A silver alloy thin film with fine crystallites and oxide particles at grain boundaries, produced via controlled sputtering, addresses the inefficiencies of conventional films by enhancing oxygen permeability and mechanical strength, enabling efficient and cost-effective pure oxygen production.
Patent Information
- Application Number
- JP2023086274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional silver-based thin films require high temperatures and significant energy for oxygen permeation, limiting their effectiveness in the medium to low temperature range below 600°C, and existing methods for producing pure oxygen are large-scale and difficult to install near oxygen-consuming equipment.
A silver alloy thin film with a silver alloy phase composed of fine crystallites (average diameter ≤100 nm) and oxide particles at grain boundaries, produced using a sputtering method with controlled Al and Mg concentrations and gas partial pressures, enhancing oxygen permeability and mechanical strength.
The silver alloy thin film achieves high oxygen permeability and mechanical strength, enabling efficient production of pure oxygen using waste heat in the medium to low temperature range, reducing equipment scale and costs, and is applicable in various industries.
Smart Images

Figure 2024169085000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a silver alloy thin film, a method for producing the silver alloy thin film, and a composite. [Background technology]
[0002] It is expected that pure oxygen will be used in various fields. For example, air combustion is used in heating furnaces in steelworks. However, the use of air combustion in heating furnaces produces NO x There is a problem that NO x In order to prevent the generation of CO2, it is effective to use pure oxygen combustion instead of air combustion. In addition, coke oven gas (COG) may be used as fuel in heating furnaces. However, since COG contains a large amount of hydrogen gas and is expensive, it is preferable to replace COG with blast furnace gas (BFG) or Linz-Donawitz converter gas (LDG). The replacement with BFG or LDG can be realized by increasing the amount of heat of combustion using pure oxygen. This makes it possible to reduce the fuel consumption rate and reduce the environmental load.
[0003] As a method for producing pure oxygen, the liquefied air distillation method (cryogenic method), which utilizes the cooling during the expansion of compressed air, and the pressure swing adsorption (PSA) method, which utilizes the difference in adsorption rate due to gas components during the compression and expansion of air, are widely used. However, these methods require large-scale facilities. On the other hand, when considering the industrial use of pure oxygen, it is desirable to place the pure oxygen production facility close to the facility that uses the pure oxygen. It is often difficult to place large-scale facilities using the cryogenic method or the PSA method close to the facility that uses the pure oxygen due to restrictions on the site area, etc. For this reason, it is desirable for the pure oxygen production facility to be able to efficiently produce pure oxygen and also to require a small site area.
[0004] As a method for producing pure oxygen different from the cryogenic method and the PSA method, a method for separating oxygen from air using a ceramic or metal membrane has been attracting attention. For example, a ceramic oxygen ion conductor having oxygen selective permeability (Patent Document 1) and an oxygen selective permeation method using a thin film of silver (Ag), which is a metal with the highest oxygen selective permeability (Patent Documents 2-4, Non-Patent Document 1), are known. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] U.S. Patent No. 5,108,465 [Patent Document 2] U.S. Pat. No. 3,359,705 [Patent Document 3] U.S. Pat. No. 3,509,694 [Patent Document 4] U.S. Pat. No. 3,550,355 [Non-patent literature]
[0006] [Non-Patent Document 1] FMG Johnson and P. Larose, Journal of American Chemical Society, Vol. 46, 1924, p. 1377 Summary of the Invention [Problem to be solved by the invention]
[0007] The oxygen selective permeation method using an oxygen permeable membrane is thought to be capable of producing the same amount of pure oxygen as the cryogenic method or PSA method, even on a smaller scale. However, oxygen permeable membranes have a low oxygen permeability coefficient at low temperatures. For example, when a silver-based thin film is used as the oxygen permeable membrane, the process of producing pure oxygen requires high temperatures of 600°C or more, and a large amount of energy is required for heating, which is an issue. As described above, there is room for improvement in the oxygen permeability coefficient of conventional silver-based thin films in the medium-low temperature range below 600°C. [Means for solving the problem]
[0008] The present application discloses the following aspects as one of the means for solving the above problems. <Aspect 1> A silver alloy thin film having a silver alloy phase, The silver alloy phase is composed of a plurality of crystallites, The average crystallite diameter of the crystallites in a cross section parallel to the surface of the silver alloy thin film is 100 nm or less. Silver alloy thin film. <Aspect 2> A plurality of oxide particles are present at the grain boundaries of the crystallites. The silver alloy thin film of embodiment 1. <Aspect 3> The oxide particles contain one or both of Al and Mg as constituent elements. The silver alloy thin film of embodiment 2. <Aspect 4> The volume ratio of the oxide particles in the silver alloy thin film is 0.1 volume % or more and 15.0 volume % or less. The silver alloy thin film according to embodiment 2 or 3. <Aspect 5> At 350℃, 2.0×10 -5 Ncc-O2 / cm / min / atm 0.5 Having an oxygen permeability coefficient of equal to or greater than The silver alloy thin film according to any one of embodiments 1 to 4. <Aspect 6> Nanoindentation hardness of 2.0 GPa or more. The silver alloy thin film according to any one of embodiments 1 to 5. <Aspect 7> Used as an oxygen permeable membrane, The silver alloy thin film according to any one of embodiments 1 to 6. <Aspect 8> A thickness of 0.1 μm or more and 100 μm or less, The silver alloy thin film according to any one of embodiments 1 to 7. <Aspect 9> A silver alloy thin film is formed by using an Ag alloy as a sputtering target and performing sputtering under the supply of Ar gas and O2 gas so that the condition of the following formula (1) is satisfied. A method for producing a silver alloy thin film, comprising: (1.6×10 -6 ×C Al -3.7×10 -8 ×C Al 2 +8.2×10 -7 ×C Mg )×SR≦P O2 ≦P Ar (1) Where: C Al is the Al concentration (at%) of the sputtering target, C Mg is the Mg concentration (at%) of the sputtering target, SR is the deposition rate (nm / min), P Ar is the Ar partial pressure in the sputtering atmosphere (Pa), P O2 is the O2 partial pressure in the sputtering atmosphere (Pa), The Al concentration C Al is 0 at% or more and 7.0 at% or less, The above Mg concentration C Mg is 0 at% or more and 10.0 at% or less, The Al concentration C Al and the Mg concentration C Mg The sum of these is equal to or greater than 0.10 at % and equal to or less than 10.0 at %. <Aspect 10> A composite material having a porous substrate and a silver alloy thin film, The silver alloy thin film is supported on the porous substrate, The silver alloy thin film is any one of aspects 1 to 8. Complex. Effect of the Invention
