Glass material and magneto-optic element
A tailored glass material composition addresses thermal lens issues in magneto-optical devices by optimizing components to enhance light transmittance and stability, ensuring consistent beam diameter and improved processing quality.
Patent Information
- Application Number
- JP2023086982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
The increase in laser light output in magneto-optical devices leads to thermal lens effects, causing beam diameter changes and deteriorating processing quality due to varying power density.
A glass material composition comprising specific ranges of Tb2O3, B2O3, Al2O3, SiO2, P2O5, and optional additives like CeO2, FeO, and Fe2O3, optimized to reduce thermal lens effects by enhancing light transmittance and stabilizing vitrification.
The glass material effectively suppresses thermal lens effects, maintaining stable beam diameter and improving processing quality by minimizing heat generation and absorption, with high light transmittance and suitable Verdet constants for magneto-optical applications.
Smart Images

Figure 2024170045000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass material and a magneto-optical element. [Background technology]
[0002] Paramagnetic glass materials are known to exhibit the Faraday effect, which is a magneto-optical effect. The Faraday effect rotates linearly polarized light passing through a material placed in a magnetic field. Magneto-optical elements that utilize this effect (e.g., Faraday rotators) are used in magneto-optical devices such as optical isolators.
[0003] Known examples of paramagnetic glass materials include SiO2-B2O3-Al2O3-Tb2O3 (Patent Document 1) and P2O5-B2O3-Tb2O3 (Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 51-46524 [Patent Document 2] Special Publication No. 52-32881 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the output of laser light irradiated to magneto-optical devices has been increasing. When the output of laser light increases, the temperature of magneto-optical elements rises, and the laser beam diameter (beam diameter change) is likely to change due to the thermal lens effect. When such a beam diameter change occurs, the power density also changes, and when used for processing, for example, the processing quality deteriorates.
[0006] In view of the above, an object of the present invention is to provide a glass material and a magneto-optical element in which the thermal lens effect is reduced. [Means for solving the problem]
[0007] Various aspects of the glass material and magneto-optical element that solve the above problems will now be described.
[0008] The glass material of aspect 1 is characterized by containing, in mole percent, 10% to 58% Tb2O3, 51% to 89% B2O3 + Al2O3 + SiO2 + P2O, and 0.01 ppm to 100 ppm FeO + Fe2O3, and further containing, in terms of mole percent, more than 1% to 20% CeO2.
[0009] The glass material of embodiment 2, in embodiment 1, preferably contains, in mole percent, 30% to 70% B2O, 30% to 70% Al2O, 20% to 70% SiO, and 50% to 20% P2O.
[0010] The glass material of embodiment 3, in embodiment 1 or embodiment 2, preferably contains, in mol %, more than 12% and 40% B2O3, 1% to 20% Al2O3, 20% to 40% SiO, and 50% to 5% P2O.
[0011] The glass material of embodiment 4, in any one of embodiments 1 to 3, preferably contains, in mol %, less than 5% Pr2O3 and less than 5% Dy2O3.
[0012] The glass material of embodiment 5 is the same as any one of embodiments 1 to 4, except that the glass material has a Tb content relative to the total Tb content. 3+ It is preferable that the ratio is 55% or more.
[0013] The glass material of embodiment 6, in any one of embodiments 1 to 5, preferably has a light transmittance of 80% or more at a wavelength of 1064 nm.
[0014] The magneto-optical element of the seventh aspect is characterized in that the glass material of any one of the first to sixth aspects is used. Effect of the Invention
[0015] According to the present invention, it is possible to provide a glass material and a magneto-optical element with a reduced thermal lens effect. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of an apparatus for producing a glass material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The glass material of the present invention is characterized by containing, in mole percent, 10% to 58% Tb2O3, 51% to 89% B2O3+Al2O3+SiO2+P2O, and 0.01 ppm to 100 ppm FeO+Fe2O3, and further containing, in mole percent, more than 1% to 20% CeO2. Here, "further containing, in mole percent, more than 1% to 20% CeO2" means that, in mole percent, the total content of components other than CeO2 is 100%, and the CeO2 content is more than 1% to 20% (i.e., the total amount is, in mole percent, more than 101% to 120%).
