Conductive adhesive film, method for producing conductive adhesive film, connection body, and method for producing connection body

The conductive adhesive film with aggregated particles addresses inefficiencies in conventional ACFs by optimizing particle placement for reliable conductivity and reduced short circuits in high-density electrode connections.

JP2024170214APending Publication Date: 2024-12-06DEXERIALS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023087249
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional anisotropic conductive films (ACF) face inefficiencies in conductive particle utilization, leading to wasted particles and insufficient conductivity and reliability in connecting smaller electrodes, especially in high-density applications like camera modules, with issues of short circuits due to misaligned particles.

Method used

A conductive adhesive film with conductive particles aggregated into arrays, arranged in patterns matching electrode configurations, allowing efficient placement and reducing misalignment risks, thereby enhancing conductivity and preventing short circuits.

Benefits of technology

The solution ensures reliable conductivity and reduces short circuits by optimizing particle placement, improving connectivity and insulation between electrodes, even in fine-pitch applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170214000001_ABST
    Figure 2024170214000001_ABST
Patent Text Reader

Abstract

To provide a conductive adhesive film that enables efficient use of conductive particles, can respond to the miniaturization and fine-pitching of electrode sizes of electronic components, and can ensure the reliability of conduction between connecting electrodes and the insulation between adjacent electrodes.SOLUTION: A conductive adhesive film 1 has a substrate 2 and an adhesive layer 4 provided on one side of the substrate 2 and containing conductive particles 3. The conductive particles 3 contained in the adhesive layer 4 constitute particle agglomerate 5 formed by agglomerating a plurality of conductive particles, and in the adhesive layer 4, arrangement elements 6 made of the particle agglomerate 5 are arranged in a predetermined arrangement pattern corresponding to the electrode arrangement of an electronic component 10 to which the conductive adhesive film 1 is attached.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present technology relates to a conductive adhesive film and a method for manufacturing the same, a connection body in which electronic components are connected to each other using a conductive adhesive film, and a method for manufacturing the connection body. [Background technology]

[0002] BACKGROUND ART Conventionally, anisotropic conductive films (ACFs) have been known as connection films for connecting various electronic components and the like. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2020-198422 [Patent Document 2] Patent No. 6489516 Summary of the Invention [Problem to be solved by the invention]

[0004] In ACF, conductive particles are evenly dispersed throughout the adhesive layer, so only a portion of the conductive particles captured on the electrodes contribute to conductive connection. Other conductive particles besides those captured on the electrodes do not contribute to conductive connection, resulting in waste. Currently, particle-arrayed ACFs have been proposed, in which relatively large conductive particles with an average particle size of 15 to 20 μm are regularly arranged. However, as with dispersed ACFs, even in particle-arrayed ACFs, conductive particles other than those captured on the electrodes do not contribute to conductive connection, resulting in inefficient use of the conductive particles. It has also been proposed to process ACFs into the shape of the substrate or electrode arrangement pattern to which the ACF is to be attached (see, for example, Patent Document 1), but this inevitably results in conductive particles being located in positions other than on the electrodes.

[0005] Furthermore, as the electrode size of electronic components connected with anisotropic conductive film becomes smaller, the number of conductive particles that can be captured by the electrode also becomes smaller, and in some cases, conventional anisotropic conductive film is unable to provide sufficient conductivity reliability. On the other hand, product trends for ACF for camera modules (CCM), for example, require even higher pixel counts and higher transmission speeds, and anisotropic conductive film is also required to increase particle density to accommodate even finer pitches, arranging more conductive particles on the electrodes to improve conductivity reliability and prevent short circuits caused by conductive particles being present between adjacent electrodes.

[0006] Therefore, the present technology aims to provide a conductive adhesive film, a manufacturing method for a conductive adhesive film, a connector, and a manufacturing method for a connector that enable efficient use of conductive particles, can accommodate miniaturization and fine pitch of electrodes in electronic components, and can ensure reliable conductivity between connecting electrodes and insulation between adjacent electrodes. [Means for solving the problem]

[0007] In order to solve the above-mentioned problems, the conductive adhesive film of the present technology is a conductive adhesive film having a substrate and an adhesive layer containing conductive particles provided on one side of the substrate, wherein the conductive particles contained in the adhesive layer form particle aggregates formed by aggregating a plurality of the conductive particles, and the adhesive layer has array elements formed by the particle aggregates arranged in a predetermined array pattern corresponding to the electrode array of an electronic component to which the conductive adhesive film is attached.

[0008] In addition, a method for manufacturing a conductive adhesive film according to the present technology is a method for manufacturing a conductive adhesive film having a substrate and an adhesive layer containing conductive particles provided on one side of the substrate, and includes an arrangement step of arranging arrangement elements consisting of particle aggregates formed by aggregating a plurality of the conductive particles in the adhesive layer in a predetermined arrangement pattern corresponding to the electrode arrangement of an electronic component to which the conductive adhesive film is attached, and the arrangement step includes providing the conductive particles in the adhesive layer via a mask having predetermined openings.

[0009] In addition, the connection body according to the present technology is a connection body in which a first electronic component and a second electronic component are connected via a conductive adhesive film containing a plurality of conductive particles, wherein the conductive adhesive film has a substrate and an adhesive layer containing conductive particles and provided on one surface of the substrate, the conductive particles contained in the adhesive layer constitute particle aggregates formed by aggregating a plurality of the conductive particles, and the adhesive layer has array elements formed by the particle aggregates arranged in a predetermined array pattern corresponding to the electrode array of the first electronic component to which the conductive adhesive film is attached.

[0010] In addition, a method for manufacturing a connection body according to the present technology includes an arrangement step of attaching a conductive adhesive film containing a plurality of conductive particles onto a first electronic component, and a connection step of connecting the first electronic component and a second electronic component via the conductive adhesive film, wherein the conductive adhesive film has a base material and an adhesive layer containing conductive particles provided on one surface of the base material, the conductive particles contained in the adhesive layer constitute particle aggregates formed by aggregating a plurality of the conductive particles, and the adhesive layer has array elements formed by the particle aggregates arranged in a predetermined array pattern corresponding to the electrode array of the first electronic component to which the conductive adhesive film is attached, and in the arrangement step, the electrodes of the first electronic component and the array elements are aligned, and the conductive adhesive film is attached to the first electronic component. [Effects of the Invention]

[0011] According to this technology, because the elements of the conductive adhesive film are composed of aggregates of conductive particles, it is easier to form an array pattern than when handling the conductive particles individually. In addition, the elements can be arranged in a desired pattern in a specific part of the adhesive layer, reducing unnecessary conductive particles that do not contribute to conductivity and conductive particles between adjacent electrodes. This makes it possible to efficiently improve the conductivity between connecting electrodes even with a fine pitch and prevent short circuits between adjacent electrodes. [Brief explanation of the drawings]