[0009] The silver alloy thin film of the present disclosure can improve the oxygen permeability coefficient in the medium-low temperature range below 600°C compared with conventional silver-based thin films. When pure oxygen is produced using the silver alloy thin film of the present disclosure, for example, unused waste heat in the medium-low temperature range (about 200°C to about 500°C) in a steelworks can be used as a heat source, which reduces the equipment for the heat source and enables a small-scale pure oxygen production device to be realized. As a result, for example, in a steelworks, it becomes possible to reduce the production cost of O2 used in the iron-making and steel-making processes. In addition, the silver alloy thin film of the present disclosure can be widely used in pure oxygen production devices for various industries other than steelmaking. [Brief description of the drawings]
[0010] [Figure 1] 1 illustrates a schematic configuration of a silver alloy thin film according to an embodiment. [Diagram 2] 1 shows a schematic configuration of a sputtering apparatus used in a method for producing a silver alloy according to one embodiment. [Diagram 3] 1 illustrates a schematic diagram of a composite structure according to one embodiment. [Figure 4] FIG. 2 is a schematic diagram for explaining a method for producing oxygen according to an embodiment. [Diagram 5] The schematic diagram shows the configuration of an apparatus for measuring oxygen transmission rate. (A) shows the overall configuration, and (B) shows an enlarged view of the thin film support part. [Figure 6] Examples of EBSD analysis images of the surfaces of thin films are shown: (A) with an average crystallite size of <50 nm, and (B) with an average crystallite size of 220 nm. [Figure 7] These are examples of TEM images of a thin film. (A) shows a longitudinal section of the thin film (a section perpendicular to the surface direction), and (B) shows a cross section of a 1 / 2 thickness portion (a section parallel to the surface direction). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] 1. Silver alloy thin film Hereinafter, a silver alloy thin film according to an embodiment will be described with reference to the drawings. As shown in FIG. 1, a silver alloy thin film 10 according to an embodiment has a silver alloy phase 11. The silver alloy phase 11 is composed of a plurality of crystallites 11a. The average crystallite diameter of the crystallites 11a in a cross section parallel to the surface of the silver alloy thin film 10 is 100 nm or less.
[0012] 1.1 Chemical composition of silver alloy phase The silver alloy phase 11 is a phase made of a silver alloy. The silver alloy constituting the silver alloy phase 11 includes Ag and an alloying element M. The alloying element M may be, for example, one or both of Al and Mg. The alloying element M may further include at least one selected from Cu, La, Ce, Nd, Zr, Li, Mn, Si, and Zn in addition to one or both of Al and Mg. The silver alloy phase 11 may include, for example, in atomic %, Ag: 72 to 99.8%, alloying element M: 0.1 to 13%, and O: 0 to 15%. More specifically, the silver alloy phase 11 may contain, in atomic %, Ag: 72-99.8%, Al: 0-7%, Mg: 0-10%, Al+Mg: 0.1-10%, Cu: 0-3%, La: 0-1%, Ce: 0-1%, Nd: 0-1%, Zr: 0-1%, Li: 0-1%, Mn: 0-1%, Si: 0-1%, Al+Mg+Cu+La+Ce+Nd+Zr+Li+Mn+Si+Zn: 0.1-13%, and O: 0-15%. The remainder other than Ag, alloy element M, and O may be impurities. If the silver alloy phase 11 does not contain the alloy element M (i.e., if it is pure silver), it becomes difficult to satisfy the requirements for the average crystallite size described later.
[0013] 1.2 Crystallites of silver alloy phase 1, the silver alloy phase 11 is composed of a plurality of crystallites 11a. That is, the silver alloy phase 11 is a polycrystalline phase having a plurality of crystallites 11a. Each of the crystallites 11a may be composed of the above-mentioned silver alloy.
[0014] In this embodiment, it is important that the average crystallite diameter of the crystallites 11a in a cross section parallel to the surface of the silver alloy thin film 10 is 100 nm or less. The "surface of the silver alloy thin film 10" refers to the front and back surfaces (main surfaces) of the thin film. The crystallites 11a in a cross section parallel to the surface of the silver alloy thin film 10 can be observed, for example, as shown in FIG. 1A. The smaller the average crystallite diameter of the crystallites 11a in a cross section parallel to the surface of the silver alloy thin film 10, the more grain boundaries in the cross section parallel to the surface of the silver alloy thin film 10. In the silver alloy thin film 10, the grain boundaries can function as a path for diffusing oxygen at high speed. That is, the more grain boundaries in a cross section parallel to the surface of the silver alloy thin film 10, the easier it is for oxygen to permeate through the silver alloy thin film 10 from the front surface to the back surface, and the oxygen permeability coefficient of the silver alloy thin film 10 is improved. The average crystallite diameter of the crystallites 11a in a cross section parallel to the surface of the silver alloy thin film 10 is 100 nm or less, and may be 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, or 50 nm or less. On the other hand, the lower limit of the average crystallite diameter is not particularly limited, and may be, for example, 5 nm or more, 10 nm or more, 15 nm or more, or 20 nm or more. In addition, the area ratio of the crystal grain boundaries to the entire cross section parallel to the surface of the silver alloy thin film 10 may be 1% or more, 2% or more, 3% or more, 4% or more, or 5% or more, and may be 30% or less, 25% or less, 20% or less, 15% or less, or 10% or less.
[0015] In addition, the "average crystallite diameter of the crystallites in the cross section parallel to the surface of the silver alloy thin film" in the present application is measured after the silver alloy thin film is subjected to heat treatment at 350 ° C. Specifically, the silver alloy thin film is inserted into a heating furnace under an air atmosphere, heated from room temperature (25 ° C.) to 350 ° C. at 30 ° C. / min, held at 350 ° C. for 1 hour, then removed from the furnace, cooled in the air, and the average crystallite diameter is measured. The cooling conditions after holding at 350 ° C. for 1 hour are not particularly limited because they do not substantially affect the average crystallite diameter. Thus, if the average crystallite diameter after holding at 350 ° C. for 1 hour is 100 nm or less, even when the silver alloy thin film is held at a medium to low temperature range (for example, about 200 ° C. to about 500 ° C.) for a long time, the crystallite diameter of the silver alloy thin film is unlikely to change, and it can withstand, for example, a manufacturing environment of pure oxygen.
