AI Technical Summary
Existing near-infrared (NIR) transparent black pigments, particularly perylene-based pigments, suffer from color variability dependent on dispersion conditions and require adjusted proportions for consistent color, and they have low crystallinity and insufficient coloring performance, affecting their use in automotive and aerospace coatings and LiDAR detection.
A solid solution of NIR transparent black perylene-based pigments is developed, comprising specific compounds with defined molecular structures and production methods, ensuring consistent color independence and high black value, low saturation, and improved NIR transparency.
The solid solution achieves consistent color performance across varying concentrations, enhances NIR transparency, and improves LiDAR signal detection by reducing absorption, making it suitable for automotive, aerospace, and autonomous vehicle applications.
Smart Images

Figure 2022136308000001 
Figure 2022136308000002 
Figure 2022136308000003
Abstract
Description
[Technical field]
[0001] The present invention relates to at least one compound according to formula (I), [ka] and at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), The present invention relates to a solid solution comprising:
[0002] [ka]
[0003] The present invention further relates to a method for producing the solid solution.The present invention further relates to a solid solution obtainable or obtained according to said method, and to the use of the solid solution of the present invention, in particular as a near infrared (NIR) transparent black colorant in a non-NIR absorbing component. [Background technology]
[0004] In many coating applications, such as automotive coatings, aerospace coatings, industrial coatings, and architectural coatings, dark colors such as black are particularly desirable for aesthetic purposes. Black pigments have traditionally been carbon blacks such as PBk6, PBk7, or inorganic black pigments such as PBk11. However, dark coatings have historically been susceptible to near-infrared absorption, as they often rely on the use of pigments such as carbon black, which absorb near-infrared radiation in addition to visible light. Near-infrared (NIR) radiation, i.e., electromagnetic radiation having wavelengths between 700 and 2500 nanometers, constitutes more than 50% of the solar energy that reaches the Earth's surface. Heat is a direct result of the absorption of near-infrared (NIR) radiation. As a result, dark coatings have historically been susceptible to significant increases in temperature, especially on sunny days, which is often undesirable for a number of reasons.
[0005] Additionally, there have been recent advances in technology that utilizes near infrared (NIR) in relation to self-driving cars ("autonomous vehicles") and other objects around the vehicle that contain markings that can be detected by sensors onboard the autonomous vehicle.
[0006] Conventional carbon black pigments strongly absorb near-infrared (NIR) LiDAR signals for navigation used by autonomous vehicles. The low return of LiDAR signals reduces object detection capabilities, especially for dark objects containing high levels of carbon black. Automotive coating formulations using near-infrared (NIR) transparent or reflective functional black pigments can provide superior signal response and therefore improve object detection. However, while black pigments are an important formulation tool, conventional carbon black pigments strongly absorb LiDAR signals. Dark, black shades with good LiDAR response are desired.
[0007] Furthermore, in WO2018 / 081613, an attempt is made to obtain a method and system for increasing the NIR detection distance of an object coated with a NIR reflective coating using a physical mixture of different perylene-based pigments. However, even if such a blend of two (or more) pigments achieves the required color characteristics, the color characteristics obtained from the dispersed mixed pigments may vary significantly depending on the dispersion conditions used and the required color level in the target color. In order to achieve the required color at all concentrations when using a physical mixture of two (or more) pigments, it is generally necessary to adjust the ratio of the blended components to achieve the same neutral color.
[0008] US7083675 describes perylene-based pigments as solid solutions produced by calcination at high temperature in vacuum or in an inert gas atmosphere. However, these pigments have low crystallinity and insufficient color performance. Furthermore, due to the process conditions at high temperature under an inert gas atmosphere, these pigments cannot be conventionally used in the field of organic pigments.
[0009] A solid solution defines a crystal in which two or more molecules are contained within the same crystal structure, whose structure is the same as that which one molecule would adopt alone. The most concentrated molecule, whose crystal structure determines the structure of the solid solution, is called the host; the other molecule is called the guest. In either case, a solid solution can be distinguished from a physical mixture of the components by examining its X-ray diffraction pattern. In a physical mixture, the X-ray diffraction pattern features of each component are identifiable, and the pattern of the mixture is the sum of the patterns of each component. However, the X-ray diffraction pattern of a solid solution is clearly distinguishable from the X-ray diffraction patterns of each component; some of the X-ray lines of the components may disappear and new lines may appear. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] WO2018 / 081613 [Patent Document 2] US7083675 [Patent Document 3] EP0636666B1 [Patent Document 4] WO91 / 02034A1 [Patent Document 5] EP2316886A1 EP504922A1 [Patent Document 6] US2012018687A1 [Patent Document 7] CN110591445A [Patent Document 8] US4,450,273 [Patent Document 9] US2010 / 0184983A1 [Non-patent literature]
[0011] [Non-Patent Document 1] Justus Liebigs Annalen der Chemie, 1984, 483 Summary of the Invention [Problem to be solved by the invention]
[0012] However, there is a demand for improved color and functionality in near infrared (NIR) transparent black perylene-based pigments. In particular, the problem remains of providing a near infrared (NIR) transparent black perylene-based pigment whose color obtained from the dispersed mixed pigments is not highly dependent on the dispersion conditions used and the required pigment level in the target color. There is a need to achieve the required color at all concentrations without changing the ratio of the blended components. [Means for solving the problem]
[0013] It is therefore an object of the present invention to provide an improved solid solution containing a single near infrared (NIR) transparent black perylene-based pigment, which solid solution exhibits advantageous performance properties, in particular neutral color, very low chroma, and high black value (M C Color dependence and M Y Thus, it has been surprisingly found that solid solutions containing near infrared (NIR) transparent black perylene-based pigments provide advantageous performance properties, in particular neutral color, very low chroma, and high black value (M C Color dependence and M Y It has been found that the coloring is color-independent.
[0014] Accordingly, the present invention provides a compound comprising: (a) at least one compound according to formula (I): [ka] and (b) at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), With respect to a solid solution comprising [ka] where R1 and R2 are each independently -(CH2) n -X, where X represents hydrogen, methyl, C1-C5 alkoxyl, hydroxy, phenyl, C1-C5 alkylphenyl, C1-C5 alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C1-C5 alkylpyridyl, C1-C5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; R3 and R4 may each independently represent phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C1- may represent C5 alkylpyridinediyl, C1-C5 alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, and the two nitrogen atoms bonded to R3 according to formulas (II) and (III) together with the two atoms of the aromatic ring of R3 form a 5- or 6-membered heterocycle; the two nitrogen atoms bonded to R4 according to formulas (II) and (III) together with the two atoms of the aromatic ring of R4 form a 5- or 6-membered heterocycle; X1 to X8 may each independently represent hydrogen, C1-C5 alkyl, C1-C5 alkoxy, hydroxy, phenyl or halide.
[0015] According to the present invention, the two nitrogen atoms bonded to R3 according to formulas (II) and (III) preferably form a five-membered heterocyclic ring together with two adjacent atoms of the aromatic ring of R3; the two nitrogen atoms bonded to R4 according to formulas (II) and (III) preferably form a five-membered heterocyclic ring together with two adjacent atoms of the aromatic ring of R4.
[0016] According to the present invention, it is preferred that X represents C1-C5 alkoxyphenyl or phenyl, n is 1 or 2; R3 and R4 are each independently phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, halogenated phenylene or naphthalenediyl; X1 to X8 are each independently hydrogen or halide.
[0017] According to the invention, it is preferred that X represents methoxyphenyl or phenyl, n is 1 or 2; R3 and R4, independently of one another, are phenylene, methyl-phenylene, methoxy-phenylene, chloro-phenylene, dichloro-phenylene or naphthalenediyl; and X1 to X8 represent hydrogen.
[0018] According to a particular and preferred embodiment of the invention, R1 and R2, independently of one another, represent -CH2C6H4OCH3 or -CH2CH2C6H5; R3 and R4, independently of one another, represent phenylene, 4-chloro-phenylene, naphthalenediyl or 4,5-dichloro-phenylene; and X1 to X8 preferably represent hydrogen.
[0019] According to the present invention, it is preferred that R1 is R2 or R3 is R4 or R1 is R2 and R3 is R4, preferably R1 is R2 and R3 is R4.
[0020] According to the invention, it is preferred that X represents 4-methoxyphenyl, n is 1; R3 and R4 represent phenylene; and X1 to X8 represent hydrogen.
[0021] According to the invention, it is preferred that X represents 4-methoxyphenyl, n is 1; R3 and R4 are naphthalenediyl; and X1 to X8 are hydrogen.
[0022] According to the invention, it is preferred that X represents 4-methoxyphenyl, n is 1; R3 and R4 represent 4-chloro-phenylene; and X1 to X8 represent hydrogen.
[0023] According to the invention, it is preferred that X represents 4-methoxyphenyl, n is 1; R3 and R4 represent 4,5-dichloro-phenylene; and X1 to X8 represent hydrogen.
[0024] According to the invention, it is preferred that X represents phenyl, n is 2; R3 and R4 represent phenylene; and X1 to X8 represent hydrogen.
[0025] According to the invention, it is preferred that X represents phenyl, n is 2; R3 and R4 represent naphthalenediyl; and X1 to X8 represent hydrogen.
[0026] According to the invention, it is preferred that X represents phenyl, n is 2; R3 and R4 represent 4-chloro-phenylene; and X1 to X8 represent hydrogen.
[0027] According to the invention, preferably the solid solutions of the invention have a color-independent black value M in the range of 200 to 350, preferably in the range of 220 to 330, more preferably in the range of 230 to 300, more preferably in the range of 242 to 280. Y and a color-dependent black value M in the range of 200 to 350, preferably in the range of 220 to 330, more preferably in the range of 230 to 300, more preferably in the range of 242 to 280. C , indicates M Y and M C is determined in accordance with DIN EN ISO 18314-3.
[0028] According to the present invention, preferably, the solid solution of the present invention is a black near infrared (NIR) neutral transparent pigment of neutral hue, where near infrared refers to wavelengths in the range of 700 to 2500 nanometers and transparent refers to transparency in the near infrared region with a transmittance of more than 70%, preferably 80%, at 1000 nm.
[0029] According to the invention, preferably the solid solutions of the invention exhibit TSR values on reflective substrates (TSR values >80%) of more than 25%, preferably more than 33%.
[0030] According to the invention, preferably, the solid solutions of the invention exhibit near infrared reflectance values of more than 65%, preferably more than 75%, on a reflective substrate (reflectance of more than 90%) at 905 nm and near infrared reflectance values of more than 50%, preferably more than 60%, on a reflective substrate (reflectance of more than 70%) at 1550 nm.
[0031] According to the present invention, the solid solution of the present invention preferably has a particle size in the range of 5 to 1000 nm, preferably in the range of 10 to 500 nm, more preferably in the range of 20 to 200 nm.
[0032] According to the invention, preferably the solid solution of the invention comprises, preferably consists of, more preferably comprises, more preferably consists of one crystal modification in an amount of more than 80% by weight, more preferably more than 90% by weight, based on the total weight of the solid solution.
[0033] According to the invention, preferably in the solid solution, the mass ratio of at least one compound of formula (I) to at least one compound according to formula (II), or to at least one compound according to formula (III), or to a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), mass((I)):mass((II)(III)) is in the range of 60:40 to 99:1, preferably in the range of 65:35 to 95:5, more preferably in the range of 70:30 to 90:10, for example in the range of 70:30 to 80:20, or in the range of 75:25 to 85:15, or in the range of 80:20 to 90:10.
[0034] According to the present invention, preferably 80 to 100% by weight, preferably 85 to 100% by weight, more preferably 90 to 100% by weight, more preferably 95 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight of the solid solution consists of (a) at least one compound according to formula (I) and (b) at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III).
[0035] According to the present invention, preferably the solid solution comprises (a) one compound according to formula (I) and (b) one compound according to formula (II), or one compound according to formula (III), or a mixture of one compound according to formula (II) and one compound according to formula (III).
[0036] Alternatively, according to the present invention, preferably 80 to 100% by weight, preferably 85 to 100% by weight, more preferably 90 to 100% by weight, more preferably 95 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight of the solid solution consists of (a) one compound according to formula (I) and (b) one compound according to formula (II), or one compound according to formula (III), or a mixture of one compound according to formula (II) and one compound according to formula (III).
[0037] According to the invention, it is preferred to exclude compounds according to formula (IV) in the solid solution: [ka] wherein X1 to X8 are each independently hydrogen, C1-C5 alkyl, C1-C5 alkoxy, hydroxy, phenyl or halide.
