Artificial leather damping material

The damping material with artificial leather and thermoplastic elastomers/nanocellulose achieves directional control of elasticity and damping, addressing the limitations of existing materials by enhancing anisotropy and compatibility.

JP2024167857APending Publication Date: 2024-12-04RIYONX
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023094401
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Existing damping materials struggle to achieve both high elasticity and damping properties in specific directional requirements, failing to address the anisotropy and compatibility of mechanical strength and damping performance.

Method used

A damping material comprising artificial leather with a woven fabric inside, coated with thermoplastic elastomers and nanocellulose on one or both sides, allowing for differential elasticity and damping properties based on the fabric's warp and weft directions, and creating asymmetric structures for enhanced control.

Benefits of technology

The material effectively controls vibration damping by varying storage modulus and damping performance according to the object's motion, improving elasticity and damping properties in desired directions, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167857000001_ABST
    Figure 2024167857000001_ABST
Patent Text Reader

Abstract

To provide a vibration damping material capable of suppressing the vibration as much as possible in order to overcome a problem that a direction in which a vibrating body vibrates is not necessarily unidirectional, and in particular, in the case of a moving body, vibration damping properties with different characteristics in the orthogonal direction may be required.SOLUTION: A damping material has an artificial leather having a woven fabric inside, a thermoplastic elastomer mixed with nano-cellulose on one and / or the other surface of the artificial leather, and further has a thermoplastic elastomer on the outside of one side without it or on one side with it on both sides.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a vibration-damping material using artificial leather, and in particular to a vibration-damping material that has different vibration-damping properties in the warp and weft directions, thereby providing vibration-damping properties while accurately controlling the movement of a damped object, and to a product using the same. [Background technology]

[0002] Traditionally, vibration-damping materials have been widely used to suppress vibrations in the fields of mobile industries such as automobiles, ships, railways, and aircraft, as well as the machinery industry, construction industry, electric mobile industry, sports industry, and daily necessities industry. In particular, in recent years, as parts and components in various fields have become more advanced and smaller, there has been a demand for vibration-damping materials that do not simply suppress vibration but also have the added functionality appropriate for each component and component, and that are more advanced and smaller.

[0003] For example, insoles for sports shoes are required to have two properties: vibration absorption when the heel touches the ground and high elasticity when kicking the ground. In addition, in moving objects such as automobiles, while vibration damping is required to reduce vibration, technology is also required to achieve both mobility during acceleration and other times.

[0004] Technological developments in pursuit of these dual properties have been made in recent years, and Patent Document 1 discloses a laminate having vibration damping properties and rebound resilience, in which a laminate having a base fabric layer, a vibration damping layer on at least one side of the base fabric layer, and a rebound resilience layer on the outermost side of the base fabric layer and / or the vibration damping layer is described as having both good vibration damping properties and rebound resilience, and the base fabric layer may be any sheet-like fibrous base material that has a suitable thickness, a solid feel, and a soft texture, and in particular, various types of fibrous base materials that have traditionally been used in the manufacture of artificial leather-like laminates can be preferably used, and examples of such fibrous sheets include entangled nonwoven sheets and knitted and woven sheets.

[0005] Patent Document 2 discloses a vibration-damping rubber composition that can achieve both vibration-damping properties and mechanical properties such as strength and hardness. The composition is prepared by combining a rubber component, a vibration-damping agent, and modified cellulose nanofibers bonded to a fluorene compound having an aryl group at the 9,9-position. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2018-108646 A [Patent Document 2] JP 2020-019886 A [Non-patent literature]

[0007] [Non-Patent Document 1] Ministry of the Environment "Guidelines for Utilizing Cellulose Nanofiber" Reiwa 3 Summary of the Invention [Problem to be solved by the invention]

[0008] In Patent Document 1, the base fabric is defined as being sufficient as long as it is a fibrous base material, and therefore the focus is mainly on its flexibility. Furthermore, since both the vibration-damping layer and the resilience layer are made of a thermoplastic elastomer, the viewpoint of actively utilizing the anisotropy due to weave is not taken into consideration.

[0009] In Patent Document 2, as described in the specification, vibration damping properties and mechanical strength are generally incompatible, but the 40% decrease in Tan delta due to the difference between carbon black and CNF is by no means small. In addition, there is no viewpoint of actively utilizing anisotropy due to the process.

[0010] Simply achieving both vibration-damping properties and high elasticity or mechanical strength, as seen in the above-mentioned conventional technology, had the problem of being unable to accommodate directions where vibration-damping properties were primarily required, directions where high elasticity was primarily required, and directions where a certain amount of distortion was required.

[0011] The problem that the present invention aims to solve is to resolve the problems encountered in the prior art, and to provide a vibration-damping material that actively produces differences in vibration-damping properties and storage elastic modulus depending on the directionality of the weft and weft, and that is suited to the movement characteristics of the body to be damped, which is the source of vibration. [Means for solving the problem]

[0012] A vibration-damping material (11) according to one embodiment of the present invention comprises artificial leather (A) having a woven fabric (a) therein, a thermoplastic elastomer (B1) applied by coating on one surface of the artificial leather (A), and nanocellulose (C1) mixed with the thermoplastic elastomer (B1).

[0013] Another embodiment of the vibration-damping material (12) of the present invention comprises artificial leather (A) having a woven fabric (a) therein, a thermoplastic elastomer (B1) applied by coating on one surface of the artificial leather (A), nanocellulose (C1) mixed with the thermoplastic elastomer (B1), and a thermoplastic elastomer (D) applied by coating on the other surface of the artificial leather (A).