[0016] The "average crystallite diameter of the crystallites in a cross section parallel to the surface of the silver alloy thin film" can be measured by the electron backscatter diffraction (EBSD) method. Specifically, based on the crystal orientation map measured by the EBSD method, image analysis software is used to identify each crystallite present on the surface of the silver alloy thin film. The circle equivalent diameter of each crystallite is calculated from its area. The area average of the circle equivalent diameters of each crystallite is calculated. This area average is defined as the "average crystallite diameter of the crystallites in a cross section parallel to the surface of the silver alloy thin film." Note that the "area average" means an average value weighted by area. For example, if a certain crystallite G1 has a circle equivalent diameter D1 and an area A1, and another crystallite G2 has a circle equivalent diameter D2 and an area A2, the area average value D of the circle equivalent diameters of these two crystallites is D=(A1×D1+A2×D2) / (A1+A2). The measurement device used for the EBSD method is the Hitachi High-Tech SU-70. The image analysis software used was ImageJ (National Institutes of Health, USA). Measurements were performed at three points on the surface of the silver alloy thin film using the EBSD method. The measurement field of view for each was 18 μm. 2 Let us assume that.
[0017] The shape of the crystallite 11a in the cross section perpendicular to the surface of the silver alloy thin film 10 is not particularly limited. The crystallite 11a in the cross section perpendicular to the surface of the silver alloy thin film 10 can be observed, for example, as shown in FIG. 1B. As shown in FIG. 1B, the crystallite 11a in the cross section perpendicular to the surface of the silver alloy thin film 10 may extend from the back surface (for example, the CaCO3 substrate side) of the silver alloy thin film 10 toward the front surface. In other words, the silver alloy thin film 10 may have columnar crystallites 11a extending from the back surface to the front surface. The columnar crystallites 11a may extend continuously from the back surface to the front surface of the silver alloy thin film 10, or may extend intermittently. That is, the length of the columnar crystallites 11a (the length in the direction perpendicular to the surface of the silver alloy thin film 10, the height of the column) may be equal to the thickness of the silver alloy thin film 10, or may be shorter than that.
[0018] 1.3 Oxide particles 1, in the silver alloy thin film 10, a plurality of oxide particles 12 may be present at the grain boundary 11b of the crystallite 11a. The oxide particle 12 has a pinning function for the crystallite 11a. In other words, the presence of a plurality of oxide particles 12 at the grain boundary 11b can more appropriately suppress the growth of the crystallite 11a, for example, when the silver alloy thin film 10 is held in a medium-low temperature range (for example, about 200°C to about 500°C) for a long period of time.
[0019] The oxide particles 12 may contain one or both of Al and Mg as constituent elements. In this case, the oxide particles 12 may contain another element M' in addition to one or both of Al and Mg and O. That is, the oxide particles 12 may be an Al oxide, an Mg oxide, a composite oxide of Al and Mg, a composite oxide of Al and element M', a composite oxide of Mg and element M', or a composite oxide of Al, Mg and element M'. The element M' is not particularly limited, and may be at least one selected from, for example, Cu, La, Ce, Nd, Zr, Li, Mn, Si and Zn. When the oxide particles 12 contain one or both of Al and Mg, the oxide particles 12 are stably present at the grain boundaries 11b of the crystallites 11a of the silver alloy phase 11, and the above-mentioned pinning effect is easily exhibited appropriately. For example, as described below, when the silver alloy thin film 10 is formed by sputtering, Al and Mg are likely to be generated and precipitated as oxides at the grain boundaries of the silver alloy, and function appropriately as pinning particles for the crystallites 11a, making it easy to refine the crystallites 11a. Furthermore, even after the silver alloy thin film 10 is heat-treated, the crystallite diameter can be maintained small.
[0020] The particle diameter of the oxide particles 12 may be a size that allows the oxide particles 12 to exist in the grain boundaries 11b of the crystallites 11a. For example, the average particle diameter of the oxide particles 12 may be 1 nm or more and 100 nm or less. The average particle diameter of the oxide particles 12 may be smaller than the average crystallite diameter of the crystallites 11a. For example, the average particle diameter D P and the average crystallite diameter D of the crystallite 11a CCompared to D P / D C may be 0.01 or more and 1 or less.
[0021] The "average particle size of oxide particles" is determined by SEM, TEM, etc. Specifically, a two-dimensional image of the silver alloy thin film is obtained by SEM or TEM, and the positions and sizes of multiple oxide particles in the two-dimensional image are identified by elemental analysis, etc. The biaxial geometric mean diameter, which is the square root of the product of the major axis diameter and the minor axis diameter of each of the multiple oxide particles contained in the two-dimensional image, is calculated, and the number average value is identified as the "particle size of the oxide particles."
[0022] When the oxide particles 12 are present at the grain boundaries 11b in the silver alloy thin film 10, the volume ratio of the oxide particles 12 in the silver alloy thin film 10 is not particularly limited. The fewer the oxide particles 12, the smaller the pinning effect. In addition, the more the oxide particles 12, the finer the crystallites 11a become, but the more brittle the silver alloy thin film 10 becomes, and there is a concern of cracks and breaks due to thermal stress concentration during heating and cooling. According to the findings of the present inventors, when the volume ratio of the oxide particles 12 in the silver alloy thin film 10 is 0.1 volume % or more and 15.0 volume % or less, a good pinning effect is obtained, the crystallites 11a are more optimally fined without cracks or breaks due to embrittlement of the silver alloy thin film, and the oxygen permeability coefficient of the silver alloy thin film 10 becomes even larger. The volume fraction of the oxide particles 12 may be 0.2 vol % or more, or 0.3 vol % or more, and may be 10.0 vol % or less, 8.0 vol % or less, 6.0 vol % or less, 4.0 vol % or less, or 2.0 vol % or less.
