Manufacturing method for lead terminal for power storage device and lead terminal for power storage device

The laser welding method addresses the challenges of reproducibility, metal adhesion, and speed limitations in arc welding by controlling the weld shape and preventing metal contamination, thereby improving the quality and yield of lead terminals for power storage devices.

JP2024169384AActive Publication Date: 2024-12-05KOHOKU KOGYO CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024083778
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-23
Publication Date
2024-12-05
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

Existing lead terminal manufacturing methods for power storage devices, particularly those using percussion arc welding, suffer from low reproducibility of weld shape, adhesion of dissimilar metals, and limitations in manufacturing speed due to the nature of arc welding, which can lead to quality issues and reduced yield.

Method used

A laser welding method is employed to align and connect wire rods and lead wires, controlling the weld shape and preventing adhesion of dissimilar metals by irradiating the wire end with a laser beam and pushing the lead wire into the molten pool, ensuring consistent and efficient welding.

Benefits of technology

This method improves the reproducibility of the welded portion shape, prevents adhesion of dissimilar metals, and enhances manufacturing speed, resulting in higher yield and quality of lead terminals suitable for power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169384000001_ABST
    Figure 2024169384000001_ABST
Patent Text Reader

Abstract

To provide a method for appropriately manufacturing a lead terminal for a power storage device having an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead terminal manufactured by the method.SOLUTION: A manufacturing method for a lead terminal for a power storage device having an electrode terminal 2 made of a wire 100 mainly containing aluminum or copper, and a lead wire 3 connected to the electrode terminal via a welded portion 4, includes a first step of aligning a wire and a lead wire in a straight line and holding the wire and the lead wire in a state where a predetermined distance is maintained between an end face 100b of the wire on the lead wire side and an end face 3b of the lead wire on the wire side, a second step of irradiating an end face 100a of the wire on the lead wire side with a laser beam using a laser irradiator 400 to melt the end, and a third step of pushing one of the wire and the lead wire axially toward the other after a predetermined time has elapsed from the start of irradiation of the laser beam in the second step, to form a welded portion.SELECTED DRAWING: Figure 2A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a lead terminal for an electricity storage device, and a lead terminal for an electricity storage device. [Background technology]

[0002] Lead terminals for electricity storage devices have been known for some time. All lead terminals for electricity storage devices include a metal electrode terminal and a lead wire. The lead wire is connected to the electrode terminal via a welded portion. For example, in a lead terminal for an electrolytic capacitor (a type of electricity storage device), the electrode terminal is connected to an electrode foil that forms a capacitor element (a component of an electrolytic capacitor), and the lead wire is connected to an electric circuit.

[0003] A typical example of a lead terminal is a lead terminal equipped with an electrode terminal made of aluminum or copper. The welded portion of such a lead terminal has generally been formed by percussion arc welding (see, for example, Patent Document 1). This is because, among the welding methods considered at the time, percussion arc welding was able to achieve the highest yield, while forming the welded portion by other welding methods, such as brazing (a type of solder joint), has the disadvantage of the risk of contamination with foreign matter, and forming the welded portion by resistance welding (a type of pressure welding) has the disadvantage of the relatively slow melting rate of the welded material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5461570 Summary of the Invention

[0005] However, the welding method using percussion arc welding is not the best, and there is room for improvement in the manufacturing method of a lead terminal having an aluminum or copper electrode terminal and the lead terminal manufactured by this manufacturing method.

[0006] The present invention has been made to address the above-mentioned problems. That is, an object of the present invention is to provide a manufacturing method for appropriately manufacturing a lead terminal for an electricity storage device having an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead terminal manufactured by the manufacturing method.

[0007] The method for manufacturing a lead terminal of the present invention is a method for manufacturing a lead terminal for an electricity storage device, comprising an electrode terminal (2) made of a wire (100) mainly containing aluminum or copper, and a lead wire (3) connected to the electrode terminal via a welded portion (4). The method for manufacturing the lead terminal includes the steps of: a first step of aligning the wire (100) and the lead wire (3) in a straight line and holding the wire and the lead wire in a state in which a distance between an end face (100b) of the wire on the lead wire side and an end face (3b) of the lead wire on the wire wire side is maintained at a predetermined distance; a second step of irradiating a laser beam to the end portion (100a) of the wire (100) on the lead wire side with a laser irradiator (400) to melt the end portion; a third step of forming the welded portion (4) by axially pushing one of the wire rod (100) and the lead wire (3) toward the other after a predetermined time has elapsed since the start of the irradiation of the laser beam in the second step; Equipped with.

[0008] Moreover, the lead terminal (101) of the present invention is The lead terminal for an electricity storage device comprises an electrode terminal (102) made of a wire material containing mainly aluminum or copper, and a lead wire (103) connected to the electrode terminal via a welded portion (104). In the lead terminal, The ratio of the diameter of the lead wire to the diameter of the wire is not less than 83% and not more than 100%.

[0009] According to the present invention, it is possible to provide a manufacturing method for appropriately manufacturing a lead terminal for an electricity storage device having an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead terminal manufactured by the manufacturing method. [Brief description of the drawings]

[0010] [Figure 1] 1 is a perspective view showing a lead terminal manufactured by a method for manufacturing a lead terminal for an electricity storage device according to an embodiment of the present invention. [Figure 2A] FIG. 2 is a diagram (part 1) for explaining a manufacturing method of the lead terminal of FIG. [Figure 2B] FIG. 2 is a diagram (part 2) for explaining the manufacturing method of the lead terminal of FIG. [Figure 2C] FIG. 3 is a diagram (part 3) for explaining the manufacturing method of the lead terminal of FIG. [Figure 2D] FIG. 4 is a fourth diagram for explaining the manufacturing method of the lead terminal of FIG. [Diagram 3] 11A and 11B are diagrams for explaining dents formed in a welded portion. [Figure 4] 10A to 10C are views for explaining a manufacturing method for a lead terminal for an electricity storage device according to Modification 1. [Figure 5A] FIG. 2 is a partially enlarged view of a defective lead terminal manufactured using percussion arc welding. [Figure 5B] FIG. 13 is a partially enlarged view of another defective lead terminal manufactured using percussion arc welding. [Figure 5C] FIG. 13 is a partial enlarged view of yet another defective lead terminal manufactured using percussion arc welding. [Figure 6] 13 is a perspective view showing a lead terminal manufactured by a method for manufacturing a lead terminal for an electricity storage device according to Modification 3. FIG. [Figure 7A] FIG. 2 is a partially enlarged view of a lead terminal having a wire diameter ratio of 83%. [Figure 7B] FIG. 7B is a schematic diagram of an X-ray image of the lead terminal of FIG. 7A. [Figure 7C]FIG. 1 is a schematic diagram of an EPMA image of a cross section of sample S having a diameter ratio of 83%. [Figure 8A] FIG. 2 is a partially enlarged view of a lead terminal having a wire diameter ratio of 83% manufactured using percussion arc welding. [Figure 8B] FIG. 8B is a schematic diagram of an X-ray image of the lead terminal of FIG. 8A. [Figure 8C] FIG. 13 is a schematic diagram of an EPMA image of a cross section of sample Sc having a diameter ratio of 83%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, a method for manufacturing a lead terminal for an electricity storage device according to an embodiment of the present invention will be described with reference to the drawings, taking as an example a lead terminal for an electrolytic capacitor, which is one type of electricity storage device. First, the configuration of the lead terminal will be described. As shown in Fig. 1, the lead terminal 1 includes an aluminum electrode terminal 2 and a lead wire 3 made of a CP wire.

