Multi-functional battery cover for motor vehicle
A composite material comprising continuous reinforced fibers and thermoplastic resin integrates battery covers and cross members in electric vehicles, addressing weight and cost issues while enhancing impact resistance and rigidity.
Patent Information
- Application Number
- JP2023084757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional electric vehicles face challenges in weight reduction, manufacturing costs, and impact resistance of battery components due to the use of steel for battery cases, covers, and floor cross members, limiting the ability to carry more batteries and ensure safety in collisions.
The use of a composite material containing continuous reinforced fibers and thermoplastic resin for the battery cover and floor cross members, which integrates these components to provide rigidity, impact resistance, and reduce weight while lowering manufacturing costs.
The composite material-based battery cover and cross members achieve a lightweight, cost-effective solution with enhanced impact resistance and rigidity, allowing for a more compact vehicle design and improved safety.
Smart Images

Figure 2024168251000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-function battery cover for an automobile. [Background technology]
[0002] Electric vehicles, hybrid vehicles, and other electrically powered vehicles are equipped with battery modules such as lithium-ion batteries (hereinafter, sometimes simply referred to as "batteries"). Such batteries are generally mounted under the floor panels that form the floor surface of the vehicle interior.
[0003] Generally, an electric vehicle includes a pair of side sills extending in the front-rear direction of the vehicle body on the outer sides in the vehicle width direction, and a floor panel that constitutes the floor surface of the vehicle compartment and is fixed to the pair of side sills. The battery is usually stored under the floor panel and covered by a lower case (battery case) and an upper case (battery cover).
[0004] Typically, multiple floor cross members are arranged on the upper part of the floor panel so as to extend in the vehicle width direction of the vehicle compartment (Patent Document 1). These floor cross members are components used for purposes such as supporting passenger seats arranged above them and increasing the rigidity of the vehicle body. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2021 / 070530 Summary of the Invention [Problem to be solved by the invention]
[0006] In the conventional electric vehicles described above, in order to ensure the rigidity of the vehicle body, all of the components, such as the battery case, the battery cover, the floor panel, and the floor cross member, are generally made of steel. Therefore, there is a limit to how much the vehicle body can be made lighter, and there are problems in that the manufacturing (processing) costs are high, leaving room for improvement.
[0007] Furthermore, in the above-mentioned conventional electric vehicles, there is a demand for loading more batteries. However, in order to meet this demand, it is necessary to secure a sufficient space to ensure the safety of the battery in the event of a collision, or to further improve the impact resistance of the parts around the battery. In particular, in order to meet the demand for a more compact vehicle body, it is more important to improve the impact resistance of the parts around the battery.
[0008] Therefore, an object of the present invention is to provide a battery cover for an automobile that is lightweight, has excellent impact resistance while maintaining the rigidity of the vehicle body, and can be manufactured at low cost. [Means for solving the problem]
[0009] In order to solve the above-mentioned problems, the inventors of the present invention have conducted extensive research into optimizing the materials used to manufacture each part. As a result, it has been found that by using a composite material containing a specific fiber and resin to manufacture the battery cover body, it is possible to not only reduce the weight by moving away from metal, but also ensure the rigidity of the vehicle body to be equal to that of steel. It has also been found that, due to the high strength of the composite material, the battery cover body made of the composite material can function as a floor panel that constitutes the floor surface of the vehicle interior.
[0010] Furthermore, it was also found that the floor cross member can be manufactured using the above composite material and joined to the battery cover body, thereby achieving high impact resistance. By combining these new findings, it is possible to integrate multiple parts and reduce the number of parts, thereby further reducing manufacturing costs. In this way, the present invention was completed.
[0011] That is, the present invention is as follows.
[0012] [1] A multi-function battery cover for a car, comprising: A battery cover body and a plurality of floor cross members joined to the battery cover body and configured to extend in one direction, The battery cover body and the floor cross member are made of a continuous reinforced fiber resin composite material containing a fiber bundle including continuous reinforced fiber and a thermoplastic resin, and the battery cover body also functions as a floor panel that constitutes the floor surface of the vehicle compartment. A multi-functional battery cover.
[0013] [2] A multi-function battery cover as described in [1], wherein a closed cross-sectional structure is formed by the battery cover body and the floor cross member.
[0014] [3] A multi-functional battery cover as described in [1] or [2], wherein the floor cross member further has a rib structure made of thermoplastic resin.
[0015] [4] A multi-function battery cover as described in [3], wherein in the floor cross member, the thermoplastic resin constituting the continuous reinforced fiber resin composite and the thermoplastic resin constituting the rib structure are the same resin.
[0016] [5] A multi-functional battery cover as described in [1] or [2], wherein the battery cover body further has a rib structure made of a thermoplastic resin.
[0017] [6] A multifunctional battery cover as described in [5], wherein in the battery cover main body, the thermoplastic resin constituting the continuous reinforced fiber resin composite and the thermoplastic resin constituting the rib structure are the same resin.
[0018] [7] The multifunctional battery cover described in [3], wherein the battery cover body further has a rib structure made of thermoplastic resin.
[0019] [8] A multifunctional battery cover as described in [7], wherein in the battery cover main body, the thermoplastic resin constituting the continuous reinforced fiber resin composite and the thermoplastic resin constituting the rib structure are the same resin.
[0020] [9] A multifunctional battery cover as described in [2], which has a thermoplastic resin foam in the closed cross-sectional structure area.
[0021]
[10] The multifunctional battery cover according to any one of [1] to [9], wherein the continuous reinforcing fibers include glass fibers. Effect of the Invention
[0022] According to the present invention, it is possible to provide a multi-functional battery cover for automobiles that is lightweight, has excellent impact resistance while maintaining the rigidity of the vehicle body, and can be manufactured at low cost. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is a schematic perspective view of a multi-function battery cover according to an embodiment of the present invention; [Diagram 2] 1 is a schematic partial cross-sectional view of a multi-function battery cover according to one embodiment of the present invention; [Diagram 3] 1 is a schematic partial cross-sectional view of a multi-function battery cover according to one embodiment of the present invention; [Figure 4] 1 is a schematic perspective view of a floor cross member in a multi-function battery cover according to one embodiment of the present invention; FIG. [Diagram 5] 1 shows load-displacement curves measured in Examples and Comparative Examples. [Figure 6]1 shows load-displacement curves measured in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention. In this specification, the term "consisting of" is used in the so-called open-ended concept.