[0012] [Figure 1] Figure 1(A) is a plan view showing a conductive adhesive film in which array elements are arranged in a predetermined array pattern, Figure 1(B) is a plan view showing conductive particle aggregates that make up the array elements, and Figure 1(C) is a plan view showing conductive particles that make up the conductive particle aggregates. [Figure 2] FIG. 2 is a cross-sectional view that schematically shows a state in which the array elements are aligned on the electrode array of the first electronic component and a conductive adhesive film is attached. [Figure 3] FIG. 3 is a plan view that schematically shows a state in which the array elements are aligned on the electrode array of the first electronic component and a conductive adhesive film is attached. [Figure 4] 4(A) and 4(B) are plan views showing a conductive adhesive film provided with individual pieces each consisting of a plurality of array elements. [Figure 5] Figure 5(A) is a plan view showing a conductive adhesive film in which array elements are arranged corresponding to the electrode array of the first electronic component shown in Figure 5(B), and Figure 5(B) is a plan view showing an electronic component in which first to third terminal rows are formed, in which terminals (electrodes) are arranged on each of the three sides of a rectangular attachment area. [Figure 6] Figure 6(A) is a plan view showing a conductive adhesive film in which an array element consisting of one particle aggregate is arranged on an adhesive layer in a predetermined array pattern corresponding to the electrode array of a first electronic component, and Figure 6(B) is a plan view showing a conductive adhesive film in which the adhesive layer is divided into individual pieces corresponding to the attachment area of ​​the first electronic component, and an array element consisting of one particle aggregate is arranged on each individual piece. [Figure 7] Figure 7(A) is a plan view showing a conductive adhesive film in which array elements consisting of two particle aggregates are arranged in an adhesive layer in a predetermined array pattern corresponding to the electrode array of a first electronic component, and Figure 7(B) is a plan view showing a conductive adhesive film in which the adhesive layer is divided into individual pieces corresponding to the attachment area of ​​the first electronic component, and each individual piece has an array element consisting of two particle aggregates arranged therein. [Figure 8]Fig. 8(A) is a plan view showing a conductive adhesive film in which array elements, each of which is formed by particle aggregates arranged in a hexagonal lattice pattern in an adhesive layer in a predetermined array pattern corresponding to the electrode array of a first electronic component. Fig. 8(B) is a plan view showing the arrangement of conductive particle aggregates constituting each array element of the conductive adhesive film shown in Fig. 8(A). Fig. 8(C) is a plan view showing each conductive particle aggregate constituting each array element. [Figure 9] Figure 9 shows a state in which the area of ​​the array element is made smaller than the area of ​​the electrode of the first electronic component, thereby preventing particle aggregates from spilling over between adjacent electrodes even when misalignment occurs between the array element and the electrode, where (A) is a cross-sectional view and (B) is a plan view. [Figure 10] Figure 10 is a diagram showing the state in which the array elements (conductive particle aggregates) of the conductive adhesive film shown in Figures 6(A) and (B) are arranged on an electrode, where (A) is a plan view showing the state in which the array elements (conductive particle aggregates) are arranged in the center of the width direction of the electrode without any misalignment, and (B) is a plan view showing the state in which the array elements (conductive particle aggregates) are misaligned in the width direction of the electrode due to a misalignment of the attachment position of the conductive adhesive film. [Figure 11] Figure 11 is a diagram showing the state in which the array elements (conductive particle aggregates) of the conductive adhesive film shown in Figures 7(A) and (B) are arranged on an electrode, where (A) is a plan view showing the state in which the array elements (two conductive particle aggregates) are arranged in the center of the electrode in the width direction without any misalignment, and (B) is a plan view showing the state in which the array elements (two conductive particle aggregates) are misaligned in the width direction of the electrode due to a misalignment in the attachment position of the conductive adhesive film. [Figure 12] FIG. 12 is a plan view showing a state in which misalignment occurs when the width W1 of an array element made of an aggregate of conductive particles with an average particle size of 20 μm is set to 200 μm, the same as the width W2 of the electrode. [Figure 13] FIG. 13 is a perspective view schematically showing a film roll. [Figure 14] FIG. 14 is a cross-sectional view that schematically shows an arrangement step in which conductive particles are printed on an adhesive layer supported on a substrate using a metal mask to arrange the arrangement elements. [Figure 15] FIG. 15 is a cross-sectional view that schematically illustrates an arrangement step in which conductive particles are printed on an adhesive layer supported on a substrate using a rotary screen to arrange the arrangement elements. [Figure 16] FIG. 16 is a cross-sectional view showing a placement step of placing a conductive adhesive film on the first electronic component. [Figure 17] FIG. 17 is a cross-sectional view showing a state in which the base material has been peeled off from the adhesive layer in the disposing step. [Figure 18] FIG. 18 is a cross-sectional view showing a connecting step of connecting a second electronic component to a first electronic component via an adhesive layer. [Figure 19] FIG. 19 is a cross-sectional view showing a connection body in which a first electronic component and a second electronic component are connected via an adhesive layer. [Figure 20] Figure 20(A) is an oblique view showing a camera module evaluation board, Figure 20(B) is an oblique view showing an anisotropic conductive film attached to the electrodes of the camera module evaluation board, Figure 20(C) is an oblique view showing an FPC placed on the camera module evaluation board with the anisotropic conductive film attached, Figure 20(D) is an oblique view showing the process of pressing the FPC from above with a crimping tool via silicone rubber, and Figure 20(E) is an oblique view showing a connection sample in which an FPC is connected to a camera module evaluation board with an anisotropic conductive film. DETAILED DESCRIPTION OF THE INVENTION

[0013] Hereinafter, a conductive adhesive film, a manufacturing method of a conductive adhesive film, a connection body, and a manufacturing method of a connection body to which the present technology is applied will be described in detail with reference to the drawings. It should be noted that the present technology is not limited to the following embodiments, and various modifications are possible within the scope of the present technology. Furthermore, the drawings are schematic, and the ratios of the dimensions may differ from the actual ones. Specific dimensions should be determined with reference to the following explanation. It should be noted that the drawings also include parts in which the dimensional relationships and ratios differ from one another.

[0014] [Conductive adhesive film] Figure 1(A) is a plan view showing a conductive adhesive film 1 in which array elements 6 are arranged in a predetermined array pattern, Figure 1(B) is a plan view showing conductive particle aggregates 5 that constitute the array elements 6, and Figure 1(C) is a plan view showing conductive particles 3 that constitute the conductive particle aggregates 5.

[0015] The conductive adhesive film 1 to which this technology is applied comprises a substrate 2 and an adhesive layer 4 provided on one side of the substrate 2 and containing conductive particles 3, wherein the conductive particles 3 contained in the adhesive layer 4 form particle aggregates 5 formed by aggregating a plurality of conductive particles 3, and the adhesive layer 4 has array elements 6 formed from the particle aggregates 5 arranged in a predetermined array pattern corresponding to the electrode array of the first electronic component 10 to which the conductive adhesive film 1 is attached.

[0016] The conductive adhesive film 1 has an adhesive layer 4 continuously provided in the longitudinal direction of the substrate 2, and array elements 6 made of particle aggregates 5 arranged in the adhesive layer 4 in a predetermined array pattern corresponding to the electrode array of the first electronic component 10. The conductive adhesive film 1 is then attached to the first electronic component 10 by aligning the electrodes 11 of the first electronic component 10, which is the adherend, with the array elements 6. Thereafter, the electrodes 11 of the first electronic component 10 are aligned with the electrodes 13 of the second electronic component 12, and the first electronic component 10 and the second electronic component 12 are connected via the conductive adhesive film 1.

[0017] Fig. 2 is a cross-sectional view showing a state in which the array elements 6 are aligned with the electrode array of the first electronic component 10 and the conductive adhesive film 1 is attached. Fig. 3 is a plan view showing a state in which the array elements 6 are aligned with the electrode array of the first electronic component 10 and the conductive adhesive film 1 is attached. The array elements 6 of the conductive adhesive film 1 shown in Figs. 2 and 3 are formed by densely gathering conductive particle aggregates 5 in predetermined regions corresponding to the electrodes 11 of the first electronic component 10.

[0018] According to the conductive adhesive film 1 to which the present technology is applied, the arrangement pattern of the arrangement elements 6 made of particle aggregates 5 is designed to match the electrode design of the first electronic component 10 to which it is attached. In this case, since the arrangement elements 6 are made of aggregates of conductive particles 3, the arrangement pattern can be formed more easily than when the conductive particles 3 are handled individually.

[0019] Furthermore, by arranging the array elements 6 in a desired pattern in specific portions of the adhesive layer 4, the conductive particles 3 can be efficiently arranged on the electrodes 11 of the first electronic component 10, reducing or eliminating unnecessary conductive particles 3 that do not contribute to conductivity and conductive particles 3 between adjacent electrodes. Therefore, the conductive particles 3 can be efficiently utilized, and even when the electrodes 11, 13 of the first and second electronic components 11, 12 are finely pitched, the conductivity between the connecting electrodes of the electrodes 11 and 12 can be improved, and the risk of short circuits between adjacent electrodes can be reduced.

[0020] Furthermore, the conductive adhesive film 1 to which the present technology is applied can further reduce the minimum connection area between connecting electrodes in an anisotropic conductive connection. In other words, in the past, a relatively large electrode area was required to capture the conductive particles necessary to establish stable conduction in order to ensure conductivity between narrowed electrodes. However, the present technology ensures conductivity by concentrating the conductive particle aggregates 5 on the electrode 11, making it possible to establish stable conduction even with a narrowed electrode area. Therefore, the minimum connection area between connecting electrodes in an anisotropic conductive connection can be further reduced.

[0021] Furthermore, according to the conductive adhesive film 1 to which the present technology is applied, the density of the conductive particles 3 trapped between the connection electrodes can be increased by concentrating the conductive particle aggregates 5 on the electrodes 11. This makes it possible to reduce the conduction resistance between the connection electrodes compared to a dispersion-type conductive adhesive film in which the conductive particles are dispersed over the entire surface of the adhesive layer or an aligned-type conductive adhesive film in which the conductive particles are evenly distributed over the entire surface of the adhesive layer.

[0022] Furthermore, in this technology, the array elements 6 of the conductive adhesive film 1 are treated not in units of individual conductive particles but in units of aggregates 5 of conductive particles 3. Therefore, the conductive particle aggregates 5 constituting the array elements 6 do not need to be highly uniform with respect to the individual conductive particles 3. This increases the degree of freedom in the selection of the conductive particles 3. For example, metal particles with non-uniform particle diameters, such as solder particles, can also be used as the conductive particles 3. Furthermore, by treating the array elements 6 in units of conductive particle aggregates 5, it becomes easy to align and arrange the array elements 6 in accordance with the pattern of the electrodes 11 of the first electronic component 10, even if the diameters of the conductive particles 3 are non-uniform.

[0023] In addition, if an array pattern is formed by arranging conductive particles one by one in a predetermined position, as in the case of aligned anisotropic conductive films, it would be necessary to create a master on which an array pattern of individual conductive particles is formed for each electrode pattern, and difficult microfabrication would be required, which would increase manufacturing costs and make it difficult to flexibly accommodate connection electrode patterns. However, with the conductive adhesive film 1 to which this technology is applied, the array elements 6 are treated as aggregates 5 of conductive particles 3, so microfabrication to the extent that it would require the arrangement of individual conductive particles is not required, and array patterns that correspond to various connection electrode patterns can be flexibly formed, including from an economical standpoint.

