Aqueous coating material

The aqueous coating material with light-shielding and translucent colored grains addresses the issue of uneven grain patterns, achieving a uniform and visually appealing design on building surfaces.

JP2024169820APending Publication Date: 2024-12-06BEKKU KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023086590
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for creating grain patterns on building surfaces, such as those using clear paints with aggregates like silica sand and mica, often result in uneven particle scattering and difficulty in achieving a homogeneous design.

Method used

Aqueous coating material containing specific colored grains dispersed in an aqueous medium, comprising light-shielding and translucent colored grains of similar and different colors, forming a uniform grain pattern with a sense of depth and perspective.

Benefits of technology

The coating material enables the formation of a uniform grain pattern with excellent design, providing stable and aesthetically appealing results on building surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169820000001
    Figure 2024169820000001
Patent Text Reader

Abstract

To provide a coating material that enables the formation of a uniform particle-patterned coating layer with superior design qualities.SOLUTION: An aqueous coating material contains liquid or gel-like colored particles dispersed in an aqueous medium. The colored particles include light-shielding colored particles (A) that contain a color pigment, and translucent colored particles (a) that contain a color pigment and have the same color as the light-shielding colored particles, as well as colored particles (B) that have a different color from the above light-shielding colored particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel water-based coating material.

[0002] Conventionally, in order to improve the design of buildings, civil engineering structures, etc., a method of applying a pattern with scattered particles (hereinafter also simply referred to as a "particle pattern") to the surface has been adopted. For example, Patent Document 1 describes a method of forming a particle pattern by spray painting using a colored coating material prepared to a specific viscosity while controlling the pattern and discharge amount during painting. Patent Document 2 also describes a method of painting a base coating material, and then unevenly painting a colored coating material of a different color from the base coating material.

[0003] However, these techniques all relate to painting methods carried out in factories, and the grain pattern is created by mechanically controlling the colored coating material and sputtering coating. Even if the techniques described in the above patent documents are applied to on-site painting of existing buildings and civil engineering structures, it is difficult to stably obtain grain patterns of the desired size, and the current situation is that they lack practicality.

[0004] On the other hand, a method is also known in which a clear paint in which aggregate such as silica sand or mica is dispersed in a resin liquid is applied to the wall surface of a building to impart a grain pattern. According to this method, a desired grain pattern can be obtained by setting the grain size of the aggregate used. For example, Patent Document 3 describes a method of applying a clear paint containing flat coloring matter such as mica on a multicolored laminated pattern coating film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-186381 [Patent Document 2] Japanese Utility Model Application Publication No. 4-77440 [Patent Document 3] Patent No. 6180678 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when a clear coating containing aggregates such as silica sand or mica is applied as in Patent Document 3, the aggregates tend to gather together on the surface to be coated, which can lead to uneven dispersion of the particles, making it difficult to obtain a uniform particle pattern.

[0007] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a coating material capable of forming a coating film exhibiting a uniform grain pattern with excellent design properties. [Means for solving the problem]

[0008] As a result of extensive research into achieving the above object, the inventors of the present invention came up with the idea of ​​an aqueous coating material in which specific color particles are dispersed in an aqueous medium, and completed the present invention.

[0009] That is, the present invention has the following features. 1. An aqueous coating material in which liquid or gel-like color particles are dispersed in an aqueous medium, The above color particles are Light-shielding color particles (A) containing a coloring pigment; (a) light-transmitting color particles containing a color pigment and having the same color as the light-shielding color particles; and Color particles (B) of a different color from the above light-blocking color particles An aqueous coating material comprising: Effect of the Invention

[0010] The aqueous coating material of the present invention can form a coating film that exhibits a uniform grain pattern with excellent design properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described.

[0012] The aqueous coating material of the present invention is a material in which liquid or gel-like color particles are dispersed in an aqueous medium. Such aqueous coating materials are classified into oil-in-water type (O / W type) and water-in-water type (W / W type) depending on the combination of color particles and aqueous medium (color particles / aqueous medium) constituting the aqueous coating material. In the present invention, a water-in-water type (W / W type) aqueous coating material is suitable. The mass ratio of the color particles to the aqueous medium (color particles:aqueous medium) is preferably 1:99 to 80:20 (more preferably 10:90 to 75:25, and even more preferably 30:70 to 70:30).

[0013] The color particles in the aqueous coating material contain color pigments, and specifically, a coloring material containing a resin, a coloring pigment, and various additives as necessary is dispersed in a liquid or gel state in an aqueous medium. Examples of the resin in the coloring material include acrylic resin, urethane resin, vinyl acetate resin, acrylic vinyl acetate resin, acrylic urethane resin, acrylic silicone resin, fluororesin, polyvinyl alcohol, biogum, galactomannan derivatives, alginic acid derivatives, and cellulose derivatives. When such a resin is in the form of a water-soluble resin and / or a water-dispersible resin (resin emulsion), dispersing the coloring material in an aqueous medium results in a water-in-water (W / W) aqueous coating material. The resin solid content ratio in the coloring material is preferably 50% by mass or less, more preferably 3 to 40% by mass, and even more preferably 5 to 30% by mass.