[0018] The reasons for defining the glass composition as above and the content of each component are explained below. In the following explanation, "%" means "mol %" unless otherwise specified. In addition, in the following explanation, "visible to near-infrared wavelength range" is the wavelength range used for visible to near-infrared lasers, and means a wavelength range of 300 nm to 2000 nm, particularly 300 nm to 1100 nm, unless otherwise specified.
[0019] Tb2O3 is a component that increases the absolute value of the Verdet constant and enhances the Faraday effect. The content of Tb2O3 is preferably 10% to 58%. More specifically, the content of Tb2O3 is preferably 10% or more, 12% or more, 15% or more, 16% or more, 18% or more, 20% or more, 21% or more, 22% or more, 25% or more, and particularly preferably 26% or more, and is preferably 58% or less, 55% or less, 52% or less, 50% or less, 49% or less, 46% or less, 45% or less, 44% or less, 43% or less, 41% or less, and particularly preferably 40% or less. If the content of Tb2O3 is too low, it is difficult to obtain the above effects. If the content of Tb2O3 is too high, it is difficult to vitrify. In addition, the light transmittance of the glass material is easily reduced, and the beam diameter change due to the thermal lens effect is easily generated. Although Tb exists in the glass in a trivalent or tetravalent state, in the present invention, all of these are represented as Tb2O3.
[0020] Tb to total Tb 3+ The ratio of Tb to the total Tb is preferably 55% or more, 60% or more, 70% or more, 80% or more, and particularly preferably 90% or more. 4+ The ratio of Tb can be reduced. 4+ has absorption at wavelengths of 300 nm to 1100 nm, and the light transmittance of the glass material is likely to decrease. 3+ By setting the ratio of Tb to the above value, the absorption of laser light in the visible to near infrared wavelength range is suppressed, and heat generation in the glass material is easily suppressed. Therefore, the thermal lens effect is easily suppressed. 3+ The upper limit of the ratio may be, for example, 100% or less.
[0021] FeO and Fe2O3 are components that reduce the light transmittance in the visible to near infrared wavelength range and are prone to cause the thermal lens effect. 2+ ) has a broad absorption peak at a wavelength of about 1200 nm. Therefore, the glass material absorbs laser light in the visible to near infrared wavelength range, generating heat and easily causing a thermal lens effect. 3+) does not have the above absorption, so it can improve light transmittance. 3+ ) may be reduced to FeO during the melting process. Therefore, the glass material of the present invention preferably has a content of FeO+Fe2O3 (the total amount of FeO and Fe2O3) of 0.01 ppm to 100 ppm. More specifically, the content of FeO+Fe2O3 is preferably 0.01 ppm or more, 0.05 ppm or more, 0.1 ppm or more, 0.2 ppm or more, 0.3 ppm or more, 0.4 ppm or more, 0.5 ppm or more, and particularly preferably 1 ppm or more, and is preferably 100 ppm or less, 50 ppm or less, 30 ppm or less, 20 ppm or less, 15 ppm or less, 14 ppm or less, 13 ppm or less, 11 ppm or less, 10 ppm or less, 9 ppm or less, 8 ppm or less, and particularly preferably 5 ppm or less. If the content of FeO+Fe2O3 is too low, the manufacturing cost is likely to increase.
[0022] CeO2 is also a component that suppresses changes in beam diameter caused by the thermal lens effect. The content (addition amount) of CeO2 is preferably more than 1% to 20% in terms of mole percent. More specifically, the content (addition amount) of CeO2 is preferably more than 1%, 1.1% or more, 1.2% or more, 1.5% or more, particularly 2% or more, and is preferably 20% or less, 19% or less, 15% or less, particularly 10% or less. If the amount of CeO2 added is too small, it becomes difficult to obtain the above effects. If the amount of CeO2 added is too large, the light transmittance of the glass material is likely to decrease.
[0023] Thus, even if the glass material of the present invention contains FeO and Fe2O3, which tend to reduce light transmittance and cause a thermal lens effect, the glass material contains CeO2 as an essential component, which makes it possible to suppress a decrease in light transmittance of the glass material in the visible to near-infrared wavelength range and reduce laser light absorption. Thus, the glass material of the present invention can reduce the thermal lens effect.
