Additive manufacturing device, manufacturing condition determination device, and manufacturing condition determination program

The additive manufacturing device addresses the challenge of controlling layer thickness in ceramic particle-containing materials by determining laser irradiation conditions based on penetration depth relationships, achieving precise and uniform layer formation.

JP2024173348APending Publication Date: 2024-12-12SINTOKOGIO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023091703
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Existing additive manufacturing devices struggle to accurately control the thickness of cured layers in three-dimensional shaped objects, particularly when using raw materials containing ceramic particles and ultraviolet curable resin, as conventional methods fail to account for the varying penetration depth and energy distribution due to multiple laser irradiations.

Method used

An additive manufacturing device that determines laser irradiation conditions by considering the relationship between the number of laser irradiations, first and second penetration depths, and target thickness, using formulas to adjust ultraviolet laser parameters such as energy, spot radius, and scanning speed to form layers with precise thickness.

Benefits of technology

Enables the formation of layers with consistent target thickness by accounting for the unique properties of ceramic particle-containing materials, ensuring uniformity and accuracy in three-dimensional object construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024173348000001_ABST
    Figure 2024173348000001_ABST
Patent Text Reader

Abstract

To provide a technique that can determine a laser irradiation condition for forming a layer with a target thickness when curing a raw material containing ceramic particles and an ultraviolet curing resin.SOLUTION: An additive manufacturing device comprises: a base; a layer forming part that forms a layer in which a raw material is cured by irradiating a raw material containing an ultraviolet curable resin and ceramic particles on the base with an ultraviolet laser multiple times so that at least a portion of the irradiation range overlaps with each other; and a controller. The controller acquires a target thickness of the layer and a number of times the layer forming part irradiates the raw material with ultraviolet laser, determines an irradiation condition of the ultraviolet laser based on a target film thickness, a number of irradiation and a previously acquired relationship, in which the previously acquired relationship is a relationship between the number of irradiation, a penetration depth into the raw material before the raw material is hardened, a penetration depth into the raw material after the raw material is hardened, and the irradiation condition, and causes the layer forming part to irradiate the ultraviolet laser based on the determined irradiation conditions.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an additive manufacturing device, a manufacturing condition determination device, and a manufacturing condition determination program. [Background technology]

[0002] Patent Document 1 discloses an additive manufacturing device that forms a three-dimensional object. This device forms a thin film of raw material containing ceramic powder and photocurable resin. This device selectively irradiates the formed thin film with an ultraviolet laser, curing the photocurable resin contained in the area irradiated with the ultraviolet laser, and forms a cured product (a layer of cured raw material) of any two-dimensional shape. This device stacks the two-dimensional cured product layer by layer to finally form a model. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-011050 Summary of the Invention [Problem to be solved by the invention]

[0004] In order to improve the quality of a three-dimensional object in the additive manufacturing device described in Patent Document 1, it is necessary to precisely control the thickness of the two-dimensional cured material that constitutes the object (the thickness of the cured layer). This disclosure provides a technique for determining the laser irradiation conditions for forming a layer with a target thickness when curing a raw material that contains ceramic particles and an ultraviolet curable resin. [Means for solving the problem]

[0005] An additive manufacturing apparatus according to one aspect of the present disclosure is an additive manufacturing apparatus for forming a three-dimensional shaped object, and includes a base, a layer forming unit, and a controller. A raw material including an ultraviolet curable resin and ceramic particles is supplied to the base. The layer forming unit forms a layer in which the raw material is hardened by irradiating the raw material on the base with an ultraviolet laser multiple times such that at least a part of the irradiation ranges overlap each other. The controller controls the layer forming unit. The controller acquires a target thickness of the layer and the number of irradiations of the raw material by the layer forming unit with the ultraviolet laser, and determines the irradiation conditions of the ultraviolet laser based on the acquired target thickness and number of irradiations and a relationship acquired in advance. The relationship acquired in advance is a relationship between the number of irradiations, a first penetration depth which is a penetration depth into the raw material before the raw material is hardened, a second penetration depth which is a penetration depth into the raw material after the raw material is hardened, and the irradiation conditions. The controller causes the layer forming unit to irradiate the ultraviolet laser based on the determined irradiation conditions. Effect of the Invention

[0006] According to the present disclosure, when a raw material containing ceramic particles and an ultraviolet curable resin is cured, it is possible to determine laser irradiation conditions for forming a layer with a target film thickness. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic diagram of an additive manufacturing apparatus according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram of an example in which a shaped object is formed. [Diagram 3] FIG. 3 is a schematic diagram of an example of scanning of an ultraviolet laser along the X direction. [Figure 4] FIG. 4 is a schematic diagram of an example in which a plurality of hardened portions are formed by irradiation with an ultraviolet laser. [Diagram 5] FIG. 5 is a schematic diagram of an example in which layers are formed by cross-hatching. [Figure 6] FIG. 6 is a flowchart showing a series of manufacturing condition determination processes performed by the controller. [Figure 7]FIG. 7 is an example of a graph showing the relationship between the irradiation energy of ultraviolet light and the curing depth of the cured portion. [Figure 8] (A) is a schematic diagram of an example of a first film, (B) is a schematic diagram of examples of the first film and the second film, and (C) is a schematic diagram of an example of a film formed when an area is irradiated with an ultraviolet laser N=(n+1) times. [Figure 9] FIG. 9 is a graph showing the predicted cured shape of the layer at each location. [Figure 10] FIG. 10 is a diagram showing the configuration of a manufacturing condition determination program. [Figure 11] FIG. 11 is a graph showing the curing depth when a raw material containing only an ultraviolet curable resin is cured. [Figure 12] FIG. 12 is a graph showing the hardening depth when a raw material containing an ultraviolet curing resin and ceramic particles is hardened. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Overview of the embodiment of the present disclosure] First, an overview of the embodiment of the present disclosure will be described.

[0009] (Clause 1) An additive manufacturing apparatus according to one aspect of the present disclosure is an additive manufacturing apparatus for forming a three-dimensional shaped object, and includes a base, a layer forming unit, and a controller. A raw material including an ultraviolet curable resin and ceramic particles is supplied to the base. The layer forming unit forms a layer in which the raw material is hardened by irradiating the raw material on the base with an ultraviolet laser multiple times such that at least a part of the irradiation ranges overlap each other. The controller controls the layer forming unit. The controller acquires a target thickness of the layer and the number of irradiations of the raw material by the layer forming unit with the ultraviolet laser, and determines the irradiation conditions of the ultraviolet laser based on the acquired target thickness and number of irradiations and a relationship acquired in advance. The relationship acquired in advance is a relationship between the number of irradiations, a first penetration depth which is a penetration depth into the raw material before the raw material is hardened, a second penetration depth which is a penetration depth into the raw material after the raw material is hardened, and the irradiation conditions. The controller causes the layer forming unit to irradiate the ultraviolet laser based on the determined irradiation conditions.

[0010] It is known that the cured shape of a raw material containing an ultraviolet curing resin and the irradiation conditions of an ultraviolet laser generally follow Lambert Beer's law. However, the present inventor found that when the raw material further contains ceramic particles, the penetration depth into the raw material after the raw material is cured changes from the penetration depth before the raw material is cured, and derived a new relationship that extends Lambert Beer's law. The new relationship is a relationship in which, when the ultraviolet laser is irradiated multiple times so that at least a part of the irradiation range overlaps with each other, if the penetration depth into the raw material before and after the curing of the raw material, the number of irradiations of the ultraviolet laser irradiated to the raw material, and the irradiation conditions of the laser are known, the cured shape of the raw material can be calculated. The penetration depth into the raw material before and after the curing of the raw material can be acquired in advance. Therefore, when the target film thickness (cured shape of the raw material) and the number of irradiations of the ultraviolet laser are set, the irradiation conditions of the laser can be determined using the above-mentioned previously acquired relationship. By using the above-mentioned previously acquired relationship, this additive manufacturing device can determine the irradiation conditions of the laser for forming a layer of the target film thickness when curing a raw material containing ceramic particles and an ultraviolet curing resin. The additive manufacturing tool can then form layers at the determined irradiation conditions.

[0011] (Clause 2) In the additive manufacturing apparatus according to Clause 1, the controller may calculate a second penetration depth based on the first penetration depth, the hardening depth of the first film formed when the ultraviolet laser is irradiated to a predetermined region of the raw material, and the hardening depth of the second film further formed when the ultraviolet laser is irradiated to the region on which the first film is formed, before determining the irradiation conditions. In this case, the additive manufacturing apparatus can obtain the second penetration depth in advance.