[0014] The coloring pigment in the coloring material is a component that imparts color to the color particles. Examples of the coloring pigment include inorganic chromatic pigments such as ferric oxide (red oxide), yellow iron oxide, ultramarine, cobalt blue, and cobalt green; organic chromatic pigments such as azo, naphthol, pyrazolone, anthraquinone, perylene, quinacridone, disazo, isoindolinone, benzimidazole, phthalocyanine, and quinophthalone; black pigments such as carbon black, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, black iron oxide, iron-chromium composite oxide, manganese-bismuth composite oxide, and manganese-yttrium composite oxide; white pigments such as titanium oxide, zinc oxide, and alumina; and pearl pigments, aluminum pigments, photoluminescent pigments, phosphorescent pigments, and fluorescent pigments. These can be used alone or in combination of two or more. The average particle size of the color pigment is preferably 2 μm or less, more preferably 0.01 to 1 μm. In the present invention, the average particle size of the pigment is an average value measured using a laser diffraction particle size distribution measuring device (measurement temperature: 25° C.).

[0015] The color pigment ratio in the colorant is preferably 0.01 to 50 mass %, more preferably 0.1 to 20 mass %, and further preferably 0.5 to 10 mass %. In the present invention, "a to b" is synonymous with "a or more and b or less".

[0016] The method of dispersing the colorant in a granular form in the aqueous medium is not particularly limited, and a known method can be adopted. For example, a method conforming to the manufacturing method of the material specified in JIS K5667:2003 "Multicolored Paint" can be adopted. Specifically, a method of dispersing the colorant in an aqueous medium containing a dispersion stabilizer can be adopted. The dispersion stabilizer is a component that stabilizes the colorant in a granular form, and acts as, for example, a gelling agent for the colorant. The dispersion stabilizer can be selected according to the type of resin and colorant. Specific examples of the dispersion stabilizer include magnesium salts, calcium salts, barium salts, aluminum salts, sodium salts, potassium salts, borates, and phosphates. In addition, for example, water-soluble polymers, clays, and the like can be used as the dispersion stabilizer. The aqueous medium can also contain the same resin (water-soluble resin, resin emulsion, etc.) as described above. The resin solid content ratio in the aqueous medium is preferably 50% by mass or less, more preferably 3 to 45% by mass, and even more preferably 5 to 40% by mass.

[0017] The colorant and the aqueous medium may each contain various additives, such as extender pigments, aggregates, fillers, matting agents, fibers, gel formers, pigment dispersants, emulsifiers, thickeners, film-forming assistants, leveling agents, coupling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, dryness adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, defoamers, adsorbents, deodorizers, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, crosslinking agents, and the like.

[0018] The coloring material and / or the aqueous medium contain an extender pigment, etc., so that the aqueous coating material film can be made matte. Examples of the extender pigment include heavy calcium carbonate, dansui stone, light calcium carbonate, white carbon, talc, kaolin, clay, china clay, diatomaceous earth, baryte powder, barium sulfate, precipitated barium sulfate, silica sand, silica stone powder, quartz powder, and resin beads, and these can be used alone or in combination of two or more. The refractive index of the extender pigment is preferably 1.4 to 1.7. The average particle size of the extender pigment is preferably 50 μm or less, more preferably 0.1 to 30 μm, and even more preferably 0.5 to 20 μm.

[0019] The ratio of the extender pigment in the colorant is preferably 50% by mass or less, more preferably 3 to 45% by mass, and even more preferably 5 to 40% by mass. The ratio of the extender pigment in the aqueous medium is preferably 50% by mass or less, more preferably 3 to 45% by mass, and even more preferably 5 to 40% by mass.

[0020] The particle size and shape of the color particles can be set appropriately. Specifically, the shape of the stirring blade during production, the size and position of the stirring blade relative to the stirring tank, the rotation speed of the stirring blade, the stirring time, the viscosity of the coloring material, the method and concentration of the dispersion stabilizer added, the viscosity of the aqueous medium, etc. may be appropriately selected and adjusted. The average particle size of the color particles is preferably 0.05 to 20 mm (more preferably 0.1 to 18 mm). In the present invention, the average particle size of the color particles is a value obtained by drying the color particles on a standard white paper for 48 hours under standard conditions (temperature 23°C, relative humidity 50%; the same applies below) and calculating the average major axis (average value of 50 color particles).

