Compound, monomer, polymer, photoresist composition and pattern forming method
Enol ether and halomethyl ether compounds with acid-labile groups address insolubility issues in EUV photoresists, enhancing sensitivity and resolution for advanced semiconductor manufacturing.
Patent Information
- Application Number
- JP2024082911
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-06
AI Technical Summary
Current photoresist compositions face challenges in achieving high resolution and sensitivity for next-generation EUV lithography due to insolubility issues of aromatic fragments in conventional developers, leading to patterning defects.
Development of enol ether and halomethyl ether compounds with acid-labile groups and halogen atoms, forming acid-sensitive monomers and polymers that create soluble cleavage fragments for improved EUV absorption and developer compatibility.
The proposed compounds and polymers enhance EUV photoresist sensitivity and resolution, reducing linewidth roughness and patterning defects, thereby improving semiconductor device manufacturing processes.
Smart Images

Figure 2024170303000001 
Figure 2024170303000002 
Figure 2024170303000003
Abstract
Description
[Technical field]
[0001] The present invention relates generally to the manufacture of electronic devices. More particularly, the present invention relates to enol ether compounds, halomethyl ether compounds, monomers and polymers formed from such compounds, photoresist compositions comprising such polymers, and patterning methods using the photoresist compositions. The compounds, monomers, polymers, photoresist compositions, and patterning methods are particularly useful in the formation of lithographic patterns useful in the manufacture of semiconductor devices. [Background technology]
[0002] A photoresist composition is a light-sensitive material used to transfer a pattern to one or more underlying layers, such as a metal, semiconductor, or dielectric layer disposed on a substrate. Positive-tone chemically amplified photoresist compositions are conventionally used for high resolution processing. Such resist compositions typically include a polymer with acid labile groups and a photoacid generator (PAG). A layer of the photoresist composition is patternwise exposed to activating radiation, and the PAG generates acid in the exposed areas. During post-exposure baking, the acid causes cleavage of the acid labile groups of the polymer. This creates a difference in solubility characteristics between the exposed and unexposed areas of the photoresist layer in a developer solution. In a positive tone development (PTD) process, the exposed areas of the photoresist layer become soluble in a developer, typically an aqueous base developer, and are removed from the substrate surface. The unexposed areas, which are insoluble in the developer, remain after development to form a positive tone relief image. The resulting relief image allows for selective processing of the substrate.
[0003] To increase the integration density of semiconductor devices and enable the formation of structures with dimensions in the nanometer (nm) range, photoresists and photolithography processing tools with high resolution capabilities have been developed and continue to be developed. One approach to achieve nm-scale feature sizes in semiconductor devices is to use activating radiation with short wavelengths, for example 193 nm or less, for exposure of the photoresist layer. To further improve lithography performance, immersion lithography tools have been developed to effectively increase the numerical aperture (NA) of the lens of the imaging device. This is achieved by using a relatively high refractive index fluid, typically water, between the final surface of the imaging device and the top surface of the semiconductor wafer.
[0004] ArF excimer laser (193 nm) immersion tools are currently pushing the limits of lithographic processing up to 16 nm and 14 nm device nodes using multiple (double, triple, or higher) patterning techniques. However, the use of multiple patterning can be costly in terms of increased material usage and the number of process steps required compared to single-exposure direct imaging patterns. Therefore, photoresist compositions useful in next-generation EUV (13.5 nm) lithography are becoming increasingly important for advanced device nodes. As a result of the shrinking feature sizes associated with these nodes, the performance requirements of photoresist compositions are becoming even more stringent. Desired performance characteristics include, for example, high sensitivity to activating radiation, high resolution, and good line width roughness (LWR).
[0005] One way to increase EUV photoresist sensitivity is to increase the absorption cross section at 13.5 nm. Absorption at 13.5 nm is an atomic property of the material and can be theoretically calculated using known atomic absorption. Typical atoms that make up resist materials, such as carbon, oxygen, hydrogen, and nitrogen, exhibit very weak EUV absorption. Absorption cross section can be increased, for example, by incorporating halogen atoms (e.g., F, Cl, Br, I) into the photoresist polymer, with iodine being particularly useful for increasing absorption. (Patent Document 1) discloses an acid-cleavable iodine-containing monomer for use in forming a photoresist polymer. The monomer includes a (meth)acryloyl polymerizable group and an acid labile group that is a tertiary ester. The acid labile group includes monocyclic or polycyclic unsubstituted or substituted C rings with one or more iodine atom substituents. 6~30 Arylene group or C 3~30 These monomers include heteroarylene groups. Incorporation of such monomers into photoresist polymers can increase the EUV absorption cross section, but the aromatic fragments that cleave upon interaction with photoacid are insoluble in conventional TMAH developers and can cause patterning defects. Therefore, it is desirable to have more developer-soluble cleavage fragments.
[0006] There is a need in the art for compounds, monomers, polymers, photoresist compositions, and patterning methods that address one or more of the problems associated with the prior art. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] U.S. Patent No. 10,095,109B1 [Patent Document 2] U.S. Patent No. 8,431,325 [Patent Document 3] U.S. Pat. No. 4,189,323 [Non-patent literature]
[0008] [Non-Patent Document 1] Wallow,T.et al Proc.SPIE 6921,69211F,2008 Summary of the Invention [Means for solving the problem]
[0009] According to a first aspect of the present invention, there is provided a compound, the compound being represented by the formula C 6~30 Aromatic or C 3~30 The compound comprises a heteroaromatic core comprising a first substituent comprising (i) an enol ether group or (ii) a substituted or unsubstituted halomethyl ether group, a second substituent comprising an acid labile group, and a third substituent that is a halogen atom, and the core is optionally further substituted.
[0010] Also provided are monomers, including the reaction product of (i) an enol ether or halomethyl ether compound described herein and (ii) a monomer precursor comprising a polymerizable group and a group selected from an -OH group or a -C(O)OH group, the reaction product including an acetal or ketal linker formed by reaction between the enol ether or halomethyl ether moiety of the compound and the -OH or -C(O)OH group of the monomer precursor.
[0011] Also provided is a method for making a monomer, the method comprising reacting (i) an enol ether or halomethyl ether compound described herein with (ii) a monomer precursor comprising a polymerizable group and a group selected from an -OH group or a -C(O)OH group, the monomer comprising an acetal or ketal linker formed by reaction between the enol ether or halomethyl ether moiety of the compound and the -OH or -C(O)OH group of the monomer precursor.
[0012] Also provided are polymers that include repeat units of the monomers described herein.
[0013] Also provided is a polymer comprising the reaction product of (i) an enol ether or halomethyl ether compound described herein and (ii) a first polymer comprising a first repeat unit comprising one or more groups selected from -OH or -C(O)OH, the reaction product including an acetal or ketal linker formed by reaction between the enol ether or halomethyl ether moiety of the compound and an -OH or -C(O)OH group of the first repeat unit, thereby forming a modified first repeat unit.
[0014] Also provided is a method for making a polymer, the method comprising reacting (i) an enol ether or halomethyl ether compound described herein with (ii) a first polymer comprising a first repeat unit comprising one or more groups selected from -OH or -C(O)OH, the polymer comprising an acetal or ketal linker formed by reaction between the enol ether or halomethyl ether moiety of the compound and an -OH or -C(O)OH group of the first repeat unit, thereby forming a modified first repeat unit.
[0015] Also provided is a photoresist composition comprising the polymer described herein and a solvent. The photoresist composition typically further comprises a photoacid generator.
[0016] Also provided is a method of forming a pattern that includes (a) forming a layer of photoresist from a photoresist composition described herein on a substrate, (b) exposing the photoresist layer to activating radiation, and (c) developing the exposed photoresist layer to provide a resist relief image. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The singular forms "a", "an" and "the" are intended to include the singular and plural unless the context dictates otherwise. All ranges disclosed herein are inclusive of the endpoints, which are independent and interoperable with each other. When an element is said to be "on" or "across" another element, it may be in direct contact with the other element or there may be intervening elements between them. In contrast, when an element is said to be "directly on" another element, there are no intervening elements present.
[0018] Unless otherwise indicated, a "substituted" group means that one or more of its hydrogen atoms have been replaced by one or more substituents. Exemplary substituents include, but are not limited to, hydroxy (OH), halogen (e.g., F, Cl, I, Br), C 1~18 Alkyl, C 1~8 Haloalkyl, C 3~12 Cycloalkyl, C with at least one aromatic ring 6~12 Aryl (e.g., phenyl, biphenyl, naphthyl, etc., where each ring is either substituted or unsubstituted aromatic), C 7~19 Aryl alkyl, C 7~12 For purposes of determining carbon number, if a group is substituted, the number of carbon atoms in the group is the total number of carbon atoms in such group, excluding the carbon atoms of any substituents.
[0019] As used herein, "acid labile group" refers to a group that is formed on the polymer with bond cleavage, optionally and typically with thermal treatment, resulting in the formation of a polar group, such as a carboxylic acid group or an alcohol group, and optionally and typically with the moiety connected to the cleaved bond being cleaved from the polymer by the catalytic action of an acid. Such acids are typically photogenerated acids, with bond cleavage occurring during post-exposure baking. Suitable acid labile groups include, for example, tertiary alkyl ester groups, secondary or tertiary aryl ester groups, secondary or tertiary ester groups with a combination of alkyl and aryl groups, tertiary alkoxy groups, acetal groups, or ketal groups. Acid labile groups are also referred to in the art as "acid cleavable groups", "acid cleavable protecting groups", "acid labile protecting groups", "acid leaving groups", "acid decomposable groups", and "acid sensitive groups".
[0020] Enol Ether Compounds The enol ether compound of the present invention is 6~30 Aromatic or C 3~30 It comprises a heteroaromatic core comprising a first substituent comprising an enol ether group, a second substituent comprising an acid labile group, and a third substituent which is a halogen atom, such as F, Cl, Br, or I, with F and I being preferred, and I being especially preferred. The core may be further substituted or unsubstituted.
[0021] Suitable enol ether compounds of the present invention include, for example, those represented by formula (1): [ka] (In the formula, Ar 1 is C 6~30 Aromatic or C 3~30 Heteroaromatic core; R 1 each independently represents a moiety containing an acid labile group; 2 are independently H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10represents haloalkyl, optionally including as part of its structure -O-, -S-, -N(R 3 )-, -C(O)-, -C(O)O-, or -C(O)N(R 3 )-, and R 3 is H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 Heteroalkyl, substituted or unsubstituted C 6~30 Aryl, or substituted or unsubstituted C 4~30 Heteroaryl, any two R 2 The groups may optionally be joined together to form a ring, and one or more R 2 Group and L 2 may optionally be joined together to form a ring; X independently represents a halogen atom; L 1 and L 2 each independently represents a single bond or a linking group; a, b, and c independently represent an integer of 1 or greater; the core may be optionally further substituted). In this specification, "optionally further substituted" means that the core may optionally contain one or more additional substituents in addition to the substituents shown in the corresponding general formula.