[0025] A multifunctional battery cover according to one embodiment of the present invention (hereinafter, sometimes simply referred to as "the battery cover according to this embodiment") is a component used in automobiles, particularly in electrically powered vehicles such as electric vehicles and hybrid vehicles. The battery cover according to this embodiment is characterized in that it comprises a battery cover main body and a plurality of floor cross members joined to the battery cover main body and configured to extend in one direction, the battery cover main body and the floor cross members being made of a continuous reinforced fiber resin composite material containing fiber bundles including continuous reinforcing fibers and a thermoplastic resin, and the battery cover main body also functions as a floor panel that constitutes the floor surface of the vehicle interior.
[0026] Fig. 1 shows a schematic perspective view of a battery cover 1 of this embodiment. The battery cover 1 in Fig. 1 includes a battery cover main body 11 and a plurality of floor cross members 12. The battery cover main body 11 is typically substantially planar and substantially rectangular in plan view so as to function as a floor panel for the electric vehicle. Furthermore, the battery cover main body 11 can have an appropriate detailed shape according to the shape of the battery so as to cover and provide good protection for the battery mounted under the electric vehicle.
[0027] In the battery cover 1, multiple floor cross members 12 are joined to the battery cover body 11 so as to extend in one direction. The direction in which the floor cross members 12 extend is typically the vehicle width direction when the battery cover 1 of this embodiment is installed on an electric vehicle. The number and positions of the floor cross members 12 in the battery cover 1 are not particularly limited and can be appropriately selected depending on the purpose.
[0028] The battery cover 1 of this embodiment, particularly the battery cover main body 11 and the multiple floor cross members 12, are made of a "continuous reinforced fiber resin composite material containing a fiber bundle containing continuous reinforced fiber and a thermoplastic resin." Therefore, the battery cover 1 can exhibit high rigidity and impact resistance while being lightweight. In addition, since the battery cover main body 11 is made of the continuous reinforced fiber resin composite material, it can also function well as a floor panel that constitutes the floor surface of the vehicle interior. In other words, the multifunctional battery cover of this embodiment has a reduced number of parts compared to the conventional one by integrating the floor panel and the battery cover, which contributes to further reducing manufacturing costs. The continuous fiber-reinforced resin composite material used in this embodiment will be described in detail later.
[0029] It is preferable that neither the battery cover body 11 nor the multiple floor cross members 12 in the battery cover 1 of this embodiment contain metal materials such as steel. However, if it is necessary to further improve the strength and / or rigidity of the parts, the battery cover body 11 and / or the multiple floor cross members 12 may be provided with a minimum number of metal material parts with optimized shapes.
[0030] 2 shows a schematic cross-sectional view of the battery cover 1 of this embodiment taken perpendicularly to the extension direction of the multiple floor cross members 12. As shown in Fig. 2, the battery cover 1 of this embodiment preferably has a closed cross-sectional structure (closed cross section 15) formed by the battery cover main body 11 and the floor cross member 12. In this case, when the battery cover 1 is disposed on an electric vehicle, it is possible to further improve the bending rigidity and torsional rigidity of the vehicle body, as well as the absorbed energy during a sudden collision.
[0031] The shape of the closed cross section 15 is not particularly limited, and may be, for example, a rectangular shape as shown in Fig. 2. The shape of the closed cross section 15 may be the same or different throughout the direction in which the floor cross member 12 extends.
[0032] Furthermore, in the battery cover 1 of this embodiment, when the battery cover body 11 and the floor cross member 12 form a closed cross-sectional structure (closed cross-section 15) as described above, it is preferable to provide a thermoplastic resin foam 17 in the area of the closed cross-sectional structure as shown in Fig. 3. In this case, the sound insulation and vibration damping properties of the battery cover 1 can be further improved. The thermoplastic resin foam will be described in detail later.
[0033] Moreover, it is preferable that the floor cross member 12 in the battery cover 1 of this embodiment further has a rib structure 18, as shown in Fig. 4. In this case, when the battery cover 1 is installed in an electric vehicle, the rigidity and strength of the vehicle body can be further improved. It is preferable that the floor cross member 12 has an open cross-sectional shape when cut perpendicularly to the direction in which the floor cross member 12 extends (FIGS. 2 to 4). In this case, the rib structure 18 can be formed in the floor cross member 12 more easily. Furthermore, the rib structure can be formed before joining the battery cover body and the floor cross member.
[0034] Specifically, as shown in FIG. 4, the rib structure 18 may have a structure in which a plurality of plates made of thermoplastic resin stand substantially upright inside the opening of the floor cross member 12 and are connected together. The rib structure 18 may be obtained by, for example, injection molding using a molding material containing at least a thermoplastic resin. The molding material may be a molding material containing only a thermoplastic resin, or may be a molding material containing a thermoplastic resin and a reinforcing fiber. In addition, when the molding material contains a reinforcing fiber, the length of the reinforcing fiber is not particularly limited. That is, the reinforcing fiber may be a short fiber of about 0.2 to 0.4 mm, or may be a long fiber of 3 mm or more. Furthermore, the molding material may be, for example, a pellet-shaped material.
[0035] In another embodiment, the rib structure 18 can be produced by pressing a random fiber reinforcement material as a molding material with a molding die having a shape corresponding to the structure of the desired rib structure. Examples of the random fiber reinforcement include chopped sheets made by cutting prepregs made of reinforced fibers impregnated with thermoplastic resin into strips. In this case, a press machine incorporating a high-output pressure injection unit is not required, and a significant reduction in capital investment can be expected. In addition, when the rib structure is produced using carbon fiber as the reinforcement fiber, the rigidity of the battery cover can be further improved.
[0036] As specific examples of reinforcing fibers that can be contained in the molding material, the description of the reinforcing fibers used in the continuous reinforcing fibers that constitute the continuous fiber-reinforced resin composite material described below can be applied.
[0037] In addition, in the floor cross member 12 having the rib structure 18, it is preferable that the thermoplastic resin constituting the rib structure 18 and the thermoplastic resin constituting the continuous fiber-reinforced resin composite material (described in detail later) are the same resin. In this case, when the floor cross member 12 made of the continuous fiber-reinforced resin composite material and the rib structure 18 are combined by thermal welding, the bonding strength between the two members can be further increased.
[0038] Although not shown, the battery cover body 11 in the battery cover 1 of this embodiment may also have a rib structure. In this case, when the battery cover 1 is installed in an electric vehicle, the rigidity and strength of the vehicle body can be further improved.