[0021] In order to obtain an aqueous coating material containing two or more kinds of color particles, for example, A method of preparing a color particle dispersion liquid in which one type of coloring material is dispersed (a color particle dispersion liquid containing one type of color particle) and then mixing these, or A method in which two or more colorants having different color tones are added simultaneously or sequentially to an aqueous medium and dispersed therein; Methods such as the above can be adopted.

[0022] In the aqueous coating material of the present invention, the color particles include light-shielding color particles (A) containing a coloring pigment (hereinafter also referred to as "light-shielding color particles (A)"), light-transmitting color particles (a) containing a coloring pigment and having the same color as the light-shielding color particles (hereinafter also referred to as "light-transmitting color particles (a)"), and color particles (B) (hereinafter also referred to as "color particles (B)") having a different color from the light-shielding color particles (A). By containing such specific color particles, the aqueous coating material of the present invention can form a coating film that exhibits a homogeneous grain pattern with excellent design. In the present invention, the light-transmitting color particles are relatively more translucent than the light-shielding color particles.

[0023] The aqueous coating material of the present invention contains two kinds of color particles of the same color but relatively different translucency in one material, that is, light-shielding color particles (A) and light-transmitting color particles (a) of the same color as the light-shielding color particles, and further contains color particles (B) of a different color. Therefore, when such an aqueous coating material is applied, the light-shielding color particles (A) and the light-transmitting color particles (a) form a background (base color) having a sense of depth with the base coating material, and a grain pattern in which the color particles (B) are scattered in such a background (base color) can be formed. The density of the color particles (B) in the formed coating film corresponds to the ratio of the color particles (B) to the total color particles of the aqueous coating material. When the coating film is observed, a sense of perspective can be given that the color particles (B) are present in the foreground. In the present invention, it is considered that such an action can form a coating film exhibiting a homogeneous grain pattern with excellent design. The base color is the color that occupies the largest area among the multiple colors in the formed coating film.

[0024] The light-shielding color particles (A) and the light-transmitting color particles (a) may be any particles that can be visually recognized as being the same color. In a preferred embodiment, the color difference (ΔE) between the coloring materials constituting each color particle is preferably less than 10 (more preferably 9.5 or less, and even more preferably 9 or less), and in particular, the brightness difference |ΔL| {L *1 -L *2 )} is more preferably less than 10 (more preferably 9.5 or less, and even more preferably 9 or less).

[0025] The color difference (ΔE) is a value measured using a colorimeter. Specifically, the coloring material that constitutes each color particle is applied to a standard white paper with a thickness of 500 μm, and the L of the coating when it is dried for 48 hours under standard conditions is * Value, a * Value, b * It can be calculated using the following formula from the value (average value of three or more measurement points). <Formula>△E={(L *1 -L *2 ) 2 +(a *1 -a *2 ) 2 +(b *1 -b *2 ) 2} 0.5 (In the formula, L *1 , a *1 , b *1 are the L of the coloring material that composes one of the color particles. * , a * , b * .L *2 , a *2 , b *2 are the L of the coloring material that composes the other color particle, * , a * , b * )

[0026] In the aqueous coating material of the present invention, the light-blocking color particles (A) are obtained by using a light-blocking colorant as the colorant constituting the color particles, and the light-transmitting color particles (a) are obtained by using a light-transmitting colorant as the colorant constituting the color particles.

[0027] As the light-shielding colorant, one having a relatively higher hiding rate than the light-transmitting colorant can be used. The difference in the hiding rate between the light-shielding colorant and the light-transmitting colorant {(light-shielding colorant hiding rate)-(light-transmitting colorant hiding rate)} is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more. The hiding rate is a value measured by the method of 7.9 "Hiding rate" of JIS K5663:2021 "Synthetic resin emulsion paint and sealer".

[0028] The hiding ratio of the light-shielding colorant is preferably 10% or more higher than the hiding ratio of the light-transmitting colorant, more preferably 20% or more higher, and even more preferably 30% or more higher. The hiding ratio of the light-shielding colorant is preferably more than 60%, more preferably 65 to 100%, and even more preferably 70 to 99%.

[0029] To obtain such a light-shielding colorant, for example, a resin, a coloring pigment, and various additives as necessary may be mixed in consideration of color tone, hiding rate, etc. The ratio of the coloring pigment in the light-shielding colorant varies depending on the type of the coloring pigment used, etc., but is preferably 0.5 to 50 mass%, more preferably 1 to 20 mass%, and even more preferably 1.6 to 10 mass%.

[0030] The average particle size of the light-blocking color particles (A) can be preferably 0.05 to 20 mm, more preferably 0.1 to 18 mm, further preferably 0.2 to 15 mm, and particularly preferably 0.3 to 12 mm. In the present invention, the average particle size of the light-blocking color particles (A) can be larger than the average particle size of the light-transmitting color particles (a). In this case, the average particle size of the light-blocking color particles (A) is preferably 1 to 20 mm, more preferably 2 to 18 mm, further preferably 2.5 to 15 mm, and particularly preferably 3 to 12 mm. The light-blocking color particles (A) having such an average particle size are preferred in terms of base covering properties and suppression of turbidity of the color particles (B), and are also suitable in terms of overall design improvement, etc.