[0038] The present invention further provides a method for preparing a solid solution comprising: (i) (a) at least one compound according to formula (I); [ka] and (b) providing a mixture comprising at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III); [ka] where R1 and R2 are each independently -(CH2) n-X, where X represents hydrogen, methyl, C1-C5 alkoxyl, hydroxy, phenyl, C1-C5 alkylphenyl, C1-C5 alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C1-C5 alkylpyridyl, C1-C5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; R3 and R4 may each independently represent phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C1-C5 alkylpyridinediyl, C1-C5 alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, and are linked to R3 according to formulae (II) and (III). wherein the two nitrogen atoms bonded to R4 according to formula (II) and (III) together with the two atoms of the aromatic ring of R4 form a 5- or 6-membered heterocyclic ring; wherein the two nitrogen atoms bonded to R4 according to formula (II) and (III) together with the two atoms of the aromatic ring of R4 form a 5- or 6-membered heterocyclic ring; X1 to X8 may each independently represent hydrogen, C1-C5 alkyl, C1-C5 alkoxy, hydroxy, phenyl or halide; (ii) mechanically treating the mixture provided according to (i); (iii) adding water to the mixture obtained from (ii); (iv) subjecting the mixture obtained from (iii) to solid-liquid separation; (v) washing the solid obtained from (iv) with at least one suitable washing agent; and (vi) drying the solid obtained from (v) to obtain a solid solution.
[0039] According to the present invention, preferably providing the mixture according to (i) comprises adding at least one suitable acid or solvent to the mixture, wherein the at least one suitable acid is preferably one or more of polyphosphoric acid and sulfuric acid, more preferably the at least one suitable acid comprises sulfuric acid, more preferably is sulfuric acid, and the at least one solvent comprises water, preferably is water.
[0040] According to the present invention, preferably providing the mixture according to (i) is carried out at a temperature of the mixture in the range of from 30 to 120°C, preferably in the range of from 40 to 110°C, more preferably in the range of from 50 to 100°C.
[0041] According to the present invention, preferably providing the mixture according to (i) is carried out at a temperature of the mixture in the range of 30 to 80°C, preferably in the range of 40 to 70°C, more preferably in the range of 45 to 60°C, and the process preferably further comprises adding at least one suitable base, solvent or sodium hydrosulfite to the mixture, wherein the at least one suitable base is preferably one or more of sodium hydroxide and potassium hydroxide, more preferably the at least one suitable base is sodium hydroxide, the at least one solvent comprises water, preferably is water, and more preferably the process further comprises adding at least one suitable oxidizing agent, more preferably the at least one suitable oxidizing agent is one or more of oxygen or hydrogen peroxide.
[0042] According to the present invention, preferably, the mechanical treatment according to (ii) comprises one or more of kneading and grinding, where kneading comprises co-extrusion, salt kneading, single screw kneading and twin screw kneading, and grinding comprises wet grinding, ball grinding, bead grinding, vibratory grinding, planetary grinding and attritor grinding.
[0043] According to the invention, preferably the mechanical treatment according to (ii) comprises, preferably is, kneading, said kneading being carried out at a temperature of the mixture in the range of from 40 to 120°C, preferably in the range of from 45 to 90°C, more preferably in the range of from 50 to 90°C, the process preferably comprises adding, either immediately before and / or during kneading, one or more suitable solvents or one or more of sodium chloride, sodium sulphate and anhydrous aluminium sulphate, preferably sodium chloride, to the mixture to be kneaded, more preferably the weight ratio of one or more of sodium chloride, sodium sulphate and anhydrous aluminium sulphate to the mixture provided according to (i) is from 20:1 to 1:1, preferably from 15:1 to 2:1, more preferably from 10:1 to 2:1, more preferably from 8:1 to 2:1, more preferably from 9:1 to 10:1, more preferably from 10 .... The ratio of the at least one solvent is preferably one or more of ethylene glycol, diethylene glycol, diacetone alcohol, dimethylformamide, glycerin, triethylene glycol, dipropylene glycol, ethylene glycol monobutyl ether, methyl ethyl ketone, cyclohexanone, dimethylacetamide, N-methylpyrrolidone, butyl acetate, glycerol triacetate, sulfolane, xylene, tetrahydrofuran, butanol, water, and dimethyl sulfoxide, and more preferably the at least one solvent comprises, and is more preferably, diethylene glycol, diacetone alcohol, dimethylformamide, xylene, butanol, water, and glycerin.
[0044] According to the invention, the mechanical treatment according to (ii) further comprises adding to the mixture to be kneaded, either immediately before and / or during kneading, at least one or more synergists, including sulfonic and carboxylic acid derivatives of perylene, indanthrone, phthalocyanine and diketopyrrolopyrrole, preferably in an amount of 1 to 15% by weight, more preferably in an amount of 1 to 5% by weight, based on the total weight of the kneaded mixture, and / or natural or synthetic resins, including esters and salts of abietic acid, hydrogenated or partially hydrogenated or dimerized rosins, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the kneaded mixture; or polysorbate-type nonionic surfactants, including esters or mixtures of esters formed from fatty acids, such as lauric acid or sebacic acid, and polyols, such as sorbitan monolaurate or dibutyl sebacate, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the kneaded mixture.
[0045] Alternatively, according to the present invention, preferably the mechanical treatment according to (ii) comprises, preferably is, grinding, said grinding being carried out at a temperature of the mixture in the range of from 40 to 120°C, preferably in the range of from 45 to 90°C, more preferably in the range of from 50 to 90°C, and the process preferably further comprises adding one or more of sodium chloride, sodium sulphate and anhydrous aluminium sulphate, preferably sodium chloride, to the mixture to be ground, either immediately prior to and / or during grinding.
[0046] According to the invention, preferably, the method further comprises adding at least one suitable acid or solvent to the milled mixture under stirring immediately after milling, at a temperature of the mixture in the range of 40 to 200° C., preferably in the range of 45 to 150° C., more preferably in the range of 50 to 120° C., wherein the at least one suitable acid is preferably one or more of polyphosphoric acid and sulfuric acid, more preferably the at least one suitable acid comprises sulfuric acid, more preferably is sulfuric acid, and the at least one solvent is preferably one or more of ethylene glycol, diethylene glycol, diacetone alcohol, dimethylformamide, glycerin, triethylene glycol, dipropylene glycol, ethylene glycol monobutyl ether, methyl ethyl ketone, cyclohexanone, dimethylacetamide, N-methylpyrrolidone, butyl acetate, glycerol triacetate, sulfolane, xylene, tetrahydrofuran, butanol, water and dimethyl sulfoxide, more preferably the at least one solvent comprises, more preferably is, diethylene glycol, diacetone alcohol, dimethylformamide, xylene, butanol, water and glycerin.
[0047] According to the present invention, preferably, the wet grinding is carried out with steel balls, silicon / aluminum / zirconium oxide beads, glass beads, ceramic beads and agate balls, preferably having a diameter in the range of 0.1-5 cm, the grinding being wet grinding, the wet grinding being carried out in water or in a mixture of water with at least one suitable organic solvent and optionally at least one suitable base, more preferably, the at least one suitable solvent comprises, more preferably, methanol, ethanol, propanol, isopropanol, butanol, pentanol, ethylene glycol, diethylene glycol, triethylene glycol and dipropylene glycol, more preferably, the at least one suitable base comprises, more preferably, sodium hydroxide, potassium hydroxide, sodium hydroxide, lithium hydroxide and benzyltrimethylammonium hydroxide.
[0048] Furthermore, according to the invention, preferably, the mechanical treatment according to (ii) further comprises adding to the mixture to be ground, either immediately before and / or during grinding, at least one or more synergists, preferably in an amount of 1 to 15% by weight, more preferably in an amount of 1 to 5% by weight, based on the total weight of the ground mixture, and / or esters and salts of abietic acid, natural or synthetic resins including hydrogenated or partially hydrogenated or dimerized rosins, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the ground mixture, or polysorbate-type nonionic surfactants including esters or mixtures of esters formed from fatty acids such as lauric acid or sebacic acid and polyols such as sorbitan monolaurate or dibutyl sebacate, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the ground mixture.
[0049] According to the present invention, preferably, at least one or more of the synergists include sulfonic and carboxylic acid derivatives of perylene, indanthrone (PB60), copper, aluminum or zinc phthalocyanines, quinacridones (PV19, PR202), dioxazines (PV23, PV37, PB80) and diketopyrrolopyrroles (PR254, PR255).
[0050] Furthermore, according to the present invention, it is preferred that at least one or more of the synergists comprises sulfonic acid and carboxylic acid derivatives of perylene, indanthrone, copper, aluminum or zinc phthalocyanine, quinacridone, dioxazine and diketopyrrolopyrrole, wherein the sulfonic acid and carboxylic acid derivatives of perylene, indanthrone, copper, aluminum or zinc phthalocyanine, quinacridone, dioxazine and diketopyrrolopyrrole are independently selected from the group consisting of -COO - M + , -COOR'5, -CONR'5R'6, -COO - N + R'5R'6R'7R'8, -SO2NR'5R'6, -CH2NR'5R'6, -CH2N + R'5R'6R'7R'8R'5-COO -and / or -CH2R'9, benzoyl, and further C1-C 12 -alkyl, C1-C6-alkoxy, nitro and / or halogen; R'5, R'6, R'7, R'8 may each independently represent hydrogen; C1-C 12 -Alkyl or C2-C 12 -alkenyl, the hydrocarbon chain of which may in each case be interrupted by one or more -O-, -S-, -NR'9-, -CO- or -SO2- moieties and / or may be mono- or polysubstituted by hydroxyl, halogen, aryl, C1-C4-alkoxy and / or acetyl; C3-C8-cycloalkyl, the carbon skeleton of which may be interrupted by one or more -O-, -S-, -NR' 10 R' may be interrupted by - or -CO- moieties and / or substituted by acetyl; R' represents phthalimidyl; R' 10 represents hydrogen or C1-C8-alkyl; M + represents hydrogen or a metal cation, in particular an alkali metal cation, more preferably sodium or potassium. Suitable synergists are described in EP0636666B1, preferably perylene derivatives of formula I; WO2005078023A2, preferably perylene derivatives of formula Ia' and Ib'; WO91 / 02034A1, preferably perylene derivatives of formula I; EP2316886A1, preferably compounds of formula DS-1, DS-2, DS-3; EP504922A1, preferably compounds of formula I; US2012018687A1, preferably compounds of formula I; US20050001202A1, preferably compounds of formula I-VII; EP0700420B1, preferably compounds of formula I-VII, or CN110591445A, preferably compounds of formula I, IA, IB, II, III, IV.
[0051] According to the present invention, preferably, the solid-liquid separation according to (iv) comprises one or more of centrifugation and filtration, more preferably filtration.
[0052] According to the present invention, preferably the at least one suitable washing agent according to (v) comprises water, more preferably is water, and the solid obtained from (iv) is preferably washed until the water obtained from the washing exhibits a conductivity of at most 100 microSiemens / cm.
[0053] Further, according to the present invention, preferably, drying of the solid obtained from (v) is carried out in a gas atmosphere, said gas atmosphere being preferably one or more of nitrogen, air, and lean air, and preferably having a temperature in the range of 50-150°C, more preferably 50-95°C, more preferably 60-90°C, more preferably 70-85°C.
[0054] According to the present invention, preferably in the method, n, X, R1, R2, R3, R4, X1 to X8, and specific combinations thereof are as defined for the solid solutions described in any of the specific and preferred embodiments described herein.
[0055] According to the present invention, preferably the solid solution is a solid solution as described in any of the specific and preferred embodiments described herein.
[0056] The present invention further relates to a solid solution obtainable or obtained by the process described in any of the particular and preferred embodiments described herein.
[0057] According to the present invention, a solid solution obtainable or obtainable by the method described in any of the specific and preferred embodiments described herein is preferred, wherein R1 and R2 are each independently -(CH2) n-X, where X represents hydrogen, methyl, C1-C5 alkoxyl, hydroxy, phenyl, C1-C5 alkylphenyl, C1-C5 alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C1-C5 alkylpyridyl, C1-C5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; R3 and R4 may each independently represent phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C1-C5 may represent alkylpyridinediyl, C1-C5 alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, wherein the two nitrogen atoms bonded to R3 according to formulae (II) and (III) together with the two atoms of the aromatic ring of R3 form a 5- or 6-membered heterocyclic ring; the two nitrogen atoms bonded to R4 according to formulae (II) and (III) together with the two atoms of the aromatic ring of R4 form a 5- or 6-membered heterocyclic ring; X1 to X8 may each independently represent hydrogen, C1-C5 alkyl, C1-C5 alkoxy, hydroxy, phenyl or halide.
