Conductive composition

A conductive composition with a binder resin, amine compound, and polyisocyanate in specific ratios addresses issues of air bubbles, surface irregularities, and conductivity in screen-printed films, providing a stable and conductive cured film for electronic devices.

JP2024168074APending Publication Date: 2024-12-05NOF CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084471
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing conductive compositions used in screen printing for electronic devices suffer from issues such as air bubble formation, surface irregularities, bleeding at edges, and reduced conductivity due to poor thixotropy, especially when using acrylic resins as binders.

Method used

A conductive composition comprising a binder resin, a specific amine compound with an ethylenediamine skeleton, conductive particles, and polyisocyanate in predetermined ratios, which improves thixotropy and reduces surface irregularities and bleeding while maintaining high conductivity.

Benefits of technology

The composition forms a cured film with minimal air bubbles, small surface irregularities, and reduced edge bleeding, ensuring excellent electrical conductivity and adhesion to the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168074000001
    Figure 2024168074000001
  • Figure 2024168074000002
    Figure 2024168074000002
  • Figure 2024168074000003
    Figure 2024168074000003
Patent Text Reader

Abstract

To provide a conductive composition capable of forming a cured film in which air bubbles are scarcely produced in a printed film before curing formed by, for example, screen printing, irregularity of a cured film surface is small, blur at an end part thereof is scarcely generated, and which has excellent conductivity.SOLUTION: A conductive composition comprises (A) 1-30 mass% binder resin, (B) 0.1-5 mass% amine compound having an ethylene diamine skeleton, (C) 50-98 mass% conductive particles, and (D) 0.5-15 mass% polyisocyanate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrically conductive composition, and in particular to an electrically conductive composition that is applied to screen printing. [Background technology]

[0002] In recent years, a method of forming wiring for electronic devices by screen printing a conductive composition on an electronic substrate and then curing it has attracted attention. This method has the advantage that wiring can be formed directly on the housing, etc., allowing for a reduction in the number of parts and a reduction in size and weight.

[0003] Conductive compositions generally contain metal particles such as silver or copper, or carbon conductive powder such as carbon black as the main component, and also contain binder resins and dispersants. As binders used in conductive compositions, polyester resins, polyurethane resins, epoxy resins, phenolic resins, acrylic resins, etc. are often used, and among them, acrylic resins can be given various functions such as impact resistance, thermoplasticity, and photoreactivity depending on the type of monomer to be copolymerized. For example, oxidized metal particles with poor dispersibility can be improved in dispersibility by copolymerizing a monomer having a hydrophilic functional group, and it is also possible to reduce the amount of dispersant that reduces the durability of the conductive composition.

[0004] On the other hand, when an acrylic resin is used as a binder for screen printing, there is a problem that, due to poor stringiness and flowability, air is entrained during screen printing, causing many air bubbles to exist in the printed film before curing after printing, and the surface of the cured film has a significantly large and numerous unevenness. One method for suppressing this is to add a large amount of diluent, but when this method is implemented, there is a problem that the thixotropy (hereinafter also referred to as thixotropy) deteriorates, causing bleeding at the edge of the cured film after printing, and the filling rate of the conductive particles decreases, causing the conductivity to deteriorate.

[0005] For example, Patent Document 1 discloses a method for suppressing bleeding at the ends of a conductor pattern formed by screen printing. The conductive composition disclosed in Patent Document 1 has excellent thixotropy due to the inclusion of a metal oxide, and a wiring pattern without bleeding can be obtained without impairing conductivity. However, there is a risk that the metal oxide may cause air bubble marks on the surface of the cured film of the conductive composition, increasing the possibility of increasing the surface unevenness.

[0006] Furthermore, Patent Document 2 describes a conductive composition for printing that is composed of a binder resin having an isocyanate structure, a conductive material, and a solvent that dissolves the binder resin. This conductive composition has a carboxylate metal salt moiety in the binder resin, and is capable of forming a highly conductive print pattern with low energy. However, if the conductive composition has poor thixotropy and the amount of solvent is large, bleeding at the edge of the print pattern and deterioration of the conductivity may occur, and if the amount of solvent is small, the surface unevenness of the cured film may become large. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Unexamined Patent Publication No. 7-6623 [Patent Document 2] International Publication No. 2017 / 163615 Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved by the present invention is to provide a conductive composition capable of forming a cured film which is unlikely to generate air bubbles in a printed film before curing formed by, for example, screen printing, has small irregularities on the surface of the cured film, is unlikely to bleed at the edges, and has good electrical conductivity. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by a conductive composition containing a binder resin, conductive particles, a specific amine compound, and a polyisocyanate in a specific ratio, and have completed the present invention. That is, the present invention relates to the following [1] to [3].

[0010] [1] (A) 1 to 30 mass% of a binder resin, (B) 0.1 to 5 mass% of an amine compound having an ethylenediamine skeleton, (C) Conductive particles 50-98% by mass, (D) 0.5 to 15 mass% polyisocyanate, 1. A conductive composition comprising:

[0011] [2] The conductive composition according to [1] above, wherein the (B) amine compound having an ethylenediamine skeleton is at least one selected from an amine represented by the following formula (1), an amine represented by the following formula (2), and a polyethyleneimine having a molecular weight of 100 to 10,000.

[0012] [ka]

[0013] (In formula (1), the degree of polymerization n is 1 to 5.)

[0014] [ka]

[0015] (In formula (2), R 1 is a hydrocarbon group having 1 to 3 carbon atoms, and R 2 is a hydrocarbon group having 1 to 5 carbon atoms.

[0016] [3] The conductive composition according to the above [1] or [2], wherein the binder resin (A) is a polymer composed of 20 to 100 mol % of a structural unit derived from a monomer (a1) represented by the following formula (3) and 0 to 80 mol % of a structural unit derived from a monomer (a2) copolymerizable with the monomer (a1):

[0017] [ka]

[0018] (In formula (3), R 3 is a single bond, an amide group or an ester group, R 4 is a hydrogen atom or a methyl group. Effect of the Invention

[0019] According to the present invention, it is possible to provide a conductive composition which is capable of forming a cured film having good electrical conductivity, in which air bubbles are unlikely to form in the printed film before curing formed by, for example, screen printing, the surface of the cured film has small irregularities, and bleeding is unlikely to occur at the edges. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto. In this specification, a numerical range defined using the symbol "to" includes both ends (upper and lower limits) of the symbol "to". For example, "2 to 5" means 2 or more and 5 or less. Furthermore, when a concentration or amount is specified, any higher concentration or amount can be associated with any lower concentration or amount. For example, when "2 to 10% by mass" and "preferably 4 to 8% by mass" are described, the descriptions "2 to 4% by mass", "2 to 8% by mass", "4 to 10% by mass", and "8 to 10% by mass" are also included.

