Polyvinyl acetal resin and resin composition for ceramic green sheet
A polyvinyl acetal resin with specified molecular weight and group content characteristics addresses the strength and stability issues in ceramic green sheets, enhancing the reliability and quality of multilayer ceramic capacitors by preventing delamination and dimensional changes.
Patent Information
- Application Number
- JP2023110834
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-07-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Conventional polyvinyl acetal resins used in ceramic green sheets for multilayer ceramic capacitors suffer from insufficient strength, leading to delamination and dimensional changes during the lamination and drying processes, which affect the quality and reliability of the final product.
A polyvinyl acetal resin with a Z average molecular weight (Mz) of 700,000 to 2,500,000 and a molecular weight differential distribution value at LogM=6.00 of 5.00 to 110.0, along with specific acetal, hydroxyl, and acetyl group contents, is used to enhance dispersibility, dispersion stability, and mechanical strength, preventing delamination and dimensional changes.
The resin composition results in ceramic green sheets with improved dispersibility, stability, and high strength, producing reliable multilayer ceramic capacitors with reduced defects.
Smart Images

Figure 2024170269000003 
Figure 2024170269000001 
Figure 2024170269000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyvinyl acetal resin and a resin composition for ceramic green. [Background technology]
[0002] 2. Description of the Related Art In recent years, electronic components mounted in various electronic devices have become smaller and more laminated, and laminated electronic components such as multilayer circuit boards, laminated coils, and laminated ceramic capacitors are widely used. Among them, multilayer ceramic capacitors are generally manufactured through the following steps. First, a plasticizer, a dispersant, etc. are added to a solution in which a binder resin such as polyvinyl butyral resin or poly(meth)acrylic acid ester resin is dissolved in an organic solvent, and then a ceramic raw material powder is added and mixed uniformly with a mixing device such as a bead mill or a ball mill to obtain a ceramic slurry composition having a certain viscosity after defoaming. This slurry composition is cast onto a support surface such as a release-treated polyethylene terephthalate film or a SUS plate using a doctor blade, reverse roll coater, etc., and the volatile matter such as the solvent is distilled off by heating, etc., and then peeled off from the support to obtain a ceramic green sheet. Next, a conductive paste that will become the internal electrodes is applied to the obtained ceramic green sheets by screen printing, and multiple sheets are alternately stacked and heated and pressed to produce a laminate. After that, a process to thermally decompose and remove the binder resin components and the like contained in the laminate, that is, a so-called degreasing process, is performed, and external electrodes are sintered onto the end faces of the ceramic sintered body obtained by firing to obtain a multilayer ceramic capacitor.
[0003] The resin composition for ceramic green sheets used for producing ceramic green sheets is generally used as a solution in which polyvinyl acetal resin is dissolved in an organic solvent such as methyl ethyl ketone, toluene, alcohol, or a mixture thereof. However, when conventional polyvinyl acetal resins are dissolved in an organic solvent, a small amount of undissolved matter is generated. When such undissolved matter is present, when the resin is used in a multilayer ceramic capacitor, voids tend to remain in the degreasing process and the firing process, and the dispersibility of ceramic powder and the like is reduced, resulting in a deterioration in the electrical properties of the resulting product. For this reason, when using polyvinyl acetal resin for ceramic green sheets, it was necessary to mix it with organic or inorganic compounds, dissolve it in an organic solvent, and then perform a filtration process to remove any undissolved materials.
[0004] In response to this, Patent Document 1 proposes a polyvinyl acetal resin in which a reduction rate of the filtration flow rate is less than 10% when a polyvinyl acetal resin solution, which is prepared by dissolving the polyvinyl acetal resin in a 1:1 mixed solvent of methyl ethyl ketone and / or toluene and ethanol to prepare a 5 wt % solution, is filtered using a filter with an opening of 5 μm under conditions of a filtration temperature of 25° C. and a filtration pressure of 10 mmHg. It is also proposed that the use of such a polyvinyl acetal resin results in less undissolved matter when dissolved in an organic solvent, and the filtration time can be shortened, thereby improving productivity. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-325342 A Summary of the Invention [Problem to be solved by the invention]
[0006] Meanwhile, in recent years, with the trend toward greater functionality and smaller size of electronic devices, multilayer ceramic capacitors are being demanded to have larger capacitance and smaller size, and ceramic green sheets are being demanded to be even thinner. However, when the polyvinyl acetal resin described in Patent Document 1 is used, there is a problem that the strength of the obtained ceramic green sheet is insufficient. In addition, delamination (peeling between layers) and dimensional changes may occur during the process of stacking and drying the ceramic green sheets. If delamination or dimensional changes occur as the ceramic green sheets become thinner, there is a problem that poor appearance occurs after cutting the laminate.
