Film

A film with a resin layer containing spherical silica particles of specific properties addresses the issue of reduced transparency in anti-blocking films by minimizing light scattering and friction, enhancing both transparency and anti-blocking capabilities.

JP2024170300APending Publication Date: 2024-12-06AGC INC +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024081011
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-17
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing films with anti-blocking properties suffer from reduced transparency due to surface irregularities formed to prevent blocking, leading to increased friction and potential damage during unwinding.

Method used

A film comprising a resin layer with spherical silica particles having a specific BET surface area of 4.5 m²/g or less, a median diameter of 1.0 to 30.0 μm, circularity of 0.85 or more, and a content of 0.1 to 60.0% by mass, which minimizes light scattering and surface roughness while maintaining anti-blocking properties.

Benefits of technology

The film achieves high transparency with improved anti-blocking properties by reducing light scattering and friction, suitable for optical applications such as liquid crystal displays and organic EL displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170300000001
    Figure 2024170300000001
  • Figure 2024170300000002
    Figure 2024170300000002
  • Figure 2024170300000003
    Figure 2024170300000003
Patent Text Reader

Abstract

To provide a film having high transparency while imparting anti-blocking property to the film.SOLUTION: A film includes a resin layer containing a resin and spherical silica particles, wherein a BET specific surface area of the spherical silica particles is 4.5 m2 / g or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film, and more particularly to a film suitable for optical applications. [Background technology]

[0002] In order to protect the image display surface of a display or the surface of a molded product from scratches, a film with a hard coat is attached. In addition, optical films such as polarizing plate protective films are used in display devices such as liquid crystal display devices and organic EL display devices.

[0003] Due to the smooth surface of the transparent substrate, these various resin films tend to have the front and back of the film stick together (blocking) when wound into a roll, and when the film is unwound from the roll, friction caused by blocking occurs, which can damage the film surface.

[0004] As a method for improving blocking, a coating film containing inert particles is formed on a transparent substrate, and unevenness is created on the surface of the film, thereby increasing the surface roughness of the film.

[0005] For example, Patent Document 1 proposes forming a film using an active energy ray-curable composition containing an active energy ray-curable compound (A) and silica particles (B). Patent Document 1 describes that the silica particles (B) are produced by a wet method, are obtained by pulverizing secondary aggregates of silica particles having a primary average particle size, and have an average particle size of 50 nm to 500 nm.

[0006] Patent Document 2 proposes a transparent electrode film including a laminate having a laminated structure in which a resin layer (B) is laminated directly or via one or more other layers on at least one surface of a light-transmitting substrate layer (A). Patent Document 2 describes that the resin layer (B) is a layer obtained by curing a curable composition (S) containing particles (R) and a curable compound (Q) that exhibits curability by active energy rays, and that particles (R) having an average particle diameter (median diameter) of 1000 nm or less are used. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6508559 [Patent Document 2] Patent No. 7078169 Summary of the Invention [Problem to be solved by the invention]

[0008] When projections and recesses are formed on the surface of a film, the blocking resistance improves but the transparency of the film tends to decrease. An object of the present invention is to provide a film that has high transparency while being endowed with antiblocking properties. [Means for solving the problem]

[0009] As a result of intensive research conducted by the present inventors to solve the above problems, 2 The inventors have found that the above problems can be solved by using the following spherical silica particles, and have completed the present invention.

[0010] The present invention relates to the following (1) to (13). (1) A resin layer containing a resin and spherical silica particles, the BET specific surface area of ​​the spherical silica particles being 4.5 m 2 / g or less of the film. (2) The median diameter (D50 ) is 1.0 to 30.0 μm. (3) The film according to (1) above, wherein the spherical silica particles have a circularity of 0.85 or more. (4) The film according to (1) above, wherein the content of the spherical silica particles in the resin layer is 0.1 to 60.0% by mass. (5) The BET specific surface area of ​​the spherical silica particles is 4.0 m 2 / g or less. (6) The film according to (1) above, wherein the resin has a refractive index of 1.40 to 1.50. (7) The film according to (1) above, further comprising a transparent substrate layer, and the resin layer is laminated on at least one surface of the transparent substrate layer directly or via one or more other layers. (8) The film according to (1) above, having a dynamic friction coefficient of 0.80 or less. (9) The film according to (1) above, having a haze of 20.0% or less. (10) The film according to (1) above, having a thickness of 1.0 to 100 μm. (11) The film according to (1) above, which is an optical film. (12) A display device having the film according to any one of (1) to (11) above. (13) The display device according to (12) above, which is a liquid crystal display device or an organic EL display. Effect of the Invention

[0011] According to the present invention, a film that combines antiblocking properties with high transparency can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described below, but the present invention is not limited to the examples in the following description. In this specification, the symbol "to" indicating a numerical range means that the numerical range includes the numerical ranges before and after the symbol as the lower and upper limits.

[0013] The film of the present invention has a resin layer containing a resin and spherical silica particles. The resin layer is located on at least one surface of the film of the present invention, and the film may be composed of only the resin layer, or may include any layer laminated on the resin layer. Each component will be described below.

[0014] <Resin layer> (Spherical silica particles) The spherical silica particles contained in the film of the present invention are solid silica particles having a BET specific surface area of ​​4.5 m 2 / g or less. The BET specific surface area of ​​the spherical silica particles is 4.5 m 2 / g or less, the presence of pores in the particles is reduced, and the spherical silica particles become close to non-porous. Since the number of pores in the spherical silica particles is reduced, light scattering caused by the pores is less likely to occur, and the inclusion of spherical silica particles forms irregularities on the surface of the resin layer, imparting anti-blocking properties to the film and resulting in a highly transparent film that is less likely to scatter light. The BET specific surface area of ​​spherical silica particles is 4.0m 2 / g or less, and 3.5m 2 / g or less is more preferable, and 3.0m 2 The BET specific surface area of ​​the spherical silica particles is preferably 0.09 m 2 / g or more, and 0.20m 2 / g or more is more preferable, and 0.30m 2 More preferably, the BET specific surface area of ​​the spherical silica particles is 0.09 to 4.5 m / g or more. 2 / g range is preferred.

[0015] The BET specific surface area can be calculated using the BET theory after obtaining an adsorption isotherm by a nitrogen adsorption method.

[0016] In addition, because the silica particles are spherical, the roughness of the film surface is reduced, thereby reducing frictional force, and the area of ​​the interface between the resin and the silica particles is minimized, making it difficult for light to be reflected, thereby maintaining transparency.