[0058] The present invention further relates to a solid solution comprising one or more of a thermoplastic polymer, an elastomeric polymer, a crosslinked polymer or an essentially crosslinked polymer, preferably a polyolefin, a polyamide, a polyurethane, a polyacrylate, a polyacrylamide, a polyvinyl alcohol, a polycarbonate, a polystyrene, a polyester, a polyacetal, a natural or synthetic rubber, and a vinyl halide polymer, in an amount of 0.01% to 70% by weight, based on the total weight of the polymer.
[0059] The present invention further relates to a solid solution comprised in one or more of a thermoplastic polymer, an elastomeric polymer, a crosslinked polymer, or an intrinsically crosslinked polymer in the form of a coating composition applied to the surface of a substrate, preferably in the form of a film or coating applied to the surface of a substrate, or in the form of a fiber, sheet, or other molded or shaped article.
[0060] The present invention further relates to the solid solutions contained in one or more of coating compositions, light detection and ranging (LiDAR) devices, near infrared (NIR) non-absorbing components, photovoltaic components, thermal management components, thermal insulation components, pigmented coatings, printing inks, recyclable plastic products, biodegradable mulches, toners, charge generating materials, color filters, LC displays, and security printing components.
[0061] The present invention further relates to the solid solution, preferably for use as a component in one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
[0062] Additionally, in another embodiment, the present invention relates to the use of the solid solutions as one or more components of coating compositions, light detection and ranging (LiDAR) devices, near infrared (NIR) non-absorbing components, photovoltaic components, thermal management components, thermal insulation components, pigmented coatings, printing inks, recyclable plastic products, biodegradable mulches, toners, charge generating materials, color filters, LC displays, and security printing components.
[0063] Alternatively, the present invention relates to a coating composition, and / or a light detection and / or ranging (LiDAR) device, and / or a near infrared (NIR) non-absorbing component, and / or a photovoltaic component, and / or a thermal management component, and / or a thermal insulation component, and / or a pigmented coating, and / or a printing ink, and / or a recyclable plastic product, and / or a biodegradable mulch, and / or a toner, and / or a charge generating material, and / or a color filter, and / or an LC display, and / or a security printing component, comprising the solid solution described in any of the specific preferred embodiments described herein.
[0064] The present invention further relates to a multi-layer coating comprising a primer coating comprising a solid solution as described in any of the specific preferred embodiments herein and a white or reflective pigment having a reflectance of greater than 50% in the range of 700-2500 nm, in a weight ratio of 1: to 99:1, preferably 1:95 to 95:1; a base coat comprising a black (preferably comprising a solid solution as described in any of the specific preferred embodiments herein), colored pigment, metallic pigment or interference pigment; and, optionally, a clear top coat.
[0065] The present invention further relates to the use of the solid solution as described in any of the certain preferred embodiments described herein to manufacture one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a plastic, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
[0066] The invention further relates to a method for producing one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a plastic, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component, the method comprising providing and processing a solid solution as any of the certain preferred embodiments described herein.
[0067] The invention further relates to a method for identifying an article, the article comprising a feature comprising an effective amount of a solid solution as described in any of the specific preferred embodiments described herein, the feature being recorded under irradiation with electromagnetic radiation of a wavelength between 700 and 2500 nm, and an image of the feature being used to identify the article.
[0068] The present invention further relates to a method for laser welding articles, in which a solid solution as described in any of the certain preferred embodiments described herein is incorporated into a polymeric composition that is in contact with a surface of a meltable substrate containing a near infrared absorbing material, and then near infrared radiation from a laser, preferably at a wavelength in the range of 700-2500 nm, is passed through the layer containing a solid solution as described in any of the certain preferred embodiments described herein to the substrate underneath, generating sufficient heat at the point of irradiation to melt the two materials together.
[0069] The present invention further relates to a method for identifying recyclable plastic articles comprising a solid solution as described in any of the specific preferred embodiments described herein, preferably using a laser signal at a wavelength in the range of 700-2500 nm.
[0070] The present invention further relates to the use of a solid solution as described in any of the certain preferred embodiments described herein as a near infrared (NIR) transparent colorant that can replace a near infrared (NIR) absorbing black pigment in a coating or object to increase the signal to noise ratio in near infrared (NIR) radiation detection.
[0071] The present invention further relates to the use of a solid solution as described in any of the specific preferred embodiments described herein for LiDAR detection using a laser signal with a wavelength in the range of 700 to 2500 nm.
[0072] The present invention further relates to the use of a solid solution as described in any of the specific preferred embodiments described herein as a near infrared (NIR) transparent black colorant in a non-NIR absorbing component.
[0073] The present invention further relates to a coating comprising a solid solution according to any of the specific preferred embodiments described herein and at least one organic pigment and / or at least one inorganic pigment and / or effect pigment, the organic pigment being selected from the group consisting of: Colour Index (Cl) Pigment Yellow 109, 110, 139, 151, 154; Cl Pigment Orange 61, 64, 69, 73; Cl Pigment Red 122, 179, 202, 254, 264, 272, 282; Cl Pigment Brown 29; Cl Pigment Violet 19, 23, 37; Cl Pigment Blue 15:1, 15:2, 15:3, 15:4, 15:6, 60, 80; Cl Pigment Green 7, 36; Cl Pigment Black 31, 32, Spectrasense™ Black K 0087 (Lumogen® BLACK K 0087) and pigment preparations of said pigments; and the inorganic pigment is selected from the group consisting of Cl Pigment Yellow 53, 184, Cl Pigment Brown 24, 29, 33, 35, Cl Pigment Blue 28, 36, Cl Pigment Green 17, 26, 50, Cl Pigment Black 12, 30 and pigment preparations of said pigments.
[0074] The present invention is further described by the following series of embodiments and combinations of embodiments, which are derived from the indicated dependencies and back references. In particular, in each instance where a range of embodiments is mentioned, it is to be noted that in the context of a term such as "embodiing any one of embodiments 1-4...", all embodiments within this range are meant to be expressly disclosed for those skilled in the art, i.e., the expression of this term is understood by those skilled in the art to be equivalent to "embodiing any one of embodiments 1, 2, 3, and 4...". Furthermore, it is to be expressly noted that the following series of embodiments represents a properly organized part of the description directed to the general and preferred aspects of the present invention, rather than a series of claims determining the scope of protection.
[0075] According to embodiment 1, the present invention provides a method for producing a pharmaceutical composition comprising the steps of: (a) at least one compound according to formula (I) [ka] and (b) at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), With respect to a solid solution comprising [ka] where R1 and R2 are each independently -(CH2) n -X, where X is hydrogen, methyl, C1-C5 alkoxyl, hydroxy, phenyl, C1-C5 alkylphenyl, C1-C5 alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C1-C5 alkylpyridyl, C1-C5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; R3 and R4 are each independently phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C1-C 5 alkylpyridinediyl, C1-C5 alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, wherein the two nitrogen atoms bonded to R3 according to formulas (II) and (III) together with the two atoms of the aromatic ring of R3 form a 5- or 6-membered heterocyclic ring; the two nitrogen atoms bonded to R4 according to formulas (II) and (III) together with the two atoms of the aromatic ring of R4 form a 5- or 6-membered heterocyclic ring; X1 to X8 are each independently hydrogen, C1-C5 alkyl, C1-C5 alkoxy, hydroxy, phenyl or halide.
[0076] A preferred embodiment 2 embodying embodiment 1 is that X is C1-C5 alkoxyphenyl or phenyl, n is 1 or 2; R3 and R4 are each independently phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, halogenated phenylene, or naphthalenediyl; and X1 to X8 are each independently hydrogen or halide.
[0077] A preferred embodiment 3 embodying embodiment 1 or 2 is where X is methoxyphenyl or phenyl, n is 1 or 2; R3 and R4 are each independently phenylene, methyl-phenylene, methoxy-phenylene, chloro-phenylene, dichloro-phenylene, or naphthalenediyl; and X1 to X8 are hydrogen.
[0078] A preferred embodiment 4 embodying any one of embodiments 1 to 3 is where R1 and R2 are, independently of each other, -CH2C6H4OCH3 or -CH2CH2C6H5; R3 and R4 are, independently of each other, phenylene, 4-chloro-phenylene, naphthalenediyl or 4,5-dichloro-phenylene; and X1 to X8 are hydrogen.
[0079] A preferred embodiment 5 embodying any one of embodiments 1 to 4 is where R1 is R2, or R3 is R4, or R1 is R2 and R3 is R4, preferably R1 is R2 and R3 is R4.
[0080] A preferred embodiment 6 embodying any one of embodiments 1 to 5 is where X is 4-methoxyphenyl, n is 1; R3 and R4 are phenylene; and X1 to X8 are hydrogen.
[0081] A preferred embodiment 7 embodying any one of embodiments 1 to 5 is where X is 4-methoxyphenyl, n is 1; R3 and R4 are naphthalenediyl; and X1 to X8 are hydrogen.
[0082] A preferred embodiment 8 embodying any one of embodiments 1 to 5 is where X is 4-methoxyphenyl, n is 1; R3 and R4 are 4-chloro-phenylene; and X1 to X8 are hydrogen.
[0083] A preferred embodiment 9 embodying any one of embodiments 1 to 5 is where X is 4-methoxyphenyl, n is 1; R3 and R4 are 4,5-dichloro-phenylene; and X1 to X8 are hydrogen.
[0084] A preferred embodiment 10 embodying any one of embodiments 1 to 5 is where X is phenyl, n is 2; R3 and R4 are phenylene; and X1 to X8 are hydrogen.
[0085] A preferred embodiment 11 embodying any one of embodiments 1 to 5 is where X is phenyl, n is 2; R3 and R4 are naphthalenediyl; and X1 to X8 are hydrogen.
[0086] A preferred embodiment 12 embodying any one of embodiments 1 to 5 is where X is phenyl, n is 2; R3 and R4 are 4-chloro-phenylene; and X1 to X8 are hydrogen.
[0087] A preferred embodiment 13 embodying any one of the embodiments 1 to 12 has a color-independent black value M in the range of 200 to 350, preferably in the range of 220 to 330, more preferably in the range of 230 to 300, more preferably in the range of 242 to 280. Y and a color-dependent black value M in the range of 200 to 350, preferably in the range of 220 to 330, more preferably in the range of 230 to 300, more preferably in the range of 242 to 280. C , indicates M Y and M C is determined in accordance with DIN EN ISO 18314-3.
[0088] A preferred embodiment 14 embodying any one of the embodiments 1 to 13 is a black near infrared (NIR) neutral transparent pigment of neutral hue, where near infrared refers to wavelengths in the range of 700 to 2500 nanometers and transparent refers to transparency in the near infrared range having a transmittance of more than 70%, preferably 80%, at 1000 nm.
[0089] A preferred embodiment 15 embodying any one of embodiments 1 to 14 exhibits a TSR value on a reflective substrate (TSR value >80%) of greater than 25%, preferably greater than 33%.
[0090] A preferred embodiment 16 embodying any one of embodiments 1 to 15 exhibits a near infrared reflectance at 905 nm of greater than 65%, preferably greater than 75%, on a reflective substrate (greater than 90% reflectance) and a near infrared reflectance at 1550 nm of greater than 50%, preferably greater than 60%, on a reflective substrate (greater than 70% reflectance).
[0091] A preferred embodiment 17 embodying any one of embodiments 1 to 16 has a particle size in the range of 5 to 1000 nm, preferably in the range of 10 to 500 nm, and more preferably in the range of 20 to 200 nm.
[0092] A preferred embodiment 18 embodying any one of the embodiments 1 to 17, wherein the solid solution comprises, preferably consists of, more preferably comprises, more preferably consists of one crystal modification in an amount of more than 80% by weight, more preferably more than 90% by weight, based on the total weight of the solid solution.
[0093] A preferred embodiment 19 embodying any one of the embodiments 1 to 18, wherein in the solid solution, the mass ratio of at least one compound of formula (I) to at least one compound according to formula (II), or to at least one compound according to formula (III), or to a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), mass((I)):mass((II)(III)) is in the range of 60:40 to 99:1, preferably in the range of 65:35 to 95:5, more preferably in the range of 70:30 to 90:10, such as in the range of 70:30 to 80:20, or in the range of 75:25 to 85:15, or in the range of 80:20 to 90:10.
[0094] A preferred embodiment 20 embodying any one of the embodiments 1 to 19, is characterized in that 80 to 100% by weight, preferably 85 to 100% by weight, more preferably 90 to 100% by weight, more preferably 95 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight of the solid solution is (a) at least one compound according to formula (I), and (b) at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), It consists of:
[0095] A preferred embodiment 21 embodying any one of the embodiments 1 to 20 is (a) one compound according to formula (I), and (b) one compound according to formula (II), or one compound according to formula (III), or a mixture of one compound according to formula (II) and one compound according to formula (III), Includes.