[0021] The conductive composition according to the embodiment of the present invention contains (A) 1 to 30 mass% of binder resin, (B) an amine compound having an ethylenediamine skeleton, (C) 50 to 98 mass% of conductive particles, and (D) 0.5 to 15 mass% of polyisocyanate. Here, the content of components (A) to (D) is based on the content excluding a solvent component such as a solvent, if the conductive composition contains such a solvent. Therefore, if a solvent component is contained in components (A) to (D), the content is based on the content excluding such a solvent. The same applies to other components other than components (A) to (D) described later, except for the solvent. Each component will be described below.

[0022] [Component (A): Binder resin] The component (A) used in the embodiment of the present invention is a binder resin, and for example, a known binder resin used in circuit formation can be adopted. Examples of such binder resins include acrylic resins, polyester resins, polyurethane resins, epoxy resins, and phenolic resins. Among these, a polymer composed of a monomer having an ethylenic double bond is preferred. The polymer composed of a monomer having an ethylenic double bond is not particularly limited, but a vinyl polymer having a phenolic hydroxyl group as a side chain is preferred. Examples of such vinyl polymers include a polymer containing a monomer (a1) represented by the following formula (3) or a monomer (a1) and a monomer (a2) copolymerizable with the monomer (a1). Among these, a polymer (hereinafter referred to as polymer (A)) composed of 20 to 100 mol % of a constituent unit derived from the monomer (a1) and 0 to 80 mol % of a constituent unit derived from the monomer (a2) copolymerizable with the monomer (a1) is preferred.

[0023] [ka]

[0024] (In formula (3), R 3 is a single bond, an amide group or an ester group, R 4 is a hydrogen atom or a methyl group.

[0025] The monomer (a1) is not particularly limited as long as it is a compound represented by formula (3). 3 R may be any of the above groups, but from the viewpoint of electrical conductivity, an ester group is preferred. 4 may be any of the above, but is preferably a methyl group from the viewpoint of hydrolysis resistance. Specific examples of the monomer (a1) include 4-hydroxyphenyl methacrylate, 4-hydroxystyrene, N-(4-hydroxyphenyl) methacrylamide, 4-hydroxyphenyl acrylate, etc. The compound represented by formula (3) may be used alone or in combination of two or more.

[0026] The polymer (A) may be a polymer composed of only the monomer (a1), or may be a copolymer of the monomer (a1) and a monomer (a2) copolymerizable therewith. By forming a copolymer with the monomer (a2), it is possible to impart properties based on the monomer (a2). The monomer (a2) is not particularly limited as long as it is a vinyl monomer copolymerizable with the monomer (a1), and examples thereof include known substances such as anionic and cationic ionic monomers, nonionic monomers, (meth)acrylic acid ester compounds (excluding those contained in the monomer (a1)), aromatic alkenyl compounds such as styrene, vinyl cyanide compounds, acrylamide compounds, vinyl esters, vinyl ethers, maleates, fumarates, and α-olefins. From the viewpoint of electrical conductivity, methacrylic acid ester compounds are preferred, and those having a primary hydroxyl group are preferred. Specific examples of the methacrylic acid ester compound include methyl methacrylate, hydroxyethyl methacrylate, polyethylene glycol monomethacrylate, polypropylene glycol monomethacrylate, and polyethylene glycol-tetramethylene glycol monomethacrylate. The monomer (a2) may be used alone or in combination of two or more. From the viewpoint of electrical conductivity, it is preferable to use at least one monomer having a primary hydroxyl group. In addition, the structure of the monomer (a2) having a primary hydroxyl group is not particularly limited, but from the viewpoint of electrical conductivity during screen printing, the linker part between the (meth)acrylic acid moiety and the hydroxyl group moiety preferably has 1 to 6 carbon atoms in the case of an alkylene skeleton, and preferably has 1 to 10 repeating units in the case of an alkylene oxide skeleton. Specifically, an ester of (meth)acrylic acid and a polyhydric alcohol having two or more hydroxyl groups including at least one primary hydroxyl group is preferred, and as the polyhydric alcohol, one having an alkylene skeleton or one having an alkylene oxide skeleton is more preferred, and when the polyhydric alcohol has an alkylene skeleton, it is further preferred that the skeleton has 1 to 6 carbon atoms, and when the polyhydric alcohol has an alkylene oxide skeleton, it is further preferred that the skeleton has 1 to 10 repeating units.

[0027] The molar percentages of the constituent units derived from the monomer (a1) and the monomer (a2) in the polymer (A) are preferably in the above-mentioned ratios. That is, the constituent units derived from the monomer (a1) in the polymer (A) are 20 to 100 mol %, and the constituent units derived from the monomer (a2) are 0 to 80 mol %. The ratio of the constituent units derived from the monomers contained in the polymer (A) can be measured by GC / MS analysis. It can also be calculated from the blending ratio of the monomers during synthesis. The preferred molar ratios of each constituent unit are 30 to 100 mol % of the monomer (a1) and 0 to 70 mol % of the monomer (a2). When the monomer (a2) is contained, the more preferred molar ratios of each monomer are 30 to 80 mol % of the monomer (a1) and 20 to 70 mol % of the monomer (a2). If the molar ratio of the component (a2) is more than 80%, the dispersibility of the conductive particles decreases, and it may be difficult to obtain a cured film exhibiting excellent conductivity.

[0028] The polymer (A) may contain structural units derived from monomers other than the monomers (a1) and (a2). In this case, the content is preferably such that the physical properties are not impaired, and is preferably, for example, 0 to 40 mol % of the entire polymer (A).

[0029] The weight average molecular weight of the polymer (A) is not particularly limited, but from the viewpoints of the strength and viscosity of the polymer (A), the solvent solubility and printability, it is preferably 1,000 to 1,000,000, more preferably 2,000 to 800,000, and even more preferably 3,000 to 300,000. The weight average molecular weight can be determined in terms of polystyrene using gel permeation chromatography (GPC).

[0030] When the polymer (A) is a copolymer, the copolymer may have a random or block structure, but is preferably a random copolymer.

