Solid electrolyte particle

Solid electrolyte particles with tailored Li, Ge, and P compositions and a core-shell structure address the oxidation resistance issue in sulfide electrolytes, maintaining high ionic conductivity and stability in all-solid-state batteries.

JP2024169928AActive Publication Date: 2024-12-06TOYOTA JIDOSHA KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023086797
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Sulfide solid electrolytes used in all-solid-state batteries suffer from low oxidation resistance, leading to the formation of polysulfides that reduce ionic conductivity and accelerate performance deterioration.

Method used

Solid electrolyte particles composed of Li, Ge, and P, with specific peak height ratios and crystallinity adjustments in X-ray diffraction and Raman spectra, and a core-shell structure with an LGPS type crystal phase core and amorphous phase shell, enhancing oxidation resistance while maintaining high ionic conductivity.

Benefits of technology

The proposed configuration achieves improved oxidation resistance and ionic conductivity, ensuring stable battery performance by balancing crystallinity and impurity phase presence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169928000001_ABST
    Figure 2024169928000001_ABST
Patent Text Reader

Abstract

To improve oxidation resistance.SOLUTION: A solid electrolyte particle includes Li, Ge, P, and S. The solid electrolyte particle satisfies relationships of 0.20≤IB / IA≤0.35 and 0.30≤IC / IA≤0.45. IA, IB, and IC each indicate a peak height in an X-ray diffraction spectrum measured using a CuKα ray as an X-ray source. IA indicates a peak height at a diffraction angle of 29.4±0.5°. IB indicates a peak height at a diffraction angle of 41.4±0.5°. IC indicates a peak height at a diffraction angle of 47.3±0.5°.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to solid electrolyte particles. [Background technology]

[0002] WO 2017 / 155119 discloses a sulfide solid electrolyte. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2017 / 155119 Summary of the Invention [Problem to be solved by the invention]

[0004] Solid electrolytes are the key materials for all-solid-state batteries. Conventionally, sulfide solid electrolytes containing Li, P, and S have been developed. -3 Sulfide solid electrolytes can have high ionic conductivity on the order of S / cm. However, sulfide solid electrolytes tend to have low oxidation resistance. When sulfide solid electrolytes undergo oxidative decomposition, polysulfides can form. The formation of polysulfides can reduce ionic conductivity.

[0005] The positive electrode has a high potential. In the positive electrode, the sulfide solid electrolyte may be oxidized and decomposed, for example, to form a resistive layer (polysulfide) at the interface between the positive electrode active material and the sulfide solid electrolyte. -10 The formation of a resistive layer may accelerate the degradation of the performance of the solid-state battery.

[0006] An objective of the present disclosure is to improve oxidation resistance. [Means for solving the problem]

[0007] 1. A solid electrolyte particle according to one aspect of the present disclosure has the following composition: The solid electrolyte particle contains Li, Ge, P, and S. The solid electrolyte particle satisfies the relationship of the following formula (1) and formula (2). 0.20≦I B / I A ≦0.35 …(1) 0.30≦I C / I A ≦0.45 …(2) In the above formula (1) and formula (2), I A , I B and I C Each indicates the peak height in the X-ray diffraction spectrum measured using CuKα radiation as the X-ray source. A indicates the peak height at a diffraction angle of 29.4±0.5°. B indicates the peak height at a diffraction angle of 41.4±0.5°. C indicates the peak height at a diffraction angle of 47.3±0.5°.

[0008] In the X-ray diffraction (XRD) spectrum of the solid electrolyte particles, the peaks appearing at diffraction angles (2θ) of 29.4±0.5°, 41.4±0.5°, and 47.3±0.5° are considered to belong to the LGPS-type crystal phase. The LGPS-type crystal phase can have high ionic conductivity. B / I A , I C / I A ) is an index of crystallinity. B / I A , I C / I A ) indicates lower crystallinity. According to the new findings of the present disclosure, an improvement in oxidation resistance is expected due to a moderately low crystallinity. However, if the crystallinity is excessively reduced, the oxidation resistance may actually decrease. In other words, when the relationship of the above formula (1) and formula (2) is satisfied, an improvement in oxidation resistance is expected.