[0012] The electrode terminal 2 is formed by radially pressing a part in the axial direction of a wire material mainly containing aluminum (hereinafter simply referred to as "aluminum wire"), and has a rod-shaped part 21 at one end and a rolled part 22 at the other end. The rod-shaped part 21 is a part that remains without being pressed (i.e., the other part in the axial direction of the aluminum wire). The rolled part 22 is formed by pressing the part of the aluminum wire into a flat plate and cutting its outer periphery along the thickness direction. The axis of the rolled part 22 (a line passing through the center in the width direction and thickness direction) is coaxial with the axis of the rod-shaped part 21. However, a configuration in which the rolled part 22 is eccentric with respect to the rod-shaped part 21 may be adopted. This aluminum wire has been previously subjected to a well-known anodizing process, and an oxide coating is formed on its outer periphery. The diameter of the aluminum wire is about 2 mm. The electrode terminal 2 may be formed using an aluminum wire that has not been subjected to anodizing process.

[0013] The lead wire 3 is connected to one end of the rod-shaped portion 21 via a welded portion 4. The diameter of the lead wire 3 is about 0.8 mm, which is smaller than the rod-shaped portion 21. The axis of the lead wire 3 is coaxial with the axis of the rod-shaped portion 21. In this embodiment, the CP wire constituting the lead wire 3 is a metal wire in which the outer circumferential surface of an iron wire is covered with a copper plating layer, and the copper plating layer is further covered with a tin plating layer. The thicknesses of the copper plating layer and the tin plating layer are both on the order of several tens of μm. However, instead of the tin plating layer, a CP wire covered with a nickel plating layer, a silver plating layer, or a lead-free solder plating layer may be used. Alternatively, the CP wire constituting the lead wire 3 may be a metal wire in which the outer circumferential surface of an iron wire is covered only with a copper plating layer.

[0014] 2A to 2D, a method for manufacturing the lead terminal 1 will be described. First, a long aluminum wire (strictly speaking, an aluminum wire that has been anodized) that is the material of the electrode terminal 2 is cut to a predetermined length to form the wire material 100. In addition, a long CP wire that is the material of the lead wire 3 is cut to a predetermined length to form the lead wire 3.

[0015] Next, as shown in FIG. 2A, the wire 100 is held in a jig 200, and the lead wire 3 is held in a jig 300, so that the wire 100 and the lead wire 3 are aligned in a straight line so that their axes are coaxial, and the distance between the end face 100b of one end 100a of the wire 100 and the end face 3b of the other end 3a of the lead wire 3 is maintained at a predetermined distance (2 mm in this embodiment) (first step).

[0016] Next, a laser beam is irradiated from a direction perpendicular to the axis of the wire 100 (hereinafter, simply referred to as the "orthogonal direction") to a predetermined position P on the end 100a of the wire 100 by the laser irradiator 400. The position P is located on the outer peripheral surface 100c of the end 100a at a position spaced a predetermined distance L (0.10 mm in this embodiment) from the end surface 100b. When the wire 100 is viewed in plan from the direction of irradiation of the laser beam, the position P is located at the center in the radial direction of the wire 100. That is, the laser beam is irradiated toward the axis of the wire 100. The irradiator 400 is a single-mode infrared laser (IR laser) having an output of 700 W. The laser beam is irradiated for 0.030 s with a spot diameter of 30 μm. By irradiating the position P of the wire 100 with a laser beam by the irradiator 400, the end portion 100a is melted over its entirety to form a molten pool A, as shown in Fig. 2B (second step). Note that the distance L may be appropriately changed depending on the output of the irradiator 400, the spot diameter, the irradiation time, etc.

[0017] The jig 300 is provided with a pushing mechanism (not shown). The pushing mechanism is configured to be able to apply an external force in a predetermined direction. In this embodiment, the pushing mechanism applies an external force to the lead wire 3, pushing the lead wire 3 in the axial direction toward the wire 100, immediately after the irradiation of the laser beam by the irradiator 400 is completed (in other words, after the irradiation time has elapsed from the start of the laser beam irradiation). This external force is applied so that the lead wire 3 moves a predetermined distance at a predetermined speed (200 mm / s in this embodiment). As a result, the end 3a of the lead wire 3 is pushed into the molten pool A of the wire 100, as shown in FIG. 2C. Then, a part of the molten pool A spreads out so as to cover the outer peripheral surface 3c of the end 3a of the lead wire 3. Thereafter, when the molten pool A (if the end 3a is partially melted, the molten pool A and the molten portion of the end 3a) solidifies, as shown in FIG. 2D, a cone-shaped (strictly speaking, approximately a truncated cone shape whose diameter decreases from the wire 100 toward the lead wire 3) weld 4 is formed between the wire 100 and the lead wire 3, and the wire 100 and the lead wire 3 are connected (third step).

[0018] Thereafter, the other end of the wire 100 is pressed to form the rolled portion 22 shown in Fig. 1, and is subjected to a well-known anodizing treatment and a resin coating treatment as necessary. In this manner, the lead terminal 1 is manufactured. Note that, as a result of a strength test, it was confirmed that the strength of the lead terminal 1 manufactured by laser welding was equivalent to that of a lead terminal manufactured by percussion arc welding.