[0017] The circularity of the spherical silica particles is preferably 0.85 or more. When the circularity is 0.85 or more, the shape of the particles becomes close to a sphere, so that anisotropic scattering can be suppressed. The circularity is preferably 0.87 or more, more preferably 0.89 or more, even more preferably 0.90 or more, and particularly preferably 0.91 or more. The upper limit of the circularity is not particularly limited, and is most preferably 1.

[0018] The circularity is expressed as the average value of the maximum diameter (DL) and the minor diameter (DS) perpendicular to the maximum diameter (DL) of 100 random particles in a photographic projection obtained by photographing with a scanning electron microscope (SEM), and the ratio (DS / DL) of the minimum diameter (DS) to the maximum diameter (DL) is calculated.

[0019] The median diameter (D 50 The median diameter (D) of the spherical silica particles is preferably 1.0 to 30.0 μm. 50 When the median diameter (D) of the spherical silica particles is 1.0 μm or more, the protrusions on the film surface are larger than those of nano-sized particles, making it easier to exhibit anti-blocking properties, and the distance between the protrusions is larger than that of nano-sized particles, making it possible to reduce frictional force. 50 ) is 30.0 μm or less, high transparency can be expected. The median diameter of spherical silica particles (D 50 ) is more preferably 2.0 μm or more, even more preferably 3.0 μm or more, and particularly preferably 5.0 μm or more, and is more preferably 25.0 μm or less, even more preferably 20.0 μm or less, and particularly preferably 15.0 μm or less.

[0020] Median diameter (D 50 ) can be measured by the Coulter counter method using an electrical detection zone particle size distribution measuring device (e.g., Beckman Coulter's "Multisizer III") and calculated on a volume basis.

[0021] From the viewpoint that the area of ​​the interface between the resin and the spherical silica particles is reduced by the fine particles, thereby making it difficult for the haze of the film to increase, it is preferable that the volume fraction of particles having a particle size of 1.0 μm or less is 7% or less, and more preferably 5% or less.

[0022] In addition, from the viewpoint of reducing the roughness of the film surface caused by coarse particles and thereby preventing the deterioration of the haze of the film, it is preferable that the volume fraction of particles having a particle size of 40.0 μm or more is 15% or less, and more preferably 10% or less.

[0023] The volume percentage of particles having a particle size of 1.0 μm or less and the volume percentage of particles having a particle size of 40.0 μm or more can be calculated using the particle size distribution measuring device by the electrical detection zone method described above.

[0024] Spherical silica particles have a pore volume of 0.001 to 0.15 cm 3 / g. Here, the pore volume means the pore volume derived from pores having a pore diameter of 1 to 100 nm. The pore volume of a spherical silica particle is 0.1 cm 3 / g or less is more preferable, and 0.05 cm 3 / g or less is more preferable, and 0.01 cm 3 / g or less is particularly preferred. 3 When the molecular weight is 1.0 or less than 1 g, light scattering can be reduced and the transparency of the film can be improved.

[0025] The pore volume can be calculated by the nitrogen adsorption method using the BJH method.

[0026] The spherical silica particles used in the present embodiment may be obtained by manufacturing, or may be commercially available products. For example, the manufacturing method of spherical silica particles may be a wet method or a granulation method. Among them, from the viewpoint of obtaining spherical silica particles with a small specific surface area and a moderately narrow particle size distribution, the silica particles manufactured by the wet method are preferred.

[0027] The wet method refers to a method that includes a process of using a liquid silica source and gelling it to obtain raw material for silica particles. By using the wet method, it is easy to adjust the shape of the silica particles. In particular, it is easy to prepare spherical silica particles, and there is no need to adjust the shape of the particles by crushing, etc., and as a result, it is easy to obtain particles with a small specific surface area. In addition, the wet method is difficult to produce particles that are significantly smaller than the average particle size, and the specific surface area tends to be small after firing. In addition, in the wet method, the amount of impurity elements such as titanium can be adjusted by adjusting the impurities in the silica source, and the above-mentioned impurity elements can be uniformly dispersed in the particles.

[0028] Examples of the wet method include the spray method and the emulsion-gelling method. In the emulsion-gelling method, for example, a dispersed phase containing a silica precursor and a continuous phase are emulsified, and the resulting emulsion is gelled to obtain spherical silica particles. As an emulsification method, a method in which a dispersed phase containing a silica precursor is supplied to a continuous phase through a micropore or a porous membrane to produce an emulsion is preferred. This produces an emulsion with a uniform droplet size, resulting in spherical silica particles with a uniform particle size. Here, the particle size of the silica particles can be adjusted by adjusting the stirring speed during emulsification.

[0029] As such an emulsification method, a micromixer method or a membrane emulsification method can be used. For example, the micromixer method is disclosed in International Publication No. 2013 / 062105.

[0030] The spherical silica particles used in this embodiment are preferably subjected to a heat treatment, which has the effect of sintering the spherical silica particles and densifying the shell.

[0031] The heat treatment means is not particularly limited, and examples thereof include heat treatment by standing, heat treatment by rotary furnace, and heat treatment by spray combustion. For heat treatment by standing, a stationary electric furnace, a roller hearth kiln, a continuous furnace classified as a tunnel furnace, and the like can be used. For heat treatment by rotary furnace, a horizontal rotary furnace (rotary kiln), a rotary tubular furnace, and the like can be used. Among these, from the viewpoint of uniformity of firing, it is preferable to perform firing by heat treatment by a continuous furnace or a rotary furnace.

[0032] The heat treatment temperature is preferably 700° C. or higher, more preferably 800° C. or higher, even more preferably 900° C. or higher, and particularly preferably 1000° C. or higher. From the viewpoint of suppressing crystallization, the heat treatment temperature is preferably 1600° C. or lower, more preferably 1500° C. or lower, and even more preferably 1400° C. or lower.

[0033] The heat treatment time may be appropriately adjusted depending on the apparatus used, but is preferably performed for, for example, 0.5 to 50 hours, and more preferably 1 to 10 hours.

[0034] The spherical silica particles used in this embodiment may be surface-treated with a silane coupling agent. By treating the surface of the spherical silica particles with a silane coupling agent, the affinity with the resin is improved, and the dispersibility and film strength can be improved.

[0035] The conditions for the surface treatment are not particularly limited, and general surface treatment conditions may be used, and a wet treatment method or a dry treatment method may be used. From the viewpoint of performing uniform treatment, the wet treatment method is preferred.

[0036] Examples of the silane coupling agent include epoxysilane coupling agents, aminosilane coupling agents, mercaptosilane coupling agents, silane coupling agents, silane coupling agents, organosilazane compounds, etc. These may be used alone or in combination of two or more. In addition, from the viewpoint of not affecting the color of the optical film, it is preferable to use a silane coupling agent that does not have a double bond.