[0031] The light-transmitting color particles (a) in the aqueous coating material can be obtained by setting the hiding rate of the light-transmitting coloring material constituting the light-transmitting color particles (a) relatively lower than the hiding rate of the light-shielding coloring material. The hiding rate of the light-transmitting coloring material can be set to a value relatively lower than the hiding rate of the light-shielding coloring material, for example, within the range of a hiding rate of 0 to 80%. The hiding rate of the light-transmitting coloring material is preferably 60% or less, more preferably 6 to 55%, even more preferably 7 to 50%, and particularly preferably 8 to 45%.

[0032] To obtain such a light-transmitting colorant, for example, a method of mixing a resin, a coloring pigment, and various additives as necessary, a method of mixing a light-shielding colorant with a resin and / or an extender pigment, a method of mixing a light-transmitting colorant with a light-shielding colorant, etc. can be adopted in consideration of color tone, hiding rate, etc. The coloring pigment ratio in the light-transmitting colorant varies depending on the type of coloring pigment used, etc., but is preferably 0.01 to 10 mass%, more preferably 0.1 to 5 mass%, further preferably 0.5 to 2 mass%, and particularly preferably 0.51 to 1.5 mass%.

[0033] The average particle size of the light-transmitting color particles (a) can be preferably 0.05 to 20 mm, more preferably 0.1 to 18 mm, even more preferably 0.2 to 15 mm, and particularly preferably 0.3 to 12 mm. In the present invention, the average particle size of the light-transmitting color particles (a) can be smaller than the average particle size of the light-shielding color particles (A), and in that case, the average particle size of the light-transmitting color particles (a) is preferably 0.05 to 5 mm, more preferably 0.1 to 3 mm, even more preferably 0.2 to 2 mm, and particularly preferably 0.3 to 1.9 mm. The light-transmitting color particles (a) having such an average particle size can fully exhibit the effect of filling the gaps in the grain pattern and the effect of imparting a sense of depth, and are suitable in terms of base covering properties, design improvement, and the like.

[0034] In the aqueous coating material, the mass ratio of the light-shielding color particles (A) to the light-transmitting color particles (a) is preferably 99:1 to 5:95, more preferably 98:2 to 30:70, and further preferably 97:3 to 50:50. Such a mass ratio is preferable in terms of base coverage and imparting a sense of depth, and can further enhance the design.

[0035] The light-shielding color particles (A) and the light-transmitting color particles (a) are color particles that exhibit a base color in the formed coating film, and are contained in the largest proportion of the color particles of multiple colors contained in the aqueous coating material. The total mass ratio of the light-shielding color particles (A) and the light-transmitting color particles (a) in the aqueous coating material is preferably 20 to 99 mass%, more preferably 50 to 98 mass%, and even more preferably 55 to 97 mass% of the total amount of the light-shielding color particles (A), the light-transmitting color particles (a), and the color particles (B). With such a mass ratio, the effect of the present invention can be fully exhibited.

[0036] The color particles (B) in the water-based coating material can be visually recognized as having a different color from the light-shielding color particles (A). In a preferred embodiment, the color difference (ΔE) between the coloring materials constituting each color particle is preferably 10 or more (more preferably 13 or more, and even more preferably 15 or more), and in particular, the brightness difference |ΔL| {the above (L *1 -L *2 )} is more preferably 10 or more (more preferably 11 or more, further preferably 13 or more, and particularly preferably 15 or more).

[0037] The color particles (B) may be either light-shielding color particles or light-transmitting color particles. The light-shielding color particles (B) are obtained by using a light-shielding coloring material as a coloring material constituting the color particles (B), and the light-transmitting color particles (B) are obtained by using a light-transmitting coloring material as a coloring material constituting the color particles (B).

[0038] When the color particles (B) are light-shielding color particles, a clear grain pattern can be formed, which is also suitable in terms of imparting a sense of perspective. In this case, the hiding ratio of the coloring material constituting the color particles (B) is preferably more than 60%, more preferably 65 to 100%, and even more preferably 70 to 99%. To obtain such a coloring material, for example, a resin, a coloring pigment, and various additives, etc., may be mixed in consideration of the color tone, hiding ratio, etc. The coloring pigment ratio in such a coloring material is preferably 0.5 to 50 mass%, more preferably 1 to 20 mass%, and even more preferably 1.6 to 10 mass%, depending on the type of coloring pigment used.

[0039] The average particle size of the color particles (B) is preferably 0.05 to 20 mm, more preferably 0.1 to 18 mm, further preferably 0.2 to 15 mm, and particularly preferably 0.3 to 12 mm. Color particles (B) having such an average particle size are suitable in terms of improving the design of the particle pattern.

