Apparatus and method for producing concrete, particularly high early strength concrete
Patent Information
- Application Number
- JP2023533594
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-04-09
- Filing Date
- 2021-11-30
- Publication Date
- 2024-11-29
AI Technical Summary
Existing concrete production methods face challenges in achieving high initial strength while maintaining uniform suspension quality and avoiding increased production costs, with issues arising from low water-to-cement ratios, abrasive mixing, and inefficient two-stage mixing processes.
A device comprising a cement premixer with ultrasound and multiple crystallization tanks allows for the activation and crystallization of cement suspension at an optimal water-to-cement ratio, followed by storage and mixing with aggregates, optimizing the water content and reducing the need to premix the entire cement amount.
This approach enhances initial concrete strength significantly, reduces equipment wear, and maintains process efficiency by using ultrasound to activate a fraction of cement, ensuring sufficient water for mixing and minimizing energy consumption.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus for producing concrete, in particular high early strength concrete, and to a method for producing a corresponding concrete. [Background technology]
[0002] An important parameter of concrete composition is its early strength. Options for increasing the early strength of concrete include established processes such as heat treatment, the use of accelerated concrete admixtures, or the use of concrete engineering techniques such as increasing the cement content or lowering the w / c ratio (water to cement ratio) beyond that required for the structure. However, these modifications are often compromised by a time factor with a significant increase in production costs. In addition, although early strength is improved, the change in composition may result in undesirable changes in the overall material properties (e.g., shrinkage cracking).
[0003] DE 3716438 A1 describes an apparatus with a cement premixer, a concrete mixer and a tank arranged between them, in which cement and water are mixed to form a cement paste, which is temporarily stored and then mixed with aggregates for concrete production in the usual way.
[0004] When mixing cement paste, only at (very) high w / c ratios does the obstacle arise that there is enough free water to mix the cement and water correctly. Most of the water is often bound as surface water on the aggregates in the concrete mixer, reducing the amount of water available for the premix. At medium to low w / c ratios (<0.50), cement paste can only be produced using superplasticizers.
[0005] Furthermore, complete dispersion of the cement in water requires high mixing speeds, which are taken into account in E01DE3716438A1 by dependent claims 3 and 4. These high speed mixing tools wear out quickly due to the highly abrasive effect of the cement and are very prone to clogging (especially at low water contents).
[0006] The biggest challenge in this process comes from providing a uniform suspension quality throughout the entire production day. The aforementioned literature does not provide any answers. However, it must be assumed here that the suspension is stored in tanks (storage silos), which are emptied and refilled for the mixing of the concrete, thereby having to wait again the pre-storage time. Economic operation of the mixing plant is therefore not possible. When large tanks are filled and gradually emptied, the suspension contained in them ages over time, causing the resulting concrete properties to change significantly. Eventually, the cement suspension in the tanks solidifies and further processing is not possible.
[0007] Furthermore, a two-stage mixing process is known which improves the early strength. The application of the two-stage mixing process is described, inter alia, in DE 1584305 A or DE 102016003644 B4, where the workability and early strength of concrete are improved by a two-stage mixing process: 1) intensive premixing of the binder components with or without sand and 2) final mixing in a concrete mixer.
[0008] Ultrasonic premixing is also known, as described in more detail in DE 10 2007 027 080 A1, especially in DE 10 2019 120 939 A1.
[0009] In this connection, all two-stage concrete mixing processes suffer from the obstacle of the need to supply a certain amount of (mixing) water for the production of the suspension. The water content of concrete depends on the aggregate water demand (Gk), the w / c ratio and the cement content. However, since the added aggregates, especially the sand, are never completely dry (for example, the aggregates are spread during the filling of underground storage facilities to keep dust generation low), the moisture adhering to the aggregates needs to be subtracted from the mixing water. This is done by measuring the moisture either during the weighing or transportation process or in the concrete mixer. If the moisture content of the aggregates is medium to high (approximately 3-8% by weight), this moisture needs to be subtracted from the mixing water accordingly. For illustration, an example calculation of precast concrete with a w / c ratio of 0.46 in the running production of a precast concrete plant is shown below.