[0037] Specific examples of the surface treatment agent include epoxysilane coupling agents such as glycidoxypropyltrimethoxysilane, glycidoxypropyltriethoxysilane, glycidoxypropylmethyldiethoxysilane, glycidylbutyltrimethoxysilane, and (3,4-epoxycyclohexyl)ethyltrimethoxysilane; aminosilane coupling agents such as aminopropylmethoxysilane, aminopropyltriethoxysilane, N-phenylaminopropyltrimethoxysilane, and N-2(aminoethyl)aminopropyltrimethoxysilane; and mercaptosilane coupling agents such as mercaptopropyltrimethoxysilane and mercaptopropyltriethoxysilane. , silane coupling agents such as methyltrimethoxysilane, vinyltrimethoxysilane, octadecyltrimethoxysilane, phenyltrimethoxysilane, methacryloxypropyltrimethoxysilane, imidazole silane, and triazine silane, CF3(CF2)7CH2CH2Si(OCH3)3, CF3(CF2)7CH2CH2SiCl3, CF3(CF2)7CH2CH2Si(CH3)(OCH3)2, CF3(CF2)7CH2CH2Si(CH3)C12, CF3(CF2)5CH2CH2SiCl3, CF3(CF2)5CH2CH2Si(OCH3)3, CF3CH2CH2SiCl3, CF3CH2CH2Si(OCH3)3, C8F 17 SO2N(C3H7)CH2CH2CH2Si(OCH3)3, C7F 15 CONHCH2CH2CH2Si(OCH3)3, C8F 17 CO2CH2CH2CH2Si(OCH3)3, C8F 17 Examples of suitable coupling agents include fluorine-containing silane coupling agents such as -O-CF(CF3)CF2-O-C3H6SiCl3 and C3F7-O-(CF(CF3)CF2-O)2-CF(CF3)CONH-(CH2)3Si(OCH3)3, and organosilazane compounds such as hexamethyldisilazane, hexaphenyldisilazane, trisilazane, cyclotrisilazane, and 1,1,3,3,5,5-hexamethylcyclotrisilazane.

[0038] The amount of the silane coupling agent used for treatment is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, and even more preferably 0.10 parts by mass or more, per 100 parts by mass of the spherical silica particles, and is preferably 5 parts by mass or less, and more preferably 2 parts by mass or less.

[0039] Examples of methods for treating with a silane coupling agent include a dry method in which the silane coupling agent is sprayed onto spherical silica particles, and a wet method in which the spherical silica particles are dispersed in a solvent and then a silane coupling agent is added to cause a reaction.

[0040] The fact that the surface of the spherical silica particles has been treated with a silane coupling agent can be confirmed by detecting a peak due to a substituent of the silane coupling agent by infrared spectroscopy (IR). The amount of the silane coupling agent attached can be measured by the amount of carbon.

[0041] The spherical silica particles are preferably contained in the resin layer in the range of 0.1 to 60.0% by mass. If the content of the spherical silica particles in the resin layer is 0.1% by mass or more, the surface contact between the films is reduced, thereby enabling anti-blocking properties to be exhibited, and if it is 60.0% by mass or less, the interface area between the resin and the silica particles is reduced, thereby enabling the deterioration of the transparency of the film to be suppressed. The content of spherical silica particles in the resin layer is preferably 0.5% by mass or more, even more preferably 0.7% by mass or more, and particularly preferably 1.0% by mass or more, and more preferably 30.0% by mass or less, even more preferably 20.0% by mass or less, and particularly preferably 10.0% by mass or less.

[0042] (resin) The resin used in the resin layer can be appropriately selected according to the application of the film and is not particularly limited, but is preferably transparent when used for optical applications. From the viewpoint of improving mechanical strength, the resin layer preferably contains a cured product of a curable resin. Examples of the curable resin include a thermosetting resin and an ionizing radiation curable resin. In other words, the resin layer preferably contains a cured product of a thermosetting resin composition or a cured product of an ionizing radiation curable resin composition, and more preferably contains a cured product of an ionizing radiation curable resin composition.

[0043] The thermosetting resin composition is a composition that contains at least a thermosetting resin, and is a resin composition that is cured by heating.

[0044] Examples of the thermosetting resin include acrylic resin, urethane resin, phenol resin, urea melamine resin, epoxy resin, unsaturated polyester resin, silicone resin, etc. In the thermosetting resin composition, a curing agent is added to the curable resin as required.

[0045] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group (hereinafter, also referred to as "ionizing radiation curable compound"). Examples of the ionizing radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl group, vinyl group, and allyl group, as well as epoxy group, oxetanyl group, and the like. "(meth)acryloyl" refers to acryloyl and methacryloyl in general. As the ionizing radiation curable compound, a compound having an ethylenically unsaturated bond group is preferred, a compound having two or more ethylenically unsaturated bond groups is more preferred, and among them, a polyfunctional (meth)acrylate-based compound having two or more ethylenically unsaturated bond groups is even more preferred. "(meth)acrylate" refers to a general term for acrylate and methacrylate. As the polyfunctional (meth)acrylate-based compound, either a monomer or an oligomer can be used.

[0046] Here, ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Usually, ultraviolet rays (UV) or electron beams (EB) are used, but other types of radiation, such as electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams, can also be used.

[0047] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxy diacrylate, bisphenol A tetrapropoxy diacrylate, and 1,6-hexanediol diacrylate. Examples of trifunctional or higher (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and isocyanuric acid-modified tri(meth)acrylate. The (meth)acrylate monomers may have a part of the molecular skeleton modified, and those modified with ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, alkyl, cyclic alkyl, aromatic, bisphenol, and the like may also be used.

[0048] In addition, examples of the polyfunctional (meth)acrylate oligomer include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, and polyether (meth)acrylate. The urethane (meth)acrylate is obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate. In addition, preferred epoxy (meth)acrylates are (meth)acrylates obtained by reacting trifunctional or higher aromatic epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc. with (meth)acrylic acid, (meth)acrylates obtained by reacting difunctional or higher aromatic epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc. with polybasic acids and (meth)acrylic acid, and (meth)acrylates obtained by reacting difunctional or higher aromatic epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc. with phenols and (meth)acrylic acid.

[0049] In addition, for the purpose of adjusting the viscosity of the resin kneaded product, a monofunctional (meth)acrylate may be used in combination as the ionizing radiation curable compound. Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate. The above ionizing radiation curable compounds may be used alone or in combination of two or more.

[0050] When the ionizing radiation curable compound is an ultraviolet ray curable compound, the ionizing radiation curable composition preferably contains additives such as a photopolymerization initiator and a photopolymerization accelerator. The photopolymerization initiator may be one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc. The photopolymerization accelerator is capable of reducing polymerization inhibition caused by air during curing and accelerating the curing speed, and may be one or more selected from p-dimethylaminobenzoic acid isoamyl ester, p-dimethylaminobenzoic acid ethyl ester, etc.

