NOx OCCLUSION MATERIAL

A cerium oxide-based NOx storage material with neodymium substitution and palladium support addresses low-temperature NOx storage inefficiencies by enhancing oxygen activation and NOx conversion to solid forms, improving exhaust gas purification efficiency.

JP2024169030APending Publication Date: 2024-12-05TOYOTA JIDOSHA KK +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023086200
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing NOx storage materials exhibit insufficient NOx storage capacity at low temperatures, particularly below 200°C, especially in the range of 100°C to 150°C, which is critical for exhaust gas purification in vehicles with cold engines.

Method used

A NOx storage material comprising cerium oxide (CeO2) with palladium (Pd) supported on it, where 10 to 30 at.% of cerium is replaced with neodymium (Nd), optionally further substituted with praseodymium (Pr), yttrium (Y), lanthanum (La), or zirconium (Zr), and optionally containing aluminum oxide, enhances oxygen activation and NOx storage capacity at low temperatures.

Benefits of technology

The material achieves significant NOx storage capacity even at low temperatures below 200°C, effectively converting gaseous NO into solid nitrites and nitrates for efficient exhaust gas purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169030000001_ABST
    Figure 2024169030000001_ABST
Patent Text Reader

Abstract

To provide an NOx occlusion material that maintains sufficient NOx occlusion capability even in low temperature ranges of 200°C or lower.SOLUTION: An NOx occlusion material contains cerium oxide, and palladium supported on the cerium oxide. In the cerium oxide, 10 atom%-30 atom% of cerium are substituted with neodymium.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a NOx storage material. [Background technology]

[0002] 2. Description of the Related Art Exhaust gas discharged from internal combustion engines for automobiles and the like, such as gasoline engines or diesel engines, contains harmful components, such as carbon monoxide (CO), hydrocarbons (HC), and nitrogen oxides (NOx).

[0003] For this reason, internal combustion engines are generally equipped with exhaust gas purification devices for decomposing and removing these harmful components, and these harmful components are rendered almost harmless by exhaust gas purification catalysts installed in the exhaust gas purification devices. Known examples of such exhaust gas purification catalysts include three-way catalysts and NOx storage reduction catalysts.

[0004] A three-way catalyst is a catalyst that simultaneously oxidizes CO and HC and reduces NOx in a stoichiometric (theoretical air-fuel ratio) atmosphere.

[0005] In addition, the NOx storage reduction catalyst is a catalyst that oxidizes and stores NO in exhaust gas to NO2 in a lean atmosphere and reduces this to nitrogen (N2) in a stoichiometric atmosphere and rich atmosphere, making clever use of the changes in exhaust gas components in lean, stoichiometric, and rich atmospheres.

[0006] In recent years, the demand for fuel-efficient vehicles has increased, and it is expected that the exhaust gas temperature will become lower as a result of the electrification of internal combustion engines. Therefore, it is necessary to promote the purification of harmful gas components, especially NOx, at low temperatures, particularly at temperatures lower than 200°C, at which exhaust gas purification catalysts become active. However, since the temperature range at which conventional exhaust gas purification catalysts function is 250°C or higher, it has been difficult to sufficiently purify NOx generated at low temperatures when the engine is not sufficiently warmed up, such as when starting the engine.

[0007] Therefore, as a means of suppressing NOx emissions from the low temperature range where warm-up is not sufficient to the temperature range where the catalyst functions, a method is being considered in which, for example, a NOx storage material is placed in front of the catalyst, and NOx is retained in this NOx storage material in the low temperature range where the catalyst does not function, and NOx is desorbed from the NOx storage material in the temperature range where the catalyst is active, and the desorbed NOx is purified.

[0008] For example, U.S. Patent No. 5,399,633 discloses a lean NOx trap catalyst comprising: i) a first layer comprising one or more platinum group metals, a first ceria-containing material, an alkali metal or alkaline earth metal, and a first inorganic oxide; and ii) a second layer comprising a precious metal, a second ceria-containing material, and a second inorganic oxide, wherein the precious metal is a mixture of platinum and palladium or an alloy of platinum and palladium, wherein the total loading of the first ceria-containing material is greater than the total loading of the second ceria-containing material, and the ratio of the total loading of the precious metals in the second layer to the total loading of the one or more platinum group metals in the first layer is at least 2:1 on a w / w basis.