[0023] The "volume ratio of oxide particles in the silver alloy thin film" is determined by TEM. Specifically, a thin film sample cut into a 100 nm thick slice by FIB method is observed by TEM at 1 million times magnification, and the obtained image is binarized with ImageJ to measure the oxide particle size and volume ratio. In addition, the oxide species is determined by SEM-EDX method. That is, the oxide constituent elements are identified from the characteristic X-ray wavelength generated when the oxide particles are irradiated with an electron beam.
[0024] 1.4 Oxygen permeability coefficient The silver alloy thin film 10 has a high oxygen permeability coefficient by having the fine crystallites 11a as described above. For example, the silver alloy thin film 10 has a high oxygen permeability coefficient of 2.0×10 at 350° C. -5 Ncc-O2 / cm / min / atm 0.5 The silver alloy thin film 10 having such an oxygen permeability coefficient may have a thickness of 1 μm, and when the air pressure on one side of the thin film is set to 10 atm, pure oxygen at 1 atm can be delivered from the other side at a rate of 0.1 Ncc-O 2 / cm 2 / min or more, making the thin film more practical. The oxygen permeability coefficient of the silver alloy thin film 10 is 3.0×10 -5 Ncc-O2 / cm / min / atm 0.5 That's it, 4.0 x 10 -5 Ncc-O2 / cm / min / atm 0.5 That's it, 5.0 x 10 -5 Ncc-O2 / cm / min / atm 0.5 That's it, 6.0 x 10 -5 Ncc-O2 / cm / min / atm 0.5 That's it, 7.0 x 10 -5 Ncc-O2 / cm / min / atm 0.5 That's it, 8.0 x 10 -5 Ncc-O2 / cm / min / atm 0.5 That's it, 9.0 x 10 -5 Ncc-O2 / cm / min / atm 0.5 or more than 1.0×10 -4 Ncc-O2 / cm / min / atm 0.5 It may be more than that.
[0025] 1.5 Nanoindentation hardness The silver alloy thin film 10 has improved nanoindentation hardness and excellent strength due to the fine crystallites 11a as described above. For example, the silver alloy thin film 10 may have a nanoindentation hardness of 2.0 GPa or more. The nanoindentation hardness may be 2.1 GPa or more, 2.2 GPa or more, 2.3 GPa or more, 2.4 GPa or more, or 2.5 GPa or more, and may be 5.0 GPa or less, 4.8 GPa or less, or 4.6 GPa or less. If a porous ceramic with a pore diameter of 1 mm is assumed as a carrier for a thin film when 1 atm pure oxygen is selectively separated from 10 atm high-pressure air by a silver alloy thin film with a thickness of 2 μm, if the indentation hardness of the thin film at room temperature is 2.0 GPa or more, the deformation strain of the thin film caused by the pressure difference will be within the range of elastic deformation.
[0026] The "nanoindentation hardness of the silver alloy thin film" refers to the nanoindentation hardness after the heat treatment at 350°C. Details of the heat treatment at 350°C are as described above. The nanoindentation hardness of the silver alloy thin film is obtained by fixing the thin film to a nanoindentation tester and measuring the hardness and elastic modulus at a maximum load of 300μN according to ISO14577. The sample temperature is room temperature. The maximum load is adjusted and determined so that the indentation depth is 1 / 10 or less of the film thickness. Ten measurement points are arbitrarily selected in the thin film. For example, when the maximum load is set to 300μN, the load is increased at a rate of +60μN / s for 5 seconds, held at the maximum load of 300μN for 2 seconds, and then removed at a rate of -60μN / s for 5 seconds. A Bruker TI980 triboindenter is used as the nanoindentation hardness measuring device.
[0027] 1.6 Film Thickness The thickness of the silver alloy thin film 10 is not particularly limited, and an appropriate thickness may be selected depending on the application. However, the thinner the silver alloy thin film 10, the greater the oxygen permeation amount. The oxygen permeability coefficient of the silver alloy thin film 10 does not depend on the film thickness. The silver alloy thin film 10 may have a thickness of, for example, 0.1 μm or more and 100 μm or less. In particular, when the thickness of the silver alloy thin film 10 is 50 μm or less, 40 μm or less, 30 μm or less, 20 μm or less, or 10 μm or less, the cost of the silver alloy thin film 10 is reduced and the practicality is more excellent. The silver alloy thin film 10 may be used as a free-standing film, or may be supported on a porous substrate or the like as described later. When the silver alloy thin film 10 is thin, for example, 50 μm or less, it is difficult to use the silver alloy thin film 10 as a free-standing film. In this case, the silver alloy thin film 10 may be supported on a porous substrate or the like.
[0028] 1.7 Electrical resistivity The silver alloy thin film 10 has a thickness of, for example, 5.0×10 -8 The silver alloy thin film 10 may have an electrical resistivity of 10.0×10 -8 Ωm or less, or 9.5×10 -8 It may be Ωm or less. The electrical resistivity of the silver alloy thin film can be determined by a four-probe method. The equipment used is, for example, a K-504RB type manufactured by Kyowa Riken Co., Ltd. as a four-probe unit, and a Keithley 2450 as a voltage and current application measuring instrument. The applied current range is -1A to +1A, and the measurement voltage is on the order of several mV or less. The resistance value R is calculated from the VI curve, the film thickness t is determined from cross-sectional SEM observation of the thin film, and the electrical resistivity ρ (Ωm) is calculated by the following formula. The measurement of the film thickness t will be described in detail in the Examples. ρ=R×4.532×t
[0029] 1.7 Application The silver alloy thin film 10 has a high oxygen permeability coefficient. Therefore, the silver alloy thin film 10 can be used, for example, as an oxygen permeable membrane. It is considered that the oxygen selective permeation method using an oxygen permeable membrane can produce the same amount of pure oxygen as the cryogenic method or the PSA method, even on a small scale. The general configuration of a production facility for producing pure oxygen by the oxygen selective permeation method using an oxygen permeable membrane is publicly known. A detailed description will be omitted here.