[0012] (Clause 3) In the additive manufacturing apparatus described in Clause 2, the second penetration depth may satisfy the relationship of the following mathematical formula (1).

number

[0013] (Clause 4) In the additive manufacturing apparatus according to any one of clauses 1 to 3, the previously acquired relationship may further include a minimum ultraviolet laser energy value at which the slurry-like raw material hardens. In this case, the additive manufacturing apparatus can determine the irradiation conditions in consideration of a critical value at which the slurry-like raw material changes into a solid state.

[0014] (Clause 5) In the additive manufacturing apparatus described in any one of clauses 1 to 4, the layer formation unit performs a first irradiation in which a scan of an ultraviolet laser along a first direction is moved a predetermined distance along a second direction intersecting the first direction, and the raw material is hardened by irradiating multiple times so that parts of the irradiation ranges overlap each other, and the number of irradiations, the first penetration depth, the second penetration depth, and the irradiation conditions may satisfy the relationships of the following mathematical formulas (2) to (5) as pre-acquired relationships.

number

[0015] (Clause 6) In the additive manufacturing apparatus described in Clause 5, after the first irradiation, the layer formation unit performs a second irradiation in which scanning along a second direction with an ultraviolet laser is performed multiple times while moving a predetermined distance along the first direction to harden the raw material, and the number of irradiations of the ultraviolet laser, the first penetration depth, and the second penetration depth may satisfy the relationship of the following mathematical expressions (6) and (7) as a pre-acquired relationship.

number

[0016] (Clause 7) In the additive manufacturing apparatus according to any one of clauses 1 to 6, the irradiation conditions determined by the controller may include at least one of the irradiation output, irradiation radius, and irradiation speed of the ultraviolet laser. In this case, the additive manufacturing apparatus can determine parameters of the ultraviolet laser that affect the formation of the target film thickness.

[0017] (Clause 8) Another additive manufacturing device according to one aspect of the present disclosure is an additive manufacturing device that forms a three-dimensional object, and includes: a base to which a raw material containing an ultraviolet curable resin and ceramic particles is supplied; a layer formation unit that forms a layer of hardened raw material by irradiating the raw material on the base with an ultraviolet laser multiple times so that at least a portion of the irradiation ranges overlap each other; and a controller that controls the layer formation unit, wherein the controller inputs a target film thickness of the layer and the number of times the raw material is irradiated with the ultraviolet laser when forming the layer, and causes the layer formation unit to irradiate the raw material multiple times while moving the ultraviolet laser scan along a first direction by a predetermined distance along a second direction intersecting the first direction so that portions of the irradiation ranges overlap each other, and the irradiation conditions of the ultraviolet laser satisfy the relationship of the following mathematical expressions (8) to (11).

number

[0018] (Clause 9) A manufacturing condition determination device according to one aspect of the present disclosure is a device for determining irradiation conditions of an ultraviolet laser in additive manufacturing, in which a raw material including an ultraviolet curable resin and ceramic particles is irradiated with an ultraviolet laser multiple times so that at least a part of the irradiation range overlaps with each other to form layers, thereby forming a three-dimensional shaped object. The manufacturing condition determination device includes an acquisition unit and a determination unit. The acquisition unit acquires a target film thickness of the layer, and the number of irradiations of the ultraviolet laser to the raw material when forming the layer. The determination unit determines the irradiation conditions based on the acquired target film thickness and number of irradiations, and a relationship acquired in advance. The relationship acquired in advance is a relationship between the number of irradiations, a first penetration depth which is a penetration depth into the raw material before the raw material is hardened, a second penetration depth which is a penetration depth into the raw material after the raw material is hardened, and an irradiation condition. For the same reason as the additive manufacturing device, the manufacturing condition determination device of the present disclosure can determine the irradiation conditions of a laser for forming a layer of a target film thickness when hardening a raw material including ceramic particles and an ultraviolet curable resin.

[0019] (Clause 10) Another manufacturing condition determination device according to an aspect of the present disclosure is a device for determining ultraviolet laser irradiation conditions in additive manufacturing, in which a raw material containing an ultraviolet curable resin and ceramic particles is irradiated multiple times with an ultraviolet laser while moving the scanning along a first direction by a predetermined distance along a second direction intersecting the first direction so that parts of the irradiation ranges overlap each other to form layers, thereby forming a three-dimensional object. The manufacturing condition determination device includes an acquisition unit and a determination unit. The acquisition unit acquires a target film thickness of the layer and the number of times the raw material is irradiated with the ultraviolet laser when forming the layer. The determination unit receives the acquired target film thickness and the number of times of irradiation and determines the irradiation conditions. The irradiation conditions satisfy the relationships of the following mathematical expressions (12) to (15).

number

[0020] (Clause 11) A manufacturing condition determination program according to one aspect of the present disclosure causes a computer to function as an apparatus for determining irradiation conditions of an ultraviolet laser in additive manufacturing, which forms layers by irradiating a raw material including an ultraviolet curable resin and ceramic particles with an ultraviolet laser multiple times so that at least a part of the irradiation range overlaps with each other, thereby forming a three-dimensional shaped object. The manufacturing condition determination program causes a computer to function as an acquisition unit and a determination unit. The acquisition unit acquires a target film thickness of the layer and the number of irradiations of the ultraviolet laser to the raw material when forming the layer. The determination unit determines the irradiation conditions based on the acquired target film thickness and number of irradiations, and a relationship acquired in advance. The relationship acquired in advance is a relationship between the number of irradiations, a first penetration depth which is a penetration depth into the raw material before the raw material is hardened, a second penetration depth which is a penetration depth into the raw material after the raw material is hardened, and an irradiation condition. For the same reason as the additive manufacturing device, the manufacturing condition determination program of the present disclosure can determine the laser irradiation conditions for forming a layer of a target film thickness when hardening a raw material including ceramic particles and an ultraviolet curable resin.

[0021] [Examples of the embodiments of the present disclosure] The embodiments of the present disclosure will be described in detail with reference to the drawings. In the description of the drawings, the same elements are given the same reference numerals, and duplicated description will be omitted. The dimensional ratios of the drawings do not necessarily match those in the description. The terms "upper", "lower", "left" and "right" are based on the illustrated state and are for convenience.

[0022] [An example of additive manufacturing equipment] FIG. 1 is a schematic diagram of an additive manufacturing apparatus 1. In the figure, the X direction (first direction) and the Y direction (second direction) are horizontal directions, and the Z direction is vertical. Hereinafter, the Z direction is also referred to as the up-down direction. The additive manufacturing apparatus 1 forms a three-dimensional object. The additive manufacturing apparatus 1 forms a model based on, for example, three-dimensional CAD data. The three-dimensional CAD data includes data on the cross-sectional shape of each layer. As an example, the additive manufacturing apparatus 1 forms the cross section of the model layer by layer based on the cross-sectional shape data. The additive manufacturing apparatus 1 forms layers by irradiating a raw material containing an ultraviolet curing resin and ceramic particles with ultraviolet light. The raw material is the material of the model. The raw material is a slurry-like mixture containing an ultraviolet curing resin and ceramic particles. In addition to the ultraviolet curing resin and ceramic particles, the raw material may also contain metals and other resins. The ultraviolet curing resin is a synthetic organic material that absorbs light of an ultraviolet wavelength and changes into a solid.

[0023] The additive manufacturing apparatus 1 includes a layer formation unit 2, a stage mechanism 3, a raw material supply unit 4, and a controller (manufacturing condition determination device) 10.

[0024] The layer forming unit 2 is one of the components for forming a layer. The stage mechanism 3 includes a base 31. The layer forming unit 2 irradiates light onto the raw material on the base 31, thereby forming a layer in which the raw material is hardened. The raw material is supplied to the base 31. The method of forming a layer by the layer forming unit 2 will be described in detail later.

[0025] The layer forming section 2 includes, for example, an optical unit 20, light reflecting members 21, 23, and rotary drive units 22, 24. The optical unit 20 includes, for example, a light source 20a and an optical member 20b, and emits an ultraviolet laser L. The light reflecting members 21, 23 are, for example, galvano mirrors, and change the optical path of the ultraviolet laser L emitted from the optical unit 20. The light reflecting members 21, 23 rotate around a predetermined rotation axis by the rotary drive units 22, 24. By controlling the rotation of the light reflecting members 21, 23, the layer forming section 2 can irradiate the ultraviolet laser L at a predetermined position in the horizontal direction at the layer formation height position. The layer formation height position is a height that is predetermined as a height position at which the ultraviolet laser L is irradiated. When the ultraviolet laser L is irradiated, the ultraviolet curable resin contained in the raw material is cured, so that only the part irradiated with the ultraviolet laser L is formed as a layer. The layer forming unit 2 irradiates the ultraviolet laser L so as to reproduce a cross-sectional shape based on CAD data, and forms one layer of the cross section of the shaped object.