[0009] Patent Document 2 discloses a NOx storage material containing a composite oxide of silver and gallium.

[0010] Non-Patent Document 1 discloses that a material obtained by ion-exchanging Pd into a zeolite compound such as chabazite exhibits high NOx adsorption properties.

[0011] Non-Patent Document 2 discloses that Mn--Ce composite oxide exhibits high NOx adsorption properties at low temperatures. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Special Publication No. 2020-515393 [Patent Document 2] JP 2019-188389 A [Non-patent literature]

[0013] [Non-Patent Document 1] Hai-Ying Chen et al., “Low Temperature NO Storage of Zeolite Supported Pd for Low Temperature Diesel Engine Emission Control”, Catal Lett, 2016, 146, pp. 1706-1711 [Non-Patent Document 2] Masato Machida et al., "MnOx-CeO2 Binary Oxides for Catalytic NOx Sorption at Low Temperatures. Sorptive Removal of NOx", Chem. Mater., 2000, 12, pp. 3158-3164. Summary of the Invention [Problem to be solved by the invention]

[0014] However, even in the materials described in the above patent documents and non-patent documents, the NOx storage capacity in the low temperature range of 200°C or less, particularly in the range of 100°C to 150°C, is still insufficient.

[0015] Therefore, an object of the present invention is to provide a NOx storage material that has sufficient NOx storage capacity even in a low temperature range of 200° C. or less. [Means for solving the problem]

[0016] The inventors have investigated various means for solving the above problems, and as a result have found that in a NOx storage material having palladium (Pd) supported on cerium oxide (CeO2), by substituting a specific amount of Ce in CeO2 with neodymium (Nd), the lattice oxygen in CeO2 is activated, and as a result, the NOx storage capacity can be improved at temperatures below 200°C, particularly in the low temperature range of 100°C to 150°C, and have completed the present invention.

[0017] That is, the gist of the present invention is as follows. (1) A NOx storage material comprising cerium oxide and palladium supported on the cerium oxide, in which 10 atomic % to 30 atomic % of the cerium in the cerium oxide is replaced with neodymium. (2) The NOx occlusion material according to (1), in which 15 atomic % to 25 atomic % of cerium in the cerium oxide is substituted with neodymium. (3) The NOx occlusion material according to (1) or (2), in which a portion of the neodymium substituted for cerium in the cerium oxide is substituted with one or more additional elements selected from the group consisting of praseodymium, yttrium, lanthanum, and zirconium. (4) A NOx occlusion material according to any one of (1) to (3), in which a portion of the neodymium substituted for cerium in the cerium oxide is substituted with one or more additional elements selected from the group consisting of praseodymium, yttrium, lanthanum, and zirconium, neodymium accounts for 5 atomic % to 15 atomic % of the total metal elements in the cerium oxide, and the additional elements account for 5 atomic % to 15 atomic % of the total metal elements in the cerium oxide. (5) The NOx occlusion material according to any one of (1) to (4), further comprising aluminum oxide. (6) The NOx occlusion material according to any one of (1) to (5), further comprising aluminum oxide, the aluminum oxide being present in an amount of 5 mol % to 15 mol % of the total metals contained in the cerium oxide and the aluminum oxide. (7) A method for producing a NOx occlusion material according to any one of (1) to (4), comprising dissolving a salt of a metal constituting cerium oxide and a polydentate ligand in a solvent, removing the solvent by heating, drying and calcining the obtained powder, and supporting palladium on the powder. (8) A method for producing a NOx storage material according to (5) or (6), comprising dissolving a salt of a metal constituting cerium oxide, an aluminum salt and a polydentate ligand in a solvent, removing the solvent by heating, drying and calcining the resulting powder, and supporting palladium on the powder. (9) An exhaust gas purification system comprising a NOx occlusion material according to any one of (1) to (6) and an exhaust gas purification catalyst. Effect of the Invention