[0030] 2. Manufacturing method of silver alloy thin film The present inventors have focused on the sputtering method as a method for obtaining nm-sized crystallites in a silver alloy thin film. As a sputtering method, a reactive sputtering method is known in which Ag or Cu is used as a target material, O2 or N2 is mixed with Ar, which is an inert gas, to form a film of Ag2O, Cu2O, Cu3N, etc. As a reactive sputtering method, a method of forming a mixed thin film of Ag and its oxide Ag2O, and a method of forming an Ag2O oxide thin film by completely oxidizing the parent phase are known. The present inventors have developed these findings and have intensively studied a method for producing a silver alloy thin film by the sputtering method. Specifically, the present inventors have developed a "sputtering film formation simultaneous internal oxidation method" in which a sputtering target containing Ag as well as Al and / or Mg is used when producing a silver alloy thin film, and Al and / or Mg are internally oxidized at the same time as the sputtering film formation, and have conducted various studies. As a result, it was found that by adjusting the alloy composition of the sputtering target, the sputtering deposition rate, and the Ar and O2 partial pressures during sputtering deposition, oxide particles containing Al and / or Mg as constituent elements are dispersed at the grain boundaries of the crystallites of the silver alloy phase during deposition of the silver alloy thin film, and the growth of the crystallites of the silver alloy phase can be significantly suppressed by the pinning effect. It was also found that the silver alloy thin film thus obtained maintains a small crystallite diameter even after heat treatment at 350°C.
[0031] That is, a method for producing a silver alloy thin film according to one embodiment includes forming a silver alloy thin film by using an Ag alloy as a sputtering target and performing sputtering under the supply of Ar gas and O2 gas so that the condition of the following formula (1) is satisfied. (1.6×10 -6 ×C Al -3.7×10 -8 ×C Al 2 +8.2×10 -7 ×C Mg )×SR≦P O2 ≦P Ar (1) Where: C Al is the Al concentration (at%) of the sputtering target, C Mg is the Mg concentration (at%) of the sputtering target, SR is the deposition rate (nm / min), P Ar is the Ar partial pressure in the sputtering atmosphere (Pa), P O2 is the O2 partial pressure in the sputtering atmosphere (Pa), The Al concentration C Al is 0 at% or more and 7.0 at% or less, The above Mg concentration C Mg is 0 at% or more and 10.0 at% or less, The Al concentration C Al and the Mg concentration C Mg The sum of these is equal to or greater than 0.10 at % and equal to or less than 10.0 at %.
[0032] More specifically, the method for producing a silver alloy thin film according to one embodiment includes the steps of: A substrate 101 is placed inside a sputtering apparatus 100 using Ar as a plasma source. Placing a sputtering target 102 inside a sputtering apparatus 100; Introducing Ar gas and O2 gas into the sputtering apparatus 100 at predetermined concentrations; and forming a silver alloy thin film 10 on the substrate 101; The sputtering target 102 is an Ag alloy. The silver alloy thin film 10 is formed on the substrate 101 by sputtering so that the condition of the above formula (1) is satisfied.
[0033] 2.1 Substrate In this embodiment, a silver alloy thin film is formed on a substrate by sputtering. The substrate may be a porous stainless steel substrate, a porous alumina substrate, a substrate made of processed glass such as borosilicate or quartz, a NaCl substrate, a CaCO3 substrate, or the like, but is not limited thereto. When the substrate on which the silver alloy thin film is formed is porous, the composite of the silver alloy thin film and the substrate can be directly applied to the oxygen permeation device. On the other hand, when the substrate is a solid substrate, it is preferable to remove the substrate after forming the silver alloy thin film in order to separate the silver alloy thin film. As a method for removing the substrate, a mechanical peeling method can be mentioned. Alternatively, for example, the NaCl substrate or the CaCO3 substrate can be easily detached from the silver alloy thin film by dissolving it in water or acid (e.g., phosphoric acid, etc.). Furthermore, since the thermal expansion coefficient of the single crystal CaCO3 substrate in the direction of the plate surface along the c-axis is close to the thermal expansion coefficient of Ag, the difference in thermal contraction between the substrate and the silver alloy thin film during cooling after sputtering is small, and deformation of the thin film after the substrate is peeled off can be minimized.
[0034] 2.2 Sputtering targets In this embodiment, in the film formation process by sputtering, gas molecules such as argon that have been positively ionized by an applied voltage are collided with the surface of a sputtering target (film formation raw material) to flick off atoms on the surface of the target, and the atoms are collided and evaporated onto a substrate placed near the target to form a silver alloy thin film that reflects the composition of the target. A silver alloy can be used as the target. Specifically, the sputtering target has an Al concentration of C Al is 0 at% or more and 7.0 at% or less, and Mg concentration C Mg is 0 at% or more and 10.0 at% or less, and the Al concentration C Al and the Mg concentration C MgThe sum of Al and Mg is preferably 0.10 at% or more and 10.0 at% or less. By using such a sputtering target and mixing O2 gas with Ar gas, which is a supply gas for generating plasma, and performing sputtering, a large number of fine oxides are preferentially generated at the grain boundaries at the same time as film formation, the grain boundaries can be pinned, and the average crystallite diameter in a cross section parallel to the surface of the silver alloy thin film becomes 100 nm or less. In addition, the crystallites become columnar in a cross section perpendicular to the surface of the silver alloy thin film. By having the total concentration of Al concentration and Mg concentration of the sputtering target be 0.10 at% or more, the number density of oxide particles becomes sufficient, and it becomes easier to pin the grain boundaries of the silver alloy thin film and maintain the average crystallite diameter at 100 nm or less. In addition, by having the total concentration be 10.0 at% or less, excessive oxidation heat generation is unlikely to occur during sputtering, and melting of the silver alloy thin film can be prevented.
[0035] 2.3 Gas partial pressure during sputtering In this embodiment, the inside of the reactor during sputtering is, for example, heated with 0.1 to 10 Pa Ar gas plasma to form a film by sputtering. Al , C Mg , S.R., P. Ar , and P O2 By carrying out the film formation process under the conditions as shown in the above formula (1), a large number of fine oxides are preferentially generated at the grain boundaries at the same time as the film is formed, thereby pinning the grain boundaries, and the average crystallite size in a cross section parallel to the surface of the silver alloy thin film becomes 100 nm or less. In this embodiment, nano-sized oxides containing Al and / or Mg can be rapidly generated at the grain boundaries of the silver alloy phase during sputtering. In order to supersaturate the oxygen atoms at the grain boundaries, eliminate the dissolved Al and dissolved Mg near the grain boundaries, prevent Ostwald ripening of oxide particles, and maintain fine crystal grains for a long period of time during oxygen permeation, it is necessary to use P. O2 must be equal to or greater than the lower limit of the above formula (1). O2 The upper limit of P is set to avoid a decrease in sputtering efficiency due to oxidation of the target surface during sputtering. Ar The following is the P during film formation. O2can be controlled by adjusting the mixture ratio of O2 gas to Ar gas, which is the supply gas for generating plasma.