[0014] Another embodiment of the vibration-damping material (13) of the present invention comprises artificial leather (A) having a woven fabric (a) therein, thermoplastic elastomers (B1, B2) applied by coating on one and the other surfaces of the artificial leather (A), and nanocellulose (C1, C2) mixed with both of the thermoplastic elastomers (B1, B2).

[0015] Furthermore, a vibration-damping material (14) according to another embodiment of the present invention comprises artificial leather (A) having a woven fabric (a) therein, thermoplastic elastomers (B1, B2) applied by coating on one and other surfaces of the artificial leather (A), nanocellulose (C1, C2) mixed with both of the thermoplastic elastomers (B1, B2), and a thermoplastic elastomer (D) applied by coating on one or the other outer surface of the thermoplastic elastomers (B1, B2). Effect of the Invention

[0016] According to the present invention, by using artificial leather with a woven fabric inside as the base fabric, it is possible to have different elasticity, vibration damping, and distortion properties depending on the warp and weft directions of the fabric. This makes it possible to match the direction requiring elasticity, vibration damping, and distortion properties, enabling control in accordance with the movement of the vibrated body.

[0017] Furthermore, when the artificial leather is subjected to bending stress due to an external force such as vibration, the internal fabric is positioned between the compression side and the tension side, and one side and the other side are divided into the compression side and the tension side, respectively, making them unequal or equivalent, which enables more active vibration control, such as changing the storage modulus and improving vibration damping.

[0018] Moreover, not only is the elasticity increased, but the storage modulus can be reduced as if springs were connected in series, despite the parallel configuration.

[0019] Furthermore, by placing a thermoplastic elastomer mixed with nanocellulose on both sides of the artificial leather, and then placing a thermoplastic elastomer without nanocellulose mixed in on only one side, it becomes as if the nanocellulose mixed layer faces the non-constrained layer and the constrained layer on each side, thereby further improving the vibration damping properties.

[0020] Furthermore, although this is not reflected in the numbers, by mixing nanocellulose, the interface of the thermoplastic elastomer becomes flexible, so that the developed vibration-damping material can be used in a bent state without impeding the movement of the vibrated body. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a cross-sectional view of a vibration-damping material according to a first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the vibration-damping material according to the second embodiment. [Diagram 3] FIG. 3 is a cross-sectional view of a vibration-damping material according to the third embodiment. [Figure 4] FIG. 4 is a cross-sectional view of a vibration-damping material according to the fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The vibration-damping material of the present invention can be broadly divided into two types depending on the materials it contains: one is made of artificial leather with a built-in textile and a thermoplastic elastomer mixed with nanocellulose, and the other is made of artificial leather with a built-in textile, a thermoplastic elastomer mixed with nanocellulose, and a thermoplastic elastomer. The present invention will be explained below.

[0023] (artificial leather) First, the artificial leather that serves as the base fabric has a nonwoven structure made by intertwining fine fibers such as microfibers, and is made by impregnating it with resin such as urethane, and is roughly divided into two types: the grain type and the suede type. The grain type or the suede type can be selected according to the purpose of the artificial leather of the present invention, but it is preferable to use the suede type.

[0024] The fabric inside the artificial leather is also called a scrim, and is placed inside a nonwoven structure made of intertwined fine fibers. Its original purpose was to improve dimensional stability, stretchability, and strength, but as a vibration-damping material it is placed inside to impart anisotropy in the warp and weft directions, as mentioned above, and for the mechanical properties as an intermediate part between the compression side and the tension side.

[0025] As an example of the manufacturing process, ultrafine fibers are cut short to create a nonwoven layer on the surface of a fabric, and then the fibers are entangled with the fabric and fibers with a high-pressure water flow, and the gaps between the fibers are impregnated with polyurethane. Ultrafine fibers are made by three-dimensionally entangling fibers of about 0.1 decitex called microfibers, and depending on the difference in fineness, they may be divided into a front side and a back side to form a three-layer structure, or they may be created by forming a layer in which some ultrafine fibers are bundled together. They may also be manufactured by performing treatments such as dyeing, stain resistance, electrostatic and water repellency.

[0026] The composition of the woven fabric and the composition of the intertwined fibers may be, depending on the application, regenerated fibers such as rayon and Tencel, semi-synthetic fibers such as acetate and triacetate, organic synthetic fibers such as nylon, polyester, polyurethane and acrylic, chemical fibers such as synthetic fibers like glass fiber, metal fiber and carbon fiber, plant fibers such as cotton and hemp, and natural fibers such as animal fibers like wool and silk, which may be used alone or as a blend or mixture of two or more kinds. Organic synthetic fibers such as polyester and polyurethane are preferably used.

[0027] Woven fabrics are formed by arranging warp threads in parallel and inserting weft threads so that they cross the warp threads in a staggered pattern, and are broadly classified into three basic weaves: plain weave, twill weave, and satin weave, depending on the order and combination of the weave points, which are the crossing points, in the warp and weft directions of the fabric. Variations are also made based on these three basic weaves, but any of the weaves will do, and it would be preferable to use plain weave.

[0028] The overall thickness of the artificial leather is approximately 0.3 mm to 2.0 mm, the basis weight is approximately 100 g / m2 to 500 g / m2, and the single yarn fineness is approximately 0.03 decitex to 0.3 decitex, and these can be selected appropriately depending on the application.

[0029] A similar material to artificial leather is synthetic leather, but synthetic leather is made by applying resin to a base fabric such as knitted or woven fabric and then adhering fibers to it, whereas the artificial leather used in this vibration-damping material, as mentioned above, is made by intertwining woven and nonwoven fabric layers with fibers and fibers and impregnating them with resin such as urethane. This difference in manufacturing method means that the fibers are able to move more easily in microscopic areas, and it is thought that when a thermoplastic elastomer mixed with nanocellulose is applied to the surface of the artificial leather, the nanocellulose clings to the fibers of the artificial leather, improving the vibration-damping effect.