[0018] According to the present invention, there is provided a NOx storage material that has sufficient NOx storage capacity even in a low temperature range of 200° C. or less. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a diagram showing a schematic diagram of the NOx storage mechanism in Pd / Ce1-xNdxO2 (0.1≦x≦0.3). [Diagram 2] 1 is a graph showing XRD patterns of Comparative Examples 1 to 3 and Examples 1 to 3. [Diagram 3] 1 is a graph showing XRD patterns of Comparative Examples 4-5 and Examples 4-7. [Figure 4] 1 is a graph showing profiles (A) in H2-TPR analysis of Comparative Examples 1 to 3 and Examples 1 to 3, and the Nd(Nd+Ce)-1 ratio dependence of H2 consumption and maximum H2 consumption temperature (B). [Diagram 5] 1 is a graph showing the results of surface NOx adsorbed species analysis by NOx surface adsorption IR analysis in Example 2 and Comparative Example 1. [Figure 6] 1 is a graph showing the Nd(Nd+Ce)−1 ratio dependency of NSC in Comparative Examples 1 to 3 and Examples 1 to 3. [Figure 7] 1 is a graph showing NSC in Comparative Examples 1 to 5 and Examples 1 to 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Preferred embodiments of the present invention will now be described in detail. In this specification, the features of the present invention will be described with reference to the drawings as appropriate. In the drawings, the dimensions and shapes of each part are exaggerated for clarity, and the actual dimensions and shapes are not accurately depicted. Therefore, the technical scope of the present invention is not limited to the dimensions and shapes of each part shown in these drawings. Note that the NOx storage material of the present invention is not limited to the following embodiment, and can be embodied in various forms with modifications and improvements that a person skilled in the art can make within the scope of the gist of the present invention.

[0021] The NOx storage material of the present invention contains cerium oxide and palladium supported on the cerium oxide, and 10 atomic % to 30 atomic %, preferably 15 atomic % to 25 atomic %, of the cerium in the cerium oxide is replaced with neodymium. Therefore, the NOx storage material of the present invention is, for example, Pd / Ce 1-x Nd x It can also be expressed as O2 (0.1≦x≦0.3, preferably 0.15≦x≦0.25).

[0022] Here, the cerium oxide in the present invention is a composite oxide of cerium, neodymium, and optionally an additional element described below. Furthermore, the cerium oxide in the present invention has a structure in which cerium (IV) is substituted for neodymium (III) while maintaining the fluorite structure of cerium oxide. Note that "substitution" also includes solid solution.

[0023] By substituting neodymium for part of the cerium in cerium oxide, the oxygen atoms bonded to the cerium are activated at low temperatures below 200°C, particularly at 100°C to 150°C, as shown in FIG. 1. This activated oxygen acts to produce solid nitrite (NO2) and nitrate (NO3) from the gaseous NO contained in the exhaust gas, and can oxidatively store the NOx contained in the exhaust gas.

[0024] A part of the neodymium substituted for a part of the cerium in the cerium oxide may be further substituted with one or more additional elements selected from the group consisting of praseodymium (Pr), yttrium (Y), lanthanum (La), and zirconium (Zr). The additional element is preferably one or more selected from the group consisting of yttrium (Y), lanthanum (La), and zirconium (Zr). Even in this case, the cerium oxide maintains the fluorite structure of the cerium oxide. In this case, the neodymium is substituted for 5 atomic % to 15 atomic % of the metal elements in the entire cerium oxide, and the additional element is substituted for 5 atomic % to 15 atomic % of the metal elements in the entire cerium oxide. Therefore, the NOx storage material of the present invention is, for example, Pd / Ce 1-x-y Nd x M y O2 (wherein M is one or more selected from the group consisting of Pr, Y, La, and Zr, and 0.05≦x≦0.15, 0.05≦y≦0.15).

[0025] When a portion of the neodymium that replaces a portion of the cerium in the cerium oxide is further replaced by an additional element, the oxygen atoms bonded to the cerium are further activated in the low temperature range of 200°C or less, particularly at 100°C to 150°C, as shown in FIG. 1, and this further activated oxygen promotes the production of solid nitrites (NO2) and nitrates (NO3) from the gaseous NO contained in the exhaust gas, making it possible to oxidatively store NOx contained in the exhaust gas.

