Multi-layer resin tube

The multilayer resin pipe with a polyolefin resin and coated carbon fibers, enhanced by a crystal nucleating agent, addresses the high thermal expansion of resin pipes, reducing costs and maintaining structural integrity.

JP2024169340APending Publication Date: 2024-12-05INOAC HOUSING & CONSTR MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024078076
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional resin pipes exhibit a large coefficient of linear expansion, leading to bending issues under temperature changes, and adding inorganic fillers to reduce this expansion increases costs.

Method used

A multilayer resin pipe design featuring an inner layer of resin and an outer layer composed of polyolefin resin with coated carbon fibers treated by an epoxy or polyurethane sizing agent, combined with a crystal nucleating agent, to enhance bonding and reduce thermal expansion.

Benefits of technology

The design achieves a smaller coefficient of linear expansion compared to conventional composites, maintaining structural integrity while minimizing material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169340000001_ABST
    Figure 2024169340000001_ABST
Patent Text Reader

Abstract

To provide a new multi-layer resin tube containing resin and carbon fiber, and indicating a small linear expansion coefficient even when a content of the carbon fiber is small.SOLUTION: A multi-layer resin tube comprises an inner layer, and an outer layer arranged outside the inner layer. The inner layer comprises a resin layer containing resin. The outer layer comprises a composite layer containing polyolefin resin, coated carbon fiber obtained by treating a surface of the carbon fiber with an epoxy resin-base sizing agent and / or a polyurethane-base sizing agent, and a crystal core agent. It is preferable that the multi-layer resin tube has a component weight ratio of the outer layer of 5% or more and 95% or less. However, the component weight ratio (%) of the outer layer refers to a ratio (=t2×100 / (t1+t2)) of thickness t2 of the outer layer to the sum of thickness t1 of the inner layer and the thickness t2 of the outer layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multi-layer resin pipe, and more specifically to a multi-layer resin pipe having an inner layer made of resin and an outer layer made of a composite material containing resin and carbon fiber. [Background technology]

[0002] Conventionally, various pipes such as water supply pipes, hot water supply pipes, drainage pipes, air conditioning pipes in buildings, gas pipes, etc. (a) Resin pipes such as polyolefin pipes and polyvinyl chloride pipes, (b) Metal pipes such as steel pipes and copper pipes (c) Metal pipes with resin lining on the inside or outside etc. are used.

[0003] Of these, plastic pipes are: (A) It is lighter than metal pipes. (B) Less corroded than metal pipes (C) It has a larger coefficient of linear expansion than metal pipes. (D) Less heat resistant than metal pipes It has the following features: Therefore, when a plastic pipe is used in an environment with large temperature changes, if both ends of the plastic pipe are fixed, the plastic pipe may bend significantly due to thermal expansion. On the other hand, if the plastic pipe is connected using an expansion joint that absorbs the expansion and contraction of the plastic pipe, the bending of the plastic pipe caused by thermal expansion can be suppressed. However, the use of an expansion joint leads to high costs.

[0004] In order to solve this problem, various proposals have been made in the past. For example, Patent Document 1 states: (a) the inner layer is made of a polyethylene resin layer, (b) The outer layer is a carbon fiber reinforced resin layer containing polyethylene resin, recycled carbon fiber, and imine-modified polyolefin resin. A two-layer pipe is disclosed.

[0005] The same document states: (A) The thermal expansion coefficient of a single-layer pipe made of resin only is 11.3 x 10 -5 / ℃, whereas the thermal expansion coefficient of the two-layer pipe is 6.3×10 -5 / °C, and (B) The imine-modified polyolefin resin contained in the carbon fiber reinforced resin layer has the effect of increasing the adhesive strength between the carbon fiber and the polyethylene resin. is stated.

[0006] In Patent Document 2, (a) The inner layer is made of a vinyl chloride layer, (b) the intermediate layer is made of a layer containing polyvinyl chloride, thermally expandable graphite, and borosilicate glass; (c) The outer layer is made of vinyl chloride. A multi-layer tube is disclosed.

[0007] The same document states: (A) When only borosilicate glass is added to the intermediate layer, heat deformation resistance is obtained, but it is difficult to maintain fire resistance; and (B) By adding both borosilicate glass and thermally expandable graphite to the intermediate layer, a multi-layer pipe with fire resistance and thermal deformation suppression properties can be obtained. is stated.

[0008] As disclosed in Patent Documents 1 and 2, by adding inorganic fillers such as carbon fiber and borosilicate glass to resin, a composite having a linear expansion coefficient smaller than that of the resin can be obtained. However, conventional methods are insufficient in reducing the linear expansion coefficient. In particular, even if the amount of inorganic filler added is the same, there is a problem that the linear expansion coefficient increases as the diameter of the resin pipe increases, and the expansion amount of the resin pipe increases. On the other hand, in order to further reduce the linear expansion coefficient, it is also possible to increase the content of the inorganic filler, but increasing the content of the inorganic filler leads to higher costs. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent Publication No. 2022-072698 [Patent Document 2] JP 2022-052466 A Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a novel multi-layer resin pipe containing resin and carbon fiber. Another object of the present invention is to provide a novel multi-layer resin pipe that exhibits a small linear expansion coefficient even when the carbon fiber content is small. [Means for solving the problem]

[0011] In order to solve the above problems, the multilayer resin pipe according to the present invention comprises: The inner layer, an outer layer disposed outside the inner layer; Equipped with The inner layer is made of a resin layer containing a resin, The outer layer is A polyolefin resin, A coated carbon fiber having a surface treated with an epoxy resin-based sizing agent and / or a polyurethane-based sizing agent; Nucleating agent and The composite layer comprises: Effect of the Invention

[0012] For polyolefin resin, (a) Coated carbon fibers, the surface of which is treated with an epoxy resin-based sizing agent and / or a polyurethane-based sizing agent; and (b) Nucleating agent By adding carbon fiber, a composite having a smaller linear expansion coefficient can be obtained compared to conventional composites. Furthermore, by using such a composite as the outer layer of a multi-layer resin pipe, a multi-layer resin pipe having a small linear expansion coefficient can be obtained even if the carbon fiber content is small.