[0007] An object of the present invention is to provide a polyvinyl acetal resin and a resin composition for ceramic green sheets, which can provide ceramic green sheets that have excellent dispersibility and dispersion stability of ceramic powder, and are high in strength and are less susceptible to delamination or dimensional change during drying, and can be used to fabricate multilayer ceramic capacitors with excellent reliability. [Means for solving the problem]
[0008] The present disclosure (1) is a polyvinyl acetal resin having a Z-average molecular weight (Mz) of 700,000 or more and 2,500,000 or less, and a molecular weight differential distribution value at LogM = 6.00 of 5.00 or more and 110.0 or less. In the present disclosure (2), the amount of hydroxyl groups relative to the Z-average molecular weight (amount of hydroxyl groups / Z-average molecular weight) is 1.30×10 -5 The above is the polyvinyl acetal resin described in the present disclosure (1). The present disclosure (3) is the polyvinyl acetal resin according to the present disclosure (1) or (2), in which the amount of acetal groups is 50 to 83 mol %. The present disclosure (4) is a resin composition for a ceramic green sheet, comprising the polyvinyl acetal resin according to any one of the present disclosures (1) to (3) and a plasticizer. The present invention will be described in detail below.
[0009] As a result of extensive investigations, the present inventors have found that a polyvinyl acetal resin having a Z-average molecular weight and a molecular weight differential distribution value at LogM=6.00 within a predetermined range has excellent dispersibility and dispersion stability of ceramic powder, and can provide a ceramic green sheet which has high strength and is less susceptible to delamination or dimensional change during drying, and can fabricate a multilayer ceramic capacitor with excellent reliability, thereby completing the present invention.
[0010] The polyvinyl acetal resin of the present invention has a Z-average molecular weight (Mz) of 700,000 or more and 2,500,000 or less, and a molecular weight differential distribution value at LogM=6.00 of 5.00 or more and 110.0 or less. By containing such a polyvinyl acetal resin, it is possible to obtain a ceramic green sheet which has high strength and is less susceptible to delamination or dimensional change during drying.
[0011] The Z-average molecular weight (Mz) of the polyvinyl acetal resin of the present invention is from 700,000 to 2,500,000. By setting it within the above range, it is possible to improve the wettability with the ceramic powder and thereby improve the dispersion stability. The Mz is preferably 750,000 or more, more preferably 800,000 or more, and is preferably 2,400,000 or less, and more preferably 2,300,000 or less. That is, the Z-average molecular weight is 700,000 to 2,500,000, preferably 750,000 to 2,400,000, and more preferably 800,000 to 2,300,000. The Mz can be measured by gel permeation chromatography (GPC) using N-methylpyrrolidone as a solvent and an appropriate standard (eg, a polystyrene standard).
[0012] The molecular weight differential distribution value at LogM=6.00 of the polyvinyl acetal resin of the present invention is 5.00 or more and 110.0 or less. By setting it within the above range, it is possible to achieve a good balance between dispersibility and strength. The molecular weight differential distribution value at LogM=6.00 is preferably 7.00 or more, more preferably 8.00 or more, and is preferably 100.0 or less, more preferably 95.0 or less. That is, the molecular weight differential distribution value at LogM=6.00 is 5.00 to 110.0, preferably 7.00 to 100.0, more preferably 8.00 to 95.0.
[0013] In the present invention, the "molecular weight differential distribution value at LogM=6.00" refers to the differential distribution value when the logarithm logM of the molecular weight M is 6.00, and is the proportion of high molecular weight components. As an example of the molecular weight differential distribution value, a molecular weight differential distribution curve with LogM on the horizontal axis and molecular weight differential distribution value on the vertical axis is shown in Figure 1. In the present invention, when LogM is 6.00, the molecular weight differential distribution value is specified to be 5.00 or more and 110.0 or less. The molecular weight differential distribution value at LogM=6.00 can be measured by GPC (gel permeation chromatography).
[0014] The molecular weight differential distribution value at Mz and LogM = 6.00 can be adjusted, for example, by changing the average degree of polymerization and degree of saponification of the raw material polyvinyl alcohol resin, and the temperature and time conditions of the acetalization reaction, and by appropriately setting the amount of acetal groups, the amount of hydroxyl groups, the amount of acetyl groups, etc. of the polyvinyl acetal resin. In particular, the molecular weight differential distribution value at Mz, LogM = 6.00 can be adjusted by changing the holding temperature, holding time, temperature rise time, and temperature rise rate during the acetalization reaction described below.
[0015] The polyvinyl acetal resin of the present invention preferably has a structural unit having an acetal group represented by the following formula (1), a structural unit having a hydroxyl group represented by the following formula (2), and a structural unit having an acetyl group represented by the following formula (3).
[0016] [ka]
[0017] In the above formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.
[0018] In the above formula (1), R 1 When is an alkyl group having 1 to 20 carbon atoms, examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, an octadecyl group, etc. Among these, a methyl group and an n-propyl group are preferable.