[0026] The NOx storage material of the present invention may contain aluminum oxide. In this case, the content of aluminum oxide is usually 5 mol % to 15 mol % of the total metals contained in the cerium oxide and aluminum oxide. Therefore, the NOx storage material of the present invention may contain, for example, Pd / (Ce 1-x Nd x O2+yAlO 3 / 2 ) (0.05≦x≦0.15, 0.05≦y≦0.15).

[0027] By including aluminum oxide in the NOx storage material of the present invention, as shown in FIG. 1, the oxygen atoms bonded to cerium are further activated at low temperatures below 200°C, particularly at 100°C to 150°C. This further activated oxygen converts gaseous NO contained in exhaust gas into solid nitrite (NO2 - ) and nitrates (NO3 - ) and can oxidatively store NOx contained in exhaust gas.

[0028] The NOx storage material of the present invention has palladium supported on the surface of cerium oxide and optionally aluminum oxide which are substituted with neodymium and optionally additional elements as described above.

[0029] The amount of supported palladium is not limited, and is usually 1% by weight to 20% by weight, and preferably 2% by weight to 10% by weight, based on the total weight of the storage material.

[0030] The NOx storage material of the present invention can be produced by a method known in the art.

[0031] The NOx storage material of the present invention can be produced, for example, by dissolving salts of the metals that make up cerium oxide, i.e., a cerium salt and a neodymium salt, and optionally a salt of an additional element and an aluminum salt, and a multidentate ligand that can coordinate to the ions of the metals that make up cerium oxide, in a solvent, removing the solvent by heating, drying and calcining the resulting powder, and then supporting palladium on the powder.

[0032] The salt to be used as the raw material is not limited. Examples of the salt include inorganic salts such as nitrates, phosphates, and sulfates, organic acid salts such as oxalates and acetates, halides such as fluorides, chlorides, bromides, and iodides, and combinations of two or more of these. The salt is preferably a nitrate.

[0033] The polydentate ligand is not limited. Examples of the polydentate ligand include citric acid, oxalic acid, and combinations thereof. The polydentate ligand is preferably citric acid.

[0034] The amount of the polydentate ligand is not limited, and is usually 1 molar equivalent to 3 molar equivalents, for example 2 molar equivalents, based on the total molar amount of the metal.

[0035] The solvent is not limited. Examples of the solvent include water, alcohol, such as methanol, ethanol, and mixtures of two or more of these. Water is a preferred solvent.

[0036] The temperature, time and atmosphere in the thermal removal of the solvent and the drying and calcination of the obtained powder are not limited. The thermal removal of the solvent and the drying are carried out, for example, in the air, usually at 100°C to 170°C, preferably 120°C to 150°C, usually for 2 hours to 15 hours, preferably 4 hours to 10 hours. The calcination, including the calcination, is carried out, for example, in the air, usually at 250°C to 900°C, preferably 300°C to 800°C, usually for 2 hours to 10 hours, preferably 4 hours to 8 hours.

[0037] The method of supporting palladium on the powder is not limited. Supporting palladium on the powder can be carried out, for example, by putting the powder into a solution in which a palladium salt is dissolved, then removing the solvent in the solution by heating, and further drying and calcining the obtained palladium-supported powder. The solvent is removed by heating and the palladium-supported powder is dried, for example, in the air, usually at 100°C to 170°C, preferably 120°C to 150°C, usually for 2 hours to 15 hours, preferably 4 hours to 10 hours. The palladium-supported powder is calcined, for example, usually at 300°C to 700°C, preferably 400°C to 600°C, usually for 1 hour to 5 hours, preferably 2 hours to 4 hours.

[0038] Furthermore, the present invention also relates to an exhaust gas purification system comprising the NOx storage material of the present invention and an exhaust gas purification catalyst.

[0039] Here, the exhaust gas purifying catalyst may be a catalyst for exhaust gas purifying known in the art, such as a three-way catalyst.

[0040] As the catalytic metal in the exhaust gas purification catalyst, at least one metal selected from the group consisting of platinum (Pt), rhodium (Rh), palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), and the like can be used.