[0026] The raw material supplying unit 4 supplies raw material onto the base 31. The raw material supplying unit 4 supplies the raw material while moving, for example, in a horizontal direction. The raw material supplying unit 4 has, for example, a head that supplies the raw material and a blade that smoothes the supplied raw material. The raw material supplied from the head is smoothed by the blade, so that one layer of raw material is supplied onto the base 31.

[0027] The base 31 moves up and down relative to the layer forming unit 2. As an example, the stage mechanism 3 includes a drive unit 32. The drive unit 32 is connected to the base 31 and moves the base 31 up and down. The drive unit 32 is, for example, an electric cylinder. The drive unit 32 moves the base 31 up and down in units of the height of one layer.

[0028] The controller 10 is hardware that controls the entire additive manufacturing apparatus 1. The controller 10 is composed of a general-purpose computer having, for example, an arithmetic unit such as a CPU (Central Processing Unit), a storage device such as a ROM (Read Only Memory), a RAM (Random Access Memory), and a HDD (Hard Disk Drive), and a communication device.

[0029] The controller 10 is communicatively connected to the layer forming unit 2, the raw material supplying unit 4, and the driving unit 32. The controller 10 outputs control signals to the layer forming unit 2, the raw material supplying unit 4, and the driving unit 32 to control the layer forming unit 2, the raw material supplying unit 4, and the driving unit 32. The controller 10 is connected to an operation panel (not shown) such as a touch panel, and operates the layer forming unit 2, the raw material supplying unit 4, and the driving unit 32 in response to a command operation by an operator received by the operation panel. The controller 10 may operate the layer forming unit 2, the raw material supplying unit 4, and the driving unit 32 based on three-dimensional CAD data stored in a storage device.

[0030] [Additive manufacturing methods] First, the controller 10 forms a shaped object on the base 31. Specifically, the base 31 is moved up and down relative to the layer formation unit 2 of the additive manufacturing apparatus 1, thereby forming a shaped object on the base 31. First, the controller 10 causes the raw material supply unit 4 to supply raw material for one layer onto the base 31. Next, the controller 10 causes the layer formation unit 2 to irradiate the ultraviolet laser L. The layer formation unit 2 irradiates the supplied raw material with the ultraviolet laser L based on CAD data. The ultraviolet curable resin contained in the raw material irradiated with the ultraviolet laser L is cured. As a result, a layer of the shaped object is formed.

[0031] Next, the controller 10 causes the driving unit 32 to adjust the height of the base 31. The driving unit 32 adjusts the height of the base 31 so that the upper surface of the base 31 is at the layer formation height position. Specifically, the driving unit 32 lowers the base 31 by the height of one layer.

[0032] Next, the controller 10 causes the raw material supply unit 4 to supply one layer of raw material onto the base 31. As a result, the already formed layer is buried in the raw material. The layer forming unit 2 irradiates the supplied raw material with ultraviolet light based on CAD data. The raw material irradiated with ultraviolet light is hardened. The controller 10 repeats such layer formation, forming layers and stacking them one by one. In this way, a model is stacked. FIG. 2 is a schematic diagram of an example of forming a model. In the example shown in FIG. 2, the controller 10 causes the layer forming unit 2 to irradiate the supplied raw material with an ultraviolet laser L, thereby forming a layer i. Then, the controller 10 repeats such formation of the layer i, stacking the layers i one by one to form a model I. The model I is transported to a baking device (not shown) and baked. In this way, a model is formed.

[0033] [Layer formation method by layer formation unit] The method of forming a layer by the layer forming unit 2 will be described in detail below. Under the control of the controller 10, the layer forming unit 2 irradiates the raw material on the base 31 with the ultraviolet laser L multiple times so that at least a portion of the irradiation ranges overlap each other. Specifically, the layer forming unit 2 performs a first irradiation in which the raw material is irradiated multiple times so that at least a portion of the irradiation ranges overlap each other while moving the ultraviolet laser L along the X direction by a predetermined distance along the Y direction. In other words, the scanning to form the hardened portions is repeated to form multiple hardened portions, and the multiple hardened portions become a layer.

[0034] The first irradiation by the layer forming unit 2 will be described below with reference to the examples of Figs. 3 and 4. Fig. 3 is a schematic diagram of an example of scanning D along the X direction of an ultraviolet laser L. Fig. 4 is a schematic diagram of an example in which multiple hardened portions are formed by irradiation with an ultraviolet laser L. As in the example shown in Fig. 3, hardened portion m11 formed by hardening raw material C by scanning D has a mountain shape (parabola shape) protruding in the Z direction.

[0035] In this way, the hardened portion formed by each scan is a mountain-like shape protruding in the Z direction, so if multiple scans are performed along the X direction without parts of the irradiation ranges overlapping each other, the back surface (lower surface) of the layer will become uneven. Therefore, as shown in the example of FIG. 4, the layer forming unit 2 irradiates the ultraviolet laser L at a distance d, which is the scan interval at which the hardened portions interfere with each other. Specifically, the layer forming unit 2 irradiates multiple times while moving the scan along the X direction by a distance d along the Y direction so that parts of the irradiation ranges overlap each other. This makes the back surface of the layer closer to uniform (flat).

[0036] More specifically, first, the layer forming unit 2 forms a hardened portion m11 by the first irradiation in the first irradiation. Then, the layer forming unit 2 moves the ultraviolet laser L by a distance d along the Y direction to form a hardened portion m12 by the second irradiation. Furthermore, the layer forming unit 2 moves the ultraviolet laser L by a distance d along the Y direction to form a hardened portion m13 by the third irradiation. The overlapping irradiation portion J1 shown in FIG. 4 is a portion where a part of the irradiation range of the first irradiation and a part of the irradiation range of the second irradiation overlap each other, and the overlapping irradiation portion J2 is a portion where a part of the irradiation range of the second irradiation and a part of the irradiation range of the third irradiation overlap each other. As a result, the back surfaces of the multiple hardened portions m11 to m13 approach a uniform state. Hereinafter, a set of hardened portions constituted by the multiple hardened portions will be described as a "first hardened portion."

[0037] The number of times N of irradiation with the ultraviolet laser L when forming the first hardened portion is expressed by the following formula (16).

number

[0038] In this embodiment, the layer forming unit 2 performs cross-hatching to form the back surface of the layer more uniformly. Specifically, the layer forming unit 2 performs a second irradiation to further harden the raw material below the first hardening unit. The second irradiation is an irradiation that performs scanning along the Y direction with the ultraviolet laser L multiple times after the first irradiation while moving a predetermined distance along the X direction.

[0039] FIG. 5 is a schematic diagram of an example in which a layer is formed by cross-hatching. In the example shown in FIG. 5, hardened portions m11 to m13 are formed by the first irradiation. Then, the layer forming unit 2 performs scanning along the Y direction with the ultraviolet laser L multiple times while moving the ultraviolet laser L a predetermined distance along the X direction, thereby further forming hardened portions mz21 to mz23. Specifically, first, the layer forming unit 2 hardens the raw material C by the first irradiation in the second irradiation to form the hardened portion m21. Then, the layer forming unit 2 moves the ultraviolet laser L a predetermined distance along the X direction to form the hardened portion m22 by the second irradiation. Furthermore, the layer forming unit 2 moves the ultraviolet laser L a predetermined distance along the X direction to form the hardened portion m23 by the third irradiation. This makes the back surface of the layer more uniform. Hereinafter, a set of hardened portions constituted by the multiple hardened portions will be described as a "second hardened portion". The number of irradiations of the ultraviolet laser L when forming the second hardened portion may be calculated by the same method as in the case of the number of irradiations N of the first hardened portion.

[0040] [Irradiation condition determination process by the controller] In order to obtain the target dimensions of the molded object, each layer needs to be formed to a target cured film thickness (hereinafter referred to as "target film thickness"). The film thickness here means the thickness of the layer in the Z direction, such as the film thickness it of the layer shown in FIG. 2. In order to obtain the target film thickness of each layer, it is necessary to control the energy of the ultraviolet laser L irradiated to the raw material (hereinafter sometimes referred to as "irradiation energy of the ultraviolet laser L"). To do so, it is necessary to determine the irradiation conditions of the ultraviolet laser L suitable for the target film thickness. Therefore, in the additive manufacturing device 1, the controller 10 determines the irradiation conditions of the ultraviolet laser L suitable for the target film thickness. The following description focuses on one layer, but the method of determining the irradiation conditions of the ultraviolet laser L is similar for other layers.