[0013] The composite of the present invention exhibits a smaller linear expansion coefficient than the conventional composite, because (A) By using coated carbon fiber, the surface of which has been treated with a sizing agent, as a filler, the wettability of the coated carbon fiber with respect to the polyolefin resin is improved, and the coated carbon fiber is easily dispersed uniformly in the polyolefin resin. (B) The polyolefin resin and the carbon fiber are firmly bonded via the sizing agent, and the carbon fiber suppresses the thermal expansion of the polyolefin resin; and (C) The addition of a crystal nucleating agent increases the crystallinity of the polyolefin resin. It is thought that. [Brief description of the drawings]

[0014] [Figure 1] FIG. 4 is a diagram showing the relationship between the composition ratio of the outer layer and the linear expansion coefficient. [Diagram 2] Fig. 2(A) is an optical microscope photograph of the axial cross section and the longitudinal cross section of the outer layer of the two-layered pipe obtained in Example 3. Fig. 2(B) is an optical microscope photograph of the axial cross section and the longitudinal cross section of the outer layer of the two-layered pipe obtained in Example 4-2. [Diagram 3] FIG. 2 is a graph showing the relationship between the composition ratio of the outer layer and the linear expansion coefficient of the two-layered tubes obtained in Examples 6 to 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment of the present invention will be described in detail below. [1. Multilayer resin pipe] The multi-layer resin pipe according to the present invention has the following features: The inner layer, an outer layer disposed outside the inner layer; It is equipped with: Multi-layer resin pipes are (a) a third layer inserted between the inner and outer layers; and / or (b) A fourth layer placed on the outside of the outer layer. It may further comprise:

[0016] [1.1. Inner layer] [1.1.1. Materials] The inner layer is a resin layer containing a resin. In the present invention, the type of resin constituting the inner layer is not particularly limited, and an optimal material can be selected depending on the purpose.

[0017] Examples of the resin constituting the inner layer include: (A) polyolefin resin, (B) Thermoplastic elastomers such as thermoplastic polyurethane elastomers (TPUs), (C) A compound material in which additives are dispersed in polyolefin resin to give it functions such as improving wear resistance and reducing the coefficient of friction. etc.

[0018] Examples of polyolefin resins include: (a) Polypropylene, low density polyethylene (LDPE), high density polyethylene (HDPE), ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, copolymers of ethylene and acrylic esters (e.g., methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate), polybutene, ABS, polyacrylonitrile, polyacetal, polycarbonate, nylon, PET, (b) Halides of the above resins (e.g. polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, PTFE, etc.) etc.

[0019] Examples of the thermoplastic elastomer include urethane thermoplastic elastomer (TPU), styrene thermoplastic elastomer (SBC), olefin thermoplastic elastomer (TPO), and ester thermoplastic elastomer (TPC).

[0020] The inner layer may contain any one of these resins, or may contain two or more of them.

[0021] The resin layer may be made of only resin, or may contain other components in addition to the resin, such as antioxidants, lubricants, dispersants, and antistatic agents.

[0022] Chlorine is used to sterilize drinking water, but in drinking water it exists as hypochlorous acid (HClO), which has a high oxidizing power. HClO is unstable and easily decomposes into HCl and O (nascent oxygen). The generated O oxidizes and deteriorates resins. Carbon materials such as carbon black and carbon fiber have the effect of improving the weather resistance of resins. However, carbon materials also function as catalysts that promote the decomposition of hypochlorous acid. Therefore, when drinking water is run through a multi-layer resin pipe that uses a composite containing a carbon material in the inner layer, the resin may oxidize, causing blister-like swelling and peeling off of the surface (blister peeling phenomenon). Therefore, when the multi-layer resin pipe according to the present invention is used as a water supply pipe for drinking water, it is preferable that the inner layer does not contain a carbon material.

[0023] [1.1.2. Inner diameter and thickness] The inner diameter of the inner layer is not particularly limited, and an optimal value can be selected depending on the purpose. The inner diameter d1 of the inner layer is preferably 15 mm or more and 235 mm or less. Furthermore, the thickness t1 of the inner layer is not particularly limited as long as it satisfies the conditions described below.

[0024] [1.2. Outer layer] [1.2.1. Materials] An outer layer is disposed on the outside of the inner layer. In the present invention, the outer layer is A polyolefin resin, A coated carbon fiber having a surface treated with an epoxy resin-based sizing agent and / or a polyurethane-based sizing agent; Nucleating agent and The composite layer comprises: The materials constituting the composite layer will be described in detail below.

[0025] [1.2.2. Outer layer composition ratio] The "constituent ratio (%) of the outer layer" refers to the ratio of the thickness t2 of the outer layer to the sum of the thickness t1 of the inner layer and the thickness t2 of the outer layer (=t2×100 / (t1+t2)).

[0026] In the present invention, the composition ratio of the outer layer is not particularly limited, and an optimal value can be selected depending on the purpose. In general, the larger the composition ratio of the outer layer, the smaller the linear expansion coefficient of the multilayer resin pipe. In order to obtain such an effect, the composition ratio of the outer layer is preferably 5% or more. The composition ratio of the outer layer is more preferably 10% or more, 15% or more, 20% or more, or 25% or more. On the other hand, if the composition ratio of the outer layer is too high, the manufacturing cost may increase. Therefore, the composition ratio of the outer layer is preferably 95% or less. The composition ratio of the outer layer is more preferably 90% or less, 85% or less, 80% or less, 75% or less, or 70% or less.