[0039] In addition, in the battery cover body 11 having a rib structure, it is preferable that the thermoplastic resin constituting the rib structure and the thermoplastic resin constituting the continuous reinforced fiber resin composite material (described in detail later) are the same resin. In this case, when the battery cover body 11 made of the continuous reinforced fiber resin composite material and the rib structure are combined by thermal welding, the bonding strength between the two members can be further increased.
[0040] As specific examples of the thermoplastic resin constituting the above-mentioned rib structure, the description of the thermoplastic resin constituting the continuous fiber-reinforced resin composite material described below can be applied.
[0041] The battery cover 1 of the present embodiment is preferably configured so as to be fixed to a pair of side sills extending in the front-rear direction of the vehicle body on the outer sides in the vehicle width direction of an electric vehicle. Examples of the fixing method include adhesion with an adhesive, bolt fastening, rivet fastening, etc.
[0042] <Continuous fiber reinforced resin composite material> The continuous fiber-reinforced resin composite material used in this embodiment is a material containing a fiber bundle containing continuous reinforcing fibers and a thermoplastic resin. In the battery cover of this embodiment, the battery cover body and the molded body such as the floor cross member are made of this continuous fiber-reinforced resin composite material. Examples of continuous reinforced fiber resin composite materials include materials obtained by combining woven, knitted, braided, or tubular reinforced fibers with resin; materials obtained by combining unidirectionally aligned reinforced fibers with thermoplastic resin; materials obtained by unidirectionally aligning threads of reinforced fibers and thermoplastic resin; and materials obtained by woven, knitted, braided, or tubular reinforced fibers with threads of reinforced fibers and thermoplastic resin. Examples of intermediate materials prior to molding of continuous fiber-reinforced resin composites include mixed yarns of continuous reinforcing fibers and resin fibers, coated yarns in which bundles of continuous reinforcing fibers are covered with resin, continuous reinforcing fibers impregnated with resin in advance and formed into a tape, continuous reinforcing fibers sandwiched between resin films, continuous reinforcing fibers with resin powder attached, a bundle of continuous reinforcing fibers as a core material braided with resin fibers, and continuous reinforcing fibers impregnated with resin between bundles of continuous reinforcing fibers.
[0043] In the continuous reinforced fiber resin composite of this embodiment, the cross section of the continuous reinforced fiber is approximately circular, and the number of continuous reinforced fibers in which the porosity in the peripheral outer region away from the peripheral portion of the continuous reinforced fiber, which is 1 / 10 of the radius of one continuous reinforced fiber, is 10% or less at the extreme interface between one continuous reinforced fiber and the thermoplastic resin in the cross section perpendicular to the length direction of the continuous reinforced fiber, is preferably 10% or more of the total number of continuous reinforced fibers. That is, the continuous reinforced fiber resin composite of this embodiment contains a continuous reinforced fiber with an approximately circular cross section and a thermoplastic resin, and there are continuous reinforced fibers in which the porosity in the peripheral outer region away from the peripheral portion of the continuous reinforced fiber, which is observed at the extreme interface between one continuous reinforced fiber and the synthetic resin in the cross section perpendicular to the length direction of the continuous reinforced fiber, is 10% or less at the radial direction, which is 1 / 10 of the radius r of one continuous reinforced fiber (i.e., r / 10), and the number of such continuous reinforced fibers is preferably 10% or more of the total number of continuous reinforced fibers. The cross section of the continuous reinforcing fiber is preferably substantially circular, and may be elliptical. In this case, the "radius" refers to the shortest distance from the center of the fiber cross section toward the periphery.
[0044] The above-mentioned void ratio is, for example, measured by cutting a continuous reinforced fiber resin composite material into a 1 cm square by a band saw or the like, and polishing the cross section perpendicular to the longitudinal direction of the continuous reinforcement fiber with a pressure of 400 g / cm 2The polishing table was rotated at 100 rpm so that a force of 1000 mm was applied, and the sample was polished in the following order: 10 minutes with waterproof paper #220, 2 minutes with waterproof paper #400, 5 minutes with waterproof paper #800, 10 minutes with waterproof paper #1200, 15 minutes with waterproof paper #2000, 15 minutes with silicon carbide film grain size 9 μm, 15 minutes with alumina film grain size 5 μm, 15 minutes with alumina film grain size 3 μm, 15 minutes with alumina film grain size 1 μm, and 10 minutes with colloidal silica (Baicalox 0.1CR) with a grain size of 0.1 μm using buffing paper foamed polyurethane. Water was added at about 7 mL / min for each polishing step, and the polished sample was observed with a scanning electron microscope (SEM) and image analysis was performed using software such as ImageJ, and the following formula was used to determine the surface roughness. Void ratio (%) = (area of voids in the outer peripheral region away from the periphery of the continuous reinforcing fiber by 1 / 10 of the radius of the continuous reinforcing fiber) / (area of the outer peripheral region away from the periphery of the continuous reinforcing fiber by 1 / 10 of the radius of the continuous reinforcing fiber) × 100
[0045] Then, the porosity of an outer peripheral region of any one continuous reinforcing fiber, at a distance of 1 / 10 of the radius from the peripheral portion of the continuous reinforcing fiber, is obtained, and this is observed for any 100 fibers. From these results, the ratio of the number of continuous reinforcing fibers having a porosity of 10% or less to the total number of continuous reinforcing fibers can be obtained. From the viewpoint of increasing the rigidity and strength of the molded body, the above ratio is preferably 10% or more (i.e., 10 or more out of 100 fibers), more preferably 20% or more, even more preferably 50% or more, even more preferably 70% or more, and particularly preferably 90% or more. Furthermore, in the continuous reinforcing fiber resin composite of this embodiment, from the viewpoint of increasing rigidity and strength, the void ratio in an area that is one-tenth the diameter of the continuous reinforcing fiber is preferably 5% or less, more preferably 2% or less, and even more preferably 1% or less.
[0046] To achieve "the number of continuous reinforcing fibers in which the void ratio of an area of 1 / 10 of the diameter of the continuous reinforcing fibers is 10% or less, is 10% or more of the total number of continuous reinforcing fibers", for example, when the continuous reinforcing fibers are glass fibers, a sizing agent applied in the production of the glass fibers and a thermoplastic resin should be selected that have a μ drop generation coefficient of 10 or more and are compatible with each other, and a molding method that can seal the inside of the mold during molding, such as a spigot mold, or a molding method using a double belt press with adjusted pressure should be selected to prevent resin leakage, reduce the change before and after molding in the volume occupied by the glass fibers in the continuous reinforcing fiber resin composite (Vf, also called volume content), and perform molding under temperature conditions suitable for the sizing agent.