[0051] When the resin layer contains a cured product of the ionizing radiation curable resin composition, it is preferable that the resin layer contains a thermoplastic resin in addition to the cured product of the ionizing radiation curable resin composition. By containing the thermoplastic resin, the viscosity of the resin kneaded product increases, so that the spherical silica particles are less likely to sink, and the binder resin is less likely to flow down between the protrusions based on the spherical silica particles.

[0052] Examples of thermoplastic resins include cellulose-based resins, polystyrene-based resins, polyolefin-based resins, acrylonitrile-butadiene-styrene (ABS) resins (including heat-resistant ABS resins), acrylonitrile-styrene (AS) resins, acrylonitrile (AN) resins, polyphenylene oxide-based resins, polycarbonate-based resins, polyacetal-based resins, acrylic-based resins, polyethylene terephthalate (PET)-based resins, polybutylene terephthalate-based resins, polysulfone-based resins, and polyphenylene sulfide-based resins. From the viewpoint of transparency, it is preferable to use acrylic-based resins, and from the viewpoint of environmental impact, it is preferable to use cellulose-based resins.

[0053] In the present invention, the resin used in the resin layer is preferably a resin having a refractive index in the range of 1.40 to 1.50. Since the refractive index in this range is close to that of silica, the resin having a refractive index in this range is less susceptible to optical interference, thereby enhancing the transparency of the film.

[0054] Examples of resins having a refractive index in the range of 1.40 to 1.50 include poly-4-methylpentene-1 (refractive index 1.47), polymethyl methacrylate (refractive index 1.50), cellulose acetate resin (refractive index 1.46 to 1.50), silicone resin (refractive index 1.43), diethylene glycol bisallyl carbonate resin (refractive index 1.50), polyacetal (refractive index 1.48), polypropylene (refractive index 1.49), polytrifluoroethylene chloride (refractive index 1.43), polyvinylidene fluoride (refractive index 1.42), tetrafluoroethylene ethylene copolymer (refractive index 1.42), etc. The refractive index is more preferably 1.41 to 1.49, and even more preferably 1.42 to 1.48.

[0055] The refractive index of the resin is measured by an Abbe refractometer (JIS K 7142).

[0056] The resin content in the resin layer is preferably in the range of 40.0 to 99.9% by mass. If the resin content is 40.0% by mass or more, the resin layer can be molded into a film, and if it is 99.9% by mass or less, the added silica particles can impart anti-blocking properties. The resin content in the resin layer is more preferably 70.0% by mass or more, even more preferably 80.0% by mass or more, and particularly preferably 90.0% by mass or more, and more preferably 99.5% by mass or less, even more preferably 99.7% by mass or less, and particularly preferably 99.0% by mass or less.

[0057] (Other Ingredients) The resin layer may contain any component within the range that does not impair the effects of the present invention, such as a light stabilizer such as an ultraviolet absorber, an ultraviolet scattering agent, an infrared absorber, an infrared scattering agent, an antistatic agent, an antioxidant, a plasticizer, a coloring material, an extender pigment, a resin particle, a dispersant, a flame retardant, a lubricant, and an antifoaming agent. The content of the optional components varies depending on the use and thickness of the film of the present invention, but is preferably 60.0% by mass or less, more preferably 30.0% by mass or less, and even more preferably 10.0% by mass or less in the resin layer.

[0058] (Thickness of resin layer) The thickness of the resin layer is not particularly limited, but is preferably from 1.0 to 100 μm, more preferably from 1.5 to 50 μm, and further preferably from 2.0 to 30 μm. When the film is composed of only a resin layer, the thickness of the film is also preferably within the above range, and can be appropriately set depending on the application.

[0059] The thickness of the resin layer (film) is measured at three points in the layer using a digital caliper (for example, "Coolant Pool Micrometer" manufactured by Mitutoyo Corporation) and the average value is calculated.

[0060] (Manufacturing of resin layer) The method for producing the resin layer is not particularly limited, but includes, for example, preparing a resin mixture by kneading spherical silica particles and a resin, coating the resin mixture on a support to form a coating film, and drying the coating film to remove volatile components such as solvent. This forms a resin layer on a support. The resin mixture may contain various solvents, and may appropriately contain the above-mentioned additives as long as the resin layer (film) after preparation does not lose antiglare properties.

[0061] The solvent to be used can be appropriately selected depending on the type of resin or additive, and can dissolve at least the solid content uniformly. Examples of the solvent include ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), ethers (dioxane, tetrahydrofuran, etc.), aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), halogenated carbons (dichloromethane, dichloroethane, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), water, alcohols (ethanol, isopropanol, butanol, cyclohexanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates, sulfoxides (dimethyl sulfoxide, etc.), amides (dimethylformamide, dimethylacetamide, etc.), etc. These solvents may be used alone, or two or more solvents may be used. From the viewpoint of the solubility of the resin, it is preferable that the solvent contains a polar group.

[0062] The support is not particularly limited, and examples thereof include known films such as polyethylene terephthalate (PET) film, polyphenylene sulfide film, and polyimide film. The surface of the support may be previously surface-treated with a surface treatment agent such as silicone, a silane coupling agent, an aluminum chelating agent, or polyurea in order to improve the releasability of the resin kneaded product, which is the formed sheet. The thickness of the support is not particularly limited, and examples thereof include 10 to 100 μm.

[0063] Examples of a method for applying the resin mixture onto a support include rotation coating using a spinner, spray coating, roll coating, screen printing, and methods using a blade coater, a die coater, a calendar coater, a meniscus coater, a bar coater, a roll coater, a comma roll coater, a gravure coater, a screen coater, and a slit die coater.

[0064] The coating film can be dried, for example, by an oven, a hot plate, infrared rays, etc. The drying temperature and drying time are not particularly limited, and examples thereof include a drying temperature of 60 to 200° C. and a drying time of 1 to 360 minutes.

[0065] The thickness of the coating film is not particularly limited, and may be, for example, 1.0 to 100 μm, or may be 1.5 to 50 μm, or may be 2.0 to 30 μm, in terms of thickness after drying.

[0066] After the drying step, the resin may be cured by irradiation with ionizing radiation or heating depending on the type of resin, such as an ionizing radiation curable resin or a thermosetting resin. When the ionizing radiation is ultraviolet radiation, a far ultraviolet lamp, a low pressure mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a halogen lamp, a laser light source (light source such as a helium-cadmium laser or an excimer laser), etc. can be used as the light source.