[0040] The color particles (B) may contain one type (one color) or more, or may contain two types (two colors) or more. The aqueous coating material of the present invention may contain at least one type of color particles (B) that is a different color from the light-shielding color particles (A) so that a grain pattern can be formed.

[0041] The mass ratio of the color particles (B) in the aqueous coating material is preferably 1 to 80 mass % of the total amount of the light-shielding color particles (A), the light-transmitting color particles (a) and the color particles (B), more preferably 2 to 50 mass %, and further preferably 3 to 45 mass %. Such a mass ratio is suitable in terms of improving the design of the grain pattern.

[0042] The aqueous coating material of the present invention can be applied to, for example, the wall surfaces of buildings, civil engineering structures, etc. Examples of the substrates constituting such wall surfaces include concrete, mortar, metal, wood, glass, etc., or various plate-shaped wall materials, etc. Examples of the plate-shaped wall materials include inorganic hardened bodies mainly composed of cement, calcium silicate, lime, gypsum, etc. Specific examples of such plate-shaped wall materials include cement boards, extrusion molding boards, slate boards, PC boards, ALC boards, fiber-reinforced cement boards, siding boards, ceramic boards, calcium silicate boards, gypsum boards, hard wood chip cement boards, etc.

[0043] Before applying the aqueous coating material, the substrate may be subjected to a surface treatment as necessary. Examples of the surface treatment include cleaning, scraping, filler, putty, surfacer, and sealer. Such surface treatment may be appropriately performed taking into consideration the type and condition of the existing coating, for example.

[0044] Before the application of the aqueous coating material, a process of applying one or more colored undercoats can be performed. As the colored undercoat material, for example, a material containing a resin and a colored pigment, which can form a uniform monochromatic coating by its color development, can be used. The color tone of the colored undercoat material can be set in consideration of the color tone of the aqueous coating material, for example, it can be set to an approximate color of the aqueous coating material. As the colored undercoat material, for example, a material that forms a flat coating, a material that forms various uneven patterns, etc. can be used.

[0045] The method of applying the colored undercoat material can be, for example, spray coating, roller coating, trowel coating, brush coating, etc. The amount of the colored undercoat material applied is preferably 0.05 to 1 kg / m 2 , more preferably 0.1 to 0.8 kg / m 2 It is desirable to apply the colored undercoat material uniformly over the entire substrate to be painted. The colored undercoat material may be applied and dried preferably at room temperature (0 to 40°C).

[0046] In the present invention, the above-mentioned surface treatment, the application of a colored undercoat material, etc. are performed as necessary, and then the aqueous coating material is applied. When the colored undercoat material is applied, it is preferable to apply the aqueous coating material after the coating of the colored undercoat material has dried.

[0047] The method of applying the water-based coating material can be, for example, spray coating, roller coating, brush coating, etc. The amount of the water-based coating material applied is, for example, 1.5 kg / m 2 The concentration can be set to 0.1 to 1 kg / m or less, preferably 0.1 to 1 kg / m 2 , more preferably 0.2 to 0.7 kg / m 2 The aqueous coating material of the present invention can form a coating film with excellent design even when the coating amount is small, and the upper limit of the coating amount is 0.5 kg / m 2 Less than 0.48kg / m 2 The aqueous coating material can be applied in a range of 100 to 2000 nm, and even if the amount of the coating is relatively small, the coating material can exhibit a good base coating property. The application and drying of the aqueous coating material may be preferably carried out at room temperature.

[0048] When applying the aqueous coating material, the viscosity can be adjusted appropriately by mixing a diluent such as water. The dilution ratio is preferably 0 to 10 mass %. The viscosity of the aqueous coating material to be applied is preferably 1 to 30 Pa s (more preferably 2 to 20 Pa s), and the thixotropy index is preferably 2 to 9 (even more preferably 3 to 8).

[0049] In the present invention, the coating of the water-based coating material can be the outermost surface, and if necessary, a clear coat material can be applied to the surface of the coating of the water-based coating material. The clear coat material can be applied after the coating of the water-based coating material has dried.

[0050] As the clear coat material, for example, acrylic resin, urethane resin, silicone resin, acrylic silicone resin, fluororesin, or composite resin thereof, or colloidal silica, etc., can be used. These may have crosslinking reactivity, and may contain, for example, a hydrophilizing agent, a water repellent agent, etc., depending on the purpose. As the clear coat material, a water-based material is suitable. As the clear coat material, for example, a glossy type, a matte type, etc. can be appropriately selected and used.