[0047] The μ drop generation coefficient is an index showing the compatibility between thermoplastic resin and reinforcing fiber, and is affected not only by the main component of the resin but also by trace components contained in the resin. The μ drop generation coefficient is calculated by, for example, using a composite interface property evaluation device (HM410, Toei Sangyo Co., Ltd.) to touch the resin to the reinforcing fiber multiple times (for example, four times) when applying resin to a single reinforcing fiber thread, counting the number of μ drops generated, and calculating the μ drop generation coefficient using the following formula: (μ drop generation coefficient) = {(number of μ drops generated) / (number of times the reinforcing fiber was touched with the resin)} × 10 It can be calculated as follows.
[0048] From the viewpoint of strength, the volume ratio (Vf) of the reinforcing fibers in the continuous reinforced fiber resin composite is preferably 40% or more, more preferably 45% or more, even more preferably 50% or more, even more preferably 55% or more, and particularly preferably 65% or more. The volume ratio (Vf) of the reinforcing fibers in a continuous fiber-reinforced resin composite can be calculated by heating the continuous fiber-reinforced resin composite at 650°C for 3 hours, burning off the resin, allowing it to cool naturally to room temperature, and measuring the mass of the remaining reinforcing fibers. The ratio of reinforcing fibers to resin in the molded product can then be divided by the density to calculate the volume ratio (Vf) of the reinforcing fibers.
[0049] -Reinforced fiber- The reinforcing fibers used for the continuous reinforcing fibers are preferably fibers that do not have a yield point, from the viewpoint of obtaining an impact absorber with a higher amount of absorbed energy. From the viewpoint of impact absorption, the reinforcing fibers preferably have a tensile modulus of elasticity of 15 GPa or more as measured in accordance with JIS K7127. From the viewpoint of energy absorption at the time of breakage, the reinforcing fibers preferably have a tensile strength of 350 MPa or more as measured in accordance with JIS K7161. In this disclosure, "having no yield point" refers to a stress-strain curve in which the stress continues to increase as the strain increases. Fibers with no yield point undergo elastic deformation until they break, and return to their original shape when the load is removed.
[0050] Specific examples of the reinforcing fibers include glass fibers, aramid fibers, ultra-high strength polyethylene fibers, liquid crystal polyester fibers, polyketone fibers, ceramic fibers, polycarbonate fibers, etc. These reinforcing fibers may be used alone or in combination of two or more. Among these, glass fibers are preferred as the reinforcing fibers from the viewpoints of heat resistance, non-combustibility, flexibility, cost, ease of handling, etc. In other words, in the present embodiment, the continuous reinforcing fibers preferably contain glass fibers.
[0051] The cross section of the reinforcing fiber is preferably approximately circular, and may also be elliptical.
[0052] As the reinforcing fibers, it is preferable to use continuous reinforcing fibers to which a sizing agent containing a coupling agent, a binder, and a lubricant has been added.
[0053] Coupling agents are usually used as surface treatment agents for reinforcing fibers, and contribute to improving the interfacial adhesive strength. When the reinforcing fiber is a glass fiber, the coupling agent may be a silane coupling agent. The silane coupling agent is not limited to the following, but may be, for example, aminosilanes such as γ-aminopropyltrimethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane; mercaptosilanes such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane; epoxysilanes; vinylsilanes, maleic acids, etc. When polyamide is used as the thermoplastic resin, aminosilanes and maleic acids are preferred as the silane coupling agent, and when epoxy resin is used as the thermoplastic resin, epoxysilanes are preferred as the silane coupling agent.
[0054] The binder contributes to improving the bundling property of the reinforcing fibers and improving the interfacial adhesive strength. As the binder, a polymer or a thermoplastic resin can be used according to the purpose. Examples of the polymer used as the binder include, but are not limited to, homopolymers of acrylic acid, copolymers of acrylic acid and other copolymerizable monomers, and salts of these with primary, secondary, and tertiary amines. In addition, examples of the polymer used as the binder include m-xylylene diisocyanate, 4,4 ’ Polyurethane resins synthesized from isocyanates such as methylene bis(cyclohexyl isocyanate) and isophorone diisocyanate and polyester or polyether diols are also suitably used. Thermoplastic resins used as binders include, but are not limited to, polyolefin resins, polyamide resins, polyacetal resins, polycarbonate resins, polyester resins, polyether ketone, polyether ether ketone, polyether sulfone, polyphenylene sulfide, thermoplastic polyetherimide, thermoplastic fluorine resins, and modified thermoplastic resins obtained by modifying these resins.
[0055] The lubricant contributes to improving the opening property of the reinforcing fibers. As the lubricant, any ordinary liquid or solid lubricating material can be used depending on the purpose, and examples thereof include, but are not limited to, animal, vegetable or mineral waxes such as carnauba wax and lanolin wax; surfactants such as fatty acid amides, fatty acid esters, fatty acid ethers, aromatic esters, and aromatic ethers.
[0056] In addition to the above, the sizing agent may be, for example, one described in JP 2015-101794 A. The type and amount of the sizing agent (coupling agent, binder, and lubricant) may be appropriately selected according to the characteristics of the reinforcing fibers.
[0057] The continuous reinforcing fiber is preferably a multifilament consisting of a plurality of reinforcing fibers. From the viewpoint of handleability, the number of single yarns of the continuous reinforcing fiber is preferably 30 to 15,000. From the viewpoints of strength and handleability, the single yarn diameter of the continuous reinforcing fiber is preferably 2 to 30 μm, more preferably 4 to 25 μm, further preferably 6 to 20 μm, and particularly preferably 8 to 18 μm.