[0009] 2. The solid electrolyte particle according to the above item "1" may have the following configuration: In an X-ray diffraction spectrum, a peak at a diffraction angle of 29.4±0.5° has a full width at half maximum of 0.15° or less.

[0010] When the peak at a diffraction angle of 29.4±0.5° has a full width at half maximum (FWHM) of 0.15° or less, both high ionic conductivity and oxidation resistance are expected.

[0011] 3. The solid electrolyte particles according to the above item "1" or "2" may have the following configuration: The solid electrolyte particles further satisfy the relationship of the following formula (3). 1.2≦I E / I D …(3) In the above formula (3), I D and I E and I respectively indicate the peak height in the Raman spectrum. D is 420±10cm -1 The peak heights at the Raman shifts of I E is 360±10cm -1 The Raman spectrum shows the peak height at 388±3 cm -1 It has a shoulder peak at the Raman shift of

[0012] In the Raman spectrum of solid electrolyte particles, 388±3 cm -1 The shoulder peak that appears in the Raman shift of Li 2 This is thought to be due to impurity phases such as S. The impurity phase is thought to be generated by oxidative decomposition of the LGPS-type crystal phase. In other words, the impurity phase is a cause of reduced crystallinity. When the solid electrolyte particles satisfy the relationship of formula (3) above, it is thought that the crystallinity in the bulk is maintained. By locally introducing the impurity phase while maintaining the bulk crystallinity, it is expected that both high ionic conductivity and oxidation resistance can be achieved.

[0013] 4. The solid electrolyte particle according to any one of the above items "1" to "3" may have the following configuration. The solid electrolyte particle includes a core portion and a shell portion. The shell portion covers the periphery of the core portion. The core portion includes an LGPS-type crystalline phase. The shell portion includes an amorphous phase. The core portion has a size of 10×10 -3 The shell has an ionic conductivity of 1×10 S / cm or more. -3 It has an ionic conductivity of less than S / cm.

[0014] For example, the crystallinity may be locally decreased at the outermost surface of the particle. The solid electrolyte particle may have, for example, a core-shell structure. The LGPS type crystal phase has a tendency to have high ionic conductivity and low oxidation resistance. The amorphous phase has a tendency to have low ionic conductivity and high oxidation resistance. By including the LGPS type crystal phase in the core portion and the amorphous phase in the shell portion (outermost surface), it is expected that both high ionic conductivity and oxidation resistance can be achieved.

[0015] 5. The solid electrolyte particle described in "4" above may include, for example, the following configuration: The shell portion has a thickness of 100 nm or less.

[0016] By making the shell (amorphous phase) 100 nm thick, it is expected that both high ionic conductivity and oxidation resistance can be achieved.

[0017] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the present embodiment do not limit the technical scope of the present disclosure. The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are non-restrictive. The technical scope of the present disclosure encompasses all modifications within the meaning and scope equivalent to the description of the claims. For example, it is originally intended that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is an example of an XRD spectrum. [Diagram 2] FIG. 2 is an example of a Raman spectrum. [Diagram 3] FIG. 3 is an example of a cyclic voltammogram. [Figure 4] FIG. 4 is a conceptual diagram of the core-shell structure. [Diagram 5] FIG. 5 is a schematic flow chart of a method for producing solid electrolyte particles in this embodiment. [Figure 6] FIG. 6 is a table showing the experimental results. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] <Terminology explanation> The "XRD spectrum" is measured by a powder XRD method. The measurement conditions are as follows. However, the measurement device is an example, and an equivalent device may be used. Measuring device: Product name "RINT-2000", manufactured by Rigaku Corporation X-ray source: Cu-Kα ray Angle range: 2θ=10~60°