[0024] B2O3, Al2O3, SiO2, and P2O5 are components that form a glass skeleton and expand the vitrification range to stabilize vitrification. The content of B2O3+Al2O3+SiO2+P2O5 (the total content of B2O3, Al2O3, SiO2, and P2O5) is preferably 1% to 89%. More specifically, the content of B2O3+Al2O3+SiO2+P2O5 is preferably 1% or more, 5% or more, 10% or more, 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, and particularly preferably 48% or more, and is preferably 89% or less, 85% or less, 80% or less, 75% or less, and particularly preferably 70% or less. If the content of B2O3+Al2O3+SiO2+P2O5 is too low, vitrification becomes difficult. If the content of B2O3+Al2O3+SiO2+P2O5 is too high, it becomes difficult to obtain a sufficient Faraday effect. The preferred ranges of each component are as follows:
[0025] The content of B2O3 is preferably 0% to 70%. More specifically, the content of B2O3 is preferably 0% or more, 1% or more, 5% or more, 10% or more, particularly preferably more than 12%, and is preferably 70% or less, 67% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, particularly preferably 40% or less.
[0026] The content of Al2O3 is preferably 0% to 70%. More specifically, the content of Al2O3 is preferably 0% or more, 1% or more, and particularly preferably 2% or more, and is preferably 70% or less, 67% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, and particularly preferably 20% or less.
[0027] The SiO2 content is preferably 0% to 70%. More specifically, the SiO2 content is preferably 0% or more, 1% or more, 5% or more, and particularly preferably 10% or more, and is preferably 70% or less, 67% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, and particularly preferably 40% or less.
[0028] The content of P2O5 is preferably 0% to 20%. More specifically, the content of P2O5 is preferably 0% or more, 1% or more, particularly preferably 2% or more, and is preferably 20% or less, 15% or less, 10% or less, particularly preferably 5% or less.
[0029] In addition to the above components, the glass material of the present invention may contain the following components.
[0030] GeO2 is a component that becomes a glass skeleton and widens the vitrification range to stabilize vitrification. The content of GeO2 is preferably 0% to 60%. More specifically, the content of GeO2 is preferably 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, and particularly preferably 35% or less. If the content of GeO2 is too high, it becomes difficult to obtain a sufficient Faraday effect. From the viewpoint of widening the vitrification range, the lower limit of the content of GeO2 may be, for example, 0% or more, particularly 1% or more.
[0031] ZnO is a component that stabilizes vitrification. The ZnO content is preferably 0% to 20%. More specifically, the ZnO content is preferably 20% or less, 15% or less, 13% or less, 10% or less, 8% or less, and particularly preferably 5% or less. If the ZnO content is too high, devitrification is likely to occur. In addition, it becomes difficult to obtain a sufficient Faraday effect. From the viewpoint of stabilizing vitrification, the ZnO content may be 0% or more, and particularly 1% or more.
[0032] La2O3, Gd2O3, Y2O3, and Yb2O3 are components that stabilize vitrification. The contents of La2O3, Gd2O3, Y2O3, and Yb2O3 are preferably 10% or less, 7% or less, 5% or less, 4% or less, and 2% or less, and particularly 1% or less, respectively. If the contents of these components are too high, vitrification becomes more difficult. The lower limits of the contents of La2O3, Gd2O3, Y2O3, and Yb2O3 may be, for example, 0% or more, and particularly 0.1% or more, respectively.
[0033] Pr2O3 and Dy2O3 have light absorption in the visible to near infrared wavelength range. Therefore, the contents of Pr2O3 and Dy2O3 are preferably less than 5%, 4% or less, 3% or less, 2% or less, 1% or less, 500 ppm or less, and particularly 100 ppm or less, respectively. If the contents of these components are too high, the light transmittance in the visible to near infrared wavelength range is likely to decrease. Note that Pr and Dy exist in the glass in a trivalent or tetravalent state, but in the present invention, these are represented as Pr2O3 or Dy2O3. The lower limit of the contents of Pr2O3 and Dy2O3 may be, for example, 0% or more, and particularly 0.001 ppm or more, respectively.
