Anode catalyst, water electrolysis cell, and water electrolysis cell stack
A perovskite-structured anode catalyst with specific ion compositions enhances the durability and longevity of water electrolysis cells by stabilizing the catalyst structure under oxidative conditions.
Patent Information
- Application Number
- JP2023085750
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-24
AI Technical Summary
Anode catalysts used in water electrolysis are prone to degradation due to dissolution in the strong oxidizing atmosphere, leading to a shortened lifespan, particularly those containing elements like ruthenium and iridium.
An anode catalyst with a perovskite structure containing alkaline earth metal ions, tetravalent metal ions, and iridium ions, along with transition metal element ions, such as manganese, nickel, copper, iron, or cobalt, is developed to enhance stability and longevity.
The proposed anode catalyst exhibits improved durability and longevity by stabilizing the perovskite structure, maintaining high catalytic activity under oxidative conditions.
Smart Images

Figure 2024168800000002 
Figure 2024168800000003 
Figure 2024168800000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an anode catalyst, a water electrolysis cell, and a water electrolysis cell stack. [Background technology]
[0002] Water electrolysis (hereinafter sometimes referred to as "water electrolysis") is a method for producing hydrogen and oxygen from water by electrolysis. For example, among technologies that utilize hydrogen as an energy source, water electrolysis is a promising technology for sustainable hydrogen production.
[0003] A water electrolysis cell used for water electrolysis includes an anode separator, an anode gas diffusion layer, an anode catalyst, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, a cathode separator, etc. Regarding the anode catalyst and cathode catalyst, catalysts suitable for water electrolysis are being studied.
[0004] For example, Patent Document 1 discloses PdRu solid solution nanoparticles containing palladium (Pd) and ruthenium (Ru), and discloses that the nanoparticles are used as a catalyst for water electrolysis reactions. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2018 / 159644 Summary of the Invention [Problem to be solved by the invention]
[0006] Anode catalysts containing elements having anode activity such as ruthenium and iridium have high catalytic activity. However, since the anode catalyst is exposed to a strong oxidizing atmosphere during water electrolysis, elements such as ruthenium and iridium are easily dissolved, and the life of anode catalysts containing such elements is easily shortened.
[0007] For example, in a water electrolysis catalyst containing ruthenium as disclosed in Patent Document 1, ruthenium is easily dissolved, and there is a risk that the catalyst will have a short life.
[0008] An object of the present disclosure is to provide an anode catalyst having a long life, and a water electrolysis cell and a water electrolysis cell stack including the same. [Means for solving the problem]
[0009] The present disclosure includes the following aspects. <1> An anode catalyst comprising an oxide having a perovskite structure, the oxide further comprising a transition metal element ion, the oxide having an alkaline earth metal ion as an A site ion and a tetravalent metal ion and an iridium ion as a B site ion, the molar concentration of the iridium ion being 30 mol % or more. <2> The alkaline earth metal ions include strontium ions. <1> The anode catalyst according to claim 1, <3> The tetravalent metal ion includes a titanium ion. <1> or <2> The anode catalyst according to claim 1, <4> The transition metal element ions include at least one type of ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions. <1> ~ <3> 13. The anode catalyst according to claim 12, <5> The ratio of the number of moles of the transition metal element ion to the sum of the number of moles of the transition metal element ion and the tetravalent metal ion is 5% or more and 91% or less. <1> ~ <4> 13. The anode catalyst according to claim 12, <6> The ratio of the number of moles of the transition metal element ion to the sum of the number of moles of the transition metal element ion and the tetravalent metal ion is 14% or more and 82% or less. <1> ~ <4> 13. The anode catalyst according to claim 12, <7> The ratio of the number of moles of the transition metal element ion to the sum of the number of moles of the transition metal element ion and the tetravalent metal ion is 21% or more and 75% or less. <1> ~ <4> 13. The anode catalyst according to claim 12, <8> an anode gas diffusion layer; <1> ~ <7> A water electrolysis cell comprising the anode catalyst according to any one of the above items, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, and a separator. <9> <8> A water electrolysis cell stack in which a plurality of water electrolysis cells according to the above item are stacked. Effect of the Invention
[0010] According to the present disclosure, there is provided a long-life anode catalyst, and a water electrolysis cell and a water electrolysis cell stack including the same. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of a water electrolysis cell. [Diagram 2] FIG. 2 is a graph showing the relationship between the transition metal element ion ratio and the current density maintenance rate in each of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present disclosure will be described. The present disclosure is not limited to the following embodiments, and can be implemented with appropriate modifications within the scope of the object of the present disclosure. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.
[0013] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0014] In the present disclosure, the upper limit value described in a certain numerical range may be replaced with the upper limit value of another numerical range described in a certain numerical range, and the lower limit value described in a certain numerical range may be replaced with the lower limit value of another numerical range described in a certain numerical range. In the present disclosure, the upper limit value or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.
[0015] In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.