[0020] Peak height ratio (I B / I A , I C / I A ) is determined by the following procedure. The background is removed from the raw data of the XRD spectrum. After the background is removed, the XRD spectrum is normalized by setting the height of the peak appearing at a diffraction angle of 29.4 ± 0.5° as "1". In the normalized XRD spectrum, the peak height at a diffraction angle of 41.4 ± 0.5° is determined as the peak height ratio (I B / I A Similarly, in the normalized XRD spectrum, the peak height at a diffraction angle of 47.3 ± 0.5° is considered to be the peak height ratio (I C / I A) Note that, for example, if multiple peaks exist within a range of 29.4±0.5°, the height of the highest peak is measured. Furthermore, the FWHM of the peak at a diffraction angle of 29.4±0.5° is measured.

[0021] The "Raman spectrum" is measured by Raman spectroscopy. The measurement conditions are as follows. However, the measurement device is an example, and an equivalent device may be used. Measuring device: Product name "LabRAM HR", manufactured by Horiba, Ltd. Laser wavelength: 532nm Grating: 1200 Wave number range: 200~2000cm -1

[0022] Peak height ratio (I E / I D ) is determined by the following procedure: 460~500cm -1 The average Raman intensity in the range of 420±10cm is taken as the reference intensity. -1 The difference between the peak top Raman intensity and the reference intensity in the Raman shift of D ) is considered to be 360±10cm -1 The difference between the peak top Raman intensity and the reference intensity in the Raman shift of E ) is considered as the peak height (I E ) is the peak height (I D ) to obtain the peak height ratio (I E / I D ) is obtained.

[0023] "LGPS-type crystal phase" refers to a crystal phase having a LGPS-type structure. The LGPS-type structure includes a three-dimensional skeleton. The three-dimensional skeleton includes a plurality of one-dimensional chains. Each one-dimensional chain is made up of (Ge 0.5 P 0.5 )S 4 Tetrahedron and LiS 6 The two adjacent linear chains are connected one-dimensionally, sharing edges. 4They are connected through tetrahedra. In the LGPS type structure, P atoms can occupy the 4d site and the 2b site. The 4d site constitutes a one-dimensional chain. The 2b site constitutes a linking part that connects the one-dimensional chains together. The 4d site can be occupied by Ge atoms and P atoms. In the 4d site, the molar ratio is "Ge / P=1 / 1". The 2b site can be occupied only by P atoms. The XRD spectrum of the LGPS type crystal phase has peaks at diffraction angles (2θ) of 29.4±0.5°, 41.4±0.5°, and 47.3±0.5°.

[0024] Numerical ranges such as "m to n%" include the upper and lower limits unless otherwise specified. In other words, "m to n%" indicates a numerical range of "m% or more and n% or less." "m% or more and n% or less" includes "more than m% but less than n%."

[0025] The terms "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended terms. Open-ended terms may or may not further include additional elements in addition to the required elements. The term "consisting of" is a closed term. However, even closed terms do not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The term "consisting essentially of..." is a semi-closed term. Semi-closed terms allow for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.

[0026] Elements expressed in the singular form include the plural form unless otherwise specified. For example, "particle" includes not only "one particle" but also "multiple particles (particle group)" and "aggregate of particles (powder)."

[0027] The stoichiometric formulas are representative of the compounds. The compounds may have non-stoichiometric compositions. For example, "Al 2 O 3 " is not limited to a compound having a substance amount ratio (molar ratio) of "Al / O=2 / 3". 2 O 3" indicates a compound containing Al and O in any substance amount ratio, unless otherwise specified. Furthermore, for example, the compound may be doped with a trace element. A part of Al and O may be substituted with another element.

[0028] <Solid electrolyte particles> The solid electrolyte particles are Li-ion conductors. The solid electrolyte particles may be, for example, for an all-solid-state battery. The solid electrolyte particles may be, for example, for a positive electrode, a negative electrode, or a separator. The D50 of the solid electrolyte particles may be, for example, any of 0.01 to 10 μm, 0.01 to 1 μm, or 0.1 to 1 μm. "D50" refers to the particle size at which the cumulative distribution becomes 50% in the volume-based particle size distribution (cumulative distribution). The particle size distribution can be measured by a laser diffraction method.

