Substrate for mask blank and producing method thereof
The mask blank substrate with precise pseudo TTV map manufacturing methods addresses the flatness and precision issues in EUV lithography, ensuring high transfer accuracy and productivity for EUVL exposure masks.
Patent Information
- Application Number
- JP2024076226
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-09
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for manufacturing glass substrates for EUV lithography fail to achieve the necessary flatness and precision required for high NA EUV exposure, particularly due to challenges in measuring and correcting the refractive index distribution in multi-component glass substrates, leading to inadequate transfer accuracy.
A mask blank substrate with two main surfaces, each 152 mm x 152 mm square and 6.35 mm thick, is manufactured through local processing and final polishing, ensuring a pseudo TTV map with a difference of 35 nm or less for TTV1 and 25 nm or less for TTV2, achieved by predicting and evaluating the surface shape after final polishing to meet predetermined flatness criteria.
The substrate provides high flatness and transfer accuracy during electrostatic attraction, enabling reliable and efficient production of exposure masks for EUVL with improved productivity.
Smart Images

Figure 2024170294000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a mask blanks substrate used in photolithography and a manufacturing method thereof, and more particularly to a mask blanks substrate suitable for mask blanks used to manufacture a transfer mask for photolithography in which EUV (Extreme Ultra Violet) light is used as exposure light, and a manufacturing method thereof. [Background technology]
[0002] In recent years, interest in AI and IoT has led to the need for computational processing of huge amounts of data, which has led to demands for faster computational processing and lower power consumption. To meet this demand, it is necessary to improve the performance of IC chips, and in general, miniaturization of electrical wiring has been adopted as an effective means. The main methods used to miniaturize wiring are to increase the NA and shorten the wavelength of exposure light, but in recent years, EUV lithography (EUVL) using extreme ultraviolet (EUV) light is beginning to be put to practical use.
[0003] In EUVL, the exposure mask is one of the important elements, and improving the flatness of the glass substrate for the exposure mask original (mask blank) is extremely important for achieving accurate exposure. The mainstream method for manufacturing normal glass substrates is double-sided simultaneous polishing, but double-sided simultaneous polishing alone does not provide a flatness good enough for use in EUVL. To achieve high flatness, it is necessary to correct the flatness to match the surface shape by polishing each side at a time, and local processing techniques such as local etching and local polishing are used for this. These are techniques that remove relatively convex areas on the main surface of the substrate to make the entire substrate closer to flat. In addition, by using the wavefront correction function of the exposure tool, the surface shape of the exposure mask can be optically corrected, and it can be used as an optically highly flat exposure mask.
[0004] With the recent trend towards miniaturization, EUVL is now also required to have a high NA, and the required flatness has become increasingly strict. The flatness requirement has reached a level that cannot be met by the pursuit of polishing technology alone, and rather than simply using flatness as an indicator, it has become necessary to selectively manufacture glass substrates with shapes that can be used for exposure.
[0005] One index closely related to such performance is the TTV of a glass substrate. TTV has been used to evaluate the performance of single-component glass substrates. A transmission optical system is suitable for measuring the thickness distribution (TTV map), and it was easy to measure the TTV map of single-component glass. However, for multi-component glass substrates such as those used in EUVL, a refractive index distribution occurs due to fluctuations in the glass component concentration, making precise optical measurement of the TTV map difficult. For this reason, it was necessary to use a pseudo TTV map (hereinafter referred to as pseudo TTV map) obtained by adding together the surface shapes of the first and second main surfaces.
[0006] For example, International Publication No. 2016 / 098452 (Patent Document 1) describes that in order to obtain high transfer accuracy when a reflective mask made using a substrate that has been subjected to conventional double-sided polishing and local processing on both the front and back main surfaces is chucked to an exposure tool and subjected to exposure transfer, if the shape of the front main surface of the substrate when electrostatically chucked is made close to a shape that can be defined by a Zernike polynomial that can be corrected by the wavefront correction function of the exposure tool (virtual surface shape), even if the substrate has thickness variations that affect changes in the shape of the front main surface, the thickness variations can be made to be easily correctable by the wavefront correction function of the exposure tool, and a transfer mask having such a substrate can expose and transfer the transfer pattern to the transfer target with high accuracy. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2016 / 098452 [Patent Document 2] JP 2010-194705 A Summary of the Invention [Problem to be solved by the invention]
[0008] The method described in International Publication No. 2016 / 098452 (Patent Document 1) is composed of a process of calculating a composite plane of the front main surface and the back main surface when adsorbed to an exposure tool, a process of fitting this composite plane with Zernike polynomials, and a process of predicting the surface shape after optical correction by subtracting the fitting shape from the composite plane. However, this method specifies the flatness within a circular area with a diameter of 104 mm, which is insufficient for the area actually used for exposure (132 mm x 104 mm square). Furthermore, by excluding the relatively high-order terms from the fourth to sixth terms of the Legendre polynomials, the steep shape of the outermost periphery tends to be strongly corrected. In that case, the correction is applied to shapes that would otherwise have a negative effect on exposure, and the TTV is evaluated as if it were good.
[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide a mask blanks substrate that provides an exposure mask capable of achieving extremely advantageous transfer accuracy for next-generation high NA EUV exposure in exposure using an exposure mask, particularly exposure by EUVL, and a method for producing such a mask blanks substrate with good productivity. [Means for solving the problem]
[0010] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that in a mask blank substrate having two main surfaces, a first main surface and a second main surface, each measuring 152 mm×152 mm square and having a thickness of 6.35 mm, a pseudo-TTV map is created by adding together the height maps of the first main surface and the second main surface, and in this pseudo-TTV map, a cross-shaped region formed when a first rectangular region measuring 132 mm×104 mm and parallel to the four sides of the main surface and centered at the intersection of the diagonals of the main surface is superimposed on a second rectangular region measuring 104 mm×132 mm which is perpendicular to the first rectangular region and parallel to the four sides of the main surface and centered at the intersection of the diagonals of the main surface is superimposed. It was found that when a region is set, a mask blank substrate in which the difference between the maximum height and the minimum height of the TTV1 map excluding the first-order component when a plane function approximated by a first-order polynomial is derived in the fitting of the pseudo-TTV map (TTV1) within the cross-shaped region is 35 nm or less, and the difference between the maximum height and the minimum height of the TTV2 map excluding the first-order and second-order components when a surface function approximated by a polynomial up to second order is derived in the fitting of the pseudo-TTV map (TTV2) is 25 nm or less can be provided as an exposure mask that is sufficiently flat when electrostatically adsorbed by an exposure machine and has good transfer performance.
[0011] The present inventors have also discovered that by manufacturing a mask blank substrate by a method including a local processing step and a finish polishing step following the local processing step, and predicting the shape of the main surface after the finish polishing step after the local processing step by applying a previously determined change in the shape of the main surface after the finish polishing step to the shape of the main surface before the finish polishing step after the local processing step, and evaluating whether the predicted shape of the main surface provides a predetermined flatness, it is possible to reliably and productively manufacture a mask blank substrate which is sufficiently flat when electrostatically adsorbed by an exposure machine and which provides an exposure mask having good transfer performance, thereby completing the present invention.