[0096] A preferred embodiment 22 embodying embodiment 21 is characterized in that 80 to 100% by weight, preferably 85 to 100% by weight, more preferably 90 to 100% by weight, more preferably 95 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight of the solid solution is (a) one compound according to formula (I), and (b) one compound according to formula (II), or one compound according to formula (III), or a mixture of one compound according to formula (II) and one compound according to formula (III), It consists of:
[0097] According to embodiment 23, the present invention relates to a method for producing a solid solution, comprising the steps of: (i)(a) at least one compound according to formula (I); [ka] and (b) at least one compound according to formula (II), or at least one compound according to formula (III), or a mixture of at least one compound according to formula (II) and at least one compound according to formula (III), providing a mixture comprising: [ka] where R1 and R2 are each independently -(CH2) n-X, where X is hydrogen, methyl, C1-C5 alkoxyl, hydroxy, phenyl, C1-C5 alkylphenyl, C1-C5 alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C1-C5 alkylpyridyl, C1-C5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; R3 and R4 are each independently phenylene, C1-C5 alkylphenylene, C1-C5 alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C1-C 5 alkylpyridinediyl, C1-C5 alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, wherein the two nitrogen atoms bonded to R3 according to formulas (II) and (III) together with the two atoms of the aromatic ring of R3 form a 5- or 6-membered heterocyclic ring; the two nitrogen atoms bonded to R4 according to formulas (II) and (III) together with the two atoms of the aromatic ring of R4 form a 5- or 6-membered heterocyclic ring; X1 to X8 are each independently hydrogen, C1-C5 alkyl, C1-C5 alkoxy, hydroxy, phenyl or halide: (ii) mechanically treating the mixture provided in accordance with (i); (iii) adding water to the mixture resulting from (ii); (iv) subjecting the mixture obtained from (iii) to solid-liquid separation; (v) washing the solid obtained from (iv) with at least one suitable washing agent; (vi) drying the solid obtained from (v) to obtain a solid solution. The present invention relates to a method for producing a solid solution comprising the steps of:
[0098] A preferred embodiment 24 embodying embodiment 23 is that providing the mixture according to (i) comprises adding at least one suitable acid or solvent to the mixture, the at least one suitable acid is preferably one or more of polyphosphoric acid and sulfuric acid, more preferably the at least one suitable acid comprises sulfuric acid, more preferably is sulfuric acid, and the at least one solvent comprises water, preferably is water.
[0099] A preferred embodiment 25 embodying embodiment 23 or 24, wherein providing the mixture according to (i) is carried out at a temperature of the mixture in the range of from 30 to 120° C., preferably in the range of from 40 to 110° C., more preferably in the range of from 50 to 100° C.
[0100] A preferred embodiment 26 embodying embodiment 23 is wherein providing the mixture according to (i) is carried out at a temperature of the mixture in the range of 30 to 80° C., preferably in the range of 40 to 70° C., more preferably in the range of 45 to 60° C., and wherein the method preferably further comprises adding at least one suitable base, solvent or sodium hydrosulfite to the mixture, wherein the at least one suitable base is preferably one or more of sodium hydroxide and potassium hydroxide, more preferably the at least one suitable base is sodium hydroxide, the at least one solvent comprises water, preferably is water, and more preferably the method further comprises adding at least one suitable oxidizing agent, more preferably the at least one suitable oxidizing agent is one or more of oxygen or hydrogen peroxide.
[0101] A preferred embodiment 27 embodying any one of embodiments 23 to 26, wherein the mechanical treatment according to (ii) includes one or more of kneading and grinding, the kneading includes coextrusion, salt kneading, single-screw kneading, and twin-screw kneading, and the grinding includes wet grinding, ball grinding, bead grinding, vibration grinding, planetary grinding, and attritor grinding.
[0102] A preferred embodiment 28 embodying embodiment 27 is characterized in that the mechanical treatment according to (ii) comprises, preferably is, kneading, said kneading being carried out at a temperature of the mixture in the range of from 40 to 120°C, preferably in the range of from 45 to 90°C, more preferably in the range of from 50 to 90°C, and the process preferably comprises adding, either immediately before and / or during kneading, one or more suitable solvents and / or one or more of sodium chloride, sodium sulfate and anhydrous aluminum sulfate, preferably sodium chloride, to the mixture to be kneaded, more preferably the weight ratio of one or more of sodium chloride, sodium sulfate and anhydrous aluminum sulfate to the mixture provided according to (i) is from 20:1 to 1:1, preferably from 15:1 to 2:1, more preferably from 10:1 to 2:1, more preferably from 8:1 to 2: The ratio of the at least one solvent is preferably one or more of ethylene glycol, diethylene glycol, diacetone alcohol, dimethylformamide, glycerin, triethylene glycol, dipropylene glycol, ethylene glycol monobutyl ether, methyl ethyl ketone, cyclohexanone, dimethylacetamide, N-methylpyrrolidone, butyl acetate, glycerol triacetate, sulfolane, xylene, tetrahydrofuran, butanol, water and dimethyl sulfoxide, more preferably the at least one solvent comprises, more preferably is, diethylene glycol, diacetone alcohol, dimethylformamide, xylene, butanol, water and glycerin.
[0103] A preferred embodiment 29 embodying embodiment 27 or 28 further comprises that the mechanical treatment according to (ii) further comprises adding to the mixture to be kneaded either immediately before and / or during kneading at least one or more synergists comprising sulfonic and carboxylic acid derivatives of perylene, indanthrone, phthalocyanine and diketopyrrolopyrrole, preferably in an amount of 1 to 15% by weight, more preferably in an amount of 1 to 5% by weight, based on the total weight of the kneaded mixture, and / or natural or synthetic resins comprising esters and salts of abietic acid, hydrogenated or partially hydrogenated or dimerized rosins, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the kneaded mixture, or polysorbate-type nonionic surfactants comprising esters or mixtures of esters formed from fatty acids such as lauric acid or sebacic acid and polyols such as sorbitan monolaurate or dibutyl sebacate, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the kneaded mixture, based on the total weight of the kneaded mixture.
[0104] A preferred embodiment 30 embodying any one of embodiments 27 to 29, wherein the mechanical treatment according to (ii) comprises, preferably is, grinding, said grinding being carried out at a temperature of the mixture in the range of from 40 to 120°C, preferably in the range of from 45 to 90°C, more preferably in the range of from 50 to 90°C, and the method further comprises adding, preferably either immediately prior to and / or during grinding, one or more of sodium chloride, sodium sulfate and anhydrous aluminum sulfate, preferably sodium chloride, to the mixture to be ground.
[0105] A preferred embodiment 31 embodying embodiment 30, wherein the method further comprises adding at least one suitable acid or solvent to the grinding mixture under stirring immediately after grinding at a temperature of the mixture in the range of 40 to 200° C., preferably in the range of 45 to 150° C., more preferably in the range of 50 to 120° C., wherein the at least one suitable acid is preferably one or more of polyphosphoric acid and sulfuric acid, more preferably the at least one suitable acid comprises sulfuric acid, more preferably is sulfuric acid, and the at least one solvent is preferably one or more of ethylene glycol, diethylene glycol, diacetone alcohol, dimethylformamide, glycerin, triethylene glycol, dipropylene glycol, ethylene glycol monobutyl ether, methyl ethyl ketone, cyclohexanone, dimethylacetamide, N-methylpyrrolidone, butyl acetate, glycerol triacetate, sulfolane, xylene, tetrahydrofuran, butanol, water, and dimethyl sulfoxide, more preferably the at least one solvent comprises, more preferably is, diethylene glycol, diacetone alcohol, dimethylformamide, xylene, butanol, water, and glycerin.
[0106] A preferred embodiment 32 embodying embodiment 30 or 31 is characterized in that the grinding is carried out with steel balls, silicon / aluminum / zirconium oxide beads, glass beads, ceramic beads and agate balls, preferably having a diameter in the range of 0.1 to 5 cm, and the grinding is wet grinding, and the wet grinding is carried out in water or a mixture of water and at least one suitable organic solvent and optionally at least one suitable base, more preferably the at least one suitable solvent comprises, more preferably methanol, ethanol, propanol, isopropanol, butanol, pentanol, ethylene glycol, diethylene glycol, triethylene glycol and dipropylene glycol, and more preferably the at least one suitable base comprises, more preferably sodium hydroxide, potassium hydroxide, sodium hydroxide, lithium hydroxide and benzyltrimethylammonium hydroxide.
[0107] A preferred embodiment 33 embodying any one of the embodiments 30 to 32, further comprises adding, either immediately before and / or during the grinding, at least one or more synergists, preferably in an amount of 1 to 15% by weight, more preferably in an amount of 1 to 5% by weight, based on the total weight of the ground mixture, and / or esters and salts of abietic acid, natural or synthetic resins including hydrogenated or partially hydrogenated or dimerized rosins, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the ground mixture, or polysorbate-type nonionic surfactants including esters or mixtures of esters formed from fatty acids such as lauric acid or sebacic acid and polyols such as sorbitan monolaurate or dibutyl sebacate, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the ground mixture, to the mixture to be ground, preferably in an amount of 1 to 50% by weight, more preferably in an amount of 5 to 30% by weight, based on the total weight of the ground mixture.
[0108] A preferred embodiment 34 embodying any one of embodiments 30 to 33, wherein at least one of the synergists comprises sulfonic and carboxylic acid derivatives of perylene, indanthrone (PB60), copper, aluminum or zinc phthalocyanine, quinacridone (PV19, PR202), dioxazine (PV23, PV37, PB80) and diketopyrrolopyrrole (PR254, PR255).
[0109] A preferred embodiment 35 embodying any one of embodiments 23 to 34, wherein the solid-liquid separation according to (iv) comprises one or more of centrifugation and filtration, more preferably filtration.
[0110] A preferred embodiment 36 embodying any one of embodiments 23 to 35, wherein the at least one suitable washing agent according to (v) preferably comprises, more preferably is, water, and the solid obtained from (iv) is preferably washed until the water obtained from the washing exhibits a conductivity of at most 100 microSiemens / cm.
[0111] A preferred embodiment 37 embodying any one of embodiments 23 to 36, wherein drying of the solid obtained from (v) is carried out in a gas atmosphere, said gas atmosphere being preferably one or more of nitrogen, air, and lean air, and having a temperature preferably in the range of 50 to 150°C, more preferably 50 to 95°C, more preferably 60 to 90°C, more preferably 70 to 85°C.
[0112] A preferred embodiment 38 embodying any one of embodiments 23 to 37 is wherein n, X, R1, R2, R3, R4, X1 to X8, and specific combinations thereof are as defined in any one of embodiments 2 to 12.
[0113] A preferred embodiment 39 embodying any one of embodiments 23 to 38, wherein the solid solution is a solid solution according to any one of embodiments 1 to 22.
[0114] According to embodiment 40, the present invention relates to a solid solution, preferably according to any one of embodiments 1 to 22, obtainable or obtained by the method according to any one of embodiments 23 to 39.
[0115] According to embodiment 41, the present invention relates to a solid solution according to any one of embodiments 1 to 22 or 40, which is contained in one or more of thermoplastic polymers, elastomeric polymers, crosslinked polymers or essentially crosslinked polymers, preferably one or more of polyolefins, polyamides, polyurethanes, polyacrylates, polyacrylamides, polyvinyl alcohols, polycarbonates, polystyrenes, polyesters, polyacetals, natural or synthetic rubbers and halogenated vinyl polymers, in an amount of 0.01% to 70% by weight, based on the total weight of the polymers.
[0116] According to embodiment 42, the present invention relates to the solid solution according to any one of embodiments 1 to 22 or 40, contained in one or more of a thermoplastic polymer, an elastomeric polymer, a crosslinked polymer, or an intrinsically crosslinked polymer, in the form of a coating composition applied to the surface of a substrate, preferably a film or coating applied to the surface of a substrate, or in the form of a fiber, sheet, or other molded or shaped article.