[0024] [Individuation] The conductive adhesive film 1 may have the adhesive layer 4 continuously provided in the longitudinal direction of the substrate 2. Alternatively, as shown in FIGS. 4 and 5 , the adhesive layer 4, on which the array elements 6 are arranged according to the electrode pattern of the first electronic component 10, may be divided into individual pieces corresponding to the attachment areas of the first electronic component 10 to which the conductive adhesive film 1 is attached. The conductive adhesive film 1 shown in FIGS. 4 and 5 has individual pieces 8 corresponding to the attachment areas of the first electronic component 10 repeatedly provided in the longitudinal direction of the substrate 2. Each individual piece 8 has the array elements 6 arranged in a pattern according to the electrode pattern of the first electronic component 10. For each individual piece 8, the electrodes 11 of the first electronic component 10, which is the adherend, are aligned with the array elements 6, and the adhesive layer 4 is attached to the first electronic component 10.

[0025] 4(A) and 4(B) are plan views showing a conductive adhesive film 1 provided with pieces 8 each consisting of a plurality of array elements 6. In the conductive adhesive film 1 shown in Fig. 4(A) and 4(B), each piece 8 is attached with the array elements 6 aligned with the electrodes 11 of a first electronic component 10, which has one or more electrodes 11 spaced apart in its attachment area.

[0026] Fig. 5(A) is a plan view showing a conductive adhesive film 1 in which array elements 6 are arranged corresponding to the electrode array of a first electronic component 10 shown in Fig. 5(B). The first electronic component 10 shown in Fig. 5(B) has a first terminal row 21, a second terminal row 22, or a third terminal row 23 in which terminals (electrodes 11) are arranged on three sides of a rectangular attachment area. The conductive adhesive film 1 shown in Fig. 5(A) has array elements 6 arranged in each piece 8 corresponding to each terminal of the first to third terminal rows 21 to 23 formed in the attachment area of ​​each first electronic component 10, and the array elements 6 are aligned and attached to the terminals of the first electronic component 10.

[0027] 5(A) , the adhesive layer 4 is provided along three sides of the rectangular attachment area, rather than over the entire area, so that each piece 8 of the conductive adhesive film 1 has a generally U-shape that is open from the center of the attachment area to the one side where the terminal row is not formed. This prevents the center of the attachment area from being sealed with the adhesive layer 4, and also reduces the amount of adhesive layer 4 used. Furthermore, because the outer shape of the attachment area and the outer shape of the piece 8 match where necessary, excessive overflow of unnecessary resin after the pieces 8 are attached can be suppressed.

[0028] Array Element Furthermore, the array elements 6 constituting the array pattern may be formed by a plurality of closely packed particle aggregates 5, or may be formed by one or two particle aggregates 5. The conductive adhesive film 1 shown in FIG. 6(A) has array elements 6 each consisting of one particle aggregate 5 arranged on the adhesive layer 4 in a predetermined array pattern corresponding to the electrode array of the first electronic component 10. The conductive adhesive film 1 shown in FIG. 6(B) has the adhesive layer 4 separated into individual pieces 8 corresponding to the attachment areas of the first electronic component 10, and each individual piece 8 has an array element 6 each consisting of one particle aggregate 5 arranged thereon. The conductive adhesive films 1 shown in FIGS. 6(A) and 6(B) are aligned so that the particle aggregate 5 is located at the center of the electrode 11 in the width direction.

[0029] In the conductive adhesive film 1 shown in Figure 7(A), array elements 6 each consisting of two particle aggregates 5 are arranged in an adhesive layer 4 in a predetermined array pattern corresponding to the electrode array of a first electronic component 10. In the conductive adhesive film 1 shown in Figure 7(B), the adhesive layer 4 is separated into individual pieces 8 corresponding to the attachment areas of the first electronic component 10, and each individual piece 8 has an array element 6 each consisting of two particle aggregates 5 arranged therein. The conductive adhesive film 1 shown in Figures 7(A) and (B) is aligned so that the two particle aggregates 5 are located at the center of the electrode 11 in the width direction.

[0030] Furthermore, when the array elements 6 of the conductive adhesive film 1 are formed by a plurality of particle aggregates 5, the particle aggregates 5 may be regularly aligned. FIG. 8(A) is a plan view showing a conductive adhesive film 1 in which array elements 6 are arranged on the adhesive layer 4, each of which is formed by arranging particle aggregates 5 in a hexagonal lattice pattern in a predetermined array pattern corresponding to the electrode array of the first electronic component 10. FIG. 8(B) is a plan view showing the arrangement of the conductive particle aggregates 5 that constitute each array element 6 of the conductive adhesive film 1 shown in FIG. 8(A). FIG. 8(C) is a plan view showing each conductive particle aggregate 5 that constitutes each array element 6. In the conductive adhesive film 1 shown in FIG. 8, the adhesive layer 4 may also be divided into individual pieces corresponding to the attachment areas of the first electronic component 10. In addition to the configuration shown in FIG. 8(B), the conductive particle aggregates 5 that constitute the array elements 6 may also be aligned in the configurations shown in FIGS. 4(A) and (B) described above.

[0031] The area of ​​the array elements 6 may be equal to or smaller than the area of ​​the electrodes of the first electronic component 10. The array elements 6 are formed by filling or aligning conductive particle aggregates 5 in the adhesive layer 4 through openings 34 in a mask 33, which will be described later. That is, the maximum area and shape of the array elements 6 are determined by the area and shape of the openings 34 in the mask 33. For example, by opening the openings 34 in the same rectangular shape as the electrode 11 in correspondence with the rectangular electrode 11, array elements 6 having the same area and shape as the electrode 11 are formed. By making the openings 34 smaller than the electrode 11, array elements 6 having an area smaller than the electrode area are formed. Therefore, the area of ​​the array elements 6 refers to the maximum area determined by the openings 34 in the mask 33.

[0032] Furthermore, by making the area of ​​the array elements 6 equal to or smaller than the area of ​​the electrodes 11 of the first electronic component 10, it is possible to provide tolerance for misalignment between the array elements 6 and the electrodes. That is, when the conductive adhesive film 1 is attached to the attachment area of ​​the first electronic component 10, the electrodes 11 of the first electronic component 10 are aligned with the array elements 6, but if misalignment occurs, the conductive particle aggregates 5 that make up the array elements 6 may protrude into the space between adjacent electrodes, and depending on the amount of protrusion, this may cause a short circuit between the adjacent electrodes.

[0033] Therefore, by making the area of ​​array element 6 equal to or smaller than the area of ​​electrode 11 of first electronic component 10, even if misalignment occurs between array element 6 and electrode 11, it is possible to prevent conductive particle aggregates 5 from protruding into the space between adjacent electrodes or to limit the amount of protrusion, thereby reducing the risk of short-circuiting between adjacent electrodes. Furthermore, because array element 6 is made up of conductive particle aggregates 5, even if some conductive particle aggregates 5 protrude into the space between adjacent electrodes, conductive particle aggregates 5 located on electrode 11 can ensure sufficient conductivity between the connecting electrodes.

[0034] Figure 9 shows a state in which the area of ​​the array element 6 is made smaller than the area of ​​the electrode 11 of the first electronic component 10, thereby preventing particle aggregates 5 from spilling out between adjacent electrodes even when misalignment occurs between the array element 6 and the electrode 11, where (A) is a cross-sectional view and (B) is a plan view.

[0035] Figure 10 is a diagram showing the state in which the array elements 6 (conductive particle aggregates 5) of the conductive adhesive film 1 shown in Figures 6(A) and (B) are arranged on the electrode 11, where (A) is a plan view showing the state in which the array elements 6 (conductive particle aggregates 5) are arranged in the center of the width direction of the electrode 11 without any misalignment, and (B) is a plan view showing the state in which the array elements 6 (conductive particle aggregates 5) are misaligned in the width direction of the electrode 11 due to a misalignment of the attachment position of the conductive adhesive film 1.

[0036] Figure 11 is a diagram showing the state in which the array elements 6 (conductive particle aggregates 5) of the conductive adhesive film 1 shown in Figures 7(A) and (B) are arranged on the electrode 11, where (A) is a plan view showing the state in which the array elements 6 (two conductive particle aggregates 5) are arranged in the center of the width of the electrode 11 without any misalignment, and (B) is a plan view showing the state in which the array elements 6 (two conductive particle aggregates 5) are misaligned in the width direction of the electrode 11 due to a misalignment in the attachment position of the conductive adhesive film 1.

[0037] In both FIG. 10(B) and FIG. 11(B), the amount of particle aggregate 5 protruding into the gap between adjacent electrodes is suppressed, preventing short circuits between the adjacent electrodes.