[0027] [1.2.3. Total thickness of inner and outer layers] The total thickness t (=t1+t2) of the inner layer and the outer layer is not particularly limited, and an optimal thickness can be selected depending on the purpose. Although t varies depending on the inner diameter or outer diameter of the multi-layer pipe, it is preferably 1.0 mm or more and 31.0 mm or less. The ratio of the outer diameter D of the multi-layer pipe to the total thickness t of the inner layer and the outer layer (=D / t, hereinafter also referred to as "SDR (Standard Dimension Ratio)") is preferably 9 or more and 26 or less.

[0028] [1.3. Third layer] [1.3.1. Materials] The multi-layer resin pipe according to the present invention may further include a third layer inserted between the inner layer and the outer layer. The material of the third layer is not particularly limited, and an optimal material can be selected depending on the purpose. Examples of the material of the third layer include aluminum and stainless steel for improving pressure resistance.

[0029] [1.3.2. Thickness of the third layer] In the present invention, the thickness of the third layer is not particularly limited, and an optimal thickness can be selected depending on the purpose.

[0030] [1.4. 4th layer] [1.4.1. Materials] The multi-layer resin pipe according to the present invention may further include a fourth layer disposed on the outside of the outer layer. The material of the fourth layer is not particularly limited, and an optimum material can be selected depending on the purpose. Examples of the material of the fourth layer include: (a) Ethylene vinyl alcohol resin (EVOH) to prevent oxygen permeation, (b) Thermoplastic polyurethane elastomer (TPU) and ultra-high molecular weight polyethylene to improve abrasion resistance etc.

[0031] [1.4.2. Thickness of the fourth layer] In the present invention, the thickness of the fourth layer is not particularly limited, and an optimal thickness can be selected depending on the purpose.

[0032] [1.5. Coefficient of linear expansion] In the present invention, the "linear expansion coefficient α ( / °C)" refers to a value calculated using the following formula (1). α = (L h -L c ) / {L c (60-20)} …(1) however, L h is the length of the sample for measuring the linear expansion coefficient at 60°C, L c is the length of the sample used to measure the linear expansion coefficient at 20°C.

[0033] The multi-layered plastic pipe of the present invention has a smaller linear expansion coefficient than conventional plastic pipes because the outer layer is made of a composite layer containing carbon fiber and a crystal nucleating agent. By optimizing the composition, composition ratio, thickness, inner diameter or outer diameter of each layer, etc., a multi-layered plastic pipe that satisfies the following formula (2) can be obtained.

[0034] α≦-0.035×10-5 ×δt2+5.5×10 -5 …(2) however, α is the average linear expansion coefficient of the multilayer resin pipe ( / °C), δt2 is the composition ratio (%) of the outer layer, The "constituent ratio (%) of the outer layer" refers to the ratio of the thickness t2 of the outer layer to the sum of the thickness t1 of the inner layer and the thickness t2 of the outer layer (=t2×100 / (t1+t2)).

[0035] [2. Composite layer] In the present invention, the composite layer constituting the outer layer is A polyolefin resin, A coated carbon fiber having a surface treated with an epoxy resin-based sizing agent or a polyurethane-based sizing agent; Nucleating agent and Includes.

[0036] [2.1. Polyolefin resin] The polyolefin resin constitutes the matrix of the composite layer. In the present invention, the type of polyolefin resin is not particularly limited, and an optimal material can be selected depending on the purpose.

[0037] Examples of polyolefin resins include: (a) Polypropylene, low density polyethylene (LDPE), high density polyethylene (HDPE), ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, copolymers of ethylene and acrylic esters (e.g., methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate), polybutene, ABS, polyacrylonitrile, polyacetal, polycarbonate, nylon, PET, (b) Halides of the above resins (e.g., polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, PTFE, etc.) etc. The composite layer may contain any one of these polyolefin resins, or may contain two or more of them. Furthermore, when the inner layer is made of a polyolefin resin, the polyolefin resin contained in the outer layer may be the same material as the polyolefin resin contained in the inner layer, or may be a different material.

[0038] [2.2. Coated carbon fiber] Coated carbon fiber is Carbon fiber, An epoxy resin-based sizing agent and / or a polyurethane-based sizing agent for coating the surface of the carbon fiber; Includes.

[0039] [2.2.1. Carbon fibre] [A. Materials] In the present invention, the type of carbon fiber is not particularly limited. (a) virgin carbon fiber; (b) Carbon fibers recovered from carbon fiber reinforced resin moldings (recycled carbon fibers), or (c) A mixture of virgin and recycled carbon fibers. Either of the above may be used. As described later, commercially available virgin carbon fibers are usually coated carbon fibers whose surfaces have been treated with a sizing agent.

[0040] In addition, carbon fiber is (a) Chopped fibers obtained by cutting long fibers; (b) Milled fibers obtained by grinding long fibers, or (c) A mixture of chopped and milled fibers Either of the above may be used.

[0041] [B. Average fiber length] "Average fiber length" refers to the average fiber length measured for 10 or more randomly selected carbon fibers.