[0022] Ar 1 is preferably selected from pyridine, benzene, naphthalene, acenaphthylene, quinoline, isoquinoline, fluorene, carbazole, anthracene, phenanthrene, pyrene, coronene, triphenylene, chrysene, phenalene, benz[a]anthracene, dibenz[a,h]anthracene, benzo[a]pyrene, or pentacene, more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, chrysene, phenalene, benz[a]anthracene, dibenz[a,h]anthracene, or benzo[a]pyrene, even more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, chrysene, or phenalene, and most preferably selected from Ar 1is benzyl or naphthyl, each of which may be optionally further substituted.
[0023] R 1 Suitable acid labile groups for include, for example, one or more acid labile ester groups such as tertiary ester groups, e.g., tertiary alkyl esters, tertiary aryl esters, and tertiary esters having a combination of aryl and alkyl groups attached to a tertiary carbon atom, and secondary ester groups, e.g., secondary aryl esters, and secondary esters having an aryl and alkyl group attached to a secondary carbon atom, tertiary alkoxy groups, acetal groups, and ketal groups. Preferably, R 1 contains an acid labile ester, acetal, or ketal group.
[0024] Suitable exemplary acid labile groups include the following: [ka] (In these formulas, * represents the point of attachment to another part of the compound).
[0025] R 2 is H, substituted or unsubstituted C 1~10 Alkyl, or substituted or unsubstituted C 1~10 Fluoroalkyl is preferred, and any two R 2 The groups together may optionally form a ring.
[0026] Preferred halogen atoms for X are F, Cl, Br, and I. Among these, a fluorine atom and an iodine atom are more preferred, and iodine is particularly preferred.
[0027] L 1 and L 2 is typically a single bond or a substituted or unsubstituted C 1~30 Alkylene, substituted or unsubstituted C 1~30 Heteroalkylene, substituted or unsubstituted C 3~30 Cycloalkylene, substituted or unsubstituted C1~30 Heterocycloalkylene, substituted or unsubstituted C 6~30 Arylene, substituted or unsubstituted C 7~30 Aryl alkylene, substituted or unsubstituted C 1~30 Heteroarylene, substituted or unsubstituted C 3~30 Heteroarylalkylene, -O-, -C(O)-, -C(O)O-, -S-, -S(O)2-, or -N(R 44 )-S(O)-; R 44 is H, linear or branched C 1~20 Alkyl, monocyclic or polycyclic C 3~20 Cycloalkyl, or monocyclic or polycyclic C 3~20 It is a heterocycloalkyl.
[0028] a and b are each typically an integer of 1 to 6, more typically an integer of 1 to 3 or 1 to 2. a+b is an integer ranging from 2 to Ar 1 up to the total number of available (otherwise unsubstituted) aromatic ring carbon atoms. a+b is typically an integer from 2 to 10, more typically from 2 to 6, or 2 to 4. c is typically an integer from 1 to 3, more typically 1 or 2.
[0029] Suitable compounds of formula (1) include, for example: [ka] [ka] [ka]
[0030] The enol ether compounds described above can be readily prepared by those skilled in the art using known synthetic techniques. For example, the compounds can be prepared by mixing a reactant, such as a phenol, with a vinyloxyalkyl chloride, bromide, or iodide, a base, and a solvent, optionally with an alkali halide catalyst, preferably an alkali iodide. The solvent is typically an organic solvent, such as N,N-dimethylformamide, tetrahydrofuran, dimethylsulfoxide, N-methyl-2-pyrrolidone, 1,4-dioxane, or a combination thereof. The reaction is carried out at a temperature and for a time effective to cause reaction of the reactants in the reaction mixture to form an enol ether. The reaction temperature is typically 0 to 150°C, preferably 25 to 100°C. The reaction time is typically 1 minute to 96 hours, preferably 2 to 24 hours. The product compound can be purified by techniques known in the art, such as column chromatography.
[0031] The enol ether compounds described herein are particularly useful in forming acid-sensitive monomers and acid-sensitive polymers.In a first aspect, the enol ether compounds can be used as direct reactants to form acid-sensitive monomers, which can be polymerized to form acid-sensitive polymers.In a further aspect, the enol ether compounds can be used as direct reactants to form acid-sensitive polymers by reacting with precursor (or base) polymers.The acid-sensitive monomers and polymers of the present invention are described below.
[0032] Halomethyl Ether Compounds Suitable halomethyl ether compounds of the present invention include, for example, those represented by formula (2): [ka] (In the formula, Ar 1 , R 1 , R 2 , X, L 1 , L 2, a, b, and c are as defined above for formula (1); Y independently represents Cl, Br, or I. The core may be optionally further substituted.
[0033] Suitable halomethyl ether compounds of formula (2) include, for example: [ka] [ka]
[0034] The halomethyl ether compounds of the present invention can be easily prepared by those skilled in the art using known synthetic techniques. For example, the halomethyl ether group can be covalently attached to a substrate having an alkyl alcohol group or an aryl alcohol group by reacting the OH group with an aqueous solution of formaldehyde or paraformaldehyde, followed by treatment with an aqueous solution of hydrogen chloride or hydrogen bromide. An exemplary process for adding a halomethyl ether group to a substrate having an alkyl alcohol group, followed by an esterification reaction with a tertiary ester to form a halomethyl ether compound according to the present invention, is shown in the following scheme: [ka]
[0035] The halomethyl ether compounds described herein are particularly useful in forming acid-sensitive monomers and acid-sensitive polymers.In a first aspect, the halomethyl ether compounds can be used as reactants to form acid-sensitive monomers, which can be polymerized to form acid-sensitive polymers.In a further aspect, the halomethyl ether compounds can be used as direct reactants to form acid-sensitive polymers by reacting with precursor (or base) polymers.The acid-sensitive monomers and polymers of the present invention are described below.
[0036] Acid-Sensitive Monomers The enol ether compounds or halomethyl ether compounds described herein can be used to synthesize acid-sensitive monomers that can be used to synthesize polymers. The acid-sensitive monomers include the reaction products of (i) the enol ether compounds or halomethyl ether compounds described herein and (ii) monomer precursors that include a polymerizable group, typically a group that includes an ethylenically unsaturated carbon-carbon double bond, such as a polymerizable vinyl group, and a group selected from an -OH group or a -C(O)OH group. The reaction products include acetal or ketal linkers formed by the reaction between the enol ether moiety of the enol ether compound or the halomethyl ether moiety of the halomethyl ether compound and the -OH group or the -C(O)OH group of the monomer precursor.
[0037] Suitable polymerizable groups for the monomer precursors (and the resulting acid-sensitive monomers) include ethylenically unsaturated carbon-carbon double bonds. The polymerizable groups are typically substituted or unsubstituted C 2~20 It is selected from an alkenyl group, a substituted or unsubstituted norbornyl group, a substituted or unsubstituted (meth)acrylic group, a substituted or unsubstituted vinyl ether group, a substituted or unsubstituted vinyl ketone group, a substituted or unsubstituted vinyl ester group, a substituted or unsubstituted vinyl aromatic group, or a substituted or unsubstituted N-maleimide group. Among these, the substituted or unsubstituted (meth)acrylic group and the substituted or unsubstituted vinyl aromatic group are preferred.
[0038] Suitable monomer precursors are not particularly limited and include, for example: [ka] [ka]
[0039] Suitable monomer precursors are commercially available or can be prepared using methods known in the art.
[0040] The acid sensitive monomer preferably contains a moiety of formula (3): [ka] (In the formula, Ar 1 , R 1 , X, L 1 , L 2 , a, b, and c are as described above for formula (1); R 4 are independently H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 Heteroalkyl, substituted or unsubstituted C 6~30 Aryl, or substituted or unsubstituted C 4~30 Heteroaryl, any two R 4 The groups may optionally be joined together to form a ring, R 4 Group and L 2 may optionally be joined together to form a ring; R 4 The R group and another portion of the monomer not shown in formula (3) may optionally be joined to form a ring; * represents a point of attachment to another portion of the monomer). 4 Preferred for is H, substituted or unsubstituted C 1~5 Alkyl, substituted or unsubstituted C 1~5 Fluoroalkyl, or substituted or unsubstituted C 1~5 It is heteroalkyl.
[0041] The acid sensitive monomer is preferably of formula (4): [ka] (In the formula, Ar 1 , R 1 , R 4 , X, L 1 , L 2 , a, b, and c are as described above for formula (3); L 3 are independently a single bond or a divalent linking group; P represents a polymerizable group as described above with respect to the monomer precursor; and d is 1 or 2, except that when c is greater than 1, then d is 1.
[0042] L 3 is typically a single bond, or a substituted or unsubstituted 1~30 Alkylene, substituted or unsubstituted C 1~30 Heteroalkylene, substituted or unsubstituted C 3~30 Cycloalkylene, substituted or unsubstituted C 1~30 Heterocycloalkylene, substituted or unsubstituted C 6~30 Arylene, substituted or unsubstituted C 7~30 Aryl alkylene, substituted or unsubstituted C 1~30 Heteroarylene, substituted or unsubstituted C 3~30 Heteroarylalkylene, -O-, -C(O)-, -C(O)O-, -S-, -S(O)2- or -N(R 44 )-S(O)-; R 44 is H, linear or branched C 1~20 Alkyl, monocyclic or polycyclic C 3~20 Cycloalkyl, or monocyclic or polycyclic C 3~20 Heterocycloalkyl. 3 The divalent linking group preferably comprises aromatic groups covalently bonded to adjacent acetal or ketal oxygen atoms.
[0043] Preferred for P are polymerizable groups having vinyl groups, such as vinyl aromatic (eg styrene) groups and (meth)acrylate groups.
[0044] The acid sensitive monomer is typically of formula (4a) or (4b): [ka] (In the formula, Ar 1 , R 1 , R 4 , X, L 1 , L 2 , L 3 , a, b, c, and d are as described above for formula (4); R 5 are independently H, a halogen atom, or a substituted or unsubstituted C 1~6represents alkyl, typically H or methyl; Ar 2 is a substituted or unsubstituted C 6~30 Aromatic group, or substituted or unsubstituted C 3~30 Ar is a heteroaromatic group. 2 is selected from the polyvalent forms of benzene, pyridine, naphthalene, acenaphthylene, quinoline, isoquinoline, fluorene, carbazole, anthracene, phenanthrene, pyrene, coronene, triphenylene, chrysene, phenalene, benz[a]anthracene, dibenz[a,h]anthracene, benzo[a]pyrene, or pentacene, preferably from the polyvalent forms of benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, chrysene, phenalene, benz[a]anthracene, dibenz[a,h]anthracene, and benzo[a]pyrene, more preferably from the polyvalent forms of benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, chrysene, and phenalene, and most preferably from the polyvalent forms of benzene (e.g. phenylene).