[0030] In addition to woven fabrics, structures formed by interlacing threads include knitted fabrics, braided fabrics, lace, and rope. In knitted fabrics, the threads are interlaced in loops, whereas in woven fabrics, the threads are interlaced in straight lines when viewed from the surface direction. This structure is thought to make shear deformation more likely to occur, making it easier for the hydrogen bonds between the nanocellulose fibers to break.

[0031] (Thermoplastic elastomer) Thermoplastic elastomers consist of soft segments that have viscoelasticity and rubber elasticity, and hard segments that have fluidity at high temperatures but prevent plastic deformation at room temperature, and include polystyrene, polyolefin, vinyl chloride, polyurethane, polyester, and polyamide types. For the vibration damping material of the present invention, the type may be selected according to the application, but urethane resin and acrylic resin types would be preferable.

[0032] The form of the thermoplastic elastomer when applied to artificial leather can be selected according to the application, from emulsion types in which resin particles are dispersed in water, mainly produced by emulsion polymerization; aqueous resin suspension types produced by suspension polymerization; water-soluble types; solvent types; and solventless types.

[0033] By applying this thermoplastic elastomer to one and / or the other side of artificial leather with a woven fabric inside, it is possible to accommodate the elongation of the artificial leather when pulled horizontally while also ensuring strength in the planar direction, making it possible to use it for vibration-damping bodies ranging from soft cloth objects to hard objects such as plastic molded bodies.

[0034] Furthermore, even if a thermoplastic elastomer is provided on both sides of an artificial leather having a woven fabric, the structure is mediated by the ultra-fine fibers and woven fabric of the artificial leather, making it possible for the two to be displaced without being affected by each other.

[0035] (Nanocellulose) Nanocellulose is a type of cellulose fiber, the main component of the cell walls of plants such as wood, whose length, width, or height are in the range of 1 to 100 nanometers. Cellulose is a natural polymer in which glucose molecules are bonded in a linear chain, and plant-derived fibers in which these cellulose molecular chains are bundled together and whose diameter is in the range of 3 to 100 nanometers are generally referred to as cellulose nanofibers.

[0036] It is classified into several types according to its manufacturing method, including cellulose nanofibers (also called CNF or cellulose nanofibril) made by mechanical defibration or other physical methods, cellulose nanofibers made by chemical treatments such as TEMPO oxidation and simple mechanical defibration (TEMPO-oxidized cellulose nanofibers are called TOCNF), cellulose nanocrystals (called CNC or cellulose nanowhiskers) made by hydrolyzing the amorphous regions of cellulose fibers with acid, and bacterial cellulose (called BNC or BC) made by synthesizing cellulose using carbohydrates such as glucose as a carbon source by microorganisms such as acetic acid bacteria.

[0037] The diameter of the fibers varies depending on the production method, with the diameter ranging from 3 to 5 nanometers for TEMPO-oxidized cellulose nanofibers, 3 to several micrometers for mechanically defibrated cellulose nanofibers, 3 to 50 nanometers for cellulose nanocrystals, and approximately 20 to 100 nanometers for bacterial cellulose.

[0038] Furthermore, the length of each fiber also has its own range, with cellulose nanofibers being less than 100 micrometers, cellulose nanocrystals being 100 to 500 nanometers, and bacterial cellulose being 1.5 to 5 micrometers (for details on nanocellulose, see Non-Patent Document 1).

[0039] The nanocellulose used in the vibration-damping material of the present invention may be manufactured by any of the following methods: mechanical fiberization, chemical processing, and synthesis by microorganisms. The fibers themselves may be amphiphilic, i.e., hydrophilic and hydrophobic, or may be made amphiphilic by blending with other solvents. Any suitable material may be used, including thermoplastic elastomers.

[0040] In addition, even if fibers with diameters exceeding 100 nanometers are mixed in, it is not the case that the effect is not immediately lost, so it is sufficient to mix in a certain amount of fibers with diameters less than 100 nanometers. The length of the fibers can also be selected according to the application. It is preferable that the aspect ratio, which is the fiber length divided by the fiber diameter, is not less than 10.

[0041] (Other additives) Other additives may be added or mixed into the plastic elastomer, regardless of their name, such as water, purified water, distilled water, pigments, dyes, curing agents, crosslinking agents, preservatives, antistatic agents, and flame retardants, as long as they do not contradict the meaning of the present invention.

[0042] (Embodiment 1) Using the above materials, in embodiment 1, a thermoplastic elastomer mixed with nanocellulose is applied by coating on one side of an artificial leather having a woven fabric inside.

[0043] The nanocellulose to be mixed with the thermoplastic elastomer may be a single type or a composite of two or more types.

[0044] When mixing thermoplastic elastomers and nanocellulose, factors that must be avoided in the manufacturing process include localized static electricity due to contact friction.

[0045] Static electricity can be caused by friction, contact, peeling, or induction, and localized charging is possible during the manufacturing process of the original material, and since thermoplastic elastomer resins tend to be relatively negatively charged and nanocellulose wood-based materials tend to be relatively positively charged, there is a possibility of localized charging when these are mixed. Since static electricity can cause variations in quality, it goes without saying that static electricity must be prevented as much as possible in all manufacturing processes.

[0046] One method of preventing static electricity is to use antistatic agents as additives, but in order to achieve vibration damping even with a weak external force, we adopted a method of suppressing localized static electricity by taking into consideration the electrostatic characteristics of the mixing table and mixing container and combining them to ensure distortion within the thermoplastic elastomer.