[0029] The solid electrolyte particles contain, as chemical components, Li (lithium), Ge (germanium), P (phosphorus) and S (sulfur). The solid electrolyte particles may have, for example, a bulk composition of the following formula (4): Li 10+x Ge 1+x P 2-x S 12 (0≦x≦0.7) …(4) In the above formula (4), x may be, for example, any one of 0.5 or less, 0.3 or less, or 0.1 or less.

[0030] <XRDスペクトル> FIG. 1 is an example of an XRD spectrum. Solid electrolyte particles have a specific XRD spectrum. The peak height ratio (I B / I A ) is 0.20 to 0.35. In this range, improvement in oxidation resistance is expected. B / I A ) may be, for example, 0.31 or less. B / I A ) may be, for example, 0.29 or more.

[0031] Peak height ratio (I C / I A) is 0.30 to 0.45. In this range, improvement in oxidation resistance is expected. C / I A ) may be, for example, 0.44 or less or 0.43 or less. C / I A ) may be, for example, 0.42 or more or 0.43 or more.

[0032] The FWHM at the peak at a diffraction angle of 29.4±0.5° may be, for example, 0.15° or less. The FWHM may be, for example, 0.14° or less. The FWHM may be, for example, 0.13° or more.

[0033] <Raman spectrum> FIG. 2 is an example of a Raman spectrum. The solid electrolyte particles may have a specific Raman spectrum. The Raman spectrum has a peak at 388±3 cm -1 The shoulder peak may be due to an impurity phase (Li 2 The presence of a moderate amount of impurity phase is expected to improve oxidation resistance.

[0034] Peak height ratio (I E / I D ) may be, for example, 1.2 or more. E / I D When the peak height ratio (I E / I D ) may be, for example, 1.30 or more or 1.35 or more. E / I D ) may be, for example, 1.40 or less or 1.35 or less.

[0035] <Cyclic voltammetry> FIG. 3 is an example of a cyclic voltammogram. Oxidation resistance can be evaluated by cyclic voltammetry (CV). It is considered that the smaller the maximum value of the oxidation current (hereinafter also referred to as "maximum current") in the cyclic voltammogram (current-potential curve), the better the oxidation resistance. The solid electrolyte particles may have a maximum current of, for example, 20 μA or less. The maximum current may be, for example, either 11 μA or less, or 7 μA or less. The maximum current may be, for example, any of 1 μA or more, 3 μA or more, or 7 μA or more.

[0036] The cyclic voltammogram may have a peak (maximum value) on the oxidation side. The cyclic voltammogram may not have a peak on the oxidation side. When there is no peak on the oxidation side, improvement in oxidation resistance is expected.

[0037] The CV is measured by a half cell. The half cell includes a working electrode and a counter electrode. The counter electrode is Li metal. The working electrode is prepared by the following procedure. A sample (solid electrolyte particles) is compressed to form a first pellet (green compact). A mixture is prepared by mixing the sample with vapor grown carbon fiber (VGCF). The mixture ratio is "sample / VGCF = 1 / 1 (volume ratio)". The first pellet is used as a base material, and the mixture is compressed on the base material to form a second pellet. The working electrode is a laminate of the first pellet and the second pellet. The second pellet is pressed onto the first pellet. It is considered that the working electrode contains a conductive material (VGCF) so that an oxidation reaction that may occur in an actual electrode can be observed.

[0038] The conditions for measuring CV are as follows. However, the measuring device is only an example, and an equivalent device may be used. Measurement device: Product name "VMP3", manufactured by BioLogic Sweep speed: 0.1mV / s Sweep potential range: 2.5 to 4.8 V (vs. Li / Li + )

[0039] <AC impedance> The solid electrolyte particles can have high ionic conductivity. For example, the solid electrolyte particles can have a density of 3.0×10 -3 The ionic conductivity may be, for example, 4.5×10 S / cm or more. -3 S / cm or more, or 5.0×10 -3 The ionic conductivity may be, for example, 5.5×10 S / cm or more. -3 S / cm or less, or 5.0×10 -3 S / cm or less is acceptable.