[0045] Non-limiting examples of acid sensitive monomers include: [ka] [ka] [ka] [ka]
[0046] The monomers of the present invention can be prepared using any suitable method known in the art. For example, in the case of enol ether reactants, the monomers can be prepared by mixing the monomer precursor and the enol ether compound described herein with a suitable acid catalyst and solvent. Suitable monomer precursors are commercially available or can be prepared using methods known in the art. The acid catalyst can be an organic or inorganic acid catalyst, such as methanesulfonic acid, p-toluenesulfonic acid, hydrochloric acid, acetic acid, sulfuric acid, trifluoroacetic acid, citric acid, malic acid, formic acid, or combinations thereof. The solvent is typically an anhydrous organic solvent, such as propylene glycol methyl ether acetate, propylene glycol methyl ether, N,N-dimethylformamide, tetrahydrofuran, dimethylsulfoxide, N-methyl-2-pyrrolidone, 1,4-dioxane, or combinations thereof. The reaction is carried out at a temperature and for a time effective to cause the reaction between the reactants to form the acid sensitive monomer. The reaction temperature is typically 0 to 150°C, preferably 25 to 100°C. The reaction time is typically 1 hour to 96 hours, preferably 2 to 48 hours. The product monomer can be purified by techniques known in the art, such as precipitation, column chromatography recrystallization, or a combination thereof.
[0047] Monomers prepared from halomethyl ether reactants can be prepared by combining the monomer precursor and halomethyl ether compound described herein with a suitable acid catalyst and solvent. The monomers of the present invention can be prepared using any suitable method known in the art, for example, by combining the monomer precursor and halomethyl ether compound with a suitable base and solvent. Suitable monomer precursors are commercially available or can be prepared using any method known in the art. The base can be an inorganic or organic base, for example, potassium carbonate, cesium carbonate, sodium hydride, N,N-diisopropylethylamine, or 1,8-diazabicycloundec-7-ene. The solvent is typically an organic solvent, for example, N,N-dimethylformamide, tetrahydrofuran, dimethylsulfoxide, N-methyl-2-pyrrolidone, 1,4-dioxane, or a combination thereof. The reaction is carried out at a temperature and for a time effective to cause reaction between the reactants to form the acid-sensitive monomer. The reaction temperature is typically 0 to 150°C, preferably 25 to 100°C. The reaction time is typically 1 hour to 96 hours, preferably 2 to 48 hours. The product monomer can be purified by techniques known in the art, such as precipitation, column chromatography recrystallization, or a combination thereof.
[0048] Acid-Sensitive Polymers According to a further aspect of the present invention, an acid-sensitive polymer is provided. As described below, the polymer may be a direct or indirect reaction product of an enol ether compound or a halomethyl ether compound as described herein. The polymer may be a homopolymer, or more typically a copolymer having multiple different repeat units, for example, 2, 3, 4 or more different repeat units.
[0049] The polymer preferably comprises an acid-sensitive repeat unit comprising a moiety of formula (5): [ka] (In the formula, Ar1 , R 1 , R 4 , X, L 1 , L 2 , a, b, and c are as described above for formula (3); ** represents the point of attachment of the repeat unit to another moiety).
[0050] The acid sensitive repeat unit is preferably of formula (6): [ka] (In the formula, Ar 1 , R 1 , R 4 , X, L 1 , L 2 , L 3 a, b, c, and d are as described above with respect to formula (4); BB represents the polymer backbone. Exemplary of BB is an ethylenically unsaturated carbon-carbon double bond, preferably a polymerizable vinyl group, e.g., a substituted or unsubstituted C 2~20 It is a polymer backbone formed by polymerization of an alkenyl group, a substituted or unsubstituted norbornyl group, a substituted or unsubstituted (meth)acrylic group, a substituted or unsubstituted vinyl ether group, a substituted or unsubstituted vinyl ketone group, a substituted or unsubstituted vinyl ester group, a substituted or unsubstituted vinyl aromatic group (e.g., styrene), or a substituted or unsubstituted N-maleimide group. Among these, the substituted or unsubstituted vinyl aromatic group and the substituted or unsubstituted (meth)acrylate group are typical.
[0051] The acid sensitive repeat unit is typically of formula (6a) or (6b): [ka] (In the formula, Ar 1 , Ar 2 , R 1 , R 4 , R 5 , X, L 1 , L 2 , L 3 , a, b, c, and d are as described above with respect to formulas (4a) and (4b).
[0052] The acid sensitive repeat units are typically present in the polymer in an amount of from 5 to 100 mol %, from 5 to 90 mol %, more typically from 5 to 50 mol %, and even more typically from 10 to 30 mol %, based on all repeat units in the polymer.
[0053] When the acid-sensitive polymer is in the form of a copolymer, it may contain one or more additional structurally different acid-sensitive repeat units as described above, or may contain one or more other types of repeat units. Other suitable additional repeat units include, for example, those containing acid labile groups, base decomposable groups, hydroxyaryl groups, fluoroalcohol groups, or lactone groups.
[0054] In some embodiments, the polymer may include additional repeat units having aromatic groups, which may be substituted or unsubstituted. The aromatic groups may be monocyclic or polycyclic C 1 -C 2 -H 2 -O 3 -C 1 -O 2 -O 3 ... 5~60 When the aromatic group is polycyclic, the rings or ring groups may be fused (such as naphthyl), directly linked (such as biaryls, such as biphenyl), bridged by heteroatoms (such as triphenylamino or diphenylene ether), and / or contain a combination of fused and directly linked rings (such as binaphthyl).
[0055] Monocyclic or polycyclic C 5~60 The aromatic group may be substituted or unsubstituted. Exemplary substituents include substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 1~30 Haloalkyl, substituted or unsubstituted C 3~30 Cycloalkyl, substituted or unsubstituted C 1~30 Heterocycloalkyl, substituted or unsubstituted C 2~30 Alkenyl, substituted or unsubstituted C 2~30 Alkynyl, substituted or unsubstituted C6~30 Aryl, substituted or unsubstituted C 7~30 Aryl alkyl, substituted or unsubstituted C 7~30 Alkylaryl, substituted or unsubstituted C 3~30 Heteroaryl, substituted or unsubstituted C 4~30 Heteroarylalkyl, halogen, -OR 51 , -SR 52 , or -NR 53 R 54 These include, but are not limited to, where R 51 ~R 54 are each independently hydrogen or a substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 3~30 Cycloalkyl, substituted or unsubstituted C 2~30 Heterocycloalkyl, substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 7~30 Aryl alkyl, substituted or unsubstituted C 3~30 Heteroaryl, or substituted or unsubstituted C 4~30 Preferably, the aromatic group is a substituted C 6~30 Aryl or substituted C 7~30 heteroaryl group, where the aromatic group is -OR 51 , -SR 52 , or -NR 53 R 54 and the like, where R 51 ~R 54 are each independently hydrogen or a substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 3~20 Cycloalkyl, substituted or unsubstituted C 2~20 Heterocycloalkyl, substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 7~30 Aryl alkyl, substituted or unsubstituted C 3~30 Heteroaryl, or substituted or unsubstituted C 4~30 It is heteroarylalkyl.
[0056] The repeat units having an aromatic group are typically present in the polymer in an amount of from 5 to 80 mol %, more typically from 10 to 50 mol %, and even more typically from 10 to 40 mol %, based on all repeat units in the polymer.
[0057] The one or more additional repeat units are not particularly limited and can be selected, for example, from the optional repeat units described below with respect to further methods for forming the polymers of the present invention, or other repeat units known in the art for use in photoresist polymers.
[0058] The acid-sensitive polymer may include one or more additional repeat units that include an acid-labile group, such as an acid-labile ester or acetal group. Suitable monomers for these repeat units include, for example: [ka] [ka] (In the formula, R d is hydrogen, fluorine, C 1~5 Alkyl or C 1~5 fluoroalkyl, typically hydrogen or methyl).
[0059] The repeat units having an acid labile group are typically present in the acid-sensitive polymer in an amount of from 10 to 80 mol %, more typically from 25 to 75 mol %, and even more typically from 30 to 70 mol %, based on the total repeat units in the acid-sensitive polymer.
[0060] In some embodiments, the acid-sensitive polymer may include one or more additional repeat units having an aromatic group, which may be substituted or unsubstituted. The aromatic group may be a monocyclic or polycyclic C 1 -C 2 -H 2 -O 3 -C 1 -O 2 -O 3 ... 5~60When the aromatic group is polycyclic, the rings or ring groups may be fused (such as naphthyl), directly linked (such as biaryls, such as biphenyl), bridged by heteroatoms (such as triphenylamino or diphenylene ether), and / or contain a combination of fused and directly linked rings (such as binaphthyl).
[0061] Monocyclic or polycyclic C 5~60 The aromatic group may be substituted or unsubstituted. Exemplary substituents include substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 1~30 Haloalkyl, substituted or unsubstituted C 3~30 Cycloalkyl, substituted or unsubstituted C 1~30 Heterocycloalkyl, substituted or unsubstituted C 2~30 Alkenyl, substituted or unsubstituted C 2~30 Alkynyl, substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 7~30 Aryl alkyl, substituted or unsubstituted C 7~30 Alkylaryl, substituted or unsubstituted C 3~30 Heteroaryl, substituted or unsubstituted C 4~30 Heteroarylalkyl, halogen, -OR 51 , -SR 52 , or -NR 53 R 54 These include, but are not limited to, where R 51 ~R 54 are each independently hydrogen or a substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 3~30 Cycloalkyl, substituted or unsubstituted C 2~30 Heterocycloalkyl, substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 7~30 Aryl alkyl, substituted or unsubstituted C 3~30 Heteroaryl, or substituted or unsubstituted C 4~30 Preferably, the aromatic group is a substituted C 6~30 Aryl or substituted C7~30 heteroaryl group, where the aromatic group is -OR 51 , -SR 52 , or -NR 53 R 54 and the like, where R 51 ~R 54 are each independently hydrogen or a substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 3~20 Cycloalkyl, substituted or unsubstituted C 2~20 Heterocycloalkyl, substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 7~30 Aryl alkyl, substituted or unsubstituted C 3~30 Heteroaryl, or substituted or unsubstituted C 4~30 It is heteroarylalkyl.
[0062] When an additional repeat unit having an aromatic group is used, it is typically present in the acid-sensitive polymer in an amount of from 5 to 80 mol %, more typically from 10 to 50 mol %, and even more typically from 10 to 40 mol %, based on the total repeat units in the acid-sensitive polymer.