[0034] Eu2O3 and Sm2O3 have light absorption in the visible to near infrared wavelength range. Therefore, the contents of Eu2O3 and Sm2O3 are preferably less than 5%, 3% or less, 2% or less, 1% or less, 500 ppm or less, and particularly 100 ppm or less, respectively. If the contents of these components are too high, the light transmittance in the visible to near infrared wavelength range is likely to decrease. Note that Eu or Sm in the glass exists in a divalent or trivalent state, but in the present invention, these are represented as Eu2O3 or Sm2O3, respectively. The lower limit of the contents of Eu2O3 and Sm2O3 may be, for example, 0.001 ppm or more, respectively.
[0035] MgO, CaO, SrO and BaO are components that stabilize vitrification and easily increase chemical durability. The contents of MgO, CaO, SrO and BaO are each preferably 10% or less, particularly 5% or less. If the contents of these components are too high, it becomes difficult to obtain a sufficient Faraday effect. The lower limits of the contents of MgO, CaO, SrO and BaO may be, for example, 0% or more, particularly 1% or more.
[0036] Ga2O3 is a component that stabilizes vitrification and easily expands the vitrification range. The content of Ga2O3 is preferably 0% to 6%. More specifically, the content of Ga2O3 is preferably 6% or less, 5% or less, 4% or less, and particularly preferably 2% or less. If the content of Ga2O3 is too high, devitrification is likely to occur. In addition, it becomes difficult to obtain a sufficient Faraday effect. The lower limit of the content of Ga2O3 may be, for example, 0% or more, particularly 1% or more.
[0037] Fluorine is a component that enhances glass forming ability and easily widens the vitrification range. The fluorine content (F2 equivalent) is preferably 0% to 10%. More specifically, the fluorine content is preferably 10% or less, 7% or less, 5% or less, 3% or less, 2% or less, and particularly preferably 1% or less. If the fluorine content is too high, the components may volatilize during melting, adversely affecting vitrification. In addition, striae are likely to occur. The lower limit of the fluorine content may be, for example, 0% or more, and particularly 0.1% or more.
[0038] The glass material preferably has a light transmittance of 80% or more, 82% or more, particularly 83% or more at a wavelength of 1064 nm. At a wavelength of 633 nm, the light transmittance is preferably 60% or more, 65% or more, 70% or more, particularly 75% or more. At a wavelength of 532 nm, the light transmittance is preferably 30% or more, 50% or more, 60% or more, particularly 70% or more. High light transmittance in the above wavelength ranges suppresses heat generation in the magneto-optical element due to light absorption, and makes it easier to suppress changes in beam diameter due to the thermal lens effect. The above light transmittance is a value when the thickness of the glass material is 1 mm. At the above wavelengths, the upper limit of the light transmittance may be, for example, 100% or less, particularly 99% or less.
[0039] The glass material of the present invention, having the above-mentioned configuration, can increase light transmittance and suppress beam diameter change. For example, the beam diameter change rate can be suppressed to 30% or less, 25% or less, 20% or less, and particularly 15% or less. The beam diameter change rate can be measured, for example, as follows. First, a laser beam with a wavelength of 1064 nm and an output of 50 W is irradiated with a beam diameter of φ1 mm onto a glass sample processed to a thickness of 3 mm, and the size of the beam diameter at a position 300 mm from the sample is measured. The beam diameter is, for example, 1 / e 2 Next, the beam diameter change rate when the output is increased to 50 W can be calculated using the beam diameter at an output of 10 mW as the reference. Note that, if the beam diameter changes due to the thermal lens effect of the collimating lens even when there is no sample, the beam diameter change rate can be calculated by subtracting the beam diameter change rate when there is no sample from the measured beam diameter change rate.
[0040] The Verdet constant of the glass material of the present invention at a wavelength of 1064 nm is preferably 0.01 min / Oe·cm or more, and particularly preferably 0.02 min / Oe·cm or more. Glass materials having the above Verdet constant are suitable for use in magneto-optical elements. The upper limit of the Verdet constant at a wavelength of 1064 nm may be, for example, less than 0.5 min / Oe·cm, 0.4 min / Oe·cm or less, and particularly preferably 0.3 min / Oe·cm or less. The above Verdet constant refers to a value measured using a rotating analyzer method.