[0051] The method of applying the clear coat material can be, for example, spray coating, roller coating, brush coating, etc. The amount of the clear coat material applied is preferably 0.03 to 0.5 kg / m 2 , more preferably 0.05 to 0.4 kg / m 2 The application and drying of the clear coat material may be preferably carried out at room temperature. EXAMPLES

[0052] The following examples will clarify the features of the present invention, but the present invention is not limited to these examples.

[0053] ·Colored particle dispersion 1 75 parts by mass of synthetic resin emulsion 1 (acrylic silicone resin emulsion, solid content 40% by mass) was charged into a container, and 4 parts by mass of film-forming agent, 10 parts by mass of water, 10 parts by mass of gelling agent (5% by mass aqueous solution of ammonium borate), and 1 part by mass of defoaming agent were added and mixed uniformly to produce aqueous medium 1. Meanwhile, in another container, 40 parts by mass of synthetic resin emulsion 1 (same as above) was charged, 2 parts by mass of film-forming agent, 3.5 parts by mass of white pigment liquid (60% by mass dispersion of titanium oxide), 0.04 parts by mass of yellow pigment liquid (60% by mass dispersion of yellow iron oxide), 0.04 parts by mass of red pigment liquid (60% by mass dispersion of red iron oxide), 0.4 parts by mass of blue pigment liquid (60% by mass dispersion of cobalt blue), 15 parts by mass of extender pigment, 30 parts by mass of gel-forming substance (3% by mass aqueous solution of galactomannan), 7.52 parts by mass of water, 1 part by mass of thickener, and 0.5 parts by mass of defoamer were uniformly mixed to produce colorant 1 (light-shielding colorant). The color tone of this colorant 1 is light blue, the color pigment ratio is 2.4% by mass, and the hiding ratio is 86%. 100 parts by mass of colorant 1 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed by stirring to obtain color particle dispersion 1 in which light blue light-blocking color particles having an average particle size of 4.5 mm were dispersed.

[0054] ·Colored particle dispersion 2 In the same manner as in the above-mentioned color particle dispersion liquid 1, an aqueous medium 1 and a colorant 1 were prepared. 100 parts by mass of colorant 1 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed by stirring to obtain color particle dispersion 2 in which light blue light-blocking color particles having an average particle size of 1.0 mm were dispersed.

[0055] ·Colored particle dispersion 3 Aqueous medium 1 was prepared in the same manner as for color particle dispersion 1 described above. Meanwhile, in another container, 40 parts by mass of synthetic resin emulsion 1 (same as above) was charged, and 2 parts by mass of film-forming agent, 0.88 parts by mass of white pigment liquid (same as above), 0.1 parts by mass of blue pigment liquid (same as above), 15 parts by mass of extender pigment, 30 parts by mass of gel-forming substance (same as above), 10.32 parts by mass of water, 1.2 parts by mass of thickener, and 0.5 parts by mass of defoamer were uniformly mixed to produce colorant 2 (translucent colorant). The color tone of this colorant 2 is light blue, the color pigment ratio is 0.59% by mass, the hiding ratio is 23%, the color difference △E from colorant 1 is 1 or less, and |△L| is 1 or less. 100 parts by mass of colorant 2 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed by stirring to obtain color particle dispersion 3 in which light-blue translucent color particles having an average particle size of 0.6 mm were dispersed.

[0056] ·Colored particle dispersion 4 An aqueous medium 1 was produced in the same manner as in the above-mentioned color particle dispersion 1. A colorant 2 was produced in the same manner as in the above-mentioned color particle dispersion 3. 100 parts by mass of colorant 2 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed by stirring to obtain color particle dispersion 4 in which light blue translucent color particles having an average particle size of 1.0 mm were dispersed.

[0057] ·Colored particle dispersion 5 An aqueous medium 1 was produced in the same manner as in the above-mentioned color particle dispersion 1. A colorant 2 was produced in the same manner as in the above-mentioned color particle dispersion 3. 100 parts by mass of colorant 2 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed by stirring to obtain color particle dispersion 5 in which light blue translucent color particles having an average particle size of 1.8 mm were dispersed.

[0058] ·Colored particle dispersion 6 Aqueous medium 1 was prepared in the same manner as for color particle dispersion 1 described above. Meanwhile, in another container, 40 parts by mass of synthetic resin emulsion 1 (same as above) was charged, 2 parts by mass of film-forming agent, 7.4 parts by mass of white pigment liquid (same as above), 0.6 parts by mass of black pigment liquid (black iron oxide 60% by mass dispersion liquid), 15 parts by mass of extender pigment, 30 parts by mass of gel-forming substance (same as above), 3.5 parts by mass of water, 1 part by mass of thickener, and 0.5 parts by mass of defoamer were uniformly mixed to produce colorant 3 (light-shielding colorant). The color tone of this colorant 3 is gray, the color pigment ratio is 4.8% by mass, the hiding rate is 99%, and the color difference △E from colorant 1 is 16, and |△L| is 15. 100 parts by mass of colorant 3 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed with stirring to obtain color particle dispersion 6 in which gray light-shielding color particles having an average particle size of 8.0 mm were dispersed.