[0019] In the polyvinyl acetal resin of the present invention, the content of the structural unit having the acetal group represented by the above formula (1) (hereinafter also referred to as the "acetal group amount") is preferably 50 mol % in lower limit and 83 mol % in upper limit. When the amount of acetal groups is 50 mol % or more, the solubility in organic solvents can be improved, and when the amount of acetal groups is 83 mol % or less, the polyvinyl acetal resin can have excellent tensile strength. The acetal group amount is more preferably 55 mol % in lower limit and 80 mol % in upper limit, that is, the acetal group amount is preferably 50 to 83 mol %, and more preferably 55 to 80 mol %. The amount of acetal groups is, for example, 1 It can be measured by H-NMR. Regarding the method for calculating the amount of acetal groups, since the acetal groups of polyvinyl acetal resin are obtained by acetalizing two hydroxyl groups of polyvinyl alcohol, the method of counting the two acetalized hydroxyl groups is used.
[0020] In the polyvinyl acetal resin of the present invention, the content of the structural unit having a hydroxyl group represented by the above general formula (2) (hereinafter also referred to as the "hydroxyl group amount") is preferably 18 mol % in lower limit and 40 mol % in upper limit. If the amount of hydroxyl groups is 18 mol % or more, the polyvinyl acetal resin can have high toughness, and if the amount of hydroxyl groups is 40 mol % or less, the solubility in organic solvents can be sufficiently improved. The lower limit of the hydroxyl group amount is more preferably 22 mol % and the upper limit is more preferably 38 mol %. That is, the hydroxyl group amount is preferably 18 to 40 mol %, and more preferably 22 to 38 mol %. The amount of hydroxyl groups is, for example, 1 It can be measured by H-NMR.
[0021] In the polyvinyl acetal resin of the present invention, the content of the structural unit having an acetyl group represented by the above general formula (3) (hereinafter also referred to as the "acetyl group amount") is preferably 0.1 mol % in lower limit and 22.0 mol % in upper limit. When the amount of acetyl groups is 0.1 mol% or more, the increase in viscosity of the slurry composition for ceramic green sheets due to intramolecular and intermolecular hydrogen bonds of hydroxyl groups in the polyvinyl acetal resin can be suppressed.When the amount of acetyl groups is 22.0 mol% or less, the flexibility of the polyvinyl acetal resin is not excessively increased, and the handleability can be improved. The acetyl group amount has a more preferable lower limit of 0.5 mol % and a more preferable upper limit of 15.0 mol %. That is, the acetyl group amount is preferably 0.1 to 22.0 mol %, and more preferably 0.5 to 15 mol %. The amount of acetyl groups is, for example, 1 It can be measured by H-NMR.
[0022] The amount of hydroxyl groups relative to the Z-average molecular weight of the polyvinyl acetal resin of the present invention (amount of hydroxyl groups / Mz) is 1.30×10 -5 By making the content equal to or higher than the above lower limit, high dispersibility can be obtained. The amount of hydroxyl groups / Mz is 1.40×10 -5 More preferably, it is 1.50×10 or more. -5 More preferably, it is 2.70×10 or more. -5 It is preferable that the value is less than 2.65×10 -5 More preferably, it is 2.60×10 or less. -5 More preferably, the amount of hydroxyl groups / Mz is 1.30×10 -5 ~2.70×10 -5 It is preferable that the ratio is 1.40×10 -5 ~2.65×10 -5 More preferably, it is 1.50×10 -5 ~2.60×10 -5 It is more preferable that:
[0023] In the polyvinyl acetal resin of the present invention, from the viewpoint of maintaining mechanical strength when a thin film ceramic green sheet is produced, the average polymerization degree has a preferable lower limit of 500, more preferably 600, and from the viewpoint of solubility in organic solvents and dissolution viscosity, the average polymerization degree is preferably 10,000, more preferably 9,000. That is, the average polymerization degree is preferably 500 to 10,000, more preferably 600 to 9,000. The average degree of polymerization of the polyvinyl acetal resin is the same as that of the raw material polyvinyl alcohol, and can be measured in accordance with JIS K 6726.
[0024] The polyvinyl acetal resin of the present invention can usually be produced by acetalizing a polyvinyl alcohol resin.
[0025] As the polyvinyl alcohol resin, for example, a conventionally known polyvinyl alcohol resin such as a resin produced by saponifying a polyvinyl acetate resin with an alkali, an acid, aqueous ammonia or the like can be used. The polyvinyl alcohol resin may be fully saponified, but it does not need to be fully saponified as long as there is at least one unit having two consecutive hydroxyl groups at the meso and racemo positions at at least one position in the main chain, and may be a partially saponified polyvinyl alcohol resin. In addition, as the polyvinyl alcohol resin, a copolymer of vinyl alcohol and a monomer copolymerizable with vinyl alcohol, such as an ethylene-vinyl alcohol copolymer resin or a partially saponified ethylene-vinyl alcohol copolymer resin, may also be used. The polyvinyl acetate resin may be, for example, an ethylene-vinyl acetate copolymer.