[0016] <Anode catalyst> The anode catalyst of the present disclosure includes an alkaline earth metal ion in the A site ion, a tetravalent metal ion (hereinafter also referred to as a specific metal ion) and an iridium ion in the B site ion, the molar concentration of the iridium ion is 30 mol% or more, and the oxide includes an oxide having a perovskite structure, and the oxide further includes a transition metal element ion. The anode catalyst of the present disclosure tends to have a long life by including the oxide having the perovskite structure described above. The reason for this is presumed to be that the molar concentration of the iridium ion is 30 mol% or more, and the oxide includes a transition metal element ion, which favorably exerts the effect of stabilizing the perovskite structure of the oxide. Note that the present disclosure is not limited to the following presumption. In the present disclosure, the molar concentration of iridium ions means the molar concentration of iridium ions relative to the total molar concentration of iridium ions, tetravalent metal ions, and transition metal element ions.
[0017] The oxide having a perovskite structure containing an alkaline earth metal ion as the A site ion, a specific metal ion and an iridium ion as the B site ion, and further containing a transition metal element ion can be produced by a conventionally known method. For example, the oxide having the perovskite structure can be produced by a conventionally known solid phase method, liquid phase method, etc. The solid phase method includes a method of direct reaction of solid raw materials, and the liquid phase method includes the Pezzini method, the complex polymerization method, the hydrothermal synthesis method, etc.
[0018] The anode catalyst of the present disclosure includes an oxide having a perovskite structure. The oxide having a perovskite structure is generally represented by the chemical formula ABO3. Some oxides having a perovskite structure have oxygen indeterminacy. The amount of oxygen may be deficient or excessive compared to 3. In addition, the A-site ions and the B-site ions may be partially substituted with different elements. Whether or not the anode catalyst has a perovskite structure can be analyzed by X-ray diffraction measurement (XRD).
[0019] The A-site ions of the perovskite structure include alkaline earth metal ions. Examples of alkaline earth metal ions include calcium ions, strontium ions, barium ions, and radium ions. In the present disclosure, the alkaline earth metal ions that are the A-site ions preferably include at least one selected from the group consisting of strontium ions, calcium ions, and barium ions, and more preferably include strontium ions. The A-site ions may be one type of alkaline earth metal ion, or may be two or more types of alkaline earth metal ions. For example, the A-site ions may be only strontium ions, or may be a combination of strontium ions and one or more other alkaline earth metal ions.
[0020] The B-site ions in the perovskite structure include a specific metal ion and an iridium ion.
[0021] The specific metal ion is not particularly limited as long as it is a tetravalent metal ion, and examples thereof include at least one selected from a zirconium ion and a titanium ion, and it is preferable to include a titanium ion.
[0022] The oxide having a perovskite structure further contains transition metal element ions. For example, the transition metal element ions may be contained in A-site ions, B-site ions, or may be located on the oxide surface. When a transition metal element ion is included in the B site ions and the transition metal element ion is a tetravalent metal ion, the tetravalent transition metal element ion is classified as a specific metal ion rather than a transition metal element ion.
[0023] Examples of transition metal element ions include ions of elements present between Group 3 and Group 12 of the periodic table (excluding specific metal ions and iridium ions). Examples of such ions include scandium (Sc), yttrium (Y), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn). It is more preferable that the transition metal element ion is at least one ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions. The transition metal element ions contained in the oxide may be one type of transition metal element ion, or may be two or more types of transition metal element ions.
[0024] The transition metal element ions preferably include at least one type of ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions.
[0025] The B site ions may or may not contain other ions other than the specific metal ions and iridium ions. When the B site ions contain other ions, the other ions may include the above-mentioned transition metal element ions, gallium (Ga), indium (In), tin (Sn), antimony (Sb), and the like.
[0026] In the anode catalyst of the present disclosure, it is preferred that the A-site ions include alkaline earth metal ions and the B-site ions include titanium ions and iridium ions.
[0027] The molar concentration of iridium ions relative to the total molar concentration of iridium ions, tetravalent metal ions, and transition metal element ions is preferably 30 mol % or more, and more preferably 35 mol % or more. The molar concentration may be 70 mol % or less, or may be 50 mol % or less.
[0028] From the viewpoint of extending the life of the anode catalyst, the ratio of the number of moles of the transition metal element ion to the sum of the number of moles of the transition metal element ion and the specific metal ion (preferably titanium ion) is preferably 5% or more and 91% or less, more preferably 14% or more and 82% or less, and even more preferably 21% or more and 75% or less.
[0029] The molar concentration of iridium and the ratio of the above molar numbers to the total molar concentration of iridium ions, tetravalent metal ions, and transition metal element ions can be determined by analyzing the anode catalyst using inductively coupled plasma (ICP). In addition, the metal concentrations can be quantitatively evaluated by imaging the catalyst powder and performing elemental analysis using a scanning electron microscope (SEM) and energy dispersive X-ray spectroscopy (EDS).
[0030] The anode catalyst of the present disclosure contains alkaline earth metal ions as A-site ions, tetravalent metal ions and iridium ions as B-site ions, the molar concentration of the iridium ions is 30 mol% or more, has a perovskite structure, and may further contain components other than the oxide containing transition metal element ions. For example, the components may include components having catalytic activity other than the oxide having a perovskite structure, unreacted components of the raw materials used to generate the oxide having a perovskite structure, and side reaction components.