[0067] From the viewpoint of adhesion of the spherical silica particles, the total content of the spherical silica particles in the resin mixture is preferably 0.1 to 60 parts by mass, more preferably 0.5 to 30 parts by mass, and even more preferably 1.0 to 10 parts by mass.

[0068] The resin layer formed on the support is separated from the support to obtain a film. The resin layer has an optical function due to the spherical silica particles, and is suitably used in an optical film as, for example, an antiglare layer exhibiting antiglare properties.

[0069] <Laminate> The film of the present invention may be a single resin layer, or may be a laminate of two or more layers in which an arbitrary layer is laminated on a resin layer. The arbitrary layer may be, for example, a base layer, an antireflection layer, an antistatic layer, an antifouling layer, an electromagnetic wave shielding layer, an infrared absorbing layer, an ultraviolet absorbing layer, a color correction layer, etc., and the order of these layers is not particularly limited. The resin layer may be a single layer, or may be a laminate of multiple resin layers. In addition, the resin layer itself may be further provided with functions such as ultraviolet absorbing performance, antistatic performance, refractive index adjusting function, and hardness adjusting function. In order to improve the adhesion between each layer, a primer layer, an adhesive layer, etc. may be provided between each layer.

[0070] When the laminate is used for optical purposes, an example of the configuration of the laminate is one in which an antiglare layer, which is an optically functional layer, is provided on a substrate layer, and the surface of the antiglare layer opposite to the substrate is an uneven surface of the optical laminate. The antiglare layer may be laminated on at least one surface of the substrate layer, and may be laminated on both surfaces, but from the viewpoints of handling, mechanical properties, productivity, etc., it is usually preferable that the antiglare layer is laminated on only one surface.

[0071] When the laminate has a base layer, the base layer of the laminate of the present invention is preferably a transparent base layer from the viewpoint of enhancing the transparency of the film. The resin layer is preferably laminated on at least one surface of the transparent base layer directly or via one or more other layers.

[0072] The material of the substrate layer is not particularly limited, and glass, ceramics, and resins can be used. Among these, it is preferable to use resins from the viewpoint of processability. Examples of preferable resins include transparent polymers, such as cellulose derivatives (cellulose acetates such as cellulose triacetate (TAC) and cellulose diacetate), polyester resins (polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polyarylate resins, etc.), polysulfone resins (polysulfone, polyethersulfone (PES), etc.), polyetherketone resins (polyetherketone (PEK), polyetheretherketone (PEEK), etc.), polycarbonate resins (PC), polyolefin resins (polyethylene, polypropylene, etc.), cyclic polyolefin resins, halogen-containing resins (polyvinylidene chloride, etc.), (meth)acrylic resins, styrene resins (polystyrene, etc.), vinyl acetate or vinyl alcohol resins (polyvinyl alcohol, etc.), etc. can be exemplified. The term "(meth)acrylic" refers collectively to acrylic and methacrylic. Among these, acrylic resins are more preferred from the viewpoint of transparency.

[0073] The transparency of the transparent substrate layer is expressed as the visible light transmittance (T L , visible light transmittance as measured by ISO 9050:2003) is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more.

[0074] The thickness of the base layer is not particularly limited, but is, for example, preferably from 1.0 to 99 μm, more preferably from 1.5 to 50 μm, and further preferably from 2.0 to 50 μm.

[0075] (Thickness of laminate) The thickness of the laminate may be adjusted appropriately depending on the application. For example, when used in a display device such as a liquid crystal display device or an organic EL display, the thickness is preferably 3 to 100 μm, more preferably 5 to 70 μm, and even more preferably 20 to 50 μm.

[0076] The thickness of the laminate can be measured with a digital caliper, and the measurement method is the same as that for the resin layer (film).

[0077] (Manufacture of laminates) The laminate is manufactured by laminating the above-mentioned resin layer and any layer. For example, after preparing a resin mixture by kneading spherical silica particles and a resin composition, the resin mixture is applied onto a substrate layer to form a coating film, and the coating film is dried to remove volatile components such as solvent, thereby forming the resin layer on the substrate layer. The resin mixture may contain various solvents, and may appropriately contain the above-mentioned additives as long as the laminate (film) after preparation does not lose antiglare properties.

[0078] As the solvent, the same solvent as that used in producing the resin layer can be used.

[0079] Methods for applying the resin mixture onto the substrate layer include rotational application using a spinner, spray application, roll coating, screen printing, and methods using a blade coater, die coater, calendar coater, meniscus coater, bar coater, roll coater, comma roll coater, gravure coater, screen coater, and slit die coater.

[0080] The coating film can be dried, for example, by using an oven, a hot plate, infrared rays, etc. The drying temperature and drying time are not particularly limited, and examples thereof include a drying temperature of 40 to 120° C. and a drying time of 1 to 20 minutes.

[0081] The thickness of the coating film is not particularly limited as long as it is adjusted so that the film thickness is in the above-mentioned range of 1.0 to 100 μm. For example, the coating film may have a thickness of 1.0 to 99 μm after drying, or may be 1.5 to 50 μm or 2.0 to 30 μm.

[0082] After the drying step, the resin may be cured by irradiation with ionizing radiation or heating depending on the type of resin, such as an ionizing radiation curable resin or a thermosetting resin. When the ionizing radiation is ultraviolet radiation, a far ultraviolet lamp, a low pressure mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a halogen lamp, a laser light source (light source such as a helium-cadmium laser or an excimer laser), etc. can be used as the light source.

[0083] From the viewpoint of adhesion of the silica particles, the total content of the spherical silica particles in the resin mixture is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5.0 parts by mass, and even more preferably 1.0 to 3.0 parts by mass.

[0084] <Evaluation of optical properties of film> (Kinematic friction coefficient) The film of the present invention has a resin layer on either one of the outermost layers, and the surface of the resin layer has irregularities, and the roughness is expressed by the dynamic friction coefficient. In this specification, the dynamic friction coefficient refers to the dynamic friction coefficient on the surface of the resin layer of the film.

[0085] The dynamic friction coefficient can be measured using a static / dynamic friction measuring device (for example, "TL201Tt" manufactured by Trinity Lab Co., Ltd.) according to the following procedure. The contactor is a urethane artificial finger, the load is 50gf, the scanning distance is 40mm, the scanning speed is 10mm / sec, and the film is set in the static / dynamic friction measuring device so that the resin layer surface of the film is in contact with the contactor, and the measurement is performed. The average value of the obtained friction coefficients in the range of 1,000msec to 4,000msec is taken as the kinetic friction coefficient.

[0086] The dynamic friction coefficient is preferably 0.80 or less, more preferably 0.78 or less, and even more preferably 0.76 or less. The smaller the dynamic friction coefficient, the smaller the frictional force and the better the anti-blocking properties, so there is no particular lower limit.