[0019] According to the manufacturing method of the lead terminal of the present embodiment, it is possible to manufacture the lead terminal more appropriately compared with the conventional manufacturing method using percussion arc welding (hereinafter, also simply referred to as "arc welding"). The following will be specifically described. The conventional welding method using arc welding has several problems as described below. The first problem is low reproducibility of the weld shape. That is, in arc welding, the heat input amount is likely to vary for each work depending on the environmental conditions at the time of arc generation (type and flow rate of shielding gas, shape and state of each end face of wire material and lead wire), and as a result, there is a problem that the shape of the lead terminal is likely to vary. FIGS. 5A to 5C are partial enlarged views of a defective lead terminal 11 manufactured using arc welding. The lead terminal 11 includes an aluminum electrode terminal 12 and a lead wire 13 made of a CP wire connected to the electrode terminal 12 via a weld portion 14. In Fig. 5A, a portion 14a of the welded portion 14 covers the outer peripheral surface of the lead wire 13, while the other portion of the welded portion 14 does not cover the outer peripheral surface, resulting in an irregular shape of the welded portion 14 (so-called one-sided build-up). In Fig. 5B, a protrusion (so-called weld thorn) 14b large enough to be visible to the naked eye is generated from the welded portion 14. In Fig. 5C, a portion 14c of the welded portion 14 in the circumferential direction protrudes in the radial direction, causing a local increase in the diameter of the welded portion 14 (so-called protrusion). The low reproducibility of the welded portion shape exemplified by the lead terminal 11 in Figs. 5A to 5C has been a factor preventing an improvement in yield.

[0020] The second problem is that dissimilar metals are attached to the workpiece (particularly the electrode terminal). That is, in arc welding, an arc is generated between the wire and the lead wire by arc discharge, and the tips of both are melted, so that spatter is generated from both the wire and the lead wire. For example, if the lead wire is a CP wire covered with a copper plating layer and a tin plating layer, the spatter generated from the lead wire contains copper and tin. Therefore, when spatter containing copper and tin generated from the lead wire adheres to an aluminum wire, dissimilar metals are attached to the workpiece (strictly speaking, the part that becomes the electrode terminal after the product is completed). When a capacitor element (a component of an electrolytic capacitor) is manufactured using a lead terminal with a dissimilar metal attached to the electrode terminal, the dissimilar metal may react with the electrolyte inside the capacitor element, and in that case, the quality characteristics may be deteriorated. This problem cannot be avoided as long as the lead wire contains materials other than aluminum. The attachment of dissimilar metals to the workpiece was another factor that hindered the improvement of yield.

[0021] The third problem is that there is a limit to how quickly workpieces can be manufactured. In arc welding, an arc is generated by first contacting a wire and a lead wire and then separating them, and the tips of the wire and the lead wire are melted before they are brought into contact again (strictly speaking, one is pushed into the other). This requires multiple reciprocating motions for one workpiece, complicating the manufacturing process. In addition, there is a limit to the performance of actuators that can achieve such a series of reciprocating motions, making it difficult to control the actuator at high speed. These problems have been factors that prevent the speed of workpieces from being increased.

[0022] In contrast, in this embodiment, laser welding is adopted as the welding method. Therefore, the shape of the welded portion 4 can be controlled relatively easily (in other words, once the environmental conditions at the time of laser beam irradiation are determined, subsequent adjustments are basically unnecessary). As a result, the reproducibility of the welded portion shape can be significantly improved. In addition, since only the wire 100 is irradiated with the laser beam in laser welding, even if spatter is generated from the wire 100 by laser welding, a situation in which a different metal adheres to the electrode terminal 2 cannot occur (it is not considered to be a particular problem that the spatter generated from the wire 100 adheres to the lead wire 3). In addition, since the welded portion 4 is formed by pushing the end 3a of the lead wire 3 into the molten pool A of the wire 100 in laser welding, the welding process can be performed by moving the lead wire 3 in one direction once for one workpiece, and the manufacturing process can be simplified. In addition, since an actuator that realizes such a simple movement is easily available, the time required for the actuator to operate can be significantly reduced by introducing an actuator that operates at high speed. As described above, by adopting laser welding as the welding method, the above three problems associated with arc welding can be solved, and the yield and manufacturing speed of the lead terminals 1 can be improved.

[0023] Here, even if laser welding is used as the welding method, the following manufacturing method, i.e., "manufacturing method M in which one of the wire 100 and the lead wire 3 is axially pushed toward the other while irradiating the wire 100 with a laser beam in a state where the end face 100b of the wire 100 and the end face 3b of the lead wire 3 are butted (contacted) against each other", may not be able to form the welded portion 4 properly. A specific description will be given with reference to FIG. 3. FIG. 3 shows a partial enlarged view of the lead terminal 1 when the welded portion 4 is formed by the manufacturing method M. In this example, the laser beam is irradiated from an orthogonal direction. As shown in FIG. 3, a crater-like dent d is formed in the welded portion 4. The dent d is a depression formed due to the laser beam being continuously irradiated to one place on the outer peripheral surface 100c of the wire 100. It was found that the height hd of the welded portion 4 in the portion where the dent d is formed is larger than the height h of the welded portion 4 in the portion where the dent d is not formed, and the ratio (hd / h) tends to be about 1.5 to 2 times. A welded portion 4 with such a dent d formed therein significantly deviates from the general specifications for welded portions 4, and is therefore a factor preventing an improvement in yield. Furthermore, when an electrolytic capacitor is manufactured using a lead terminal 1 with a dent d in the welded portion 4, a gap may form between the resin sealing body and the lead terminal 1, causing the electrolyte (electrolytic solution held in the capacitor element) to leak from the gap, which may result in a deterioration in the quality characteristics of the electrolytic capacitor.

[0024] Therefore, in this embodiment, the laser beam irradiation is started while the distance between the end face 100b of the wire 100 and the end face 3b of the lead wire 3 is maintained at a predetermined distance, and one of the wire 100 and the lead wire 3 is pushed axially toward the other after a predetermined time T has elapsed from the start of the irradiation. With this configuration, dents d are less likely to occur in the welded portion 4, and as a result, the yield of the lead terminal 1 can be improved and the deterioration of the quality characteristics of the electrolytic capacitor can be suppressed.

[0025] As described above, according to the method for manufacturing a lead terminal according to the present embodiment, it is possible to appropriately manufacture a lead terminal including an electrode terminal made of a wire mainly containing aluminum. Note that the lead terminal 1 is not limited to an electrolytic capacitor and may be used as a component of other power storage devices. Other power storage devices include, for example, a lithium ion capacitor, an electric double layer capacitor (EDLC: Electric Double Layer Capacitor), or a lithium ion battery. Even when the lead terminal 1 is used as a component of other power storage devices, the same effects can be achieved.