[0041] The content of the catalytic metal in the exhaust gas purification catalyst is not limited. The content of the catalytic metal is usually 0.5 g / L to 10 g / L, preferably 0.5 g / L to 7.0 g / L, based on the total volume of the catalyst. If the content of the catalytic metal is too small, the catalytic activity (particularly the oxidation catalytic activity) obtained by the catalytic metal becomes insufficient, while if the content of the catalytic metal is too large, the catalytic metal is likely to undergo grain growth and may be disadvantageous in terms of cost.

[0042] The catalyst for exhaust gas purification can be used alone as a pellet, or can be used by being disposed on a substrate. The substrate can be any substrate that can be used for a catalyst for exhaust gas purification known in the art, and is not limited thereto. For example, the substrate can be made of a heat-resistant material having a porous structure. Examples of the heat-resistant material include cordierite, silicon carbide (SiC), aluminum titanate, silicon nitride, heat-resistant metals such as stainless steel, and alloys thereof. The substrate can have, for example, a honeycomb structure, a foam shape, a pellet shape, or the like. The outer shape of the entire substrate can be a cylindrical shape, an elliptical cylindrical shape, a polygonal cylindrical shape, or the like.

[0043] Since the exhaust gas purification system of the present invention comprises the NOx absorption material and exhaust gas purification catalyst of the present invention, the NOx absorption material of the present invention absorbs NOx in the exhaust gas at low temperatures below 200°C, such as when the internal combustion engine is started, particularly at temperatures between 100°C and 150°C, and at high temperatures above 200°C after warm-up operation, the exhaust gas purification catalyst can purify the desorbed NOx that has been desorbed from the NOx absorption material together with the exhaust gas emitted from the internal combustion engine. EXAMPLES

[0044] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.

[0045] 1. Preparation of NOx storage material (Comparative example 1: Pd / CeO2) (x=0) The synthesis of the oxide was carried out by the citrate complex method. Specifically, 43.42g (0.10mol) of Ce(NO3)3·6H2O was dissolved in 100mL of distilled water, and then 38.42g (0.2mol) of citric acid was dissolved to prepare a raw material solution. This raw material solution was heated and stirred at 150℃ for 4 hours, and the obtained slurry was dried at 120℃ for 8 hours. The obtained paste was calcined at 300℃ for 2 hours, and then fired at 750℃ for 5 hours. Next, a palladium nitrate solution (manufactured by Cataler Co., Ltd.) was diluted with distilled water so that the amount of Pd supported was 5% by weight relative to the total weight of the NOx storage material, and the powder obtained above was added and dispersed, and the dispersion medium was removed by heating while stirring. After drying at 120℃ for 12 hours, the mixture was fired in an electric furnace at 500℃ for 2 hours to obtain a sample powder. Furthermore, this was compressed into powder by 2t and pellets of 1 mm to 1.7 mm were classified to obtain sample pellets.

[0046] Example 1: Pd / Ce 0.9 Nd 0.1 O2)(x=0.1) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 39.08 g (0.09 mol) of Ce(NO3)3·6H2O and 4.38 g (0.01 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0047] Example 2: Pd / Ce 0.8 Nd 0.2 O2)(x=0.2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 34.74 g (0.08 mol) of Ce(NO3)3·6H2O and 8.77 g (0.02 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0048] Example 3: Pd / Ce 0.7 Nd 0.3 O2)(x=0.3) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 30.40 g (0.07 mol) of Ce(NO3)3·6H2O and 13.15 g (0.03 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0049] (Comparative example 2: Pd / Ce 0.6 Nd 0.4 O2)(x=0.4) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 26.05 g (0.06 mol) of Ce(NO3)3·6H2O and 17.53 g (0.04 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0050] (Comparative example 3: Pd / Ce 0.5 Nd 0.5 O2)(x=0.5) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 21.71 g (0.05 mol) of Ce(NO3)3·6H2O and 21.92 g (0.05 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0051] Example 4: Pd / Ce 0.8 Nd 0.1 Y 0.1 O2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 34.74 g (0.08 mol) of Ce(NO3)3·6H2O, 3.83 g (0.01 mol) of Y(NO3)3·6H2O, and 4.38 g (0.01 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0052] Example 5: Pd / Ce 0.8 La 0.1 Nd 0.1 O2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 34.74 g (0.08 mol) of Ce(NO3)3·6H2O, 4.33 g (0.01 mol) of La(NO3)3·6H2O, and 4.38 g (0.01 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water, and then dissolving 38.42 g (0.2 mol) of citric acid.