[0031] The content of the oxide having a perovskite structure in the anode catalyst of the present disclosure is not particularly limited, and is preferably 50 mass% to 100 mass%, more preferably 70 mass% to 100 mass%, and further preferably 90 mass% to 100 mass%, relative to the total amount of the anode catalyst.
[0032] <Water electrolysis cell> The water electrolysis cell according to the present disclosure includes an anode gas diffusion layer, the anode catalyst according to the present disclosure described above, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, and a separator.
[0033] The anode gas diffusion layer, electrolyte membrane, cathode catalyst, cathode gas diffusion layer and separator may be members used in conventional water electrolysis cells.
[0034] The water electrolysis cell may further include other components. The other components may be selected from known components of water electrolysis cells. Examples of the other components include a gasket, a sealant, and the like.
[0035] For example, the anode gas diffusion layer and the cathode gas diffusion layer may each independently be made of a material that allows fluid to flow through the layer, such as a porous material, a powder sintered material, a fiber sintered material, a metal mesh, or felt.
[0036] The anode gas diffusion layer may be coated with a corrosion-resistant conductive material to prevent the layer from becoming highly resistive due to oxidation. Examples of the coating material include platinum, gold, silver, titanium nitride, titanium carbide, and titanium carbonitride.
[0037] The electrolyte membrane may be selected from known electrolyte membranes (which may be ion exchange membranes) used in water electrolysis. The electrolyte membrane is a membrane that can exchange protons (H + ) is preferably selectively permeable. Examples of the electrolyte membrane include polymer electrolyte membranes (PEM). Examples of the polymer electrolyte membrane include perfluorocarbon membranes having sulfonic acid groups. Examples of the perfluorocarbon membranes having sulfonic acid groups include Nafion membranes.
[0038] The electrolyte membrane is a polymer having proton conductivity due to the presence of ionic groups, and may be, for example, either a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte.
[0039] Here, the fluorine-based polymer electrolyte refers to one in which most or all of the hydrogen atoms in the alkyl and / or alkylene groups in the polymer are replaced with fluorine atoms. Representative examples of fluorine-based polymer electrolytes having ionic groups include commercially available products such as "Nafion" (registered trademark) (manufactured by Chemours), "Aquivion" (registered trademark) (manufactured by Solvay), "Flemion" (registered trademark) (manufactured by AGC Corporation), and "Aciplex" (registered trademark) (manufactured by Asahi Kasei Corporation).
[0040] The hydrocarbon-based polymer electrolyte is preferably an aromatic hydrocarbon-based polymer having an aromatic ring in the main chain. Here, the aromatic ring may include not only a hydrocarbon-based aromatic ring consisting of only carbon atoms and hydrogen atoms such as a benzene ring or a naphthalene skeleton, but also a heterocycle such as a pyridine ring, an imidazole ring, or a thiol ring. In addition, a part of the polymer may be composed of an aliphatic unit together with the aromatic ring unit.
[0041] Specific examples of aromatic hydrocarbon polymers include polymers having a structure selected from polysulfone, polyethersulfone, polyphenylene oxide, polyarylene ether, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone in the main chain together with an aromatic ring. Note that polysulfone, polyethersulfone, polyether ketone, etc. referred to here are general terms for structures having sulfone bonds, ether bonds, ketone bonds, etc. in the molecular chain, and include polyether ketone ketone, polyether ether ketone, polyether ether ketone ketone, polyether ketone ether ketone ketone, and polyether ketone sulfone. The aromatic hydrocarbon polymer may have a plurality of these structures. Among these, the aromatic hydrocarbon polymer is preferably a polymer having a polyetherketone skeleton, that is, a polyetherketone polymer.
[0042] The electrolyte membrane may be combined with a reinforcing material, which, for example, can reduce the risk of gas leakage or short circuiting within the electrodes due to damage to the membrane when the electrolyte membrane and the electrodes are joined by hot pressing.
[0043] Specific examples of reinforcing materials include homogeneous porous films made of fluorine-based polymers such as PTFE (polytetrafluoroethylene), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), PVDF (polyvinylidene fluoride), and FEP (tetrafluoroethylene-hexafluoropropylene copolymer); thermoplastic resins such as PE (polyethylene) and PP (polypropylene); and engineering plastics such as PI (polyimide), PSF (polysulfone), PES (polyethersulfone), PEEK (polyetheretherketone), PPSS (polyphenylene sulfide sulfone), PPO (polyphenylene oxide), PEK (polyetherketone), PBI (polybenzimidazole), PPS (polyphenylene sulfide), PPP (polyparaphenylene), PPQ (polyphenylquinoxaline), polybenzoxazole (PBO), polybenzothiazole (PBT), and polyparaphenylene terephthalamide (PPTA).
[0044] The cathode catalyst may be selected from known catalysts used in water electrolysis. Examples of catalyst components include platinum, gold, silver, palladium, iridium, rhodium, ruthenium, tin, iron, cobalt, nickel, molybdenum, tungsten, vanadium, and alloys and oxides thereof. The catalyst may be in the form of particles. The anode catalyst may also include a catalyst supported on a carrier. Examples of the carrier include titanium oxide and tin oxide. The cathode catalyst may also include a catalyst supported on a carrier. Examples of the carrier include carbon black.