[0026] The inventors of the present application verified the generation rate of the indentation d while changing a predetermined time T (the time from the start of irradiation of the laser beam to the time when the lead wire 3 is pushed into the wire 100). As a result, when the laser beam is irradiated from the orthogonal direction, when 0 < T < irradiation time, although the generation rate of the indentation d can be reduced compared to when T = 0, it was found that the generation rate of the indentation d is higher than when T = irradiation time. Further, when T > irradiation time, although the generation rate of the indentation d could be suppressed to the same level as when T = irradiation time, since the temperature of the molten pool A decreases by the amount of delay in the timing of pushing the lead wire 3 toward the wire 100, it was found that there is a possibility that the wire 100 and the lead wire 3 cannot be appropriately connected (that is, the strength of the lead terminal 1 decreases). Therefore, in the present embodiment, when the laser beam is irradiated from the orthogonal direction, the lead wire 3 is pushed toward the wire 100 immediately after the irradiation of the laser beam ends (that is, the predetermined time T = irradiation time). According to this configuration, it is possible to further reduce the generation rate of the indentation d in the welded portion 4 while ensuring the strength of the lead terminal 1.

[0027] Note that when the laser beam is irradiated from the orthogonal direction, the position adjustment of the irradiator 400 is performed by making the axis of its irradiation port orthogonal to the axis of the wire 100. Therefore, the position adjustment of the irradiator 400 can be easily performed as compared with a configuration in which the laser beam is irradiated so as to intersect obliquely with the axis of the wire 100.

[0028] Furthermore, in this embodiment, an infrared laser is used for the irradiator 400. Therefore, the cost of the manufacturing equipment for the lead terminal 1 can be reduced compared to the case where a short-wavelength laser (typically, a blue laser or a green laser) is used for the irradiator 400. However, since the absorptivity of aluminum is equivalent over the entire wavelength band of infrared and visible light, from the viewpoint other than the manufacturing cost, the same effect as in this embodiment can be obtained even when a short-wavelength laser is used. The type of laser (for example, a fiber laser or a semiconductor laser) is not particularly limited.

[0029] The laser beam may be irradiated not only to position P of wire 100 but also to a predetermined range on outer circumferential surface 100c of end 100a, for example, in a linear or elliptical shape. During irradiation with the laser beam, wire 100 may be rotated around its axis at a predetermined speed.

[0030] (Variation 1) Next, a manufacturing method of a lead terminal for an electric storage device according to the first modified example of the present invention will be described with reference to FIG. 4. The same components as those in the embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted. This is the same for the other modified examples. As shown in FIG. 4, the manufacturing method of the first modified example differs from the manufacturing method of the embodiment in that the direction of irradiation of the laser beam is oblique to the axis of the wire 100. Specifically, in this modified example, the irradiator 400 irradiates the center C of the end face 100b of the wire 100 with the laser beam from a direction intersecting the axis of the wire 100 at 45°. The pushing mechanism applies an external force to the lead 3 to push the lead 3 in the axial direction toward the wire 100 immediately after the end of the irradiation of the laser beam (i.e., the predetermined time T=irradiation time). The spot diameter and irradiation time may be the same as or different from those in the embodiment.

[0031] With this configuration as well, the same operational effects as those of the embodiment can be achieved. In particular, in this modified example, the laser beam is irradiated onto the end face 100b (i.e., the portion that becomes the inside of the molten pool A) of the wire 100 instead of the outer peripheral surface 100c. For this reason, indentations d are not formed in the welded portion 4, and the yield of the lead terminal 1 can be more suitably improved, and a further reduction in the quality characteristics of the power storage device can be suppressed.

[0032] Note that as long as the laser beam is irradiated onto the end face 100b of the wire 100, the irradiation direction of the laser beam is not limited to the direction intersecting the axis of the wire 100 at 45°. Also, the irradiation position of the laser beam may be eccentric from the center C of the end face 100b, or may be irradiated, for example, linearly or circularly within a predetermined range on the end face 100b. Furthermore, in this modified example, since indentations d are not formed in the welded portion 4, the timing at which the lead wire 3 is pushed toward the wire 100 may be earlier than the time when the irradiation of the laser beam ends (typically, it may be several tens of ms earlier than the end of irradiation). That is, the predetermined time T can be set to any value satisfying 0 < T ≤ irradiation time.

[0033] (Modified Example 2) Next, a method for manufacturing a lead terminal for a power storage device according to Modified Example 2 of the present invention will be described. The manufacturing method of Modified Example 2 is different from the manufacturing methods of the embodiment and Modified Example 1 in that a wire mainly containing copper is used as the wire 100 constituting the electrode terminal 2, and a short-wavelength laser is used as the irradiation machine 400 instead of an infrared laser.

[0034] This wire 100 is previously subjected to a well-known anodic oxidation treatment, and an oxide film is formed on its outer peripheral surface. The diameter of the wire 100 and the method of forming the electrode terminal 2 are the same as those in the embodiment. Note that the electrode terminal 2 may be formed using a wire that has not been subjected to anodic oxidation treatment.

[0035] The lead terminal 1 can basically be manufactured by the manufacturing method described in the embodiment or Modification 1. However, in the second step, a short-wavelength laser is used as the irradiator 400. The short-wavelength laser is a multi-mode blue laser having an output of 2 kW. The laser beam is irradiated for 70 μs with a spot diameter of 600 μm. When the laser beam is irradiated on the position P of the wire 100 by the blue laser, as in the embodiment, the end portion 100a is melted throughout to form a melting pool A. Note that a green laser may be used instead of the blue laser as the short-wavelength laser. In this case, the spot diameter and the irradiation time can be appropriately adjusted according to the output of the green laser.

[0036] Here, when a wire mainly containing copper is used as the wire 100, even if a predetermined time T (the time from the start of irradiation of the laser beam until the lead wire 3 is pushed toward the wire 100) satisfies 0 < T < the irradiation time, the indentation d does not occur. Therefore, in this modification, the predetermined time T does not necessarily have to satisfy T = the irradiation time. The predetermined time T can be appropriately set based on the wire diameter ratio of the lead wire 3 to the wire 100, the output of the short-wavelength laser, the spot diameter, the irradiation time, and the like.

[0037] As described above, according to the manufacturing method of the lead terminal for the power storage device according to Modification 2, the three problems related to arc welding described in the embodiment can be solved, and the yield and the manufacturing speed of the lead terminal 1 can be improved. That is, it becomes possible to appropriately manufacture the lead terminal 1 including the electrode terminal made of a wire mainly containing copper.