[0087] (Haze) The transparency of the film of the present invention is expressed by haze. Haze can be measured using a haze meter (for example, "HAZE METER NDH 7000" manufactured by Nippon Denshoku Industries Co., Ltd.) according to the method specified in JIS K7136:2000.

[0088] The haze is preferably 20.0% or less, more preferably 15.0% or less, and even more preferably 10.0% or less. The smaller the haze measurement value, the more preferable it is, so there is no particular lower limit.

[0089] (Total light transmittance) The transparency of the film of the present invention is expressed by the total light transmittance. The total light transmittance can be measured using a haze meter (for example, "HAZE METER NDH 7000" manufactured by Nippon Denshoku Industries Co., Ltd.) according to the method specified in JIS K7136:2000.

[0090] The total light transmittance is preferably 90.0% or more, more preferably 95.0% or more, and even more preferably 98.0% or more. The higher the total light transmittance, the more preferable it is, so there is no particular upper limit.

[0091] (Arithmetic mean roughness of roughness curve: Ra) The arithmetic mean roughness (Ra) of the roughness curve of the film of the present invention is measured based on JIS B0601:2013 (ISO4287:1997, Amd.1:2009). The reference length (cutoff value) λc is 0.8 mm. In the measurement, a surface roughness measuring device (for example, "SURFTEST SJ-310" manufactured by Mitutoyo Corporation) is used to obtain Ra at a total of six locations, three locations in the direction perpendicular to the flow direction during the production of the film and three locations in the direction parallel to the flow direction, and the average value of these values ​​is taken as the Ra of the film surface.

[0092] (Maximum height of roughness curve: Rz) The roughness curve (Rz) of the film of the present invention is measured based on JIS B0601:2013 (ISO4287:1997, Amd.1:2009). The reference length (cutoff value) λc is 0.8 mm, and λs is 2.5 μm. For the measurement, a surface roughness measuring device (for example, "SURFTEST SJ-310" manufactured by Mitutoyo Corporation) is used, and the difference between the maximum peak height Zp and the maximum valley depth Zv within the reference length is defined as Rz.

[0093] (Ten-point average roughness: RzJIS) The ten-point average roughness (RzJIS) of the film of the present invention is measured based on JIS B0601:2013 (ISO4287:1997, Amd.1:2009). The reference length (cutoff value) λc is 0.8 mm, and λs is 2.5 μm. In the measurement, a surface roughness measuring device (for example, "SURFTEST SJ-310" manufactured by Mitutoyo Corporation) is used, and the sum of the average of the heights of the five peaks from the maximum peak height and the average of the depths of the five valleys from the maximum valley depth in the roughness curve of the reference length is defined as RzJIS.

[0094] <Application> The film of the present invention exhibits optical functions such as antiglare properties, and can suppress glare, haze, and the effects of structural color due to interference, and can therefore be suitably used as an optical film. For example, it can be used as an antiglare film, light-diffusing OCR, or light-diffusing adhesive layer for various display devices, such as liquid crystal display devices (LCDs), organic EL displays, and display devices with touch panels, and is particularly useful as an optical element for LCDs and organic EL displays.

[0095] As described above, the present invention includes the following: <1> ~ <13> The configuration includes: <1> A resin layer containing a resin and spherical silica particles, the spherical silica particles having a BET specific surface area of ​​4.5 m 2 / g or less of the film. <2> The median diameter (D 50 ) is 1.0 to 30.0 μm. <1> The film according to claim 1. <3> The spherical silica particles have a circularity of 0.85 or more. <1> or <2> The film according to claim 1. <4> The content of the spherical silica particles in the resin layer is 0.1 to 60.0% by mass. <1> ~ <3> 13. The film according to claim 12, <5> The BET specific surface area of ​​the spherical silica particles is 4.0 m 2 / g or less. <1> ~ <4> 13. The film according to claim 12, <6> The refractive index of the resin is 1.40 to 1.50. <1> ~ <5> 13. The film according to claim 12, <7> The optical film further comprises a transparent substrate layer, and the resin layer is laminated on at least one surface of the transparent substrate layer directly or via one or more other layers. <1> ~ <6> 13. The film according to claim 12, <8> The dynamic friction coefficient is 0.80 or less. <1> ~ <7> 13. The film according to claim 12, <9> The haze is 20.0% or less. <1> ~ <8> 13. The film according to claim 12, <10> The film thickness is 1.0 to 100 μm. <1> ~ <9> 13. The film according to claim 12, <11> The optical film is <1> ~ <10> 13. The film according to claim 12, <12> The above <1> ~ <11> 13. A display device comprising the film according to any one of the above items. <13> The display device is a liquid crystal display device or an organic EL display device. <12> The display device according to claim 1 . EXAMPLES

[0096] Next, the embodiments of the present disclosure will be specifically described with reference to examples, but the embodiments of the present disclosure are not limited to these examples. Examples 1 to 4 and 11 to 14 are examples, and Examples 5 to 10 and 15 to 19 are comparative examples.

[0097] <Test Example 1> (Example 1) 4.95 g of methanol and 4.95 g of polyvinyl acetate were added to a container to prepare a 50 mass % polyvinyl acetate methanol solution. 9.9 g of methanol and spherical silica particles (BET specific surface area: 1.3 m) were added thereto. 2 / g, median diameter (D 50 The mixture was kneaded at 2000 rpm for 120 seconds using a kneader "Awatori Rentaro" (product name, manufactured by Thinky Corporation) to obtain a resin kneaded product. This resin mixture was applied to a transparent substrate (polyethylene terephthalate (PET) film, Toray Industries, Inc.'s "Lumirror 50U-48", thickness 26-75 μm, visible light transmittance 91%) using an automatic coating device (Allgood Co., Ltd.'s "Small Automatic Film Applicator") with a Bird-type applicator to a coating thickness of 90 μm. The coating speed was 10 mm / s. Thereafter, the coating was dried at 40° C. for 3 hours to obtain a film having a resin layer formed on the surface of the transparent substrate.

[0098] (Example 2) Spherical silica particles with a BET specific surface area of ​​4.0m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 1, except that spherical silica particles having a diameter of 3.0 μm and a circularity of 0.93 were used.

[0099] (Example 3) Spherical silica particles with a BET specific surface area of ​​0.8m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 1, except that spherical silica particles having a diameter of 4.1 μm and a circularity of 0.94 were used.