[0045] The water electrolysis cell may include an anode catalyst layer containing an anode catalyst (preferably anode catalyst particles) and an ionomer, or may include a cathode catalyst layer containing a cathode catalyst (preferably cathode catalyst particles) and an ionomer, which increases the contact area between the catalyst and the ionomer in the catalyst layer and tends to promote the reaction.
[0046] The primary particle diameter of the anode catalyst is preferably 1 nm to 10 μm, more preferably 2 nm to 1 μm, and even more preferably 5 nm to 100 nm. When the primary particle diameter of the anode catalyst is 1 nm or more, the mixing ratio of the ionomer required to increase the contact area is not too large, and many electron conduction paths can be secured inside the anode catalyst layer, so that the resistance tends to be difficult to increase. When the primary particle diameter of the anode catalyst is 10 μm or less, the decrease in the contact area with the ionomer is suppressed, so that the resistance tends to be difficult to increase.
[0047] The separator may be an anode separator disposed on the anode gas diffusion layer side, or a cathode separator disposed on the cathode gas diffusion layer side. Examples of the material for the separator include titanium, stainless steel, carbon, etc. From the viewpoint of suppressing oxidation due to oxygen generated on the anode side, the anode separator preferably contains titanium.
[0048] The anode separator may be coated with a corrosion-resistant conductive material to prevent the anode separator from becoming highly resistive due to oxidation. Examples of the coating material include platinum, gold, silver, titanium nitride, titanium carbide, and titanium carbonitride.
[0049] The arrangement of each component in the water electrolysis cell may be determined with reference to known water electrolysis cells. In the water electrolysis cell, the electrolyte membrane is preferably located between the anode catalyst and the cathode catalyst. In the water electrolysis cell, the electrolyte membrane, the anode catalyst, and the cathode catalyst are preferably located between the anode gas diffusion layer and the cathode gas diffusion layer. In the water electrolysis cell, the electrolyte membrane, the anode catalyst, the cathode catalyst, and the anode gas diffusion layer and the cathode gas diffusion layer are preferably located between two separators.
[0050] The anode catalyst layer or the cathode catalyst layer may be mixed with an ionomer and a solvent to form a slurry, which may then be applied to an electrolyte membrane to form an electrolyte membrane with a catalyst layer. Alternatively, the catalyst layer may be applied to a film such as a Teflon (registered trademark) sheet, and then transferred to the electrolyte membrane. The catalyst layer may be applied to a gas diffusion layer to form a gas diffusion electrode. Apparatuses for applying the catalyst layer slurry include spray coaters, comma coaters, die coaters, reverse roll coaters, gravure coaters, bar coaters, dip coaters, slit coaters, and lip coaters.
[0051] An example of a water electrolysis cell is shown in Fig. 1. Fig. 1 is a schematic cross-sectional view of a water electrolysis cell. As shown in Fig. 1, a water electrolysis cell 100 includes, in order from the top of Fig. 1, an anode separator 60, an anode gas diffusion layer 20, an anode catalyst 12, an electrolyte membrane 11, a cathode catalyst 13, a cathode gas diffusion layer 30, and a cathode separator 70. Furthermore, a gasket 40 is disposed between the anode separator 60 and the electrolyte membrane 11, and a gasket 50 is disposed between the cathode separator 70 and the electrolyte membrane 11.
[0052] <Water electrolysis device> The water electrolysis device according to the present disclosure may be a water electrolysis cell stack formed by stacking a plurality of the above-described water electrolysis cells according to the present disclosure, or may be a device including the water electrolysis cell stack or the water electrolysis cell according to the present disclosure and other components.
[0053] The other components may be selected from known components of a water electrolysis device, such as auxiliary devices including a power conditioner, a water pump, an ion exchange resin, a heat exchanger, and a dehumidifier. EXAMPLES
[0054] The present disclosure will be described in detail below with reference to examples. However, the present disclosure is not limited to the following examples. The matters shown in the following examples may be appropriately changed without departing from the spirit of the present disclosure.