[0026] The polyvinyl alcohol resin preferably has a degree of saponification of 75 mol % or more. The saponification degree is preferably 76 mol % or more and 99.4 mol % or less, and more preferably 78 mol % or more and 98 mol % or less. That is, the saponification degree is preferably 76 to 99.4 mol %, and more preferably 78 to 98 mol %. By using the polyvinyl alcohol resin, the Mz can be set within a predetermined range.
[0027] The above acetalization is preferably carried out in a water solvent, in a mixed solvent of water and an organic solvent compatible with water, or in an organic solvent. As the organic solvent compatible with water, for example, an alcohol-based organic solvent can be used. Examples of the organic solvent include alcohol-based organic solvents, aromatic organic solvents, aliphatic ester-based solvents, ketone-based solvents, lower paraffin-based solvents, ether-based solvents, amide-based solvents, and amine-based solvents. Examples of the alcohol-based organic solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. Examples of the aromatic organic solvent include xylene, toluene, ethylbenzene, and methyl benzoate. Examples of the aliphatic ester solvent include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, methyl acetoacetate, and ethyl acetoacetate. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methylcyclohexanone, benzophenone, and acetophenone. Examples of the lower paraffin solvent include hexane, pentane, octane, cyclohexane, and decane. Examples of the ether solvent include diethyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol diethyl ether. Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetanilide. Examples of the amine solvent include ammonia, trimethylamine, triethylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, aniline, N-methylaniline, N,N-dimethylaniline, and pyridine. These solvents may be used alone or in combination of two or more. Among these, ethanol, n-propanol, isopropanol, and tetrahydrofuran are particularly preferred from the viewpoints of solubility in the resin and ease of purification.
[0028] The acetalization is preferably carried out in the presence of an acid catalyst. The acid catalyst is not particularly limited, and examples thereof include mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, carboxylic acids such as formic acid, acetic acid, and propionic acid, and sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, and paratoluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more compounds. Among them, hydrochloric acid, nitric acid, and sulfuric acid are preferred, and hydrochloric acid is particularly preferred.
[0029] The aldehyde used in the acetalization reaction may be an aldehyde having a chain aliphatic group, a cyclic aliphatic group, or an aromatic group having 1 to 10 carbon atoms. Any known aldehyde may be used as the aldehyde. The aldehyde used in the acetalization reaction is not particularly limited, and may be, for example, an aliphatic aldehyde, an aromatic aldehyde, or the like. Examples of the aliphatic aldehyde include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, n-hexylaldehyde, 2-ethylbutyraldehyde, 2-ethylhexylaldehyde, n-heptylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, and amylaldehyde. Examples of the aromatic aldehyde include benzaldehyde, cinnamaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, and β-phenylpropionaldehyde. These aldehydes may be used alone or in combination of two or more. Among them, preferred aldehydes are formaldehyde, acetaldehyde, butylaldehyde, 2-ethylhexylaldehyde, and n-nonylaldehyde, which have excellent acetalization reactivity and can provide sufficient internal plasticizing effect to the resin produced, thereby imparting good flexibility. In addition, more preferred are formaldehyde, acetaldehyde, and butylaldehyde, which can provide an adhesive composition that is particularly excellent in impact resistance and adhesion to metals.
[0030] The amount of the aldehyde to be added can be appropriately set according to the amount of acetal groups in the target polyvinyl acetal resin. In particular, it is preferable to add 50 mol% or more and 95 mol% or less, more preferably 55 mol% or more and 90 mol% or less, based on 100 mol% of polyvinyl alcohol, because this allows the acetalization reaction to proceed efficiently and makes it easy to remove unreacted aldehyde.
[0031] The acetalization reaction is preferably carried out by raising the temperature at a predetermined rate and then maintaining the temperature for a certain period of time. The temperature rise time in the acetalization reaction is preferably 120 minutes or more and 420 minutes or less, and more preferably 180 minutes or more and 360 minutes or less. That is, the temperature rise time is preferably 120 to 420 minutes, and more preferably 180 to 360 minutes. Moreover, the rate of temperature rise is preferably 0.1° C. / min or more and 0.4° C. / min or less, that is, the rate of temperature rise is preferably 0.1 to 0.4° C. / min. By raising the temperature at the above-mentioned temperature rise rate, the molecular weight differential distribution value at Mz and LogM = 6.00 can be set within a predetermined range.