[0058] -Thermoplastic resin- Examples of the thermoplastic resin in the continuous reinforced fiber resin composite include polyolefin resins such as polyethylene and polypropylene; polyamide resins such as polyamide 6, polyamide 66, and polyamide 46; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polytrimethylene terephthalate; polyacetal resins such as polyoxymethylene; polycarbonate resins; polyether ketone; polyether ether ketone; polyether sulfone; polyphenylene sulfide; thermoplastic polyetherimide; thermoplastic fluorine resins such as tetrafluoroethylene-ethylene copolymer; and modified thermoplastic resins obtained by modifying these. These thermoplastic resins may be used alone or in combination of two or more. Among these, crystalline resins are preferred as the thermoplastic resin. Among these, polyolefin resins, polyamide resins, polyester resins, polyether ketone, polyether ether ketone, polyether sulfone, polyphenylene sulfide, thermoplastic polyetherimide, and thermoplastic fluorine resins are preferred. Among these, the thermoplastic resin is more preferably a polyolefin resin, a modified polyolefin resin, a polyamide resin, or a polyester resin from the viewpoint of mechanical properties and versatility, and more preferably a polyamide resin or a polyester resin from the viewpoint of thermal properties. Furthermore, the thermoplastic resin is even more preferably a polyamide resin, and particularly preferably polyamide 66, from the viewpoint of durability against repeated loads.
[0059] The polyamide resin refers to a polymeric compound having a -CO-NH- (amide) bond in the main chain. Examples of the polyamide resin include, but are not limited to, polyamides obtained by ring-opening polymerization of lactams, polyamides obtained by self-condensation of ω-aminocarboxylic acids, polyamides obtained by condensing diamines and dicarboxylic acids, and copolymers thereof. The polyamide resin may be used alone or in combination of two or more kinds. Regarding the details of the above lactam, diamine (monomer), and dicarboxylic acid (monomer), those described in JP 2015-101794 A can be appropriately applied.
[0060] Specific examples of polyamides include polyamide 4 (poly-α-pyrrolidone), polyamide 6 (polycaproamide), polyamide 11 (polyundecane amide), polyamide 12 (polydodecanamide), polyamide 46 (polytetramethylene adipamide), polyamide 66 (polyhexamethylene adipamide), polyamide 610, polyamide 612, polyamide 6T (polyhexamethylene terephthalamide), polyamide 9T (polynonamethylene terephthalamide), and polyamide 6I (polyhexamethylene isophthalamide), as well as copolymer polyamides containing these as constituent components.
[0061] Examples of the copolymer polyamide include a copolymer of hexamethylene adipamide and hexamethylene terephthalamide, a copolymer of hexamethylene adipamide and hexamethylene isophthalamide, and a copolymer of hexamethylene terephthalamide and 2-methylpentanediamine terephthalamide.
[0062] The polyester resin refers to a polymer compound having a -CO-O- (ester) bond in the main chain. Examples of the polyester resin include, but are not limited to, polyethylene terephthalate, polybutylene terephthalate, polytetramethylene terephthalate, poly-1,4-cyclohexylene dimethylene terephthalate, and polyethylene-2,6-naphthalenedicarboxylate. Regarding details of other polyester-based resins, those described in JP-A-2015-101794 can be used as appropriate.
[0063] The proportion of the thermoplastic resin in 100% by mass of the continuous reinforced fiber resin composite material is preferably 25 to 40% by mass, and more preferably 20 to 30% by mass.
[0064] -Flame retardants- In addition, since automotive battery covers are required to have flame retardant performance, the continuous reinforced fiber resin composite preferably contains a flame retardant. Examples of the flame retardant include organic phosphinates, and more specifically, examples of the flame retardant include at least one organic phosphinate selected from the group consisting of organic phosphinates represented by the following general formula (1) (hereinafter also referred to as "phosphinate (1)"), organic diphosphinates represented by the following general formula (2) (hereinafter also referred to as "diphosphinate (2)"), and condensates thereof.
[0065] [ka]
[0066] [In formula (1), R 11 and R 12 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. m is 2 or 3. 11 and R 12 may be the same or different. 1a+ is a metal ion with a valence of a, M 1 is an ion of an element belonging to group 2 or 15 of the periodic table, an ion of a transition element, a zinc ion, or an aluminum ion, and a is 2 or 3. a=m.
[0067] [ka]
[0068] [In formula (2), R 21 and R 22 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. 23 is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. n is an integer of 1 to 3. When n is 2 or 3, a plurality of R 21 , R 22 , and R23 may be the same or different. 2b+ is a metal ion with a valence of b, and M 2 is an ion of an element belonging to Group 2 or 15 of the periodic table, an ion of a transition element, a zinc ion, or an aluminum ion, and b is 2 or 3. j is 1 or 2. When j is 2, there are multiple M 2 may be the same or different. n, b, and j are integers that satisfy the relational expression 2n=b×j.
[0069] Specific examples of preferred phosphinates (1) include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, methane di(methylphosphinate), ) calcium, magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-(dimethylphosphinate), magnesium benzene-1,4-(dimethylphosphinate), aluminum benzene-1,4-(dimethylphosphinate), zinc benzene-1,4-(dimethylphosphinate), calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, zinc diphenylphosphinate, etc. Among them, from the viewpoints of flame retardancy, compatibility with polyamide, and easy availability of raw materials, metal diethylphosphinate is preferred, and aluminum diethylphosphinate is particularly preferred.
[0070] Specific examples of preferred diphosphinates (2) include calcium methane di(methylphosphinate), magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-di(methylphosphinate), magnesium benzene-1,4-di(methylphosphinate), aluminum benzene-1,4-di(methylphosphinate), and zinc benzene-1,4-di(methylphosphinate).
[0071] The content of the flame retardant is preferably 0.5 to 20 mass%, more preferably 1 to 6 mass%, and even more preferably 1.2 to 3 mass% of the continuous reinforced fiber resin composite material (100 mass%). When the content of the flame retardant is within the above range, the flame retardancy can be improved without impairing the properties of the thermoplastic resin. Furthermore, when the content of the flame retardant is within the above range, the decrease in mechanical strength is reduced, so that a continuous reinforced fiber resin composite material having an excellent balance between flame retardancy and mechanical strength can be obtained. The flame retardant can be incorporated into the continuous fiber-reinforced resin composite material by, for example, blending it with the thermoplastic resin in advance.
[0072] -Other additives- The continuous fiber-reinforced resin composite may contain additives other than those mentioned above, if necessary. Examples of the additives include antiaging agents, antioxidants, weathering agents, metal deactivators, light stabilizers, heat stabilizers, ultraviolet absorbers, antibacterial and antifungal agents, deodorizers, conductivity imparting agents, dispersants, softeners, plasticizers, crosslinking agents, co-crosslinking agents, vulcanizing agents, vulcanization assistants, foaming agents, foaming assistants, colorants, vibration dampers, nucleating agents, neutralizing agents, lubricants, antiblocking agents, dispersants, flow improvers, and mold release agents.