[0036] 3. Complex As described above, the silver alloy thin film 10 according to one embodiment may be used in a state in which it is supported on a porous substrate. FIG. 3 shows a schematic configuration of the composite 50. As shown in FIG. 3, the composite 50 has a porous substrate 20 and a silver alloy thin film 10. Here, the silver alloy thin film 10 is supported on the porous substrate 20. The silver alloy thin film 10 has the above configuration. The porous substrate 20 may be any substrate capable of appropriately supporting the silver alloy thin film 10, and may be, for example, one of a porous metal substrate such as a porous stainless steel substrate and a porous ceramic substrate such as a porous alumina substrate. The shape of the pores in the porous substrate 20 may be any shape that allows gas to pass through. As a method for supporting the silver alloy thin film 10 on the porous substrate 20, for example, the sputtering method as described above may be mentioned. That is, the silver alloy thin film 10 may be formed on the surface of the porous substrate 20 by sputtering. Although FIG. 3 shows a form in which one surface of the silver alloy thin film 10 is supported by the porous substrate 20, the silver alloy thin film 10 may be supported by being sandwiched between two porous substrates 20.
[0037] 4. How oxygen is produced As described above, by using the silver alloy thin film 10 as an oxygen permeable membrane, for example, oxygen can be selectively separated from a mixed gas containing oxygen. That is, as shown in FIG. 4, the method for producing oxygen according to an embodiment includes supplying a mixed gas containing oxygen to one side of the silver alloy thin film 10, and permeating the oxygen in the mixed gas to the other side of the silver alloy thin film 10. For example, air is an example of the mixed gas containing oxygen. For example, the driving force for permeating the oxygen in the mixed gas to the other side of the silver alloy thin film 10 is an oxygen partial pressure difference. In one embodiment, the difference between the oxygen partial pressure in the mixed gas supplied to one side of the silver alloy thin film 10 and the oxygen partial pressure on the other side may be, for example, 0.1 atm or more and 10 atm or less. In one embodiment, the pressure of the mixed gas supplied to one side of the silver alloy thin film 10 may be 1 atm or more and 10 atm or less. In the method for producing oxygen according to an embodiment, it is preferable to control the temperature of the mixed gas and the silver alloy thin film 10 to 200° C. or more and 500° C. or less.
[0038] As described above, by miniaturizing the average crystallite diameter in the cross section parallel to the surface of the silver alloy thin film 10 to 100 nm or less, the area ratio of the grain boundary 11b, which is the high-speed diffusion flow path, becomes large (for example, 1 to 30%), and the oxygen permeability coefficient of the silver alloy thin film 10 in the medium to low temperature range becomes, for example, 2.0 × 10 -5 (Ncc-O2 / cm / min / atm 0.5 For example, when high-pressure air of 10 atm is introduced to one side of the silver alloy thin film 10 and pure oxygen of 1 atm is collected on the other side of the thin film, the oxygen separation rate J O2 is 0.1Ncc-O2 / cm 2 / min or more, which is a very practical value. EXAMPLES
[0039] The present invention will be further described below with reference to examples, but the present invention is not limited to the following examples. The present invention can adopt various conditions as long as it does not deviate from the gist of the invention and achieves its object.
[0040] 1. Preparation of silver or silver alloy thin films As described below, a silver thin film or a silver alloy thin film for evaluation was produced through the steps of a substrate cleaning step, (a target preparation step), a substrate setting step, a film formation step, and a substrate peeling step.
[0041] 1.1 Substrate cleaning process A CaCO3{10-10} single crystal substrate (manufactured by Neotron, where the number "-1" on the left means "1 with a bar drawn on it") was used as the substrate for sputtering. Its dimensions are 15 mm square x 1 mm thick, and its surface roughness is Ra<2 nm. To prevent moisture absorption, it was stored sealed in Ar gas, and was opened and used immediately before film formation according to the substrate installation process below.
[0042] 1.2 Target preparation process The sputtering target is a 5 cm diameter target manufactured by Mitsubishi Materials Corp. The target is made of pure Ag or an Ag-0-2 at% Cu-0.1-10 at% Al-0-5 at% Mg alloy.
[0043] 1.3 Board installation process In a room conditioned to 19-22°C and a relative humidity of 40% or less, the sputtering apparatus was opened to atmospheric pressure, the CaCO3 substrate was unpacked and immediately placed in the sputtering apparatus, and the apparatus was evacuated. Next, Ar-5%CO2 was introduced into the apparatus up to 0.5 atm (absolute pressure), and the apparatus was heated at 150°C for 10 minutes to dehydrate the adsorbed moisture on the surface of the CaCO3 substrate. After that, the apparatus was evacuated once.
[0044] 1.4 Film formation process Ar-0-10% O2 gas was supplied into the sputtering device at a total pressure of 1 Pa and a flow rate of 1 sccm (standard volumetric flow rate normalized under standard conditions of 1 atm and 0°C, standard cubic centimeter / min), and film formation was carried out for 10 minutes at an output of 50-100 W. The film formation rate SR was 100-240 nm / min and the film thickness was 1.0-2.4 μm. The gas concentration in the sputtering device was constantly measured using a mass spectrometer (Canon Anelva M-101QA-TDM), and the oxygen partial pressure P O2 to 10 -5 ~10 -1 The pressure was controlled in the Pa range.
[0045] 1.5 Substrate peeling process After the film formation, the substrate was immersed in a 5% aqueous solution of phosphoric acid to peel off the silver or silver alloy thin film from the substrate.