[0117] According to embodiment 43, the present invention relates to the solid solution according to any one of embodiments 1 to 22 or 40 in one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
[0118] According to embodiment 44, the present invention relates to a solid solution according to any one of embodiments 1 to 22 or 40 for use as a component in one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
[0119] According to embodiment 45, the present invention relates to the use of the solid solution according to any one of embodiments 1 to 22 or 40 as one or more components of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
[0120] According to embodiment 46, the present invention relates to a coating composition, and / or a light detection and / or ranging (LiDAR) device, and / or a near infrared (NIR) non-absorbing component, and / or a photovoltaic component, and / or a thermal management component, and / or a thermal insulation component, and / or a pigmented paint, and / or a printing ink, and / or a recyclable plastic product, and / or a biodegradable mulch, and / or a toner, and / or a charge generating material, and / or a color filter, and / or an LC display, and / or a security printing component, comprising the solid solution as described in any one of embodiments 1 to 22 or 40.
[0121] According to embodiment 47, the present invention relates to a multi-layer coating comprising a primer coating comprising a solid solution as defined in any one of embodiments 1 to 22 or 40 and a white or reflective pigment having a reflectance of more than 50% in the range of 700 to 2500 nm in a mass ratio of 1: to 99:1, preferably 1:95 to 95:1; a base coat, preferably comprising a black, colored, metallic or interference pigment comprising a solid solution as defined in any one of embodiments 1 to 22 or 40; and optionally a clear top coat.
[0122] According to embodiment 48, the present invention relates to the use of the solid solution according to any one of embodiments 1 to 22 or 40 for manufacturing one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a plastic, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
[0123] According to embodiment 49, the present invention relates to a method for manufacturing one or more of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a plastic, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component, the method comprising providing and processing a solid solution according to any one of embodiments 1 to 22 or 40.
[0124] According to embodiment 50, the present invention relates to a method for identifying an article, the article being provided with a mark comprising an effective amount of a solid solution as described in any one of embodiments 1 to 22 or 40, the mark being recorded under irradiation with electromagnetic waves having a wavelength of 700 to 2500 nm, and an image of the mark being used to identify the article.
[0125] According to embodiment 51, the present invention relates to a method for laser welding articles, in which a solid solution as described in any one of embodiments 1 to 22 or 40 is incorporated into a polymer composition that is in contact with a surface of a meltable substrate containing a near infrared absorbing material, and then near infrared radiation from a laser, preferably at a wavelength in the range of 700 to 2500 nm, passes through the layer containing the solid solution according to any one of embodiments 1 to 22 or 40 to the substrate underneath, generating sufficient heat at the point of irradiation to melt the two materials together.
[0126] According to embodiment 52, the present invention relates to a method for identifying recyclable plastic articles containing the solid solution according to any one of embodiments 1 to 22 or 40 using a laser signal with a wavelength in the range of 700 to 2500 nm.
[0127] According to embodiment 53, the present invention relates to the use of the solid solution according to any one of embodiments 1 to 22 or 40 as a near infrared (NIR) transparent colorant capable of replacing a near infrared (NIR) absorbing black pigment in a coating or object to increase the signal-to-noise ratio in near infrared (NIR) radiation detection.
[0128] According to embodiment 54, the present invention relates to the use of a solid solution as described in any one of embodiments 1 to 22 or 40 for LiDAR detection using a laser signal with a wavelength in the range of 700 to 2500 nm.
[0129] According to embodiment 55, the present invention relates to the use of a solid solution as described in any one of embodiments 1 to 22 or 40 as a near infrared (NIR) transparent black colorant in a non-NIR absorbing component.
[0130] The present invention is further illustrated by the following examples and reference examples.
[0131] Working Example Sample preparation Sample preparations 1 to 10 were prepared using the solid solution obtained in Example 1 below. As used herein below, the term "pigment" refers to a solid solution according to the present invention prepared according to Example 1 below.
[0132] Sample preparation 1: 20% by weight pigment millbase A 20% by weight pigment millbase was prepared by mixing 20% by weight pigment with 20% by weight aqueous dispersant (Dispex® Ultra PX 4585 (50% by weight dispersant and 50% by weight water), an acrylic block copolymer supplied by BASF SE, 59.5% by weight demineralized water and 0.5% by weight antifoam additive (FoamStar® ST 2400 (100% by weight antifoam) supplied by BASF SE) in a sealable vessel. Dispersing medium (e.g. glass beads 2 mm diameter) was added to the vessel in a mass ratio of millbase components:beads of 1:2 and the vessel was sealed. The vessel was then loaded into a Skandex disperser (the Skandex disperser is a well-known shaker disperser widely used in the coatings industry. Similar designs are available from various companies and are available from LAU. The millbase components were dispersed for 6 hours in a plasticizer (Plastic Epoxy Resin GmbH is one of the most well-known suppliers). After dispersion, the beads were removed from the homogeneous liquid millbase by pouring the contents through a coarse filter. The resulting 20% by weight pigment millbase could be used in paint formulations.
[0133] Sample preparation 2: 15% by weight carbon black mill base A 15% by weight carbon black mill base was prepared by mixing 15% by weight of Colour Black FW200 carbon black pigment (provided by Orion Engineered Carbons) with 15% by weight of an aqueous dispersant (Dispex® Ultra PX 4585 (50% by weight dispersant and 50% by weight water), an acrylic block copolymer supplied by BASF SE, 69.6 parts of demineralized water and 0.4% by weight of an antifoam additive (FoamStar® ST 2400 (100% by weight supplied by BASF SE)) in a sealable container. A dispersing medium (e.g. glass beads 2 mm diameter) was added to the container in a 1:2 weight ratio of mill base components:beads and the container was sealed. The container was then loaded into a Skandex disperser and the mill base components were dispersed for 6 hours. After dispersion, the beads were removed from the homogenous liquid mill base by pouring the contents through a coarse filter. The resulting 15 wt % carbon black pigment millbase was ready for use in paint formulations.
[0134] Sample preparation 3: 70% by weight pigment titanium dioxide millbase The 70% by weight pigment millbase is made of 70% by weight Kronos 2310 titanium dioxide pigment (supplied by Kronos Worldwide Inc.), 6.5% by weight aqueous dispersant (Dispex® Ultra PX 4575 (40% by weight dispersant and 60% by weight water), an acrylic block copolymer supplied by BASF SE, 23.1% by weight demineralized water, and 0.4% by weight antifoam additive (FoamStar® ST supplied by BASF SE). A 70% by weight pigment millbase was prepared by mixing 100% by weight of 1,2-dichloro-2,4-diphenyl ...
[0135] [Table 1]
[0136] 1 Pigment Black 7 carbon black pigment is commercially available from various pigment companies, e.g. Colour Black FW200, Orion Engineered Carbons. 2 Pigments according to Examples 1-2 3 Pigment White 6 titanium dioxide pigment is commercially available from various pigment companies, e.g., Kronos 2310, Kronos Worldwide Inc. 4 Commercially available from BASF SE. 5 Commercially available from BASF SE. 6 Commercially available from BASF SE.
[0137] Sample Preparation 4: Water-Based Basecoat Let-Down Resin The aqueous let-down resin system consisted of 15% by weight of an alkali swellable acrylic dispersion (Setaqua® 6802 supplied by Allnex Resins (24% by weight solid resin material, 76% by weight solvent and neutralizing base)), 9% by weight of a thermosetting aqueous acrylic emulsion (Setaqua® 6160 supplied by Allnex Resins (45% by weight solid resin material, 55% by weight volatile solvent and neutralizing base)), 52% by weight of an aliphatic polyester-based polyurethane emulsion (Daotan® TW 6466 / 36WA (36% by weight solid resin material, 64% by weight solvent and neutralizing base)), Allnex Resins (100% by weight volatile solvent and neutralizing base)). A let-down resin was prepared by mixing 4.8 wt. % of a methylated monomeric melamine crosslinker (Cymel® 303LF (>98 wt. % solid resin material, <2 wt. % volatile solvents and formaldehyde) supplied by Allnex Resins) with 1.0 wt. % of a methylated monomeric melamine crosslinker (Cymel® 303LF (>98 wt. % solid resin material, <2 wt. % volatile solvents and formaldehyde) supplied by Allnex Resins). Demineralized water, a neutralizing amine (dimethylethanolamine) and a co-solvent (butyl glycol) were also incorporated to adjust the solids, viscosity and pH parameters of the let-down resin as would be used by one skilled in the art of preparing water-based resin systems.
[0138] Sample Preparation 5: Aluminum Base 7.60% by weight of Toyal TCR 3040 silver dollar, non-leafing aluminum paste (supplied by Toyo Aluminum) was wetted with 2% by weight of Additol® XL250 pigment wetting agent (volatile components including 55% by weight solids and 45% by weight solvents, supplied by Allnex Resins) and 11% by weight of hydrophilic solvents (n-butanol and butyl glycol). Once fully wetted and homogeneous, 50% by weight of the aqueous basecoat let-down resin (Sample Preparation 4) was added under stirring, followed by 29.4% by weight of demineralized water.
[0139] Sample Preparation 6: Pigmented masstone basecoat (2.5% pigment by weight) 12.5% by weight of the 20% by weight pigment millbase (sample preparation 1) was mixed under stirring with 60% by weight of the aqueous basecoat let-down resin (sample preparation 4) and other co-solvents and application additives (e.g. wetting agents) known to those skilled in the art of aqueous coatings formulation. Viscosity and pH adjustment was achieved using a mixture of demineralized water, neutralized Rheovis® AS 1130 (30% by weight alkali swellable acrylic copolymer emulsion (ASE) in water, supplied by BASF SE) and neutralized amine (dimethylethanolamine) to obtain a viscosity of 40-45 seconds in a DIN4 flow cup and a pH in the range of 8.0-8.5.
[0140] Sample Preparation 7: Carbon Black Masstone Basecoat (2.5% Pigment by Weight) 16.7% by weight of 15% by weight carbon black mill base (Sample Preparation 2) was mixed under agitation with 60% by weight of the aqueous basecoat let down resin (Sample Preparation 4) and other co-solvents and application additives (e.g. wetting agents) known to those skilled in the art of aqueous coating formulation. Viscosity and pH adjustment was achieved using a mixture of demineralized water, neutralized Rheovis® AS 1130 (30% by weight alkali swellable acrylic copolymer emulsion (ASE) in water, supplied by BASF SE) and neutralized amine (dimethylethanolamine) to obtain a viscosity of 40-45 seconds in a DIN 4 flow cup and a pH in the range of 8.0-8.5.
[0141] [Table 2]
[0142] 1 A wetting agent solution comprising Surfynol® 104 (100% by weight defoamer) supplied by Evonik in butyl glycol. 2 Blending alcohol and glycol ether solvents to achieve good film coalescence 3Viscosity and pH adjustment is achieved using a combination of demineralized water, neutralized Rheovis® AS 1130 (alkali swellable acrylic copolymer emulsion (ASE) 30% by weight in water, supplied by BASF SE) and neutralizing amine (dimethylethanolamine). Solid content 23.3% by mass Pigment content 2.5% by mass Pigment:binder mass ratio 1:8.3
[0143] Sample preparation: 8:10:90 (mass ratio) Pigment: White titanium dioxide reduction product 10.1% by weight of the 20% pigmented millbase (Preparation 1) and 25.8% by weight of the pigmented titanium dioxide millbase (Preparation 3) were mixed under stirring with 50.7% by weight of the aqueous basecoat let-down resin (Sample Preparation 4) and other co-solvents and application additives (e.g. wetting agents) known to those skilled in the art of aqueous coatings preparation. Viscosity and pH adjustment was achieved using a mixture of demineralized water, neutralized Rheovis® AS 1130 (30% by weight alkali swellable acrylic copolymer emulsion (ASE) in water, supplied by BASF SE) and neutralized amine (dimethylethanolamine) to obtain a viscosity of 40-45 seconds in a DIN4 flow cup and a pH in the range of 8.0-8.5.
[0144] [Table 3]
[0145] 1 A wetting agent solution comprising Surfynol® 104 (100% by weight defoamer) supplied by Evonik in butyl glycol. 2 Blending alcohol and glycol ether solvents to achieve good film coalescence 3Viscosity and pH adjustment is achieved using a combination of demineralized water, neutralized Rheovis® AS 1130 (alkali swellable acrylic copolymer emulsion (ASE) 30% by weight in water, supplied by BASF SE) and neutralizing amine (dimethylethanolamine). Solid content 38.2% by mass Pigment content: 20.1% by mass (10:90 black: titanium dioxide) Pigment:binder weight ratio 1:0.9
[0146] Sample preparation: 9:50:50 (mass ratio) pigment:aluminum reduction product 28.3 wt% of aluminum base (sample preparation 5) was mixed under stirring with 45.0 wt% of aqueous basecoat let-down resin (sample preparation 4). Demineralized water, neutralized amine and co-solvent were added to adjust the solids and pH of the mixture. 8.5 wt% of 20 wt% pigment millbase was added under stirring. Flake orientation in the basecoat was controlled using Laponite® RD (clay type rheology base additive, supplied by Byk-Chemie GmbH). Adjustment of the final spray viscosity and pH was achieved using a mixture of demineralized water, neutralized Rheovis® AS 1130 (30 wt% alkali swellable acrylic copolymer emulsion (ASE) in water, supplied by BASF SE) and neutralized amine (dimethylethanolamine) to obtain a viscosity of 40-45 seconds in a DIN4 flow cup and a pH in the range of 8.0-8.5.