[0063] The acid-sensitive polymer may include a repeat unit that includes a lactone group. Suitable repeat units may be derived, for example, from monomers of formula (6a) or formula (6b): [ka]
[0064] In formula (6a), R is hydrogen, fluorine, cyano, substituted or unsubstituted C 1~10 Alkyl, or substituted or unsubstituted C 1~10 Preferably, R is hydrogen, fluorine, or a substituted or unsubstituted C 1~5 It is an alkyl group, typically methyl. 3 is a single bond or a substituted or unsubstituted C 1~30 Alkylene, substituted or unsubstituted C 1~30Heteroalkylene, substituted or unsubstituted C 3~30 Cycloalkylene, substituted or unsubstituted C 1~30 Heterocycloalkylene, substituted or unsubstituted C 6~30 Arylene, substituted or unsubstituted C 7~30 Aryl alkylene, or substituted or unsubstituted C 1~30 Heteroarylene, or substituted or unsubstituted C 3~30 L may be a divalent linking group containing one or more of heteroarylalkylene; 3 is optionally selected from, for example, -O-, -C(O)-, -C(O)-O-, -S-, -S(O)2-, and -N(R 44 )-S(O)-, R 44 is hydrogen, linear or branched C 1~20 Alkyl, monocyclic or polycyclic C 3~20 Cycloalkyl, or monocyclic or polycyclic C 3~20 R may be heterocycloalkyl. 14 is a monocyclic, polycyclic, or fused polycyclic C 4~20 In formula (6b), R 15 is a hydrogen or non-hydrogen substituent, typically a substituted or unsubstituted C 1~10 alkyl, and n is 1 or 2.
[0065] Suitable exemplary lactone-containing monomers of formulas (6a) and (6b) include the following: [ka] where R is as defined above. When present, the acid-sensitive polymer typically contains lactone repeat units in an amount of from 5 to 60 mol %, typically from 20 to 55 mol %, more typically from 25 to 50 mol %, based on the total repeat units in the acid-sensitive polymer.
[0066] The acid-sensitive polymer may include a base-soluble repeat unit having a pKa of less than or equal to 12. For example, the base-soluble repeat unit may be derived from a monomer of formula (7): [ka]
[0067] In formula (7), R g is hydrogen, fluorine, cyano, substituted or unsubstituted C 1~10 Alkyl, or substituted or unsubstituted C 1~10 Preferably, R g is hydrogen, fluorine, or substituted or unsubstituted C 1~5 Q is an alkyl group, typically methyl. 4 is a substituted or unsubstituted C 1~30 Alkylene, substituted or unsubstituted C 3~30 Cycloalkylene, substituted or unsubstituted C 1~30 Heterocycloalkylene, substituted or unsubstituted C 6~30 Arylene, substituted or unsubstituted divalent C 7~30 Aryl alkyl, substituted or unsubstituted C 1~30 Heteroarylene or substituted or unsubstituted divalent C 3~30 W may include one or more of the following: heteroarylalkyl, -C(O)-O, or -C(O)-O. W is a base-soluble group, for example, hydroxyl (OH); -C(O)-OH; fluorinated alcohol such as -C(CF3)2OH; imide; or -NH-S(O)2-Y. 1 (where Y 1 is C 1~4 alkyl or fluoroalkyl, typically C 1~4 In formula (7), a is 1, 2, or 3.
[0068] Non-limiting examples of monomers of formula (7) include: [ka] (In the formula, R gis as described above). When present, the acid-sensitive polymer typically contains the above-described base-soluble repeat units in an amount of from 5 to 60 mol %, typically from 20 to 55 mol %, more typically from 25 to 50 mol %, based on the total repeat units in the acid-sensitive polymer.
[0069] The acid-sensitive polymer may optionally include one or more additional repeat units. The additional repeat structural units may include one or more additional units for the purpose of adjusting the properties of the photoresist composition, such as, for example, etch rate and solubility. The additional units may include, for example, one or more of styrene, (meth)acrylate, vinyl ether, vinyl ketone, or vinyl ester type units. When present in the acid-sensitive polymer, the one or more additional repeat units may be used in an amount of 90 mol % or less, typically 3 to 50 mol %, based on the total repeat units of the acid-sensitive polymer.
[0070] Non-limiting examples of acid-sensitive polymers include: [ka] [ka] [ka] [ka] [ka] [ka] [ka] where a, b, c, and d represent the mole fractions of the corresponding repeat units, and the sum of the mole fractions of all repeat units in each polymer is 1.
[0071] The acid-sensitive polymer typically has a weight average molecular weight (Mw) of 1,000 to 50,000 Daltons (Da), in particular 2,000 to 30,000 Da, more particularly 3,000 to 20,000 Da, and even more particularly 3,000 to 10,000 Da. The polydispersity index (PDI) of the acid-sensitive polymer, which is the ratio of Mw to number average molecular weight (Mn), is typically 1.1 to 3, in particular 1.1 to 2. Molecular weight values are determined by gel permeation chromatography (GPC) using polystyrene standards.
[0072] The polymers of the present invention can be prepared by various methods. For example, the polymers can be produced by polymerizing the acid-sensitive monomers of the present invention described above together with one or more optional comonomers described above. The polymers can be prepared using any suitable method in the art, such as free radical polymerization, anionic polymerization, cationic polymerization, etc. One or more monomers corresponding to the repeat units of the precursor polymer can be combined, for example, using a suitable solvent and initiator, or can be fed separately and polymerized in a reactor. The polymerization can be carried out under suitable conditions, such as by heating at an effective temperature, by exposure to actinic radiation at an effective wavelength, or a combination thereof. When the polymer contains hydroxy-substituted vinyl aromatic repeat units, such repeat units can be formed by polymerization of hydroxy-substituted vinyl aromatic monomers, such as hydroxystyrene. Alternatively, hydroxy-substituted vinyl aromatic repeat units can be prepared by using protected hydroxy aromatic repeat units, such as acetoxystyrene repeat units. The acetoxy group is then removed by reaction with a base to produce the hydroxy aromatic repeat units. The base is then removed, for example, by treating the crude polymer with an acidic ion exchange resin.
[0073] Acid sensitive polymers can also be prepared by reacting (i) an enol ether or halomethyl ether compound described herein with (ii) a precursor polymer comprising a repeat unit containing one or more -OH or -C(O)OH groups. The reaction product contains an acetal or ketal linker formed by reaction between the enol ether moiety of the compound and the -OH or -C(O)OH group of the repeat unit, thereby forming a modified repeat unit.
[0074] The precursor polymer comprises one or more repeat units having an -OH or -C(O)OH group with which an enol ether compound can react. Suitable such repeat units for the precursor polymer include the following: [ka] [ka]
[0075] The repeat units of the precursor polymer containing an -OH group or a -C(O)OH group are typically present in the acid-sensitive polymer in an amount of from 1 to 100 mol %, from 5 to 100 mol %, from 5 to 90 mol %, more typically from 5 to 50 mol %, and even more typically from 10 to 30 mol %, based on all repeat units of the precursor polymer.
[0076] The precursor polymer can be prepared using any suitable method in the art, such as free radical polymerization, anionic polymerization, cationic polymerization, etc. One or more monomers corresponding to the repeating units of the precursor polymer can be combined, for example, using a suitable solvent and initiator, or can be fed separately and polymerized in a reactor. The polymerization can be carried out under any suitable conditions, such as by heating at an effective temperature, by exposure to actinic radiation at an effective wavelength, or a combination thereof. When the precursor polymer contains hydroxy-substituted vinyl aromatic repeating units, such repeating units can be formed as described above for the first polymer synthesis method by polymerization of hydroxy-substituted vinyl aromatic monomers, such as hydroxystyrene, or by using protected hydroxy aromatic repeating units, such as acetoxystyrene repeating units.
[0077] The precursor polymer can be reacted with the enol ether compound of the halomethyl ether compound of the present invention using any suitable method known in the art. For the enol ether compound, the polymer of the present invention can be prepared by mixing the precursor polymer and the enol ether compound with a suitable acid catalyst and solvent. The acid catalyst can be an organic or inorganic acid catalyst, such as methanesulfonic acid, p-toluenesulfonic acid, hydrochloric acid, acetic acid, sulfuric acid, trifluoroacetic acid, citric acid, malic acid, formic acid, or a combination thereof. The solvent is typically an organic solvent, such as propylene glycol methyl ether acetate, propylene glycol methyl ether, N,N-dimethylformamide, tetrahydrofuran, dimethylsulfoxide, N-methyl-2-pyrrolidone, 1,4-dioxane, or a combination thereof. The reaction is carried out at a temperature and for a time effective to cause the reaction of the reactants in the reaction mixture to form the polymer of the present invention. The reaction temperature is typically 0 to 150°C, preferably 25 to 100°C. The reaction time is typically 1 hour to 96 hours, preferably 2 to 48 hours. The product polymer can be purified by techniques known in the art, such as column chromatography.
[0078] For halomethyl ether compounds, the polymer of the present invention can be prepared, for example, by mixing the polymer precursor of the present invention and the halomethyl ether compound with a suitable base and solvent. The base can be an organic or inorganic base, such as potassium carbonate, cesium carbonate, sodium hydride, N,N-diisopropylethylamine (DIPEA), or 1,8-diazabicycloundec-7-ene. The solvent is typically an organic solvent, such as N,N-dimethylformamide, tetrahydrofuran, dimethylsulfoxide, N-methyl-2-pyrrolidone, 1,4-dioxane, or a combination thereof. The reaction is carried out at a temperature and for a time effective to cause reaction of the reactants in the reaction mixture to form an acid-sensitive monomer. The reaction temperature is typically 0 to 150° C., preferably 25 to 100° C. The reaction time is typically 1 hour to 96 hours, preferably 2 to 48 hours. The product polymer can be purified by techniques known in the art, such as precipitation.
[0079] Photoresist Composition The photoresist composition of the present invention comprises the above-mentioned polymer and solvent, and may also comprise one or more additional optional components. The polymer can perform various functions in the composition, depending on the nature of the polymer and other components of the photoresist composition. For example, in a preferred embodiment, the polymer can function as a photoresist matrix material. In another embodiment, the polymer can function as a surface-active polymer, and can be separated from other components of the photoresist composition during the coating process due to the relative surface energy properties of the polymer and the other components.
[0080] The photoresist composition may further comprise a photoacid generator (PAG). The PAG may be of the ionic or non-ionic type. The PAG may be in polymeric or non-polymeric form. In the polymeric form, the PAG may be present as a moiety in a repeat unit of the polymer described above or a different polymer, the repeat unit being derived from a polymerizable PAG monomer.
[0081] Suitable PAG compounds have the formula G + A - and G + is a photoactive cation, and A - is an anion capable of generating a photoacid. The photoactive cation is preferably selected from onium cations, preferably iodonium or sulfonium cations. Particularly suitable anions include those whose conjugate acids have a pKa of -15 to 10. The anion is typically an organic anion having a sulfonate group or a non-sulfonate type group (such as sulfonamidate, sulfonimidate, methide or borate).