[0031] The polymer (A) can be obtained, for example, by preparing a monomer solution containing the monomer (a1) or the monomer (a1) and the monomer (a2) and radically polymerizing each monomer. The polymerization can be performed by a known method. For example, solution polymerization, suspension polymerization, emulsion polymerization, etc. can be mentioned, but solution polymerization and suspension polymerization are preferred in terms of being easy to adjust the weight average molecular weight of the polymer (A) within a desired range. In the solution polymerization and suspension polymerization, for example, the above-mentioned monomer (a1) or the monomer (a1) and the monomer (a2) can be obtained by polymerizing the monomer (a1) in a polymerization solvent in the presence of a polymerization initiator under predetermined conditions.

[0032] The polymerization initiator usable in the above-mentioned radical polymerization can be a known one. For example, organic peroxides such as t-butyl peroxy neodecanoate, di(4-t-butylcyclohexyl) peroxy dicarbonate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, and t-butyl peroxide carbonate, and azo-based polymerization initiators such as 2,2'-azobisisobutyronitrile can be mentioned. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used can be appropriately set according to the combination of monomers used, reaction conditions, and the like. When the polymerization initiator is added, for example, the entire amount may be charged at once, a part of it may be charged at once and the rest may be dripped, or the entire amount may be dripped. In addition, it is preferable to drip the polymerization initiator together with the monomer, since it is easy to control the reaction, and it is also preferable to add the polymerization initiator after the monomer is dripped, since it is possible to reduce the remaining monomer.

[0033] In addition, in the radical polymerization, a chain transfer agent can be used as necessary. Known chain transfer agents can be used, and examples of such agents include mercaptans such as n-dodecyl mercaptan, lauryl mercaptan, thioglycolic acid, and octyl thioglycolate; mercaptocarboxylic acids and their esters such as mercaptoacetic acid and mercaptopropynic acid; mercaptoethanol; halogenated compounds; dimeric alpha-methylstyrene; and the like.

[0034] As the polymerization solvent usable in the solution polymerization, one capable of dissolving the monomer and the polymerization initiator can be used, and specific examples thereof include methanol, ethanol, 1-propanol, acetone, methyl ethyl ketone, propylene glycol monomethyl ether, etc. The concentration of all monomers (total amount) relative to the polymerization solvent is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, from the viewpoints of adjusting the weight average molecular weight of the polymer (A) and controlling heat generation during the polymerization reaction.

[0035] The method of feeding the monomers into the reaction vessel when reacting the monomers by solution polymerization is not particularly limited, and for example, the entire amount may be charged at once, a part of the monomers may be charged at once and the rest may be added dropwise, or the entire amount may be added dropwise. From the viewpoint of ease of controlling heat generation, it is preferable to charge a part of the monomers at once and the rest may be added dropwise, or to add the entire amount dropwise.

[0036] The polymerization temperature can be appropriately set depending on the type of polymerization solvent, etc., and is, for example, 50° C. to 110° C. The polymerization time can be appropriately set depending on the type of polymerization initiator and the polymerization temperature. For example, when t-butyl peroxy neodecanoate is used as the polymerization initiator, the polymerization temperature is set to 70° C. to 80° C., and the polymerization time is suitably about 4 to 9 hours.

[0037] The content of component (A) is 1 to 30% by mass, preferably 2 to 20% by mass. If the content of component (A) is less than 1% by mass, it may be difficult to provide sufficient fluidity when printing using the conductive composition. If the content of component (A) is more than 30% by mass, it may be difficult for the conductive particles of component (C) in the conductive composition to come into contact with each other, and a cured film exhibiting excellent conductivity may not be obtained.

[0038] [Component (B): Amine compound] The component (B) used in the embodiment of the present invention is an amine compound having an ethylenediamine skeleton. Among the amine compounds having an ethylenediamine skeleton, at least one selected from an amine having a linear ethylenediamine skeleton represented by the following formula (1), an amine having a cyclic ethylenediamine skeleton represented by the following formula (2), and a polyethyleneimine having a molecular weight of 100 to 10,000 is more preferable.

[0039] [ka]

[0040] (In formula (1), the degree of polymerization n is 1 to 5.)

[0041] [ka]

[0042] (In formula (2), R 1 is a hydrocarbon group having 1 to 3 carbon atoms, and R 2 is a hydrocarbon group having 1 to 5 carbon atoms.

[0043] The amine having a linear ethylenediamine skeleton represented by formula (1) is not particularly limited as long as the degree of polymerization n is 1 to 5, but those in which n is 1 to 3 are preferred from the viewpoint of electrical conductivity.

[0044] Diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and hexaethyleneheptamine.

[0045] The amine having a cyclic ethylenediamine skeleton represented by formula (2) is not particularly limited as long as it is represented by formula (2), and R 1 is a hydrocarbon group having 1 to 3 carbon atoms, R 2 From the viewpoints of achieving better electrical conductivity and better suppression of bleeding at the edges of the cured film, R 1is a hydrocarbon group having 1 to 2 carbon atoms, R 2 R is more preferably a hydrocarbon group having 1 to 2 carbon atoms. 1 The hydrocarbon group constituting R is preferably a divalent saturated aliphatic hydrocarbon group, and when it has 3 carbon atoms, the structure may be linear or branched, but linear is preferred. 2 The hydrocarbon group constituting the formula (I) is also preferably a divalent saturated aliphatic hydrocarbon group, and when it has 3 to 5 carbon atoms, the structure may be either linear or branched, but linear is preferred.

[0046] Specific examples of the amine represented by formula (2) include 2-aminoethylimidazolidine, aminomethylpiperazine, 2-aminoethylpiperazine, 3-aminopropylpiperazine, 4-aminobutylpiperazine, 5-aminopentylpiperazine, and 2-aminoethylhomopiperazine.

[0047] Polyethyleneimine is a polymer having -(CH2-CH2-NH)- as a repeating unit, and is an amine compound having an ethylenediamine skeleton. The structure of polyethyleneimine may be linear or branched, but from the viewpoint of better electrical conductivity and small unevenness of the cured film surface, those having branches containing primary, secondary, and tertiary amines are preferred. The weight-average molecular weight of polyethyleneimine is preferably 100 to 10,000. Among these, those having a weight-average molecular weight of 100 to 1,000 tend to be suitable from the viewpoint of small unevenness of the cured film surface. From the viewpoint of electrical conductivity, those having a weight-average molecular weight of 100 to 5,000 tend to be suitable.