[0147] [Table 4]
[0148] 1 A wetting agent solution comprising Surfynol® 104 supplied by Evonik in butyl glycol. 2Flake control additives including clay type additives such as Laponite® RD supplied by BYK-Chemie GmbH, low molecular weight polypropylene glycols such as Pluriol® P900 supplied by BASF SE, and demineralized water. 3 Viscosity and pH adjustment is achieved using a mixture of demineralized water, neutralized Rheovis® AS 1130 (alkali swellable acrylic copolymer emulsion in water (ASE) supplied by BASF SE) and neutralized amine (dimethylethanolamine). solid 23.7 mass Pigment content: 3.4% by mass (50:50% by mass pigment:aluminum flake) Pigment:binder mass ratio 1:5.7
[0149] Sample Preparation 10: 0.2% by weight pigment masstone in polyvinyl chloride (PVC) film Polyvinyl chloride (PVC) films with a thickness of ∼0.3 mm containing 0.2% by weight of pigment were produced by full shade coating on a twin roll mill at 150 °C.
[0150] PVC grade: SorVyl DB 2105 clear from Polymer-Chemie. Total grinding time in a twin roll mill type Collin 150 (Collin Lab & Pilot Solutions): approx. 10 min.
[0151] Reference example Determination method a)L * a * b * C * h Color tone determination As used herein, L * The term lightness is defined by the International Commission on Illumination (Commission Internationale de l'Eclairage). * a * b * It means the lightness in the color space (also called CIELAB), and a* and b * are the chromaticity coordinates. L * The value is measured at an observation angle of 25°. According to the CIELAB system, L * =100 means the brightest value (white), L * = 0 means the darkest value (black). In general, L * The value refers to an opaque coating.
[0152] In this specification, C * (Chromium) is the L defined by the International Commission on Illumination (Commission Internationale de l'Eclairag). * C * h color space (also called CIELAB), L * L * a * b * The lightness is the same as in the color space, and h is the hue angle.
[0153] Solid colors (CIELAB color measurements) were measured using a Datacolor 650 d8 integrating sphere spectrophotometer with a D65 illuminant and a 10° observer. Data processing with BASF ColorCare software.
[0154] Effect colors (CIELAB color measurements) were measured using a BYK-mac 6-angle spectrophotometer (-15°, 15°, 25°, 45°, 75°, 110°) with a D65 illuminant and a 10° observer. Data processing with BASF ColorCare software.
[0155] b) Near infrared (NIR) reflectance determination – Total Solar Reflectance (TSR) and specified near infrared (NIR) wavelengths (905nm and 1550nm) As used herein, the term TSR means total solar reflectance and is a measure of an object's surface reflectance in the wavelength range 300-2500 nm.
[0156] Near-infrared (NIR) reflectance of 905 nm and 1550 nm is considered representative of the near-infrared (NIR) wavelengths used in LiDAR-based autonomous driving applications.
[0157] TSR and the specified NIR wavelengths were measured using an Agilent Cary 5000 UV-Vis-NIR spectrophotometer. TSR was measured according to ASTM Standard Method E 903-96 using ASTM G159-98 direct solar spectral irradiance.
[0158] c) XRD X-ray diffraction was measured using a multiple sample changer operated in Bragg-Brentano geometry and equipped with a Lynx-Eye detector. A Bruker D8 Advance XDR 2 was used. Primary: Cu anode, divergence slit set at 0.1°, air scattering shield installed; Secondary: air scattering slit 8 mm, 0.5 mm Ni absorbing filter, 4° solar, Lynx-Eye detector set at 3° aperture angle. Samples were loaded into a sample holder and smoothed on a glass slide.
[0159] d) Masstone, reduced titanium dioxide and reduced aluminium test panels All basecoat samples were spray applied to unprimed Q-panel aluminum test panels using an automated HVLP spray gun (high volume low pressure, e.g. SATA LP90) mounted on an Intec lab spray robot. The basecoat layer was dried for 15 minutes at an effective metal temperature (EMT) of 80°C. The basecoat was applied to a layer thickness that provided opacity (typical dry film thickness: masstone 15-20 microns; 10:90 wt% pigment:TiO2 reduced 30-35 microns; 50:50 wt% pigment:Al reduced 15-20 microns). A typical one-part acrylic melamine-based clearcoat containing a combination of UV absorbers (e.g. Tinuvin® 400 (100% hydroxyphenyl triazine UV absorber) supplied by BASF SE) and hindered amine light stabilizers (HALS) (e.g. Tinuvin® 123 (100%) supplied by BASF SE) was then spray applied onto the dried basecoat layer. After being left at ambient temperature to evaporate the solvent, the panels were baked at 140°C EMT for 30 minutes. A clear coat was applied to a dry thickness of 35-40 microns.
[0160] These basecoat panels were used for color measurement and accelerated weathering testing.
[0161] e) Masstone Test Panels for UV-Vis-NIR Spectroscopy A 2.5 wt% masstone basecoat sample (Sample Preparation 6) was applied to Leneta Opacity Chart Form 2A using a 150 micron wire-wound applicator bar attached to a Zehntner ZAA2300 automatic film applicator. After leaving at ambient temperature to allow the solvent to evaporate, the panels were dried at 80°C for 30 minutes. A dry film thickness of 20-25 microns was applied. A typical one-part acrylic melamine-based clearcoat containing a combination of UV absorbers (e.g., Tinuvin® 400 (100% hydroxyphenyl triazine UV absorber) supplied by BASF SE) and hindered amine light stabilizers (HALS) (e.g., Tinuvin® 123 (100 wt%) supplied by BASF SE) was then applied over the dried basecoat layer using a 100 micron wire-wound applicator bar attached to a Zehntner ZAA2300 automatic film applicator. After being left at ambient temperature to evaporate the solvent, the panels were baked at 140°C EMT for 30 minutes. A clear coat was applied to a dry thickness of 35-40 microns.
[0162] These masstone panels were also used for colorimetry.
[0163] f) Masstone test panel for measuring black value A 2.5 wt% Maskstone basecoat sample (Sample Preparation 6) was spray applied to cleaned and alcohol-cleaned glass test panels using an automated HVLP spray gun (e.g., SATA LP90) mounted on an Intec lab spray robot. After being left at ambient temperature to allow the solvent to evaporate, the panels were baked at 140°C for 30 minutes. A dry film thickness of 15-20 microns was applied.
[0164] g) Black value color dependence M C Black value, color independent M Y The black value was determined according to DIN EN ISO 18314-3 using the following formula: - Black value (color independent) MY =100 * log(100 / Y) - Black value (color dependent) M C =100 * (log(X n / X)-log(Z n / Z)+log(Y n / Y)) Black value, M C indicates that a blue shade indicates a high black value and a brown shade indicates a low black value.
[0165] - Absolute contribution of hue ΔM=M C -M Y =100 * (log(X n / X)-Log(Z n / Z)) Black values were measured using a Datacolor DC45S 45 / 0 spectrophotometer with a D65 illuminant and a 10° observer. Data processing with BASF ColorCare software.
[0166] h) UV-Vis-NIR (near infrared reflectance) data UV-Vis-NIR (near infrared reflectance) data was obtained using a spectrophotometer that measures the reflectance / transmittance properties of a sample across the UV, visible, and NIR portions of the electromagnetic spectrum. UV-Vis-NIR data was measured using an Agilent Cary 5000.
[0167] i) Particle size Particle size was determined using transmission electron microscopy (TEM). A very small amount of sample powder is transferred from the tip of a microspatula onto a glass slide. To homogeneously disperse the pigment, it is wetted with 5 drops of ethanol and rubbed between another glass slide. A carbon-coated TEM grid (SF162) is immersed flat onto the coated slide. After a short drying in air, the samples were observed in a Zeiss Libra 120 transmission electron microscope, equipped with an Omega filter operated in elastic light field mode at 120 kV and at various magnifications in representative positions.
[0168] j) Color measurement of 0.2% pigment masstone in PVC film Standard colorimetric measurements at 0.2% pigment masstone (sample preparation 10) and full shade application are performed on white using the spectral method ISO 18314-1(2015) in d / 8°- or 8° / d geometry with a gloss trap. Test properties were measured on a white substrate with a D65 illuminant and a 10° standard observer according to ISO 11664-4(2008;18314-2(2015)).
[0169] Example 1 Preparation of solid solutions starting from compounds according to formula (I) and formula (II) and / or (III) Compound 1 was synthesized according to Justus Liebigs Annalen der Chemie, 1984, 483.
[0170] Compound 2 was synthesized according to Example 1 of US 4,450,273.
[0171] Compounds 3-6 were synthesized according to Example 1 of US2010 / 0184983A1.
[0172] Compounds 1 and 2 correspond to the compounds of formula (I) as defined in embodiment 1 or feature a) of claim 1.
[0173] Compounds 3 to 6 correspond to compounds of formula (II) according to the invention or to compounds of formula (III) or to mixtures of compounds of formula (II) and compounds of formula (III) as defined in embodiment 1 or feature b) of claim 1.
[0174] [Table 5]
[0175] Example 1.1: Solid solution containing compound 2 and compound 3 26.25 g of compound 2 and 8.74 g of compound 3 were added to a kneading apparatus (Z-blade kneader) of 1.0 liter capacity. 210 g of sodium chloride and 80 g of diethylene glycol (DEG) were added to the kneader and the rotation speed was set to 65 rpm. The walls of the apparatus were thermostated at 50° C. After 6 hours of kneading at 50° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 60° C. for 48 hours. The yield of the obtained solid solution was 31.70 g and contained 75% by weight of compound 2 and 25% by weight of compound 3. The obtained solid solution was ground in a mill to obtain a black powder.
[0176] Example 1.2: Solid solution containing compound 2 and compound 3 41.6 g of compound 2 and 10.4 g of compound 3 were added to a kneading apparatus (Z-blade kneader) of 1.1 liter capacity. 208 g of sodium chloride and 58 g of diacetone alcohol (DAA) were added to the kneader and the rotation speed was set to 100 rpm. The walls of the apparatus were thermostated at 60° C. After 8 hours of kneading at 60° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 48.9 g and contained 80% by weight of compound 2 and 20% by weight of compound 3. The solid solution was ground in a mill to obtain a black powder.
[0177] Example 1.3: Solid solution containing compound 2 and compound 3 A kneading apparatus (Z-blade kneader) of 1.1 liter capacity was charged with 37.4 g of compound 2, 37.4 g of compound 2, 9.4 g of compound 3, and 5.2 g of a partially hydrogenated rosin, such as Staybelite Resin E, supplied by Eastman Chemical Company. 208 g of sodium chloride and 58 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 60° C. After 8 hours of kneading at 60° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 48.9 g and contained 72% by weight of compound 2, 18% by weight of compound 3, and 10% by weight of Staybelite Resin E. This solid solution was pulverized in a mill to obtain a black powder.
[0178] Example 1.4: Solid solution containing compound 2 and compound 3 A kneading apparatus (Z-blade kneader) of 1.0 liter capacity was charged with 26.25 g of compound 2 and 8.74 g of compound 3. 210 g of sodium chloride and 80 g of diethylene glycol (DEG) were added to the kneader. The walls of the apparatus were thermostated at 50° C. After 16 hours of kneading at 50° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 60° C. for 48 hours. The yield of the obtained solid solution was 31.70 g and contained 75% by weight of compound 2 and 25% by weight of compound 3. The obtained solid solution was ground in a mill to obtain a black powder.
[0179] Example 1.5: Solid solution containing compound 2 and compound 4 A kneading apparatus (Z-blade kneader) of 1.1 liter capacity was charged with 20.8 g of compound 2 and 5.2 g of compound 4. 208 g of sodium chloride and 58 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 65° C. After 12 hours of kneading at 65° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 48.9 g and contained 80% by weight of compound 2 and 20% by weight of compound 4. The solid solution was ground in a mill to obtain a black powder.