[0082] In some embodiments, the photoactive cation can be a sulfonium cation or an iodonium cation. For example, the photoactive cation can be a sulfonium cation of formula (8) or an iodonium cation of formula (9): [ka]
[0083] In formulas (8) and (9), R 17 ~R 21 are each independently a substituted or unsubstituted C 1~20 Alkyl, substituted or unsubstituted C 3~20 Cycloalkyl, substituted or unsubstituted C 2~20 Alkenyl, substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 6~30 Iodoaryl, substituted or unsubstituted C 3~30 Heteroaryl, substituted or unsubstituted C 7~20Aryl alkyl, or substituted or unsubstituted C 4~20 Each R may be a heteroaryl, alkyl, or a combination thereof. 17 ~R 19 may be individually or may be linked to another group R via a single bond or a divalent linking group. 17 ~R 19 R may be linked to form a ring. 20 and R 21 may be individually or may be linked together via a single bond or a divalent linking group to form a ring. 17 ~R 21 may optionally include a divalent linking group as part of its structure. 17 ~R 21 may optionally include acid labile groups independently selected from, for example, tertiary alkyl ester groups, secondary or tertiary aryl ester groups, secondary or tertiary ester groups having a combination of alkyl and aryl groups, tertiary alkoxy groups, acetal groups, or ketal groups.
[0084] Exemplary sulfonium cations of formula (8) can include one or more of the following: [ka] [ka]
[0085] Exemplary iodonium cations of formula (9) can include one or more of the following: [ka]
[0086] Exemplary organic anions having a sulfonate group can include one or more of the following: [ka]
[0087] Exemplary non-sulfonated anions can include one or more of the following: [ka]
[0088] Commonly used onium salts include, for example, triphenylsulfonium trifluoromethanesulfonate, (p-tert-butoxyphenyl)diphenylsulfonium trifluoromethanesulfonate, tris(p-tert-butoxyphenyl)sulfonium trifluoromethanesulfonate, triphenylsulfonium p-toluenesulfonate; di-t-butylphenyliodonium perfluorobutanesulfonate, and di-t-butylphenyliodonium camphorsulfonate. Other useful PAG compounds are known in the chemically amplified photoresist art, such as nonionic sulfonyl compounds, such as 2-nitrobenzyl-p-toluenesulfonate, 2,6-dinitrobenzyl-p-toluenesulfonate, and 2,4-dinitrobenzyl-p-toluenesulfonate; sulfonic acid esters, such as 1,2,3-tris(methanesulfonyloxy)benzene, 1,2,3-tris(trifluoromethanesulfonyloxy)benzene, and 1,2,3-tris(p-toluenesulfonyloxy)benzene; diazomethane derivatives, such as bis(benzenesulfonyl)diazomethane, bis(p-toluenesulfonyl) Diazomethane; glyoxime derivatives such as bis-O-(p-toluenesulfonyl)-α-dimethylglyoxime and bis-O-(n-butanesulfonyl)-α-dimethylglyoxime; sulfonate derivatives of N-hydroxyimide compounds such as N-hydroxysuccinimide methanesulfonate and N-hydroxysuccinimide trifluoromethanesulfonate; and halogen-containing triazine compounds such as 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine and 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine. Suitable photoacid generators are described in detail in (Patent Document 2) and (Patent Document 3).
[0089] The photoresist composition may further include a basic quencher and / or a photodecomposable quencher (PDQ) (also known as a photodecomposable base), each of which, if used, is typically present in an amount of 0.01 to 10 wt %, based on the total solids content of the photoresist composition.
[0090] Exemplary basic quenching agents include, for example, straight chain aliphatic amines such as tributylamine, trioctylamine, triisopropanolamine, tetrakis(2-hydroxypropyl)ethylenediamine; n-tert-butyldiethanolamine, tris(2-acetoxy-ethyl)amine, 2,2',2'',2'''-(ethane-1,2-diylbis(azanetriyl))tetraethanol, 2-(dibutylamino)ethanol, and 2,2',2''-nitrilotriethanol; cyclic aliphatic amines such as 1-(tert-butoxycarbonyl)-4-hydroxypiperidine, tert-butyl 1-pyrrolidinecarboxylate, tert-butyl 2-ethyl-1H-imidazole-1-carboxylate, di-tert-butyl piperazine-1,4-dicarboxylate, and N-(2-acetoxy-ethyl)morpholine; pyridine, di-tert-butylpyridine, and pyridine. linear and cyclic amides and derivatives thereof, such as N,N-bis(2-hydroxyethyl)pivalamide, N,N-diethylacetamide, N1,N1,N3,N3-tetrabutylmalonamide, 1-methylazepan-2-one, 1-allylazepan-2-one, and tert-butyl 1,3-dihydroxy-2-(hydroxymethyl)propan-2-ylcarbamate; ammonium salts, such as quaternary ammonium salts of sulfonates, sulfamates, carboxylates, and phosphonates; imines, such as primary and secondary aldimines and ketimines; optionally substituted diazines, such as pyrazines, piperazines, and phenazines; optionally substituted diazoles, such as pyrazoles, thiadiazoles, and imidazoles; and optionally substituted pyrrolidones and cyclohexylpyrrolidines, such as 2-pyrrolidone.
[0091] The photolytic quencher PDQ generates a relatively weak acid upon irradiation that does not rapidly react with acid labile groups in the photoresist composition. Exemplary photolytic quenchers include, for example, C, which is also useful for preparing photolytic cations and preferably strong acid generators. 1~20 Weak acids such as carboxylic acids or C 1~20 Exemplary carboxylic acids include those paired with anions of sulfonic acids. Exemplary carboxylic acids include formic acid, acetic acid, propionic acid, tartaric acid, succinic acid, cyclohexane carboxylic acid, benzoic acid, salicylic acid, etc. Exemplary carboxylic acids include p-toluenesulfonic acid, camphorsulfonic acid, etc. In a preferred embodiment, the photolytic quencher is a photolytic organic zwitterionic compound such as diphenyliodonium-2-carboxylate.
[0092] The photoresist composition may further comprise a material that comprises one or more base labile groups ("base labile materials"). As referred to herein, a base labile group is a functional group that can undergo a cleavage reaction to provide a polar group such as a hydroxyl, carboxylic acid, sulfonic acid, etc., in the presence of an aqueous alkaline developer after the exposure and post-exposure bake steps. The base labile group will not significantly react (e.g., will not undergo a bond scission reaction) prior to the development step of the photoresist composition that comprises the base labile group. Thus, for example, the base labile group will be substantially inert during the pre-exposure soft bake, exposure, and post-exposure bake steps. By "substantially inert" it is meant that ≦5%, preferably ≦1%, of the base labile groups (or moieties) decompose, cleave, or react during the pre-exposure soft bake, exposure, and post-exposure bake steps. The base labile groups are highly reactive under typical photoresist development conditions, for example, using an aqueous alkaline photoresist developer such as an aqueous solution of 0.26 normal (N) tetramethylammonium hydroxide (TMAH). For example, a 0.26N aqueous solution of TMAH can be used to develop the resist pattern using a single puddle development or dynamic development process, where the 0.26N TMAH developer is dispensed onto the imaged photoresist layer for an appropriate time, such as 10-120 seconds. An exemplary base labile group is an ester group, typically a fluorinated ester group. Preferably, the base labile material is substantially immiscible with other solid components of the photoresist composition and has a lower surface energy than the other solid components. When coated onto a substrate, the base labile material can thereby separate to the top surface of the formed photoresist layer from the other solid components of the photoresist composition.
[0093] The base labile material is preferably a polymeric material, also referred to herein as a base labile polymer, which may comprise one or more repeat units that contain one or more base labile groups. For example, the base labile polymer may comprise repeat units that contain two or more base labile groups, which may be the same or different. A preferred base labile polymer comprises at least one repeat unit that contains two or more base labile groups, for example, a repeat unit that contains two or three base labile groups.
[0094] The base labile polymer may be a polymer comprising repeat units derived from a monomer of formula (E1) [ka] (In the formula, X b is a polymerizable group selected from vinyl and acrylic; L 5 is a substituted or unsubstituted linear or branched C 1~20 Alkylene, substituted or unsubstituted C 3~20 a divalent linking group containing one or more of cycloalkylene, -C(O)-, or -C(O)O-; R k is a substituted or unsubstituted C 1~20 a fluoroalkyl group, provided that the carbon atom bonded to the carbonyl (C=O) of formula (E1) is substituted with at least one fluorine atom).
[0095] Exemplary monomers of formula (E1) include: [ka]
[0096] The base labile polymer can include repeat units that include more than one base labile group. For example, the base labile polymer can include repeat units derived from monomers of formula (E2): [ka] (In the formula, X b and R kis as defined in formula (E1); L 6 is a substituted or unsubstituted linear or branched C 1~20 Alkylene, substituted or unsubstituted C 3~20 a polyvalent linking group that includes one or more of cycloalkylene, -C(O)-, or -C(O)O-; and n is an integer of 2 or greater, e.g., 2 or 3.
[0097] Exemplary monomers of formula (E2) include: [ka]
[0098] The base labile polymer may include repeat units that include one or more base labile groups. For example, the base labile polymer may include repeat units derived from monomers of formula (E3): [ka] (In the formula, X b is as defined in formula (E1); L 7 is a substituted or unsubstituted linear or branched C 1~20 Alkylene, substituted or unsubstituted C 3~20 a divalent linking group containing one or more of cycloalkylene, -C(O)-, or -C(O)O-; L f is a substituted or unsubstituted C 1~20 R is a fluoroalkylene group, in which the carbon atom bonded to the carbonyl (C=O) in formula (E1) is replaced with at least one fluorine atom; m is a substituted or unsubstituted linear or branched C 1~20 Alkyl, or substituted or unsubstituted C 3~20 (cycloalkyl).
[0099] Exemplary monomers of formula (E3) include: [ka]
[0100] In further aspects of the invention, the base labile polymer may include one or more base labile groups and one or more acid labile groups, such as one or more acid labile ester moieties (e.g., t-butyl esters) or acid labile acetal groups. For example, the base labile polymer may include a repeat unit that includes a base labile group and an acid labile group. That is, both the base labile group and the acid labile group are present on the same repeat unit. In another example, the base labile polymer may include a first repeat unit that includes a base labile group and a second repeat unit that includes an acid labile group. Preferred photoresists of the invention may exhibit reduced defects associated with resist relief images formed from the photoresist composition. When present, the content of the base labile polymer is typically 0.01 to 10 wt %, based on the total solids content of the photoresist composition.
[0101] The base labile polymer can be prepared by any suitable method in the art, including those described herein for the first and second polymers.For example, the base labile polymer can be obtained by polymerization of the respective monomers under any suitable conditions, such as by heating at an effective temperature, by irradiation with actinic radiation at an effective wavelength, or a combination thereof.In addition or alternatively, one or more base labile groups can be grafted onto the backbone of the polymer by a suitable method.