[0047] In addition, in the process of mixing the thermoplastic elastomer and nanocellulose, auxiliary agents such as dispersants are generally used to ensure uniform dispersion so that the nanocellulose fibers do not aggregate. However, the vibration-damping material of the present invention is characterized in that the materials are loosely bonded together, and no auxiliary agents such as dispersants are required.

[0048] The vibration-damping material of the present invention is configured so that the nanocellulose fibers aggregate to a certain extent, thereby preventing heat loss due to friction not only between the thermoplastic elastomer and the nanocellulose, but also between the ultrafine fibers of the artificial leather and the thermoplastic elastomer, between the ultrafine fibers of the artificial leather and the nanocellulose, and even between the aggregated nanocellulose fibers themselves.

[0049] The method of application to artificial leather may be selected appropriately according to the application, regardless of whether it is manual or mechanical, such as spatula, brush, roller, spray, stencil, silk screen, applicator, coating machine, etc. In addition, sufficient consideration should be given to static electricity countermeasures during the application process.

[0050] The surface to be coated of the artificial leather may be either the front or back. The coating area may be the entire surface or only a part of the surface of the artificial leather, and the coating may be in the form of a figure such as "XXX" or letters such as "ABC".

[0051] The amount of thermoplastic elastomer applied to the artificial leather is about 0.1 micrometer to 1 millimeter, including the amount impregnated into the surface fibers of the artificial leather, when dried, and preferably in the range of about 1 micrometer to 0.5 millimeter.

[0052] By applying a thermoplastic elastomer mixed with nanocellulose to one side of artificial leather with a woven fabric inside, it is possible to impart vibration damping properties in the tensile direction in the low-frequency range while retaining the flexibility and texture of the artificial leather.

[0053] (Embodiment 2) In embodiment 2, a thermoplastic elastomer mixed with nanocellulose is applied by coating one side of an artificial leather having a woven fabric inside, and a thermoplastic elastomer is applied by coating the other side of the artificial leather.

[0054] As in embodiment 1, the nanocellulose to be mixed with the thermoplastic elastomer may be a single type or a composite of two or more types.

[0055] The thermoplastic elastomer containing nanocellulose and the thermoplastic elastomer not containing nanocellulose may be the same or different types, and may be selected according to the application.

[0056] Other aspects are the same as those of the first embodiment.

[0057] By configuring it in this manner, the vibration damping properties under simple tension are inferior to those of embodiment 1, but even when embodiment 2 is folded in half, the elastic forces of the thermoplastic elastomer containing nanocellulose and the thermoplastic elastomer not containing nanocellulose differ on the compression side and the tension side, which causes shear forces to occur within the artificial leather, and the presence of nanocellulose makes it possible to maintain vibration damping properties.

[0058] (Embodiment 3) In the third embodiment, a thermoplastic elastomer mixed with nanocellulose is applied to both one and the other surfaces of an artificial leather having a woven fabric inside.

[0059] In the third embodiment, the nanocellulose mixed into the thermoplastic elastomer may be the same or different on one side of the artificial leather as the type on the other side, and may be a single type on each side or a combination of two or more types.

[0060] Also, with regard to the thermoplastic elastomer, the type of thermoplastic elastomer on one side of the artificial leather may be the same as or different from the type of thermoplastic elastomer on the other side.

[0061] Other aspects are the same as those of the first embodiment.

[0062] By configuring in this manner, improvement in vibration damping properties in tension cannot be obtained, but improvement in vibration damping properties in the direction perpendicular to the surface of the artificial leather can be expected.

[0063] (Embodiment 4) In embodiment 4, a thermoplastic elastomer mixed with nanocellulose is applied by coating on one and other surfaces of an artificial leather having a woven fabric inside, and a thermoplastic elastomer is applied by coating on the outer surface of one or the other of the thermoplastic elastomers.

[0064] In the fourth embodiment, the nanocellulose mixed into the thermoplastic elastomer may be the same or different on one side of the artificial leather as the type on the other side, and may be a single type on each side or a combination of two or more types.

[0065] In addition, the thermoplastic elastomers mixed with nanocellulose may be of the same or different types, and the thermoplastic elastomers not mixed with nanocellulose may be of the same or different types.

[0066] The amount of thermoplastic elastomer not mixed with nanocellulose that can be applied can be about the same as the amount of thermoplastic elastomer mixed with nanocellulose, and since there is almost no impregnation into the artificial leather, it can be slightly thinner.

[0067] Other aspects are the same as those of the first embodiment.

[0068] By configuring in this way, it is possible to have the characteristics of the first to third embodiments in a comprehensive manner. Also, when focusing on the thermoplastic elastomer mixed with nanocellulose on one side and the other side of the artificial leather, the artificial leather has a non-constrained form and a constrained form with the woven fabric inside the artificial leather at the center. Furthermore, when the thermoplastic elastomer without nanocellulose is included, the artificial leather has an asymmetrical configuration with the woven fabric inside the artificial leather at the center, and although it is not shown in numerical values, the vibration damping properties are maintained even when the vibrated body is moving.

[0069] Furthermore, the vibration-damping properties can be exhibited whether the film is folded in half and sewn onto soft objects such as clothing, or whether it is attached to foam material, or whether it is attached to hard objects such as plastic or metal, making it suitable for a variety of uses. EXAMPLES

[0070] The vibration damping material of the present invention will be specifically described below with reference to each example, but the vibration damping material of the present invention is not limited to these examples in any way.