[0038] Furthermore, assuming that the arrangement direction of the elements 6 in the arrangement pattern is the width direction of the elements 6 and that the arrangement direction of the electrodes 11 in the electrode arrangement of the first electronic component 10 is the width direction of the electrodes 11, it is preferable that the width W1 of the elements 6 be 40% to 100% of the width W2 of the electrodes 11. When the width W1 of the elements 6 is 100% of the width W2 of the electrodes 11, the width of the elements 6 is the same as the width of the electrodes 11. If the width W1 of the elements 6 is greater than 100%, even a slight misalignment poses a risk of causing a short circuit between adjacent electrodes. FIG. 12 is a plan view showing a state in which misalignment occurs when the width W1 of the elements 6, which are composed of aggregates 5 of conductive particles 3 with an average particle size of 20 μm, is 200 μm, the same as the width W2 of the electrodes 11. When the space S between adjacent electrodes is 200 μm, a slight misalignment (approximately 160 μm) is permitted to ensure conductivity between the connecting electrodes and prevent short circuits between the adjacent electrodes.

[0039] 6(A)(B) and 7(A)(B), the state in which the width W1 of the array elements 6 is 40% of the width W2 of the electrodes 11 corresponds to, for example, a case in which the particle size of the conductive particle aggregates 5 (the conductive particles 3 have an average particle size of 20 μm) is 80 μm and the width of the electrodes 11 of the first electronic component 10 is 200 μm. When the state in which the conductive particle aggregates 5 are arranged at the center of the electrode 11 in the width direction is an ideal state without misalignment (see FIGS. 10(A) and 11(A)), even if misalignment of about half the width of the electrode 11 (100 μm) occurs, part of the conductive particle aggregates 5 will be on the electrodes 11, ensuring conductivity between the connecting electrodes and preventing short circuits between adjacent electrodes.

[0040] [Conductive adhesive film] Hereinafter, each component of the conductive adhesive film 1 will be specifically described. As described above, the conductive adhesive film 1 has a substrate 2 and an adhesive layer 4 that is provided on one surface of the substrate 2 and contains conductive particles 3. The conductive particles 3 contained in the adhesive layer 4 constitute particle aggregates 5 formed by aggregating a plurality of conductive particles 3.

[0041] [Base material] The conductive adhesive film 1 is wound into a roll and provided as a film winding body 30. FIG. 13 is a perspective view schematically showing a film winding body. As shown in FIG. 13, the film winding body 30 is formed by winding the conductive adhesive film 1, which includes a tape-shaped substrate 2 and an adhesive layer 4 formed on the substrate 2, around a winding core 31. The winding core 31 has an axial hole into which a rotating shaft for rotating the reel is inserted, and one end of the conductive adhesive film 1 in the longitudinal direction is connected to the winding core 31 to wind the conductive adhesive film 1. The length of the conductive adhesive film 1 wound around the film winding body 30 is not particularly limited, but the lower limit of the length is 5 m or more, 10 m or more, or 50 m or more, and the upper limit of the length is preferably 5,000 m or less, 3,000 m or less, or 1,000 m or less.

[0042] The substrate 2 is a support film formed into a tape shape and supporting the adhesive layer 4. Examples of the substrate 2 include PET (Poly Ethylene Terephthalate), OPP (Oriented Polypropylene), PMP (Poly-4-methylpentene-1), and PTFE (Polytetrafluoroethylene). Preferably, the substrate 2 has at least the surface on the adhesive layer 4 side treated with a release agent such as a silicone resin.

[0043] The thickness of the substrate 2 is not particularly limited. The lower limit of the thickness of the substrate 2 is preferably 10 μm or more in order to separate it from the adhesive layer 4, more preferably 25 μm or more, and even more preferably 38 μm or more. The upper limit of the thickness of the substrate 2 is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 75 μm or less, because if the substrate 2 is too thick, there is a concern that excessive pressure will be applied to the adhesive layer 4. It may also be 50 μm or less.

[0044] The width of the substrate 2 is not particularly limited. The lower limit of the width of the substrate 2 is preferably 1 mm or more in consideration of winding, more preferably 2 mm or more, and even more preferably 4 mm or more. The upper limit of the width of the substrate may be 250 mm or less, preferably 120 mm or less, more preferably 60 mm or less, and even more preferably 10 mm or less, because if the width of the substrate is too large, it may be difficult to carry or handle. The width of the substrate 2 may be adjusted appropriately based on the arrangement pattern of the arrangement elements 6. From the viewpoint of productivity, it is preferable that the width of the substrate 2 and the width of the adhesive layer 4 are the same width, and that the ends in the width direction are aligned.

[0045] [Adhesive layer] The adhesive layer 4 supported on the substrate 2 is a connection film used for conductive connection between the first electronic component 10 and the second electronic component. The curing type of the adhesive layer 4 is not particularly limited, and examples include a thermosetting type, a photocuring type, and a photothermal and combined photocuring and thermal curing type. The adhesive layer 4 may also be a hot-melt type using a thermoplastic resin.

[0046] The following description will be given taking as an example an anisotropic conductive film containing aggregates 5 of conductive particles 3 in an insulating binder. The lower limit of the thickness of the anisotropic conductive film may be, for example, the same as the diameter of the conductive particles, and preferably 1.3 times or more the diameter of the conductive particles or 10 μm or more. The upper limit of the thickness of the anisotropic conductive film may be, for example, 40 μm or less or 2 times or less the diameter of the conductive particles. The anisotropic conductive film may also be laminated with insulating adhesive layers or pressure-sensitive adhesive layers that do not contain conductive particles 3, and the number of layers and lamination surface can be selected appropriately depending on the target and purpose. The insulating resin for the insulating adhesive layer or pressure-sensitive adhesive layer can be the same as that for the anisotropic conductive film. As described above, the conductive particle aggregates 5 may be dispersed or aligned in the resin. When the conductive particle aggregates 5 are dispersed in the resin, they may be in close contact or may be individually spaced apart without contacting each other.

[0047] Known insulating binders can be used as the insulating binder (insulating resin). Examples of curing types include heat-curing, photo-curing, and photo-thermal curing. Examples include photo-radical polymerization resin compositions containing a (meth)acrylate compound and a photo-radical polymerization initiator, thermal radical polymerization resin compositions containing a (meth)acrylate compound and a thermal radical polymerization initiator, thermal cationic polymerization resin compositions containing an epoxy compound and a thermal cationic polymerization initiator, and thermal anionic polymerization resin compositions containing an epoxy compound and a thermal anionic polymerization initiator. Known pressure-sensitive adhesive compositions may also be used. For hot-melt adhesives, the composition disclosed in JP 2014-060025 A can be used.

[0048] Hereinafter, a specific example will be described, taking as an example a thermal radical polymerization insulating binder containing a film-forming resin, an elastomer, a (meth)acrylic monomer, a polymerization initiator, and a silane coupling agent. Note that the term "(meth)acrylic monomer" means both an acrylic monomer and a methacrylic monomer.

[0049] The film-forming resin is not particularly limited, and examples thereof include phenoxy resin, unsaturated polyester resin, saturated polyester resin, urethane resin, butadiene resin, polyimide resin, polyamide resin, and polyolefin resin. The film-forming resin may be used alone or in combination of two or more. Among these, phenoxy resin is particularly preferred from the viewpoints of film-forming ability, processability, and connection reliability. The phenoxy resin is a resin synthesized from bisphenol A and epichlorohydrin, and an appropriately synthesized product or a commercially available product may be used. The content of the film-forming resin is not particularly limited, and is preferably, for example, 10% to 60% by mass.

[0050] The elastomer is not particularly limited, and examples thereof include polyurethane resin (polyurethane-based elastomer), acrylic rubber, silicone rubber, and butadiene rubber.

[0051] The (meth)acrylic monomer is not particularly limited and may be, for example, a monofunctional (meth)acrylic monomer or a polyfunctional (meth)acrylic monomer having two or more functionalities. From the viewpoint of stress relaxation of the polymer, it is preferable that 80 mass % or more of the (meth)acrylic monomers in the insulating binder are monofunctional (meth)acrylic monomers.

[0052] From the viewpoint of adhesiveness, the monofunctional (meth)acrylic monomer preferably has a carboxylic acid. The molecular weight of the monofunctional (meth)acrylic monomer having a carboxylic acid is preferably 100 to 500, more preferably 200 to 350. The content of the monofunctional (meth)acrylic monomer having a carboxylic acid in the insulating binder is preferably 3% by mass to 20% by mass, more preferably 5% by mass to 10% by mass.

[0053] The polymerization initiator is not particularly limited as long as it can cure the (meth)acrylic monomer at a predetermined temperature during thermocompression bonding, and examples thereof include organic peroxides. Examples of organic peroxides include lauroyl peroxide, butyl peroxide, benzyl peroxide, dilauroyl peroxide, dibutyl peroxide, peroxydicarbonate, and benzoyl peroxide. These may be used alone or in combination of two or more. The content of the polymerization initiator in the insulating binder is not particularly limited, and is preferably, for example, 0.5% to 15% by mass.