[0032] The retention time in the acetalization reaction is preferably 1 hour or more and 10 hours or less, and more preferably 2 hours or more and 9 hours or less. That is, the retention time is preferably 1 to 10 hours, and more preferably 2 to 9 hours or less. By setting the retention time as described above, the Mz can be set within a predetermined range. The holding temperature in the acetalization reaction is preferably 30° C. or higher and 80° C. or lower, and more preferably 40° C. or higher and 70° C. or lower. That is, the holding temperature is preferably 30 to 80° C., and more preferably 40 to 70° C. By setting the holding temperature as above, the molecular weight differential distribution value at Mz and LogM=6.00 can be set within a predetermined range.
[0033] The present invention also includes a resin composition for a ceramic green sheet, which contains the polyvinyl acetal resin of the present invention and a plasticizer. The resin composition for a ceramic green sheet of the present invention may contain components such as an antioxidant, a surfactant, an ultraviolet absorber, and an antifoaming agent, so long as they do not impair the effects of the present invention.
[0034] As a method for producing the resin composition for a ceramic green sheet of the present invention, for example, a plasticizer and other additives added as necessary are added to a polyvinyl acetal resin obtained by acetalizing a polyvinyl alcohol resin with an aldehyde, and then mixed to obtain a resin composition for a ceramic green sheet.
[0035] The resin composition for a ceramic green sheet of the present invention contains a plasticizer. By adding the plasticizer, the mechanical strength and flexibility of the obtained ceramic green sheet can be significantly improved. Examples of the plasticizer include phthalic acid diesters such as dioctyl phthalate (DOP) and dibutyl phthalate (DBP), adipic acid diesters such as dioctyl adipate, and alkylene glycol diesters such as triethylene glycol-di-2-ethylhexanoate, tetraethylene glycol-di-2-ethylhexanoate, triethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-heptanoate, and triethylene glycol-di-heptanoate.
[0036] In the resin composition for a ceramic green sheet of the present invention, the content of the above-mentioned plasticizer, relative to 100 parts by weight of the polyvinyl acetal resin, is preferably such that the lower limit is 7 parts by weight, more preferably 8.5 parts by weight, and preferably such that the upper limit is 18 parts by weight, more preferably 13.5 parts by weight.
[0037] A slurry composition for a ceramic green sheet can be prepared by mixing an organic solvent and ceramic powder with the resin composition for a ceramic green sheet of the present invention.
[0038] The organic solvent is not particularly limited, and may be any solvent capable of dissolving the polyvinyl acetal resin, such as ketones, including acetone, methyl ethyl ketone, dipropyl ketone, and diisobutyl ketone. Other examples include alcohols, such as methanol, ethanol, isopropanol, and butanol, and aromatic hydrocarbons, such as toluene and xylene. Other examples include esters, such as methyl propionate, ethyl propionate, butyl propionate, methyl butanoate, ethyl butanoate, butyl butanoate, methyl pentanoate, ethyl pentanoate, butyl pentanoate, methyl hexanoate, ethyl hexanoate, butyl hexanoate, 2-ethylhexyl acetate, and 2-ethylhexyl butyrate. Other examples include methyl cellosolve, ethyl cellosolve, butyl cellosolve, terpineol, dihydroterpineol, butyl cellosolve acetate, butyl carbitol acetate, terpineol acetate, and dihydroterpineol acetate. In particular, alcohols, ketones, aromatic hydrocarbons and mixed solvents thereof are preferred in terms of coating and drying properties, with a mixed solvent of ethanol and toluene and a mixed solvent of methyl ethyl ketone and toluene being more preferred.
[0039] The content of the organic solvent in the ceramic green sheet slurry composition is set according to the type of polyvinyl acetal resin used, and is not particularly limited, but if it is too small, it is difficult to exhibit the solubility required for kneading. Also, if it is too large, the viscosity of the ceramic green sheet slurry composition becomes too low, which may cause poor handling when producing a ceramic green sheet. For this reason, the content of the organic solvent is preferably 20% by weight or more and 80% by weight or less.
[0040] The ceramic powder includes powders of oxides or non-oxides of metals or non-metals used in the manufacture of ceramics. The composition of these powders may be a single composition, a compound state, or a mixture. The constituent elements of the metal oxide or non-oxide may be a single element or a plurality of elements, both as cations and anions, and may further include additives added to improve the properties of the oxide or non-oxide. Specific examples of the oxides or non-oxides include oxides, carbides, nitrides, borides, and sulfides of Li, K, Mg, B, Al, Si, Cu, Ca, Sr, Ba, Zn, Cd, Ga, In, Y, lanthanides, actinides, Ti, Zr, Hf, Bi, V, Nb, Ta, W, Mn, Fe, Co, Ni, etc. In addition, specific oxide powders containing multiple metal elements, usually called double oxides, can be classified based on their crystal structure as follows: those with a perovskite structure include NaNbO3, SrZrO3, PbZrO3, SrTiO3, BaZrO3, PbTiO3, BaTiO3, etc.; those with a spinel structure include MgAl2O4, ZnAl2O4, CoAl2O4, NiAl2O4, MgFe2O4, etc.; those with an ilmenite structure include MgTiO3, MnTiO3, FeTiO3, etc.; and those with a garnet structure include GdGa5O4, GdGa5O5, etc. 12 , Y6Fe5O 12 Among these, the modified polyvinyl acetal resin of the present invention exhibits high properties when mixed with BaTiO3 powder in a ceramic green sheet.