[0041] In the additive manufacturing device 1, the penetration depth into the raw material is utilized. The penetration depth is the depth in the Z direction from the surface (upper surface) of the raw material to the point where the light (ultraviolet light) intensity decreases to 1 / e when the raw material is irradiated with laser light. Specifically, the controller 10 determines the irradiation conditions of the ultraviolet laser L based on a relationship that is previously acquired using the penetration depth into the raw material before and after the raw material is hardened. The details of the previously acquired relationship will be described later. Hereinafter, the penetration depth into the raw material before the raw material is hardened is referred to as the first penetration depth D. p The penetration depth into the raw material after the raw material has hardened is called the second penetration depth D p ' he said.

[0042] 1, the controller 10 has, as functional components, a first acquisition unit 11, a first calculation unit 12, a second acquisition unit 13 (an example of an acquisition unit), and a determination unit 14. In the description of the manufacturing condition determination method described later, the function (operation) of each functional unit will be described in detail, so here, the function of each functional unit will be briefly described.

[0043] The first acquisition unit 11 has a first penetration depth D p , and the critical energy (energy value) E c Obtain the first penetration depth D p , and the critical energy E cis used to calculate the irradiation conditions described later. The first acquisition unit 11 receives the first penetration depth D p , and the critical energy E c The first calculation unit 12 obtains the second penetration depth D p The second acquisition unit 13 acquires a target film thickness of the layer and the number of times the raw material is irradiated with the ultraviolet laser L when forming the layer. The determination unit 14 determines the irradiation conditions based on the acquired target film thickness and number of times of irradiation and the relationship acquired in advance.

[0044] Hereinafter, the manufacturing condition determination process by the controller 10 will be described with reference to the flowchart shown in FIG. 6. FIG. 6 is a flowchart showing a series of manufacturing condition determination processes by the controller 10. First, the first acquisition unit 11 acquires the first penetration depth D p , and the critical energy E c (Step S01). The critical energy E c is the minimum energy value of the ultraviolet laser L at which the slurry-like raw material hardens. In other words, the critical energy E c is the critical value of the ultraviolet laser L at which the material hardens. p , and the critical energy E c is the second penetration depth D in step S02 described later. p As an example, the first penetration depth D p , and the critical energy E c are stored in a storage unit (not shown) in the additive manufacturing apparatus 1.

[0045] Hereinafter, the first penetration depth D p , and the critical energy E c First, a specific region of the raw material is irradiated to form a hardened portion. Next, the hardening depth C of the hardened portion is calculated. dThe "hardening depth" is the maximum thickness among the thicknesses (size in the Z direction) at each position in the surface of the formed hardened portion. The irradiation energy of the ultraviolet laser L is then changed to multiple different values, and the formation and measurement of the hardened portion are repeated. Next, on a semi-logarithmic graph, the horizontal axis represents each irradiation energy of the ultraviolet laser L, and the vertical axis represents the hardening depth C of each formed hardened portion. d The relationship between the UV irradiation energy and the curing depth C of the cured part plotted in this way is d The multiple points showing the relationship are approximately linear. The slope of the line obtained based on the multiple points is the first penetration depth D p and the hardening depth C d The irradiation energy when E = 0 (i.e., the lowest point of the line) is the critical energy E c is obtained as:

[0046] Figure 7 shows the relationship between the ultraviolet irradiation energy and the curing depth C of the cured part. d 7 is an example of a graph G1 showing the relationship between the ultraviolet laser L and the laser power V. In the example shown in FIG. Irradiation output P L =100~300mW Scanning speed V s =500~5000mm / s, Spot radius w of ultraviolet laser L o =419.7(Irradiation power P L =300mW),426.5(irradiation output P L =200mW),443.8(irradiation output P L =100mW)

[0047] Graph G1, which is a log-log graph, shows a straight line Li based on a number of points plotted on graph G1. The equation representing straight line Li is y=201.8(x)-317.6. Therefore, the slope of straight line Li, 201.8 μm, is the first penetration depth D p and the hardening depth C d Irradiation energy at 4.82 mJ / cm 2 is the critical energy Ec is obtained as:

[0048] Returning to FIG. 6, the first calculation unit 12 calculates the second penetration depth D p The first calculation unit 12 calculates D′ from the hardening depth of the hardened portion formed by the first irradiation and the hardened portion formed by the second irradiation when two irradiations are performed on a predetermined region of the raw material. p ' is calculated.

[0049] Second penetration depth D p The second penetration depth D ′ can be calculated using the hardening depth of two hardened parts formed when a predetermined region of the raw material is irradiated twice with the ultraviolet laser L. Specifically, the second penetration depth D p ' is calculated using the hardening depth of the first film formed during the first irradiation, and the hardening depth of the second film formed when the area is irradiated a second time after the formation of the first film.

[0050] FIG. 8(A) is a schematic diagram of an example of the first film M1, and FIG. 8(B) is a schematic diagram of an example of the first film M1 and the second film M2. In the example shown in FIG. 8(A), a first irradiation of the irradiation energy E by the ultraviolet laser L is performed on a predetermined region R in the raw material, and the first film M1 is formed. In the example shown in FIG. 8(B), a second irradiation of the irradiation energy E by the ultraviolet laser L is performed on the region R, and the second film M2 is formed below the region where the first film M1 was formed. In the examples shown in FIG. 8(A) and FIG. 8(B), the curing depth of the first film M1 is indicated as Z1, and the curing depth of the second film M2 is indicated as a2.

[0051] Using such a first film M1 and a second film M2, the first calculation unit 12 calculates the second penetration depth D p ' is calculated as follows:

[0052] First, the hardening depth Z1 of the first film M1 is expressed, for example, by the following formula (17).

number

number

[0053] Moreover, the hardening depth a2 of the second film M2 is expressed by the following formula (19).

number

number

[0054] By substituting E1 in formula (19) with formula (20), the hardening depth a2 of the second film M2 is obtained as shown in formula (21) below. Furthermore, Z2, which is the sum of the hardening depth Z1 of the first film M1 and the hardening depth a2 of the second film M2, is expressed by formula (22) below.

number

[0055] Next, by transforming the formula (22), the second penetration depth D is calculated as shown in the following formula (23): p ' is obtained.

number

[0056] As described above, the first calculation unit 12 calculates the first penetration depth D p Based on the hardening depth of the first film formed when the ultraviolet laser L is irradiated to a predetermined region of the raw material, and the hardening depth of the second film further formed when the ultraviolet laser L is irradiated to the region where the first film is formed, a second penetration depth D p ' is calculated. Also, the second penetration depth D p ' satisfies the relationship of the above formula (23). As a result, the additive manufacturing apparatus 1 calculates the second penetration depth D p ' can be obtained in advance.

[0057] Returning to FIG. 6, the second acquisition unit 13 acquires the target film thickness and the number of times the raw material is irradiated with the ultraviolet laser L by the layer forming unit 2 (step S03). As an example, the second acquisition unit 13 accepts the target film thickness by receiving an input of the target film thickness from an operator via an operation panel. The second acquisition unit 13 also acquires the distance d and the film formation width L w The number of irradiations may be calculated based on the above-mentioned formula (16) by acquiring information indicating the number of irradiations, or the number of irradiations may be received by receiving input of the number of irradiations from an operator via an operation panel.

[0058] Next, the determination unit 14 determines the irradiation conditions of the ultraviolet laser L (step S04). The determination unit 14 determines the irradiation conditions of the ultraviolet laser L based on the target film thickness obtained in step S03, the number of times the raw material is irradiated with the ultraviolet laser L, and the first penetration depth D obtained in step S01. p and the second penetration depth D calculated in step S02 p The irradiation conditions are determined based on a previously acquired relationship between the light intensity and the light intensity distribution. The previously acquired relationship will be described below.

[0059] The relationship obtained in advance is the number of irradiations and the first penetration depth D p and the second penetration depth D, which is the penetration depth into the raw material after the raw material has hardened. p ' and the critical energy E c and the irradiation conditions. The previously acquired relationship is expressed by a plurality of derived formulas described below. Each of the plurality of derived formulas is a formula for calculating the film thickness of a layer. The film thickness of a layer is the cumulative thickness of the first hardened portion and the second hardened portion.