[0040] The ionic conductivity is measured by an AC impedance method. Solid electrolyte particles (powder) are compressed to produce a pellet. The pellet is sandwiched between non-activated electrodes to form a symmetric cell. The non-activated electrodes and the solid electrolyte particles have different carrier ions. The non-activated electrodes may include, for example, stainless steel. The ionic conductivity is measured in the symmetric cell. The measurement conditions are as follows. However, the measurement device is an example, and an equivalent device may be used. Measurement device: Product name "VMP3", manufactured by BioLogic Frequency range: 1MHz~0.1Hz Applied voltage: 10mV Measurement temperature: 25±1℃

[0041] The measured data is plotted on a complex plane to create a Cole-Cole plot. The resistance is calculated from the intersection of the curve with the real axis. The ionic conductivity is calculated using the following formula (5). σ = 1 / {(r × s) / t} … (5) σ: Ionic conductivity r: resistance s: area of ​​working electrode t: thickness of the working electrode

[0042] <Core-shell structure> 4 is a conceptual diagram of a core-shell structure. The solid electrolyte particle 10 may have, for example, a core-shell structure. That is, the solid electrolyte particle 10 may include a core portion 11 and a shell portion 12.

[0043] The core portion 11 includes a highly ion-conductive phase. The core portion 11 may include, for example, an LGPS-type crystal phase. The core portion 11 may include, for example, a 10×10 -3 The ion conductivity of the core portion 11 may be, for example, 15×10 -3 S / cm or more, or 20×10 -3 The ionic conductivity of the core portion 11 may be, for example, 20×10 -3 S / cm or less, or 15×10 -3 S / cm or less. Core portion 11 may have a Feret diameter of, for example, 0.1 to 1 μm. The "Feret diameter" refers to the distance between the two most distant points on the contour line of core portion 11 in a cross-sectional image of solid electrolyte particle 10.

[0044] The shell portion 12 covers the periphery of the core portion 11. The shell portion 12 may cover the entire core portion 11. The shell portion 12 may cover a part of the core portion 11. The shell portion 12 includes a low ion conductive phase. The shell portion 12 may have oxidation resistance. The shell portion 12 may have, for example, lower crystallinity than the core portion 11. The shell portion 12 may include, for example, an amorphous phase. The shell portion 12 may have, for example, a crystallinity of 1×10 -3 The ionic conductivity of the shell portion 12 may be, for example, 0.5×10 S / cm or less. -3 S / cm or less, or 0.1×10 -3 The ionic conductivity of the shell portion 12 may be, for example, 0.1×10 S / cm or less. -3 S / cm or more, or 0.5×10 -3S / cm or more. Shell portion 12 may have a thickness of, for example, 100 nm or less. Shell portion 12 may have a thickness of, for example, 50 nm or less, or 10 nm or less. Shell portion 12 may have a thickness of, for example, 1 nm or more, 10 nm or more, or 50 nm or more.

[0045] <Method of manufacturing solid electrolyte particles> 5 is a schematic flow chart of a method for producing solid electrolyte particles in this embodiment. Hereinafter, the "method for producing solid electrolyte particles in this embodiment" may be abbreviated as "this production method." This production method includes "(a) synthesis of solid electrolyte particles" and "(b) surface treatment."

[0046] (a) Synthesis of solid electrolyte particles The method includes synthesizing solid electrolyte particles. The solid electrolyte particles may be synthesized, for example, by a solid-state reaction. The solid electrolyte particles may be synthesized, for example, by a mechanochemical reaction. The solid electrolyte particles are synthesized to include an LGPS-type crystal phase. For example, Li 2 S, P 2 S 5 and GeS 2 are mixed in a predetermined ratio to form a mixture. For example, the mixing may be performed using a planetary ball mill. The mixing may be performed under an Ar atmosphere. The mixture is subjected to a heat treatment (sintering) to synthesize solid electrolyte particles.