[0048] Polyethyleneimine may be synthesized according to a standard method, or commercially available polyethyleneimine may be used. Examples of commercially available polyethyleneimine having a branched structure include Epomin (registered trademark) SP-003, SP-006, and SP-012 manufactured by Nippon Shokubai Co., Ltd.

[0049] Component (B) may be used alone or in combination of two or more kinds, but by combining amines with different properties, excellent conductivity and thixotropy can be imparted. When two or more kinds of component (B) are combined, for example, two or more kinds selected from the amine represented by the above formula (1), the amine represented by formula (2), and polyethyleneimine are preferred. For example, it is preferred to use a combination of the amine represented by formula (1) and / or formula (2) with polyethyleneimine, and the mixing ratio is preferably 50 to 80 mass% of the amine represented by formula (1) and / or formula (2) and 20 to 50 mass% of the polyethyleneimine. Specifically, the amine represented by formula (1) having a degree of polymerization n of 1 to 2 and / or R which is a hydrocarbon group having 1 to 2 carbon atoms are preferably used. 1 and R 2 and the like. An example is a combination of an amine represented by formula (2) with a polyethyleneimine having a weight average molecular weight of 100 to 1,000 and a branched structure. In particular, a combination of diethylenetriamine and / or 2-aminoethylpiperazine with a polyethyleneimine having a weight average molecular weight of 300 and a branched structure (for example, Epomin SP-003, manufactured by Nippon Shokubai Co., Ltd.) is preferred.

[0050] The content of component (B) is 0.1 to 5 mass%, and preferably 0.5 to 3 mass%. If the content of component (B) is less than 0.1 mass% or more than 5 mass%, the volume resistivity of the cured film obtained using the conductive composition may increase.

[0051] [Component (C): Conductive particles] The component (C) used in the embodiment of the present invention is a conductive particle, and inorganic conductive particles such as silver, nickel, gold, and copper can be used. From the viewpoint of conductivity, silver and copper are preferable, and from the viewpoint of migration resistance and use in a high applied voltage region such as driving a device, copper is preferable. The copper particles may be composed of only copper, but may further contain metals other than copper such as silver and platinum, metal oxides, and metal sulfides. When the copper particles further contain metals other than copper, metal oxides, and metal sulfides, the mass ratio of copper in the copper particles is preferably 50 mass% or more. In addition, the copper particles may have a shape in which a surface layer or protrusions are formed.

[0052] Although commercially available conductive particles may be used as they are, it is preferable to use surface-coated conductive particles whose surfaces are coated for the purpose of improving oxidation resistance, etc. Among them, it is preferable to use surface-coated conductive particles whose surfaces are coated with an amine compound, and it is more preferable to use surface-coated conductive particles whose surfaces are coated with an amine compound represented by the following formula (4).

[0053] [ka]

[0054] (In formula (4), m is an integer of 0 to 3, n is an integer of 0 to 2, and when n=0, m is any of 0 to 3, and when n=1 or n=2, m is any of 1 to 3.)

[0055] From the viewpoint of obtaining better oxidation resistance, it is preferable that the surface-coated conductive particles whose surfaces are coated with the amine compound or the like represented by the above formula (4) are further coated with an aliphatic monocarboxylic acid to obtain surface-coated conductive particles. As a result, the conductive particle surface is coated with a first coating layer formed with the amine compound and a second coating layer formed with the aliphatic monocarboxylic acid. Preferably, the first coating layer is formed on the conductive particle surface, and the second coating layer is formed on the first coating layer.

[0056] The aliphatic monocarboxylic acid forming the second coating layer is preferably an aliphatic monocarboxylic acid having a carbon number of 8 to 24. Examples of the aliphatic monocarboxylic acid include linear saturated aliphatic monocarboxylic acids, linear unsaturated aliphatic monocarboxylic acids, branched saturated aliphatic monocarboxylic acids, and branched unsaturated aliphatic monocarboxylic acids.

[0057] Examples of linear saturated aliphatic monocarboxylic acids having 8 to 24 carbon atoms include caprylic acid, pelargonic acid, capric acid, undecylic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, nonadecylic acid, and arachidic acid. Examples of linear unsaturated aliphatic monocarboxylic acids having 8 to 24 carbon atoms include myristoleic acid, palmitoleic acid, petroselinic acid, and oleic acid. Examples of branched saturated aliphatic monocarboxylic acids having 8 to 24 carbon atoms include 2-ethylhexanoic acid. As the aliphatic monocarboxylic acids, one selected from the above compounds may be used alone, or two or more may be used in combination.

[0058] The method for producing the surface-coated conductive particles is not particularly limited. For example, the method for obtaining the surface-coated conductive particles whose surface is coated with an amine compound includes washing the conductive particles with an ammonium chloride aqueous solution or the like, adding the washed conductive particles to a solution of an amine compound, and heating as necessary, or adding the conductive particles to a solution containing, for example, ammonium chloride and an amine compound, and heating as necessary.

[0059] As a method for producing the surface-coated conductive particles coated with a first coating layer formed by an amine compound and a second coating layer formed by an aliphatic monocarboxylic acid, for example, a method of adding the surface-coated conductive particles coated with an amine compound to a solution of an aliphatic monocarboxylic acid can be mentioned. After adding to the solution of the aliphatic monocarboxylic acid, heating may be performed as necessary.

[0060] The average particle size (D50) of the conductive particles is not particularly limited, but in order to enable the conductive composition containing the conductive particles as component (C) to be printed well by various printing methods such as dispenser printing and screen printing, it is preferable to control the average particle size (D50) of the conductive particles. Specifically, the average particle size (D50) of the conductive particles is preferably 5 nm to 20 μm, and more preferably 10 nm to 10 μm. The average particle size (D50) of the conductive particles can be measured by a laser diffraction / scattering type particle size distribution measuring device (for example, Microtrack MT3000II manufactured by Microtrack Bell Co., Ltd.).

[0061] The BET specific surface area of ​​the conductive particles is 0.05 to 400 m 2 / g, and 0.1 to 200m 2 / g It is more preferable that the BET specific surface area of ​​the conductive particles can be measured by a BET single point method using a specific surface area measuring device (for example, Monosorb, manufactured by Yuasa Ionics Co., Ltd.).

[0062] There are no particular limitations on the shape or aspect ratio (ratio of the long axis to the short axis) of the conductive particles, and various shapes such as spherical, polyhedral, flat, plate, flake, thin plate, rod, dendritic, fibrous, etc. The conductive particles may be used alone or in combination of two or more types selected from those differing in components, average particle size, shape, aspect ratio, etc.