[0038] Further, when manufacturing the lead terminal 1 by the same manufacturing method as in the embodiment, the position adjustment of the short-wavelength laser can be easily performed as compared with the configuration in which the laser beam is irradiated so as to intersect obliquely with the axis of the wire 100.

[0039] Furthermore, in general, the absorptivity of a laser beam to a metal varies depending on the wavelength of the laser beam and the type of metal, but the absorptivity of a short-wavelength laser beam to copper is significantly higher than that of an infrared laser beam. Therefore, when the wire 100 is a wire that mainly contains copper, the end 100a of the wire 100 can be appropriately melted by using a short-wavelength laser.

[0040] (Variation 3) 6 to 8C, a lead terminal for an electric storage device and a manufacturing method thereof according to Modification 3 of the present invention will be described using a lead terminal for an electrolytic capacitor as an example. The lead terminal of Modification 3 differs from the lead terminal 1 of the embodiment and Modifications 1 and 2 in that the wire diameter ratio (described later) of the lead wire to the wire material is relatively large.

[0041] As shown in FIG. 6, the lead terminal 101 according to this modification includes an aluminum electrode terminal 102 and a lead wire 103 made of CP wire. The electrode terminal 102 has a rod-shaped portion 121 at one end and a rolled portion 122 at the other end. The lead wire 103 is connected to one end of the rod-shaped portion 121 via a welded portion 104. The diameter of the wire (aluminum wire) (i.e., the diameter of the rod-shaped portion 121) is, for example, 1.2 mm, and the diameter of the lead wire 103 is, for example, 1.0 mm. Hereinafter, the ratio of the diameter of the lead wire to the diameter of the wire (i.e., the diameter of the rod-shaped portion) is referred to as the "wire diameter ratio of the lead wire to the wire" or the "wire diameter ratio of the lead terminal". The wire diameter ratio is calculated as an integer value by rounding off the decimal point. The upper limit of the wire diameter ratio is 100%. In the above example, the wire diameter ratio of the lead terminal 101 is 1.0 / 1.2=83%, which is greater than the wire diameter ratio of 40% (=0.8 / 2) of the lead terminal 1 according to the embodiment and modifications 1 and 2. The lead terminal according to this modification is characterized in that the wire diameter ratio is in the range of 83% or more and 100% or less. In other words, as long as the wire diameter ratio of the lead terminal 101 is within this range, the diameters of the wire material and the lead wire 103 are not limited to the above values.

[0042] The lead terminal 101 can be manufactured by using the wire material and the lead wire 103 having a wire diameter ratio of 83% or more and 100% or less in the first step of the embodiment. The lead terminal 1 can also be manufactured by the manufacturing method of the first modification.

[0043] FIG. 7A is a diagram showing the welded portion 104 of the lead terminal 101 and its vicinity. The diameter of the rod-shaped portion 121 is 1.2 mm, and the diameter of the lead wire 103 is 1.0 mm. FIG. 7B is a schematic diagram of an X-ray image of FIG. 7A. FIG. 7C is a schematic diagram of an EPMA (Electron Probe Micro Analyzer) image of a cross section including the axis of the sample S. The sample S is manufactured by laser welding (strictly speaking, the manufacturing method according to the embodiment) using a material having the same dimensions as the lead terminal 101. On the other hand, FIG. 8A is a diagram showing the welded portion 114 of the lead terminal 111 as a comparative example manufactured by arc welding and its vicinity. The diameter of the rod-shaped portion 131 is 1.2 mm, and the diameter of the lead wire 113 is 1.0 mm. FIG. 8B is a schematic diagram of an X-ray image of FIG. 8A. FIG. 8C is a schematic diagram of an EPMA image of a cross section including the axis of the sample Sc. The sample Sc is manufactured by arc welding using a material having the same dimensions as the lead terminal 111.

[0044] 7A and 8A, in FIG. 7A, the surface of welded portion 104 of lead terminal 101 is relatively smooth, whereas in FIG. 8A, the surface of welded portion 114 of lead terminal 111 has many projections and recesses. Although welded portion 104 has slight bulges in some places, its shape is almost symmetrical about the axis. In contrast, welded portion 114 protrudes significantly in the radial direction, and its shape is asymmetrical about the axis. In general, when an electrolytic capacitor is manufactured using a lead terminal whose welded portion is asymmetrical about the axis, a gap may be generated between the sealing body and the lead terminal, causing electrolyte leakage from the gap, which may result in a deterioration in the quality characteristics of the electrolytic capacitor.

[0045] Therefore, in this modified example, an upper limit value dmu is set for the maximum diameter dm of the welded part, and only lead terminals that satisfy dm < dmu are regarded as acceptable products. The upper limit value dmu is a value that can sufficiently suppress the leakage of the electrolytic solution, and for example, it can be set to "the diameter of the wire + 0.100 mm" (dmu = the diameter of the wire + 0.100 mm). In the examples of FIGS. 7A and 8A, the maximum diameter dm of the welded part 104 is less than the upper limit value dmu, while the maximum diameter dm of the welded part 114 greatly exceeds the upper limit value dmu. For this reason, when manufacturing an electrolytic capacitor using lead terminals with a wire diameter ratio of 83%, laser welding can appropriately suppress the leakage of the electrolytic solution, but arc welding may cause a deterioration in the quality characteristics of the electrolytic capacitor due to the leakage of the electrolytic solution.

[0046] It is considered that the reason why the shape of the welded part of the lead terminal 101 can be adjusted compared to the lead terminal 111 is due to the difference in the welding method. That is, in laser welding, by presetting the environmental conditions during irradiation to conditions corresponding to the wire diameter ratio, the shape of the welded part 104 can be appropriately controlled regardless of the value of the wire diameter ratio. On the other hand, in arc welding, as the wire diameter ratio increases (in other words, as the wire diameter difference between the wire and the lead wire 113 decreases), it becomes more difficult for the lead wire 113 made of CP wire to melt. For this reason, the tip of the lead wire 113 that is not sufficiently melted is vigorously inserted into the molten pool formed at the end of the wire, and as a result, the molten pool is pushed out in the radial direction while mixing with a small amount of molten metal at the tip of the lead wire 113, and it is considered that the welded part 114 has a shape that greatly protrudes in the radial direction.