[0047] (b) Surface treatment The manufacturing method includes reducing the crystallinity of at least a portion of the surface of a solid electrolyte particle. For example, a damaged layer may be formed by applying mechanical energy to the surface of the particle. The damaged layer has low crystallinity with respect to the base material. The damaged layer may form the shell portion 12 of the core-shell structure. The base material excluding the damaged layer may form the core portion 11 of the core-shell structure.

[0048] For example, the solid electrolyte particles may be subjected to a wet milling process. For example, the solid electrolyte particles may be pulverized in the presence of a solvent by a planetary ball mill. The solvent may include at least one selected from the group consisting of butyl butyrate, heptane, and tetralin. After the wet milling process, the solvent may be removed by drying.

[0049] For example, ZrO 2 Metal media (grinding balls) may be used. The rotation speed of the planetary ball mill may be, for example, 200 to 250 rpm. The treatment time may be, for example, 1 hour or more. The treatment time may be, for example, 24 hours or less. EXAMPLES

[0050] <Sample> 6 is a table showing the experimental results. Solid electrolyte particles No. 1 to No. 6 were produced by the following procedure.

[0051] No.1 3.902 parts by mass Li 2 S, 3.775 parts by weight P 2 S 5 1.2 parts by mass of GeS and 2.323 parts by mass of GeS were mixed in a mortar until the mixture was approximately uniform, to prepare a first mixture. 2 , volume: 500 mL), and the first media (material: ZrO 2 A first pot (diameter: 5 mm) was prepared. 450 parts by mass of the first media and the first mixture were charged into the first pot. Dry milling was carried out at a rotation speed of 300 rpm for 20 hours. Thus, a second mixture was prepared. The second mixture was formed into pellets. The pellets were sealed in quartz tubes. The quartz tubes were carbon-coated. The pellets were subjected to heat treatment. The heat treatment temperature was 600° C. and the heat treatment time was 6 hours. Thus, a solid electrolyte was synthesized. After the heat treatment, the pellets were pulverized, and solid electrolyte particles were collected.

[0052] The second pot for the planetary ball mill (material: ZrO 2 , volume: 45mL), second media (material: ZrO 2 , diameter: 1 mm), and the third media (material: ZrO 2 A second pot (diameter: 0.1 mm) was prepared. 10 parts by mass of the second media, 40 parts by mass of the third media, 0.75 parts by mass of the solid electrolyte particles, and 6 parts by mass of butyl butyrate (solvent) were placed in the second pot. Wet milling was carried out at a rotation speed of 200 rpm for 1 hour. After the wet milling, the solvent was removed by a drying operation.

[0053] No.2~No.6 As shown in the "Wet Milling" section of Figure 6, solid electrolyte particles were produced in the same manner as in No. 1, except that the rotation speed in the wet milling was changed. Note that No. 3 was not subjected to the wet milling process. No. 3 is the base material (unprocessed product).

[0054] <Evaluation> FIG. 1 shows the XRD spectra of samples No. 1 to No. 6. All samples have peaks at 2θ=29.4±0.5°, 41.4±0.5°, and 47.3±0.5°. The higher the rotation speed of the wet milling process, the higher the peak height ratio (I B / I A ), (I C / I A ) tends to be smaller. This is thought to be because the wet milling process reduces crystallinity.

[0055] FIG. 2 shows the Raman spectra of No. 1 and No. 3 to No. 5. In No. 1, the peak intensity was 388±3 cm. -1 A shoulder peak was clearly observed in the Raman shift of the impurity phase (Li 2 The impurity phase is believed to be generated by slight decomposition of the LGPS-type crystal phase during the wet milling process.