[0042] The average fiber length of the carbon fibers is not particularly limited, and an optimal value can be selected depending on the purpose. For example, in the case of unused chopped fibers, the average fiber length is about 3 mm to 24 mm. In addition, in the case of unused milled fibers, the average fiber length is about 20 μm to 500 μm. Unused carbon fibers are (a) The variation in fiber length is small, (b) prone to breaking apart into individual filaments; (c) Easily dispersed uniformly in polyolefin resin It has the following features:

[0043] In the case of recycled carbon fibers, the average fiber length varies depending on the type and manufacturing history of the carbon fiber reinforced resin molding from which the carbon fibers are recovered. In the case of recycled carbon fibers, the average fiber length is usually about 20 μm to 3 mm. The average fiber length is preferably 100 μm to 400 μm. Recycled carbon fibers usually have a large variation in fiber length. In addition, when the recycled carbon fibers are recovered from the composite material, the composite material is heated. Depending on the amount of carbonized matter remaining after heating, the way in which the recycled carbon fibers break apart may differ, and the recycled carbon fibers may become less compatible with the molten polyolefin resin. However, when the method according to the present invention is used, the compatibility between the recycled carbon fibers and the molten polyolefin resin is improved even for recycled carbon fibers with a large variation in fiber length.

[0044] [C. Diameter] "Carbon fiber diameter" refers to the maximum cross-sectional dimension of a single fiber.

[0045] When the content of coated carbon fibers in the composite layer is the same, the smaller the diameter of the carbon fibers, the more carbon fibers are dispersed in the composite layer. As a result, the mechanical properties of the composite layer are improved. In addition, the contact area between the carbon fibers and the polyolefin resin is increased, so that the linear expansion coefficient of the composite layer is also reduced. To obtain such an effect, the diameter of the carbon fiber is preferably 6.5 μm or less, and more preferably 6.3 μm or less, 6.0 μm or less, 5.7 μm or less, or 5.5 μm or less.

[0046] [D. Elasticity] The "elastic modulus of carbon fiber" refers to the elastic modulus of a single fiber. Since a sizing agent usually has a small effect on the elastic modulus of carbon fiber, the elastic modulus of carbon fiber can be considered to be equivalent to the elastic modulus of a coated carbon fiber.

[0047] When carbon fibers are dispersed in a polyolefin resin, the greater the elastic modulus of the carbon fibers, the more improved the mechanical properties of the composite. To achieve this effect, the elastic modulus of the carbon fibers is preferably 250 GPa or more. More preferably, the elastic modulus is 260 GPa or more, 260 GPa or more, 270 GPa or more, 280 GPa or more, or 290 GPa or more. The higher the elastic modulus of the carbon fibers, the better.

[0048] [F. Linear expansion coefficient] "Linear expansion coefficient of carbon fiber" refers to the average linear expansion coefficient of a single fiber from 10°C to 200°C. Since a sizing agent usually has a small effect on the linear expansion coefficient of carbon fiber, the linear expansion coefficient of carbon fiber can be considered to be equivalent to the linear expansion coefficient of coated carbon fiber.

[0049] When carbon fibers are dispersed in a polyolefin resin, the smaller the linear expansion coefficient of the carbon fibers, the smaller the linear expansion coefficient of the composite. To obtain such an effect, the linear expansion coefficient of the carbon fibers should be less than -1.4×10 -6 The linear expansion coefficient is preferably -1.5×10 -6 / ℃ or less, or -1.6×10 -6 / ℃ or less.

[0050] [2.2.2. Sizing agents] [A. Materials] "Epoxy resin (EP)-based sizing agent" refers to a liquid resin in which an epoxy resin is dispersed in a dispersion medium. "Polyurethane (PU)-based sizing agent" refers to a liquid resin in which polyurethane is dispersed in a dispersion medium.

[0051] Epoxy resin-based sizing agents and polyurethane-based sizing agents (hereinafter collectively referred to as "sizing agents") are generally used to cover and converge carbon fibers, suppress damage to the carbon fibers, and make the carbon fibers easier to handle. Unlike recycled carbon fibers, commercially available virgin carbon fibers are usually coated carbon fibers whose surfaces have been treated with a sizing agent. Treating the surface of carbon fiber with a sizing agent improves the wettability of the surface of the carbon fiber to polyolefin resin. Therefore, when a composite layer is produced using carbon fiber treated with a sizing agent (coated carbon fiber), the carbon fiber is uniformly dispersed in the polyolefin resin. In addition, even when recycled carbon fiber with non-uniform length is used as a reinforcing material, the recycled carbon fiber can be uniformly dispersed in the polyolefin resin.

[0052] In the present invention, the type of epoxy resin or polyurethane contained in the sizing agent, the concentration of the epoxy resin or polyurethane contained in the sizing agent, and the like are not particularly limited. Examples of epoxy resins include bisphenol A type epoxy resins, novolac type epoxy resins, alicyclic epoxy resins, cresol type epoxy resins, amine type epoxy resins, and bisphenol F type epoxy resins. The concentration of the epoxy resin or polyurethane contained in the sizing agent is usually about 0.1 mass % to 8.0 mass %.

[0053] [B. Amount of Coating] "Coating amount (mass%)" refers to the ratio of the mass of the epoxy resin or polyurethane to the total mass of the coated carbon fiber.

[0054] In the present invention, the coating amount is not particularly limited, and an optimal value can be selected depending on the purpose. In general, if the coating amount is too small, the feedability of the coated carbon fiber may decrease. In addition, the wettability with the polyolefin resin may decrease, and the coated carbon fiber may become difficult to disperse in the polyolefin resin. On the other hand, even if the coating amount is increased more than necessary, there is no difference in effect and there is no practical benefit. The coating amount is usually about 1.0 mass% to 8.0 mass%. The coating amount is preferably 1.0 mass% to 5.0 mass%, or 1.5 mass% to 4.0 mass%.

[0055] [2.3. Nucleating agents] The term "crystal nucleating agent" refers to an additive that, even in small amounts, significantly promotes the crystallization of a crystalline resin and produces uniform, fine crystals. When a nucleating agent is added to a polyolefin resin and the resin is melted and solidified, fine crystals made of the polyolefin resin are generated. As a result, the appearance and physical properties of the outer layer can be improved and the linear expansion coefficient of the outer layer can be reduced compared to when no nucleating agent is added.