[0012] Therefore, the present invention provides the following mask blank substrate and method for manufacturing a mask blank substrate. A mask blank substrate having two main surfaces, a first main surface and a second main surface, each of which is 1.152 mm × 152 mm square, and a thickness of 6.35 mm, In a pseudo-TTV map obtained by adding a height map of the first main surface and a height map of the second main surface based on respective positions on the least squares plane of the first main surface and the second main surface, Within a cross-shaped region formed when a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered at the intersection of the diagonals of the main surface of the substrate, In fitting the pseudo-TTV map, when a plane function approximated by a first-order polynomial is derived, the difference between the maximum height and the minimum height of the TTV1 map excluding the first-order component (TTV1) is 35 nm or less, and when a curved surface function approximated by a polynomial up to the second order is derived in fitting the pseudo-TTV map, the difference between the maximum height and the minimum height of the TTV2 map excluding the first-order component and the second-order component (TTV2) is 25 nm or less. A substrate for mask blanks comprising: 2. The mask blank substrate according to 1, wherein the flatness within the cross-shaped region of the first main surface is 35 nm or less. A method for manufacturing a mask blank substrate having two main surfaces, a first main surface and a second main surface, each of which is 3.152 mm × 152 mm square, and a thickness of 6.35 mm, comprising the steps of: A local processing step for at least one of the first main surface and the second main surface, and a finish polishing step subsequent to the local processing step, The local processing step includes: (A) locally processing at least one of the first main surface and the second main surface; (B) measuring the shape of the locally machined main surface after the step (A) as the shape of the main surface before the finish polishing step; (C) a step of predicting a shape of the locally processed main surface after the finish polishing step by applying a previously determined change in surface shape during the finish polishing step to a shape of the main surface before the finish polishing step obtained in the step (B); (D) a step of evaluating whether the shape after the finish polishing step predicted in the step (C) is a shape that gives a predetermined TTV; A method for producing a substrate for a mask blank, comprising: 4. The shape that gives the predetermined TTV in the step (D) is (1) arranging the substrate so that the first main surface and the second main surface are aligned in a substantially vertical direction, and setting a calculation area in the shape of a regular rectangular cylinder extending in a horizontal direction passing through the four sides of a 132 mm × 132 mm square that is aligned with the four sides of the first main surface and the second main surface at the center of the first main surface and the second main surface; (2) in a state facing the first main surface, a portion within the calculation region is cut out from the first main surface to define a first region surface; (3) setting a vertical plane that passes through a reference point, which is an arbitrary point on the central axis of a regular square cylinder of the calculation area, and is perpendicular to the central axis, as a reference plane; setting a rotation axis that passes through the reference point and is parallel to any one of the four sides of the regular square that is the intersection line between the regular square cylinder of the calculation area and the vertical plane; rotating the substrate 180 degrees along the rotation axis from a state where the substrate faces the first main surface; and cutting out a portion of the calculation area from the second main surface to set it as a second area surface; (4) calculating a least squares plane on each of the first and second domain surfaces; (5) converting the first and second domain surfaces into a height map of the first domain surface and a height map of the second domain surface based on respective positions on the least squares plane of the first and second domain surfaces; (6) The height map of the second region surface is symmetrically moved with respect to a vertical plane passing through the rotation axis and aligned in the 90° direction of the rotation to obtain an inverted height map of the second region surface; (7) At each position (X coordinate, Y coordinate) on the reference plane, a height of the height map of the first area surface and a height of the inverted height map of the second area surface are added together to generate a predicted pseudo-TTV map; (8) In the predicted pseudo-TTV map, a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered at the intersection of the diagonals of the main surface of the substrate, in a cross-shaped region formed by superimposing the first rectangular region and the second rectangular region of 104 mm x 132 mm parallel to the four sides of the main surface of the substrate, A shape in which the difference (TTV1') between the maximum height and the minimum height of a TTV1' map excluding the first-order component when a plane function approximated by a first-order polynomial is derived in fitting the predicted pseudo-TTV map is 35 nm or less, and the difference (TTV2') between the maximum height and the minimum height of a TTV2' map excluding the first-order component and the second-order component when a surface function approximated by a first-order polynomial is derived in fitting the predicted pseudo-TTV map is 25 nm or less. 4. The method for producing a compound according to claim 3, Effect of the Invention
[0013] The mask blanks substrate of the present invention can provide an exposure mask that has a highly flat shape when electrostatically attracted to an exposure device in exposure using an exposure mask, particularly exposure by EUVL with a high NA. Moreover, according to the manufacturing method of the mask blanks substrate of the present invention, such a mask blanks substrate can be manufactured reliably and with good productivity. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a diagram for explaining an embodiment of a mask blank substrate of the present invention, in which (A) is a side view of a state in which a first main surface and a second main surface of the mask blank substrate are arranged along the vertical direction, and (B) is a front view of the first main surface located on the right side in (A). [Diagram 2]FIG. 1 is a diagram for explaining an embodiment of a mask blank substrate of the present invention, in which (A) is a side view of the mask blank substrate after rotation by 180 degrees, and (B) is a front view of the second main surface located on the right side in (A) after rotation. [Diagram 3] FIG. 2 is a diagram for explaining an embodiment of a mask blank substrate of the present invention, in which (A) to (C) are a height map of a first region surface, a height map of a second region surface, and an inverted height map of the second region surface, respectively. [Figure 4] FIG. 2 is a diagram for explaining an embodiment of a mask blank substrate of the present invention, and is a pseudo-TTV map (Z coordinate map) obtained from a height map of a first region surface and an inverted height map of a second region surface. [Diagram 5] FIG. 1 is a diagram for explaining an embodiment of a mask blank substrate according to the present invention, in which (A) is a diagram showing a cross-shaped region that is a target region for evaluation in a pseudo TTV map, (B) is a diagram showing a first rectangular region (vertical region) that constitutes the cross-shaped region, and (C) is a diagram showing a second rectangular region (horizontal region) that constitutes the cross-shaped region. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. The mask blank substrate of the present invention has two main surfaces, a first main surface and a second main surface, each of which is 152 mm×152 mm square, and is 6.35 mm thick. A substrate of this size is known as a 6025 substrate, and has two main surfaces, a first main surface and a second main surface, each of which is 6 inches×6 inches square, and is 0.25 inches thick.
[0016] The material of the mask blank substrate of the present invention may be a conventional material and is not particularly limited, but since the substrate is exposed to high-energy exposure light in drawing a fine pattern, TiO2-doped quartz glass containing 3 to 10 mass% TiO2, which has very high dimensional stability at high temperatures, is preferably used. The raw material substrate for the mask blank substrate may be one that has been synthesized, molded, and processed according to a conventional method.