[0059] ·Colored particle dispersion 7 Aqueous medium 1 was prepared in the same manner as for color particle dispersion 1 described above. Meanwhile, in another container, 40 parts by mass of synthetic resin emulsion 1 (same as above) was charged, 2 parts by mass of film-forming agent, 4.6 parts by mass of white pigment liquid (same as above), 1.2 parts by mass of black pigment liquid (same as above), 0.32 parts by mass of yellow pigment liquid (same as above), 0.54 parts by mass of red pigment liquid (same as above), 15 parts by mass of extender pigment, 30 parts by mass of gel-forming substance (same as above), 4.84 parts by mass of water, 1 part by mass of thickener, and 0.5 parts by mass of defoamer were uniformly mixed to produce colorant 4 (light-shielding colorant). The color tone of this colorant 4 is reddish brown, the color pigment ratio is 4.0% by mass, the hiding rate is 97%, the color difference △E from colorant 1 is 19, and |△L| is 17. 100 parts by mass of colorant 4 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed with stirring to obtain color particle dispersion 7 in which reddish-brown light-shielding color particles having an average particle size of 5.6 mm were dispersed.

[0060] ·Colored particle dispersion liquid 8 Aqueous medium 1 was prepared in the same manner as for color particle dispersion 1 described above. Meanwhile, in another container, 40 parts by mass of synthetic resin emulsion 1 (same as above) was charged, and 2 parts by mass of film-forming agent, 4.0 parts by mass of black pigment liquid (same as above), 15 parts by mass of extender pigment, 30 parts by mass of gel-forming substance (same as above), 7.5 parts by mass of water, 1 part by mass of thickener, and 0.5 parts by mass of defoamer were uniformly mixed to produce colorant 5 (light-shielding colorant). The color tone of this colorant 5 is black, the color pigment ratio is 2.4% by mass, the hiding ratio is 81%, the color difference △E from colorant 1 is 49, and |△L| is 49. 100 parts by mass of colorant 5 was added to the above-mentioned aqueous medium 1 (100 parts by mass) and dispersed with stirring to obtain color particle dispersion 8 in which black light-blocking color particles having an average particle size of 3.8 mm were dispersed.

[0061] In the production of each of the above color particle dispersions, the average particle size of the color particles was adjusted by appropriately setting the stirring speed and stirring time after adding the colorant to the aqueous medium.

[0062] Example 1 By mixing color particle dispersion 1, color particle dispersion 3, and color particle dispersion 6 in a mass ratio of 60:15:25, water-based coating material 1 (light blue light-blocking color particles: light blue light-transmitting color particles: gray light-blocking color particles = 60:15:25 (mass ratio)) was obtained. Water-based coating material 1 was applied to the base (slate board coated with a white-colored primer) at a rate of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated as follows.

[0063] As Evaluation 1, the base coverage was evaluated. The evaluation criteria were a three-level scale (A>B>C: poor), with "A" being the grade where the base between the grains was sufficiently concealed by the base color.

[0064] As evaluation 2, the depth of the coating was evaluated. The evaluation criteria were a three-level scale (A>B>C: poor), with A being a coating that had a depth.

[0065] As evaluation 3, the uniformity and clarity of the grain pattern were evaluated. The evaluation criteria were a three-level scale (A>B>C: poor), with "A" being a uniform and clear grain pattern.

[0066] The coating film obtained in Example 1 had a base color (light blue) with gray particles scattered therein, and was excellent in all evaluations.

[0067] Example 2 By mixing color particle dispersion 1, color particle dispersion 4, and color particle dispersion 6 in a mass ratio of 60:15:25, an aqueous coating material 2 (light blue light-blocking color particles: light blue light-transmitting color particles: gray light-blocking color particles = 60:15:25 (mass ratio)) was obtained. The same substrate as in Example 1 was coated with the water-based coating material 2 at a coating amount of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating obtained in Example 2 had a base color (light blue) with gray particles scattered therein, and was excellent in all evaluations.

[0068] Example 3 By mixing color particle dispersion 1, color particle dispersion 5, and color particle dispersion 6 in a mass ratio of 60:15:25, an aqueous coating material 3 (light blue light-blocking color particles: light blue light-transmitting color particles: gray light-blocking color particles = 60:15:25 (mass ratio)) was obtained. The water-based coating material 3 was applied to the same substrate as in Example 1 at a coating amount of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating obtained in Example 3 had gray particles scattered across the base color (light blue), and was excellent in all evaluations.