[0056] In the present invention, the type of the crystal nucleating agent is not particularly limited. Examples of the crystal nucleating agent include (a) fatty acid amides such as oleic acid amide, erucic acid amide, stearic acid amide, and behenic acid amide; (b) Fatty metal salts such as magnesium stearate, zinc stearate, and calcium stearate etc. The outer layer may contain any one of these crystal nucleating agents, or may contain two or more of them.

[0057] [2.4. Other ingredients] The composite layer may consist of only the polyolefin resin, the coated carbon fiber, and the crystal nucleating agent, or may contain other components in addition to these, such as an antioxidant, a lubricant, a dispersant, and an antistatic agent.

[0058] [2.5. Content] [2.5.1. Content of coated carbon fiber] The "content of coated carbon fiber" refers to the mass of the coated carbon fiber when the mass of the polyolefin resin is taken as 100.

[0059] In general, the higher the content of the coated carbon fiber, the more improved the mechanical properties of the outer layer. To achieve such an effect, the content of the coated carbon fiber is preferably 0.5 parts by mass or more. More preferably, the content is 1.0 parts by mass or more, 2.0 parts by mass or more, or 3.0 parts by mass or more. On the other hand, if the content of the coated carbon fiber is excessive, the moldability of the outer layer may decrease. Therefore, the content of the coated carbon fiber is preferably 15 parts by mass or less. The content is more preferably 13 parts by mass or less, 11 parts by mass or less, or 10 parts by mass or less.

[0060] [2.5.2. Content of nucleating agent] The "content of crystal nucleating agent" refers to the mass of the crystal nucleating agent when the mass of polyolefin resin B is taken as 100.

[0061] In general, the higher the content of the crystal nucleating agent, the finer the crystals of the polyolefin resin B. To obtain such an effect, the content of the crystal nucleating agent is preferably 0.01 parts by mass or more. The content is more preferably 0.02 parts by mass or more. On the other hand, even if the crystal nucleating agent is added more than necessary, there is no difference in the effect and there is no practical benefit. Therefore, the content of the crystal nucleating agent is preferably 0.05 parts by mass or less. The content is more preferably 0.04 parts by mass or less.

[0062] [3. Manufacturing method of multi-layer pipes] The multi-layer pipe according to the present invention can be manufactured by various methods, such as injection molding, extrusion molding, blow molding, etc. In particular, the extrusion molding method is suitable as a molding method because the carbon fibers are easily oriented in one direction.

[0063] [4. Effect] For polyolefin resin, (a) Coated carbon fibers, the surface of which is treated with an epoxy resin-based sizing agent and / or a polyurethane-based sizing agent; and (b) Nucleating agent By adding carbon fiber, a composite having a smaller linear expansion coefficient can be obtained compared to conventional composites. Furthermore, by using such a composite as the outer layer of a multi-layer resin pipe, a multi-layer resin pipe having a small linear expansion coefficient can be obtained even if the carbon fiber content is small.

[0064] The composite of the present invention exhibits a smaller linear expansion coefficient than the conventional composite, because (A) By using coated carbon fiber, the surface of which has been treated with a sizing agent, as a filler, the wettability of the coated carbon fiber with respect to the polyolefin resin is improved, and the coated carbon fiber is easily dispersed uniformly in the polyolefin resin. (B) The polyolefin resin and the carbon fiber are firmly bonded via the sizing agent, and the carbon fiber suppresses the thermal expansion of the polyolefin resin; and (C) The addition of a crystal nucleating agent increases the crystallinity of the polyolefin resin. It is thought that. EXAMPLES

[0065] (Examples 1 to 2, Comparative Examples 1 to 3) [1. Sample preparation] [1.1. Raw materials] Polyolefin resins include: (A) Polyolefin resin 1: High density polyethylene (HDPE) (Hi-Zex (registered trademark) 7700M, manufactured by Prime Polymer Co., Ltd.), or (B) Polyolefin resin 2: High density polyethylene (HDPE) (Prime Polymer Co., Ltd., SP5505) was used.

[0066] Fillers include: (a) Carbon black (Prime Polymer Co., Ltd., 5505BKMB1), (b) Carbon fiber 1: Recycled carbon fiber (recycled CF) (milled fiber, average fiber length: 25 μm), (c) Carbon fiber 2: Recycled carbon fiber (recycled CF) (chopped fiber, average fiber length: 3 mm), (d) Coated carbon fiber 1: Recycled carbon fiber (recycled CF) (chopped fiber, average fiber length: 3 mm) whose surface is coated with an epoxy resin (EP)-based sizing agent, or (e) Coated carbon fiber 2: virgin carbon fiber (V-CF) whose surface is coated with a polyurethane (PU)-based sizing agent (chopped fiber, average fiber length: 6 mm) was used.

[0067] The nucleating agent used was a master batch containing a nucleating agent (Rikemaster (registered trademark) CN-002, manufactured by Riken Vitamin Co., Ltd., (nucleating agent) zinc stearate 1.36% / (main component) high density polyethylene (HDPE)). Compatibilizers for carbon fiber include: (a) Compatibilizer 1: acid-modified polyolefin resin (manufactured by Sanyo Chemical Industries, Ltd., UMEX (registered trademark)), (b) Compatibilizer 2: imine-modified polyolefin resin (1) (manufactured by Mitsui Chemicals, Inc., Admer (registered trademark) IP AT309), or (c) Compatibilizer 3: Imine-modified polyolefin resin (2) (Mitsui Chemicals, Inc., Admer (registered trademark) IP AT334) was used.