[0060] The multiple derivation formulas are derived by taking into consideration the following two points. First, as described above, the first hardened portion is a collection of multiple hardened portions formed by multiple irradiations of the ultraviolet laser L, and in the multiple hardened portions, parts of the irradiation ranges overlap with each other. Therefore, the hardening depth of the first hardened portion may differ for each position y of the layer (first hardened portion) along the Y direction. Second, the manner in which a hardened portion is formed differs between when a hardened portion is formed by irradiating an area where no hardened portion exists with the ultraviolet laser L and when a hardened portion already exists with the ultraviolet laser L to form a new hardened portion below the hardened portion. This is because the degree of light absorption of the raw material differs before and after hardening, and the penetration depth of the raw material after hardening (i.e., the second penetration depth D p ') is the penetration depth into the raw material before hardening (i.e., the first penetration depth D p Considering these two points, the above derived formulas are based on the position y of the first hardened part, the first penetration depth D p , and the second penetration depth D pThe above derived formulas are expressed taking into consideration the following details.

[0061] The above-mentioned multiple derived formulas include multiple formulas expressing the hardened shape of each hardened portion constituting the first hardened portion at position y, and a formula expressing the hardened shape of each hardened portion constituting the second hardened portion at position y. The hardened shape is the thickness of the hardened portion at position y. That is, the hardening depth is the maximum thickness of the hardened portion, whereas the hardened shape is the thickness of the hardened portion at a predetermined position along the Y direction (size in the Z direction). Below, first, the multiple formulas expressing the hardened shape of each hardened portion constituting the first hardened portion at position y will be described, and then the formulas expressing the hardened shape of each hardened portion constituting the second hardened portion at position y will be described.

[0062] The multiple formulas representing the hardened shape of each hardened portion constituting the first hardened portion at position y include a formula corresponding to the hardened portion formed by the first irradiation of the ultraviolet laser L in the first irradiation, and a formula corresponding to the hardened portion formed by the second or subsequent irradiations.

[0063] The formula corresponding to the hardened portion formed by the first irradiation in the first irradiation will be described. First, the contributed irradiation energy E1(y,z) at position y of the hardened portion formed by hardening the raw material by the irradiation of the first ultraviolet laser L is expressed by the following formula (24) based on Lambert Beer's law.

number

number

[0064] Next, the contributing irradiation energy E1(y,z) in this formula (24) is converted into the critical energy E c This results in the following equation (26) which expresses z1(y), the hardened shape z at the position y.

number

[0065] Next, we will explain the formulas corresponding to each hardened portion formed by the second and subsequent irradiations in the first irradiation. First, the contributed irradiation energy E n (y, z) are expressed by the following formula (27). n is an integer equal to or greater than 2 and equal to or less than the acquired number of irradiations. In other words, formula (27) represents the contributed irradiation energy at position y of the hardened portion formed by the irradiation of the nth ultraviolet laser L among the total number of irradiations.

number

[0066] Then, by converting this formula (27), the hardened shape z at the position y is obtained as a n The following equation (28) is obtained to represent (y). In other words, the hardened shape a n (y) is the thickness (size in the Z direction) at position y of the hardened portion formed only by irradiation with the n-th ultraviolet laser beam L.

number

[0067] At the time when the first to nth ultraviolet laser beams L are irradiated, the cumulative result of each cured shape obtained as described above is the cured shape at the position y of the first cured portion (layer). Therefore, the cured shape z at the position y of the first cured portion after the first to nth ultraviolet laser beams L are irradiated in the first irradiation is n (y) is expressed by the following formula (29). n (y) is used to derive the film thickness of a layer, which will be described later.

number

[0068] Next, a formula corresponding to the second cured portion formed by the second irradiation will be described. First, the contributed irradiation energy E ch The equation representing (y) is expressed by the following equation (30).

number

[0069] Next, in this formula (30), the contributing irradiation energy E ch (y) is the critical energy E c and the hardened shape z is the hardened shape a at the position y of the hardened portion formed by the irradiation of the ultraviolet laser L during the second irradiation. ch (y) and convert equation (30). This results in the hardened shape a ch The following equation (31) is obtained, which represents (y).

number

[0070] The hardened shape z of the first hardened portion obtained as described above n (y) and the hardened shape of the second hardened part a chThe cumulative effect of the second irradiation with the second radiation is the hardened shape at the position y of the layer. Therefore, the hardened shape at the position y of the layer after the second irradiation is z ch (y) is expressed by the following equation (32).

number

[0071] Here, the above formulas (24) to (32) will be explained with reference to the graph shown in Fig. 9. Fig. 9 is a graph Gp showing a prediction of the hardened shape of the layer at position y when the layer is viewed from the X direction. In the graph Gp, the horizontal axis represents position y, and the left vertical axis represents the hardened shape (hardened depth) Z of each hardened portion. n The right side of the vertical axis represents the contributed irradiation energy E n Represents.

[0072] The upper half of the graph Gp shows the contribution irradiation energy E1 to E5 of the first to fifth ultraviolet lasers L in the first irradiation, and the contribution irradiation energy E ch The lower half of the graph G shows the hardened shapes z1 to z5 of the hardened portions mz11 to mz15 constituting the first hardened portion, and the hardened shape z ch are shown. Hardened portion mz11 is a hardened portion formed by hardening the raw material by the first irradiation in the first irradiation. Hardened portion mz12 is a hardened portion formed by the second irradiation in the first irradiation. Hardened portion mz13 is a hardened portion formed by hardening the raw material by the third irradiation in the first irradiation. Hardened portion mz14 is a hardened portion formed by the fourth irradiation in the first irradiation. Hardened portion mz15 is a hardened portion formed by the fifth irradiation in the first irradiation. As shown in FIG. 9, each of the hardened portions mz11 to mz15 is formed in order from the left side of graph G so that parts of them overlap each other. Hardened portion mz2 is a hardened portion formed by the second irradiation after the first irradiation.

[0073] The contributing irradiation energy E1 is energy that contributes to the formation of the hardened portion mz11. The contributing irradiation energy E2 is energy that contributes to the formation of the hardened portion mz12. The contributing irradiation energy E3 is energy that contributes to the formation of the hardened portion mz13. The contributing irradiation energy E4 is energy that contributes to the formation of the hardened portion mz14. The contributing irradiation energy E5 is energy that contributes to the formation of the hardened portion mz15. The contributing irradiation energy E ch is the energy contributing to the formation of the hardened part mz2.

[0074] The contributing irradiation energy E1 at the position y is calculated based on the formula (24). The contributing irradiation energies E2 to E5 at the position y are calculated based on the formula (27). The contributing irradiation energy E ch is calculated based on the formula (30). Specifically, the positions y, the number of irradiations n, and the first penetration depth D p , second penetration depth D p ', distance d, irradiation power P of ultraviolet laser L L , the scanning speed V of the ultraviolet laser L s , the critical energy E c By substituting appropriate values ​​for each contributing irradiation energy E1 to E5, E ch A prediction is made.

[0075] The hardened shape z1 at the position y of the hardened portion mz11 is calculated based on the formula (26). The hardened shapes z2 to z5 at the positions y of the hardened portions mz12 to mz15 are calculated based on the formulas (28) and (29). ch is calculated based on the formulas (31) and (32). Specifically, the positions y, the number of irradiations n, and the first penetration depth D p , second penetration depth D p ', distance d, irradiation power P of ultraviolet laser L L , and the scanning speed V of the ultraviolet laser L s , and the critical energy E cBy substituting appropriate values ​​for the parameters in the formula, each hardening shape z1 to z5, z ch A prediction is made.

[0076] The controller 10 determines the irradiation conditions using the above-described formulas (25), (26), (28), (29), (31), and (32). More specifically, when the controller 10 acquires the target film thickness and the number of irradiations, the controller 10 calculates the target film thickness by dividing the cured shape z ch (y). Then, the controller 10 sets the target film thickness at each position y of the layer as z n (y)+a n Fitting is performed by adjusting predetermined parameters in formulas (25), (26), (28), (29), (31), and (32) so that the relationship of (y) is satisfied.

[0077] Specifically, the controller 10 determines parameters as irradiation conditions of the ultraviolet laser L so that each position y of the layer formed by irradiating the ultraviolet laser L N times is as close to the target film thickness as possible. The irradiation conditions of the ultraviolet laser L are determined by E max The spot radius w of the ultraviolet laser L in formula (25) represents o , the irradiation power P of the ultraviolet laser L L , and the scanning speed V of the ultraviolet laser L s That is, the controller 10 adjusts the spot radius w so that each position of the layer is as close to the target film thickness as possible. o , irradiation power P L , and the scanning speed V s This allows the additive manufacturing apparatus 1 to determine parameters of the ultraviolet laser L that affect the formation of the target film thickness. As an example, the controller 10 determines at least one of the irradiation output P L , and the scanning speed V of the ultraviolet laser L s Determine.