[0046] 2. Evaluation methods for silver thin films and silver alloy thin films The average crystallite size in a cross section parallel to the plane direction of the thin film prepared as described above, and the average particle size and volume fraction of oxide particles contained in the thin film were measured by electron backscatter diffraction (EBSD) and transmission electron microscopy (TEM). The hardness of the thin film was measured by a nanoindentation test. The electrical resistivity ρ of the thin film was measured by a four-point probe method. To further investigate the heat resistance of the thin film, the above characteristic values were measured again after heat treatment in air at 350°C for 1 hour, and the values before and after the heat treatment were compared. The selective oxygen transmission rate of the thin film was then measured. The specific details of each are as follows:
[0047] 2.1 Electron backscatter diffraction method The average crystallite size in the cross section parallel to the plane direction of the prepared thin film, and the average grain size and volume fraction of the oxide grains contained in the thin film were measured by electron backscatter diffraction (EBSD). Specifically, the average crystal grain size in area fraction was calculated based on the crystal orientation map measured by EBSD. The evaluation was performed in the same manner in three different fields of view. The equipment used was a Hitachi High-Tech SU-70. The image analysis software used was ImageJ, manufactured by the National Institutes of Health.
[0048] 2.2 Nanoindentation test The thin film formed on the substrate was fixed to a nanoindentation tester without peeling it off from the substrate, and hardness and elastic modulus were measured at a maximum load of 300μN according to ISO14577. The maximum load was adjusted so that the indentation depth was 1 / 10 or less of the film thickness. Ten measurement points were selected arbitrarily on the film sample. The equipment used was a Bruker TI980 triboindenter. In addition, assuming that a porous ceramic with a pore diameter of 1mm is used as a support for a thin film when selectively separating 1atm pure oxygen from 10atm high-pressure air using a 2μm-thick Ag alloy thin film, it has been confirmed that if the indentation hardness of the thin film at room temperature is 2.0GPa or more, the deformation strain of the thin film caused by the pressure difference will be within the elastic deformation range.
[0049] 2.3 Four-probe method The electrical resistivity of the above thin film was determined by the four-probe method. The equipment used was a Kyowa Riken K-504RB model four-probe unit and a Keithley 2450 voltage and current application measuring device. The applied current range was -1A to +1A, and the measurement voltage was on the order of a few mV or less. The resistance value R was calculated from the VI curve. The film thickness t was determined from cross-sectional SEM observation of the thin film, and the electrical resistivity ρ (Ωm) was calculated using the following formula. ρ=R×4.532×t Here, the method for measuring the film thickness t is as follows. The Ag alloy thin film formed on the CaCO3 substrate was placed on a Mo mesh, and carbon deposition was performed to protect the surface of the thin film. The film was then processed into a 100 nm-thick slice sample with a focused Ga ion beam, and immediately observed with an SEM to determine the film thickness t. The measurements were performed at three randomly selected points in the center of the thin film, spaced at least 1 μm apart, and the average of the measured values was taken as the film thickness t. The focused ion beam processing SEM observation device used for the measurements was a Cryo FIB SEM NB5000 manufactured by Hitachi High-Tech Corporation.
[0050] 2.4 Heat treatment conditions The heat treatment conditions for the thin film were as follows: the Ag alloy thin film was inserted into a heating furnace in an air atmosphere, heated from room temperature (25°C) to 350°C at a rate of 30°C / min, held at 350°C for 1 hour, and then removed from the furnace and cooled in the air.
[0051] 2.5 Oxygen transmission rate measurement The CaCO3 single crystal substrate was dissolved by immersing it in a 5% phosphoric acid aqueous solution for 48 hours to obtain an Ag alloy thin film with a thickness of 1 to 2.4 μm and a diameter of 10 mm. The Ag alloy thin film was placed on a porous alumina plate (porous refractory) with a smooth surface, an average pore size of 50 μm, and a porosity of 70%, and attached to an alumina tube with heat-resistant adhesive Pyroduct 597 manufactured by Aremco to ensure airtightness. Using the device shown in Figure 5, 1 atm of air was flowed on the primary side and 1 atm of He was flowed on the secondary side under PO2 differential pressure conditions, and the oxygen concentration in the He sweep gas flowing on the secondary side at 150 Ncc / min in the range of 200 to 500°C was measured by gas chromatography to determine the oxygen gas flow rate J that permeated the alloy membrane. O2 (Ncc-O2 / cm 2 The gas chromatograph used was an Agilent 490 Micro GC manufactured by GL Sciences Inc. O2 The value of the primary O2 partial pressure P O2 (I) and secondary O2 partial pressure P O2 (II) The oxygen permeability coefficient K(Ncc-O2 / cm / min / atm) 0.5 ) was converted to J O2 =D S (√P O2 (I)-√P O2 (II)) / d K=D·S =J O2 d / (√P O2 (I)-√P O2 (II)
[0052] 3. Evaluation results Tables 1 to 3 below show the sputtering deposition conditions and the evaluation results of the obtained thin films. For reference, FIG. 6 shows examples of EBSD analysis images of the surface of the thin film. FIG. 6(A) shows the thin film with an average crystallite diameter of <50 nm, and FIG. 6(B) shows the thin film with an average crystallite diameter of 220 nm. FIG. 7 shows an example of a TEM image of the cross section of the thin film. FIG. 7(A) shows a TEM image of the longitudinal section (cross section perpendicular to the surface direction) of the thin film, and FIG. 7(B) shows a TEM image of the 1 / 2 thickness section (cross section parallel to the surface direction). As shown in FIG. 7, simultaneous internal oxidation during sputtering causes oxides (black particles) of several nm in size to be dispersed at the grain boundaries of the silver alloy phase, which pin the crystallites of the silver alloy phase and maintain fine crystallites.
[0053] In addition, in Table 1 below, "Lower limit P O2 " is calculated by the following formula (A) and "Actual P O2 " is the actual oxygen partial pressure in the sputtering atmosphere. Lower limit P O2 =(1.6×10 -6 ×C Al -3.7×10 -8 ×C Al 2 +8.2×10 -7 ×C Mg ) × SR ···(A) Where: C Al is the Al concentration (at%) of the sputtering target, C Mg is the Mg concentration (at%) of the sputtering target, SR is the deposition rate (nm / min).