[0041] The average particle size of the ceramic powder is not particularly limited, but for example, for producing a thin ceramic green sheet (thickness 5 μm or less), it is preferably 0.5 μm or less.
[0042] The above-mentioned slurry composition for ceramic green sheet may contain other resins such as polyvinyl acetal resins other than the polyvinyl acetal resin of the present invention, acrylic resins, ethyl cellulose, etc., within the range that does not impair the effects of the present invention. In such a case, the content of the polyvinyl acetal resin of the present invention relative to the total binder resins is preferably 50% by weight or more.
[0043] The above-mentioned slurry composition for ceramic green sheets may contain, as necessary, a dispersant, an antioxidant, an ultraviolet absorber, a surfactant, a filler, etc., and in some cases, a small amount of other resin such as an acrylic resin or a urethane resin may be added.
[0044] The method for producing the above-mentioned slurry composition for ceramic green sheets is not particularly limited, and examples thereof include a method in which the polyvinyl acetal resin of the present invention, an organic solvent, a ceramic powder, and various additives added as necessary are mixed using various mixers such as a ball mill, a blender mill, and a three-roll mill.
[0045] After the slurry composition for ceramic green sheets is applied, the composition is heated and dried to obtain ceramic green sheets. The ceramic green sheets can be used to manufacture ceramic electronic components. For example, the ceramic electronic components can be manufactured by carrying out a step of applying a paste for electrode layers to the surfaces of the ceramic green sheets, and a step of stacking the ceramic green sheets on which the electrode layers have been formed, and heat-pressing the stack to obtain a laminate, followed by degreasing and firing the laminate.
[0046] The method for applying the slurry composition for ceramic green sheets is not particularly limited, and examples thereof include methods using a roll coater, a die coater, a curtain coater, etc. As for other specific methods, conventionally known methods can be used.
[0047] The ceramic electronic components are not particularly limited, and examples thereof include multilayer ceramic capacitors, multilayer ceramic inductors, capacitors, piezoelectric actuators, multilayer varistors, multilayer thermistors, EMI filters, aluminum nitride multilayer substrates, and alumina multilayer substrates.
[0048] The method for producing a ceramic electronic component includes a step of applying a paste for electrode layers to the surfaces of the ceramic green sheets. The electrode layer paste can be obtained by dissolving, for example, polyvinyl acetal resin, ethyl cellulose, acrylic resin, etc. as a binder resin in an organic solvent and dispersing conductive powder, etc. These resins may be used alone or in combination of two or more. The electrode layer paste containing polyvinyl acetal resin is preferred because it exhibits excellent adhesion to the ceramic green sheet in the heat-pressing step.
[0049] In the method for producing a ceramic electronic component, the above-mentioned ceramic green sheets having electrode layers formed thereon are produced, and then similarly produced ceramic green sheets having electrode layers formed thereon are stacked and heated and pressed to obtain a laminate, which is then degreased and fired, thereby obtaining a multilayer ceramic electronic component in which problems such as sheet attack and cracks are solved. The above-mentioned heat-pressure bonding step and the steps of degreasing and firing the laminate are not particularly limited, and conventionally known methods can be used. Effect of the Invention
[0050] According to the present invention, it is possible to obtain a ceramic green sheet having high strength and being resistant to delamination and dimensional change during drying, and it is possible to provide a polyvinyl acetal resin and a resin composition for a ceramic green sheet with which a multilayer ceramic capacitor having excellent reliability can be produced. Furthermore, by using the polyvinyl acetal resin of the present invention, the dispersibility and dispersion stability of ceramic powder can be significantly improved. [Brief description of the drawings]
[0051] [Figure 1] FIG. 2 is a diagram showing an example of a molecular weight differential distribution curve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0053] Example 1 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 1,700, saponification degree 99.0 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 120g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.2°C / min (heating time 250 minutes). The mixture was kept at 70°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin.
[0054] (Preparation of Resin Composition for Ceramic Green Sheet) 1.25 parts by weight of the obtained polyvinyl acetal resin was added to 48.75 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and dissolved by stirring to obtain a resin composition for ceramic green sheets.
[0055] (Preparation of resin sheet) The obtained resin composition for ceramic green sheet was applied onto a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and then the film was heated and dried at 70° C. for 60 minutes to produce a resin sheet.