[0055] <Example 1> Using the Pezzini method, a catalyst powder containing oxides with a perovskite structure was obtained by incorporating iridium ions and manganese ions into strontium titanate (SrTiO3). The starting materials were strontium carbonate (SrCO3), titanium tetrabutoxide (C 16 H 36 The materials used were O4Ti), potassium hexachloroiridate (K2IrCl6) and manganese nitrate hexahydrate. Manganese nitrate hexahydrate was weighed out so that the manganese ion concentration was 4M (mol / L) and dissolved in water to prepare an aqueous solution. The concentration of the manganese nitrate aqueous solution was analyzed by ICP. 0.2794g of SrCO3, 0.0800g of K2IrCl6, 17.7μL of manganese nitrate aqueous solution, 0.2800g of citric acid monohydrate (C6H8O7·H2O) and 0.3mL of nitric acid (1.38) were weighed out and added to 10mL of pure water, mixed, and dissolved by stirring at room temperature for more than 10 minutes. This mixed solution was named solution A. C 16 H 360.081g of O4Ti was weighed out and mixed with 4mL of ethylene glycol (C2H6O2), and the mixture was stirred for 10 minutes or more. This mixed solution was named solution B. After adding solution A to solution B, the mixture was stirred and mixed at 70°C for 3 hours or more using a hot stirrer. The mixed solution was then transferred to a zirconia crucible and heat-treated at 180°C for 12 hours, 200°C for 6 hours, 300°C for 6 hours, 500°C for 3 hours, and 600°C for 6 hours. The powder after the heat treatment was collected and put into a beaker together with 50mL of 1M hydrochloric acid solution and stirred for 3 hours or more to remove unreacted components. The obtained mixed solution was washed with water using a suction filter and dried in an oven at 60°C to obtain a catalyst powder. When X-ray diffraction measurement was performed on the synthesized catalyst powder, a diffraction pattern derived from a perovskite structure was obtained. The composition of the obtained powder was analyzed by FE-SEM / EDS. The powder composition was applied onto a carbon tape, and the atomic concentrations of iridium, titanium and manganese were evaluated by mapping analysis in three fields of view magnified 10,000 times, and the average atomic concentration of each element was defined as the concentration of the element. As a result, the molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions and manganese ions was 35 mol%, and the ratio of the number of moles of the transition metal element ions (manganese ions in Example 1) to the sum of the number of moles of the transition metal element ions and titanium ions (hereinafter also referred to as the "manganese ion ratio", which corresponds to the transition metal element ion ratio in Table 1) was 7.8%.
[0056] <Example 2> The manganese ions incorporated into the synthesized SrTiO3 were adjusted to a manganese ion ratio of 11.8% by adding 35.5 μL of manganese nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0564 g.
[0057] <Example 3> The manganese ions incorporated into the synthesized SrTiO3 were adjusted to a manganese ion ratio of 19.1% by adding 47.3 μL of manganese nitrate solution and C16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0401 g.
[0058] <Example 4> The manganese ions incorporated into the synthesized SrTiO3 were adjusted to a manganese ion ratio of 26.7% by adding 59.1 μL of manganese nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0242 g.
[0059] <Example 5> The manganese ions incorporated into the synthesized SrTiO3 were adjusted to a manganese ion ratio of 37.4% by adding 71.0 μL of manganese nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0080 g.
[0060] <Example 6> A catalyst powder containing an oxide having a perovskite structure in which iridium ions and nickel ions are incorporated into SrTiO3 was obtained by the Pezzini method in the same manner as in Example 1, except that nickel ions were incorporated instead of manganese ions as the transition metal element ions. The starting materials were SrCO3, C 16 H 36 The nickel nitrate hexahydrate was weighed out so that the nickel ion concentration was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the nickel nitrate aqueous solution was analyzed by ICP. 0.2794g of SrCO3, 0.0800g of K2IrCl6, 17.7μL of nickel nitrate aqueous solution, 0.2800g of C6H8O7·H2O, and 0.3mL of nitric acid (1.38) were weighed out, added to 10mL of pure water, mixed, and stirred at room temperature for more than 10 minutes to dissolve. This mixed solution was named solution A. C 16 H 360.0805 g of O4Ti was weighed out and mixed with 4 mL of C2H6O2, and the mixture was stirred for 10 minutes or more. This mixed solution was designated as solution B. The subsequent operations were performed in the same manner as in Example 1 to recover the catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and nickel ions, determined in the same manner as in Example 1, was 35 mol%, and the ratio of the number of moles of the transition metal element ions (nickel ions in Example 6) to the sum of the number of moles of the titanium ions (hereinafter also referred to as the "nickel ion ratio") was 13.5%.
[0061] <Example 7> A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of nickel nitrate aqueous solution was changed to 35.5 μL so that the nickel ion ratio in the synthesized SrTiO3 was 17.9%.
[0062] <Example 8> The nickel ions incorporated into the synthesized SrTiO3 were adjusted to a nickel ion ratio of 19.6% by adding 35.5 μL of nickel nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0564 g.
[0063] <Example 9> The nickel ions incorporated into the synthesized SrTiO3 were adjusted to a nickel ion ratio of 60.3% by adding 59.1 μL of nickel nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0242 g.
[0064] <Example 10> The nickel ions incorporated into the synthesized SrTiO3 were adjusted to a nickel ion ratio of 80.1% by adding 71.0 μL of nickel nitrate solution and C 16 H36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0080 g.
[0065] <Example 11> A catalyst powder containing an oxide having a perovskite structure in which iridium ions and copper ions are incorporated into SrTiO3 was obtained by the Pechini method in the same manner as in Example 1, except that copper ions were incorporated instead of manganese ions as the transition metal element ions. The starting materials were SrCO3, C 16 H 36 The copper nitrate trihydrate was weighed out so that the copper ion concentration was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous copper nitrate solution was analyzed by ICP. 0.2794g of SrCO3, 0.0800g of K2IrCl6, 17.7μL of aqueous copper nitrate solution, 0.2800g of C6H8O7·H2O, and 0.3mL of nitric acid (1.38) were weighed out, added to 10mL of pure water, mixed, and stirred at room temperature for more than 10 minutes to dissolve. This mixed solution was named solution A. C 16 H 36 0.0805 g of O4Ti was weighed out and mixed with 4 mL of C2H6O2, and the mixture was stirred for 10 minutes or more. This mixed solution was designated as solution B. The subsequent operations were performed in the same manner as in Example 1 to recover the catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and copper ions, determined in the same manner as in Example 1, was 35 mol%, and the ratio of the number of moles of the transition metal element ions (copper ions in Example 11) to the sum of the number of moles of the titanium ions (hereinafter also referred to as the "copper ion ratio") was 19.4%.