[0102] The photoresist composition may further include one or more additional optional additives. For example, the optional additives may include chemical dyes and contrast agents, anti-streak agents, plasticizers, speed enhancers, sensitizers, surfactants, and the like, or combinations thereof. When present, the content of each optional additive is typically 0.01 to 10 wt % based on the total solids content of the photoresist composition.
[0103] Exemplary surfactants include fluorinated and non-fluorinated surfactants, and can be ionic or non-ionic, with non-ionic surfactants being preferred.Exemplary fluorinated non-ionic surfactants include perfluorinated C4 surfactants such as FC-4430 and FC-4432 surfactants (3M Corporation); and fluorodiols such as POLYFOX PF-636, PF-6320, PF-656, and PF-6520 fluorosurfactants (Omnova).
[0104] The photoresist composition further comprises a solvent for dissolving the components of the composition and facilitating its coating on a substrate. Preferably, the solvent is an organic solvent conventionally used in the manufacture of electronic devices. Suitable solvents include, for example, aliphatic hydrocarbons such as hexane and heptane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as dichloromethane, 1,2-dichloroethane and 1-chlorohexane; alcohols such as methanol, ethanol, 1-propanol, isopropanol, tert-butanol, 2-methyl-2-butanol, 4-methyl-2-pentanol, and diacetone alcohol (4-hydroxy-4-methyl-2-pentanone) (DAA); propylene glycol monomethyl ether (PGME); ethers such as diethyl ether, tetrahydrofuran, 1,4-dioxane, and anisole; acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, and tetrahydrofuran; ketones such as ethyl acetate, n-butyl acetate, propylene glycol monomethyl ether acetate (PGMEA), ethyl lactate (EL), hydroxyisobutyrate methyl ester (HBM) and ethyl acetoacetate; lactones such as gamma-butyrolactone (GBL) and epsilon-caprolactone; lactams such as N-methylpyrrolidone; nitriles such as acetonitrile and propionitrile; cyclic or acyclic carbonates such as propylene carbonate, dimethyl carbonate, ethylene carbonate, propylene carbonate, diphenyl carbonate and propylene carbonate; polar aprotic solvents such as dimethylsulfoxide and dimethylformamide; water; and combinations thereof. Of these, preferred solvents are PGME, PGMEA, EL, GBL, HBM, CHO, DAA, and combinations thereof. The solvent is typically organic. This means that the cumulative content of organic solvents (minor impurities) in the solvent is 50% by weight or more, typically 95% by weight or more, 95% by weight or more, 98% by weight or more, or 100% by weight, based on the total weight of the solvent.The total solvent content in the photoresist composition (i.e., the cumulative solvent content for all solvents) is typically 40-99% by weight, such as 70-99% by weight, or 85-99% by weight, based on the total photoresist composition. The desired solvent content will depend, for example, on the desired thickness of the photoresist layer to be coated and the coating conditions.
[0105] The photoresist composition can be prepared according to known procedures. For example, the composition can be prepared by dissolving the solid components of the photoresist composition in a solvent. The photoresist composition or one or more components of the composition can be optionally subjected to one or more purification processes, such as filtration and / or ion exchange processes. The desired total solids content of the composition will depend on factors such as the desired final layer thickness. The solids content of the photoresist composition is typically 1 to 10 wt %, more preferably 1 to 5 wt %, based on the total weight of the composition.
[0106] Pattern Formation Method A patterning method using the photoresist composition of the present invention is described below. Suitable substrates on which the photoresist composition can be coated include electronic device substrates. A variety of electronic device substrates, such as semiconductor wafers; polycrystalline silicon substrates; packaging substrates such as multichip modules; flat panel display substrates; substrates for light emitting diodes (LEDs) such as organic light emitting diodes (OLEDs), and the like, can be used in the present invention, with semiconductor wafers being typical. Such substrates are typically composed of one or more of silicon, polysilicon, silicon oxide, silicon nitride, silicon oxynitride, silicon germanium, gallium arsenide, aluminum, sapphire, tungsten, titanium, titanium-tungsten, nickel, copper, and gold. Suitable substrates can be in the form of wafers, such as those used in the manufacture of integrated circuits, optical sensors, flat panel displays, optical integrated circuits, and LEDs. Such substrates can be of any suitable size. A typical wafer substrate diameter is 200-300 millimeters (mm), although wafers having smaller and larger diameters can be suitably used in accordance with the present invention. The substrate may include one or more layers or structures that may optionally include operating or operable parts of the device being formed.
[0107] Typically, one or more lithographic layers, such as a hardmask layer, e.g., a spin-on carbon (SOC), amorphous carbon, or metal hardmask layer, a CVD layer, such as a silicon nitride (SiN), silicon oxide (SiO), or silicon oxynitride (SiON) layer, an organic or inorganic underlayer, or a combination thereof, are provided on the upper surface of the substrate prior to coating the photoresist composition of the invention. Such layers, together with an overcoated photoresist layer, form a lithographic material stack.
[0108] Optionally, a layer of adhesion promoter can be applied to the substrate surface before coating the photoresist composition. If an adhesion promoter is desired, any suitable adhesion promoter for polymer films can be used, such as silanes, typically organosilanes such as trimethoxyvinylsilane, triethoxyvinylsilane, hexamethyldisilazane, or aminosilane couplers such as gamma-aminopropyltriethoxysilane. Particularly suitable adhesion promoters include those sold under the names AP 3000, AP 8000, and AP 9000S, available from DuPont Electronics & Imaging, Marlborough, Massachusetts.
[0109] The photoresist composition may be coated on the substrate by any suitable method, such as spin coating, spray coating, dip coating, or doctor blading. For example, application of a layer of photoresist may be achieved by spin coating the photoresist in a solvent using a coating track, where the photoresist is dispensed onto a rotating wafer. During dispensing, the wafer is typically rotated at a speed of up to 4,000 revolutions per minute (rpm), e.g., 200-3,000 rpm, e.g., 1,000-2,500 rpm, for a period of 15-120 seconds to obtain a layer of the photoresist composition on the substrate. It will be appreciated by those skilled in the art that the thickness of the coated layer may be adjusted by varying the rotation speed and / or the solids content of the composition. The photoresist layer formed from the composition of the present invention typically has a dry layer thickness of 10-200 nanometers (nm), preferably 15-100 nm, more preferably 20-60 nm.
[0110] The photoresist composition is typically then soft baked to minimize the solvent content in the layer, thereby forming a tack-free coating and improving the adhesion of the layer to the substrate. The soft bake is performed, for example, on a hot plate or in an oven, with a hot plate being typical. The soft bake temperature and time will depend, for example, on the particular photoresist composition and thickness. The soft bake temperature is typically 90-170°C, for example 110-150°C. The soft bake time is typically 10 seconds to 20 minutes, for example 1 minute to 10 minutes or 1 minute to 5 minutes. The heating time can be readily determined by one of ordinary skill in the art based on the components of the composition.
[0111] The photoresist layer is then patternwise exposed to activating radiation to create a solubility difference between exposed and unexposed regions. Reference herein to exposing a photoresist composition to radiation activating for the composition indicates that the radiation can form a latent image in the photoresist composition. Exposure is typically performed through a patterned photomask having optically transparent and optically opaque regions corresponding to the exposed and unexposed regions of the resist layer, respectively. Such exposure may alternatively be performed without a photomask in a direct write process, typically used for electron beam lithography. Activating radiation typically has a wavelength of less than 400 nm, less than 300 nm, or less than 200 nm, with wavelengths of 248 nm (KrF), or 13.5 nm (EUV), or electron beam lithography being preferred. Of these, 13.5 nm (EUV) is particularly preferred. Exposure energy is typically between 1 and 200 millijoules per square centimeter (mJ / cm2). 2 ), preferably 10 to 100 mJ / cm 2 , more preferably 20 to 50 mJ / cm 2 and depends on the exposure tool and the components of the photoresist composition. In some embodiments, the activating radiation is EUV at a wavelength of 13.5 nm.
[0112] Exposure of the photoresist layer is followed by a post-exposure bake (PEB) of the exposed photoresist layer. PEB can be performed, for example, on a hotplate or in an oven, with a hotplate being typical. The conditions for PEB will depend, for example, on the particular photoresist composition and layer thickness. PEB is typically performed at a temperature of 80-150° C. and for a time of 30-120 seconds. A latent image is formed in the photoresist, defined by polarity switching (exposed regions) and polarity non-switching regions (unexposed regions).
[0113] The exposed photoresist layer is then developed with a suitable developer to selectively remove areas of the layer that are soluble in the developer, while the remaining insoluble areas form a resultant photoresist pattern relief image. In a positive tone development (PTD) process, the exposed areas of the photoresist layer are removed during development, while the unexposed areas remain. Conversely, in a negative tone development (NTD) process, the exposed areas of the photoresist layer remain, while the unexposed areas are removed during development. Application of the developer can be accomplished by any suitable method, such as those described above with respect to application of the photoresist composition, with spin coating being typical. The development time is a period of time effective to remove the soluble areas of the photoresist, with times of 5 to 60 seconds being typical. Development is typically performed at room temperature.
[0114] Suitable developers for the PTD process include aqueous base developers, such as tetramethylammonium hydroxide (TMAH), preferably 0.26 normal (N) TMAH, quaternary ammonium hydroxide solutions such as tetraethylammonium hydroxide, tetrabutylammonium hydroxide, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, and the like. Suitable developers for the NTD process are organic solvent based, meaning that the cumulative content of organic solvent in the developer is 50% by weight or more, typically 95% by weight or more, 95% by weight or more, 98% by weight or more, or 100% by weight based on the total weight of the developer. Suitable organic solvents for NTD developers include, for example, those selected from ketones, esters, ethers, hydrocarbons, and mixtures thereof. NTD developers are typically n-butyl acetate or 2-heptanone.
[0115] A coated substrate can be formed from the photoresist composition of the invention. Such a coated substrate comprises (a) a substrate having one or more layers on a surface thereof and (b) a layer of a photoresist composition over the one or more layers.
[0116] The photoresist pattern can be used, for example, as an etching mask, thereby allowing the pattern to be transferred to one or more successive underlying layers by known etching techniques, typically dry etching such as reactive ion etching. The photoresist pattern can be used, for example, for pattern transfer to an underlying hard mask layer, which in turn is used as an etching mask for pattern transfer to one or more layers below the hard mask layer. If the photoresist pattern is not consumed during pattern transfer, it can be removed from the substrate by known techniques, for example, oxygen plasma ashing or a wet strip process. When the photoresist composition is used in one or more such patterning processes, it can be used to manufacture semiconductor devices such as memory devices, processor chips (CPUs), graphic chips, optoelectronic chips, LEDs, OLEDs, as well as other electronic devices.