[0078] In this way, the determination unit 14 determines the irradiation conditions using the acquired target film thickness and the number of irradiations as inputs. This makes it possible to determine the laser irradiation conditions for forming a layer with a target film thickness when hardening a raw material containing ceramic particles and an ultraviolet curable resin.

[0079] In this manner, the manufacturing condition determination process is completed. In this manner, the controller 10 functions not only as a control device for the layer forming unit 2 of the additive manufacturing apparatus 1, but also as a manufacturing condition determination device. The manufacturing condition determination device is a device that determines the irradiation conditions of the ultraviolet laser L in additive manufacturing, which forms layers by irradiating a raw material containing an ultraviolet curable resin and ceramic particles with an ultraviolet laser L multiple times so that at least a part of the irradiation ranges overlap each other to form a three-dimensional shaped object.

[0080] After the irradiation conditions are determined, the controller 10 controls the layer forming unit 2 to irradiate the ultraviolet laser L based on the irradiation conditions. o , irradiation power P L , and the scanning speed V s The raw material on the base 31 is irradiated with the ultraviolet laser L set to at least one of the above conditions, thereby forming a hardened layer of the raw material.

[0081] [Manufacturing condition determination program] A manufacturing condition determination program PR1 for causing a computer to function as the controller 10 having the function of a manufacturing condition determination device will be described with reference to Fig. 10. Fig. 10 is a diagram showing the configuration of the manufacturing condition determination program PR1.

[0082] 10, the manufacturing condition determination program PR1 includes a main module PR11, a first acquisition module PR12, a first calculation module PR13, a second acquisition module PR14, and a determination module PR15. The main module PR11 is a part that controls the overall processing related to the manufacturing condition determination device. Functions realized by executing the first acquisition module PR12, the first calculation module PR13, the second acquisition module PR14, and the determination module PR15 are similar to the functions of the first acquisition unit 11, the first calculation unit 12, the second acquisition unit 13, and the determination unit 14 in the above embodiment, respectively.

[0083] The manufacturing condition determination program PR1 is provided by a computer-readable recording medium MD such as a CD-ROM (Compact Disc Read Only Memory), a DVD-ROM (Digital Versatile Disc Read Only Memory), a semiconductor memory, etc. The manufacturing condition determination program PR1 may be provided as a data signal via a network.

[0084] [Summary of the embodiment] In the additive manufacturing device 1, the manufacturing condition determination device, and the manufacturing condition determination program PR1, the number of irradiations of the ultraviolet laser L and the first penetration depth D p and the second penetration depth D p The irradiation conditions of the ultraviolet laser L are determined based on the previously acquired relationship between the thickness of the ultraviolet laser L and the target thickness of the layer. Therefore, even when forming a layer made of raw materials containing an ultraviolet curable resin and ceramic particles and having an overlapping region, the additive manufacturing device 1 can obtain appropriate laser irradiation conditions for the target thickness of the layer.

[0085] In general, it is considered that there is a correlation between the film thickness of a layer and the irradiation energy of the ultraviolet laser L. Therefore, by grasping the correlation between the film thickness of a layer and the irradiation energy of the ultraviolet laser L in advance, it is possible to calculate the irradiation conditions suitable for the target film thickness. However, grasping the correlation between the target film thickness of the layer formed by the additive manufacturing apparatus 1 and the irradiation energy of the ultraviolet laser L by the conventional method has the following problems.

[0086] That is, first, for the hardened shape of the hardened portion formed by scanning 1, the above correlation can be obtained by the Lambert Beer's law shown in the above formula (26). However, in the layer formed by the additive manufacturing device 1, in order to make the back surface of the layer uniform, the ultraviolet laser L is scanned multiple times so that parts of the irradiation range overlap each other. In this case, an overlapping area (interference area) where the layers are hardened in an overlapping manner is generated in the layer. Therefore, when actually forming a layer, it is difficult to grasp the irradiation energy of the ultraviolet laser L appropriate for obtaining the target film thickness based on the above formula (26).

[0087] Furthermore, the raw material used in the additive manufacturing apparatus 1 contains ceramic particles in addition to the ultraviolet curing resin. For example, when the raw material is made of only resin, the thickness of the layer is determined by the total energy of the ultraviolet light irradiated. However, when the raw material contains ceramic particles in addition to the ultraviolet curing resin, the thickness of the layer will differ depending on the number of irradiations of the ultraviolet laser L, even if the total energy is the same.

[0088] Here, a comparison between the state of the curing depth of a raw material containing only an ultraviolet curing resin and the state of the curing depth of a raw material containing an ultraviolet curing resin and ceramic particles will be described with reference to Figs. 11 and 12. Fig. 11 is a graph G2 showing the curing depth when a raw material containing only an ultraviolet curing resin is cured. In the graph G2, the horizontal axis shows the number of irradiations n, and the vertical axis shows the curing depth. Fig. 12 is a graph G3 showing the curing depth when a raw material containing an ultraviolet curing resin and ceramic particles is cured. In the graph G3, the horizontal axis shows the number of irradiations n, and the vertical axis shows the curing depth.

[0089] In each of the examples shown in FIG. 11 and FIG. 12, the curing depth in the case where an ultraviolet laser L is irradiated once to a certain region and the curing depth in the case where the region is irradiated multiple times are shown. In the case of one irradiation and the case of multiple irradiation, the total irradiation energy of the ultraviolet laser L irradiated to the above region and the time for which the ultraviolet laser L is irradiated to the above region are the same. In each of the examples shown in FIG. 11 and FIG. 12, in the case of multiple irradiation, the curing depths in the cases of one, five, and ten irradiations are plotted. In addition, in each of the examples shown in FIG. 11 and FIG. 12, in the case of one irradiation, the curing depths under the same conditions as the case of one, five, and ten irradiations are plotted as in the case of multiple irradiations.

[0090] As shown in FIG. 11, when a raw material containing only ultraviolet curing resin was cured, the curing depths of the cases of multiple irradiations were equal to those of the case of one irradiation at each irradiation count. In contrast, as shown in FIG. 12, when a raw material containing ultraviolet curing resin and ceramic particles was cured, the curing depths of the cases of multiple irradiations were smaller than those of the case of one irradiation at 5 and 10 irradiations. That is, when a raw material containing only ultraviolet curing resin was cured, the curing depth (film thickness) of the layer was determined by the total irradiation energy of the ultraviolet laser L, regardless of the number of irradiations of the ultraviolet laser L. In contrast, when the raw material contained ultraviolet curing resin and ceramic particles, the film thickness of the layer was dependent on the number of irradiations of the ultraviolet laser L, and it was difficult to determine the film thickness of the layer by the total irradiation energy of the ultraviolet laser L.

[0091] Therefore, in the additive manufacturing apparatus 1, the penetration depth into the raw material is utilized. The penetration depth into the raw material after the raw material is hardened changes from the penetration depth before the raw material is hardened. This is because it is considered that the energy required for hardening is not required after hardening, so light is more easily transmitted than before hardening. Then, by using such penetration depth into the raw material before and after hardening, it is possible to predict the irradiation conditions of the ultraviolet laser L suitable for obtaining the target film thickness of the layer. Specifically, in the additive manufacturing apparatus 1, the laser irradiation conditions are determined based on the previously acquired relationship between the penetration depth into the raw material before hardening, the penetration depth into the raw material after hardening, the number of irradiations of the ultraviolet laser L, and the laser irradiation conditions, and the acquired target film thickness of the layer. Therefore, this additive manufacturing apparatus 1 can obtain the laser irradiation conditions suitable for the target film thickness of the layer even when forming a layer made of a raw material containing an ultraviolet curable resin and ceramic particles and having an overlapping region.

[0092] In the additive manufacturing apparatus 1, the above-mentioned previously acquired relationship is used to determine the critical energy E c This allows the additive manufacturing apparatus 1 to determine the irradiation conditions taking into account the critical value at which the slurry-like raw material changes into a solid state.

