light source onto a surface or inside of a transparent measurement medium via a semi-transparent mirror and an objective lens; a spectroscopic step of forming an image of the focal point of the objective lens by an imaging lens, passing at least a part of the light of the image of the focal point of the objective lens through a pinhole, and spectroscopically separating the light that has passed through the pinhole; an imaging step of detecting the intensity of the spectrum obtained in the spectroscopic step and converting the intensity into an electrical signal; A calculation step of processing the electrical signal; having the objective lens, the imaging lens, and the pinhole constitute a confocal Raman spectroscopic microscope that measures a Raman spectrum, which is a spectrum of Raman scattered light from a portion of the measurement medium; In the imaging step, the intensity of the surface reflection spectrum of the light and the intensity of the Raman spectrum are simultaneously measured.

33. The physical quantity evaluation method according to claim 32 , wherein the measurement medium is glass.

Citation Information

Patent Citations

  • Surface stress measuring apparatus of chemically tempered glass

    JP1978136886A

  • Memory control system

    JP1987003355A

  • Method and apparatus for measuring stress

    JP1994347343A

  • Surface stress measurement method and surface stress measurement device

    JP2016142600A

  • Method for evaluating residual stress of chemically strengthened glass

    JP2020139940A