[0073] The content of the additive in the continuous reinforcing fiber resin composite material may be 10% by mass or less relative to 100% by mass of the total of the reinforcing fibers and the thermoplastic resin. These additives can be incorporated into the continuous fiber-reinforced resin composite material, for example, by blending them with the thermoplastic resin in advance.
[0074] <Thermoplastic resin foam> The thermoplastic resin foam is a material that can be disposed in the region of the closed cross-sectional structure when a closed cross-sectional structure (closed cross-section 15) is formed by the battery cover main body 11 and the floor cross member 12 in the battery cover of this embodiment. There are no particular limitations on the method for producing the thermoplastic resin foam, but for example, a foaming agent is contained (impregnated) in a thermoplastic resin having foamability, and resin particles (pre-expanded particles) are obtained by foaming, and then the resin particles are filled into a molding die having a predetermined shape and heated with steam or the like to foam the resin particles and simultaneously heat-fuse the resin particles together, thereby obtaining a thermoplastic resin foam as a foamed molded product.
[0075] Examples of the foamable thermoplastic resin include polyester resins, polyamide resins, polyphenylene ether resins, (meth)acrylic resins, etc. The foamable thermoplastic resins may be used alone or in combination of two or more.
[0076] Examples of methods for containing (impregnating) a blowing agent in a thermoplastic resin include a method using an aqueous medium in a suspension system such as water (suspension impregnation method), a method using a thermal decomposition type blowing agent such as sodium bicarbonate (blowing agent decomposition method), a method in which a gas blowing agent is in a liquid phase state in an atmosphere above the critical pressure and contacted with a thermoplastic resin (liquid phase impregnation method), and a method in which a gas blowing agent is in a gas phase state in an atmosphere below the critical pressure and contacted with a thermoplastic resin (gas phase impregnation method). Among these, the gas phase impregnation method is preferred. The reason for this is that in the gas phase impregnation method, the solubility of the gas in the thermoplastic resin is higher than in the suspension impregnation method carried out under high temperature conditions, and the content of the blowing agent can be increased. Therefore, in the gas phase impregnation method, it is easy to achieve a high expansion ratio, and as a result, the bubble size in the resin particles is easily uniform.
[0077] The shape of the thermoplastic resin used in the gas phase impregnation method is not particularly limited, but examples include beads, pellets, spheres, irregularly shaped pulverized material, etc. The size of the thermoplastic resin is preferably an average diameter of 0.2 to 3 mm, from the viewpoints of making the size of the pre-expanded particles after expansion appropriate, improving the ease of handling of the pre-expanded particles, and making the packing during molding denser.
[0078] The conditions for the gas phase impregnation method are not particularly limited. For example, from the viewpoint of more efficiently dissolving the gas into the resin, the atmospheric pressure is preferably 0.5 to 6.0 MPa, and the atmospheric temperature is preferably 5 to 30°C.
[0079] As the gas blowing agent, those which have little impact on the environment and are not flammable or combustible are preferred, and from the viewpoint of safety during handling, inorganic compounds which are not flammable or combustible are more preferred, and from the viewpoints of solubility in resins and ease of handling, carbon dioxide gas (carbon dioxide gas) is particularly preferred.
[0080] The method of filling the molding die with resin particles (pre-expanded particles) is not particularly limited, but examples include a cracking method in which resin particles are filled with the die slightly open, a compression method in which compressed resin particles are filled with the die closed, and a compression cracking method in which compressed resin particles are filled into the die and then the above-mentioned cracking method is carried out. The thermoplastic resin foam can be placed in the closed cross-sectional structure area before joining the battery cover body and the floor cross member.
[0081] <Battery cover manufacturing method> The battery cover of the present embodiment may be manufactured by any method as long as the battery cover body and the floor cross member are each manufactured using the above-mentioned continuous fiber-reinforced resin composite material. (A1) a step of hot pressing continuous reinforcing fibers and a thermoplastic resin to a temperature equal to or higher than the melting point of the thermoplastic resin, and then cooling to a temperature equal to or lower than the melting point of the thermoplastic resin to obtain a continuous reinforcing fiber resin composite material (prepreg); (A2) a step of heating the continuous reinforced fiber resin composite material (prepreg) obtained in the step (A1) to a temperature equal to or higher than the melting point of the thermoplastic resin by a heater or oven, and then disposing the continuous reinforced fiber resin composite material (prepreg) in a molding die having a predetermined shape and performing a cooling press; (A3) after the step (A2), a step of cooling the thermoplastic resin to a temperature equal to or lower than the melting point of the thermoplastic resin to obtain a floor cross member as a molded article made of a continuous fiber-reinforced resin composite material; (A4) a step of heating the continuous reinforced fiber resin composite material (prepreg) obtained in the step (A1) to a temperature equal to or higher than the melting point of the thermoplastic resin by a heater or oven, and then disposing the continuous reinforced fiber resin composite material (prepreg) in a molding die having a predetermined shape and performing a cooling press; (A5) after the step (A4), a step of cooling the thermoplastic resin to a temperature equal to or lower than the melting point of the thermoplastic resin to obtain a battery cover body as a molded product made of a continuous fiber-reinforced resin composite material; (A6) A step of joining the battery cover body obtained in the (A5) step and the floor cross member obtained in the (A3) step; It can be produced by a production method including the steps of:
[0082] The battery cover of the present embodiment can be produced, for example, by the following steps: (B1) a step of hot pressing continuous reinforcing fibers and a thermoplastic resin to a temperature equal to or higher than the melting point of the thermoplastic resin, and then cooling to a temperature equal to or lower than the melting point of the thermoplastic resin to obtain a continuous reinforcing fiber resin composite material (prepreg); (B2) a step of heating the continuous fiber reinforced resin composite material (prepreg) and the random fiber reinforced material obtained in the step (B1) to a temperature equal to or higher than the melting point of the thermoplastic resin by a heater or oven, and then arranging the random fiber reinforced material and the continuous fiber reinforced resin composite material (prepreg) in this order in a molding die having a predetermined shape and performing a cooling press; (B3) after the (B2) step, a step of cooling the thermoplastic resin to a temperature equal to or lower than the melting point thereof to obtain a floor cross member as a molded product composed of a continuous fiber reinforced resin composite material and a random fiber reinforced material; (B4) a step of heating the continuous fiber reinforced resin composite material (prepreg) and the random fiber reinforced material obtained in the step (B1) to a temperature equal to or higher than the melting point of the thermoplastic resin by a heater or oven, and then arranging the random fiber reinforced material and the continuous fiber reinforced resin composite material (prepreg) in this order in a molding die having a predetermined shape and performing a cooling press; (B5) after the step (B4), a step of cooling the thermoplastic resin to a temperature equal to or lower than the melting point thereof to obtain a battery cover body as a molded product composed of a continuous fiber reinforced resin composite material and a random fiber reinforced material; (B6) a step of joining the battery cover body obtained in the step (B5) and the floor cross member obtained in the step (B3); It can also be produced by a production method including the steps of: In this case, a battery cover is obtained in which the floor cross member has a rib structure and the battery cover body has a rib structure.