[0017] Substrates for mask blanks are required to have a high degree of flatness. This is because the higher the flatness, the easier it is to achieve the desired exposure, and it can be said that a substrate with a higher flatness is a substrate for mask blanks that is more suitable for drawing fine patterns. Substrates for mask blanks have a first main surface on which an exposure pattern (such as a wiring pattern) is formed after film formation, and a second main surface on which an exposure pattern is not formed, and the second main surface is adsorbed and held by the exposure machine. Of these, reflective masks are the mainstream for cutting-edge applications, so an extremely high level of flatness is required for the first main surface. Therefore, various local processing techniques for flattening are being considered in order to improve the flatness of the first main surface.
[0018] On the other hand, the exposure machine has a wavefront correction function, which optically corrects the surface shape of the substrate even if the substrate has low flatness, so that even if the substrate has low flatness, exposure results equivalent to those of a substrate with high flatness can be obtained.
[0019] In the mask blank substrate of the present invention, in a pseudo-TTV map obtained by adding together a height map of the first main surface and a height map of the second main surface, based on the respective positions on the least squares plane of the first main surface and the second main surface, a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate, and a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered on the intersection of the diagonals of the main surface of the substrate, are superimposed on each other to form a cross-shaped region, in which the difference between the maximum height and the minimum height of the TTV map excluding the primary component (TTV1) is 35 nm or less, and the difference between the maximum height and the minimum height of the TTV map excluding the primary component and the secondary component (TTV2) is 25 nm or less.
[0020] Specifically, the mask blank substrate of the present invention is (1) A substrate is arranged with a first main surface and a second main surface aligned in a substantially vertical direction, and a calculation area in the shape of a regular rectangular cylinder is set, the calculation area passing through the four sides of a 132 mm × 132 mm square along the four sides of the first main surface and the second main surface at the center of the first main surface and the second main surface, and extending in the horizontal direction; (2) In a state facing the first main surface, a portion within the calculation region is cut out from the first main surface to be used as a first region surface; (3) A vertical plane that passes through a reference point, which is an arbitrary point on the central axis of a regular square cylinder of the calculation area, and is perpendicular to the central axis is set as a reference plane, a rotation axis that passes through the reference point and is parallel to one of the four sides of the regular square that is the intersection line between the regular square cylinder of the calculation area and the vertical plane is set, and the substrate is rotated 180 degrees along the rotation axis from a state where the substrate is directly facing the first main surface, and in a state where the substrate is directly facing the second main surface, a portion within the calculation area is cut out from the second main surface to be used as a second area surface; (4) calculating a least squares plane on each of the first and second domain surfaces; (5) converting the first and second domain surfaces into a height map of the first domain surface and a height map of the second domain surface based on respective positions on the least squares plane of the first and second domain surfaces; (6) The height map of the second region surface is symmetrically moved with respect to a vertical plane that passes through the rotation axis in (3) and is aligned in the 90 degree direction of the rotation in (3) to obtain an inverted height map of the second region surface; (7) At each position (X coordinate, Y coordinate) on the reference plane, the height of the height map of the first region surface and the height of the inverted height map of the second region surface are added together to generate a pseudo-TTV map; (8) In a pseudo-TTV map, in a cross-shaped region formed when a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered on the intersection of the diagonals of the main surface of the substrate, It is preferable that the difference between the maximum height and the minimum height of the TTV1 map excluding the primary component (TTV1) is 35 nm or less, and the difference between the maximum height and the minimum height of the TTV2 map excluding the primary and secondary components (TTV2) is 25 nm or less.
[0021] The above (1) to (8) will be specifically described with reference to Figs. 1 to 4 for explaining the embodiment of the mask blank substrate of the present invention. First, in Fig. 1, (A) is a side view of the state in which the first main surface and the second main surface of the mask blank substrate are arranged along the vertical direction, and (B) is a front view of the first main surface located on the right side in (A). In (1), as shown in Fig. 1(A), the first main surface 1 and the second main surface 2 of the substrate 500, each having a square of 152 mm x 152 mm, are arranged along the approximately vertical direction, and a calculation area C of a regular square cylinder extending horizontally is set, which passes through the four sides of a 132 mm x 132 mm square along the four sides of the first main surface 1 and the second main surface 2 at the center of the first main surface 1 and the second main surface 2.
[0022] Next, in (2), as shown in Fig. 1(B), in a state facing the first main surface 1, a portion within the calculation region C is cut out from the first main surface 1 to define the first region surface 11. Here, for convenience, it is assumed that the first main surface 1 has a convex portion 11a, and the second main surface 2 also has a convex portion 21a, as shown in Fig. 2(B) described later.
[0023] 1(A) and 1(B), a vertical plane that passes through reference point P, which is an arbitrary point on the central axis CA of the square cylinder of calculation area C, and is perpendicular to the central axis CA is set as a reference plane S (here, reference plane S is a plane extending in the depth direction of the drawing). A rotation axis RA is set that passes through reference point P and is parallel to one of the four sides of the square that is the intersection line between the square cylinder of calculation area C and the vertical plane. Then, from a state directly facing first main surface 1, substrate 500 is rotated 180 degrees along rotation axis RA (with rotation axis RA as the center).
[0024] 2A is a side view of the mask blank substrate after rotation by 180 degrees, and (B) is a front view of the second main surface located on the right side in (A) after rotation. After the rotation of the substrate 500, as shown in FIG. 2B, in a state facing the second main surface 2, a portion within the calculation region C is cut out from the second main surface 2 to define the second region surface 21.
[0025] Next, in (4), least square planes are calculated for each of the first and second regions 11 and 21, and in (5), the first and second regions 11 and 21 are converted into a height map 111 of the first region as shown in Fig. 3(A) and a height map 211 of the second region as shown in Fig. 3(B), based on the positions on the least square planes of the first and second regions 11 and 21. In addition, in (6), the height map 211 of the second region is moved symmetrically with respect to a vertical plane V (here, the vertical plane V is a plane extending in the depth direction of the drawing) that passes through the rotation axis RA in (3) and is aligned along the 90 degree direction of the rotation in (3), as shown in Fig. 3(B), to obtain an inverted height map 211R of the second region as shown in Fig. 3(C). In addition, since the inverted height map 211R of the second area surface shown in Figure 3 (C) is obtained by symmetrically moving the height map 211, 21aR in the inverted height map 211R is not inverted in the height direction and is a convex portion similar to 21a.
[0026] Next, in (7), the height map 111 of the first area surface shown in Figure 3(A) is superimposed on the inverted height map 211R of the second area surface shown in Figure 3(C), and the height of the height map 111 of the first area surface and the height of the inverted height map 211R of the second area surface are added together at each position (X coordinate, Y coordinate) on the reference plane S shown in Figure 1(A) to create a pseudo TTV map (Z coordinate map) 3 as shown in Figure 4.