[0053] Example 6: Pd / Ce 0.8 Nd 0.1 Zr 0.1 O2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 34.74 g (0.08 mol) of Ce(NO3)3·6H2O, 2.67 g (0.01 mol) of ZrO(NO3)2·2H2O, and 4.38 g (0.01 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0054] Example 7: Pd / Al 0.1 Ce 0.8 Nd 0.1 O2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 3.75 g (0.01 mol) of Al(NO3)3·9H2O, 34.74 g (0.08 mol) of Ce(NO3)3·6H2O, and 4.38 g (0.01 mol) of Nd(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0055] (Comparative example 4: Pd / Ce 0.9 Y 0.1 O2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 39.08 g (0.09 mol) of Ce(NO3)3·6H2O and 3.83 g (0.01 mol) of Y(NO3)3·6H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0056] (Comparative example 5: Pd / Ce 0.9 Zr 0.1 O2) In Comparative Example 1, samples (sample powder and sample pellets) were prepared in the same manner as in Comparative Example 1, except that a raw material solution was used that was prepared by dissolving 39.08 g (0.09 mol) of Ce(NO3)3·6H2O and 2.67 g (0.01 mol) of ZrO(NO3)2·2H2O in 100 mL of distilled water and then dissolving 38.42 g (0.2 mol) of citric acid.

[0057] 2. Analysis method for NOx storage materials 2-1.X-ray diffraction (XRD) analysis XRD was performed using SmartLab (Rigaku Corporation). The X-ray source was CuKα (λ = 1.5418 nm), and measurements were taken in the range of 10° to 90° with a step width of 0.02° / 0.12 seconds.

[0058] 2-2.H2-Temperature Programmed Reduction (TPR) Analysis H2-TPR was performed using Belcat A (Microtrac-Bell Co., Ltd.). 1. After weighing out about 50 mg of the sample powder prepared in the preparation of NOx storage material and introducing it into a sample tube, the sample was heated to 500°C while flowing 20% ​​O2 / He at 30 mL / min and maintained at the same temperature for 10 minutes (referred to as O2 pretreatment), or heated to 500°C while flowing 1% H2 / He at 30 mL / min and maintained at the same temperature for 60 minutes (referred to as H2+O2 pretreatment), and then cooled to -80°C. After replacing with Ar gas at -80°C, the sample was heated to 1000°C while flowing 5% H2 / Ar at 30 mL / min and heating at 10°C / min, and the H2 consumption was analyzed. The analysis was performed using a thermal conductivity detector (TCD), and a desiccant was placed in front of the TCD to trap the water produced. A similar analysis was performed using CuO powder, and the H2 consumption of each sample was quantified.

[0059] 2-3. NOx surface adsorption infrared absorption spectroscopy (IR) analysis For the NOx surface adsorption IR analysis, a transmission type in situ FT-IR analyzer equipped with an FT-IR spectrophotometer (manufactured by JASCO Corporation) and a gas generator (manufactured by ACE Corporation) was used. 1. The sample powder prepared in the preparation of the NOx storage material and potassium bromide (KBr) were mixed in a mortar in a weight ratio of 3:7, 11 mg was precisely weighed, and a Φ8 mm sample disk was produced by powder compaction. Calcium fluoride (CaF) was used as the window material. As a pretreatment operation, the sample disk was heated to 350°C, and 5% O2 / Ar and 1% H2 / Ar were alternately passed through the sample disk for 2 minutes at a flow rate of 500 mL / min for a total of 20 minutes. Next, the sample disk was cooled to 100°C or 150°C while passing 5% O2 / Ar. After switching to Ar gas and performing background measurement, 1000 ppm NO / Ar gas was passed through the sample disk for 1 minute, and then purged with Ar for 1 minute, after which the IR spectrum was measured. 1000 cm -1 ~4000cm -1 Measurement range with resolution of 4cm -1 This was accumulated 128 times.