[0047] Another factor that degrades the quality characteristics of an electrolytic capacitor is the bending strength of the welded part of the lead terminal. The bending strength is an index representing the strength of the welded part. When the operation of bending the lead wire 90° in one direction with respect to the wire and then returning it, and then bending it 90° in the other direction (the direction opposite to the one side) and returning it is defined as one cycle, it is represented by the number of cycles n until the lead wire breaks. For example, when the lead wire breaks in 2 cycles, n = 2. The larger the number of cycles n, the higher the strength of the welded part. In addition, when the lead wire breaks when it is bent 90° in one direction with respect to the wire and then returned, the number of cycles n is defined as "the number of cycles up to that point + 0.5". When manufacturing an electrolytic capacitor using lead terminals with low bending strength, the lead terminals may break due to vibrations or minor impacts during use. In that case, the quality characteristics of the electrolytic capacitor may deteriorate.

[0048] Therefore, in this modification example, a lower limit value nl is set for the number of cycles n, and only lead terminals that satisfy n ≥ nl are regarded as non-defective products. The lower limit value nl is a value that can sufficiently suppress the breakage of the lead terminal caused by vibrations or minor impacts. In the dimensional specifications of this modification example, for example, it can be set to 1.0 cycle. As a result of performing a bending strength test on the lead terminals 101 and 111, the number of cycles n of the lead terminal 101 was 1.5 cycles, which satisfied n ≥ nl, while the number of cycles n of the lead terminal 111 was 0.5 cycles, and n < nl. For this reason, when manufacturing an electrolytic capacitor using lead terminals with a wire diameter ratio of 83%, laser welding can appropriately suppress the breakage of the lead terminals, but arc welding may cause a deterioration in the quality characteristics of the electrolytic capacitor due to the breakage of the lead terminals.

[0049] The reason why the bending strength of the lead terminal 101 is higher than that of the lead terminal 111 is considered to be due to the difference in composition between the welded portion 104 and the welded portion 114. Hereinafter, a description will be given with reference to Figs. 7B, 7C, 8B, and 8C. In Fig. 7B, the portion p1 corresponds to the rod-shaped portion 121, the portion p2 and the upper end of the portion p3 correspond to the welded portion 104, and the remaining portion of the portion p3 corresponds to the lead wire 103. The portion p2 occupies the majority of the welded portion 104. The shading of the colors of the portions p1 to p3 is due to the amount of X-rays transmitted through them. The portion p1 shows a color derived from the main component of the wire (aluminum), and the portion p3 shows a color derived from the main component of the lead wire 103 (iron). Since the portion p2 shows a color intermediate between the two, it is considered that aluminum and iron (strictly speaking, in addition to iron, small amounts of copper and tin) melt and solidify in the portion p2.

[0050] This is also supported by FIG. 7C. That is, in FIG. 7C, the portion p4 corresponds to the rod-shaped portion 121, the portion p5 and the upper end of the portion p6 correspond to the welded portion 104, and the remaining portion of the portion p6 corresponds to the lead wire 103. The portion p5 occupies the majority of the welded portion 104. The shades of the colors of the portions p4 to p6 are due to the types and concentrations of the elements. The portion p4 shows a color derived from the main component (aluminum) of the wire, and the portion p6 shows a color derived from the main component (iron) of the lead wire 103. The portion p5, like the portion p2, shows a color intermediate between the two. From the above, it can be seen that the majority of the welded portion 104 has a composition in which aluminum and iron (strictly speaking, in addition to iron, trace amounts of copper and tin) melt and mix together and then solidify. Hereinafter, such a composition will be referred to as a "mixed composition."

[0051] On the other hand, in FIG. 8B, the portion of portion p11 excluding its lower end corresponds to the rod-shaped portion 131, the lower end of portion p11, portion p12, and the upper end of portion p13 (in other words, the portion of portion p13 covered by portions p11 and p12) correspond to the welded portion 114, and the remaining portion of portion p13 corresponds to the lead wire 113. The portion p13 accounts for the majority of the welded portion 114. The portion p11 shows a color derived from the main component of the wire (aluminum), and the portion p13 shows a color derived from the main component of the lead wire 103 (iron). Since the portion p12 shows a color intermediate between the two, it is considered that aluminum and iron (strictly speaking, in addition to iron, trace amounts of copper and tin) have melted and solidified in the portion p12.

[0052] This is also supported by Fig. 8C. That is, in Fig. 8C, the portion of portion p14 excluding the lower end corresponds to the rod-shaped portion 131, the lower end of portion p14, portion p15, and the upper end of portion p16 (in other words, the portion of portion p16 covered by portions p14 and p15) correspond to the welded portion 114, and the remaining portion of portion p16 corresponds to the lead wire 113. The portion p16 occupies the majority of the welded portion 114. The portion p14 shows a color derived from the main component of the wire (aluminum), and the portion p16 shows a color derived from the main component of the lead wire 113 (iron). Like portion p12, portion p15 shows a color intermediate between the two. From the above, it can be seen that the majority of the welded portion 114 has an iron composition, and that a boundary between different metals (iron and aluminum) is formed between parts p13 and p11 (or between parts p16 and p14) in the welded portion 114. In addition, it can be seen that the mixed composition is formed only in the outer peripheral portion of the welded portion 114.

[0053] Thus, most of the welded portion 104 has a mixed composition of aluminum and iron. Therefore, when a bending load is applied to the lead terminal 101, the welded portion 104 plays a role of a buffer material, so that stress is less likely to concentrate on the welded portion 104, and as a result, it is considered that the bending strength is high. In contrast, most of the welded portion 114 has an iron composition, and a boundary between different metals (iron and aluminum) is formed in the welded portion 114. Therefore, when a bending load is applied to the lead terminal 111, stress is concentrated on the welded portion 114 due to the difference in physical properties (typically hardness and bendability) between iron and aluminum. In particular, in the examples of FIGS. 8A to 8C, the wire diameter ratio is relatively large (in other words, the wire diameter difference between the wire material and the lead wire 113 is small), so the area of ​​the boundary between iron and aluminum increases, and a large stress is concentrated accordingly. As a result, it is considered that the bending strength is low.