[0071] [Artificial leather] The artificial leather with a woven fabric inside was a suede-like leather with a thickness of 0.6 mm [manufactured by Toray Industries, Inc.; product name "ultrasuede" (registered trademark) LX CB1]. For comparison, the artificial leather with no woven fabric inside was a suede-like leather with a thickness of 0.7 mm [manufactured by Toray Industries, Inc.; product name "Ecsaine" (registered trademark), former product orange].

[0072] The artificial leather was cut into a piece 10 cm long in the warp direction and 5 cm long in the weft direction to form a base fabric for an artificial leather vibration damping material.

[0073] [Thermoplastic elastomer] The thermoplastic elastomer mainly used was a urethane resin-based binder for printing on fabric products.

[0074] [Nanocellulose] The nanocellulose used was mainly TEMPO-oxidized cellulose nanofibers, but mechanically defibrated cellulose nanofibers and bacterial cellulose were also used.

[0075] [Mixing method] The thermoplastic elastomer and nanocellulose were mixed in two ways. In the first method, a 15 mm thick wooden board (shina) and a 9 mm thick cork board were used as the mixing table, and a glass petri dish and a stainless steel petri dish were used as the mixing container on a laboratory bench with a relatively rough surface, and the thermoplastic elastomer and nanocellulose were mixed with a resin painting knife (manufactured by Richeson). In the second method, a cupra (manufactured by Asahi Kasei Corporation; product name "Bemberg" (registered trademark) AK850) was laid on a relatively smooth table top, and the thermoplastic elastomer and nanocellulose were mixed with a glass petri dish and a resin painting knife (manufactured by Richeson) as the mixing container.

[0076] [Coating method] Two methods were used to apply the thermoplastic elastomer to the artificial leather. In the first method, a 12 mm thick cypress laminate was used as the application table, the artificial leather was placed on top of it, and the material was secured in place with masking tape, and the material was applied directly using a resin painting knife (Richeson) as a spatula. In the second method, the cypress laminate was also used as the application table, and the material was secured in place with masking tape, and a rectangular plate of 80 count Tetoron gauze was created from a three-layer sheet, and the material was applied using the silk screen method with a resin squeegee.

[0077] [Drying method] After coating, the thermoplastic elastomer surface was dried by applying hot air from a dryer for 2 minutes, followed by drying in a constant temperature dryer at 110 degrees for 3 minutes or by natural drying.

[0078] [Test piece for evaluation] After the thermoplastic elastomer had sufficiently dried, the artificial leather vibration damping material was cut into pieces of 8 mm and 30 mm in the vertical and horizontal directions to prepare test pieces for evaluation.

[0079] [Evaluation method] The evaluation method used a dynamic viscoelasticity measuring device [DMA Q800, manufactured by TA Instruments Japan, Inc.] to determine the storage modulus (E'), loss modulus (E"), and loss tangent (Tan δ) of E' / E" at a frequency of 1 Hz using a frequency-dependent tensile test method for the above-mentioned evaluation specimens, and the measured values ​​of storage modulus (E') and loss tangent (Tan δ) were evaluated. The gripping distance was approximately 20 mm, and the strain rate was 0.1%.

[0080] The measurements obtained with this method were obtained by applying a 1Hz sine wave force to the test piece to deform it, measuring the storage modulus, which indicates elasticity, and the loss modulus, which indicates viscosity, when a strain of about 20 micrometers is generated, and calculating the ratio of these as the loss tangent. In other words, the storage modulus is the elastic force required to generate a strain of about 20 micrometers in the test piece, and the loss tangent is the viscosity ratio of the test piece at that time. EXAMPLES

[0081] The artificial leather used had a woven fabric inside, and the thermoplastic elastomer used was an aqueous urethane emulsion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910]. The nanocellulose used was mechanically defibrated cellulose nanofiber [manufactured by Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) softwood pulp, highly defibrated]. Note that highly defibrated refers to fibers that have been defibrated to a width of approximately 5 nanometers to 200 nanometers.

[0082] The mixing method consisted of 100 parts by mass of aqueous urethane emulsion and 60 parts by mass of mechanically defibrated cellulose nanofibers, which were mixed on a wooden board (Japanese linden) using a glass petri dish and a resin painting knife.

[0083] The coating method was to directly coat the surface of the artificial leather with an aqueous urethane emulsion mixed with mechanically defibrated coniferous cellulose nanofibers using a resin painting knife, and then dry at a constant temperature, as in embodiment 1.

[0084] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 1. EXAMPLES

[0085] The materials and mixing method were the same as in Example 1, but the application method involved directly applying an aqueous urethane emulsion mixed with mechanically defibrated cellulose nanofibers to the surface of the artificial leather and then applying the aqueous urethane emulsion to the back of the artificial leather using a resin painting knife, and drying was performed at a constant temperature, resulting in the configuration of embodiment 2.

[0086] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 2. EXAMPLES

[0087] The materials and mixing method were the same as in Example 1, but the application method involved directly applying an aqueous urethane emulsion mixed with mechanically defibrated cellulose nanofibers to both the front and back sides of the artificial leather using a resin painting knife, and drying at a constant temperature, resulting in the configuration of embodiment 3.

[0088] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 3. EXAMPLES

[0089] The artificial leather used had a woven fabric inside, and the thermoplastic elastomer used was an acrylic resin paste [manufactured by Matsui Shikiso Kagaku Kogyosho Co., Ltd.; product name "Stretch Clear 701B"]. The nanocellulose used was mechanically defibrated cellulose nanofiber [manufactured by Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) hardwood pulp, strong defibration]. Note that strong defibration refers to fibers that have been defibrated to a width of approximately 5 nanometers to 200 nanometers.