[0083] As described above, it is preferable to use, as the continuous reinforcing fiber, a continuous reinforcing fiber to which a sizing agent containing a coupling agent, a binder, and a lubricant is added, and it is preferable to use, as the thermoplastic resin, a thermoplastic resin having a terminal functional group reactive with the coupling agent.
[0084] Moreover, additives (such as a flame retardant) may be blended in advance into the thermoplastic resin.
[0085] The method of hot pressing when obtaining a continuous reinforced fiber resin composite (prepreg) is not particularly limited, but from the viewpoint of productivity, a hot pressing method using a double belt press is preferred. At this time, the base material constituting the continuous reinforced fiber resin composite may be fed by unloading reinforcing fibers and thermoplastic resin from multiple rolls and feeding them into a double belt press device, or a desired number of reinforcing fibers and thermoplastic resin cut to a desired size may be stacked and fed. In addition, at this time, guide sheets (for example, Teflon (registered trademark) sheets) may be fed together in front of and behind the base material.
[0086] Specifically, the cold pressing method for obtaining the battery cover body and the floor cross member can be, for example, to cut the substrate constituting the continuous reinforced fiber resin composite material according to the desired molded body, stack the required number of sheets in consideration of the thickness of the target product, and set according to the shape of the mold. The substrate can be cut one by one, or after stacking the desired number of sheets. From the viewpoint of productivity, it is preferable to cut in a stacked state. The cutting method can be any method, and for example, cutting can be performed using a water jet, a blade press machine, a hot blade press machine, a laser, a plotter, etc. The appropriate cutting shape can be adjusted by repeating trial and error, but it is preferable to set it by performing simulations using CAE (computer aided engineering) in accordance with the shape of the mold.
[0087] After the substrate is set in the mold, the mold is closed and pressed (compressed). The temperature of the mold is then adjusted to a temperature below the melting point of the thermoplastic resin constituting the continuous reinforced fiber resin composite (prepreg) to solidify the thermoplastic resin and form it. The mold clamping pressure is not particularly limited, but is preferably 1 MPa or more, more preferably 3 MPa or more. From the viewpoint of warping of the molded product, the longer the compression molding time, the better, but from the viewpoint of productivity, it is preferably within 2 minutes, more preferably within 1 minute.
[0088] Methods for joining the battery cover body and the floor cross member include adhesion with an adhesive, mechanical fastening such as bolt fastening or rivet fastening, and the like.
[0089] It is preferable that the floor cross member has many fastening points with the vehicle body frame. In this case, the rigidity of the battery cover can be further improved. More specifically, it is preferable that the number of fastening points with the vehicle body frame of the floor cross member is 50 or more. EXAMPLES
[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0091] (Example 1-1) [Preparation of continuous reinforcing fibers] As the continuous reinforcing fiber, a glass fiber with a fineness of 11,500 dtex and 2,000 single fibers was prepared with 0.45% by mass of a sizing agent attached. The winding form was a direct wind roving (DWR), and the average single fiber diameter was 17 μm. The above-mentioned sizing agent was prepared by copolymerizing 0.5 mass% of γ-aminopropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBE-903") as a coupling agent, 1 mass% of a lubricant (carnauba wax), 2 mass% of a polyurethane resin (manufactured by ADEKA Corporation, "Y65-55") as a binding agent, 40 mass% of maleic anhydride, 50 mass% of methyl acrylate, and 10 mass% of methyl methacrylate, and preparing the copolymerized compound having a weight-average molecular weight of 20,000 at 3 mass% and the copolymerized compound aqueous solution at 3 mass% with deionized water.
[0092] The glass fibers were used as warp and weft yarns to produce a glass cloth using a rapier loom (weaving width: 2 m). The weaving form of the obtained glass cloth was plain weave, the weaving density was 6.5 threads / 25 mm, and the basis weight was 600 g / m 2 It was.
[0093] [Preparation of thermoplastic resin film] As a thermoplastic resin, polyamide 66 ("Leona 1300S" manufactured by Asahi Kasei Corporation, melting point 265°C, carboxyl end group number 70μmol / g, amino end group 32μmol / g) was prepared, and this thermoplastic resin was molded with a T-die extrusion molding machine (manufactured by Soken Co., Ltd.) to obtain a film. The thickness of the film was 100μm.
[0094] [Preparation of samples for strength testing] Five sheets of glass cloth and six sheets of thermoplastic resin film were stacked and molded (heat-pressed) using a specified molding machine (mold). Next, the mold was quenched and then opened, and the obtained flat continuous reinforced fiber resin composite material (prepreg) (floor cross member intermediate, thickness 2.2 mm) was taken out. The molding time was 1 minute after reaching 265°C, the melting point of polyamide 66, and the maximum temperature during molding was 285°C.
[0095] Next, the floor cross member intermediate and the random fiber reinforcement (material for obtaining a rib structure, containing the same thermoplastic resin as the continuous fiber reinforced resin composite material) were heated by a heater to above the melting point of the thermoplastic resin (polyamide 66), and then the random fiber reinforcement and the floor cross member intermediate were placed in this order in a molding die having a predetermined shape and cold pressed. Next, it was cooled to a temperature below the melting point of the thermoplastic resin (polyamide 66), and a floor cross member with a rib structure formed in the opening as shown in Figure 4 was obtained. The temperature of the molding die was in the range of 90°C to 150°C.
[0096] In producing the above floor cross member, the orientation direction of the glass fibers was set at 0 degrees and 90 degrees to the longitudinal direction of the floor cross member.
[0097] On the other hand, a battery cover body equivalent was obtained as a flat continuous fiber-reinforced resin composite material (prepreg) as described above. In producing the battery cover body equivalent, the orientation direction of the glass fiber was set to 0 degrees and 90 degrees with respect to the longitudinal direction of the battery cover body equivalent.