[0010] [Table 1]
[0011] After deducting the moisture content of the aggregate, the water available for preparation of the suspension is 106 kg / m 3 , i.e. about 2 / 3 of the initial amount. For the preparation of the suspension, a w / c ratio of 0.30 needs to be selected. To mix correctly with such a low w / c ratio, a high dose of superplasticizer is required, which may increase the concrete slump beyond the required level and further retard the hardening reaction of the cement.
[0012] Illustrative Example 2: For example, if a w / c ratio of 0.35 is applied in the manufacturing process of a prestressed concrete element, the calculation results are: [Table 2]
[0013] The water available for making the suspension in the premix process is 67 kg / m 3, resulting in a suspension w / c ratio of 0.19, which is no longer possible to accurately premix and weigh based on currently available technology.
[0014] Known methods try to solve this problem, for example by pretreating the fine fraction of the aggregate (usually sand) which has the highest moisture content in a premixer (DE1584305A or DE102016003644B4). This is evident, however, because more water is then available for the suspension mixing process. However, with this method it can be expected that the well-known problems of increased wear of the stirring elements by the abrasive sand and of "overmixing" will occur. In the case of overmixing, small fractions of sand particles are broken apart by the fast rotating stirring tool, i.e. the sand is crushed, which increases the water demand and worsens the workability.
[0015] Therefore, the challenges for the application of the two-stage mixing process can be summarized as follows: a low w / c ratio ensures high early compressive strength and a short mixing time ensures a fast concreting process, especially for large amounts of components filled in several steps; partially high inherent moisture reduces the water available for the suspension mixing process.
[0016] In extreme cases, for example in humid climates, not enough water is available for the suspension mixing process. Currently, this can only be compensated for by increasing the concentration of superplasticizers, but this increases the fluidity of the concrete beyond the required level, potentially retarding hardening and increasing the cost of the concrete. Summary of the Invention
[0017] Based on this preliminary consideration, it is an object of the present invention to provide an apparatus and a method for the production of concrete having high early strength whilst avoiding the above mentioned problems.
[0018] The present invention solves this object by means of a device having the features of claim 1 and a method for producing concrete having the features of claim 18.
[0019] The device for producing concrete according to the invention comprises: i) a cement premixer for mixing a cement suspension; ii) at least one first crystallization tank for increasing the early strength of the concrete; and iii) a concrete mixer for producing a concrete mixture from said premixed cement suspension, in particular with the addition of aggregates; Equipped with.
[0020] In particular, the device according to the invention comprises one or more crystallization tanks, which allow the crystallization of the individual components contained in the cement before it is added to the concrete. A plurality of crystallization tanks can form a crystallization tank train within the scope of the invention. In this case, the crystallization tanks are preferably arranged one above the other in the crystallization tank train, such that the cement suspension can be transferred by gravity from the upper crystallization tank to the crystallization tank arranged below.
[0021] The device is based on the finding that there is a preferred water-to-cement ratio (w / c) in the premix that activates the reaction between cement and water, especially when ultrasound is used. This w / c ratio depends on the type of cement and is preferably in the range of 0.50 to 2.0. Lower w / c ratios result in stronger particle interactions due to the higher solids content, which promotes strong heating of the suspension, which may have negative effects under certain circumstances.
[0022] Pre-treatment of cement suspensions, especially with ultrasound, produces metastable crystallization nuclei which are given additional time to grow by storage in a crystallization tank and are then metered into the concrete mixer as stable crystallization nuclei.
[0023] The crystallization tank preferably contains an agitator equipped with a stirrer that keeps the cement suspension moving at a slow speed during the crystallization period.
[0024] The preferred stirring speed is less than 50 rpm, preferably 2 to 25 rpm, and more preferably 5 to 20 rpm.
[0025] Due to the early crystallization of the cement components, the concrete subsequently produced achieves significantly higher early strength concrete than would be achieved without the use of a crystallization tank.