[0180] Example 1.6: Solid solution containing compound 2 and compound 3 A mixture of 8 g of compound 2 and 2 g of compound 3 was milled with 40 g of sodium chloride and 0.4 g of lorol in a vibratory mill charged with 1.5 kg of steel balls (diameter: 2.5 cm) at 70 °C for 48 hours. After 48 hours at 70 °C, the milling was stopped and the mixture was removed from the mill. 1500 g of water was added to the mixture and stirred for 1 hour. The mixture was then filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80 °C for 24 hours. The yield of the resulting solid solution was 9.5 g and contained 80 wt% compound 2 and 20 wt% compound 3. The resulting solid solution was milled to obtain a black powder.
[0181] Example 1.7: Solid solution containing compound 2 and compound 3 A mixture of 80 g of compound 2 and 20 g of compound 3 was milled for 50 h at 50 °C in a 900 mL steel chamber charged with 1.5 kg of steel balls (diameter: 2.5 cm). After removing the steel balls, 40 g of the milled material was added to 400 g of 75% sulfuric acid in a 500 mL round-bottom flask and stirred at 350 rpm for 16 h at 70 °C. The mixture was subsequently precipitated in 1500 mL of water with stirring for 30 min. The resulting solid solution was filtered, dried and contained 80% compound 2 and 20% compound 3 by mass.
[0182] Example 1.8: Solid solution containing compound 2 and compound 3 A kneading apparatus (Z-blade kneader) with a capacity of 1.1 liters was charged with 22.2 g of compound 2 and 5.5 g of compound 3. 222 g of sodium chloride and 43 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 65° C. After 15 hours of kneading at 65° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 26.5 g and contained 80% by weight of compound 2 and 20% by weight of compound 3. The solid solution was ground in a mill to obtain a black powder.
[0183] Example 1.9: Solid solution containing compound 2 and compound 3 A kneading apparatus (Z-blade kneader) with a capacity of 1.1 liters was charged with 27.2 g of compound 2 and 6.8 g of compound 3. 215 g of sodium chloride, 1.79 g of IBMS (indanthrone blue sulfonic acid) and 58 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 60° C. After kneading for 20 hours at 60° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 35 g and contained 80% by weight of compound 2 and 20% by weight of compound 3. The solid solution was ground in a mill to obtain a black powder.
[0184] Example 1.10: Solid solution containing compound 2 and compound 3 A kneading apparatus (Z-blade kneader) with a capacity of 3.5 liters was charged with 102.9 g of compound 2, 25.7 g of compound 3, and 14.3 g of a partially hydrogenated rosin, such as Staybelite Resin E, supplied by Eastman Chemical Company. 857 g of sodium chloride and 193 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 90° C. After 12 hours of kneading at 90° C., the kneading was stopped. 10 L of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 127 g and contained 72% by weight of compound 2, 18% by weight of compound 3, and 10% by weight of Staybelite Resin E. The solid solution was ground in a mill to obtain a black powder.
[0185] Example 1.11: Solid solution containing compound 2 and compound 6 A kneading apparatus (Z-blade kneader) with a capacity of 1.1 liters was charged with 23.1 g of compound 2 and 5.8 g of compound 6. 231 g of sodium chloride and 56 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 65° C. After 12 hours of kneading at 65° C., the kneading was stopped. 1500 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 26.8 g and contained 80% by weight of compound 2 and 20% by weight of compound 6. The solid solution was ground in a mill to obtain a black powder.
[0186] Example 1.12: Solid solution containing compound 2 and compound 5 29.7 g of compound 2 and 7.4 g of compound 5 were charged into a kneading apparatus (Z-blade kneader) with a capacity of 1.1 liters. 223 g of sodium chloride and 55 g of diacetone alcohol (DAA) were added to the kneader. The walls of the apparatus were thermostated at 90° C. After 8 hours of kneading at 90° C., the kneading was stopped. 1600 g of water was added to the kneaded mass. The mixture was filtered and washed until the conductivity of the filtrate was less than 100 μS / cm. The wet press cake was dried in an oven at 80° C. for 24 hours. The yield of the resulting solid solution was 35.7 g and contained 80% by weight of compound 2 and 20% by weight of compound 5. The solid solution was ground in a mill to obtain a black powder.
[0187] Comparative Example Comparative Example 1 represents a single Compound 1 (Spectrasense™ Black S 0084, formally Paliogen® Black S 0084, supplied by BASF Colors and Effects). A comparative millbase containing only Compound 1 was prepared according to Sample Preparation 1. A comparative 2.5 wt. % pigment masstone containing only Compound 1 was prepared according to Sample Preparation 6. A comparative 10:90 (by weight) Compound 1:titanium dioxide reduced product was prepared according to Sample Preparation 8. A comparative 50:50 (by weight) Compound 1:aluminum reduced product was prepared according to Sample Preparation 9.
[0188] Comparative Example 2 represents a single Compound 2 (Spectrasense™ Black L 0086, formally Paliogen® Black L 0086, supplied by BASF Colors and Effects). A comparative millbase containing only Compound 2 was prepared according to Sample Preparation 1. A comparative 2.5 wt. % pigment masstone containing only Compound 2 was prepared according to Sample Preparation 6. A comparative 10:90 (wt. ratio) Compound 2:titanium dioxide reduced was prepared according to Sample Preparation 8. A comparative 50:50 (wt. ratio) Compound 2:aluminum reduced was prepared according to Sample Preparation 9.
[0189] Comparative Example 3 represents a single Compound 3 (Spectrasense™ Black K 0087, formally known as Lumogen® Black K 0087, supplied by BASF Colors and Effects). A comparative millbase containing only Compound 3 was prepared according to Sample Preparation 1. A comparative 2.5 wt. % pigment masstone containing only Compound 3 was prepared according to Sample Preparation 6. A comparative 10:90 (by weight) Compound 3:titanium dioxide reduced product was prepared according to Sample Preparation 8. A comparative 50:50 (by weight) Compound 3:aluminum reduced product was prepared according to Sample Preparation 9.
[0190] Comparative Example 4 corresponds to a physical mixture of 80% by weight of Compound 2 (Spectrasense™ Black L 0086, formally Paliogen® Black L 0086, supplied by BASF Colors and Effects) and 20% by weight of Compound 3 (Spectrasense™ Black K 0087, formally Lumogen® Black K 0087, supplied by BASF Colors and Effects), which do not form a solid solution. A comparative millbase containing a mixture of Compound 2 and Compound 3 was prepared according to Sample Preparation 1. A comparative 2.5% by weight pigment masstone containing a mixture of Compound 2 and Compound 3 was prepared according to Sample Preparation 6. A comparative 10:90 (by weight) mixture of Compound 2 and Compound 3: titanium dioxide reduced was prepared according to Sample Preparation 8. A comparative 50:50 (by weight) mixture of Compound 2 and Compound 3: aluminum reduced was prepared according to Sample Preparation 9.
[0191] Comparative Example 5 represents carbon black (Pigment Black 7). A comparative millbase containing only carbon black (Pigment Black 7) was prepared according to Sample Preparation 2. A comparative 2.5 wt. % pigment masstone containing only carbon black (Pigment Black 7) was prepared according to Sample Preparation 7.
[0192] [Table 6]
[0193] [Table 7]
[0194] From the above, by carefully considering the processing conditions and the composition of the ingredients used, it is possible to prepare solid solution pigments. The solid solution pigments of the present invention have highly desirable neutral black (masstone) color characteristics and M c It has been found to exhibit properties that are lower a compared to existing, available, single-component black perylene pigments. * value and b * Value and high M C It is characterized by a color-dependent black value.
[0195] [Table 8]
[0196] Thus, by careful consideration of the processing conditions and the composition of the components used, solid solution pigments can be prepared. The individual pigments are found to exhibit highly desirable neutral gray (reduced) color characteristics, which exhibit very low a values compared to existing, available, single-component black perylene pigments of the comparative example. * value and b * It is characterized by its value.
[0197] [Table 9]
[0198] Thus, by careful consideration of the processing conditions and the composition of the components used, solid solution pigments can be prepared. The individual pigments are found to exhibit highly desirable neutral gray (reduced) color characteristics, which are significantly lower than existing, available, single component perylene pigments. * value and b* It is characterized by its value.
[0199] Examples 1.2, 1.3, 1.4 and 1.7 (based on Compound 2 and Compound 3 in a ratio of 80:20) and Example 1.5 (based on Compound 2 and Compound 4 in a ratio of 80:20) prepared using appropriate processing methods show very neutral black / grey color characteristics from a single solid solution pigment.
[0200] The described solid solution pigments, when dispersed in a binder system for use in, for example, coatings, behave as single pigments that provide predictable, neutral color properties at all concentrations based on the mass content of the pigment in the formulation. Alternatively, pigment blends such as Comparative Example 4 can be used to obtain neutral black / gray color properties. However, the color-dependent black value M of Comparative Example 4 c It can be seen that the color properties of the solid solution pigments in Examples 1.1 to 1.4 are inferior (see Table 6). In addition, in Comparative Examples 1 to 4, since two (or more) pigments are required to achieve the required neutral color properties, the color properties obtained from the dispersed mixed pigments can vary greatly depending on the dispersion conditions used and the required shade level of the target color. When using a physical mixture of two (or more) pigments, in order to achieve the required color at full concentration, the ratio of the blended components generally needs to be adjusted to achieve the same neutral color.
[0201] [Table 10]
[0202] Coatings containing conventional carbon black (Pigment Black 7) absorb strongly at all wavelengths in the visible and NIR wavelength range (400-2500 nm). This can be observed in Comparative Example 5, where low NIR reflectance values are observed at 905 nm and 1550 nm.
[0203] Thus, by careful consideration of the processing conditions and composition of the components used, solid solution pigments can be prepared. Individual solid solution pigments of the present invention have been found to exhibit highly desirable NIR non-absorbing properties, as characterized by TSR values compared to existing, available, single component comparative black perylene pigments.
[0204] [Table 11]
[0205] Coatings containing conventional carbon black (Pigment Black 7) absorb strongly at all wavelengths in the visible and near infrared wavelength range (400-2500 nm), which can be observed in Comparative Example 5, where low TSR values are observed.
[0206] Thus, by careful consideration of the processing conditions and composition of the components used, solid solution pigments can be prepared. Each of the solid solution pigments of the present invention has been found to exhibit highly desirable NIR non-absorbing properties, as characterized by TSR values compared to comparative, existing, available, single-component black perylene pigments.
[0207] The total solar reflectance is more affected by visible light and short wavelength NIR radiation than by long wavelength NIR radiation, in other words, slight differences in the absorption behavior of the solid solutions of the present invention in the range of 700-1000 nm strongly affect the TSR value.
[0208] The higher the wavelength at which the solid solution pigment of the present invention becomes transparent (the reflectance against white increases), the lower the TSR value. In Example 1.2, the absorption band is slightly extended to the NIR to improve the color tone in the visible region, so that it starts to become transparent at about 780 nm. Thus, Example 1.2 is NIR non-absorbing over a region about 100 nm narrower than Comparative Example 1, and as a result, the TSR value is inferior, even though the color in the visible region is significantly better. Thus, the solid solution pigment of the present invention provides good color properties combined with good TSR performance, which makes the solid solution pigment of the present invention a good tool for controlling NIR absorption.
[0209] As can be seen from Tables 10 and 11, in all examples based on the solid solutions of the present invention, the NIR reflectance and TSR values are significantly improved compared to carbon black, as shown by Comparative Example 5.
[0210] [Table 12]
[0211] The solid solution pigments of the present invention are compared to existing, available, single-component black perylene pigments of Comparative Examples Comparative Examples 2 and 3, which show that the L * Value, a * value and b * It can be seen that the resulting pigment exhibits highly desirable neutral to bluish black (mastone) color characteristics characterized by a value. [Brief description of the drawings]
[0212] [Figure 1] 1 shows the XRD spectrum of Example 1.1. [Diagram 2] 1 shows the XRD spectrum of Example 1.2. [Diagram 3] 1 shows the XRD spectrum of Example 1.5. [Figure 4] 1 shows the XRD spectrum of Example 1.6. [Diagram 5] 1 shows the XRD spectrum of Example 1.7. [Figure 6] 1 shows an XRD spectrum of Comparative Example 1. [Figure 7] 1 shows an XRD spectrum of Comparative Example 2. [Figure 8] 1 shows an XRD spectrum of Comparative Example 3. [Figure 9] 1 shows an XRD spectrum of Comparative Example 4. [Figure 10] 1 shows an XRD spectrum of Comparative Example 5. [Figure 11] 1 shows a pigmented masstone basecoat (2.5% Example 1 pigment) prepared according to Sample Preparation 6. [Figure 12] 10:90% by weight of Pigment (Example 1): Titanium dioxide white reduced product prepared according to Sample Preparation 8. [Figure 13] Figure 13a shows a full angle zoom of a 50:50 wt% pigment (Example 1):aluminum reduction CIELAB panel prepared according to Sample Preparation 9. Figure 13b shows a full angle zoom of a 50:50 wt% pigment:aluminum reduction CIELAB panel prepared according to Sample Preparation 9. [Figure 14] Shows Vis-NIR reflectance. [Figure 15] 1 shows the XRD spectrum of Example 1.11. [Figure 16] 1 shows the XRD spectrum of Example 1.12.