[0054] In order to verify the superiority of laser welding over arc welding in terms of wire diameter ratio, the inventors of the present application manufactured seven lead terminal samples (samples 1 to 7) with different wire diameter ratios by laser welding and arc welding, respectively, and conducted tests to investigate their quality. Table 1 below shows the test results of samples 1 to 7 of lead terminals in which the wire material is an aluminum wire and the lead wire is a CP wire. [Table 1]

[0055] In this test, when the maximum diameter dm of the welded part satisfies dm < dmu and the number of cycles n of the bending strength test satisfies n ≧ nl, the quality of the lead terminal is evaluated as good (○), and when dm ≧ dmu or n < nl, the quality of the lead terminal is evaluated as bad (×). The upper limit value dmu is "the diameter of the wire + 0.100 mm" regardless of the wire diameter ratio. On the other hand, the lower limit value nl is set to a predetermined value for each dimensional standard of the lead terminal. For example, when the wire diameter ratio is 33%, nl = 1.5; when the wire diameter ratio is 40%, nl = 2.0; when the wire diameter ratio is 53%, nl = 2.0; when the wire diameter ratio is 57%, nl = 1.5; when the wire diameter ratio is 67%, nl = 1.0; when the wire diameter ratio is 83%, nl = 1.0; when the wire diameter ratio is 100%, nl = 1.0 can be set respectively. Note that different types of CP wires (for example, CP wires with different copper plating layer thicknesses) may be used according to the dimensional standards of the lead terminals.

[0056] In laser welding, the quality is good for all samples 1 to 7. In contrast, in arc welding, although the quality is good for samples 1 to 5, the quality is bad for samples 6 and 7.

[0057] It is considered that the quality of the lead terminals by laser welding is good for all samples 1 to 7 for the following two reasons. That is, the first reason is that in laser welding, by presetting the environmental conditions during irradiation to conditions commensurate with the wire diameter ratio, the shape of the welded part can be appropriately controlled regardless of the value of the wire diameter ratio. The second reason is that in laser welding, since most of the welded part has a mixed composition, stress is less likely to concentrate in the welded part, and high bending strength can be achieved.

[0058] In contrast, the quality of the arc-welded lead terminals of samples 6 and 7 is poor, which is believed to be due to the following two reasons. The first reason is that in arc welding, as the wire diameter ratio increases, the lead wire made of CP wire becomes more difficult to melt, so in lead terminals with a wire diameter ratio of 83% or more, the tip of the insufficiently molten lead wire is forcefully inserted into the molten pool formed at the end of the wire, causing the welded part to protrude significantly in the radial direction. The second reason is that in arc welding, most of the welded part has an iron composition, and in lead terminals with a wire diameter ratio of 83% or more, the area of ​​the boundary between dissimilar metals (iron and aluminum) in the welded part increases, so when a bending load is applied to the lead terminal, large stress is likely to concentrate in the welded part, and the bending strength of the lead terminal decreases.

[0059] The good quality of the arc-welded lead terminals for Samples 1 to 5 is believed to be due to the following two reasons. The first reason is that in lead terminals with a wire diameter ratio of 67% or less, the lead wire made of CP wire melts sufficiently even by arc welding, so that even if the tip of the lead wire is forcefully inserted into the molten pool formed at the end of the wire, the welded part is unlikely to protrude significantly in the radial direction. The second reason is that in lead terminals with a wire diameter ratio of 67% or less, the area of ​​the boundary between different metals in the welded part is relatively small, so that stress is not concentrated in the welded part even when a bending load is applied to the lead terminal.

[0060] According to Table 1, the quality of the lead terminals produced by laser welding can be guaranteed regardless of the wire diameter ratio. However, in this modification, the invention targets lead terminals with a wire diameter ratio of 83% or more and 100% or less. This is because, with the recent development of the automobile industry and the computer industry, the applications of electrolytic capacitors are expected to become more and more diverse in the future, and as a result, there is a demand for the development of lead terminals with a relatively large wire diameter ratio as one of the lead terminals having various dimensional standards. Conventional lead terminals have mostly been manufactured by arc welding, but as is clear from Table 1, it is difficult to ensure the quality when the wire diameter ratio is relatively large with arc welding. In contrast, the lead terminals produced by this modification are manufactured by laser welding, and therefore the quality can be appropriately guaranteed even for lead terminals with a wire diameter ratio (i.e., 83% to 100%) whose quality could not be guaranteed with arc welding.

[0061] In addition, because the wire diameter ratio is large, if the diameter of the wire 100 is the same as that of a conventional wire, a thicker lead wire can be used for the lead wire 103. If the diameter of the lead wire 103 is increased, the thickness of the copper plating layer also increases accordingly. Since the conductivity of the lead wire 103 is mainly provided by copper, this configuration can reduce the electrical resistance of the lead terminal 101 and improve the electrical characteristics of the electrolytic capacitor.

[0062] Moreover, the lead terminal 101 may be manufactured by a manufacturing method according to Modification 2. That is, a wire material mainly containing copper may be used instead of an aluminum wire as the wire material 100. In this case as well, the same results as those in Table 1 were obtained.

[0063] Furthermore, a metal wire mainly containing copper (hereinafter also referred to as a "copper lead wire") may be used as the lead wire 103 instead of the CP wire. Here, "metal wire mainly containing copper" means a metal wire whose outer surface is coated with a tin plating layer or a silver plating layer. In this case, the lead terminal 101 includes two types: "a lead terminal in which the wire material 100 is an aluminum wire and the lead wire 103 is a copper lead wire" and "a lead terminal in which the wire material 100 is a wire material mainly containing copper and the lead wire 103 is a copper lead wire." For both types of lead terminals 101, results similar to those in Table 1 were obtained.

[0064] As described above, the manufacturing method of the lead terminal 101 and the lead terminal 101 according to the third modification can provide a manufacturing method for appropriately manufacturing the lead terminal 101 having the electrode terminal 102 made of the wire 100 mainly containing aluminum or copper, and the lead terminal 101 manufactured by the manufacturing method. The lead terminal 101 may be used as a component of other electricity storage devices, not limited to electrolytic capacitors. The other electricity storage devices include, for example, lithium ion capacitors, electric double layer capacitors, and lithium ion batteries. The same effects can be obtained even when the lead terminal 101 is used as a component of other electricity storage devices.

[0065] Although the embodiment and modifications 1 to 3 have been described above, the present invention is not limited to the above-described embodiment and modifications, and various modifications are possible without departing from the object of the present invention.