[0041] The glass material of the present invention can be suitably used for magneto-optical elements (for example, Faraday rotators) constituting magnetic devices such as optical isolators, optical circulators, and magnetic sensors.
[0042] The glass material of the present invention can be produced, for example, by a containerless levitation method. Fig. 1 is a schematic cross-sectional view showing one embodiment of an apparatus for producing the glass material of the present invention. Hereinafter, the method for producing the glass material of the present invention will be described with reference to Fig. 1.
[0043] The glass material manufacturing apparatus 1 has a molding die 10. The molding die 10 also serves as a melting container. The molding die 10 has a molding surface 10a and a plurality of gas outlets 10b opening on the molding surface 10a. The gas outlets 10b are connected to a gas supply mechanism 11 such as a gas cylinder. Gas is supplied from the gas supply mechanism 11 to the molding surface 10a via the gas outlets 10b. The type of gas is not particularly limited, and may be, for example, air or oxygen, or a reducing gas containing nitrogen gas, argon gas, helium gas, carbon monoxide gas, carbon dioxide gas, or hydrogen. Among these, it is preferable to use an inert gas from the viewpoint of suppressing oxidation of the glass material and safety.
[0044] The glass material can be manufactured using the glass material manufacturing apparatus 1 as follows. First, the glass raw material lump 12 is placed on the molding surface 10a. Examples of the glass raw material lump 12 include a raw material powder integrated by press molding or the like, a sintered body obtained by integrating raw material powder by press molding or the like and then sintering, and an aggregate of crystals having a composition equivalent to a target glass composition.
[0045] Next, the frit lump 12 is levitated on the forming surface 10a by ejecting gas from the gas ejection hole 10b. That is, the frit lump 12 is held in a state where it is not in contact with the forming surface 10a. In this state, the frit lump 12 is irradiated with laser light from the laser light irradiation device 13. As a result, the frit lump 12 is heated and melted to be vitrified to obtain molten glass. Then, the molten glass is cooled to obtain a glass material. At this time, the molten glass and the glass material are cooled until the temperature is at least below the softening point. In the process of heating and melting the frit lump 12 and the process of cooling the frit lump 12 until the temperature is at least below the softening point, it is preferable to continue ejecting at least gas and suppress the contact between the frit lump 12, the molten glass, and even the glass material and the forming surface 10a. The frit lump 12 may be levitated on the forming surface 10a by utilizing a magnetic force generated by applying a magnetic field. In addition to the method of irradiating laser light, the frit lump 12 may be heated and melted by radiation heating or the like.
[0046] The manufacturing method of the glass material of the present invention is not limited to the above-mentioned containerless levitation method. For example, the glass material of the present invention may be manufactured by crucible melting. In the case of crucible melting, a large amount of raw material powder can be melted at once, so that it is easy to obtain a large glass material. The large glass material can be suitably used for high power laser applications, etc. EXAMPLES
[0047] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0048] Tables 1 to 3 show Examples 1 to 17 of the present invention and Comparative Examples 1 and 2.
[0049] [Table 1]
[0050] [Table 2]
[0051] [Table 3]
[0052] Each sample was prepared as follows. First, raw materials were mixed to have the glass composition shown in Tables 1 to 3, and press-molded. The press-molded raw materials were sintered at 800° C. for 5 hours to prepare glass raw material blocks.
[0053] Next, the glass raw material lump was roughly crushed in a mortar to obtain small pieces of 1 g. Next, a glass material (diameter about 9 mm) was produced by a containerless levitation method using the small pieces of the glass raw material lump and an apparatus similar to that shown in Figure 1. A 100 W CO2 laser oscillator was used as a heat source. Nitrogen gas was used as the gas for levitating the glass raw material lump in the air, and the supply flow rate was 1 to 30 L / min. The obtained glass material was annealed in a 4%-H2 / N2 atmosphere at 770°C for 6 hours, and then the following measurements were performed. The results are shown in Tables 1 to 3. In Examples 1 to 17, when the total amount of all components including CeO2 is converted to 100 mol%, the glass material containing, in mol%, 12.6% to 51% Tb2O3, 47.1% to 71.4% B2O3+Al2O3+SiO2+P2O5, 1.1% to 16.7% CeO2, and 0.1 ppm to 4.9 ppm FeO+Fe2O3 was obtained. At this time, the contents of B2O3, Al2O3, SiO2, and P2O5 were 0% to 58.3% B2O3, 0% to 60.2% Al2O3, 0% to 61.8% SiO2, and 50% to 9.2% P2O, respectively.