[0213] List of cited prior art WO2018 / 081613 US7083675 EP0636666B1 WO91 / 02034A1 EP2316886A1 EP504922A1 US2012018687A1 CN110591445A Justus Liebigs Annalen der Chemie, 1984, 483 US4,450,273 US2010 / 0184983A1
Claims
1. (a) at least one compound represented by formula (I); 【Chemistry 1】 (b) at least one compound represented by formula (II), or at least one compound represented by formula (III), or a mixture of at least one compound represented by formula (II) and at least one compound represented by formula (III), A solid solution containing 【Chemistry 2】 (In the formula, - R 1 and R 2 are each independently -(CH 2 ) n -X (wherein X is a hydrogen atom, a methyl, 1 -C 5 Alkoxyl, hydroxyl, phenyl, C 1 -C 5 Alkylphenyl, C 1 -C 5 Alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C 1 -C 5 Alkylpyridyl, C 1 -C 5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; - R 3 and R 4 are each independently phenylene, C 1 -C 5 Alkylphenylene, C 1 -C 5 Alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C 1 -C 5 Alkylpyridinediyl, C 1 -C 5 Alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, R in formula (II) and (III) 3 The two nitrogen atoms bonded to R 3 R in formula (II) and (III) forms a 5- or 6-membered heterocyclic ring together with two atoms of the aromatic ring; 4 The two nitrogen atoms bonded to R 4 form a 5- or 6-membered heterocyclic ring together with two atoms of the aromatic ring; -X 1 From X 8 are each independently a hydrogen atom, C 1 -C 5 Alkyl, C 1 -C 5 alkoxy, hydroxy, phenyl or halide).
2. X is methoxyphenyl or phenyl and n is 1 or 2; - R 3 and R 4 are each independently phenylene, methyl-phenylene, methoxy-phenylene, chloro-phenylene, dichloro-phenylene or naphthalenediyl; -X 1 From X 8 is a hydrogen atom, The solid solution of claim 1.
3. - R 1 and R 2 are each independently -CH 2 C 6 H 4 OCH 3 or -CH 2 CH 2 C 6 H 5 and - R 3 and R 4 are each independently phenylene, 4-chloro-phenylene, naphthalenediyl or 4,5-dichloro-phenylene; -X 1 From X 8 is a hydrogen atom, 3. The solid solution according to claim 1 or 2.
4. X is 4-methoxyphenyl and n is 1; - R 3 and R 4 is phenylene; -X 1 From X 8 is a hydrogen atom; and / or X is 4-methoxyphenyl and n is 1; - R 3 and R 4 is naphthalenediyl; -X 1 From X 8 is a hydrogen atom; and / or X is 4-methoxyphenyl and n is 1; - R 3 and R 4 is 4-chloro-phenylene; -X 1 From X 8 is a hydrogen atom; and / or X is 4-methoxyphenyl and n is 1; - R 3 and R 4 is 4,5-dichloro-phenylene; -X 1 From X 8 is a hydrogen atom; and / or - X is phenyl and n is 2; - R 3 and R 4 is phenylene; -X 1 From X 8 is a hydrogen atom; and / or - X is phenyl and n is 2; - R 3 and R 4 is naphthalenediyl; -X 1 From X 8 is a hydrogen atom; and / or - X is phenyl and n is 2; - R 3 and R 4 is 4-chloro-phenylene; -X 1 From X 8 is a hydrogen atom, The solid solution according to any one of claims 1 to 3.
5. A color-independent black value M in the range of 200 to 350, preferably in the range of 220 to 330, more preferably in the range of 230 to 300, more preferably in the range of 242 to 280. Y and a color-dependent black value M in the range of 200 to 350, preferably in the range of 220 to 330, more preferably in the range of 230 to 300, more preferably in the range of 242 to 280. C indicates M Y and M. C The solid solution according to any one of claims 1 to 4, wherein is determined according to DIN EN ISO 18314-3.
6. 6. The solid solution according to claim 1, wherein the mass ratio of at least one compound of formula (I) to at least one compound of formula (II), or at least one compound of formula (III), or a mixture of at least one compound of formula (II) and at least one compound of formula (III) [mass (I):mass ((II)(III))] is in the range of 60:40 to 99:1, preferably in the range of 65:35 to 95:5, more preferably in the range of 70:30 to 90:10, for example in the range of 70:30 to 80:20, or in the range of 75:25 to 85:15, or in the range of 80:20 to 90:
10.
7. 80 to 100% by weight, preferably 85 to 100% by weight, more preferably 90 to 100% by weight, more preferably 95 to 100% by weight, more preferably 99 to 100% by weight, more preferably 99.5 to 100% by weight of said solid solution, (a) at least one compound represented by formula (I), and (b) at least one compound represented by formula (II), or at least one compound represented by formula (III), or a mixture of at least one compound represented by formula (II) and at least one compound represented by formula (III), The solid solution according to any one of claims 1 to 6, consisting of:
8. A method for producing a solid solution, comprising the steps of: (i) (a) at least one compound represented by formula (I); 【Chemistry 3】 (b) at least one compound represented by formula (II), or at least one compound represented by formula (III), or a mixture of at least one compound represented by formula (II) and at least one compound represented by formula (III), providing a mixture comprising: 【Chemistry 4】 (In the formula, - R 1 and R 2 are each independently -(CH 2 ) n -X (wherein X is a hydrogen atom, a methyl, 1 -C 5 Alkoxyl, hydroxyl, phenyl, C 1 -C 5 Alkylphenyl, C 1 -C 5 Alkoxyphenyl, hydroxyphenyl, halogenated phenyl, pyridyl, C 1 -C 5 Alkylpyridyl, C 1 -C 5 alkoxypyridyl, halogenated pyridyl, pyridylvinyl or naphthyl; n is 0, 1, 2, 3, 4 or 5; - R 3 and R 4 are each independently phenylene, C 1 -C 5 Alkylphenylene, C 1 -C 5 Alkoxyphenylene, hydroxyphenylene, halogenated phenylene, pyridinediyl, C 1 -C 5 Alkylpyridinediyl, C 1 -C 5 Alkoxypyridinediyl, halogenated pyridinediyl, anthraquinonediyl or naphthalenediyl, R in formula (II) and (III) 3 The two nitrogen atoms bonded to R 3 R in formula (II) and (III) forms a 5- or 6-membered heterocyclic ring together with two atoms of the aromatic ring; 4 The two nitrogen atoms bonded to R 4 form a 5- or 6-membered heterocyclic ring together with two atoms of the aromatic ring; -X 1 From X 8 are each independently a hydrogen atom, C 1 -C 5 Alkyl, C 1 -C 5 alkoxy, hydroxy, phenyl or halide): (ii) subjecting the mixture provided in (i) to a mechanical treatment; (iii) adding water to the mixture resulting from (ii); (iv) subjecting the mixture obtained from (iii) to solid-liquid separation; (v) washing the solid obtained from (iv) with at least one suitable washing agent; (vi) drying the solid obtained from (v) to obtain a solid solution; A method comprising:
9. 9. The method of claim 8, wherein the mechanical treatment in (ii) comprises one or more of kneading and grinding, wherein kneading comprises co-extrusion, salt kneading, single screw kneading and twin screw kneading, and grinding comprises wet milling, ball milling, bead milling, vibratory milling, planetary milling and attritor milling.
10. the mechanical treatment in (ii) comprises, preferably is, kneading, said kneading being carried out at a temperature of the mixture in the range of from 40 to 120° C., preferably in the range of from 45 to 90° C., more preferably in the range of from 50 to 90° C., The method preferably further comprises adding, either immediately prior to and / or during kneading, one or more suitable solvents and / or one or more of sodium chloride, sodium sulfate and anhydrous aluminum sulfate, preferably sodium chloride, to the mixture to be kneaded, more preferably the mass ratio of the one or more of sodium chloride, sodium sulfate and anhydrous aluminum sulfate to the mixture provided in (i) is in the range of 20:1 to 1:1, preferably 15:1 to 2:1, more preferably 10:1 to 2:1, more preferably 8:1 to 2:1, more preferably 6:1 to 2:1, more preferably 4:1 to 2:1, and the at least one solvent is preferably ethylene glycol.
10. The method of claim 9, wherein the at least one solvent comprises (and more preferably is) one or more of: diethylene glycol, diacetone alcohol, dimethylformamide, glycerin, triethylene glycol, dipropylene glycol, ethylene glycol monobutyl ether, methyl ethyl ketone, cyclohexanone, dimethylacetamide, N-methylpyrrolidone, butyl acetate, glycerol triacetate, sulfolane, xylene, tetrahydrofuran, butanol, water and dimethyl sulfoxide.
11. 11. The method according to claim 9 or 10, wherein the mechanical treatment in (ii) further comprises adding, either immediately before and / or during kneading, at least one or more of synergists comprising sulfonic and carboxylic acid derivatives of perylene, indanthrone, phthalocyanine and diketopyrrolopyrrole, preferably in an amount of 1 to 15% by weight, more preferably 1 to 5% by weight, based on the total weight of the kneaded mixture.
12. 10. The method according to claim 9, wherein the mechanical treatment in (ii) comprises, preferably is, grinding, the grinding being carried out at a temperature of the mixture in the range of from 40 to 120°C, preferably in the range of from 45 to 90°C, more preferably in the range of from 50 to 90°C, and the method preferably further comprises adding, either immediately prior to and / or during grinding, one or more of sodium chloride, sodium sulphate and anhydrous aluminium sulphate, preferably sodium chloride, to the mixture to be ground.
13. 13. The method of claim 12, further comprising adding at least one suitable acid or solvent to the ground mixture under stirring immediately after grinding, at a temperature of the mixture in the range of from 40 to 200°C, preferably in the range of from 45 to 150°C, more preferably in the range of from 50 to 120°C, wherein the at least one suitable acid is preferably one or more of polyphosphoric acid and sulfuric acid, more preferably the at least one suitable acid comprises sulfuric acid, more preferably is sulfuric acid, and the at least one solvent is preferably one or more of ethylene glycol, diethylene glycol, diacetone alcohol, dimethylformamide, glycerin, triethylene glycol, dipropylene glycol, ethylene glycol monobutyl ether, methyl ethyl ketone, cyclohexanone, dimethylacetamide, N-methylpyrrolidone, butyl acetate, glycerol triacetate, sulfolane, xylene, tetrahydrofuran, butanol, water and dimethyl sulfoxide, more preferably the at least one solvent comprises (and more preferably is) diethylene glycol, diacetone alcohol, dimethylformamide, xylene, butanol, water and glycerin.
14. A solid solution according to any one of claims 1 to 7, preferably obtainable or obtained by a method according to any one of claims 8 to 13.
15. 15. Use of the solid solution of any one of claims 1 to 7 or 14 as one or more components of a coating composition, a light detection and ranging (LiDAR) device, a near infrared (NIR) non-absorbing component, a photovoltaic component, a thermal management component, a thermal insulation component, a pigmented coating, a printing ink, a recyclable plastic product, a biodegradable mulch, a toner, a charge generating material, a color filter, an LC display, and a security printing component.
16. 15. Use of the solid solution of any one of claims 1 to 7 or 14 as a near infrared (NIR) transparent colorant capable of replacing a near infrared (NIR) absorbing black pigment in a coating or object to increase the signal to noise ratio in near infrared (NIR) radiation detection.
17. - a primer coating comprising a solid solution according to any one of claims 1 to 7 or 14 and a white or reflective pigment having a reflectance of more than 50% in the range from 700 to 2500 nm in a mass ratio of 1:99 to 99:1, preferably 1:95 to 95:1; - a base coat comprising a black, preferably a solid solution, a coloured pigment, a metallic pigment or an interference pigment as claimed in any one of claims 1 to 7 or 14; and - optional clear topcoat, A multi-layer coating including
18. 15. The solid solution according to any one of claims 1 to 7 or 14, present in one or more of thermoplastic, elastomeric, crosslinked or essentially crosslinked polymers, preferably one or more of polyolefins, polyamides, polyurethanes, polyacrylates, polyacrylamides, polyvinyl alcohols, polycarbonates, polystyrenes, polyesters, polyacetals, natural or synthetic rubbers and vinyl halide polymers in an amount of 0.01% to 70% by weight based on the total weight of the polymer.