[0054] [Table 1]
[0055] [Table 2]
[0056] [Table 3]
[0057] In addition, in the above Tables 1 to 3, some numerical values are underlined for ease of understanding, but this does not limit the present invention. The results shown in Tables 1 to 3 reveal the following. Samples No. 7 and 12 generated excessive heat during sputtering, causing some melting, making it difficult to obtain an appropriate thin film. This was probably due to the Al concentration in the sputtering target being too high. In samples No. 13-15, 23, 24, 29, 30 and 43, the average crystallite diameter in the cross section parallel to the surface of the silver alloy thin film exceeded 100 nm, and the oxygen permeability coefficient decreased. It is considered that because the oxygen partial pressure during sputtering was insufficient, the oxygen atoms at the crystal grain boundaries in the thin film did not become supersaturated, the solid solution Al and solid solution Mg near the grain boundaries were maintained, the Ostwald ripening of oxide particles occurred, and fine crystal grains could not be maintained. In samples No. 16-18, 26-28, 33, 34, 40-43 and 49, the average crystallite diameter in the cross section parallel to the surface of the silver alloy thin film exceeded 100 nm, and the oxygen permeability coefficient was small. It is considered that the total concentration of Al and Mg in the sputtering target was too low, so that the amount of fine oxides generated during film formation was small, and the grain boundaries could not be pinned. Sample No. 53 generated excessive heat during sputtering, and some of it melted, making it difficult to obtain an appropriate thin film. This was probably due to the total concentration of Al and Mg in the sputtering target being too high. In contrast, in samples Nos. 1 to 6, 8 to 11, 19 to 22, 25, 31, 32, 35 to 39, 44 to 48, and 50 to 52, the average crystallite diameter in the cross section parallel to the surface of the silver alloy thin film was 100 nm or less, and the oxygen permeability coefficient was large. It is considered that by using a sputtering target containing Al and Mg at a predetermined concentration during sputtering and setting the oxygen partial pressure to a predetermined level or higher, a large number of fine oxides were generated during film formation, and the grain boundaries were pinned.
[0058] It can be seen from the results shown in Tables 1 to 3 that a silver alloy thin film that satisfies the following (1) has a relatively improved oxygen permeability coefficient. (1) The silver alloy phase is composed of a plurality of crystallites, and the average crystallite diameter in a cross section parallel to the surface of the silver alloy thin film is 100 nm or less.
[0059] The results shown in Tables 1 to 3 show that a silver alloy thin film that satisfies the following (2) to (4) in addition to the above (1) has a further improved oxygen permeability coefficient. (2) The silver alloy phase has multiple oxide particles at the grain boundaries of the crystallites. (3) The oxide particles contain one or both of Al and Mg as constituent elements. (4) The volume ratio of the oxide particles in the silver alloy thin film is 0.1 volume % or more and 15.0 volume % or less.
[0060] The results shown in Tables 1 to 3 show that a silver alloy thin film satisfying the above (1) can be produced by a production method that satisfies the following (A) and (B). (A) Using an Ag alloy as a sputtering target, sputtering is performed under the supply of Ar gas and O2 gas so that the condition represented by the following formula (1) is satisfied, thereby forming a silver alloy thin film. (1.6×10 -6 ×C Al -3.7×10 -8 ×C Al 2 +8.2×10 -7 ×C Mg )×SR≦P O2 ≦P Ar (1) Here, C Al is the Al concentration (at%) of the sputtering target, and C Mg is the Mg concentration (at%) of the sputtering target, SR is the deposition rate (nm / min), and P Ar is the Ar partial pressure in the sputtering atmosphere (Pa), and P O2is the O2 partial pressure (Pa) in the sputtering atmosphere. (B) The above Al concentration C Al is 0 at% or more and 7.0 at% or less, and the Mg concentration C Mg is 0 at% or more and 10.0 at% or less, and the Al concentration C Al and the Mg concentration C Mg The sum of these is 0.10 at % or more and 10.0 at % or less. [Explanation of symbols]
[0061] 10 Silver alloy thin film 11 Silver alloy phase 11a Crystallite 11b Grain boundary 12 Oxide particles 20 Porous substrate 50 Complex 100 Sputtering Equipment 101 Substrate 102 Sputtering target
Claims
1. A silver alloy thin film having a silver alloy phase, The silver alloy phase is composed of a plurality of crystallites, The average crystallite diameter of the crystallites in a cross section parallel to the surface of the silver alloy thin film is 100 nm or less. Silver alloy thin film.
2. A plurality of oxide particles are present at the grain boundaries of the crystallites. The silver alloy thin film according to claim 1 .
3. The oxide particles contain one or both of Al and Mg as constituent elements. The silver alloy thin film according to claim 2.
4. a volume ratio of the oxide particles in the silver alloy thin film is 0.1 volume % or more and 15.0 volume % or less; The silver alloy thin film according to claim 3.
5. At 350° C., 2.0×10 -5 Ncc-O 2 / cm / min / atm 0.5 Having an oxygen permeability coefficient of equal to or greater than The silver alloy thin film according to claim 1 .
6. Having a nanoindentation hardness of 2.0 GPa or more; The silver alloy thin film according to claim 1 .
7. Used as an oxygen permeable membrane, The silver alloy thin film according to claim 1 .
8. Having a thickness of 0.1 μm or more and 100 μm or less, The silver alloy thin film according to claim 1 .
9. A Ag alloy was used as the sputtering target, and Ar gas and O 2 sputtering is performed under the supply of a gas such that the condition of the following formula (1) is satisfied, thereby forming a silver alloy thin film; A method for producing a silver alloy thin film, comprising: (1.6 x 10 -6 ×C Al -3.7 x 10 -8 ×C Al 2 +8.2 x 10 -7 ×C Mg ) × SR≦P O2 ≦P Ar ...(1) Where: C Al is the Al concentration (at%) of the sputtering target, C Mg is the Mg concentration (at%) of the sputtering target, SR is the deposition rate (nm / min), P Ar is the Ar partial pressure in the sputtering atmosphere (Pa), P O2 is the O in the sputtering atmosphere 2 is the partial pressure (Pa), The Al concentration C Al is 0 at% or more and 7.0 at% or less, The Mg concentration C Mg is 0 at% or more and 10.0 at% or less, The Al concentration C Al and the Mg concentration C Mg The sum of these is equal to or greater than 0.10 at % and equal to or less than 10.0 at %.
10. A composite material having a porous substrate and a silver alloy thin film, The silver alloy thin film is supported on the porous substrate, The silver alloy thin film is according to any one of claims 1 to 8. Complex.
Citation Information
Patent Citations
Oxygen permeable membranes
US3359705A
Process and apparatus for selectively permeating oxygen
US3509694A
Oxygen separation process
US3550355A
Process and device for obtaining pure oxygen
US5108465A