[0027] Next, in (8), for the pseudo-TTV map obtained in (7), a cross-shaped region 31 shown in FIG. 5(A) is cut out, which is formed when a first rectangular region (vertical region) 31a of 132 mm × 104 mm parallel to the four sides of the main surface of the substrate whose center is the intersection of the diagonals of the main surface (first main surface or second main surface) 10 of the substrate 500 as shown in FIG. 5(B) is superimposed on a second rectangular region (horizontal region) 31b of 104 mm × 132 mm perpendicular to the first rectangular region 31a and parallel to the four sides of the main surface of the substrate whose center is the intersection of the diagonals of the main surface (same main surface) 10 of the substrate 500 as shown in FIG. 5(C). The parameters (TTV1, TTV2) obtained by numerical processing of the pseudo-TTV of the pseudo-TTV map within this cross-shaped region 31 are evaluated.
[0028] The minimum area on the main surface of the substrate that may be used for exposure is a first rectangular area of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface, and a second rectangular area of 104 mm x 132 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate, and it is effective to target a cross-shaped area obtained by superimposing the two on each other for the pseudo TTV map. Therefore, in the present invention, this cross-shaped area is used as the target area for evaluation.
[0029] In the present invention, in a multi-component glass substrate used in EUVL, TTV is used as an index of the shape of a mask blank substrate that can be used well for exposure. In a pseudo-TTV map, TTV1 calculated from a TTV1 map excluding a simple first-order component, and TTV2 calculated from a TTV2 map excluding a somewhat complicated first-order component and second-order component, are important indexes that greatly affect exposure performance. In fitting a pseudo-TTV map, when a plane function approximated by a first-order polynomial (specifically, a function represented by the following formula (1)) or a curved surface function approximated by a polynomial up to second order (specifically, a function represented by the following formula (2)) is derived, the components of the first-order function are the first-order components, and the components of the second-order function are the second-order components.
[0030] Here, the method of calculating TTV1 and TTV2 will be described. First, a pseudo-TTV map (S TTV Next, the pseudo TTV map is approximated by the following equations (1) and (2).
[0031]
number
[0032] In the formula, a1, a2, b1, b2, b3, b4, and b5 are all constants. TTV ) to obtain the approximate formula S'(S' TTV1 , S' TTV2 ) and subtract the TTV1 map (S TTV1 ), and TTV2 map (S TTV2 )
[0033]
number
[0034] And the TTV1 map (S TTV1 ), and TTV2 map (S TTV2 ) are the differences between the maximum and minimum heights of TTV1 and TTV2, respectively.
[0035] The steeper the outer periphery shape, the more likely it is to have a negative effect on exposure. Such shapes can be considered to be composed mainly of second-order or higher components. Therefore, by evaluating TTV1, which excludes only the first-order components and leaves the second-order or higher components, it is possible to avoid exposure defects caused by steep outer periphery shapes. In addition, the wavefront correction function of an exposure machine is usually well approximated up to the second-order components. In other words, a substrate with a poor pseudo-TTV calculated by excluding components up to the second-order components can be identified as a substrate that is difficult to correct using the wavefront correction function, and by evaluating TTV2, which excludes the first-order and second-order components, it is possible to select a substrate that is easy to correct using the wavefront correction function.
[0036] The shape of the main surface of the mask blank substrate can be measured using, for example, a laser interferometer, although there is no particular limitation. The shape that can be measured by a laser interferometer is the raw data of the height map of the main surface of the substrate, and in this case, the reference for the height is the stage on which the substrate is placed during measurement. In the present invention, the least squares plane of the main surface (the least squares plane of the surface or height map) is calculated for the height map of the main surface of the substrate, and the height map is corrected to one based on the least squares plane, thereby eliminating the influence of the shape of the stage on which the substrate is placed.
[0037] Among the height maps corrected in this way, the inverted height map of the second region surface obtained by symmetrically moving the height map of the second region surface with respect to a plane passing through the rotation axis in (3) and aligned in the 90 degree direction of the rotation in (3) does not change the positive and negative of the height direction, but both sides of the direction perpendicular to the rotation axis in (3) are inverted. The pseudo-TTV map can be calculated by adding up the inverted height maps of the first main surface and the second main surface so as to obtain the plate thickness distribution of the mask blank substrate. Here, the pseudo-TTV is the difference between the maximum value (maximum height) and the minimum value (minimum height) within a predetermined range.
[0038] The pseudo-TTV of the mask blanks substrate of the present invention is such that the difference (TTV1) between the maximum height and the minimum height of the TTV1 map (pseudo-TTV1 map) excluding the primary component is 35 nm or less, preferably 30 nm or less, and more preferably 25 nm or less. If TTV1 is 35 nm or less, such a mask blanks substrate is a mask blanks substrate that can advantageously realize exposure with good transfer accuracy in exposure using an exposure mask obtained from the mask blanks substrate via the mask blanks. On the other hand, if TTV1 is greater than 35 nm, such a mask blanks substrate is disadvantageous in terms of transfer accuracy.
[0039] Furthermore, the pseudo-TTV of the mask blanks substrate of the present invention has a difference (TTV2) between the maximum height and the minimum height of a TTV2 map (pseudo-TTV2 map) excluding primary and secondary components, which is 25 nm or less, preferably 20 nm or less, and more preferably 18 nm or less. Such a mask blanks substrate is a mask blanks substrate that can advantageously realize exposure with good transfer accuracy in exposure using an exposure mask obtained from the mask blanks substrate via the mask blanks.
[0040] TTV1 is calculated from a TTV1 map obtained by removing the first-order component from the pseudo-TTV map, and TTV1 can be said to be similar to flatness, but in the present invention, the upper limit (threshold) of TTV2 calculated from a TTV2 map obtained by removing (relaxing) the first-order and second-order components from the pseudo-TTV map is set to 25 nm or less. TTV2 reflects the actual flatness at the time of exposure better than TTV1, and a mask blank substrate in which TTV1 and TTV2 are within a predetermined range is a mask blank substrate that can achieve good exposure when actually subjected to exposure, and photomask blanks with high exposure performance can be provided.
[0041] Conventionally, for example, a 138 mm×138 mm range parallel to the four sides of the main surface of the substrate centered on the intersection of the diagonals of the main surface was evaluated, but this range extended not only to the area used for exposure but also to the area including the part of the main surface on the side that is vacuum-adsorbed to the exposure device that is vacuum-adsorbed to the exposure device. In the present invention, the cross-shaped area obtained by overlapping the two 132 mm×104 mm areas described above is evaluated. This cross-shaped area is narrower than the conventional range, but the area outside the cross-shaped area is not usually used for exposure and is likely to have a high degree of flatness.
[0042] The mask blank substrate of the present invention has a TTV1 of 35 nm or less and a TTV2 of 25 nm or less in the above-mentioned cross-shaped region, and is compatible with not only the conventional NA0.33 generation but also the NA0.55 generation, which requires stricter flatness, and can be suitably used as a mask blank substrate for next-generation EUV exposure equipment.