[0054] The silane coupling agent is not particularly limited, and examples thereof include epoxy-based silane coupling agents, acrylic-based silane coupling agents, thiol-based silane coupling agents, amine-based silane coupling agents, etc. The content of the silane coupling agent in the insulating binder is not particularly limited, and is preferably, for example, 0.1% by mass to 5.0% by mass.

[0055] [Conductive particles] The conductive particles 3 can be appropriately selected from those used in known anisotropic conductive films. Examples include metal particles such as nickel, copper, silver, gold, and palladium, and metal-coated resin particles in which the surface of resin particles such as polyamide and polybenzoguanamine is coated with a metal such as nickel. The surface may be insulated to the extent that it does not impair conductivity. The surface may also have protrusions. Furthermore, the conductive particles 3 may be particles such as solder particles that have good properties but large particle size variations. This is because the conductive adhesive film 1 according to the present technology treats the conductive particles 3 as conductive particle aggregates 5 rather than as individual particles. The particle size of the solder particles is not particularly limited, but type 5 (particle diameter 15 to 25 μm) is preferred. The type of solder particles is also not particularly limited, and various solder particles such as tin, tin-bismuth, tin-bismuth-copper, indium, and tin-indium can be used.

[0056] The particle diameter of the conductive particles 3 is not particularly limited, but the lower limit of the particle diameter is preferably 2 μm or more, and the upper limit of the particle diameter is preferably 50 μm or less, more preferably 20 μm or less, for example, from the viewpoint of the thickness of the adhesive layer 4. The particle diameter of the conductive particles 3 can be a value measured using an imaging particle size distribution analyzer (for example, FPIA-3000, manufactured by Malvern Instruments). The number of particles is preferably 1,000 or more, and more preferably 2,000 or more.

[0057] [Particle aggregates / array elements] A plurality of conductive particles 3 aggregate to form conductive particle aggregates 5. The conductive particle aggregates 5 can be formed by forming openings 34 having a diameter at least twice the average particle diameter of the conductive particles 3 in a mask 33 described below, and filling the adhesive layer 4 with the conductive particles 3 through the openings 34. For example, conductive particles 3 having a diameter of 20 μm are filled into openings 34 having a diameter of 80 μm to obtain conductive particle aggregates 5 having a diameter of 80 μm.

[0058] The aggregate diameter of the conductive particle aggregates 5 is not particularly limited, but the lower limit is preferably at least twice the particle diameter of the conductive particles 3. Furthermore, the upper limit of the aggregate diameter of the conductive particle aggregates 5 is preferably at most three times, more preferably at most four times, the diameter of the conductive particles 3 from the viewpoints of the capture efficiency of the conductive particle aggregates 5 in the connector and the insulation resistance between adjacent electrodes. For example, when the particle diameter is 2 μm, the lower limit of the aggregate diameter is preferably at least 4 μm, and the upper limit of the aggregate diameter is preferably at most 6 μm, more preferably at most 8 μm. When the particle diameter is 20 μm, the lower limit of the aggregate diameter is preferably at least 40 μm, and the upper limit of the aggregate diameter is preferably at most 60 μm, more preferably at most 80 μm. The aggregate diameter of the conductive particle aggregates 5 can also be measured in the same manner as the particle diameter of the conductive particles 3. The number of particles measured is preferably at least 5, more preferably at least 10.

[0059] As described above, one or more conductive particle aggregates 5 gather together to form an array element 6. The conductive particle aggregates 5 in each array element 6 may be densely packed, individually spaced apart, or aligned. The alignment pattern is not particularly limited and may be striped or lattice-like, with a hexagonal lattice being preferred.

[0060] The arrangement pattern of the arrangement elements 6 corresponds to the arrangement pattern of the electrodes 11 of the first electronic component 10, and they are arranged in the same direction and at the same pitch as the arrangement pattern of the electrodes 11. The arrangement elements 6 are aligned with the electrodes 11 of the first electronic component 10, so that a large number of conductive particle aggregates 5 are superimposed over the entire surface of the electrode 11, or one or more conductive particle aggregates 5 are dispersed or aligned within the electrode 11.

[0061] [Conductive adhesive film manufacturing process] Next, a manufacturing process for the conductive adhesive film 1 will be described. The manufacturing process for the conductive adhesive film 1 is a method for manufacturing a conductive adhesive film having a substrate 2 and an adhesive layer 4 that is provided on one surface of the substrate 2 and contains conductive particles 3, and includes an arrangement step of arranging arrangement elements 6, each consisting of particle aggregates 5 formed by aggregating a plurality of conductive particles 3, on the adhesive layer 4 in a predetermined arrangement pattern that corresponds to the electrode arrangement of the first electronic component 10 to which the conductive adhesive film 1 is attached. In the arrangement step, the arrangement elements 6 are provided by printing the conductive particles 3 on the adhesive layer 4 through a mask 33 that has predetermined openings 34.

[0062] The adhesive layer 4 can be provided on the substrate 2 by applying an adhesive resin composition such as the insulating binder described above onto the substrate 2 such as a PET film, and drying it at a predetermined temperature.

[0063] On the adhesive layer 4 supported on the substrate 2, array elements 6 made of conductive particle aggregates 5 are arranged in a predetermined array pattern. A known metal mask 33a can be used as the mask 33 used in this arraying step (see FIG. 14). By setting the opening diameter of the openings 34 of the mask 33 to 200% or more of the average particle diameter of the conductive particles 3, the conductive particles 3 can be filled into the adhesive layer 4 through the openings 34 to form the conductive particle aggregates 5. Furthermore, by using a rotary screen 33b as the mask 33, the array elements 6 can be formed continuously in the longitudinal direction of the adhesive layer 4 (see FIG. 15).

[0064] The processing of openings 34 for arranging conductive particle aggregates 5 can be performed easily and at low cost, and it is possible to prepare masks 33 corresponding to predetermined array patterns corresponding to the electrode arrays of various first electronic components 10. It is also easy to adjust the area of ​​array elements 6 in anticipation of misalignment with fine-pitch electrode patterns.

[0065] When dividing the adhesive layer 4 provided with the array elements 6 into individual pieces, the conductive adhesive film 1 is subjected to half-cutting, punching, punch press, or the like to form the predetermined individual pieces 8. Alternatively, only the adhesive layer 4 on the substrate 2 may be processed and removed. Furthermore, a step of providing a cover film on the adhesive layer 4 may be provided. Therefore, the above-mentioned processing may be performed on the substrate 2 and the adhesive layer 4 using the cover film as a support (substitute for the substrate 2). As described above, the substrate 2 is peeled (separated) from the adhesive layer 4 during use, and therefore the processing technology is highly difficult. The material of the cover film may be the same as that of the substrate 2 described above. It is preferable that the thickness of the cover film is thinner than that of the substrate 2.

[0066] [Connector] A connection body 40 to which the present technology is applied is formed by connecting a first electronic component 10 and a second electronic component 12 via a conductive adhesive film 1. In this specification, of the first and second electronic components 10 and 12 to be joined together, the electronic component to which the conductive adhesive film 1 is attached is referred to as the first electronic component 10.

[0067] [First electronic component / Second electronic component] The first electronic component 10 and the second electronic component 12 are not particularly limited and can be appropriately selected depending on the purpose. Examples of the first electronic component 10 include a ceramic substrate, a rigid substrate, a flexible substrate (FPC: Flexible Printed Circuits), a glass substrate, a plastic substrate, a resin multilayer substrate, an IC (Integrated Circuit) module, an IC chip, etc. Examples of the second electronic component 12 include a ceramic substrate, a rigid substrate, a flexible substrate (FPC: Flexible Printed Circuits), a glass substrate, a plastic substrate, a resin multilayer substrate, etc.

[0068] The connector and manufacturing method thereof according to the present technology can be used in any electronic device that uses electrical connections and in manufacturing methods thereof, such as semiconductor devices (including driver ICs as well as all devices that use semiconductors, such as optical elements, thermoelectric conversion elements, and photoelectric conversion elements), display devices (monitors, televisions, head-mounted displays, etc.), mobile devices (tablet devices, smartphones, wearable devices, etc.), game consoles, audio equipment, imaging devices (using image sensors such as camera modules), electrical mounting for vehicles (mobile devices), medical equipment, sensor devices (touch sensors, fingerprint authentication, iris authentication, etc.), and home appliances.

[0069] [Connector manufacturing process] The manufacturing process of the connector 40 includes an arrangement process of attaching the conductive adhesive film 1 onto the first electronic component 10, and a connection process of arranging the second electronic component 12 on the conductive adhesive film 1 and connecting the first electronic component 10 and the second electronic component 12 via the conductive adhesive film 1.

[0070] [Placement process] FIG. 16 is a cross-sectional view showing the placement step of placing the conductive adhesive film 1 on the first electronic component 10, and FIG. 17 is a cross-sectional view showing the state in which the substrate 2 has been peeled off from the adhesive layer 4 in the placement step. In the placement step, the electrodes 11 of the first electronic component 10 are aligned with the array elements 6, and the adhesive layer 4 of the conductive adhesive film 1 is attached to the first electronic component 10. For example, a bonding device is used to press the conductive adhesive film 1 from the substrate 2 side, and the adhesive layer 4 is attached to the mounting surface of the first electronic component 10 on the stage. When a plurality of adhesive layers 4 are provided on a single substrate, such as when the adhesive layers 4 are separated into individual pieces, the plurality of pieces 8 may be attached to the electronic component 10 all at once, or each individual piece 8 may be attached separately. The conductive adhesive film 1 to which the adhesive layer 4 has been transferred is then rolled up, leaving only the substrate 2.