[0117] The following non-limiting examples illustrate the present invention. EXAMPLES
[0118] Synthesis of enol ether compounds Example 1 (Compound SM1) [ka] In a reaction vessel, 1-ethylcyclopentyl-2-hydroxy-5-iodobenzoate (36.0 g, 100 mmol) was suspended in DMF to give a 9 wt% solution. Cesium carbonate (65.1 g, 200 mmol) and sodium iodide (1.50 g, 10 mmol) were added neat to the solution to form a reaction mixture. (2-chloroethoxy)ethene (12.8 g, 120 mmol) was then slowly added dropwise to the reaction mixture with stirring. The reaction mixture was heated to an internal temperature of 70° C. for 4 hours. Additional (2-chloroethoxy)ethene (10.7 g, 100 mmol) was then added to the reaction mixture and the reaction mixture was heated at 70° C. for an additional 14 hours. The reaction mixture was allowed to cool to room temperature and then diluted with DI water (1.5 L) and the aqueous mixture was extracted with methyl tert-butyl ether (3×250 mL). The organic layers were combined, washed with water (5×200 mL), and the solvent was removed under reduced pressure to give the enol ether compound SM1 as a colorless oil (37.5 g, 87% yield). 1 H-NMR (500MHz, chloroform-d) δ(ppm): 7.94(d,1H,ArH), 7.66(dd,1H,ArH), 6.73(d,1H,ArH), 6.51(dd,1H,alkenyl-H), 4.27-4.18(m,3H,CH2 / alkenyl-H), 4.08-4.00(m,3H,CH2 / alkenyl-H), 2.29-2.18(m,2H,CH2), 2.09(q,2H,CH2), 1.82-1.68(m,4H,CH2), 1.67-1.57(m,2H,CH2), 0.93(t,3H,CH3).
[0119] Example 2 (Compound SM2) [ka] In a reaction vessel, 1-ethylcyclopentyl-2-hydroxy-3,5-diiodobenzoate (36.5 g, 75 mmol) was suspended in DMF to give a 12 wt% solution. Cesium carbonate (48.9 g, 150 mmol) and sodium iodide (1.12 g, 7.5 mmol) were added neat to form a reaction mixture. (2-chloroethoxy)ethene (12.8 g, 120 mmol) was then slowly added dropwise to the reaction mixture with stirring. The reaction mixture was heated to an internal temperature of 70° C. for 16 hours. Additional (2-chloroethoxy)ethene (9.6 g, 100 mmol) was then added to the reaction mixture and the reaction temperature was increased to 85° C. for 1 hour. The reaction mixture was allowed to cool to room temperature and then diluted with DI water (1.5 L) and the aqueous mixture was extracted with ethyl acetate (4×200 mL). The organic layers were combined, washed with DI water (5×200 mL), and the solvent was removed under reduced pressure to give the enol ether compound SM2 as a colorless oil (37.5 g, 90% yield). 1 H-NMR (500MHz, chloroform-d) δ(ppm): 8.20(d,1H,ArH), 7.92(d,1H,ArH), 6.52(dd,1H,alkenyl-H), 4.30-4.20(m,3H,CH2 / alkenyl-H), 4.10(t,2H,CH2), 4.05(dd,1H,alkenyl-H), 2.28-2.15(m,2H,CH2), 2.10(q,2H,CH2), 1.84-1.71(m,4H,CH2), 1.70-1.60(m,2H,CH2), 0.93(t,3H,CH3).
[0120] Example 3 (Compound SM3) [ka] In a reaction vessel, 2-phenylpropan-2-yl 2-hydroxy-5-iodobenzoate (11.5 g, 30 mmol) was suspended in DMP to give an 11.5 wt % solution. Cesium carbonate (19.5 g, 60 mmol) and sodium iodide (0.5 g, 3 mmol) were added neat to the solution to form a reaction mixture. (2-chloroethoxy)ethene (3.8 g, 36 mmol) was then slowly added dropwise to the reaction mixture with stirring. The reaction mixture was heated to an internal temperature of 70° C. for 4 hours. Additional (2-chloroethoxy)ethene (3.2 g, 30 mmol) was then added to the reaction mixture and the reaction mixture was heated at 70° C. for an additional 16 hours. The reaction mixture was allowed to cool to room temperature and then diluted with DI water (1.0 L) and the aqueous mixture was extracted with ethyl acetate (3×100 mL). The organic layers were combined, washed with DI water (5×100 mL), and the solvent was removed under reduced pressure to give the enol ether compound SM3 as a colorless oil (11.1 g, 82% yield). 1 H-NMR (500MHz, acetone-d6) δ(ppm): 7.90(s,1H,ArH), 7.79(d,1H,ArH), 7.53(d,2H,ArH), 7.34(t,2H,ArH), 7.23(t,1H,ArH), 7.00(d,1H,ArH), 6.57(dd,1H,alkenyl-H), 4.34(t,2H,CH2), 4.27(d,1H,alkenyl-H), 4.13(t,2H,CH2), 4.01(d,1H,alkenyl-H), 1.86(s,6H,CH3).
[0121] Synthesis of acid-sensitive monomers Example 4 (Monomer MC1) [ka] A reaction vessel is charged with monomer HPMA (5.0 g, 28.06 mmol) and 50 mL of anhydrous tetrahydrofuran. Trifluoroacetic acid (0.03 g) and the enol ether compound SM1 (12.0 g, 28.06 mmol) are added to the anhydrous solution to obtain a reaction mixture. The reaction mixture is stirred at room temperature (about 23° C.) for 24 hours. The reaction mixture is then passed through an alumina column and the solvent is completely removed under reduced pressure. Monomer MC1 is expected to be obtained.
[0122] Example 5 (Monomer MC2) [ka] A reaction vessel is charged with monomer HVN (5.1 g, 30.0 mmol) and 75 mL of anhydrous tetrahydrofuran. Trifluoroacetic acid (0.03 g) and enol ether compound SM2 (16.68.0 g, 30.0 mmol) are added to the anhydrous solution to obtain a reaction mixture. The reaction mixture is stirred at room temperature (about 23° C.) for 24 hours. The reaction mixture is then passed through an alumina column and the solvent is completely removed under reduced pressure. Monomer MC2 is expected to be obtained.
[0123] Example 6 (Monomer MC3) [ka] A reaction vessel is charged with monomer MVP (4.50 g, 30.0 mmol) and 60 mL of anhydrous tetrahydrofuran. Trifluoroacetic acid (0.03 g) and enol ether compound SM1 (13.56 g, 30.0 mmol) are added to the anhydrous solution to obtain a reaction mixture. The reaction mixture is stirred at room temperature (about 23° C.) for 24 hours. The reaction mixture is then passed through an alumina column and the solvent is completely removed under reduced pressure. Monomer MC3 is expected to be obtained.
[0124] Polymer synthesis The following polymers were prepared using the following materials: [ka]
[0125] Example 7 (Polymer CP-1) Polymer CP-1 was prepared from monomers MA-1 and MB-1 in a 50 / 50 molar feed ratio. A feed solution was prepared by dissolving monomer MA-1 (22.6 g, 140 mmol) and monomer MB-1 (28.5 g, 140 mmol) in 50 g of PGMEA. Separately, an initiator solution was prepared by dissolving 4.4 g of 2,2'-azobis(2,4-dimethylvaleronitrile) (obtained as V-65 from Wako Pure Chemical Industries, Ltd.) in 13 g of PGMEA and THF (wt / wt 1 / 1). The polymerization was carried out in a three-neck round bottom flask equipped with a water condenser and a thermometer to monitor the reaction in the flask. The reactor was charged with 25 g of PGMEA and heated to 75°C. The feed solution and initiator solution were each fed separately into the reactor over a period of 6 hours using a syringe pump. After the addition, the contents were stirred for an additional 2 hours. The contents were then cooled to room temperature and precipitated into 1 liter (L) of heptane. The resulting product was isolated by filtration and dried overnight at 35° C. under reduced pressure. The product was then dissolved in methanol (500 mL) and combined with a 30 wt % solution of sodium methoxide in methanol (0.6 g). The reaction mixture was heated at 67° C. until the reaction was complete. The reaction mixture was allowed to cool to room temperature and then neutralized by adding an acidic ion exchange resin C381H (Evoqua Water Technologies LLC). This reaction converts the repeat unit structure derived from 4-acetoxystyrene (MA-1) to 4-hydroxystyrene (MA-2). The polymer solution was precipitated in DI water to isolate a white solid (approximately 36.3 g) [Mw=6.5 kilodaltons (kDa), PDI=1.63], which was further dried under vacuum at 35° C. The molecular weight was determined by gel permeation chromatography (GPC) using polystyrene standards. [ka]
[0126] Example 8 (Polymer CP-2) Polymer CP-2 was prepared from monomers MA-1 and MB-2 in a 50 / 50 molar feed ratio. A feed solution was prepared by dissolving monomer MA-1 (28.22 g, 174 mmol) and monomer MB-2 (31.78 g, 174 mmol) in 40 g of PGMEA. Separately, an initiator solution was prepared by dissolving 4.41 g of 2,2'-azobis(2,4-dimethylvaleronitrile) (obtained as V-65 from Wako Pure Chemical Industries, Ltd.) in 13.23 g of PGMEA and THF (wt / wt 1 / 1). The polymerization was carried out in a three-neck round bottom flask equipped with a water condenser and a thermometer to monitor the reaction in the flask. The reactor was charged with 20 g of PGMEA and heated to 75°C. The feed solution and the initiator solution were fed separately into the reactor over a period of 6 hours using a syringe pump, respectively. After the addition, the contents were stirred for an additional 2 hours. The contents were then cooled to room temperature and precipitated into 1 liter (L) of heptane. The resulting product was isolated by filtration and dried overnight at 35° C. under reduced pressure. The product was then dissolved in methanol (600 mL) and combined with a 30 wt % solution of sodium methoxide in methanol (0.75 g). The reaction mixture was heated at 67° C. until the reaction was complete. The reaction mixture was allowed to cool to room temperature and then neutralized by adding an acidic ion exchange resin C381H (Evoqua Water Technologies LLC). This reaction converts the repeat unit structure derived from 4-acetoxystyrene (MA-1) to that derived from 4-hydroxystyrene (MA-2). The polymer solution was precipitated in DI water to isolate a white solid (approximately 42.2 g) [Mw=7.1 kilodaltons (kDa), PDI=1.74], which was further dried under vacuum at 35° C. The molecular weight was determined by gel permeation chromatography (GPC) using polystyrene standards. [ka]
[0127] Example 9 (Polymer P1) Polymer CP1 (15.0 g) and PGMEA were placed in a reaction vessel to obtain a 20 wt% solution. Traces of water were removed by azeotropic distillation. Trifluoroacetic acid (0.014 g) and the enol ether compound SM1 (4.38 g) were added to the anhydrous solution to obtain a reaction mixture. The reaction mixture was stirred at room temperature (about 23° C.) for 24 hours. The reaction mixture was then passed through an alumina column and the solvent was removed under reduced pressure to obtain polymer P1 in PGMEA (48.8 g, solids content 26.0%, yield 65.5%). The molecular weight was determined by gel permeation chromatography (GPC) using polystyrene standards. [Mw=7.9 kilodaltons (kDa), PDI=2.54]. [ka]
[0128] Example 10 (Polymer P2) Polymer CP-2 (15.2 g) and PGMEA were placed in a reaction vessel to obtain a 20 wt% solution. Traces of water were removed by azeotropic distillation. Trifluoroacetic acid (0.032 g) and the enol ether compound SM2 (8.39 g) were added to the anhydrous solution to obtain a reaction mixture. The reaction mixture was stirred at room temperature (about 23° C.) for 24 hours. The reaction mixture was then passed through an alumina column and the solvent was removed under reduced pressure to obtain polymer P2 in PGMEA (84.1 g, solids content 22.3%, yield 79.5%). The molecular weight was determined by gel permeation chromatography (GPC) using polystyrene standards. [Mw=8.9 kilodaltons (kDa), PDI=3.48]. [ka]
[0129] Example 11 (Polymer P3) Polymer CP-2 (14.1 g) and PGMEA were placed in a reaction vessel to obtain a 20 wt% solution. Traces of water were removed by azeotropic distillation. Trifluoroacetic acid (0.03 g) and the enol ether compound SM3 (8.09 g) were added to the anhydrous solution to obtain a reaction mixture. The reaction mixture was stirred at room temperature (about 23° C.) for 24 hours. The reaction mixture was then passed through an alumina column and the solvent was removed under reduced pressure to obtain polymer P3 in PGMEA (86.5 g, solids content 20.8%, yield 78.0%). (Mw=9.0 kilodaltons (kDa), PDI=3.49). It was further dried under vacuum at 35° C. The molecular weight was determined by gel permeation chromatography (GPC) using polystyrene standards. [ka]
[0130] Preparation of the Photoresist Composition Examples 12 to 16 Photoresist compositions were prepared by combining the components in the relative amounts shown in Table 1, where the amounts are expressed as weight percent (wt%) based on total solids. The photoresist compositions were prepared in a 1:1 weight ratio solvent mixture of PGMEA and methyl-2-hydroxyisobutyrate, respectively, resulting in a total solids content of 2.15 wt% based on the total composition. The compositions were shaken on a mechanical shaker and then filtered through a PTFE disk filter having a pore size of 0.2 microns.