[0060] 2-4.NOx storage test 4 g of sample pellets prepared in 1. Preparation of NOx storage material were placed in a fixed-bed flow reactor, and the conversion behavior of each gas was examined using an FT-IR analyzer (SESAM-HL, Best Instruments Co., Ltd.) and an oxygen meter (BEX, Best Instruments Co., Ltd.). The sample pellets were heated to 500°C while flowing reduction pretreatment gas (Table 1) at a flow rate of 20 L / min. After reduction treatment for 5 minutes at the same temperature and gas composition, the pellets were purged with N2 gas for 1 minute, and oxidation pretreatment gas (Table 1) was flowed for 5 minutes. Next, the sample pellets were cooled to a specified temperature while flowing the oxidation pretreatment gas, and an inert gas (Table 1) was flowed through the sample at the same temperature for 2 minutes, after which a stoichiometric simulated exhaust gas (Table 1) was flowed through the sample for 1 minute, and the pellets were purged with N2 gas for 1 minute. The above tests were performed with the inlet gas temperature set to 150°C, 100°C, or 50°C, and the NO conversion (storage) amount (NSC) during the introduction of the stoichiometric simulated exhaust gas was calculated.

[0061] [Table 1]

[0062] 3. Analysis results of NOx storage material 3-1.X-ray diffraction (XRD) analysis results Figure 2 shows the XRD pattern of the prepared sample. The diffraction peaks correspond to the Nd molar ratio (Nd(Ce+Nd) -1 )(x) increases, the angle shifts to the lower side. 4+ (8-coordinated Ce 4+ : 0.97Å) with a large ionic radius of Nd 3+ (8-coordinate Nd 3+ : 1.11 Å) is substituted according to Vegard's law. It was also found that the diffraction peaks broaden with increasing Nd ratio x. This is because 3+ This indicates that the substitution reduces the crystallite size.

[0063] FIG. 3 shows the XRD patterns of the other samples (Examples 4 to 7 and Comparative Examples 4 and 5). Example 4 (Pd / Ce 0.8 Nd 0.1Y 0.1 O2), Example 5 (Pd / Ce 0.8 La 0.1 Nd 0.1 O2), Example 6 (Pd / Ce 0.8 Nd 0.1 Zr 0.1 O2), Comparative Example 4 (Pd / Ce 0.9 Y 0.1 O2) and Comparative Example 5 (Pd / Ce 0.9 Zr 0.1 The diffraction pattern of Example 7 (Pd / AlO2) is consistent with that of CeO2 in terms of intensity ratio, and a shift in the diffraction peak is observed. Therefore, it is considered that the oxides formed are those in which the Ce in CeO2 is partially substituted with La, Y, Nd, or Zr. 0.1 Ce 0.8 Nd 0.1 As for Al2O2), the diffraction pattern and intensity ratio match those of CeO2, and at the same time, significant broadening of the diffraction peaks was observed. In addition, it is known that Al does not substitute for or form a solid solution in CeO2, so it is thought to be a mixture of CeO2 and Al2O3.

[0064] 3-2.H2-Temperature Programmed Reduction (TPR) Analysis Results The oxidation of NO to nitrite and / or nitrate by self-oxygen is 3+ In order to investigate the factors that promote the partial substitution of Nd, H2-TPR analysis was carried out. Figure 4A shows the profile, and Figure 4B shows the H2 consumption and the maximum H2 consumption temperature of Nd(Nd+Ce). -1 The ratio dependence is shown in FIG. 4A. In the measurement of Comparative Example 1 (Pd / CeO2), the reaction between the oxide self-oxygen and H2 (Pd 2+ and Ce 4+ At 44°C, a large consumption attributable to hydrogen absorption by Pd was detected, and at 56°C, a negative signal attributable to desorption of absorbed hydrogen was detected. Furthermore, from Figure 4A, the main peak attributable to the reaction of self-oxygen with H2 was Nd (Nd + Ce) -1 It was found that when the ratio was increased to 0.2, the temperature shifted slightly (5°C) to a higher temperature, and when the ratio was increased to 0.3 or more, the temperature shifted significantly (30°C or more at x = 0.4). -1This shows that the reactivity of the self-oxygen is significantly reduced when the ratio is 0.3 or more. On the other hand, from FIG. 4B, the H2 consumption calculated from the main peak assigned to the reaction of the self-oxygen with H2 is 0.53 mmol g in Comparative Example 1 (Pd / CeO2). -1 and this consumption is Nd(Nd+Ce) -1 The amount of H2 consumption increases with increasing ratio, and converges at 0.3. The amount of self-oxygen that can react with H2 and NO increases with the introduction of Nd, and Nd(Nd+Ce) -1 It shows that the ratio is saturated at 0.3. Therefore, the H2 consumption and the maximum H2 consumption temperature, that is, the reactivity of self-oxygen, Nd(Nd+Ce) -1 The ratio-dependent trade-off relationship is explained below for Nd(Nd+Ce) in NSC. -1 This is interpreted as being due to a mountain-shaped hierarchy with the ratio at its peak at 0.2 (see Figure 6).