[0071] [Connection process] Next, a second electronic component 12 is placed on the adhesive layer 4, and the first electronic component 10 and the second electronic component 12 are connected via the conductive adhesive film 1 (see FIG. 2). The second electronic component 12 has electrodes 13 arranged in a pattern corresponding to the arrangement pattern of the electrodes 11 of the first electronic component 10. In the connection step, the electrodes 13 of the second electronic component 12 are aligned with the electrodes 11 of the first electronic component 10, and the second electronic component 12 is mounted on the first electronic component 10 via the adhesive layer 4.

[0072] 18 is a cross-sectional view showing a connecting step of connecting a second electronic component 12 to a first electronic component 10 via an adhesive layer 4. As shown in Fig. 18, in the connecting step, for example, a crimping tool 42 is used to press against electrodes 11 of the first electronic component 10 and electrodes 13 of the second electronic component 12 via a buffer material 41. Depending on the curing type of the adhesive layer 4, heating, light irradiation, or the like is performed to cure the adhesive layer 4, thereby connecting the first electronic component 10 and the second electronic component 12.

[0073] Fig. 19 is a cross-sectional view showing a connection body 40 in which a first electronic component 10 and a second electronic component 12 are connected via a cured film 4a formed by curing an adhesive layer 4. As shown in Fig. 19, in the connection body 40, an electrode 11 of the first electronic component 10 and an electrode 13 of the second electronic component 12 are electrically connected via conductive particle aggregates 5 that constitute an array element 6, and there are no conductive particle aggregates 5 present between adjacent electrodes in amounts sufficient to cause a short circuit. [Example]

[0074] <First Example> Examples of the present technology are described below. In the first example, a connection was fabricated using an anisotropic conductive film as the adhesive layer of a conductive adhesive film, and the conduction characteristics (conduction resistance between connecting electrodes, insulation resistance between adjacent electrodes) were measured and evaluated when there was no misalignment between the anisotropic conductive film and the evaluation substrate and when there was misalignment.

[0075] [Creating a connector] 20, a camera module evaluation substrate 10 (ceramic substrate, width 6.0 mm, terminal row mounting surface width 1.0 mm, electrode width 200 μm, electrode length 500 μm, line:space ratio 1:1, terminal thickness 10 μm, Ni (undercoat) / Au (surface) plating, cavity structure, terminal rows on two opposing sides) was thermocompression bonded to an FPC 12 (polyimide film, 400 μm pitch, line:space ratio 1:1, terminal thickness 12 μm, Ni (undercoat) / Au (surface) plating) via an anisotropic conductive film 4 to produce a connector 40. Thermocompression bonding was performed by pressing a tool 42 from the FPC side through a 200 μm-thick silicone rubber 41 under conditions of a temperature of 130°C, a pressure of 1 MPa, and a time of 6 seconds.

[0076] Figure 20(A) is an oblique view showing an evaluation substrate 10, Figure 20(B) is an oblique view showing an anisotropic conductive film 4 attached to an electrode 11 of the evaluation substrate 10, Figure 20(C) is an oblique view showing an FPC 12 placed on the evaluation substrate 10 with the anisotropic conductive film 4 attached, Figure 20(D) is an oblique view showing the process of pressing the FPC 12 from above with a crimping tool 42 via silicone rubber 41, and Figure 20(E) is an oblique view showing a connection sample 40 in which the FPC 12 is connected to the evaluation substrate 10 with the anisotropic conductive film 4.

[0077] [Evaluation of conduction characteristics] Using a digital multimeter (Yokogawa Electric Corporation), the conduction resistance between the connecting electrodes of the connector and the insulation resistance between adjacent electrodes were measured when a current of 1 mA was passed using the four-terminal method. Measurements were performed on the connector immediately after connection and on the connector after a reliability evaluation test under conditions of a temperature of 121°C, humidity of 100%, and atmospheric pressure of 2 atm for 24 hours. The conduction resistance of 10 samples of the connector was measured (N=10), and the sample with the highest resistance value was used for evaluation.

[0078] Example 1 [Fabrication of anisotropic conductive film] Five parts by mass of resin-core conductive particles (Ni (undercoat) / Au (surface) plating, resin core) with an average particle size of 20 μm and 95 parts by mass of an insulating binder composed of the following components were prepared. The insulating binder was placed in a planetary mixer (product name: Awatori Rentaro, manufactured by THINKY Co., Ltd.) and stirred for 1 minute to prepare an adhesive composition. The adhesive composition was then applied to a 50 μm-thick PET film and dried in an oven at 80°C for 5 minutes to form an adhesive layer composed of the adhesive composition on the PET film, producing an insulating adhesive layer 6.0 mm wide and 25 μm thick. Conductive particles were densely arranged in this insulating adhesive layer using a metal mask with an opening pattern corresponding to the electrode pattern formed on the evaluation substrate 10, forming array elements composed of conductive particle aggregates with an average particle size of 80 μm. In Example 1, an anisotropic conductive film was used in which array elements 6 having the same shape as the electrodes 11 formed on the evaluation substrate 10 were arranged in accordance with the electrode pattern of the evaluation substrate 10.

[0079] The insulating binder was a mixed solution of ethyl acetate and toluene containing 47 parts by mass of phenoxy resin (trade name: YP-50, manufactured by Shin-Nichika Epoxy Manufacturing Co., Ltd.), 3 parts by mass of monofunctional monomer (trade name: M-5300, manufactured by Toagosei Co., Ltd.), 25 parts by mass of urethane resin (trade name: UR-1400, manufactured by Toyobo Co., Ltd.), 15 parts by mass of rubber component (trade name: SG80H, manufactured by Nagase ChemteX Corporation), 2 parts by mass of silane coupling agent (trade name: A-187, manufactured by Momentive Performance Materials Japan), and 3 parts by mass of organic peroxide (trade name: Nyper BW, manufactured by NOF Corporation) so that the solid content was 50% by mass.

[0080] <Example 2> In Example 2, an anisotropic conductive film was produced under the same conditions as in Example 1, except that, as shown in Figure 6(A), an arrangement element 6 was formed and arranged so that one conductive particle aggregate (average particle size 80 μm) was positioned at the center of the electrode width for an electrode 11 formed on an evaluation substrate 10.

[0081] Example 3 In Example 3, as shown in Figure 7(A), an anisotropic conductive film was produced under the same conditions as Example 1, except that an arrangement element 6 was formed and arranged so that two conductive particle aggregates (average particle size 80 μm) were arranged parallel to each other in the center of the electrode width and in the electrode length direction for an electrode 11 formed on an evaluation substrate 10.

[0082] <Comparative Example 1> In Comparative Example 1, 5 parts by mass of resin-core conductive particles (Ni (undercoat) / Au (surface) plating, resin core) with an average particle size of 20 μm and 95 parts by mass of an insulating binder consisting of the following components were added to a planetary mixer (product name: Awatori Rentaro, manufactured by THINKY Co., Ltd.) and stirred for 1 minute to prepare an anisotropic conductive adhesive composition. The anisotropic conductive adhesive composition was then applied to a 50 μm thick PET film and dried in an oven at 80°C for 5 minutes to form an adhesive layer made of the anisotropic conductive adhesive composition on the PET film, producing a dispersed anisotropic conductive film with a width of 6.0 mm and a thickness of 25 μm. The conductive particles had a particle density of 300 particles / mm 2 The insulating binder was the same as in Example 1.

[0083] <Comparative Example 2> In Comparative Example 2, a resin plate with recesses arranged in a hexagonal lattice pattern was prepared, and conductive particles (average particle size 20 μm) were filled into the recesses. The conductive particles were then transferred onto an insulating adhesive layer prepared in the same manner as in Example 1, thereby producing an aligned anisotropic conductive film with conductive particles arranged in a hexagonal lattice pattern over the entire surface. The conductive particles had a particle density of 600 particles / mm 2 The pixels are aligned so that:

[0084] <Comparative Example 3> In Comparative Example 3, an anisotropic conductive film was produced using a method similar to that of Example 1, in which aggregates of conductive particles with an average particle size of 20 μm (average particle size 80 μm) were arranged in a hexagonal lattice pattern over the entire surface of the insulating adhesive layer.

[0085] [Initial connection] First, the results of evaluation of the electrical conductivity characteristics at the initial stage of connection immediately after the connection body was fabricated will be described.

[0086] [Insulation resistance between adjacent electrodes (no misalignment)] [Table 1]

[0087] Table 1 shows the results of measuring whether or not short circuits occurred between adjacent electrodes when the spacing between adjacent electrodes was set to 20 μm, 40 μm, 90 μm, and 200 μm. There was no misalignment between the adjacent electrodes on the anisotropic conductive film and the evaluation substrate 10. 8 Ω or more: ○ (no short circuit), 10 8 Less than Ω was rated as × (short circuit).