[0056] (Preparation of Slurry Composition) 2 parts by weight of the obtained polyvinyl acetal resin and 2 parts by weight of dioctyl phthalate (DOP) were added to 96 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and dissolved with stirring to prepare a resin solution. In addition, 3 parts by weight of polyvinyl acetal resin "BL-1" (manufactured by Sekisui Chemical Co., Ltd.) was added to 40 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and dissolved by stirring. Next, 100 parts by weight of barium titanate powder (manufactured by Sakai Chemical Industry Co., Ltd., BT01) was added and stirred for 180 minutes with a bead mill (Ready Mill manufactured by Imex Co., Ltd.) to prepare an inorganic dispersion. The above resin solution (100 parts by weight) was added to the inorganic dispersion obtained and stirred with a bead mill to obtain a slurry composition. During stirring, sampling was performed every 5 minutes, and 0.1 parts by weight of the obtained slurry composition was added to 10 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1), and stirred with an ultrasonic disperser (US-303, manufactured by SND Co., Ltd.) to prepare a dispersion evaluation solution. The particle size distribution was measured using a laser diffraction particle size distribution meter (LA-910, manufactured by Horiba, Ltd.), and stirring was stopped when the D50 value of the particle size distribution reached 1.0 μm.
[0057] Example 2 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 3,000, saponification degree 98.9 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 120g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butyl aldehyde were added thereto, and the temperature was increased at a rate of 0.2°C / min (temperature increase time 250 minutes). The mixture was kept at 70°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0058] Example 3 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 5,000, saponification degree 98.9 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 120g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butyl aldehyde were added thereto, and the temperature was increased at a rate of 0.2°C / min (heating time 250 minutes). The mixture was kept at 70°C for 2 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0059] Example 4 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 9,000, saponification degree 98.9 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 120g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butyl aldehyde were added thereto, and the temperature was increased at a rate of 0.2°C / min (heating time 250 minutes). The mixture was kept at 70°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0060] Example 5 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 1700, saponification degree 98.8 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 120g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.16°C / min (heating time 250 minutes). The mixture was kept at 60°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0061] Example 6 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 800, saponification degree 98.8 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 150g of hydrochloric acid with a concentration of 35% by weight and 145g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.16°C / min (heating time 250 minutes). The mixture was kept at 60°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0062] Comparative Example 1 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 300, saponification degree 99.0 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 150g of hydrochloric acid with a concentration of 35% by weight and 145g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.5°C / min (temperature increase time 10 minutes). The mixture was kept at 25°C for 4 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0063] Comparative Example 2 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 500, saponification degree 98.5 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 150g of hydrochloric acid with a concentration of 35% by weight and 145g of n-butyl aldehyde were added thereto, and the temperature was increased at a rate of 0.5°C / min (temperature increase time 10 minutes). The mixture was kept at 25°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0064] Comparative Example 3 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 800, saponification degree 99.0 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 150g of hydrochloric acid with a concentration of 35% by weight and 145g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.7°C / min (heating time 7 minutes). The mixture was kept at 25°C for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0065] Comparative Example 4 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 9000, saponification degree 99.0 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 150g of hydrochloric acid with a concentration of 35% by weight and 145g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.7°C / min (temperature increase time 10 minutes). The mixture was kept at 25°C for 2.5 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0066] Comparative Example 5 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 8800, saponification degree 99.0 mol%), and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 20°C, and 150g of hydrochloric acid with a concentration of 35% by weight and 150g of n-butylaldehyde were added thereto, and the temperature was increased at a rate of 0.7°C / min (heating time 7 minutes). The mixture was kept at 25°C for 2.5 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was neutralized, washed with water, and dried by a conventional method to obtain a white powder of polyvinyl acetal resin, a resin composition for ceramic green sheets, a resin sheet, and a slurry composition.
[0067] (evaluation) The polyvinyl acetal resins, resin compositions for ceramic green sheets, resin sheets, and slurry compositions obtained in the Examples and Comparative Examples were evaluated as follows. The results are shown in Table 1.
[0068] (1) Evaluation of polyvinyl acetal resin (1-1) Amount of acetal groups, hydroxyl groups, and acetyl groups The polyvinyl acetal resin thus obtained was analyzed using an AV400 spectrometer (manufactured by Bruker Corporation). 1 H-NMR measurement was carried out, and the amounts of acetal groups, hydroxyl groups, and acetyl groups were calculated. The obtained polyvinyl acetal resin was dissolved in DMSO-D6 to a concentration of 1.6% by weight to prepare a measurement solution. 1 H-NMR measurements were carried out at 80 °C.
[0069] (1-2) Molecular weight differential distribution value at Mz, LogM = 6.00 The obtained polyvinyl acetal resin was dissolved in tetrahydrofuran (THF) at a concentration of 0.2% by weight, and measured using a GPC apparatus HLC-8220 (manufactured by Tosoh Corporation). From the measurement results obtained, the Z-average molecular weight Mz was calculated using a molecular weight calibration curve prepared using a monodisperse polystyrene standard sample. From the obtained molecular weight differential distribution curve, the molecular weight differential distribution value at LogM=6.00 was measured. The column used was TSKgel SuperHZ (manufactured by Tosoh Corporation).