[0131] [Table 1] [ka]
[0132] Lithography evaluation Line / Space (L / S) patterning Examples 17 to 21 The photoresist composition was evaluated for line / space (l / s) patterning under KrF exposure using a bright field mask pattern. 200 nm wafers for photolithography testing were coated with AR™ 3 organic antireflective agent (DuPont Electronics & Industrial) and soft baked at 205° C. for 60 seconds to obtain a first BARC layer of 60 nm. A coating of AR™ 40A organic antireflective agent (DuPont Electronics & Industrial) was then placed on top of the first BARC layer and soft baked at 215° C. for 60 seconds to obtain a second BARC layer with a thickness of about 80 nm. The photoresist composition was then coated onto the dual BARC stack and soft baked at 110° C. for 60 seconds to obtain a photoresist film layer with a thickness of about 50 nm. The wafers were exposed to 248 nm radiation on a Canon FPA-5000 ES4 scanner (NA=0.8, outer sigma=0.85, inner sigma=0.57) using a mask with 120 nm l / s patterns, respectively. The wafers were post-exposure baked at 100° C. for 60 seconds, developed with MF-CD26™ TMAH developer (DuPont Electronics & Industrial) for 60 seconds, rinsed with DI water, and dried. Critical dimension (CD) measurements of the formed l / s patterns were performed on a HITACHI S-9380 CD SEM. The sizing energy (E size ) and LWR (nm) of the lines were determined based on the CD measurements. The sizing energy is the exposure energy at which the target 120 nm line-space pattern was resolved.
[0133] The pseudo Z-factors reported below were determined according to Equation 1: Pseudo Z factor = (E size )×(LWR) 2 (Formula 1) (In the formula, E size is millijoules per square centimeter (mJ / cm 2 ), LWR is reported in nanometers (nm), and pseudo Z-factor is mJ×10 -11(The pseudo Z-factor is reported in units of 100 nm.) The pseudo Z-factor is a modified measure of photoresist performance based on the Z-factor, a known parameter indicator of RLS (Resolution, Line Edge Roughness, Sensitivity) photoresist performance (see, for example, Non-Patent Document 1). The pseudo Z-factor is calculated at a constant resolution (CD size). The results are shown in Table 2.
[0134] [Table 2]
[0135] As shown in Table 2, the inventive photoresist compositions PR-1, PR-2, and PR-3 achieved improved (lower) LWR and improved (lower) pseudo Z-factor compared to the comparative photoresist compositions CPR-1 and CPR-2.
[0136] Trench (TR) patterning Examples 22 to 26 The photoresist compositions were evaluated for trench (TR) patterning under KrF exposure using dark field mask patterns as described in Examples 17-21. size The LWR of the pattern and space was determined based on the CD measurement. The sizing energy was determined from the irradiation energy at which the target 120 nm trench pattern was resolved. The results are shown in Table 3.
[0137] [Table 3]
[0138] As shown in Table 3, the inventive photoresist compositions PR-1B, PR-2B, and PR-3B achieved improved (lower) LWR and improved (lower) pseudo Z-factor compared to the comparative photoresist compositions CPR1-B and CPR-2B.
Claims
1. A compound comprising: 6~30 Aromatic or C 3~30 A compound comprising a heteroaromatic core, said core comprising a first substituent comprising (i) an enol ether group or (ii) a substituted or unsubstituted halomethyl ether group, a second substituent comprising an acid labile group, and a third substituent that is a halogen atom, said core being optionally further substituted.
2. The compound has the formula (1) or (2): 【Chemistry 1】 (In the formula, Ar 1 is C 6~30 Aromatic or C 3~30 a heteroaromatic core; R 1 independently represents a moiety containing an acid labile group; Each R 2 are independently H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 represents haloalkyl, optionally including as part of its structure -O-, -S-, -N(R 3 )-, -C(O)-, -C(O)O-, or -C(O)N(R 3 )-, R 3 is H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 Heteroalkyl, substituted or unsubstituted C 6~30 Aryl, or substituted or unsubstituted C 4~30 Any two R in formula (1) represent heteroaryl. 2 group or two R in formula (2) 2 may optionally be joined together to form a ring, and one or more R 2 Group and L 2 may optionally be joined together to form a ring; X independently represents a halogen atom; Y independently represents Cl, Br, or I; Each L 1 and L 2 each independently represents a single bond or a divalent linking group; a, b, and c independently represent an integer of 1 or more; Ar 1 is optionally further substituted) The compound according to claim 1 ,
3. The compound according to claim 2, wherein X is a fluorine atom or an iodine atom.
4. R 1 The compound of claim 2 or 3, wherein is an acid labile ester, acetal, or ketal group.
5. The compound according to any one of claims 2 to 4, wherein c is 1.
6. The compound according to any one of claims 2 to 4, wherein c is 2.
7. L 2 Ga-S (O) 2 The compound according to any one of claims 2 to 6, comprising a - group.
8. 8. A monomer comprising the reaction product of (i) a compound according to any one of claims 1 to 7, and (ii) a monomer precursor comprising a polymerizable group and a group selected from an -OH group or a -C(O)OH group, the reaction product comprising an acetal or ketal linker formed by reaction between an enol ether or halomethyl ether moiety of the compound and the -OH or -C(O)OH group of the monomer precursor.
9. The monomer is represented by the following general formula (4): 【Chemistry 2】 (In the formula, P is a polymerizable group; Ar 1 is C 6~30 Aromatic or C 3~30 a heteroaromatic core; R 1 independently represents a moiety containing an acid labile group; R 4 are independently H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 Heteroalkyl, substituted or unsubstituted C 6~30 Aryl, or substituted or unsubstituted C 4~30 Heteroaryl, any two R 4 The groups may optionally be joined together to form a ring, R 4 Group and L 2 may optionally be joined together to form a ring; X independently represents a halogen atom; L 1 , L 2 , and L 3 each independently represents a single bond or a linking group; a, b, and c independently represent an integer of 1 or more; d is 1 or 2, except that when c is greater than 1, then d is 1; The core may be optionally further substituted. The monomer of claim 8 ,
10. A polymer comprising repeating units formed from the monomer according to claim 8 or 9.
11. 8. A polymer comprising the reaction product of (i) a compound according to any one of claims 1 to 7; and (ii) a first polymer comprising a first repeat unit comprising a group selected from one or more of -OH or -C(O)OH, wherein the reaction product comprises an acetal or ketal linker formed by reaction between an enol ether or halomethyl ether moiety of the compound and the -OH or -C(O)OH group of the first repeat unit, thereby forming a modified first repeat unit.
12. The modified first repeat unit has formula (4): 【Chemistry 3】 (In the formula, Ar 1 is C 6~30 Aromatic or C 3~30 a heteroaromatic core; R 1 independently represents a moiety containing an acid labile group; R 4 are independently H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 Heteroalkyl, substituted or unsubstituted C 6~30 Aryl, or substituted or unsubstituted C 4~30 Heteroaryl, any two R 4 The groups may optionally be joined together to form a ring, R 4 Group and L 2 may optionally be joined together to form a ring, R 4 The group and another portion of the monomer not shown in formula (4) may optionally be joined to form a ring; X independently represents a halogen atom; L 1 and L 2 each independently represents a single bond or a divalent linking group; a, b, and c independently represent an integer of 1 or more; ** represents the point of attachment of said modified first repeat unit to another moiety; The core is optionally further substituted. The polymer of claim 11 comprising the moiety:
13. 13. The polymer of claim 11 or 12, wherein the first repeat unit of the first polymer is formed from a monomer that includes a polymerizable vinyl group.
14. 14. The polymer of any one of claims 10 to 13, further comprising a second repeat unit comprising an acid labile group, a base labile group, a hydroxyaryl group, a fluoroalcohol group, or a lactone group, wherein the second repeat unit is structurally distinct from the modified first repeat unit.
15. A photoresist composition comprising the polymer according to any one of claims 10 to 14 and a solvent.
16. The photoresist composition of claim 15 further comprising a photoacid generator.
17. A pattern formation method comprising the steps of: (a) forming a photoresist layer on a substrate from the photoresist composition of claim 15 or 16; (b) exposing the photoresist layer to activating radiation; (c) developing the exposed photoresist layer to obtain a resist relief image; A pattern forming method comprising the steps of:
Citation Information
Patent Citations
US10,095,109B1
Radiation-sensitive copying composition
US4189323A
Compound, resin, resist composition and method for producing resist pattern
US8431325B2