[0100] (Example 4) 4.75 g of methanol and 4.75 g of polyvinyl acetate were added to a container to prepare a 50 mass % polyvinyl acetate methanol solution. 9.5 g of methanol and spherical silica particles (BET specific surface area: 0.8 m) were added thereto. 2 / g, median diameter (D 50The mixture was kneaded at 2000 rpm for 120 seconds using a kneader "Awatori Rentaro" (product name, manufactured by Thinky Corporation) to obtain a resin kneaded product. Using this resin mixture, a coating film was formed on a transparent substrate in the same manner as in Example 1, and then dried at 40° C. for 3 hours to obtain a film in which a resin layer was formed on the surface of the transparent substrate.

[0101] (Example 5) 5.0 g of methanol and 5.0 g of polyvinyl acetate were added to a container to prepare a 50% by mass solution of polyvinyl acetate in methanol. 10.0 g of methanol was added thereto, and the mixture was kneaded at 2000 rpm for 120 seconds using a kneader "Awatori Rentaro" (product name, manufactured by Thinky Corporation) to prepare a resin kneaded product. Using this resin mixture, a coating film was formed on a transparent substrate in the same manner as in Example 1, and then dried at 40° C. for 3 hours to obtain a film in which a resin layer was formed on the surface of the transparent substrate.

[0102] (Example 6) Instead of spherical silica particles, amorphous silica particles (Mizukasil P-603 manufactured by Mizusawa Chemical Industry Co., Ltd., BET specific surface area: 30.0 m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 1, except that a crystalline polymer having a diameter of 1.0 mm and a circularity of 0.80 was used.

[0103] (Example 7) Instead of spherical silica particles, diatomaceous earth particles (Oplite W3005K manufactured by Oplite Kogyo Co., Ltd.) were used. The median diameter (D 50 A film was obtained in the same manner as in Example 1, except that a crystalline polymer having a diameter of 100 nm and a circularity of 0.75 was used.

[0104] (Example 8) Instead of spherical silica particles, polymethyl methacrylate (PMMA) resin particles (Matsumoto Yushi Pharmaceutical Co., Ltd. "M-201"; median diameter (D 50 A film was obtained in the same manner as in Example 4, except that a crystalline powder (CuO2: 5.0 μm, circularity: 0.90) was used.

[0105] (Example 9) Spherical silica particles were replaced with spherical silica particles having a large BET specific surface area ("NP-30" manufactured by AGC Inc., BET specific surface area: 34.0 m 2 / g, median diameter (D 50 ): 4.2 μm, circularity: 0.93), and a film was obtained in the same manner as in Example 4.

[0106] (Example 10) Spherical silica particles were replaced with amorphous silica particles ("Mizukasil P-603" manufactured by Mizusawa Chemical Industry Co., Ltd., BET specific surface area: 30.0 m 2 / g, median diameter (D 50 ): 3.0 μm, circularity: 0.80), and a film was obtained in the same manner as in Example 4.

[0107] The following measurements were performed on the particles and the obtained films used in Examples 1 to 10. The results are shown in Tables 1 and 2.

[0108] <Measurement of median diameter> The median diameter of the particles was measured by the Coulter counter method using a Coulter counter device ("Multisizer III" manufactured by Beckman Coulter, Inc.) and calculated on a volume basis.

[0109] <BET specific surface area, pore volume> The BET specific surface area and pore volume of the particles were measured by the BET method and the BJH method using a specific surface area and pore distribution measuring device ("BELSORP-mini II" manufactured by MicrotracBEL Corp.).

[0110] <Circularity> The circularity of the particles was measured for 100 arbitrary particles in the photographic projection diagram obtained by photographing with a scanning electron microscope (SEM). The major axis (DL) and the minor axis (DS) orthogonal to this were measured for each particle, and the ratio (DS / DL) of the minor axis (DS) to the major axis (DL) was calculated, and the average value was obtained.

[0111] <Film thickness> The thickness of the resin layer of the film was measured at three points using a digital caliper (coolant pool micrometer, manufactured by Mitutoyo Corporation), and the average value was taken as the film thickness of the resin layer.

[0112] <Haze, total light transmittance> The haze and total light transmittance were measured using a haze meter ("HAZE METER NDH 7000" manufactured by Nippon Denshoku Industries Co., Ltd.) according to the method specified in JIS K7136:2000.

[0113] <Kinematic friction coefficient> The dynamic friction coefficient was determined using a static / dynamic friction tester (TL201Tt, manufactured by Trinity Lab Co., Ltd.). The contactor was a urethane artificial finger, the load was 30 gf, the scanning distance was 40 mm, and the scanning speed was 10 mm / sec. The film with a resin layer formed on a transparent substrate was set in the static / dynamic friction tester so that the surface of the resin layer was in contact with the contactor, and measurements were taken. The average value of the obtained friction coefficients in the range of 1,000 msec to 4,000 msec was taken as the dynamic friction coefficient.

[0114] <Arithmetic mean roughness of roughness curve: Ra> The arithmetic mean roughness (Ra) of the roughness curve was measured based on JIS B0601:2013 (ISO4287:1997, Amd.1:2009). The reference length (cutoff value) λc was set to 0.8 mm. For the measurement, a surface roughness measuring instrument ("SURFTEST SJ-310" manufactured by Mitutoyo Corporation) was used to obtain Ra at a total of six locations, three locations in the direction perpendicular to the flow direction during film production and three locations in the direction parallel to the flow direction, and the average of these values ​​was taken as the Ra of the film surface.

[0115] <Maximum height of roughness curve: Rz> The maximum height roughness (Rz) of the roughness curve was measured based on JIS B0601:2013 (ISO4287:1997, Amd.1:2009). The reference length (cutoff value) λc was 0.8 mm, and λs was 2.5 μm. The measurement was performed using a surface roughness measuring instrument (Mitutoyo Corporation's "SURFTEST SJ-310"), and the difference between the maximum peak height Zp and the maximum valley depth Zv within the reference length was taken as Rz.

[0116] <Ten-point average roughness: RzJIS> The ten-point average roughness (RzJIS) was measured based on JIS B0601:2013 (ISO4287:1997, Amd.1:2009). The reference length (cutoff value) λc was 0.8 mm, and λs was 2.5 μm. A surface roughness measuring instrument (Mitutoyo Corporation's "SURFTEST SJ-310") was used for the measurement, and the sum of the average of the heights of the five peaks from the maximum peak height and the average of the depths of the five valleys from the maximum valley depth on the roughness curve of the reference length was taken as RzJIS.

[0117] [Table 1]

[0118] [Table 2]

[0119] In the films of Examples 1 to 10, a resin layer with a thickness of about 15 μm is formed on the surface of the substrate. As shown in Tables 1 and 2, the films of Examples 1 to 4 have a smaller dynamic friction coefficient and improved anti-blocking properties than the film of Example 5 due to the addition of spherical silica particles to the resin layer. Comparing Examples 1 to 3 with Examples 6 and 7, it is clear that the BET specific surface area is 4.5 m 2 / g or less, the haze can be reduced and the transparency is improved. Furthermore, a comparison of Example 4 with Examples 8 to 10 shows that the transparency is unlikely to decrease even when a large amount of filler particles is added.