[0063] The content of component (C) is 50 to 98% by mass. The lower limit of the content of component (C) is preferably 70% by mass, and more preferably 80% by mass. If the content of component (C) is less than 50% by mass, contact between conductive particles during curing becomes difficult, and a cured film exhibiting excellent conductivity may not be obtained. In addition, the upper limit of the content of component (C) is preferably 93% by mass from the viewpoint of fluidity.

[0064] [Component (D): Polyisocyanate] The component (D) used in the embodiment of the present invention is a polyisocyanate. Examples of polyisocyanates include aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, and their adducts, biurets, and isocyanurates. From the viewpoint of electrical conductivity, aliphatic diisocyanates, and their adducts, biurets, and isocyanurates are preferred. From the viewpoint of adhesion, isocyanurates of aliphatic diisocyanates are more preferred.

[0065] The polyisocyanate may be blocked with a blocking agent. Blocking extends the usable time and also works favorably on print stability. Any blocking agent may be used as long as it contains active hydrogen (hydrogen bonded to oxygen, sulfur, or nitrogen) that reacts with isocyanate and the product is reversible, i.e., the blocking agent is deblocked by heat. Representative blocking agents include oximes, lactams, phenols, active methylenes, pyrazoles, mercaptans, imidazoles, amines, imines, triazoles, hydroxylamines, and aliphatic, alicyclic, or aromatic alkyl monoalcohols. Among them, pyrazoles have a relatively low dissociation temperature and work favorably on plastic substrates such as polyethylene terephthalate (PET) that cannot be heated to high temperatures. Examples of pyrazoles include 2,2-dimethylpyrazole and 3,5-dimethylpyrazole. An example of a commercially available polyisocyanate having three isocyanate groups composed of an isocyanurate skeleton and a skeleton derived from hexamethylene diisocyanate and blocked with 3,5-dimethylpyrazole is Duranate SBN-70D manufactured by Asahi Kasei Corporation, but is not limited thereto.

[0066] The above polyisocyanates may be used alone or in combination of two or more. The content of component (D) is 0.5 to 15 mass %, preferably 1 to 10 mass %, and more preferably 1.5 to 7 mass %.

[0067] [Other ingredients] In addition to the above components (A) to (D), the conductive composition according to the embodiment may contain various additives such as solvents, antioxidants, lubricants, dispersants, curing agents, curing accelerators, viscosity modifiers, foaming agents, and antifoaming agents, as necessary, within the range that does not impair the effects of the present invention. The conductive composition may also contain impurities that may be inevitably mixed in from raw material components and equipment in the manufacturing process. When any of these components is contained, the content thereof may be more than 0 mass% and 50 mass% or less, and is preferably 30 mass% or less. The content of the solvent will be described later.

[0068] (solvent) The conductive composition according to the embodiment may contain a solvent for the purpose of improving the coatability and adjusting the viscosity. Examples of the solvent include ether alcohols such as ethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol monoethyl ether acetate, propylene glycol diacetate, dipropylene glycol monomethyl ether, ethylene glycol monobutyl ether acetate, triethylene glycol monomethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol, and dipropylene glycol; non-ether alcohols such as propylene glycol and 1,4-butanediol; esters such as cyclohexanol acetate, methyl methoxypropionate, ethyl ethoxypropionate, and 1,6-hexanediol acetate; ketones such as isophorone and cyclohexanone; terpenes such as terpineol, dihydroterpineol, dihydroterpinyl acetate, and isobornylcyclohexanol; and other hydrocarbons such as octane, decane, dodecane, tetradecane, hexadecane, and propylene carbonate, but are not limited thereto. The solvent may be used alone or in combination of two or more. When two or more types are used in combination, the mixing ratio is not particularly limited.

[0069] The type of solvent is preferably one or more selected from the above ether alcohols, esters, and terpenes. When two or more of these solvents are mixed, the mixing ratio is not particularly limited.

[0070] When the conductive composition according to the embodiment contains a solvent, the content of the solvent is preferably 1 to 30 mass %, more preferably 1 to 20 mass %, based on the total amount of the conductive composition. When the components (A) to (D) and other components contain a solvent, the content is determined taking this into consideration.

[0071] (Antioxidants) The conductive composition according to the embodiment may contain an antioxidant for the purpose of maintaining the performance of each component during storage. The type of antioxidant is not particularly limited, and various antioxidants can be used depending on the application. For example, nitrogen-containing heterocyclic compounds such as 2,2-bipyridyl and 1,10-phenanthroline; Schiff bases such as N,N'-bis(salicylidene)ethylenediamine, N,N'-bis(salicylidene)-1,2-propanediamine, N,N'-bis(salicylidene)-1,3-propanediamine, and N,N'-bis(salicylidene)-1,2-phenylenediamine; 1,2-phenylenediamine, 1,3-phenylenediamine, 1,4-phenylenediamine, 2,5-dimethyl-1,4-phenylenediamine, 2,3,5,6-tetramethyl-1,4-phenylenediamine, and N,N-dimethyl-1,4-phenylenediamine. Examples of the antioxidant include, but are not limited to, aromatic diamines such as amine, N,N,N'N'-tetramethyl-1,4-phenylenediamine, and N,N'-diphenyl-1,4-phenylenediamine; phenols such as p-methoxyphenol, hydroquinone, tert-butylhydroquinone, dibutylhydroxytoluene, catechol, 4-tert-butylcatechol, pyrogallol, eugenol, and propyl gallate; and ascorbic acids such as L-ascorbic acid, 6-O-palmitoyl-L-ascorbic acid, 6-O-stearoyl-L-ascorbic acid, and tetra-2-hexyldecanoic acid ascorbyl. The antioxidant may be used alone or in combination of two or more. When two or more types are used in combination, the mixing ratio is not particularly limited.

[0072] Among the specific examples of the antioxidants mentioned above, it is preferable to use one or more selected from 2,2-bipyridyl, N,N'-bis(salicylidene)ethylenediamine, N,N'-bis(salicylidene)-1,2-propanediamine, 1,2-phenylenediamine, 1,3-phenylenediamine, 1,4-phenylenediamine, p-methoxyphenol, hydroquinone, tert-butylhydroquinone, 6-O-palmitoyl-L-ascorbic acid, and 6-O-stearoyl-L-ascorbic acid. When two or more of these antioxidants are mixed, the mixing ratio is not particularly limited.

[0073] When the conductive composition according to the embodiment contains an antioxidant, the content of the antioxidant is preferably 0.01 to 10 mass %, and more preferably 0.1 to 6 mass %.