[0069] Example 4 By mixing color particle dispersion 1, color particle dispersion 4, color particle dispersion 6, color particle dispersion 7, and color particle dispersion 8 in a mass ratio of 55:15:10:10:10, an aqueous coating material 4 (light blue light-blocking color particles: light blue translucent color particles: gray light-blocking color particles: reddish-brown light-blocking color particles: black light-blocking color particles = 55:15:10:10:10 (mass ratio)) was obtained. The water-based coating material 4 was applied to the same substrate as in Example 1 at a rate of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating film obtained in Example 4 had a base color (light blue) with gray particles, reddish brown particles, and black particles scattered throughout, and was excellent in all evaluations.

[0070] Example 5 By mixing color particle dispersion 1, color particle dispersion 4, color particle dispersion 6, color particle dispersion 7, and color particle dispersion 8 in a mass ratio of 65:5:10:10:10, an aqueous coating material 5 (light blue light-blocking color particles: light blue translucent color particles: gray light-blocking color particles: reddish-brown light-blocking color particles: black light-blocking color particles=65:5:10:10:10 (mass ratio)) was obtained. The water-based coating material 5 was applied to the same substrate as in Example 1 at a coating amount of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating film obtained in Example 5 had a base color (light blue) with gray particles, reddish brown particles, and black particles scattered throughout, and was excellent in all evaluations.

[0071] Example 6 By mixing color particle dispersion 1, color particle dispersion 4, color particle dispersion 6, color particle dispersion 7, and color particle dispersion 8 in a mass ratio of 40:30:10:10:10, an aqueous coating material 6 (light blue light-blocking color particles: light blue light-transmitting color particles: gray light-blocking color particles: reddish-brown light-blocking color particles: black light-blocking color particles = 40:30:10:10:10 (mass ratio)) was obtained. The water-based coating material 6 was applied to the same substrate as in Example 1 at a rate of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating film obtained in Example 6 had a base color (light blue) with gray particles, reddish brown particles, and black particles scattered throughout, and was excellent in all evaluations.

[0072] Example 7 By mixing color particle dispersion 2, color particle dispersion 4, color particle dispersion 6, color particle dispersion 7, and color particle dispersion 8 in a mass ratio of 20:50:10:10:10, an aqueous coating material 7 (light blue light-blocking color particles: light blue translucent color particles: gray light-blocking color particles: reddish-brown light-blocking color particles: black light-blocking color particles=20:50:10:10:10 (mass ratio)) was obtained. The water-based coating material 7 was applied to the same substrate as in Example 1 at a rate of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating obtained in Example 7 had a base color (light blue) with gray particles, reddish brown particles, and black particles scattered throughout, and generally showed good evaluation results.

[0073] Comparative Example 1 The color particle dispersion 1 and the color particle dispersion 6 were mixed in a mass ratio of 75:25 to obtain a water-based coating material 8 (light blue light-blocking color particles: gray light-blocking color particles=75:25 (mass ratio)). The water-based coating material 8 was applied to the same substrate as in Example 1 at a coating amount of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating obtained in Comparative Example 1 had gray particles scattered across the base color (light blue), but was not sufficient in terms of ratings of 1 (base hiding power) or 2 (depth).

[0074] Comparative Example 2 The color particle dispersion 2 and the color particle dispersion 6 were mixed in a mass ratio of 75:25 to obtain a water-based coating material 9 (light blue light-blocking color particles: gray light-blocking color particles=75:25 (mass ratio)). The water-based coating material 9 was applied to the same substrate as in Example 1 at a coating amount of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating obtained in Comparative Example 2 had gray grains scattered across the base color (light blue), but was not sufficient in terms of ratings of 2 (sense of depth) or 3 (sharpness of grain pattern).

[0075] Comparative Example 3 The color particle dispersion 1, the color particle dispersion 2, and the color particle dispersion 6 were mixed in a mass ratio of 60:15:25 to obtain a water-based coating material 10 (light blue light-blocking color particles: gray light-blocking color particles=75:25 (mass ratio)). The water-based coating material 10 was applied to the same substrate as in Example 1 at a coating amount of 0.3 kg / m 2 After drying for 48 hours, the appearance of the coating was observed and evaluated in the same manner as in Example 1. The coating obtained in Comparative Example 3 had gray grains scattered across the base color (light blue), but was insufficient in terms of evaluations of 2 (sense of depth) and 3 (sharpness of grain pattern).

[0076] [Table 1]

Claims

[Claim 1] An aqueous coating material in which liquid or gel-like color particles are dispersed in an aqueous medium, The above color particles are A light-shielding color particle (A) containing a color pigment; A light-transmitting color particle (a) containing a color pigment and having the same color as the light-blocking color particle; and Color particles (B) of a different color from the light-shielding color particles An aqueous coating material comprising:

Citation Information

Patent Citations

  • Folding method of jacket for magnetic disk

    JP1986080678A

  • Decoration of construction material

    JP1991186381A

  • JP1992077440U