[0090] The mixing method involved mixing 100 parts by mass of acrylic resin paste and 60 parts by mass of mechanically defibrated cellulose nanofibers on a cork board using a glass petri dish and a resin painting knife.

[0091] The application method involved directly applying an acrylic resin paste mixed with mechanically defibrated hardwood cellulose nanofibers to the front and back surfaces of the artificial leather using a resin painting knife. After drying the front surface, an acrylic resin not mixed with nanocellulose was directly applied to the outer surface of the acrylic resin mixed with hardwood cellulose nanofibers on the back surface of the artificial leather using a resin painting knife, and drying was performed at a constant temperature, resulting in the configuration of embodiment 4.

[0092] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 4. EXAMPLES

[0093] The artificial leather used had a woven fabric inside, the thermoplastic elastomer was a water-based acrylic silicone resin [manufactured by Campe Hapio Co., Ltd.; product name "Nuro" clear coat transparent], and the nanocellulose was mechanically defibrated cellulose nanofiber [manufactured by Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) softwood pulp, strong defibration].

[0094] The mixing method consisted of 100 parts by mass of water-based acrylic silicone resin and 60 parts by mass of mechanically defibrated cellulose nanofiber, which were mixed on a cork board using a stainless steel petri dish and a resin painting knife.

[0095] The coating method was to directly coat the front and back surfaces of the artificial leather with a resin painting knife using a water-based acrylic / silicone resin mixed with mechanically defibrated softwood cellulose nanofibers. After the surface was dried, the water-based acrylic / silicone resin not mixed with nanocellulose was directly coated on the outer surface of the water-based acrylic / silicone resin mixed with softwood cellulose nanofibers on the back surface of the artificial leather using a resin painting knife, and the coating was dried at a constant temperature, resulting in the configuration of embodiment 4.

[0096] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 5. EXAMPLES

[0097] The artificial leather used had a woven fabric inside, and the thermoplastic elastomers used were an aqueous urethane emulsion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-810] and an aqueous urethane emulsion titanium dispersion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-820]. The nanocellulose used was mechanically defibrated cellulose nanofiber [manufactured by Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) softwood pulp, strong defibration].

[0098] The mixing method consisted of 100 parts by mass of aqueous urethane emulsion, 60 parts by mass of mechanically defibrated cellulose nanofiber, and 100 parts by mass of aqueous urethane emulsion titanium dispersion, and 60 parts by mass of mechanically defibrated cellulose nanofiber. The mixture was mixed on a wooden board (Japanese navy) using a stainless steel petri dish and a resin painting knife.

[0099] The coating method was as follows: the titanium aqueous urethane emulsion dispersion mixed with mechanically defibrated softwood cellulose nanofibers was directly coated on the surface of the artificial leather using a resin painting knife. The aqueous urethane emulsion mixed with mechanically defibrated softwood cellulose nanofibers was directly coated on the back surface of the artificial leather using a resin painting knife. After the surface was dried, the aqueous urethane emulsion not mixed with nanocellulose was directly coated on the outer surface of the aqueous urethane mixed with softwood cellulose nanofibers on the back surface of the artificial leather using a resin painting knife, and the drying was performed at a constant temperature, resulting in the configuration of the fourth embodiment.

[0100] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 6. EXAMPLES

[0101] The artificial leather used had a woven fabric inside, and the thermoplastic elastomer used was an aqueous acrylic ester resin [Tanaka Chemical Co., Ltd.; product name "Tanakarabar No. 600 Binder"] and an aqueous urethane emulsion [Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910]. The nanocellulose used was mechanically defibrated cellulose nanofiber [Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) softwood pulp, strong defibration].

[0102] The mixing method involved mixing 100 parts by mass of aqueous acrylic ester resin and 60 parts by mass of mechanically defibrated cellulose nanofibers on a wooden board (Japanese linden) using a glass petri dish and a resin painting knife.

[0103] The coating method was as follows: an aqueous acrylic ester resin mixed with mechanically defibrated softwood cellulose nanofibers was directly coated on the front and back surfaces of the artificial leather using a resin painting knife. After the front surface was dried, an aqueous urethane emulsion not mixed with nanocellulose was directly coated on the outer surface of the aqueous acrylic ester resin mixed with softwood cellulose nanofibers on the back surface of the artificial leather using a resin painting knife, and the coating was dried at a constant temperature, resulting in the configuration of embodiment 4.

[0104] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 7. EXAMPLES

[0105] The artificial leather used had a woven fabric inside, and the thermoplastic elastomer used was an aqueous urethane emulsion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910]. The nanocellulose used was mechanically defibrated cellulose nanofiber [manufactured by Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) softwood pulp defibrated]. Note that defibrated refers to fibers whose width is defibrated to a range of approximately 5 nanometers to 500 nanometers.

[0106] The mixing method consisted of 100 parts by mass of aqueous urethane emulsion and 60 parts by mass of mechanically defibrated cellulose nanofibers, which were mixed on a wooden board (Japanese linden) using a glass petri dish and a resin painting knife.

[0107] The coating method was to directly coat the front and back surfaces of the artificial leather with an aqueous urethane emulsion mixed with mechanically defibrated softwood cellulose nanofibers using a resin painting knife. After drying the front surface, an aqueous urethane emulsion not mixed with nanocellulose was directly coated on the outer surface of the aqueous urethane mixed with softwood cellulose nanofibers on the back surface of the artificial leather using a resin painting knife, and the coating was dried at a constant temperature, resulting in the configuration of embodiment 4.

[0108] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 8. EXAMPLES

[0109] The materials and manufacturing method were the same as in Example 8, except that TEMPO oxidized cellulose nanofiber [manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; product name "LeoCrysta" I-2SX] (containing preservative) was used as the nanocellulose.