[0093] In the additive manufacturing device 1, the number of irradiations and the first penetration depth D p , second penetration depth D p ' and the irradiation conditions satisfy the relationships of the above formulas (25), (26), (28), and (29) as previously acquired relationships. As a result, the additive manufacturing device 1 can determine the irradiation conditions of the ultraviolet laser L for the target film thickness based on the above formulas (25), (26), (28), and (29). In addition, the number of irradiations, the first penetration depth D p , second penetration depth D p ' and the irradiation conditions further satisfy the relationships of the above formulas (31) and (32) as previously acquired relationships. This allows the additive manufacturing apparatus 1 to determine the laser irradiation conditions for forming a layer with a target thickness, even when a layer is formed by cross-hatching in which the scanning directions are crossed so that the hardened portion becomes a flat layer.

[0094] [Variations] Although various exemplary embodiments have been described above, various omissions, substitutions, and modifications may be made without being limited to the above exemplary embodiments.

[0095] The controller 10 only needs to include the second acquisition unit 13 and the determination unit 14, and may not include the first acquisition unit 11 and the first calculation unit 12. In that case, the controller 10 receives the second penetration depth D from, for example, a storage unit of the additive manufacturing apparatus 1 or an external server (not shown) of the additive manufacturing apparatus 1. p The manufacturing condition determining program PR1 may only have the second obtaining module PR14 and the determining module PR15, and may not have the first obtaining module PR12 and the first calculation module PR13.

[0096] The manufacturing condition determination device may be a device separate from the controller 10, and may be, for example, a server external to the additive manufacturing apparatus 1.

[0097] The layer forming unit 2 does not have to perform cross-hatching. That is, the layer forming unit 2 may perform only the first irradiation to form the first hardened portion without performing the second irradiation.

[0098] The layer forming unit 2 may form a layer by irradiating a predetermined region multiple times with the ultraviolet laser L. In this case, the controller 10 may determine the irradiation conditions of the ultraviolet laser L using a predetermined relationship described below with reference to FIG.

[0099] FIG. 8(C) is a schematic diagram of an example of a film Mn formed when an ultraviolet laser L is irradiated N=(n+1) times on a region R. First, the hardening depth a of the film Mn formed by hardening the raw material by the n-th irradiation of the ultraviolet laser L is n+1 is expressed by the following equation (33).

number

number

[0100] E in formula (33) n By substituting equation (34) into the hardening depth a of the Mn film, n+1 is expressed by the following formula (35). In addition, the total hardening depth Z of each film formed by irradiation of the first to nth ultraviolet laser beams L is n+1 is expressed by the following equation (36).

number

[0101] Next, by subtracting (Dp' / Dp) × Z1 from each side of equation (36), the hardening depth Z n+1 is expressed by the following equation (37).

number

[0102] Here, since formula (37) is a geometric progression, it is expressed as the following formula (38). By converting formula (38), the hardening depth Z n We obtain equation (39) which shows

number

[0103] Moreover, by using the hardening depths Z1 and Z2, the formula (39) can be expressed as the following formula (40).

number

[0104] By using the above-mentioned multiple formulas, even when the layer forming unit 2 irradiates a specified area with an ultraviolet laser L multiple times to form a layer, the controller 10 can determine the irradiation conditions of the ultraviolet laser L suitable for the target film thickness, as in the above embodiment.

[0105] Furthermore, the irradiation conditions of the ultraviolet laser may satisfy the relationship of the formulas (2) to (5), and the method of determining the irradiation conditions may be implemented by various methods. For example, the controller 10 may execute a program to calculate the formulas (2) to (5) and determine the irradiation conditions of the ultraviolet laser. Alternatively, the controller 10 may calculate the formulas (2) to (5) by a logic circuit or an integrated circuit to determine the irradiation conditions of the ultraviolet laser. Alternatively, the controller 10 may have a table that stores the target film thickness, the number of irradiations, and the irradiation conditions of the ultraviolet laser, and may determine the irradiation conditions of the ultraviolet laser that satisfy the relationship of the formulas (2) to (5) by referring to the table. Alternatively, for example, the number of irradiations, the first penetration depth that is the penetration depth into the raw material before the raw material is hardened, the second penetration depth that is the penetration depth into the raw material after the raw material is hardened, and the irradiation conditions may be compiled into a database, and the irradiation conditions may be used as training data to determine the irradiation conditions of the ultraviolet laser that satisfy the relationship of the formulas (2) to (5) by machine learning. Regarding formulas (8) to (11) and formulas (12) to (15), the irradiation conditions of the ultraviolet laser can be determined in the same manner as formulas (2) to (5). [Example]

[0106] The effects of the embodiments confirmed by the inventors will be described below.

[0107] A laser marker (Kokkyo) was prepared as the ultraviolet laser L. The ultraviolet laser L has a wavelength of 355 nm and an irradiation output of P L = 300mW, scanning speed V s = 71 mm / s, spot radius w o = 419.7 μm, and distance d = 210, 420, 630 μm.

[0108] A slurry-like raw material containing ultraviolet curing resin and ceramic particles was prepared as the raw material. In the raw material, the resin was Aronix OT-2506 (Toa Gosei), and the ceramic was 40 vol% white TZ-PX-245 (Tosoh). The initiator was 1.0 wt% OMirad380 (IGM). The first penetration depth D p is 38.0 μm, the critical energy E cis 58.8mJ / cm 2 It is.

[0109] The raw material was irradiated with the ultraviolet laser L in the layer forming section 2 to form a plurality of layers with different distances d. Specifically, a layer was formed when the distance d=200 μm, a layer when the distance d=400 μm, and a layer when d=800 μm. Then, the thickness of each layer was measured. In addition, the thickness of each layer was predicted. Specifically, first, the first and second films formed by irradiating the ultraviolet laser L were measured, and the second penetration depth D was calculated using the formula (23). p ' was calculated. Next, the layer position y, the number of irradiations n, and the first penetration depth D p , second penetration depth D p ', distance d, critical energy E c The above irradiation conditions of the ultraviolet laser L are appropriately substituted into each of the formulas (25), (26), (28), (29), and (31) to obtain the cured shape z as the layer thickness calculated by the formula (32). ch was obtained and used as a prediction of the layer thickness.

[0110] As a result, for the layer with a distance d = 200 μm, the predicted thickness was 134.9-138.0 μm, while the measured thickness was 136.8 μm. For the layer with a distance d = 400 μm, the predicted thickness was 132.7-135.9 μm, while the measured thickness was 134.0 μm. For the layer with a distance d = 800 μm, the predicted thickness was 122.6-133.6 μm, while the measured thickness was 126.4 μm. For all distances d, the predicted thickness was close to the measured thickness. In other words, the first penetration depth D p and the second penetration depth D p According to this method using the above, the thickness of the layer can be predicted with high accuracy. In other words, according to this method, the irradiation conditions of the ultraviolet laser L suitable for the target thickness of the layer can be determined. In addition, when the error between the prediction and the actual measurement of the thickness of the layer is taken into consideration, the optimal distance d is determined by multiplying the spot radius w of the ultraviolet laser L by 1 / 2. o is considered to be equivalent to [Explanation of symbols]

[0111] 1...additive manufacturing device, 2...layer formation unit, 10...controller (manufacturing condition determination device), I...modeled object, 13...second acquisition unit (acquisition unit), 14...determination unit, m11, m12, m13, m21, m22, m23, mz2, mz11, mz12, mz13, mz14, mz15...hardening unit, 31...base, C...raw material, i...layer, D...scanning, d...distance, L...ultraviolet laser, M1...first film, M2...second film, PR1...manufacturing condition determination program, R...area, z1 to z5, z ch ...hardened shape.

Claims

1. An additive manufacturing apparatus for forming a three-dimensional object, comprising: a base to which a raw material containing an ultraviolet curable resin and ceramic particles is supplied; a layer forming unit that forms a layer of the raw material by irradiating the raw material on the base with an ultraviolet laser multiple times such that at least a portion of the irradiation ranges overlap each other; A controller for controlling the layer forming unit; Equipped with The controller: Acquire a target thickness of the layer and the number of times the raw material is irradiated with the ultraviolet laser by the layer forming unit; determining irradiation conditions of the ultraviolet laser based on the acquired target film thickness and the number of irradiations and a relationship acquired in advance, the relationship being a relationship between the number of irradiations, a first penetration depth which is a penetration depth into the raw material before the raw material is hardened, a second penetration depth which is a penetration depth into the raw material after the raw material is hardened, and the irradiation conditions; irradiating the ultraviolet laser from the layer forming unit based on the determined irradiation conditions; Additive manufacturing equipment.

2. The additive manufacturing device of claim 1, wherein the controller calculates the second penetration depth based on the first penetration depth, a hardening depth of a first film formed when the ultraviolet laser is irradiated to a specified area of ​​the raw material, and a hardening depth of a second film further formed when the ultraviolet laser is irradiated to the area where the first film is formed, before determining the irradiation conditions.