[0043] Furthermore, at least one of the flatness in the cross-shaped region of the first main surface and the flatness in the cross-shaped region of the second main surface of the mask blanks substrate of the present invention, preferably the flatness in the cross-shaped region of the first main surface when the side on which the optical film is formed is the first main surface and the side vacuum-adsorbed to the exposure device is the second main surface, is preferably 35 nm or less, more preferably 20 nm or less, and even more preferably 18 nm or less. Such a mask blanks substrate is a mask blanks substrate that can more advantageously realize exposure with good transfer accuracy in exposure using an exposure mask obtained from the mask blanks substrate via the mask blanks.
[0044] Next, a method for producing a substrate for a mask blank according to the present invention will be described. The method for producing a mask blank substrate of the present invention includes a local processing step for at least one of the first and second main surfaces of a mask blank substrate, and a finish polishing step following the local processing step.
[0045] In the manufacture of a mask blank substrate, a raw material substrate for the mask blank substrate is prepared from a glass ingot before the local processing step. The raw material substrate for the mask blank substrate is usually prepared by first cutting a glass ingot into a predetermined shape, processing the outer shape, and then polishing the main surface and end face. The polishing can be performed in several steps, such as rough polishing, precision polishing, and ultra-precision polishing. This polishing can be performed using a polishing cloth and abrasive. The abrasive is not particularly limited, but can be, for example, an aqueous dispersion of cerium oxide having an average primary particle size of 10 to 100 nm, an aqueous dispersion of silica nanoparticles having an average primary particle size of 10 to 100 nm (aqueous dispersion of colloidal silica), or the like.
[0046] The shape of the surface obtained by only local processing is not flat, and usually has a shape that cancels the change in the shape of the surface in the finish polishing performed thereafter (generally a convex shape (a shape in which the center of the main surface protrudes) or a concave shape (a shape in which the center of the main surface is recessed), etc.), and even if the flatness of the shape of the surface obtained by only local processing is evaluated, the evaluation result will be different from the evaluation result of the shape of the main surface of the mask blanks substrate finally obtained. The change in the shape of the main surface caused by the finish polishing performed under specified polishing conditions after the local processing is reproducible, and by grasping the change in the shape of the main surface after the finish polishing under specified polishing conditions and applying this to the shape of the main surface after the local processing, the shape of the surface obtained after the finish polishing performed under specified polishing conditions can be evaluated at the stage of local processing before the finish polishing, and the quality of the shape of the main surface obtained by the finish polishing can be evaluated. The local processing step can be repeated until the specified shape is obtained.
[0047] In the manufacture of a mask blank substrate of the present invention, the local processing step includes: (A) locally processing at least one of the first main surface and the second main surface; (B) measuring the shape of the locally machined main surface after the (A) step as the shape of the main surface before the finish polishing step; (C) a step of predicting a shape of the locally machined main surface after the finish polishing step by applying the previously determined change in surface shape during the finish polishing step to the shape of the main surface before the finish polishing step obtained in the step (B); (D) a step of evaluating whether the shape after the finish polishing step predicted in the step (C) is a shape that gives a predetermined TTV; It is preferred that the compound contains
[0048] In step (A), the main surface is locally processed, and the local processing is performed under predetermined processing conditions, taking into consideration the shape of the main surface before the local processing and the change in the shape of the main surface in the finish polishing process, so that the main surface has a predetermined shape. Specifically, for example, when the main surface is changed to a convex shape by the finish polishing, the main surface is preferably shaped to cancel this change (e.g., a low convex shape or a concave shape) in consideration of this change, and when the main surface is changed to a concave shape by the finish polishing, the main surface is preferably shaped to cancel this change (e.g., a shallow concave shape or a convex shape) in consideration of this change. Before the local processing, the shape of the main surface is appropriately measured, and the measurement can be performed using, for example, a laser interferometer, but is not particularly limited thereto.
[0049] In the local processing, a relatively convex portion of the main surface of the mask blank substrate is selectively removed. The local processing can be performed by polishing using an abrasive cloth and an abrasive. The abrasive is not particularly limited, but for example, an aqueous dispersion of cerium oxide having an average primary particle size of 10 to 100 nm, an aqueous dispersion of silica nanoparticles having an average primary particle size of 10 to 100 nm (aqueous dispersion of colloidal silica), etc. can be used. In addition, a method such as magnetorheological finishing (MRF) can also be applied to the local processing.
[0050] In step (B), the shape of the main surface after step (A), i.e., after actual local processing, is measured as the shape of the main surface before the finish polishing step. This measurement can be performed using, but is not limited to, a laser interferometer, for example.
[0051] In step (C), the shape of the locally machined main surface after the finish polishing process is predicted by applying the previously determined change in surface shape during the finish polishing process to the shape of the main surface before the finish polishing process obtained in step (B).
[0052] Specifically, the change in the surface shape of the main surface before and after the finish polishing process (the change in the surface shape after the finish polishing process relative to the surface shape after the local processing process) is grasped, and this change can be grasped, for example, from the mask blanks substrate on which the local processing has been performed, by selecting another mask blanks substrate having a main surface with a similar shape, and performing a predetermined finish polishing on this other mask blanks substrate, from the shape of the main surface obtained. The grasp of this change in the surface shape can also be performed by simulation. In this case, the other mask blanks substrate is preferably one whose main surface shape is a concave shape, which is the target shape in the local processing process, and is preferably one whose main surface has a flatness of less than 300 nm. The change in the surface shape in the finish polishing process grasped in advance is selected according to the shape of the main surface after local processing obtained in the (B) process.
[0053] Here, for example, when the shape of the pseudo-TTV map of the main surface after the local processing process of the main surface is S1, and the change in shape of the pseudo-TTV map of the main surface when a predetermined finish polishing is performed is ΔS, the following formula is obtained. S1+ΔS=S2 Thus, the shape of the locally processed main surface after the finish polishing process can be predicted as the shape (S2) of the pseudo TTV map (predicted pseudo TTV map) of the main surface after the finish polishing process.
[0054] In step (D), it is evaluated whether the shape after the finish polishing step predicted in step (C) is a shape that provides a predetermined flatness, specifically, whether it is a shape that provides a predetermined TTV. As a method of this evaluation, a technique can be used in which the shape of the main surface is measured and a predetermined value calculated from the measured shape or a predetermined value obtained by mathematically processing the measured shape is evaluated.
[0055] In step (D), for example, in a pseudo-TTV map obtained by adding together a height map of the first main surface and a height map of the second main surface based on the respective positions on the least-squares plane of each of the first and second main surfaces of a mask blank substrate, it is possible to evaluate whether or not the difference (TTV1) between the maximum height and the minimum height of the TTV1 map excluding the primary component (pseudo-TTV1 map) is 35 nm or less and the difference (TTV2) between the maximum height and the minimum height of the TTV2 map excluding the primary component and the secondary component (pseudo-TTV2 map) is 25 nm or less within a cross-shaped region formed when a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered on the intersection of the diagonals of the main surface of the substrate.