[0068] Antioxidants include: (a) Antioxidant 1: Adeka STAB (registered trademark) AO-60 manufactured by ADEKA CORPORATION, or (b) Antioxidant 2: Adeka STAB (registered trademark) 2112, manufactured by ADEKA Corporation was used. The lubricant used was Metablen (registered trademark) L-1000 manufactured by Mitsubishi Chemical Corporation.

[0069] [1.2. Preparation of composite pellets] The above raw materials were mixed in a predetermined ratio and melt-kneaded in a kneading extruder (KTX-30, manufactured by Kobe Steel, Ltd.). The molten composition was extruded into an underwater cooling layer in the form of a strand with a diameter of 3 mm and cut into a length of 3 to 4 mm with a pelletizer (strand cutter, manufactured by Tanaka Co., Ltd.) to obtain composite pellets. The melt-kneading conditions were as follows: Barrel and die temperature: 200°C, Screw speed: 400 rpm, Discharge rate: 20kg / h.

[0070] [1.3. Preparation of resin pipe] [1.3.1. Preparation of single-layer tube] The obtained composite pellets were put into an extrusion molding machine (MK-65I / MK-50II, manufactured by Mitsubishi Yuka Engineering Co., Ltd.) and extrusion molding was performed to produce a single-layer tube. The outer diameter of the single-layer tube was 32 mm. The thickness of the single-layer tube was 3.0 mm. The molding conditions were as follows. Die temperature: 215℃, Screw speed: 63.3 rpm, Take-up speed: 2.5m / min.

[0071] [1.3.2. Fabrication of two-layer tube] The pellets for the inner layer and the pellets for the outer layer were put into an extruder, and a two-layer tube was produced by extrusion molding. The extruder for producing a small-diameter two-layer tube was MK-65I type / MK-50II type manufactured by Mitsubishi Yuka Engineering Co., Ltd. The extruder for producing a large-diameter two-layer tube was RH-801-1-90-33WE / RH-501-1-60-33D manufactured by Reifenhauser. The outer diameter of the two-layer tube was 25 mm to 250 mm, the composition ratio of the outer layer was 16% to 100%, and the total thickness of the two-layer tube was 2.3 to 22.7 mm (SDR = 11). The molding conditions were selected to be optimal depending on the total thickness of the two-layer tube. The molding conditions when the outer diameter of the two-layered tube is 32 mm are as follows. Die temperature: 215℃, Screw rotation speed (inner layer / outer layer): 52.8 rpm / 34.6 rpm, Take-up speed: 2.5m / min.

[0072] 2. Test Method The linear expansion coefficient of the single-layered or double-layered tube was measured according to the following procedure. That is, a tube with a length of 200 mm was used as a sample for measuring the linear expansion coefficient. After the sample was kept in a thermostatic chamber at 20° C. for 2 hours or more, the length L c Next, the sample was kept in a thermostatic chamber at 60°C for 2 hours or more, and then the length L h The obtained L c and L h was substituted into equation (1) to calculate the linear expansion coefficient.

[0073] [3. Results] The results are shown in Tables 1 to 5. The relationship between the composition ratio of the outer layer and the linear expansion coefficient is shown in Figure 1. From Tables 1 to 5 and Figure 1, the following can be seen.

[0074] (1) Comparative Example 1 is a two-layer pipe with carbon black added to the outer layer. The linear expansion coefficient of Comparative Example 1 is 10.0×10 -5 / ℃.

[0075] (2) Comparative Examples 2-1 to 2-3 and 2-6 to 2-10 (hereinafter collectively referred to as "Comparative Example 2") are single-layer pipes made of a composite layer containing recycled carbon fiber (recycled CF) not treated with a sizing agent and a compatibilizer, or two-layer pipes having such a composite layer as the outer layer or inner layer. In Comparative Example 2, the linear expansion coefficient varied widely, and even when the composition ratio of the outer layer was changed, the linear expansion coefficient did not change much (see Figure 1). This is thought to be because the effect of the compatibilizer was insufficient and the bonding strength between the HDPE and the carbon fiber was weak.

[0076] (3) Comparative Examples 2-4 and 2-5 are single-layer pipes made of a composite layer containing recycled carbon fibers (chopped fibers) that were not treated with a sizing agent and did not contain a compatibilizing agent. In Comparative Examples 2-4 and 2-5, the recycled carbon fiber surface was not treated with a sizing agent, the recycled carbon fiber was long, and no compatibilizer was included, so the moldability was extremely poor and holes were observed in the tube. Therefore, the linear expansion coefficient was not measured.

[0077] (4) Comparative Examples 3-1 to 3-11 (hereinafter collectively referred to as "Comparative Example 3") are single-layer pipes made of a composite layer containing recycled carbon fibers whose surface has been treated with an epoxy resin (EP)-based sizing agent but does not contain a crystal nucleating agent, or two-layer pipes with such a composite layer as the outer layer. The linear expansion coefficient of Comparative Example 3 was smaller than those of Comparative Examples 1 and 2. Moreover, the linear expansion coefficient of Comparative Example 3 became smaller as the composition ratio of the outer layer became larger. See Fig. 1. This is considered to be because the bonding strength between HDPE and carbon fiber was strengthened by using carbon fiber whose surface was treated with an EP-based sizing agent as the filler.

[0078] (5) Examples 1-1 to 1-5, Reference Example 1-6, and Examples 1-7 to 1-18 (hereinafter collectively referred to as "Example 1") are two-layer pipes having an outer layer of a composite layer containing recycled carbon fibers whose surfaces have been treated with an EP-based sizing agent and a crystal nucleating agent, or a single-layer pipe (Reference Example 1-6 only) made of such a composite layer. The linear expansion coefficient of Example 1 was smaller than those of Comparative Examples 1 to 3. Moreover, the linear expansion coefficient of Example 1 became smaller as the composition ratio of the outer layer became larger. See FIG. 1. This is considered to be because the bonding strength between HDPE and carbon fiber was strengthened by using carbon fiber whose surface was treated with an EP-based sizing agent as a filler, and because the crystallization degree of HDPE was increased by adding a crystal nucleating agent.