[0070] (2) Evaluation of resin sheets (2-1) Tensile modulus, elongation at break and stress at break The obtained resin sheet was subjected to measurement of the breaking stress (MPa), breaking elongation (%) and tensile modulus (MPa) at a tensile speed of 20 mm / min using a tensile tester (Shimadzu Corporation, AUTOGRAPH AGS-J) in accordance with JIS K 7113.
[0071] (3) Evaluation of slurry composition (3-1) Dispersibility (Preparation of dispersibility evaluation solution) 0.1 parts by weight of the obtained slurry composition was added to 10 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and stirred with an ultrasonic disperser (manufactured by SND Corporation, US-303) to prepare a solution for dispersibility evaluation.
[0072] (Dispersibility evaluation) The particle size distribution of the obtained solution for evaluating dispersibility was measured 60 minutes after the end of stirring. The particle size distribution was measured using a laser diffraction particle size distribution analyzer (LA-910, manufactured by Horiba, Ltd.) to measure the average particle size.
[0073] (3-2) Dispersion stability The dispersibility evaluation solution obtained in (3-1) above was left to stand at 23° C. for 1 week, after which particle size distribution was measured to determine the average particle size.
[0074] (4) Evaluation of ceramic green sheets (Preparation of ceramic green sheets) The obtained slurry composition was applied onto a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and then the film was dried by heating to prepare a ceramic green sheet.
[0075] (4-1) Tensile modulus, elongation at break and stress at break (Preparation of ceramic green sheets) One part by weight of polyvinyl acetal resin (BL-1, manufactured by Sekisui Chemical Co., Ltd.) was added to a mixed solvent of 20 parts by weight of toluene and 20 parts by weight of ethanol, and dissolved by stirring. Next, 100 parts by weight of barium titanate powder (BT01, manufactured by Sakai Chemical Industry Co., Ltd., average particle size 0.1 μm) was added to the obtained solution, and the mixture was stirred for 180 minutes with a bead mill (Ready Mill, manufactured by Imex Co., Ltd.) to prepare an inorganic dispersion. The resin composition for ceramic green sheets obtained in the Examples and Comparative Examples was added to the inorganic dispersion obtained, and the mixture was stirred for 90 minutes in a bead mill, and then coated on a release-treated PET film using a coater so that the thickness after drying was 20 μm. The mixture was then dried by heating at 40° C. for 30 minutes, and the PET film was peeled off to produce a ceramic green sheet. The resulting ceramic green sheets were subjected to measurement of the breaking stress (MPa), tensile modulus (MPa), and breaking elongation (%) at a tension speed of 20 mm / min using a tensile tester (Shimadzu Corporation, AUTOGRAPH AGS-J) in accordance with JIS K 7113.
[0076] (4-2) Cutting cross section After measuring "(4-1) Tensile modulus, elongation at break, and stress at break," the fracture surface was observed by SEM and evaluated according to the following criteria. ◎: No chips, cracks or scratches on the fracture surface ○: There are no chips or cracks on the fracture surface, but there are scratches. △: There are no chips on the fracture surface, but there are cracks ×: There are chips on the fracture surface and peeling between sheets.
[0077] (4-3) Dimensional change rate A ceramic green sheet was prepared in the same manner as in "(4-1) Tensile modulus, elongation at break, and stress at break." The obtained ceramic green sheet was dried at 70°C for 3 hours, and the dimensional change rate before and after drying at 70°C was calculated and evaluated according to the following criteria. ◎: Less than 2% ○: More than 2% and 3% or less △: More than 3% and less than 4% ×: More than 4%
[0078] [Table 1] [Industrial Applicability]
[0079] According to the present invention, it is possible to obtain a ceramic green sheet which has excellent dispersibility and dispersion stability of ceramic powder, and is strong and unlikely to undergo delamination or dimensional change during drying, and it is possible to provide a polyvinyl acetal resin and a resin composition for ceramic green sheets which are capable of producing a multilayer ceramic capacitor with excellent reliability.
Claims
1. The Z-average molecular weight (Mz) is 700,000 or more and 2,500,000 or less, A polyvinyl acetal resin having a molecular weight differential distribution value at Log M = 6.00 of 5.00 or more and 110.0 or less.
2. The amount of hydroxyl groups relative to the Z-average molecular weight (amount of hydroxyl groups / Z-average molecular weight) is 1.30×10 -5 The polyvinyl acetal resin according to claim 1 .
3. 3. The polyvinyl acetal resin according to claim 1, wherein the amount of acetal groups is 50 to 83 mol %.
4. A resin composition for a ceramic green sheet, comprising the polyvinyl acetal resin according to claim 1 or 2 and a plasticizer.
Citation Information
Patent Citations
Polyvinyl acetal resin and method for producing polyvinyl acetal resin
JP2005325342A