[0065] 3-3. NOx surface adsorption infrared absorption spectroscopy (IR) analysis results Example 2 (Pd / Ce 0.8 Nd 0.2 Surface NOx adsorbed species analysis was performed for Example 2 (Pd / CeO2) and Comparative Example 1 (Pd / CeO2) by NOx surface adsorption IR analysis. The results are shown in Figure 5. Each surface NOx adsorbed species was assigned with reference to a previous report [Bruno Azambre, Idriss Atribak, Agustn Bueno-Lopez, and Avelina Garcia-Garc J. Phys. Chem. C, 2020 114, 13300-13312]. In both the IR spectra of Example 2 and Comparative Example 1, the 1190 cm -1 ~1240cm -1 Nitrite NO2 nearby - A gentle absorption or shoulder attributed to the NO stretching was observed, and furthermore, at 1400 cm -1 , 1320cm -1 Each has monodentate nitrate NO3 - , uncoordinated nitrate NO3 - In Example 2, the absorption due to NO stretching was observed. 0.8 Nd 0.21460cm in O -1 Bidentate nitrate NO3 - These results were obtained from Example 2 (Pd / Ce 0.8 Nd 0.2 This shows that in the case of the catalyst (Pd / CeO2) and Comparative Example 1 (Pd / CeO2), an oxidation reaction of NO to nitrite and nitrate occurs due to self-oxygen.

[0066] 3-4.NOx storage test results The NOx storage capacity (NSC) of the prepared samples was evaluated. Figure 6 shows the NSC of Nd (Nd + Ce) -1 From Figure 6, at 150℃ and 100℃, NSC is Nd(Nd+Ce) -1 The order is mountain-shaped with the ratio x = 0.2 at the top. On the other hand, at 50°C, the amount of absorption is small in all cases, and no significant uniqueness was observed. As shown in Figure 2, considering that the crystallite size decreases with increasing Nd substitution amount, NSC does not depend on the specific surface area of ​​the material, but on the Nd(Nd+Ce) -1 This suggests that changes in the chemical properties of the material that contribute to an increase in NSC occur around the ratio x = 0.2.

[0067] Furthermore, the NSC evaluation results for all the synthesized samples (Examples 1 to 7 and Comparative Examples 1 to 5) are shown in Figure 7. It was found that the oxides in which Ce in CeO2 was partially replaced with Nd and Y, La, or Zr (Examples 4 to 6) and the composite with Al2O3 (Example 7) also showed high NOx storage capacity. On the other hand, Pd / Ce, which does not contain Nd, 0.9 Y 0.1 O2 (Comparative Example 4) and Pd / Ce 0.9 Zr 0.1 It was found that the amount of NOx stored was small in the case of O2 (Comparative Example 5).

Claims

1. The NOx storage material contains cerium oxide and palladium supported on the cerium oxide, and 10 atomic % to 30 atomic % of the cerium in the cerium oxide is replaced with neodymium.

2. 2. The NOx storage material according to claim 1, wherein a portion of the neodymium substituted for cerium in the cerium oxide is substituted with one or more additional elements selected from the group consisting of praseodymium, yttrium, lanthanum, and zirconium.

3. The NOx storage material according to claim 1 , further comprising aluminum oxide.

4. An exhaust gas purification system comprising the NOx storage material according to any one of claims 1 to 3 and an exhaust gas purification catalyst.

Citation Information

Patent Citations

  • Nitrogen oxide occlusion material and exhaust purification method

    JP2019188389A

  • NOx is attracted by the catalyst

    JP2020515393A