[0074] (lubricant) A lubricant may be appropriately added to the conductive composition according to the embodiment for the purpose of adjusting the dispersibility of the conductive particles of the component (C). Examples of the types of lubricants include fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid; fatty acid metal salts formed from metals such as sodium, potassium, barium, magnesium, calcium, aluminum, iron, cobalt, manganese, zinc, and tin and the fatty acids; fatty acid amides such as stearic acid amide, oleic acid amide, behenic acid amide, palmitic acid amide, and lauric acid amide; fatty acid esters such as butyl stearate; waxes such as paraffin wax and liquid paraffin; alcohols such as ethylene glycol and stearyl alcohol; polyethers made of polyethylene glycol, polypropylene glycol, and modified products thereof; polysiloxanes such as silicone oil; and fluorine compounds such as fluorine-based oil. The lubricant may be used alone or in combination of two or more kinds. When two or more kinds are used, the mixing ratio is not particularly limited.

[0075] Among these lubricants, from the viewpoint of dispersibility, it is preferable to use one or more selected from fatty acids and fatty acid metal salts, and it is more preferable to use at least one selected from magnesium stearate and lauric acid.

[0076] When the conductive composition according to the embodiment contains a lubricant, the content of the lubricant is preferably 0.01% to 10% by mass, more preferably 0.1 to 5% by mass, and further preferably 0.2 to 3% by mass.

[0077] (Dispersant) The conductive composition according to the embodiment may appropriately contain a dispersant for the purpose of adjusting the dispersibility of the conductive particles of component (C). Examples of the dispersant include sarcosine compounds such as lauroyl sarcosine, myristoyl sarcosine, palmitoyl sarcosine, stearoyl sarcosine, and oleoyl sarcosine; polymeric amine compounds; and polymeric polycarboxylic acid compounds. Examples of the polymeric amine compounds include commercially available compounds, such as Filanol PA-075F, PA-085C, and PA-107P manufactured by NOF Corporation, and Esream (registered trademark) AD-3172M, AD-374M, and AD-508E. Examples of the polymeric polycarboxylic acid compounds include commercially available compounds, such as Marialim AKM-0531, AFB-1521, AAB-0851, AWS-0851, SC-0505K, SC-1015F, and SC-0708A manufactured by NOF Corporation. The dispersant may be used alone or in combination of two or more kinds. When two or more kinds are used, the mixing ratio is not particularly limited.

[0078] Among these dispersants, it is preferable to use one or more types selected from sarcosine compounds, and it is more preferable to use oleoyl sarcosine.

[0079] When the conductive composition according to the embodiment contains a dispersant, the content of the dispersant is preferably 0.01 to 10 mass %, more preferably 0.2 to 5 mass %, and further preferably 0.3 to 3 mass %.

[0080] The conductive composition can be obtained by mixing the above-mentioned components in a predetermined amount and kneading them according to a standard method. In addition, a desired pattern is printed on the surface of a substrate by screen printing or the like according to a standard method to prepare a printed film, and then a heat treatment or the like is performed to obtain a cured film. The conductive composition contains the above-mentioned components (A) to (D) in a predetermined ratio, and therefore has good thixotropy. Therefore, even if the binder resin is an acrylic resin, the printed film produced by screen printing in particular has a suitable fluidity during printing and can suppress the entrapment of air bubbles. Note that the finer the mesh used, the more likely air bubbles are to be entrapped, but there is no particular restriction on the mesh, and the effect of the present invention can be obtained even when printing with a high mesh screen having a mesh number of 300 or more. In addition, the conductive composition has good thixotropy, so there is no need to dilute it with a large amount of solvent (diluent), and there is no need to use powder of an inorganic composition as in the conventional technology. For example, it is possible to suppress the occurrence of bleeding at the edge of the printed film formed by screen printing, and the formation of air bubbles inside and on the surface of the printed film can be suppressed. In addition, the formation of bubbles is suppressed at the interface with the printed substrate, and thus the adhesion of the printed film and its cured film to the printed substrate can be improved. As a result, the resulting cured film also suppresses the occurrence of bubbles on the surface, unevenness caused by bubbles, and bleeding at the ends, and has few bubbles inside the film and on the surface (including the interface with the printed substrate), making it ideal as a wiring material for electronic devices. Therefore, the conductive composition described above is suitable for forming circuits by screen printing, that is, for screen printing. The presence or absence of bubbles on the surface of the printed film of the conductive composition, the conductivity of the cured film obtained by curing the printed film, bleeding at the ends of the cured film (thixotropy of the conductive composition), and the unevenness of the cured film surface can be evaluated, for example, by the method described in the Examples section below. EXAMPLES

[0081] The embodiments of the present invention will be described more specifically below with reference to examples and comparative examples.

[0082] [Synthesis Example 1] (Production of Polymer (A)) A 1L separable flask equipped with a stirrer, a thermometer, a condenser, a dropping funnel and a nitrogen inlet tube was charged with 90g of diethylene glycol monoethyl ether as a polymerization solvent and 84g of hydroxyethyl methacrylate as monomer (a2), and the atmosphere in the separable flask was replaced with nitrogen to create a nitrogen atmosphere. A monomer solution in which 196g of 4-hydroxyphenyl methacrylate was dissolved in 267g of diethylene glycol monoethyl ether as monomer (a1), and a polymerization initiator solution in which 43g of t-butyl peroxide carbonate and 43g of diethylene glycol monoethyl ether were mixed were prepared. Next, the temperature in the separable flask was raised to 75°C, and the monomer solution and the polymerization initiator solution were simultaneously dropped over 2 hours. After that, the mixture was reacted at 75°C for 3 hours to obtain a diethylene glycol monoethyl ether solution (solid content 40%) of polymer (A) (acrylic resin), which is a copolymer of 4-hydroxyphenyl methacrylate (a1) and hydroxyethyl methacrylate (a2) (molar ratio: a1 / a2 = 61 / 39).