[0079] (6) Examples 2-1 to 2-5 (hereinafter collectively referred to as "Example 2") are two-layer pipes having an outer layer of a composite layer containing virgin carbon fiber (V-CF) whose surface has been treated with a PU-based sizing agent and a crystal nucleating agent. In Example 2, the linear expansion coefficient was slightly increased compared to Example 1.

[0080] [Table 1]

[0081] [Table 2]

[0082] [Table 3]

[0083] [Table 4]

[0084] [Table 5]

[0085] (Examples 3 to 5) [1. Sample preparation] [1.1. Preparation of dumbbell-shaped tensile test specimens and strands] In order to investigate the influence of the physical properties of the carbon fiber on the mechanical properties of the outer layer, the following two types of test specimens were prepared. (a) Dumbbell-shaped tensile test piece (JIS K 7139: Type A1 (ISO3167: Type A)). (b) Strand (diameter approximately 5.0 mm).

[0086] As the polyolefin resin, high density polyethylene (HDPE) (Hi-Zex (registered trademark) 7700M, manufactured by Prime Polymer Co., Ltd.) was used. The nucleating agent used was a master batch containing a nucleating agent (Rikemaster (registered trademark) CN-002, manufactured by Riken Vitamin Co., Ltd., (nucleating agent) zinc stearate 1.36% / (main component) high density polyethylene (HDPE)).

[0087] The following coated carbon fibers were used. Table 6 shows the details of each coated carbon fiber. (a) Recycled carbon fiber whose surface is coated with an epoxy-based sizing agent (Example 3) (b) Unused carbon fiber whose surface is coated with an epoxy-based sizing agent (Example 4-1) (c) Unused carbon fiber whose surface is coated with a urethane-based sizing agent (Example 4-2) (d) Unused carbon fiber with a surface coated with a urethane-based sizing agent (Example 5)

[0088] [Table 6]

[0089] HDPE, a crystal nucleating agent, and coated carbon fiber were mixed in a predetermined ratio. The amount of coated carbon fiber was 6.0 parts by mass relative to 100 parts by mass of HDPE. The amount of crystal nucleating agent (master batch) was 2.0 parts by mass relative to 100 parts by mass of HDPE. Composite pellets were then prepared in the same manner as in Example 1. The composite pellets thus obtained were then injection molded to obtain dumbbell-shaped tensile test pieces under the following injection molding conditions: Cylinder temperature: 210℃ Injection speed: 40mm / s Similarly, the obtained composite pellets were extruded to obtain strands under the following extrusion conditions. Die temperature: 205℃ Screw rotation speed (inner layer / outer layer): 26.8 rpm / 34.0 rpm Take-off speed: 2.75m / min

[0090] [1.2. Fabrication of two-layer tube] A two-layer pipe was produced using a material having the same composition as the above dumbbell-shaped tensile test piece and strand. The production conditions for the two-layer pipe were the same as those in Example 1-2.

[0091] 2. Test Method [2.1. Evaluation using dumbbell-shaped tensile test specimens and strands] [2.1.1. Appearance evaluation] The appearance of the test pieces was evaluated visually.

[0092] [2.1.2. Tensile strength, tensile elongation] The tensile strength and tensile elongation were measured using dumbbell-shaped test pieces in accordance with JIS K 7139 (ISO3167).

[0093] [2.1.3. Coefficient of linear expansion] The linear expansion coefficient was measured using the dumbbell-shaped test piece and the strand. The linear expansion coefficient was calculated using the above-mentioned (1).

[0094] [2.1.4. Fracture surface observation] The cut surfaces of the strands were visually observed.

[0095] [2.2. Evaluation using a two-layer tube] [2.2.1. Optical microscope observation] The axial and longitudinal cross sections of the two-layered tube were observed under an optical microscope.

[0096] [2.2.2. Observation of carbon fibers] Carbon fibers were taken out of the two-layer pipe and the fiber diameter, weight average aspect ratio, and weight average remaining fiber length were measured. The "remaining fiber length" refers to the length of the carbon fibers actually taken out of the two-layer pipe.

[0097] [2.2.3. Evaluation of carbon fiber adhesion] The pull-out strength (IFSS) of the carbon fibers before fabricating the two-layered tube was measured by the microdroplet method.

[0098] [3. Results] [3.1. Evaluation using dumbbell-shaped tensile test specimens and strands] The results of the evaluation using the dumbbell-shaped tensile test pieces and strands are shown in Table 7. From Table 7, the following can be seen. (1) In Examples 4-1 and 4-5, in which virgin carbon fiber was used, no roughness was observed on the test piece surface. However, in Example 3, in which recycled carbon fiber was used, some roughness was observed on the test piece surface. This is thought to be due to the fact that the length of the recycled carbon fiber was not uniform, or that a small amount of impurities (carbonized resin) was mixed into the recycled carbon fiber.

[0099] (2) Example 5 had the best mechanical properties and linear expansion coefficient. (3) Example 3 corresponds to the recycled carbon fiber of Example 5. Example 3 has a larger tensile elongation and a slightly larger linear expansion coefficient than Example 5. This is thought to be because the recycled carbon fibers are not uniform in length or because trace amounts of impurities (carbonized resin) are mixed in the recycled carbon fibers. (4) Example 4-1 was inferior to Examples 3 and 5 in mechanical properties and linear expansion coefficient. (5) The cut cross section was good, with only a few fine dents (almost no large voids) in all of Examples 3, 4-1, and 5. In addition, no difference was observed due to the type of carbon fiber.