[0098] Next, this battery cover body equivalent was joined to the floor cross member obtained above by rivet fastening (blind rivet) to produce a strength test sample having the cross-sectional shape shown in Figure 2. The mass of the obtained strength test sample was 0.29 kg (not including the rivets).
[0099] (Example 1-2) A strength test sample was prepared in the same manner as in Example 1-1, except that a rib structure was not formed in the opening of the floor cross member in Example 1-1. The mass of the obtained strength test sample was 0.23 kg (not including the rivet).
[0100] (Example 2-1) A strength test sample was prepared in the same manner as in Example 1-1, except that the orientation direction of the glass fiber in the floor cross member was set to 45 degrees and 135 degrees with respect to the longitudinal direction of the floor cross member. The mass of the obtained strength test sample was 0.29 kg (not including the rivets).
[0101] (Example 2-2) A strength test sample was prepared in the same manner as in Example 2-1, except that a rib structure was not formed in the opening of the floor cross member in Example 2-1. The mass of the obtained strength test sample was 0.23 kg (not including the rivet).
[0102] Comparative Example 1 A floor cross member having the same shape as the above-mentioned example was fabricated using 780MPa high tensile steel (thickness 0.8mm), and these were joined by spot welding to fabricate a strength test sample having the same shape as the above-mentioned example. The mass of the obtained strength test sample was 0.34kg.
[0103] <Load-displacement curve> Load-displacement curves were created by a three-point bending test for the strength test samples of Example 1-1, Example 1-2, Example 2-1, Example 2-2, and Comparative Example 1. The load-displacement curves of Example 1-1 and Example 1-2 (examples in which the fiber orientation directions are 0 degrees and 90 degrees) and Comparative Example 1 are shown in Figure 5, and the load-displacement curves of Example 2-1 and Example 2-2 (examples in which the fiber orientation directions are 45 degrees and 135 degrees) and Comparative Example 1 are shown in Figure 6. In these figures, the maximum load is an index of strength, the slope is an index of rigidity (elastic modulus), and the integral value of the load-displacement curve is an index of the amount of absorbed energy.
[0104] 5 and 6, it can be seen that the strength test samples of the Examples are superior in strength and rigidity to the strength test samples of the Comparative Examples. In particular, it can be seen that, as in Examples 1-1 and 2-1, by forming a rib structure in the area of the closed cross-sectional structure formed by the battery cover body and the floor cross member, the strength, rigidity, and amount of absorbed energy (impact resistance) are effectively improved with only a slight increase in mass.
[0105] Example 3 In Example 3, a thermoplastic resin foam was formed within the opening of the strength test sample in Example 1-1 to obtain a strength test sample having a thermoplastic resin foam in a closed cross-sectional structure region as shown in Figure 3.
[0106] <Three-point bending test> A three-point bending test was performed to measure the amount of energy absorption for the strength test samples of Example 3 and Comparative Example 1. As a result, the amount of energy absorption per unit mass of Example 3 was 1.7 times that of Comparative Example 1.
[0107] <Drop weight test> A drop weight test was carried out on the strength test samples of Example 3 and Comparative Example 1 under the conditions of a 20 kg weight and a drop height of 5 m. As a result, the amount of displacement during energy absorption was (Example 3) < (Comparative Example 1). The smaller this value, the smaller the energy absorption is possible with a smaller displacement (excellent impact resistance).
[0108] (Estimated total weight of battery cover) The components for storing a conventional battery are assumed to be one battery cover (upper case under the floor panel), one floor panel, and 20 floor cross member parts. Based on the CAD drawings and the type of metal material (steel), the total weight was estimated to be 47 kg. On the other hand, assuming that the components of the multifunctional battery cover of the present invention are one battery cover body made of continuous reinforced fiber resin composite material and five floor cross members made of continuous reinforced fiber resin composite material, the total weight is estimated to be 28 kg. From the above, it is expected that the multifunctional battery cover of the present invention can reduce the number of parts and achieve a weight reduction of about 20 kg compared to conventional products. [Industrial Applicability]
[0109] According to the present invention, it is possible to provide a multi-functional battery cover for automobiles that is lightweight, has excellent impact resistance while maintaining the rigidity of the vehicle body, and can be manufactured at low cost. [Explanation of symbols]
[0110] 1 Battery cover 11 Battery cover body 12Floor cross member 15 Closed section 17 Thermoplastic resin foam 18 Rib structure
Claims
1. A multi-function battery cover for a car, comprising: A battery cover body and a plurality of floor cross members joined to the battery cover body and configured to extend in one direction, The battery cover body and the floor cross member are made of a continuous reinforced fiber resin composite material containing a fiber bundle including continuous reinforced fiber and a thermoplastic resin, and the battery cover body also functions as a floor panel that constitutes the floor surface of the vehicle compartment. A multi-functional battery cover.
2. The multi-function battery cover according to claim 1 , wherein the battery cover body and the floor cross member form a closed cross-sectional structure.
3. The multi-functional battery cover according to claim 1 or 2, wherein the floor cross member further comprises a rib structure made of a thermoplastic resin.
4. The multi-functional battery cover according to claim 3, wherein in the floor cross member, the thermoplastic resin constituting the continuous reinforced fiber resin composite material and the thermoplastic resin constituting the rib structure are the same resin.
5. The multi-functional battery cover according to claim 1 or 2, wherein the battery cover body further comprises a rib structure made of a thermoplastic resin.
6. The multifunctional battery cover according to claim 5, wherein in the battery cover main body, the thermoplastic resin constituting the continuous reinforced fiber resin composite material and the thermoplastic resin constituting the rib structure are the same resin.
7. The multi-functional battery cover according to claim 3 , wherein the battery cover body further comprises a rib structure made of a thermoplastic resin.
8. The multifunctional battery cover according to claim 7, wherein in the battery cover main body, the thermoplastic resin constituting the continuous reinforced fiber resin composite material and the thermoplastic resin constituting the rib structure are the same resin.
9. The multi-functional battery cover according to claim 2 , further comprising a thermoplastic resin foam in the area of the closed cross-sectional structure.
10. The multi-functional battery cover according to claim 1 or 2, wherein the continuous reinforcing fibers include glass fibers.
Citation Information
Patent Citations
Vehicle body structure and vehicle
CN110329362A
Protective member for battery structure of electric vehicle
CN115427245A
Battery pack case assembly for electric vehicle and method for manufacturing the same
JP2013201112A
Lower structure of vehicle body for electric vehicle
JP2021120244A
Automotive Vehicle Structure
JP2022516047A