[0083] (Measurement of weight average molecular weight) The weight average molecular weight of the obtained polymer (A) was determined by gel permeation chromatography (GPC) under the following conditions, and was found to be 26,000. Equipment: Tosoh Corporation, HLC-8220 Column: Shodex, LF-804 Standard material: polystyrene Eluent: THF (tetrahydrofuran) Flow rate: 1.0ml / min Column temperature: 40℃ Detector: RI (Differential Refractive Index Detector)

[0084] [Synthesis Example 2] (Copper particles (1): Production of surface-coated copper particles (1)) An aqueous solution of ammonium chloride was prepared by dissolving 5 g of ammonium chloride in 100 g of water. Copper particles a [Mitsui Mining & Smelting Co., Ltd. "1200Y"; particle size (D50) 2 μm, BET specific surface area 0.40 m 2 50 g of ammonium chloride solution (100 g / g, shape: spherical) was added to an aqueous ammonium chloride solution and stirred at 30°C for 60 minutes under nitrogen bubbling. Stirring was performed using a mechanical stirrer at a rotation speed of 150 rpm. The following stirring was performed at the same rotation speed using a similar stirring device. After stirring was completed, the copper particles were filtered out by vacuum filtration using a Kiriyama funnel with 5C filter paper, and then the copper particles were washed twice with 150 g of water on the Kiriyama funnel. The washed copper particles were added to 250 g of a 40% by mass aqueous solution of diethylenetriamine, and the mixture was heated and stirred at 60° C. for 1 hour while bubbling with nitrogen. After stopping the stirring and leaving it to stand for 5 minutes, about 200 g of the supernatant was removed. Next, 200 g of isopropanol was added to the precipitate as a cleaning solvent, and the mixture was stirred at 30° C. for 3 minutes. After stopping the stirring and leaving it to stand for 5 minutes, about 200 g of the supernatant was removed, and then 250 g of a 2% by mass lauric acid isopropanol solution was added, followed by stirring at 30° C. for 30 minutes. After the stirring was completed, the copper particles were filtered out by vacuum filtration using a Kiriyama funnel with 5C filter paper. The obtained copper particles were dried under reduced pressure at 25° C. for 3 hours to obtain surface-coated copper particles (1) (copper particles (1)).

[0085] [Synthesis Example 3] (Copper particles (2): Production of surface-coated copper particles (2)) Copper particles a were mixed with copper particles b [Mitsui Mining & Smelting Co., Ltd. "1400YP"; particle size (D50) 6 μm, BET specific surface area 0.60 m 2 Surface-coated copper particles (2) (copper particles (2)) were obtained in the same manner as in Synthesis Example 2, except that the composition was changed to [0.1 g / g, shape: plate-like].

[0086] Example 1 (Production of Conductive Composition) As component (A), 0.7 g of polymer (A) (acrylic resin) obtained in Synthesis Example 1 (solid content 40% by mass, solvent diethylene glycol monoethyl ether), as component (B), 0.08 g of diethylenetriamine (amine compound B-1), as component (C), 7.0 g of surface-coated copper particles (copper particles (1)) obtained in Synthesis Example 2 and 3.0 g of surface-coated copper particles (copper particles (2)) obtained in Synthesis Example 3 as component (C), 0.3 g of pyrazole-blocked polyisocyanate [Asahi Kasei Corporation, Duranate SBN-70D, solid content 70% by mass, solvent: dipropylene glycol monomethyl ether] as component (D), 0.05 g of N,N'-bis(salicylidene)ethylenediamine which is a Schiff base as an antioxidant and 0.3 g of hydroquinone which is a phenol, 0.1 g of lauric acid as a lubricant, and 0.3 g of diethylene glycol monoethyl ether which is an ether-based alcohol as a solvent were mixed. Next, the mixture was mixed at room temperature at a rotation speed of 2000 rpm for 60 seconds using a planetary mixer [ARV-310, manufactured by Thinky Corporation] to perform primary mixing. Next, the mixture was passed through a three-roll mill [EXAKT-M80S, manufactured by Nagase Screen Printing Laboratory Co., Ltd.] five times at room temperature and a roll distance of 5 μm to perform secondary mixing. The mixture obtained by the secondary mixing was mixed at room temperature and under vacuum conditions at a rotation speed of 1000 rpm for 90 seconds to produce a conductive composition by degassing and kneading. The blending ratio of the conductive composition is shown in Table 4. The blending ratio of the total solvent in the entire conductive composition is 6.8 mass%.

[0087] [Evaluation of electrical conductivity (volume resistivity)] (Formation of hardened film) The obtained conductive composition was applied onto a polyimide film (Kapton 500H, manufactured by Toray DuPont Co., Ltd.) using a metal mask (pattern: width × length × thickness = 1.0 mm × 30 mm × 50 μm). The polyimide film onto which the conductive composition was applied was heated in a convection oven at 130°C under atmospheric conditions for 30 minutes to produce a cured film.

[0088] (Method for evaluating volume resistivity) The thickness of the obtained cured film was measured at three points using a stylus-type film thickness meter (DektakXT, manufactured by Bruker) and the average value was calculated. The volume resistivity of the cured film was measured by pressing the measurement probe of a low resistivity meter (Loresta-GP MCP-T610, manufactured by Nitto Seiko Analytech Co., Ltd.) against the obtained cured film, converting the film thickness to 30 μm. The volume resistivity of the cured film was calculated from the average film thickness and the volume resistivity measured by the above method using the following formula. Volume resistivity (Ω·cm) = measured volume resistivity (Ω·cm) × {average film thickness (μm) / 30 (μm)}

[0089] The electrical conductivity of the cured film was evaluated according to the following evaluation criteria. The smaller the volume resistivity value, the easier it is for a current to flow through the cured film, indicating superior electrical conductivity. ◎: The volume resistivity value is less than 30 μΩ·cm. Good: The volume resistivity value is 30 μΩ·cm or more and less than 60 μΩ·cm. ×: The volume resistivity value is 60 μΩ·cm or more.

[0090] [Evaluation of bleeding at the edges of the cured film of the screen print] The obtained conductive composition was printed on a polyimide film using a screen printer (MT-320T, manufactured by Micro-Tech Co., Ltd.) and a screen plate (manufactured by SONOCOM, mesh size: 400 mesh, emulsion thickness: 20 μm) to obtain a screen print. The printing pattern was a thin line of width x length x thickness = 2.0 mm x 100 mm x 20 μm. The polyimide film on which the conductive composition was printed was heated in a convection oven under atmospheric pressure for 130 o The screen print was heated at 300 C for 30 minutes to obtain a cured product (cured film of thin lines). The cured film of thin lines was observed with a digital microscope (DINOAM3103, Sanko Co., Ltd.) (magnification: 50x), and the line width of the cured film of thin lines was measured at three locations, both ends and the center in the length direction of the thin lines, and the average value was taken as the measured value. The bleeding at the ends of the cured film was evaluated according to the following evaluation criteria. The smaller the deviation in the line width between the printed pattern and the cured film of thin lines, the better the thixotropy of the conductive composition and the less bleeding at the ends of the cured film. ◎: The measured line width is 1.9 mm or more and less than 2.1 mm. ○: The measured line width is 2.1 mm or more and less than 2.3 mm. ×: The measured line width is 2.3 mm or more.