[0100] [Table 7]

[0101] [3.2. Evaluation using a two-layer tube] Table 8 shows the specifications of the carbon fibers used and the results of various evaluations. FIG. 2(A) shows optical microscope photographs of the axial and longitudinal cross sections of the outer layer of the two-layered pipe obtained in Example 3. FIG. 2(B) shows optical microscope photographs of the axial and longitudinal cross sections of the outer layer of the two-layered pipe obtained in Example 4-2. The following can be seen from Table 8 and FIG. 2.

[0102] (1) There was no significant difference in the dispersion state of the carbon fibers in HDPE between Example 3 (recycled carbon fibers) and Example 4-2 (virgin carbon fibers). See Figure 2. That is, it was found that the difference in the mechanical properties and linear expansion coefficient between Example 3 and Example 4-2 was not due to the difference in the dispersion state of the carbon fibers.

[0103] (2) The weight average aspect ratio and weight average remaining fiber length of the carbon fiber of Example 4-2 were almost the same as those of Example 3. However, the diameter of the carbon fiber of Example 4-2 was 7.0 μm, whereas that of Example 3 was 5.5 μm. When the mass of carbon fiber added to HDPE is the same, the smaller the diameter of the carbon fiber, the greater the number of carbon fibers dispersed in HDPE. The mechanical properties and linear expansion coefficient of Examples 3 and 5 were superior to those of Example 4-2, which is considered to be due in part to the smaller diameter of the carbon fiber.

[0104] (3) The carbon fiber used in Example 3 has its surface coated with an epoxy-based sizing agent, whereas the carbon fiber used in Examples 4-2 and 4-5 has its surface coated with a urethane sizing agent. However, the pull-out strengths of these fibers are the same, and no difference due to the type of sizing agent was observed. In other words, it was found that the type of sizing agent has little effect on the mechanical properties and linear expansion coefficient of the composite layer.

[0105] (4) The modulus of elasticity of the carbon fiber used in Example 5 was greater than that of the carbon fiber used in Example 4-2. Similarly, the linear expansion coefficient of the carbon fiber used in Example 5 was smaller than that of the carbon fiber used in Example 4-2. Since the type of sizing agent had almost no effect on the mechanical properties and linear expansion coefficient of the composite layer, it is believed that the mechanical properties and linear expansion coefficient of Examples 3 and 5 were superior to those of Example 4-2 in part due to the greater modulus of elasticity of the carbon fiber and the smaller linear expansion coefficient of the carbon fiber.

[0106] [Table 8]

[0107] (Examples 6 to 11) [1. Sample preparation] The effects of the composition ratio of the outer layer, the drawdown ratio during extrusion molding (the ratio of the outer diameter of the pipe after calibration to the outer diameter of the pipe extruded from the mold), and the carbon fiber content in the outer layer on the linear expansion coefficient of the two-layer pipe were investigated.

[0108] The material of the inner layer was high density polyethylene (HDPE) (Evolue (registered trademark) H, SP5505, manufactured by Prime Polymer Co., Ltd.).

[0109] The following materials were used for the outer layer: (a) Polyolefin resin: High density polyethylene (HDPE) (manufactured by Prime Polymer Co., Ltd., Evolue (registered trademark) H, SP5505) (b) Nucleating agent: Nucleating agent-containing masterbatch (RIKEMASTER (registered trademark) CN-002, manufactured by Riken Vitamin Co., Ltd., (nucleating agent) zinc stearate 1.36% / (main component) high density polyethylene (HDPE)) (c) Coated carbon fiber: Teijin Limited, IM C443

[0110] The polyolefin resin, the crystal nucleating agent, and the coated carbon fiber were mixed in a predetermined ratio. The amount of the coated carbon fiber was 6.0 mass% or 8.0 mass% based on the total mass of the outer layer. The amount of the crystal nucleating agent (master batch) added was 2.0 parts by mass based on 100 parts by mass of HDPE. Composite pellets were then prepared in the same manner as in Example 1. Next, the pellets for the inner layer and the pellets for the outer layer were put into an extruder and extruded to produce a two-layer pipe. The extrusion conditions were the same as those in Example 1.

[0111] [2. Test Method and Results] The linear expansion coefficient of the obtained two-layered pipe was measured. The calculation method of the linear expansion coefficient was the same as in Example 1. The results are shown in Table 9. Fig. 3 shows the relationship between the composition ratio of the outer layer and the linear expansion coefficient of the two-layered pipe obtained in Examples 6 to 11. The following can be seen from Table 9 and Fig. 3.

[0112] (1) The linear expansion coefficient tends to decrease as the composition ratio of the outer layer increases. See Figure 3. (2) The coefficient of linear expansion hardly changed even when the drawdown rate during extrusion molding was changed. (3) The linear expansion coefficient tended to decrease as the carbon fiber content increased.

[0113] [Table 9]

[0114] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0115] The multilayer resin pipe according to the present invention can be used as a water supply pipe, a hot water supply pipe, a drainage pipe, a piping for air conditioning in a building, a gas pipe, and the like.

Claims

[Claim 1] The inner layer, an outer layer disposed outside the inner layer; Equipped with The inner layer is made of a resin layer containing a resin, The outer layer is A polyolefin resin, A coated carbon fiber having a surface treated with an epoxy resin-based sizing agent and / or a polyurethane-based sizing agent; Nucleating agent and A composite layer comprising Multilayer resin pipe.

Citation Information

Patent Citations

  • Multilayer pipe and resin composition for the same

    JP2022052466A

  • Resin pipe

    JP2022072698A