[0056] Specifically, in step (D), (1) A substrate is arranged with a first main surface and a second main surface aligned in a substantially vertical direction, and a calculation area in the shape of a regular rectangular cylinder is set, the calculation area passing through the four sides of a 132 mm × 132 mm square along the four sides of the first main surface and the second main surface at the center of the first main surface and the second main surface, and extending in the horizontal direction; (2) In a state facing the first main surface, a portion within the calculation region is cut out from the first main surface to be used as a first region surface; (3) A vertical plane that passes through a reference point, which is an arbitrary point on the central axis of a regular square cylinder of the calculation area, and is perpendicular to the central axis is set as a reference plane, a rotation axis that passes through the reference point and is parallel to one of the four sides of the regular square that is the intersection line between the regular square cylinder of the calculation area and the vertical plane is set, and the substrate is rotated 180 degrees along the rotation axis from a state where the substrate is directly facing the first main surface, and in a state where the substrate is directly facing the second main surface, a portion within the calculation area is cut out from the second main surface to be used as a second area surface; (4) calculating a least squares plane on each of the first and second domain surfaces; (5) converting the first and second domain surfaces into a height map of the first domain surface and a height map of the second domain surface based on respective positions on the least squares plane of the first and second domain surfaces; (6) The height map of the second region surface is symmetrically moved with respect to a vertical plane that passes through the rotation axis in (3) and is aligned in the 90 degree direction of the rotation in (3) to obtain an inverted height map of the second region surface; (7) At each position (X coordinate, Y coordinate) on the reference plane, the height of the height map of the first region surface and the height of the inverted height map of the second region surface are added together to generate a predicted pseudo-TTV map; (8) In a predicted pseudo-TTV map, in a cross-shaped region formed when a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered on the intersection of the diagonals of the main surface of the substrate, It can be evaluated whether the difference (TTV1') between the maximum height and the minimum height of the TTV1' map (predicted pseudo TTV1' map) excluding the primary component is 35 nm or less, and whether the difference (TTV2') between the maximum height and the minimum height of the TTV2' map (predicted pseudo TTV2' map) excluding the primary and secondary components is 25 nm or less.
[0057] In step (D), if the shape of the main surface predicted in step (C) has a predetermined flatness, the process can proceed to a finish polishing process. On the other hand, if the shape does not have the predetermined flatness in step (D), the local processing step, specifically the local processing step including steps (A) to (D), can be carried out again, and the local processing step, specifically the local processing step including steps (A) to (D), can be repeated until the shape of the main surface predicted in step (C) is evaluated in step (D) as having the predetermined flatness.
[0058] The surface defect level obtained by only local processing may not be sufficient, particularly for mask blanks substrates for cutting-edge products, and in the manufacture of mask blanks substrates, a finish polishing step is generally performed following the local processing step. In the manufacturing method of the mask blanks substrate of the present invention, a finish polishing step is also performed following the local processing step. The shape of the main surface of the mask blanks substrate obtained after the finish polishing step is also measured using, but is not particularly limited to, a laser interferometer, for example. The shape of the main surface of the mask blanks substrate obtained after the finish polishing step can be evaluated by creating a pseudo TTV map as necessary, and evaluating the difference between the maximum height and the minimum height of the TTV1 map (TTV1) and the difference between the maximum height and the minimum height of the TTV2 map (TTV2).
[0059] For example, it is relatively easy to obtain a mask blank substrate with a TTV1 of about 100 nm by repeating general local processing about twice, but with conventional methods, it is difficult to achieve a TTV1 of 35 nm or less and a TTV2 of 25 nm or less in the above-mentioned cross-shaped region.
[0060] According to the present invention, it is possible to provide a mask blanks substrate having high flatness during exposure of an exposure mask obtained by forming a film and a pattern on the mask blanks substrate, and such a mask blanks substrate can be manufactured with good productivity by evaluating the TTV using the pseudo-TTV map. Furthermore, by evaluating the TTV using the pseudo-TTV map, the flatness of the mask blanks substrate after finish polishing can be estimated as a predicted pseudo-TTV map, and thus, it is possible to provide a mask blanks substrate having good flatness by evaluating the pseudo-TTV map of the mask blanks substrate after finish polishing using the predicted pseudo-TTV map.
[0061] According to the present invention, it is also possible to evaluate whether the flatness of an exposure mask obtained by forming a film and a pattern on a mask blank substrate is good or not by using the pseudo TTV map of the mask blank substrate after finish polishing. EXAMPLES
[0062] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0063] [Example 1] Six glass substrates (size of first and second main surfaces: 152 mm × 152 mm square, thickness 6.35 mm) formed of SiO2 and TiO2 (TiO2 concentration: about 7 mass%) were prepared. The end faces (four faces that are not the main surfaces) of the glass substrates were chamfered and ground, and further, the two main surfaces were roughly polished and finely polished with a polishing solution containing cerium oxide abrasive grains. Thereafter, the six glass substrates (substrates 1-1 to 1-6) were set in a carrier of a double-sided polishing machine to which a suede-type soft polishing cloth was applied, and the first and second main surfaces were ultra-precisely polished using a polishing solution containing colloidal silica abrasive grains. After the ultra-precise polishing, the substrates were washed with a cleaning solution containing KOH to remove silica nanoparticles, and after drying, the shapes of the first and second main surfaces were measured using a surface shape measuring device (UltraFlat, manufactured by Tropel).
[0064] Next, a local processing step was carried out. First, the processing conditions for the local processing were determined based on the shape of the obtained main surface, and the first main surface and the second main surface of the glass substrate were locally processed by a local processing device based on the determined processing conditions (step (A)). The local processing device used was the local processing device described in JP 2010-194705 A (Patent Document 2). The local processing using this device polishes the entire surface of the substrate while controlling the moving speed of a fine polishing tool, and the polishing tool is moved slowly in relatively convex parts and moved quickly in relatively concave parts to obtain a target shape. The processing tool of the local processing device was a wool felt buff, and the polishing slurry used was a mixture of silica nanoparticles (AJ-3540, manufactured by Nissan Chemical Co., Ltd.) and a small amount of defoaming agent (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0065] After the local processing, the glass substrate was washed with a cleaning solution containing KOH to remove the silica nanoparticles, and then dried. The shapes of the first and second main surfaces were measured using a surface profiler (UltraFlat, manufactured by Tropel) (step (B)).
[0066] Here, in order to grasp the change in the shape of the main surface after the finish polishing with respect to the surface after the local processing, another glass substrate was used and similarly subjected to the local processing and further subjected to the same finish polishing as the finish polishing described later, so as to grasp the change in the shape of the surface before and after the finish polishing process in advance. After that, for the six glass substrates after the local processing (substrate 1-1 to substrate 1-6), the grasped change in the shape of the main surface was applied to the shapes of the glass substrates after the local processing to predict the shape of the surface after the finish polishing (step (C)).