[0110] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 9. EXAMPLES

[0111] The artificial leather used had a woven fabric inside, the thermoplastic elastomer used was an aqueous urethane emulsion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910], and the nanocellulose used was TEMPO-oxidized cellulose nanofiber [manufactured by Nippon Paper Industries Co., Ltd.; product name "Cellenpia" TC-01A3%].

[0112] The mixing method involved mixing 100 parts by mass of the aqueous urethane emulsion and 40 parts by mass of TEMPO oxidized cellulose nanofibers using a glass petri dish with cupra underneath and a resin painting knife.

[0113] The coating method was as follows: an aqueous urethane emulsion mixed with TEMPO oxidized cellulose nanofibers was applied by silk screen coating to the front and back surfaces of the artificial leather. After the front surface was dried, an aqueous urethane emulsion not mixed with nanocellulose was applied by silk screen coating to the outer surface of the aqueous urethane mixed with TEMPO oxidized cellulose nanofibers on the back surface of the artificial leather, and the coating was naturally dried, resulting in the configuration of embodiment 4.

[0114] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 10. EXAMPLES

[0115] The materials and manufacturing method were the same as in Example 10, except that an aqueous urethane emulsion not containing nanocellulose was applied to the aqueous urethane containing TEMPO oxidized cellulose nanofiber on the surface side of the artificial leather.

[0116] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 11. EXAMPLES

[0117] The materials and manufacturing method were the same as in Example 10, except that TEMPO oxidized cellulose nanofiber [manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; product name "Leocrysta" I-2AX] (blended with polar solvent) was used as the nanocellulose.

[0118] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 12. EXAMPLES

[0119] The artificial leather used had a woven fabric inside, the thermoplastic elastomer was a water-based resin [manufactured by Mino Group Co., Ltd.; product name "Aqua PEX"], and the additive was a hardener [manufactured by Mino Group Co., Ltd.; product name "Aqua P Hardener"]. The nanocellulose used was TEMPO-oxidized cellulose nanofiber [manufactured by Nippon Paper Industries Co., Ltd.; product name "Cellenpia" TC-01A3%].

[0120] The mixing method involved adding 100 parts by mass of aqueous resin, 20 parts by mass of TEMPO oxidized cellulose nanofiber, and a small amount of hardener, and mixing them using a glass petri dish and a resin painting knife with cupra placed underneath.

[0121] The coating method was to coat the front and back surfaces of the artificial leather with an aqueous resin mixed with TEMPO oxidized cellulose nanofibers by silk screen coating.Then, after drying the front surface, an aqueous resin not mixed with nanocellulose was coated by silk screen coating on the outer surface of the aqueous resin mixed with TEMPO oxidized cellulose nanofibers on the back surface of the artificial leather, and the coating was naturally dried, resulting in the configuration of embodiment 4.

[0122] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 13. EXAMPLES

[0123] The artificial leather used had a woven fabric inside, and the thermoplastic elastomer used was an aqueous urethane emulsion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910]. The nanocellulose used was mechanically defibrated cellulose nanofiber [manufactured by Masuko Sangyo Co., Ltd.; product name "Fibrima" (registered trademark) hardwood pulp defibrated] and bacterial cellulose [Kusano Sakuko Co., Ltd.; product name "Five Nano" (registered trademark) HP-NFBC]. The additive used was an aqueous pigment [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "New Lactimin Color" Blue].

[0124] The mixing method was to mix 100 parts by mass of aqueous urethane emulsion, 60 parts by mass of mechanically defibrated cellulose nanofiber, and 60 parts by mass of bacterial cellulose in a glass petri dish with cupra underneath and a resin painting knife. A small amount of aqueous pigment was added to the aqueous urethane emulsion, and the mixture was mixed in a glass petri dish with a resin painting knife.

[0125] The coating method was to apply the aqueous urethane emulsion mixed with the two types of nanocellulose to the front and back of the artificial leather by silk screen method. Then, after drying the front surface, the aqueous urethane emulsion with added aqueous pigment was applied to the outer surface of the aqueous urethane mixed with the two types of nanocellulose on the back side of the artificial leather by silk screen method. Drying was done by natural drying, and the configuration of embodiment 4 was adopted.

[0126] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Example 14. EXAMPLES

[0127] The artificial leather used had a woven fabric inside, and the thermoplastic elastomer used was an aqueous urethane emulsion [manufactured by Dainichi Seika Color & Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910]. The nanocellulose used was TEMPO-oxidized cellulose nanofiber [manufactured by Nippon Paper Industries Co., Ltd.; product name "Cellenpia" TC-01A3%]. The additives used were an aqueous pigment [manufactured by Dainichi Seika Color & Chemicals Mfg. Co., Ltd.; product name "New Lactimin Color" Blue] and vetiver distilled water.

[0128] The mixing method was to mix 100 parts by mass of aqueous urethane emulsion, 40 parts by mass of TEMPO oxidized cellulose nanofiber, and a small amount of aqueous pigment with cupra underneath using a glass petri dish and a resin painting knife.Also, 100 parts by mass of aqueous urethane emulsion, 40 parts by mass of TEMPO oxidized cellulose nanofiber, and a small amount of vetiver distilled water with cupra underneath using a glass petri dish and a resin painting knife.

[0129] The application method was as follows: first, masking tape was applied to the surface of the artificial leather so that the width was 1 cm, and then an aqueous urethane emulsion containing TEMPO oxidized cellulose nanofiber and aqueous pigment was applied to the surface by silk screen printing to a width of 1 cm. After the surface was dried, an aqueous urethane emulsion containing TEMPO oxidized cellulose nanofiber and vetiver distilled water was applied to the back side of the artificial leather by silk screen printing. Furthermore, the aqueous urethane emulsion was applied to the outer surface of the aqueous urethane containing TEMPO oxidized cellulose nanofiber and vetiver distilled water on the back side of the artificial leather by silk screen printing. The drying was natural, resulting in the configuration of embodiment 4.