3. The additive manufacturing device of claim 2 , wherein the second penetration depth satisfies the relationship of the following equation (1): [0010] Here, D p is the first penetration depth, D p ' is the second penetration depth, Z 1 is the hardening depth of the first film, Z 2 is the sum of the hardening depth of the first film and the hardening depth of the second film.

4. The additive manufacturing apparatus of claim 1 , wherein the pre-acquired relationship further comprises a minimum energy value of the ultraviolet laser at which the raw material in a slurry form hardens.

5. the layer forming unit performs a first irradiation in which the ultraviolet laser is scanned along a first direction and irradiated a plurality of times such that parts of the irradiation ranges overlap each other while moving the ultraviolet laser by a predetermined distance along a second direction intersecting the first direction, thereby hardening the raw material; The additive manufacturing device of claim 1, wherein the number of irradiations, the first penetration depth, the second penetration depth, and the irradiation conditions satisfy the following mathematical expressions (2) to (5) as the previously acquired relationship. [0025] where y is the position of the layer in the direction along the second direction, Z 1 (y) is the hardened shape at the position y of the hardened portion formed by hardening the raw material by the first irradiation of the ultraviolet laser in the first irradiation, D p is the first penetration depth, w o is the spot radius of the ultraviolet laser, E max is the irradiation energy of the ultraviolet laser, E c is the minimum energy value of the ultraviolet laser at which the raw material hardens, Z n (y) is the cured shape of the layer at the position y after the first to nth (n is an integer of 2 or more) irradiations of the ultraviolet laser in the first irradiation, Z n-1 (y) is the hardened shape at the position y of the hardened portion formed by hardening the raw material by the first to (n-1)th irradiations of the ultraviolet laser in the first irradiation, a n is the hardened shape at the position y of the hardened portion formed by hardening the raw material by the n-th irradiation of the ultraviolet laser in the first irradiation, d is the distance, D p ' is the second penetration depth, P L is the irradiation output of the ultraviolet laser, and V s is the irradiation speed of the ultraviolet laser.

6. the layer forming unit performs a second irradiation, after the first irradiation, by performing a scanning along a second direction with the ultraviolet laser a plurality of times while moving a predetermined distance along the first direction, thereby hardening the raw material; The additive manufacturing device of claim 5, wherein the number of irradiations of the ultraviolet laser, the first penetration depth, and the second penetration depth satisfy the following mathematical expressions (6) and (7) as the previously acquired relationship. [0030] Here, z ch (y) is the cured shape of the layer at the position y after the second irradiation, a ch (y) is the hardened shape at the position y of the hardened portion formed by hardening the raw material by the irradiation of the ultraviolet laser during the second irradiation.

7. An additive manufacturing apparatus according to any one of claims 1 to 6, wherein the irradiation conditions determined by the controller include at least one of an irradiation output, an irradiation radius, and an irradiation speed of an ultraviolet laser.

8. An additive manufacturing apparatus for forming a three-dimensional object, comprising: a base to which a raw material containing an ultraviolet curable resin and ceramic particles is supplied; a layer forming unit that forms a layer of the raw material by irradiating the raw material on the base with an ultraviolet laser multiple times such that at least a portion of the irradiation ranges overlap each other; A controller for controlling the layer forming unit; Equipped with the controller inputs a target thickness of the layer and the number of times the raw material is irradiated with the ultraviolet laser when forming the layer, and causes the layer forming unit to perform scanning along a first direction with the ultraviolet laser while moving a predetermined distance at a time along a second direction intersecting the first direction, so that parts of the irradiation ranges overlap each other, An additive manufacturing apparatus, wherein the ultraviolet laser irradiation conditions satisfy the relationships of the following formulas (8) to (11). [0045] where y is the position of the layer in the direction along the second direction, Z 1 (y) is the hardened shape at the position y of the hardened portion formed by hardening the raw material by the irradiation of the first ultraviolet laser, D p is the first penetration depth, which is the penetration depth into the raw material before the raw material is hardened, w o is the spot radius of the ultraviolet laser, E max is the irradiation energy of the ultraviolet laser, E c is the minimum energy value of the ultraviolet laser at which the raw material hardens, Z n (y) is the cured shape of the layer at the position y after irradiation with the ultraviolet laser from the first to the nth (n is an integer of 2 or more), Z n-1 (y) is the shape of the cured portion at the position y formed by curing the raw material by irradiation with the 1st to (n-1)th ultraviolet lasers, a n is the hardened shape at the position y of the hardened portion formed by hardening the raw material by irradiation with the n-th ultraviolet laser, d is the distance, D p P′ is the second penetration depth, which is the penetration depth into the raw material after the raw material has hardened; L is the irradiation output of the ultraviolet laser, and V s is the irradiation speed of the ultraviolet laser.

9. 1. An apparatus for determining irradiation conditions of an ultraviolet laser in additive manufacturing for forming layers by irradiating a raw material containing an ultraviolet curable resin and ceramic particles with an ultraviolet laser multiple times such that at least a portion of the irradiation ranges overlap each other to form a three-dimensional object, comprising: an acquisition unit that acquires a target thickness of the layer and a number of times the raw material is irradiated with the ultraviolet laser when forming the layer; a determination unit that determines the irradiation conditions based on the acquired target film thickness and the number of irradiations and a relationship acquired in advance, the relationship being a relationship between the number of irradiations, a first penetration depth that is a penetration depth into the raw material before the raw material is hardened, a second penetration depth that is a penetration depth into the raw material after the raw material is hardened, and the irradiation conditions; A manufacturing condition determination device comprising:

10. 1. An apparatus for determining irradiation conditions of an ultraviolet laser in additive manufacturing, comprising: a raw material including an ultraviolet curable resin and ceramic particles; a scanning direction of the ultraviolet laser along a first direction is moved by a predetermined distance along a second direction intersecting the first direction, and the irradiation ranges are irradiated multiple times so as to overlap each other to form layers; and a three-dimensional object is formed by the above-mentioned additive manufacturing method, an acquisition unit that acquires a target thickness of the layer and a number of times the raw material is irradiated with the ultraviolet laser when forming the layer; a determination unit that receives the acquired target film thickness and the number of irradiations and determines the irradiation conditions; Equipped with The manufacturing condition determination device, wherein the irradiation conditions satisfy the relationships of the following formulas (12) to (15). [0050] where y is the position of the layer in the direction along the second direction, Z 1 (y) is the hardened shape at the position y of the hardened portion formed by hardening the raw material by the irradiation of the first ultraviolet laser, D p is the first penetration depth, which is the penetration depth into the raw material before the raw material is hardened, w o is the spot radius of the ultraviolet laser, E max is the irradiation energy of the ultraviolet laser, E c is the minimum energy value of the ultraviolet laser at which the raw material hardens, Z n (y) is the cured shape of the layer at the position y after irradiation with the ultraviolet laser from the first to the nth (n is an integer of 2 or more), Z n-1 (y) is the shape of the cured portion at the position y formed by curing the raw material by irradiation with the 1st to (n-1)th ultraviolet lasers, a n is the hardened shape at the position y of the hardened portion formed by hardening the raw material by irradiation with the n-th ultraviolet laser, d is the distance, D p P′ is the second penetration depth, which is the penetration depth into the raw material after the raw material has hardened; L is the irradiation output of the ultraviolet laser, and V s is the irradiation speed of the ultraviolet laser.

11. In additive manufacturing, a raw material including an ultraviolet curable resin and ceramic particles is irradiated with an ultraviolet laser multiple times so that at least a part of the irradiation ranges overlap each other to form layers, thereby forming a three-dimensional shaped object, the manufacturing condition determination program causes a computer to function as a device for determining irradiation conditions of the ultraviolet laser, the manufacturing condition determination program comprising: An acquisition unit that acquires a target thickness of the layer and a number of times the raw material is irradiated with the ultraviolet laser when forming the layer; and a determination unit that determines the irradiation conditions based on the acquired target film thickness and the number of irradiations and a relationship acquired in advance, the relationship being a relationship between the number of irradiations, a first penetration depth that is a penetration depth into the raw material before the raw material is hardened, a second penetration depth that is a penetration depth into the raw material after the raw material is hardened, and the irradiation conditions; A manufacturing condition determination program that functions as a

Citation Information

Patent Citations

  • Powder for lamination molding, slurry for lamination molding, three-dimensional lamination molded body, sintered compact, method for producing slurry for lamination molding, lamination molding method and sintering method

    JP2021011050A