[0067] Next, the predicted shape after the final polishing process was evaluated as to whether it was a shape that gave a specified TTV (step (D)). The surface shape of the glass substrate after local processing and the predicted surface shape after final polishing were evaluated within a cross-shaped area formed when a first rectangular area of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate was superimposed on a second rectangular area of 104 mm x 132 mm perpendicular to the first rectangular area and centered on the intersection of the diagonals of the main surface of the substrate and parallel to the four sides of the main surface of the substrate.
[0068] Here, the evaluation of whether or not a shape provides a predetermined TTV is as follows: (1) A substrate is arranged with a first main surface and a second main surface aligned in a substantially vertical direction, and a calculation area in the shape of a regular rectangular cylinder is set, the calculation area passing through the four sides of a 132 mm × 132 mm square along the four sides of the first main surface and the second main surface at the center of the first main surface and the second main surface, and extending in the horizontal direction; (2) In a state facing the first main surface, a portion within the calculation region is cut out from the first main surface to be used as a first region surface; (3) A vertical plane that passes through a reference point, which is an arbitrary point on the central axis of a regular square cylinder of the calculation area, and is perpendicular to the central axis is set as a reference plane, a rotation axis that passes through the reference point and is parallel to one of the four sides of the regular square that is the intersection line between the regular square cylinder of the calculation area and the vertical plane is set, and the substrate is rotated 180 degrees along the rotation axis from a state where the substrate is directly facing the first main surface, and in a state where the substrate is directly facing the second main surface, a portion within the calculation area is cut out from the second main surface to be used as a second area surface; (4) calculating a least squares plane on each of the first and second domain surfaces; (5) converting the first and second domain surfaces into a height map of the first domain surface and a height map of the second domain surface based on respective positions on the least squares plane of the first and second domain surfaces; (6) The height map of the second region surface is symmetrically moved with respect to a vertical plane that passes through the rotation axis in (3) and is aligned in the 90 degree direction of the rotation in (3) to obtain an inverted height map of the second region surface; (7) At each position (X coordinate, Y coordinate) on the reference plane, the height of the height map of the first region surface and the height of the inverted height map of the second region surface are added together to generate a predicted pseudo-TTV map; (8) In a predicted pseudo-TTV map, in a cross-shaped region formed when a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered on the intersection of the diagonals of the main surface of the substrate, The evaluation was based on whether the difference between the maximum height and the minimum height of the TTV1' map excluding the primary component (TTV1') was 35 nm or less, and whether the difference between the maximum height and the minimum height of the TTV2' map excluding the primary and secondary components (TTV2') was 25 nm or less.
[0069] Regarding the surface shape after the first local processing step, a predicted shape of the main surface after finish polishing of each glass substrate (predicted pseudo-TTV map) was created, and the TTV1' and TTV2' in the predicted pseudo-TTV1' map and the predicted pseudo-TTV2' map were evaluated. The results are shown in Table 1.
[0070] For all the substrates, TTV1' and TTV2' did not become equal to or less than the predetermined value in the first processing. Therefore, steps (A) to (D) were repeated to perform local processing until TTV1' and TTV2' became equal to or less than the predetermined value. Table 1 shows the values at which TTV1' and TTV2' became equal to or less than the predetermined value and the number of steps (A) to (D) performed until TTV1' and TTV2' became equal to or less than the predetermined value. As a result, for all the glass substrates, TTV1' was 35 nm or less and TTV2' was 25 nm or less, so it was evaluated that a shape of the main surface having a predetermined flatness could be obtained, and a finish polishing process was performed.
[0071] The glass substrate was set on a carrier of a polishing device with a suede-type soft polishing cloth applied, polished with a polishing solution of colloidal silica, and after polishing, washed with a cleaning solution containing KOH to remove the colloidal silica, and dried to obtain a mask blank substrate. The shapes of the first and second main surfaces of the obtained mask blank substrate were measured with a surface shape measuring device (UltraFlat, manufactured by Tropel), and a pseudo TTV map was created to evaluate TTV1, TTV2, and the flatness of the first main surface. The results are shown in Table 1.
[0072] [Table 1]
[0073] [Comparative Example 1] Fifteen glass substrates (size of first and second main surfaces: 152 mm × 152 mm square, thickness 6.35 mm) formed of SiO2 and TiO2 (TiO2 concentration: about 7 mass%) were prepared. The end faces (four faces that are not the main surfaces) of the glass substrates were chamfered and ground, and further, the two main surfaces were roughly polished and finely polished with a polishing solution containing cerium oxide abrasive grains. Thereafter, the 15 glass substrates (substrates C1-1 to C1-15) were set in a carrier of a double-sided polishing machine to which a suede-type soft polishing cloth was applied, and the first and second main surfaces were ultra-precisely polished using a polishing solution containing colloidal silica abrasive grains. After the ultra-precise polishing, the substrates were washed with a cleaning solution containing KOH to remove silica nanoparticles, and after drying, the shapes of the first and second main surfaces were measured using a surface shape measuring device (UltraFlat, manufactured by Tropel).
[0074] Next, a local processing step was carried out. First, the processing conditions for the local processing were determined based on the shape of the obtained main surface, and the first main surface and the second main surface of the glass substrate were locally processed by a local processing device based on the determined processing conditions. The local processing device used was the local processing device described in JP 2010-194705 A (Patent Document 2). The local processing using this device polishes the entire surface of the substrate while controlling the moving speed of a fine polishing tool, and the polishing tool is moved slowly in relatively convex parts and moved quickly in relatively concave parts to obtain a target shape. The processing tool of the local processing device was a wool felt buff, and the polishing slurry used was a mixture of silica nanoparticles (AJ-3540, manufactured by Nissan Chemical Co., Ltd.) and a small amount of defoaming agent (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0075] After the local processing, the glass substrate was washed with a cleaning solution containing KOH to remove the silica nanoparticles, and then dried, and the shapes of the first main surface and the second main surface were measured with a surface profiler (UltraFlat, manufactured by Tropel).
[0076] Here, in order to grasp the change in the shape of the main surface after the finish polishing with respect to the surface after the local processing, another glass substrate was used and similarly subjected to the local processing, and further subjected to the same finish polishing as the finish polishing described later, to grasp the change in the shape of the surface before and after the finish polishing process in advance. After that, for 15 glass substrates after the local processing (substrates C1-1 to C1-15), the grasped change in the shape of the main surface was applied to the shape of the main surface of the glass substrate after the local processing, and the shape of the surface after the finish polishing was predicted.