[0130] After sufficient drying, a test piece for evaluation was prepared so that the 1 cm wide portion of the aqueous urethane mixed with TEMPO oxidized cellulose nanofiber and aqueous pigment on the surface side of the artificial leather was positioned approximately in the center of the test piece, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the table below as Example 15.

[0131] Comparative Example 1 An artificial leather without any woven fabric inside [manufactured by Toray Industries, Inc.; product name "Ecsaine" (registered trademark), formerly orange] was prepared as a test piece for evaluation, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Comparative Example 1.

[0132] Comparative Example 2 The materials and manufacturing method were the same as those in Example 10, except that the artificial leather used in Comparative Example 1 was used.

[0133] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Comparative Example 2.

[0134] Comparative Example 3 An artificial leather with a woven fabric inside [manufactured by Toray Industries, Inc.; product name "ultrasuede" (registered trademark) LX CB1] was prepared as a test piece for evaluation, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Comparative Example 3.

[0135] Comparative Example 4 An artificial leather with a woven fabric inside was used, and the thermoplastic elastomer was an aqueous urethane emulsion [manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd.; product name "Seikaprene" UD-910]. No nanocellulose was mixed in, and one layer was applied to the front side of the artificial leather and two layers were applied to the back side. The application method was the same as in Example 10.

[0136] After sufficient drying, a test piece for evaluation was prepared, and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the following table as Comparative Example 4.

[0137] [Reference example] For reference, a 1 mm thick natural rubber specimen was prepared as it was and the storage modulus (E') and loss tangent (Tan δ) were measured using a dynamic viscoelasticity measuring device. The values ​​are shown in the table below as a reference example.

[0138] [Table 1]

[0139] From the measured values ​​in Table 1, first comparing the artificial leather with and without woven fabric inside, an improvement in Tan δ was observed in the longitudinal direction of the artificial leather for all of the examples, demonstrating the effect of improving vibration damping properties of the present invention.

[0140] In addition, compared to artificial leather with woven fabric inside, all examples showed improved Tan δ values, except for Example 3, which was about the same. Since Example 3 showed improved storage modulus, it is believed that there is hope for membrane vibration elements in the planar direction. Note that the measurement in the lateral direction of Comparative Example 3 was unstable, so no values ​​are listed.

[0141] Furthermore, when looking at the storage modulus, compared to artificial leather alone with a woven fabric inside, the combination of thermoplastic elastomer and nanocellulose makes it possible to make the modulus higher or lower, just like springs connected in series and in parallel.

[0142] In addition, while the natural rubber of the reference example has similar storage modulus and Tan δ in the longitudinal and transverse directions, by using artificial leather with woven fabric inside as the base fabric, it is possible to differentiate between the storage modulus and Tan δ in the longitudinal and transverse directions, making it possible to design the material to suit the characteristics of the body being damped. [Industrial Applicability]

[0143] From the above, the damping material of the present invention can change the storage modulus (in other words, elastic force) and Tan δ (in other words, loss factor) between the vertical and horizontal directions, and can be used not only for stationary damped objects, but also for objects that move in a fixed direction or freely. For example, as with sports equipment, the vibration characteristics and movement characteristics of vertical movement and front-back or horizontal directions differ depending on the movement of the body, and by using the damping material of the present invention according to these characteristics, it is possible to ensure movement stability without impeding the vibration suppression and movement of the body.

[0144] Furthermore, not only in sporting goods, but also in moving indoor spaces such as cars, trains, ships, and aircraft, it is necessary to suppress vibrations specific to the location while not creating resistance to movement in the direction of travel, and by using the vibration-damping material of the present invention, it is possible to precisely control the directionality. [Explanation of symbols]

[0145] 11, 12, 13, 14 Damping material A Artificial leather a textile BC1, BC2 Thermoplastic elastomers mixed with nanocellulose B1, B2 Thermoplastic elastomer C1, C2 Nanocellulose D Thermoplastic elastomer

Claims

1. A vibration-damping material (11) comprising artificial leather (A) having a woven fabric (a) therein, a thermoplastic elastomer (B1) applied to one surface of the artificial leather (A) and nanocellulose (C1) mixed with the thermoplastic elastomer (B1).

2. A vibration-damping material (12) comprising artificial leather (A) having a woven fabric (a) therein, a thermoplastic elastomer (B1) applied to one surface of the artificial leather (A), nanocellulose (C1) mixed with the thermoplastic elastomer (B1), and a thermoplastic elastomer (D) applied to the other surface of the artificial leather (A).

3. A vibration-damping material (13) comprising artificial leather (A) having a woven fabric (a) therein, thermoplastic elastomers (B1, B2) provided by application on one and the other surfaces of the artificial leather (A), and nanocellulose (C1, C2) mixed with both of the thermoplastic elastomers (B1, B2).

4. A vibration-damping material (14) comprising: artificial leather (A) having a woven fabric (a) therein; thermoplastic elastomers (B1, B2) applied to one and other surfaces of the artificial leather (A); nanocellulose (C1, C2) mixed with both of the thermoplastic elastomers (B1, B2); and a thermoplastic elastomer (D) applied to one or the other outer surface of the thermoplastic elastomers (B1, B2).

Citation Information

Patent Citations

  • Laminate

    JP2018108646A

  • Vibration-damping fiber-reinforced rubber composition and production method thereof

    JP2020019886A