[0066] For example, as in the third modification, in the embodiment, the first modification, and the second modification, the type of the lead wire is not limited to the CP wire. The lead wire may be, for example, a copper lead wire (a metal wire mainly containing copper). When a copper lead wire is used in the second modification (i.e., when the main metal materials of the wire 100 and the lead wire 3 are both copper), the following effects can be obtained in addition to the above-mentioned effects. That is, when the main metal materials of the wire 100 and the lead wire 3 are both copper, there is a problem that the lead wire 3 melts excessively when attempting to melt the wire 100 by arc welding, and the wire 100 and the lead wire 3 cannot be properly connected (in other words, the welded portion 4 cannot be properly formed). On the other hand, when the discharge amount is suppressed in order to properly melt the lead wire 3, the wire 100 does not melt sufficiently, and in this case, there is also a problem that the wire 100 and the lead wire 3 cannot be properly connected. In contrast, in the manufacturing method according to the modified example 2, only the end 100a of the wire 100 is melted by laser welding, and the lead wire 3 is pushed into the molten pool A and then melted by the heat of the molten pool A. The molten pool A at the end 100a and the molten copper at the end 3a of the lead wire 3 are mixed and solidified to form the welded portion 4. This manufacturing method can prevent the lead wire 3 from melting excessively or the wire 100 from melting insufficiently, so that the lead terminal 101, in which the main metallic materials of both the wire 100 and the lead wire 3 are copper, which has been difficult to manufacture by arc welding, can be appropriately manufactured. Note that the welded portion 4 is mostly a solidified structure of copper, and contains a small amount of an alloy of copper and other metals (e.g., tin).

[0067] Furthermore, the pushing mechanism may be provided in the jig 200, not in the jig 300. That is, the pushing mechanism may be configured to apply an external force to the wire 100 that pushes the wire 100 axially toward the lead wire 3 by a predetermined distance at a predetermined speed.

[0068] Furthermore, in the above embodiment (and variants 1 to 3), the wire 100, which is the material of the electrode terminal 2, is welded to the lead wire 3, and then the wire 100 is pressed to form the electrode terminal 2. Alternatively, the wire 100 may first be pressed to form the electrode terminal 2, and then the lead wire 3 may be welded to one end of the rod-shaped portion 21.

[0069] Furthermore, in the above embodiment and modifications 1 to 3, the laser irradiator 400 may be a hybrid laser that combines an infrared laser and a short-wavelength laser.

[0070] Furthermore, as described in the above embodiment, the absorptivity of aluminum is equivalent over the entire wavelength bands of infrared light and visible light. Therefore, when an aluminum wire is used for the wire rod 100, other inexpensive laser irradiators may be used in addition to the infrared laser or short wavelength laser. [Explanation of symbols]

[0071] 1,101: lead terminal, 2,102: electrode terminal, 3,103: lead wire, 3a: end of lead wire, 3b: end face of lead wire, 3c: outer circumferential surface of lead wire, 4,104: welded portion, 21,121: rod-shaped portion, 22,122: rolled portion, 100: wire material, 100a: end of wire material, 100b: end face of wire material, 100c: outer circumferential surface of wire material, 200: jig, 300: jig, 400: laser irradiation device

Claims

1. A method for manufacturing a lead terminal for an electricity storage device, the lead terminal comprising an electrode terminal made of a wire material mainly containing aluminum or copper, and a lead wire connected to the electrode terminal via a welded portion, the method comprising the steps of: a first step of aligning the wire and the lead wire in a straight line and holding the wire and the lead wire in a state in which a distance between an end face of the wire on the lead wire side and an end face of the lead wire on the wire wire side is maintained at a predetermined distance; a second step of irradiating a laser beam onto the end of the wire on the lead wire side with a laser irradiator to melt the end; a third step of axially pushing one of the wire rod and the lead wire toward the other to form the welded portion after a predetermined time has elapsed since the start of irradiation of the laser beam in the second step; Equipped with A manufacturing method for lead terminals.

2. 2. A method for manufacturing a lead terminal according to claim 1, comprising the steps of: In the first step, a CP wire or a metal wire mainly containing copper is used as the lead wire. A manufacturing method for lead terminals.

3. 2. A method for manufacturing a lead terminal according to claim 1, comprising the steps of: In the second step, the laser beam is irradiated onto an outer peripheral surface of the end portion of the wire rod in a direction perpendicular to the axial direction. A manufacturing method for lead terminals.

4. 4. The method for manufacturing a lead terminal according to claim 3, In the second step, the laser beam is irradiated to a predetermined position on the outer circumferential surface of the wire. A manufacturing method for lead terminals.

5. 4. The method for manufacturing a lead terminal according to claim 3, In the first step, a wire material mainly containing aluminum is used as the electrode terminal, The predetermined time in the third step is a time for irradiating the laser beam. A manufacturing method for lead terminals.

6. 5. A method for manufacturing a lead terminal according to claim 4, comprising the steps of: In the first step, a wire material mainly containing aluminum is used as the electrode terminal, The predetermined time in the third step is a time for irradiating the laser beam. A manufacturing method for lead terminals.

7. 2. A method for manufacturing a lead terminal according to claim 1, comprising the steps of: In the second step, the laser beam is irradiated onto the end surface of the end of the wire from a direction obliquely intersecting the axial direction. A manufacturing method for lead terminals.

8. A method for manufacturing a lead terminal according to claim 7, comprising the steps of: In the first step, a wire material mainly containing aluminum is used as the electrode terminal, The predetermined time in the third step is a time for irradiating the laser beam. A manufacturing method for lead terminals.

9. A method for manufacturing a lead terminal according to any one of claims 1 to 8, comprising the steps of: In the first step, a wire material mainly containing aluminum is used as the electrode terminal, The laser irradiator is an infrared laser. A manufacturing method for lead terminals.

10. A method for manufacturing a lead terminal according to any one of claims 1 to 4 and 7, comprising the steps of: In the first step, a wire material mainly containing copper is used as the electrode terminal, The laser irradiator is a short wavelength laser or a hybrid laser; A manufacturing method for lead terminals.

11. A method for manufacturing a lead terminal according to any one of claims 1 to 8, comprising the steps of: In the first step, the wire and the lead wire are used such that a wire diameter ratio of the lead wire to the wire is 83% or more and 100% or less. A manufacturing method for lead terminals.

12. A lead terminal for an electricity storage device, comprising: an electrode terminal made of a wire material mainly containing aluminum or copper; and a lead wire connected to the electrode terminal via a welded portion, A ratio of a diameter of the lead wire to a diameter of the wire material is 83% or more and 100% or less. Lead terminal.

13. The lead terminal according to claim 12, The lead wire is a CP wire or a metal wire mainly containing copper. Lead terminal.

Citation Information

Patent Citations

  • Terminal structure of an electrolytic capacitor

    JP1982102125U

  • JP1986065741U

  • Terminal for electronic component and manufacturing method thereof

    JP2004335859A

  • Aluminum electrolytic capacitor

    JP2009043749A

  • Method for producing terminal for electronic component, and terminal for electronic component produced by the production method

    WO2011052091A1