[0077] Next, the shape of the predicted surface after the finish polishing process was evaluated as to whether it was a shape that gave a predetermined TTV. The shape of the surface of the glass substrate after the local processing and the shape of the predicted surface after the finish polishing were evaluated within a cross-shaped area formed when a first rectangular area of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate centered on the intersection of the diagonals of the main surface of the substrate and a second rectangular area of 104 mm x 132 mm parallel to the four sides of the main surface of the substrate centered on the intersection of the diagonals of the main surface of the substrate were superimposed. The evaluation of whether the shape gave a predetermined TTV was performed in the same manner as in Example 1.
[0078] Regarding the surface shape after the first local processing step, a predicted shape of the main surface after finish polishing of each glass substrate (predicted pseudo-TTV map) was created, and the TTV1' and TTV2' in the predicted pseudo-TTV1' map and the predicted pseudo-TTV2' map were evaluated. The results are shown in Table 2.
[0079] For all of the substrates, the TTV1' and TTV2' did not become equal to or less than the predetermined values in the first processing, but the finish polishing process was still carried out.
[0080] The glass substrate was set on a carrier of a polishing device with a suede-type soft polishing cloth applied, polished with a polishing solution of colloidal silica, and after polishing, washed with a cleaning solution containing KOH to remove the colloidal silica, and dried to obtain a mask blank substrate. The shapes of the first and second main surfaces of the obtained mask blank substrate were measured with a surface shape measuring device (UltraFlat, manufactured by Tropel), and a pseudo TTV map was created to evaluate TTV1 and TTV2. The results are shown in Table 2.
[0081] [Table 2]
[0082] The mask blank substrates obtained in the examples had a TTV1 of 35 nm or less and a TTV2 of 25 nm or less. From such mask blank substrates, an exposure mask with extremely good flatness when adsorbed to an exposure tool can be obtained, and it is expected that good exposure results will be obtained as an exposure mask for next-generation high NA exposure tools. [Explanation of symbols]
[0083] 10 Main surface 1 First major surface 11 First area surface 11a Convex part 111 Height map of the first area surface 2 Second main surface 21 Second area surface 21a, 21aR convex part 211 Second area surface height map 211R Inverted height map of the second area surface 3 Pseudo TTV map 31 Cross-shaped area 31a First rectangular area 31b Second rectangular area 500 boards C calculation area CA center axis P reference point RA Rotational Axis S reference plane V vertical plane
Claims
1. A mask blank substrate having two main surfaces, a first main surface and a second main surface, each of which is 152 mm × 152 mm square, and a thickness of 6.35 mm, A pseudo-TTV map obtained by adding a height map of the first main surface and a height map of the second main surface based on the positions of the first main surface and the second main surface on the least squares plane, Within a cross-shaped region formed when a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered at the intersection of the diagonals of the main surface of the substrate, When a plane function approximated by a first-order polynomial is derived in the fitting of the pseudo-TTV map, the difference (TTV1) between the maximum height and the minimum height of the TTV1 map excluding the first-order component is 35 nm or less, and when a curved surface function approximated by a polynomial up to the second order is derived in the fitting of the pseudo-TTV map, the difference (TTV2) between the maximum height and the minimum height of the TTV2 map excluding the first-order component and the second-order component is 25 nm or less. A substrate for mask blanks comprising:
2. 2. The mask blank substrate according to claim 1, wherein the flatness within the cross-shaped region of the first main surface is 35 nm or less.
3. A method for manufacturing a mask blank substrate having two main surfaces, a first main surface and a second main surface, each of which is 152 mm × 152 mm square, and a thickness of 6.35 mm, comprising the steps of: A local processing step for at least one of the first main surface and the second main surface, and a finish polishing step subsequent to the local processing step, The local processing step includes: (A) locally processing at least one of the first main surface and the second main surface; (B) measuring the shape of the locally machined main surface after the step (A) as the shape of the main surface before the finish polishing step; (C) predicting a shape of the locally processed main surface after the finish polishing process by applying a previously determined change in surface shape during the finish polishing process to the shape of the main surface before the finish polishing process obtained in the process (B); (D) a step of evaluating whether the shape after the finish polishing step predicted in the step (C) is a shape that gives a predetermined TTV; A method for producing a substrate for a mask blank, comprising:
4. The shape that gives the predetermined TTV in the step (D) is (1) arranging the substrate with the first main surface and the second main surface aligned in a substantially vertical direction, and setting a calculation region in the shape of a regular rectangular cylinder extending in a horizontal direction passing through the four sides of a 132 mm × 132 mm square along the four sides of the first main surface and the second main surface at the center of the first main surface and the second main surface; (2) in a state facing the first main surface, a portion within the calculation area is cut out from the first main surface to form a first area surface; (3) A vertical plane that passes through a reference point, which is an arbitrary point on the central axis of a regular square cylinder of the calculation area, and is perpendicular to the central axis is set as a reference plane, a rotation axis that passes through the reference point and is parallel to any one of the four sides of the regular square that is the intersection line between the regular square cylinder of the calculation area and the vertical plane is set, and the substrate is rotated 180 degrees along the rotation axis from a state where the substrate is directly facing the first main surface, and in a state where the substrate is directly facing the second main surface, a portion within the calculation area is cut out from the second main surface to be a second area surface; (4) calculating a least squares plane on each of the first and second domain surfaces; (5) converting the first and second domain surfaces into a height map of the first domain surface and a height map of the second domain surface based on respective positions on the least squares plane of the first and second domain surfaces; (6) The height map of the second region surface is symmetrically moved with respect to a vertical plane passing through the rotation axis and aligned in the 90 degree direction of the rotation to obtain an inverted height map of the second region surface; (7) At each position (X coordinate, Y coordinate) on the reference plane, a height of the height map of the first area surface and a height of the inverted height map of the second area surface are added together to generate a predicted pseudo-TTV map; (8) In the predicted pseudo-TTV map, a first rectangular region of 132 mm x 104 mm parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonals of the main surface of the substrate is superimposed on a second rectangular region of 104 mm x 132 mm perpendicular to the first rectangular region and centered at the intersection of the diagonals of the main surface of the substrate, in a predicted pseudo-TTV map within a cross-shaped region formed by superimposing the first rectangular region and the second rectangular region of 104 mm x 132 mm parallel to the four sides of the main surface of the substrate, A shape in which the difference (TTV1') between the maximum height and the minimum height of a TTV1' map excluding the first-order component when a plane function approximated by a first-order polynomial is derived in fitting the predicted pseudo-TTV map is 35 nm or less, and the difference (TTV2') between the maximum height and the minimum height of a TTV2' map excluding the first-order component and the second-order component when a surface function approximated by a first-order polynomial is derived in fitting the predicted pseudo-TTV map is 25 nm or less. The method according to claim 3, wherein
Citation Information
Patent Citations
Method of processing synthetic quartz glass substrate for semiconductor
JP2010194705A
Substrate for mask blank, mask blank, methods for manufacturing substrate for mask blank and mask blank, method for manufacturing transfer mask, and method for manufacturing semiconductor device
WO2016098452A1
Cited By
Substrate with conductive film, reflective mask blank, reflective mask, and semiconductor device manufacturing method
WO2026164206A1