[0066] <Example 12> The copper ions incorporated into the synthesized SrTiO3 were adjusted to a copper ion ratio of 22.2% by adding 35.5 μL of copper nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0564 g.
[0067] <Example 13> The copper ions incorporated into the synthesized SrTiO3 were adjusted to a copper ion ratio of 37.4% by adding 59.1 μL of copper nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0242 g.
[0068] <Example 14> The copper ions incorporated into the synthesized SrTiO3 were adjusted to a copper ion ratio of 46.2% by adding 71.0 μL of copper nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0080 g.
[0069] <Example 15> A catalyst powder containing an oxide having a perovskite structure in which iridium ions and iron ions are incorporated into SrTiO3 was obtained by the Pezzini method in the same manner as in Example 1, except that iron ions were incorporated instead of manganese ions as the transition metal element ions. 16 H 36 The samples were O4Ti, K2IrCl6, and iron nitrate nonahydrate. The iron nitrate nonahydrate was weighed out so that the iron ion concentration was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous iron nitrate solution was analyzed by ICP. 0.2794g of SrCO3, 0.0800g of K2IrCl6, 17.7μL of aqueous iron nitrate solution, 0.2800g of C6H8O7·H2O, and 0.3mL of nitric acid (1.38) were weighed out, added to 10mL of pure water, mixed, and stirred at room temperature for more than 10 minutes to dissolve. This mixed solution was named solution A. C 16 H 360.0805 g of O4Ti was weighed out and mixed with 4 mL of C2H6O2, and the mixture was stirred for 10 minutes or more. This mixed solution was designated as solution B. The subsequent operations were performed in the same manner as in Example 1 to recover the catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and iron ions, determined in the same manner as in Example 1, was 35 mol%, and the ratio of the number of moles of the transition metal element ions (iron ions in Example 15) to the sum of the number of moles of the titanium ions (hereinafter also referred to as the "iron ion ratio") was 10.1%.
[0070] <Example 16> The iron ion ratio of the synthesized SrTiO3 was 19.5%. 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0564 g.
[0071] <Example 17> The iron ion ratio of the synthesized SrTiO3 was 34.9%, so that 59.1 μL of iron nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0242 g.
[0072] <Example 18> The iron ions incorporated into the synthesized SrTiO3 were adjusted to a ratio of 50.5% by adding 71.0 μL of iron nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0080 g.
[0073] <Example 19> A catalyst powder containing an oxide having a perovskite structure in which iridium ions and cobalt ions are incorporated into SrTiO3 was obtained by the Pezzini method in the same manner as in Example 1, except that cobalt ions were incorporated instead of manganese ions as the transition metal element ions. 16 H 36 The cobalt nitrate hexahydrate was weighed out so that the concentration of cobalt ions was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous cobalt nitrate solution was analyzed by ICP. 0.2794 g of SrCO3, 0.0800 g of K2IrCl6, 17.7 μL of cobalt nitrate, 0.2800 g of C6H8O7·H2O, and 0.3 mL of nitric acid (1.38) were weighed out, added to 10 mL of pure water, mixed, and stirred at room temperature for more than 10 minutes to dissolve. This mixed solution was named solution A. C 16 H 36 0.0805 g of O4Ti was weighed out and mixed with 4 mL of C2H6O2, and the mixture was stirred for 10 minutes or more. This mixed solution was designated as solution B. The subsequent operations were performed in the same manner as in Example 1 to recover the catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and cobalt ions, determined in the same manner as in Example 1, was 35 mol%, and the ratio of the number of moles of the transition metal element ions (cobalt ions in Example 19) to the sum of the number of moles of the transition metal element ions and titanium ions (hereinafter also referred to as the "cobalt ion ratio") was 12.4%.
[0074] <Example 20> The cobalt ion ratio was adjusted to 20.8% by adding 35.5 μL of cobalt nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0564 g.
[0075] <Example 21> The cobalt ion ratio of the synthesized SrTiO3 was 62.3%. 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0242 g.
[0076] <Example 22> Regarding the cobalt ions incorporated into the synthesized SrTiO3, 71.0 μL of cobalt nitrate solution and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0080 g.
[0077] <Example 23> The molar concentration of iridium ions incorporated in the synthesized SrTiO3 was 67 mol% and the manganese ion ratio was 32.6%. To this end, 0.2920 g of SrCO3, 9.3 μL of manganese nitrate solution, and C 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of O4Ti was changed to 0.0152 g.