[0054] The Verdet constant was measured using a rotating analyzer method. Specifically, the obtained glass material was polished to a thickness of 1 mm, and the Faraday rotation angle was measured in a wavelength range of 500 nm to 1100 nm in a magnetic field of 10 kOe, and the Verdet constant at a wavelength of 1064 nm was calculated.
[0055] The light transmittance was measured using a spectrophotometer (V-670 manufactured by JASCO Corporation). Specifically, the obtained glass material was polished to a thickness of 1 mm, and the light transmittance at a wavelength of 1064 nm was read from the light transmittance curve. The light transmittance is the external transmittance including reflection.
[0056] Tb to total Tb 3+ The ratio of Tb to total Tb was measured using XAFS. Specifically, the X-ray absorption near edge structure (XANES) spectrum was obtained, and the shift in the peak position of each Tb ion was used to calculate the ratio of Tb to total Tb. 3+ The ratio (mol %) of was calculated.
[0057] The rate of change in beam diameter was measured as follows. First, a laser beam with a wavelength of 1064 nm and an output of 50 W was irradiated onto a glass sample processed to a thickness of 3 mm with a beam diameter of φ1 mm, and the size of the beam diameter was measured at a position 300 mm from the sample. The beam diameter was 1 / e 2 Next, the beam diameter change rate was calculated when the output was set to 50 W, based on the beam diameter at an output of 10 mW. Note that even when there was no sample, changes in the beam diameter were observed due to the thermal lens effect of the collimator lens, so the beam diameter change rate was calculated by subtracting the amount of beam diameter change when there was no sample from the measured beam diameter change rate.
[0058] As shown in Tables 1 to 3, the glass materials of Examples 1 to 17 had absolute values of the Verdet constants of 0.027 to 0.215 at a wavelength of 1064 nm. Furthermore, the light transmittance was 82.2% or more at a wavelength of 1064 nm, and the beam diameter change rate was low, at 15% or less.
[0059] On the other hand, the glass materials of Comparative Examples 1 and 2 had a light transmittance of 79.5% or less and a beam diameter change rate of 33% or more. [Industrial Applicability]
[0060] The glass material of the present invention can be suitably used for magneto-optical elements (for example, Faraday rotators) constituting magnetic devices such as optical isolators, optical circulators, and magnetic sensors. [Explanation of symbols]
[0061] 1. Glass manufacturing equipment 10 mold 10a Molding surface 10b Gas vent 11 Gas supply mechanism 12 Glass raw material lump 13 Laser light irradiation device
Claims
1. In mole percent, Tb 2 O 3 10% to 58%, B 2 O 3 +Al 2 O 3 +SiO 2 +P 2 O 5 1% to 89%, FeO+Fe 2 O 3 Contains 0.01 ppm to 100 ppm, and further contains CeO 2 A glass material containing more than 1% to 20%.
2. In mole percent, B 2 O 3 0% to 70%, Al 2 O 3 0% to 70%, SiO 2 0% to 70%, P 2 O 5 The glass material according to claim 1, containing 0% to 20%.
3. In mole percent, B 2 O 3 More than 12% to 40%, Al 2 O 3 1% to 20%, SiO 2 0% to 40%, P 2 O 5 The glass material according to claim 1, containing 0% to 5%.
4. In mole percent, Pr 2 O 3 Less than 5%, Dy 2 O 3 The glass material according to any one of claims 1 to 3, containing less than 5%.
5. Tb to total Tb 3+ The glass material according to any one of claims 1 to 3, wherein the proportion of
6. 4. The glass material according to claim 1, which has a light transmittance of 80% or more at a wavelength of 1064 nm.
7. A magneto-optical element using the glass material according to any one of claims 1 to 3.
Citation Information
Patent Citations
Imonozunanoshiwakesochi
JP1976046524A
Continuous crystallization equipment
JP1977032881A