[0091] [Evaluation of surface irregularities (surface roughness Ra) of the cured film of screen print] The obtained conductive composition was printed on a polyimide film using a screen printer (MT-320T, manufactured by Micro-Tech Co., Ltd.) and a screen plate (manufactured by SONOCOM, mesh size: 400 mesh, emulsion thickness: 20 μm) to obtain a screen print. The printing pattern was a solid film with a width x length x thickness of 30 mm x 30 mm x 20 μm. The polyimide film on which the conductive composition was printed was heated in a convection oven under atmospheric pressure for 130 o The screen-printed cured film was obtained by heating at 400°C for 30 minutes. The surface roughness Ra was measured using a stylus-type film thickness gauge (DektakXT, manufactured by Bruker) as an index of the surface irregularities of the cured film. The surface irregularities of the cured film were evaluated according to the following evaluation criteria. The smaller the Ra, the less the surface irregularities of the cured film. ⊚: Ra is less than 1.5 μm. ◯: Ra is 1.5 μm or more and less than 2.0 μm. ×: Ra is 2.0 μm or more.

[0092] [Evaluation of the presence or absence of air bubbles on the surface of screen-printed material (printed film)] A screen print (printed film) was obtained in the same manner as in "Evaluation of the surface irregularities (surface roughness Ra) of the cured film of the screen print". The presence or absence of air bubbles on the surface of the printed film was visually confirmed using a digital microscope (DINOAM3103, manufactured by Sanko Co., Ltd.) (magnification 50x, observation area 1.4 cm2). 2 If air bubbles are found on the surface of the printed film, the surface will become uneven when the film is cured, and voids will exist in the cured film as traces of the air bubbles, leading to a decrease in electrical conductivity.

[0093] [Examples 2 to 17, Comparative Examples 1 to 6] In Examples 2 to 17 and Comparative Examples 2 to 6, the predetermined amine compounds shown in Tables 1 to 3 were used, and in Examples 2 to 17 and Comparative Examples 1 to 6, the blending ratios were as shown in Tables 4 and 5. Except for this, conductive compositions were produced in the same manner as in Example 1. The blending ratios of the total solvent in the entire conductive composition in Examples 14, 15, Comparative Examples 1 and 2 were 6.7 mass%, 18.0 mass%, 6.9 mass%, and 6.5 mass%, respectively. Each evaluation was performed using the obtained conductive composition. The results are shown in Tables 4 and 5.

[0094] [Table 1]

[0095] [Table 2]

[0096] [Table 3]

[0097] [Table 4]

[0098] [Table 5]

[0099] In Examples 1 to 17, the volume resistivity was a maximum of 58 μΩ·cm, which showed good conductivity, and the line width of the fine lines was 1.9 mm to 2.2 mm, which was a small difference from the printed pattern, and it was confirmed that bleeding at the ends was well suppressed. In addition, the surface roughness Ra was a maximum of 1.9 μm in all cases, and it was confirmed that the unevenness of the cured film surface was small. In addition, the amine compound having an ethylenediamine skeleton provided high dispersibility of the conductive particles and excellent fluidity of the conductive composition, so no air bubbles were observed on the printed film surface.

[0100] In Comparative Example 1, in which a conductive composition was prepared without blending component (B), the volume resistivity was 89 μΩ·cm, the conductivity was poor, and air bubbles were observed on the surface of the printed film, and it was found that the surface roughness Ra of the cured film was 2.0 μm and the unevenness of the cured film surface was not sufficiently suppressed. In Comparative Example 2, in which a conductive composition was prepared with a content of component (B) of 6.0 mass%, no air bubbles were observed on the surface, but the volume resistivity was 5,000 μΩ·cm or more, the line width of the thin line was large at 2.4 mm, the occurrence of bleeding at the ends was not sufficiently suppressed, and the roughness of the cured film surface was large at 2.4 μm, and it was found that the unevenness of the cured film surface was not sufficiently suppressed. In Comparative Examples 3 to 6 in which conductive compositions were prepared using amines other than the specified amine compound, the volume resistivity was extremely high, the line width of the thin lines significantly deviated from the printed pattern, the cured film surface roughness Ra was high, and air bubbles were observed on the printed film surface. None of the comparative examples achieved all of the conductivity, edge bleeding, and cured film surface unevenness at a practical level.

[0101] As described above, the conductive composition containing the predetermined components (A) to (D) in a predetermined ratio has good thixotropy. In addition, by using the conductive composition, air bubbles are unlikely to occur on the surface and inside of the printed film formed by screen printing, for example, and the cured film of the printed film has good conductivity, the occurrence of surface irregularities is suppressed, and bleeding at the edges is also suppressed. Therefore, it is found that the conductive composition is suitable for use as a wiring forming material for electronic devices.

Claims

1. (A) binder resin: 1 to 30 mass% (B) 0.1 to 5 mass% of an amine compound having an ethylenediamine skeleton, (C) conductive particles 50 to 98% by mass, (D) polyisocyanate 0.5 to 15 mass% 1. A conductive composition comprising:

2. The conductive composition according to claim 1, wherein the amine compound (B) having an ethylenediamine skeleton is at least one selected from an amine represented by the following formula (1), an amine represented by the following formula (2), and a polyethyleneimine having a molecular weight of 100 to 10,000: [Case 1] (In formula (1), the degree of polymerization n is 1 to 5.) [Case 2] (In formula (2), R 1 is a hydrocarbon group having 1 to 3 carbon atoms, R 2 is a hydrocarbon group having 1 to 5 carbon atoms.

3. The conductive composition according to claim 1 or 2, wherein the binder resin (A) is a polymer composed of 20 to 100 mol % of a structural unit derived from a monomer (a1) represented by the following formula (3) and 0 to 80 mol % of a structural unit derived from a monomer (a2) copolymerizable with the monomer (a1): [C3] (In formula (3), R 3 is a single bond, an amide group or an ester group, R 4 is a hydrogen atom or a methyl group.

Citation Information

Patent Citations

  • Binder resin for electroconductive composition, composition containing same for electroconductive pattern formation, and polyurethane

    WO2017163615A1