[0078] <Comparative Example 1> A catalyst powder containing an oxide having a perovskite structure in which iridium ions were incorporated into SrTiO3 was obtained by the Pezzini method in the same manner as in Example 1, except that no transition metal element ions were incorporated. The starting materials were SrCO3, C 16 H 36 The mixture was dissolved in 10 mL of pure water, stirred at room temperature for 10 minutes or more. The mixture was named Solution A. C 16 H 360.1048 g of O4Ti was weighed out and mixed with 4 mL of C2H6O2, and the mixture was stirred for 10 minutes or more. This mixed solution was designated as solution B. The subsequent operations were carried out in the same manner as in Example 1 to recover the catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and titanium ions, determined in the same manner as in Example 1, was 35 mol%.
[0079] <Comparative Example 2> A catalyst powder containing an oxide having a perovskite structure in which iridium ions were incorporated into the B-site ions of strontium manganate (SrMnO3) was obtained by the Pechini method in the same manner as in Example 1, except that titanium ions were not incorporated into the B-site ions. The starting materials were SrCO3, K2IrCl6, and manganese nitrate hexahydrate. Manganese nitrate hexahydrate was weighed so that the concentration of manganese ions was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous manganese nitrate solution was analyzed by ICP. 0.2794 g of SrCO3, 0.0800 g of K2IrCl6, 76.9 μL of aqueous manganese nitrate, 0.2800 g of C6H8O7·H2O, and 0.3 mL of nitric acid (1.38) were weighed, introduced into 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was named solution A. Using only solution A, the subsequent operations were carried out in the same manner as in Example 1 to recover a catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and manganese ions, determined in the same manner as in Example 1, was 35 mol %, and the proportion of manganese ions was 100%.
[0080] <Comparative Example 3> A catalyst powder containing an oxide having a perovskite structure in which iridium ions were incorporated into the B-site ions of strontium nickel oxide (SrNiO3) was obtained by the Pechini method in the same manner as in Example 6, except that titanium ions were not incorporated into the B-site ions. The starting materials were SrCO3, K2IrCl6, and nickel nitrate hexahydrate. Nickel nitrate hexahydrate was weighed so that the nickel ion concentration was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the nickel nitrate aqueous solution was analyzed by ICP. 0.2794 g of SrCO3, 0.0800 g of K2IrCl6, 76.9 μL of nickel nitrate aqueous solution, 0.2800 g of C6H8O7·H2O, and 0.3 mL of nitric acid (1.38) were weighed, introduced into 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was named solution A. Using only solution A, the subsequent operations were carried out in the same manner as in Example 1 to recover a catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and nickel ions, which were determined in the same manner as in Example 1, was 35 mol %, and the proportion of nickel ions was 100%.
[0081] <Comparative Example 4> A catalyst powder containing an oxide having a perovskite structure in which iridium ions were incorporated into the B-site ions of strontium cuprate (SrCuO3) was obtained by the Pechini method in the same manner as in Example 11, except that titanium ions were not incorporated into the B-site ions. The starting materials were SrCO3, K2IrCl6, and copper nitrate trihydrate. Copper nitrate trihydrate was weighed so that the copper ion concentration was 4M, and dissolved in water to make an aqueous solution. The concentration of the copper nitrate aqueous solution was analyzed by ICP. 0.2794 g of SrCO3, 0.0800 g of K2IrCl6, 76.9 μL of copper nitrate aqueous solution, 0.2800 g of C6H8O7·H2O, and 0.3 mL of nitric acid (1.38) were weighed, introduced into 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was called solution A. Using only solution A, the subsequent operations were carried out in the same manner as in Example 1 to recover a catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and copper ions, which were determined in the same manner as in Example 1, was 35 mol %, and the proportion of copper ions was 100%.
[0082] <Comparative Example 5> A catalyst powder containing an oxide having a perovskite structure in which iridium ions were incorporated into the B-site ions of strontium cobalt oxide (SrCoO3) was obtained by the Pechini method in the same manner as in Example 19, except that titanium ions were not incorporated into the B-site ions. The starting materials were SrCO3, K2IrCl6, and cobalt nitrate hexahydrate. Cobalt nitrate hexahydrate was weighed so that the concentration of cobalt ions was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the cobalt nitrate aqueous solution was analyzed by ICP. 0.2794 g of SrCO3, 0.0800 g of K2IrCl6, 76.9 μL of cobalt nitrate aqueous solution, 0.2800 g of C6H8O7·H2O, and 0.3 mL of nitric acid (1.38) were weighed, introduced into 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was named solution A. Using only solution A, the subsequent operations were carried out in the same manner as in Example 1 to recover a catalyst powder. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and cobalt ions, which were determined in the same manner as in Example 1, was 35 mol %, and the proportion of cobalt ions was 100%.
[0083] <Comparative Example 6> The molar concentration of iridium ions incorporated into the B-site ions of the synthesized SrTiO3 was 20 mol%, and the manganese ion ratio was 23.3%. 16 H 36 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that O4Ti was changed to 0.0844 g.