[0056] Between each sample, the peak height ratio (IE / I D ) is small. From this result, it is considered that the bulk crystallinity (symmetry of the LGPS structure) is hardly changed by the wet milling treatment. It is considered that the crystallinity is locally decreased at the outermost surface of the particles in the wet milling treatment.

[0057] Figure 3 shows the cyclic voltammograms of No. 1 to No. 6. There is a tendency for the oxidation current peak to become smaller as the rotation speed in the wet milling process increases (No. 1 to No. 6). It is believed that the wet milling process imparts oxidation resistance to the particle surface. However, when the rotation speed in the wet milling process exceeds 250 rpm, the oxidation current increases again (No. 6). This is believed to be due to the destruction of the particles. The destruction of the particles leads to the formation of fine particles. It is believed that the oxidation reaction is promoted by the increase in the amount of interface between the fine particles and VGCF (conductive material).

[0058] FIG. 6 shows the ionic conductivity of No. 1 to No. 6. There is a tendency for the wet milling process to reduce the ionic conductivity. However, -3 High ionic conductivity on the order of S / cm is maintained.

[0059] From the above results, the peak height ratio (I B / I A ) is 0.20 to 0.35, and the peak height ratio (I C / I A ) is 0.30 to 0.45, improvement in oxidation resistance is expected.

[0060] <Additional Notes> In one aspect of the present disclosure, a method for producing solid electrolyte particles is provided. The method for producing solid electrolyte particles includes the following steps (a) and (b). (a) Synthesize solid electrolyte particles containing an LGPS-type crystal phase. (b) The solid electrolyte particles are subjected to a surface treatment. The surface treatment changes the LGPS type crystal phase into an amorphous phase in at least a portion of the surface of the solid electrolyte particle.

[0061] The above (b) may include subjecting the solid electrolyte particles to a wet milling treatment. The wet milling treatment may be performed using a planetary ball mill. The rotation speed of the planetary ball mill may be, for example, 200 to 250 rpm. The treatment time may be, for example, 1 hour or more. [Explanation of symbols]

[0062] 10 solid electrolyte particle, 11 core part, 12 shell part.

Claims

1. Contains Li, Ge, P and S, Formula (1) and Formula (2): 0.20≦I B / I A ≦0.35 …(1) 0.30≦I C / I A ≦0.45 …(2) Fulfilling the relationship, In the formula (1) and the formula (2), I A , I B and I C respectively indicate peak heights in an X-ray diffraction spectrum measured using CuKα radiation as an X-ray source, I A indicates the peak height at a diffraction angle of 29.4±0.5°, I B indicates a peak height at a diffraction angle of 41.4±0.5°, and I C indicates the peak height at a diffraction angle of 47.3±0.5°; Solid electrolyte particles.

2. In the X-ray diffraction spectrum, The peak at a diffraction angle of 29.4±0.5° has a full width at half maximum of 0.15° or less. The solid electrolyte particle according to claim 1 .

3. Formula (3): 1.20≦I E / I D …(3) Further satisfying the relationship In the formula (3), I D and I E indicate the peak heights in the Raman spectrum, I D is 420±10cm -1 and I E is 360±10cm -1 and The Raman spectrum is at 388±3 cm -1 A shoulder peak is present at the Raman shift of The solid electrolyte particle according to claim 1 or 2.

4. Contains a core portion and a shell portion, The shell portion covers the periphery of the core portion, The core portion contains an LGPS type crystal phase, The shell portion includes an amorphous phase, The core portion is 10×10 -3 S / cm or more of ionic conductivity, and The shell part is 1×10 -3 S / cm or less of ionic conductivity; The solid electrolyte particle according to claim 1 or 2.

5. The shell portion has a thickness of 100 nm or less. The solid electrolyte particle according to claim 4 .

Citation Information

Patent Citations

  • Sulfide solid electrolyte material and preparation method thereof

    CN105098228A

  • Sulfide solid electrolyte particle

    WO2018164224A1

  • Sulfide solid electrolyte and all-solid-state battery

    WO2020045633A1

  • Sulfide solid electrolyte

    WO2017155119A1