[0120] <Test Example 2> (Example 11) 4.95 g of methanol and 4.95 g of polyvinyl acetate were added to a container to prepare a 50 mass % polyvinyl acetate methanol solution. 9.9 g of methanol and spherical silica particles (BET specific surface area: 0.4 m) were added thereto. 2 / g, median diameter (D 50 The mixture was kneaded at 2000 rpm for 120 seconds using a kneader "Awatori Rentaro" (product name, manufactured by Thinky Corporation) to obtain a resin kneaded product. This resin mixture was applied to a transparent substrate (polyethylene terephthalate (PET) film, Toray Industries, Inc.'s "Lumirror 50U-48", thickness 26-75 μm, visible light transmittance 91%) using an automatic coating device (Allgood Co., Ltd.'s "Small Automatic Film Applicator") with a Bird-type applicator to a coating thickness of 200 μm. The coating speed was 10 mm / s. Thereafter, the coating was dried at 40° C. for 3 hours to obtain a film having a resin layer formed on the surface of the transparent substrate.

[0121] (Example 12) 4.75 g of methanol and 4.75 g of polyvinyl acetate were added to a container to prepare a 50 mass % polyvinyl acetate methanol solution. 9.5 g of methanol and spherical silica particles (BET specific surface area: 4.0 m) were added thereto. 2 / g, median diameter (D 50 The mixture was kneaded at 2000 rpm for 120 seconds using a kneader "Awatori Rentaro" (product name, manufactured by Thinky Corporation) to obtain a resin kneaded product. Using this resin mixture, a coating film was formed on a transparent substrate in the same manner as in Example 11, and then dried at 40° C. for 3 hours to obtain a film in which a resin layer was formed on the surface of the transparent substrate.

[0122] (Example 13) Spherical silica particles with a BET specific surface area of ​​0.8m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 12, except that spherical silica particles having a diameter of 4.1 μm and a circularity of 0.94 were used.

[0123] (Example 14) Spherical silica particles with a BET specific surface area of ​​0.4 m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 12, except that spherical silica particles having a diameter of 11.0 μm and a circularity of 0.92 were used.

[0124] (Example 15) 5.0 g of methanol and 5.0 g of polyvinyl acetate were added to a container to prepare a 50% by mass solution of polyvinyl acetate in methanol. 10.0 g of methanol was added thereto, and the mixture was kneaded at 2000 rpm for 120 seconds using a kneader "Awatori Rentaro" (product name, manufactured by Thinky Corporation) to prepare a resin kneaded product. Using this resin mixture, a coating film was formed on a transparent substrate in the same manner as in Example 11, and then dried at 40° C. for 3 hours to obtain a film in which a resin layer was formed on the surface of the transparent substrate.

[0125] (Example 16) Instead of spherical silica particles, amorphous silica particles (Mizukasil P-603 manufactured by Mizusawa Chemical Industry Co., Ltd., BET specific surface area: 30.0 m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 11, except that a crystalline polymer having a diameter of 1.0 mm and a circularity of 0.80 was used.

[0126] (Example 17) Instead of spherical silica particles, amorphous silica particles (Mizukasil P-603 manufactured by Mizusawa Chemical Industry Co., Ltd., BET specific surface area: 30.0 m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 12, except that a crystalline polymer having a diameter of 1.0 mm and a circularity of 0.80 was used.

[0127] (Example 18) Instead of spherical silica particles, diatomaceous earth particles (Oplite W3005K manufactured by Oplite Kogyo Co., Ltd.) were used. The median diameter (D 50 A film was obtained in the same manner as in Example 12, except that a crystalline polymer having a diameter of 100 nm and a circularity of 0.75 was used.

[0128] (Example 19) Instead of spherical silica particles, spherical silica particles with a large BET specific surface area (AGC Si-Tech "NP-100", BET specific surface area: 127.0 m 2 / g, median diameter (D 50 A film was obtained in the same manner as in Example 12, except that a crystalline polymer having a diameter of 10.4 μm and a circularity of 0.95 was used.

[0129] The particles used in Examples 11 to 19 and the resulting films were subjected to the same measurements as in Test Example 1. The results are shown in Tables 3 and 4.

[0130] [Table 3]

[0131] [Table 4]

[0132] In the films of Examples 11 to 19, a resin layer with a thickness of about 30 μm is formed on the surface of the substrate. As shown in Tables 3 and 4, the films of Examples 11 to 14 have a smaller dynamic friction coefficient and improved anti-blocking properties than the film of Example 15 due to the addition of spherical silica particles to the resin layer. A comparison of Example 11 and Example 16 shows that the BET specific surface area is 4.5 m 2 It was found that the use of spherical silica particles having a particle size of 0.1 to 0.5 μm / g or less can reduce haze and improve transparency. Furthermore, a comparison of Examples 11 to 13 with Examples 17 to 19 shows that transparency is unlikely to decrease even when a large amount of filler particles is added.

Claims

1. A resin layer containing a resin and spherical silica particles, the spherical silica particles having a BET specific surface area of ​​4.5 m 2 / g or less.

2. The median diameter (D 50 2. The film of claim 1, wherein the thickness of the film is from 1.0 to 30.0 μm.

3. The film according to claim 1 , wherein the spherical silica particles have a circularity of 0.85 or more.

4. The film according to claim 1, wherein the content of the spherical silica particles in the resin layer is 0.1 to 60.0% by mass.

5. The BET specific surface area of ​​the spherical silica particles is 4.0 m 2 The film of claim 1, wherein the film has a viscosity of 1 / g or less.

6. 2. The film according to claim 1, wherein the resin has a refractive index of 1.40 to 1.

50.

7. The film according to claim 1 , further comprising a transparent substrate layer, and the resin layer is laminated on at least one surface of the transparent substrate layer directly or via one or more other layers.

8. 10. The film of claim 1, having a dynamic friction coefficient of 0.80 or less.

9. 10. The film of claim 1 having a haze of 20.0% or less.

10. The film of claim 1, having a thickness of 1.0 to 100 μm.

11. The film of claim 1 which is an optical film.

12. A display device comprising the film according to any one of claims 1 to 11.

13. The display device according to claim 12, which is a liquid crystal display device or an organic electroluminescence display device.

Citation Information

Patent Citations

  • Active energy ray curable composition and film using the same

    JP6508559B2

  • Transparent electrode film

    JP7078169B1