[0088] As shown in Table 1, in the connections of Examples 1 to 3, the array elements could be arranged on the electrodes 11 of the evaluation substrate 10, and no short circuits occurred between adjacent electrodes, regardless of the width of the space between adjacent electrodes. On the other hand, in Comparative Example 1, in which the anisotropic conductive film was made of an anisotropic conductive adhesive composition in which conductive particles were dispersed over the entire surface, short circuits occurred when the space between adjacent electrodes was 40 μm or less. In Comparative Example 2, in which the anisotropic conductive film was made of conductive particles densely aligned over the entire surface of the adhesive layer, short circuits occurred when the space between adjacent electrodes was 20 μm, which is less than the particle diameter. Furthermore, in Comparative Example 3, in which conductive particle aggregates were aligned over the entire surface of the adhesive layer, short circuits occurred when the space between adjacent electrodes was 40 μm or less, which was smaller than the diameter of the conductive particle aggregates.

[0089] [Conductivity resistance between connecting electrodes] [Table 2]

[0090] Table 2 shows the results of measuring the conduction resistance between the connection electrodes in connections formed by misalignment between the electrodes of the anisotropic conductive film and the evaluation substrate. Conduction resistance of 50 mΩ or less was rated as ○○ (excellent), more than 50 mΩ but not exceeding 100 mΩ was rated as ○ (good), more than 100 mΩ but not exceeding 120 mΩ was rated as △ (fair), and more than 120 mΩ was rated × (poor). Note that in Comparative Examples 1 to 3, conductive particles or conductive particle aggregates are dispersed or aligned over the entire surface of the adhesive layer, eliminating the need to align the alignment elements with the electrodes of the evaluation substrate as in Examples 1 to 3, and therefore eliminating misalignment. Therefore, these comparative examples are intended as reference examples.

[0091] As shown in Table 2, in Example 1, when the array elements formed with a width of 200 μm were misaligned by up to 200 μm, the conductive particle aggregates were not captured, resulting in poor conductivity. In Example 2, when the array elements were misaligned by up to 100 μm from the center of the 200 μm-wide electrode in the width direction, only about half of the conductive particle aggregates were captured, resulting in high conductivity resistance. When the array elements were misaligned by up to 120 μm, the conductive particle aggregates were not captured, resulting in poor conductivity. In Example 3, the array elements were configured so that two conductive particle aggregates were arranged per electrode, ensuring conductivity up to a misalignment of 120 μm. However, when the array elements were misaligned by up to 140 μm, the conductive particle aggregates were not captured, resulting in poor conductivity.

[0092] [Insulation resistance between adjacent electrodes (with misalignment)] [Table 3]

[0093] Table 3 shows the results of measuring the insulation resistance between adjacent electrodes in a connection formed by causing misalignment between the electrodes of the anisotropic conductive film and the evaluation substrate. 8 Ω or more: ○ (no short circuit), 10 8A resistance of less than Ω was rated as × (short circuit occurred). Note that in Comparative Examples 1 to 3, since the conductive particles or conductive particle aggregates were dispersed or aligned over the entire surface of the adhesive layer, there was no need to align the positions of the array elements and the electrodes of the evaluation substrate as in Examples 1 to 3, and therefore no misalignment occurred, and therefore these are meant to be reference examples.

[0094] As shown in Table 3, in Example 1, when the array elements formed with a width of 200 μm were misaligned to 200 μm, the same as the space width between adjacent electrodes, a short circuit occurred. In Examples 2 and 3, no short circuit occurred even when the misalignment was up to 200 μm.

[0095] [Reliability test] Next, we will explain the evaluation results of the electrical conductivity of the connector after the reliability test. The reliability test was conducted under the conditions of a temperature of 121°C, humidity of 100%, and atmospheric pressure of 2 atm for 24 hours, and the electrical conductivity resistance between the connecting electrodes and the insulation resistance between adjacent electrodes in the connector were measured in the same manner as in the initial connection. The evaluation criteria were the same as in the initial connection.

[0096] [Insulation resistance between adjacent electrodes (no misalignment)] [Table 4]

[0097] Table 4 shows the results of measuring whether or not short circuits occurred between adjacent electrodes when the spacing between adjacent electrodes was set to 20 μm, 40 μm, 90 μm, and 200 μm. No misalignment occurred between the adjacent electrodes on the anisotropic conductive film and the evaluation substrate.

[0098] As shown in Table 4, in the connections of Examples 1 to 3, the array elements could be arranged on the electrodes of the evaluation substrate, and no short circuits occurred even after the reliability test, regardless of the width of the space between adjacent electrodes. On the other hand, in the connections of Comparative Examples 1 to 3, short circuits occurred, just as they did at the initial stage of connection. Furthermore, in Comparative Example 3, in which the conductive particle aggregates were aligned over the entire surface of the adhesive layer, short circuits occurred even when the space between adjacent electrodes was 90 μm, which was larger than the diameter of the conductive particle aggregates, and the insulation between the adjacent electrodes deteriorated after the reliability test.

[0099] [Conductivity resistance between connecting electrodes] [Table 5]

[0100] Table 5 shows the results of measuring the conduction resistance between connection electrodes in connections formed by misalignment between the electrodes of the anisotropic conductive film and the evaluation substrate. Note that in Table 5, Comparative Examples 1 to 3 are also meant as reference examples.

[0101] As shown in Table 5, in Example 1, as in the initial connection, when the array elements formed with a width of 200 μm were misaligned by less than 200 μm, the conductive particle aggregates were captured, but when the misalignment reached 200 μm, the conductive particle aggregates were not captured, resulting in poor electrical continuity. In Example 2, when the array elements were misaligned by less than 100 μm from the center of the 200 μm-wide electrode in the width direction, the conductive particle aggregates were captured, but when the misalignment reached 100 μm or more, the conductive particle aggregates were not captured, resulting in poor electrical continuity. In Example 3, when the array elements were misaligned by less than 120 μm, the conductive particle aggregates were not captured, resulting in poor electrical continuity.

[0102] [Insulation resistance between adjacent electrodes (with misalignment)] [Table 6]

[0103] Table 6 shows the results of measuring the insulation resistance between adjacent electrodes in connections formed by misaligning the electrodes of the anisotropic conductive film and the evaluation substrate. Note that, in Table 6, Comparative Examples 1 to 3 are also meant as reference examples.

[0104] As shown in Table 6, in Example 1, the array elements formed with a width of 200 μm did not short-circuit until the misalignment was 140 μm or less, but short-circuiting occurred when the misalignment reached 180 μm. In Examples 2 and 3, no short-circuiting occurred even when the misalignment reached 200 μm.

[0105] <Second Example> Next, a second example will be described. In the second example, anisotropic conductive films with different conductive particle content were fabricated, and a connection sample 40 was fabricated by connecting an FPC 12 to an evaluation substrate 10 using this anisotropic conductive film, and the conductivity performance (conduction resistance between connecting electrodes, insulation resistance between adjacent electrodes) was measured and evaluated. The evaluation substrate 10 and FPC 12 were the same as those in the first example.

[0106] The conduction resistance between the connection electrodes was measured at the initial stage of connection and after a reliability test. The reliability test conditions were the same as those in the first embodiment. The measurement method and evaluation criteria for the conduction resistance between the connection electrodes were also the same as those in the first embodiment. The insulation resistance between adjacent electrodes was measured to determine whether or not a short circuit occurred between adjacent electrodes when the spacing between the adjacent electrodes was set to 20 μm, 40 μm, and 80 μm. The measurement method and evaluation criteria for the insulation resistance between adjacent electrodes were also the same as those in the first embodiment.

[0107] Example 4 In Example 4, a connection sample 40 was produced in which an FPC 12 was connected to an evaluation substrate 10 using the same anisotropic conductive film as in Example 1 described above. There was no misalignment between the array elements 6 and the electrodes 11. The connection process was the same as in Example 1, except that the hot pressurization conditions of the tool were 130°C, 2 MPa, and 6 seconds.

[0108] <Example 5> In Example 5, connection body sample 40 was produced under the same conditions as in Example 4, except that solder particles with an average particle size of 20 μm were used as the conductive particles.

[0109] <Comparative Example 4> In Comparative Example 4, the particle density of the conductive particles was 150 particles / mm 2 A connection sample 40 was produced using the same anisotropic conductive film as in Comparative Example 1. The connection process was the same as in Example 1 except that the hot pressurization conditions for the tool were 130°C, 2 MPa, and 6 seconds.

[0110] <Comparative Example 5> In Comparative Example 5, a connection body sample 40 was produced using the same anisotropic conductive film as in Comparative Example 1. The connection process was the same as in Example 1 except that the hot pressurization conditions of the tool were 130°C, 2 MPa, and 6 seconds.