[0084] [Current density measurement] The relationship between the current density and voltage of the synthesized catalyst was evaluated at room temperature using the rotating disk electrode method. 10 mg of catalyst powder, 0.1 mL of 5 mass% Nafion dispersion solution, 0.4 mL of 2-propanol, and 1.5 mL of pure water were weighed and transferred to a glass container and mixed for more than 30 minutes using a homogenizer. 10 μL of the resulting mixed solution was taken and applied to a glassy carbon electrode with a diameter of 5 mm. After drying, it was set using a rotating disk electrode device to form a working electrode. A platinum wire was used as the counter electrode, and an aqueous Ag / AgCl reference electrode was used as the reference electrode. These and the working electrode were placed in a beaker containing 0.5 M sulfuric acid aqueous solution. After holding the catalyst in an open circuit for 10 minutes or more, 60 cycles of cyclic voltammetry measurements were performed at room temperature in the range of 0.05 V to 1.4 V relative to the reversible hydrogen electrode (RHE), at a sweep rate of 100 mV / s, and at a rotation speed of 1,600 rpm, to perform electrochemical cleaning of the catalyst surface. After that, 30 cycles of cyclic voltammetry measurements were performed in the range of 1.2 V to 1.6 V relative to the RHE, at a sweep rate of 5 mV / s, and at a rotation speed of 1,600 rpm, to measure the current at 1.6 V in the first cycle and the 30th cycle. The current value was divided by the area of the glassy carbon electrode to obtain the current density (unit: mA / cm 2 Based on the measurement results of the current density in the first cycle and the current density in the 30th cycle, the current density retention rate (unit: %) was calculated. The results are shown in Table 1.
[0085] [Table 1]
[0086] As shown in Table 1, Examples 1 to 23 had a higher current density retention rate than Comparative Examples 1 to 6. For example, Examples 1 to 23, in which the molar concentration of iridium ions was 30 mol% or more and transition metal element ions and titanium ions were incorporated, had a higher current density retention rate than Comparative Examples 1 to 5, which did not contain transition metal element ions or titanium ions. Moreover, Examples 1 to 23 had a higher current density retention rate than Comparative Example 6, in which the molar concentration of iridium ions was less than 30 mol% and transition metal element ions and titanium ions were incorporated.
[0087] FIG. 2 is a graph showing the relationship between the transition metal element ion ratio and the current density retention rate in each example and each comparative example. As shown in FIG. 2, there was a tendency that a high current density retention rate could be obtained by adjusting the transition metal element ion ratio. For example, it can be seen from the graph that at threshold 1 where the transition metal element ion ratio is 5% or more and 91% or less, the current density retention rate is 60% or more, at threshold 2 where the transition metal element ion ratio is 14% or more and 82% or less, the current density retention rate is 75% or more, and at threshold 3 where the transition metal element ion ratio is 21% or more and 75% or less, the current density retention rate is 85% or more. In other words, it was found that a high current density retention rate could be obtained by incorporating transition metal element ions at a molar concentration of iridium ions of 30 mol% or more, and an even higher current density retention rate could be obtained by adjusting the transition metal element ion ratio. [Explanation of symbols]
[0088] 11: Electrolyte membrane 12: Anode catalyst 13: Cathode catalyst 20: Anode gas diffusion layer 30: Cathode gas diffusion layer 40: Gasket 50: Gasket 60: Anode separator 70: Cathode separator 100: Water electrolysis cell
Claims
1. The A-site ions include an alkaline earth metal ion, and the B-site ions include a tetravalent metal ion and an iridium ion. The molar concentration of the iridium ions is 30 mol% or more, and the oxide has a perovskite structure; The oxide further comprises a transition metal element ion.
2. 2. The anode catalyst of claim 1, wherein the alkaline earth metal ions comprise strontium ions.
3. 2. The anode catalyst according to claim 1, wherein the tetravalent metal ions include titanium ions.
4. 2. The anode catalyst according to claim 1, wherein the transition metal element ions include at least one type of ion selected from the group consisting of manganese ions, nickel ions, copper ions, iron ions and cobalt ions.
5. 2. The anode catalyst according to claim 1, wherein a ratio of the number of moles of the transition metal element ions to a sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 5% or more and 91% or less.
6. 2. The anode catalyst according to claim 1, wherein a ratio of the number of moles of the transition metal element ions to a sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 14% or more and 82% or less.
7. 2. The anode catalyst according to claim 1, wherein a ratio of the number of moles of the transition metal element ions to a sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 21% or more and 75% or less.
8. A water electrolysis cell comprising: an anode gas diffusion layer; the anode catalyst according to any one of claims 1 to 7; an electrolyte membrane; a cathode catalyst; a cathode gas diffusion layer; and a separator.
9. A water electrolysis cell stack comprising a plurality of water electrolysis cells according to claim 8 stacked together.
Citation Information
Patent Citations
Synthesis for catelysis of bifunctional perovskite compound
US20100140569A1
Electrocatalysts for efficient water electrolysis
WO2016156599A1
Pd-Ru SOLID SOLUTION NANOPARTICLES, PRODUCTION METHOD AND CATALYST THEREFOR, METHOD FOR CONTROLLING CRYSTAL STRUCTURE OF Pt-Ru SOLID SOLUTION NANOPARTICLES, Au-Ru SOLID SOLUTION NANOPARTICLES, AND METHOD FOR MANUFACTURING SAME
WO2018159644A1