[0026] Also, it is not necessary to use all the cement used in the concrete for this type of pretreatment, instead it is sufficient to activate a portion, which in turn promotes the crystallization of the remaining cement that is fed directly to the concrete mixer. Thus, the dimensions and energy budget for operating the cement premixer and the crystallization tank can be optimized.
[0027] According to the invention, the cement premixer comprises at least one ultrasonic generator, in particular an ultrasonic probe, for providing a cement suspension.
[0028] Unlike DE 3716438 A1, in the present invention the decomposition is not produced by a high speed mixing tool but by the use of ultrasound.
[0029] At the same time, the fact that only a small portion (e.g. 20%) of cement with a high water content (w / c >>1.0) is premixed means at the same time less attenuation of ultrasound and less heating of the concrete due to the smaller proportion of suspension in the total concrete.
[0030] A higher water content is also advantageous for loading and cleaning of the equipment, especially during the process of operation of the equipment and the subsequent cleaning process.
[0031] Further advantageous designs of the device according to the invention are the subject matter of the dependent claims.
[0032] An ideal ultrasonically assisted cement premixer is known from DE 10 2019120939 A1, to which reference is made in full with regard to the structural design of preferred cement premixers within the scope of the present invention.
[0033] Such a cement premixer not only achieves a pure mixture of cement and water, but also achieves activation of the cement components and the cement suspension, which in turn accelerates crystallization. The cement premixer also preferably has an agitator that moves the cement suspension at a higher agitation speed than the agitator in the first crystallization tank.
[0034] Premixing at the aforementioned parameters and / or stirring speeds typically leads to the formation of air bubbles in the cement suspension, which can have a detrimental effect on the final strength of the concrete. These air bubbles are expelled during the continuous gentle mixing of the cement suspension in the crystallization tank. Therefore, the combination of a crystallization tank with an ultrasonic cement premixer is particularly preferred.
[0035] Another preferred aspect of the use of the crystallization tank is that, due to its design, the ultrasonic cement premixer can only deliver small amounts of cement suspension within a time interval, since for larger amounts of cement suspension, ultrasound has a limited penetration depth. In this case, the crystallization tank can also be used for the storage of the cement suspension.
[0036] Preferably, for low energy and trouble-free operation, the cement premixer, the crystallization tank and the concrete mixer are positioned relative to the earth's gravitational field so that the cement suspension can flow by gravity from the cement premixer into the crystallization tank and from there into the concrete mixer. If this is not possible, a pump can be used to deliver the suspension into the concrete mixer.
[0037] The connections between the respective tanks and the mixer may be flange connections each equipped with a closure device, for example a flat slide valve.
[0038] Each of the first and further crystallization tanks may comprise an agitation tool and in particular a drive for operating the agitation tool.
[0039] Each of the first and subsequent crystallization tanks may have side walls and a bottom surface, preferably a curved bottom surface. The side walls may extend parallel to the longitudinal axis of the crystallization tank. The agitator may have an agitator extension that is rotatable as an agitator. Preferably, these formations may be helical formations. The formations may be designed such that they can be guided over at least 50% of the bottom surface at a distance of less than 10 cm, preferably less than 5 cm, in particular 0.5 to 4 cm. This allows the movement and preferably re-suspension of a large volume of cement suspension with the settled components.
[0040] The formation, especially in the design as a helical formation, may have an edge wiper in the direction of the bottom. The formation may preferably be made of metal, while the edge wiper is preferably made of a softer material than the formation. Preferably, the edge wiper may be in the form of a rubber and / or PTFE lip.
[0041] Between the first crystallization tank and the concrete mixer, the apparatus can have a second, third, fourth, fifth and further crystallization tanks, preferably equipped with separate agitators. In this way, an increase in the volume of storable cement suspension for crystallization can be achieved. The second tank is particularly advantageous when large volumes are required, since it can be used to meter the activated (premixer) and upstream (crystallization tank I) suspension to the concrete mixer. This ensures that the suspension does not leave the crystallization tank without sufficient pre-storage time.