[0111] <Comparative Example 6> In Comparative Example 6, the particle density of the conductive particles was 600 particles / mm 2 Except for the blending so as to obtain the above, a connection body sample 40 was produced using the same anisotropic conductive film as in Comparative Example 1. The connection process was the same as in Example 1 except that the hot pressurization conditions of the tool were 130°C, 2 MPa, and 6 seconds.

[0112] <Comparative Example 7> In Comparative Example 7, a connection body sample 40 was produced using the same anisotropic conductive film as in Comparative Example 2. The connection process was the same as in Example 1 except that the hot pressurization conditions of the tool were 130°C, 2 MPa, and 6 seconds.

[0113] <Comparative Example 8> In Comparative Example 8, solder particles with an average particle size of 20 μm were used as conductive particles, and the particle density was 150 particles / mm 2 A connection sample 40 was produced using the same anisotropic conductive film as in Comparative Example 1. The connection process was the same as in Example 1 except that the hot pressurization conditions for the tool were 130°C, 2 MPa, and 6 seconds.

[0114] <Comparative Example 9> In Comparative Example 9, the particle density was 300 particles / mm 2 A connection sample 40 was produced using the same anisotropic conductive film as in Comparative Example 8. The connection process was the same as in Example 1 except that the hot pressurization conditions of the tool were 130°C, 2 MPa, and 6 seconds.

[0115] <Comparative Example 10> In Comparative Example 9, the particle density was 600 particles / mm 2 A connection sample 40 was produced using the same anisotropic conductive film as in Comparative Example 8. The connection process was the same as in Example 1 except that the hot pressurization conditions of the tool were 130°C, 2 MPa, and 6 seconds.

[0116] [Table 7]

[0117] As shown in Table 7, in Example 4, the array elements were formed with the same width as the electrode width, so the conduction resistance between the connection electrodes at the initial stage of connection was evaluated as ○ (good). However, after the reliability test, the conduction resistance between the connection electrodes was evaluated as △ (fair). This is a phenomenon caused by the repulsion of the resin core of the conductive particles. In Example 5, in which the array elements were formed with solder particles with the same width as the electrode width, the conduction resistance between the connection electrodes at the initial stage of connection and after the reliability test were both evaluated as ○○ (excellent). This shows that an anisotropic conductive film using solder particles as the conductive particles has excellent conductivity both at the initial stage of connection and after the reliability test.

[0118] On the other hand, in Comparative Examples 4 to 10, the evaluation of the electrical resistance between the connection electrodes at the initial stage of connection was ○○ (excellent), ○ (good), or △ (acceptable), but after the reliability test, it was × (poor) except for Comparative Examples 8 to 10, which used solder particles.

[0119] In addition, in Examples 4 and 5, the array elements could be arranged on the electrodes of the evaluation substrate, and the insulation resistance between adjacent electrodes was evaluated as ○ (no short circuit) regardless of the width of the space between adjacent electrodes.

[0120] On the other hand, in Comparative Examples 4 to 10, the evaluation of the insulation resistance between adjacent electrodes deteriorated as the space between adjacent electrodes narrowed, and when the space between adjacent electrodes was 20 μm, all samples were rated × (short circuit occurred).

[0121] <Third Example> Next, a third example will be described. In the third example, a connection sample 40 was fabricated by connecting an FPC 12 to an evaluation substrate 10 using the anisotropic conductive film used in the second example, and the conductivity performance (conduction resistance between connection electrodes, insulation resistance between adjacent electrodes) was measured and evaluated. The size of each electrode on the evaluation substrate 10 and FPC 12 was 150 μm wide and 100 μm long. In other words, the third example uses electrodes that are smaller in size than those used in the second example.

[0122] The conduction resistance between the connection electrodes was measured at the initial stage of connection and after a reliability test. The reliability test conditions were the same as those in the first embodiment. The measurement method and evaluation criteria for the conduction resistance between the connection electrodes were also the same as those in the first embodiment. The insulation resistance between adjacent electrodes was measured to determine whether or not a short circuit occurred between adjacent electrodes when the spacing between the adjacent electrodes was set to 20 μm, 40 μm, and 80 μm. The measurement method and evaluation criteria for the insulation resistance between adjacent electrodes were also the same as those in the first embodiment.

[0123] [Table 8]

[0124] As shown in Table 8, the evaluation of the conduction resistance between the connection electrodes at the initial connection time and after the reliability test for Examples 4 and 5 was the same as that for Example 2 (Table 7), and it can be seen that the conductive performance is stable even when the electrode size is further reduced.

[0125] On the other hand, in Comparative Examples 4 to 10, except for Comparative Examples 9 and 10, the evaluation of the conduction resistance between the connection electrodes at the initial stage of connection was △ (fair), and after the reliability test it was × (poor).

[0126] In addition, in Examples 4 and 5, the array elements could be arranged on the electrodes of the evaluation substrate, and the insulation resistance between adjacent electrodes was evaluated as ○ (no short circuit) regardless of the width of the space between adjacent electrodes.

[0127] On the other hand, in Comparative Examples 4 to 10, the evaluation of the insulation resistance between adjacent electrodes deteriorated as the space between adjacent electrodes narrowed, and when the space between adjacent electrodes was 20 μm, all samples were rated × (short circuit occurred). [Explanation of symbols]

[0128] REFERENCE SIGNS LIST 1 conductive adhesive film, 2 substrate, 3 conductive particles, 4 adhesive layer, 5 conductive particle aggregate, 6 array element, 8 piece, 10 first electronic component, 11 electrode, 12 second electronic component, 21 first terminal row, 22 second terminal row, 23 third terminal row, 30 film winding body, 31 winding core, 33 mask, 34 opening, 40 connecting body, 41 cushioning material, 42 crimping tool

Claims

1. A substrate; A conductive adhesive film having an adhesive layer containing conductive particles and provided on one surface of the substrate, the conductive particles contained in the adhesive layer constitute a particle aggregate formed by aggregating a plurality of the conductive particles, the adhesive layer has array elements made of the particle aggregates arranged in a predetermined array pattern corresponding to the electrode array of an electronic component to which the conductive adhesive film is attached; Conductive adhesive film.

2. The conductive adhesive film according to claim 1 , wherein the arrangement elements constituting the arrangement pattern are made up of one or more of the particle aggregates.

3. the array elements constituting the array pattern are each composed of a plurality of the particle aggregates, The conductive adhesive film according to claim 1 , wherein the arrangement elements are formed by assembling, dispersing or aligning a plurality of the particle aggregates.

4. 4. The conductive adhesive film according to claim 1, wherein the area of ​​the array elements is equal to or smaller than the area of ​​the electrodes that constitute the electrode array.

5. A conductive adhesive film according to any one of claims 1 to 3, wherein when the arrangement direction of the array elements in the array pattern is the width direction of the array elements, and the arrangement direction of the electrodes in the electrode array is the width direction of the electrodes, the width of the array elements is 40% or more and 100% or less of the width of the electrodes.

6. A method for producing a conductive adhesive film having a substrate and an adhesive layer containing conductive particles and provided on one surface of the substrate, comprising: an arrangement step of arranging, on the adhesive layer, arrangement elements each made of a particle aggregate formed by aggregating a plurality of the conductive particles in a predetermined arrangement pattern corresponding to an electrode arrangement of an electronic component to which the conductive adhesive film is attached; The arranging step includes providing the conductive particles on the adhesive layer through a mask having a predetermined opening. A method for producing a conductive adhesive film.

7. The method for producing a conductive adhesive film according to claim 6 , wherein the arranging step provides the conductive particles on the adhesive layer using a metal mask or a rotary screen as the mask.

8. 8. The method for producing a conductive adhesive film according to claim 6, wherein the opening diameter of the mask is 200% or more of the average particle diameter of the conductive particles.

9. A connection body in which a first electronic component and a second electronic component are connected via a cured film of an adhesive layer containing a plurality of conductive particles of a conductive adhesive film, The conductive adhesive film is A substrate; an adhesive layer provided on one surface of the base material and containing conductive particles; the conductive particles contained in the adhesive layer constitute a particle aggregate formed by aggregating a plurality of the conductive particles, the adhesive layer has array elements made of the particle aggregates arranged in a predetermined array pattern corresponding to the electrode array of the first electronic component to which the conductive adhesive film is attached; Connection body.

10. A placement step of attaching a conductive adhesive film containing a plurality of conductive particles onto a first electronic component; a connecting step of connecting the first electronic component and the second electronic component via the conductive adhesive film, The conductive adhesive film is The adhesive layer includes a substrate and an adhesive layer that is provided on one surface of the substrate and contains conductive particles. the conductive particles contained in the adhesive layer constitute a particle aggregate formed by aggregating a plurality of the conductive particles, the adhesive layer has array elements made of the particle aggregates arranged in a predetermined array pattern corresponding to an electrode array of the first electronic component to which the conductive adhesive film is attached, In the arranging step, the electrodes of the first electronic component and the array elements are aligned, and the conductive adhesive film is attached onto the first electronic component. A method for manufacturing a connector.

Citation Information

Patent Citations

  • spinner

    JP1989089516A

  • Method for producing connecting structure, connecting structure, film structure, and method for producing film structure