[0042] Furthermore, the device can be designed as a pressureless operating system. An open or pressureless operating system means that the pressure conditions in each vessel, i.e. the mixer and / or the crystallization tank, are the same or, in case of pressure differences in the transfer of the cement suspension, pressure compensation is performed via an open valve.
[0043] Along the connection between at least the first and / or second crystallization tank and the concrete mixer, an adjustment member is arranged for discharging and / or partially discharging the respective crystallization tank into the concrete mixer, which adjustment member can preferably be designed as a valve, in particular a pinch valve.
[0044] Likewise, corresponding adjustment elements, for example valves, in particular pinch valves, may also be arranged between the cement premixer and the first crystallization tank and / or between the crystallization tanks.
[0045] Furthermore, the device may also have an arrangement for detecting a measurement variable for controlling the emergency drainage of each of the first and / or further crystallization tanks. Such an arrangement may for example be a sensor for detecting the torque of a rotatable agitator and / or, in case of a rotating crystallization tank, a sensor for detecting the torque of a rotatable drum of the crystallization tank. This measurement makes it possible to indirectly determine the hardening state of the cement suspension.
[0046] Other measured variables such as viscosity, density, associated changes in the speed of sound of the reflected ultrasonic signal, and / or temperature of the cement suspension may also be used to monitor the emergency drainage.
[0047] The device may also have a feeding device, in particular a metering device, for feeding the superplasticizer, in particular as a function of the detected measured variable, so that the composition of the cement suspension can be readjusted when a set value is exceeded.
[0048] The apparatus, in particular at least one of the crystallization tanks, can also advantageously have a sensor for determining the temperature of the cement suspension. Ideally, the temperature should be between 25 and 45°C. The corresponding setpoints of the residence time of the cement suspension during the automatic drainage and / or partial drainage of the crystallization tanks can be adjusted depending on the determined temperature.
[0049] Preferably, the first and / or second or any further crystallization tanks can be designed for a volume of cement suspension of at least 2 cubic meters, preferably 0.5-4 cubic meters. Such volumes are not typical for cement premixers, especially ultrasonic cement premixers, because the ultrasonic input, especially in case of intensive ultrasound, cannot be made sufficiently homogenous over the whole volume of the mixer in case of larger volumes.
[0050] Intensive ultrasonic treatment allows the activation of the cement components. In contrast to ultrasonic, vibration or other methods of ultrasonically initiated vibration mixing, the ultrasonic treatment in a preferred variant of the method has the following characteristic data, individually or in combination with each other, which characterize the type of ultrasonic treatment in more detail: In particular, the ultrasonic probe is designed as a sonotrode and preferably operates within the scope of the method in the following ranges (values refer to T=25° C. and normal pressure):
[0051] Ultrasonic wave intensity emitted by the ultrasonic probe: 25~250W / cm 2 . When ultrasound waves are introduced into a medium, the particles and the medium vibrate. This vibration transfers the kinetic energy of the ultrasound. Intensity (I) corresponds to the power transferred per area, e.g., in watts. The units are power per area (e.g., W / cm2). 2 ).
[0052] Amplitude of ultrasound emitted by the ultrasonic probe: 15 to 500 μm, preferably 15 to 120 μm. The amplitude (u) represents the ultrasonic deflection (e.g. μm). At a constant frequency, a higher amplitude results in a higher intensity. The higher the amplitude, the greater the pressure difference between the high and low pressure cycles.
[0053] · Frequency of ultrasound emitted by the ultrasonic probe: preferably 10-30kHz. Frequency (f) represents the vibration velocity at the tip of the ultrasonic probe. Since the formation, growth, and implosion of vapor bubbles are time-dependent processes, higher frequencies result in smaller cavitation bubbles.
[0054] ·Specific energy input (to medium-water): preferably 25-250Ws / ml. The above mentioned values can be determined electroacoustically in water, for example, using a hydrophone.
[0055] To meter the cement into the premixer, a changeover valve can be installed after the cement metering device so that the cement is metered not only into the premixer, but also into the concrete mixer. However, a separate metering screw can also lead to the premixer.
[0056] It has proven to be favorable in terms of energy and / or technology if only a portion of the cement required for the production of concrete is mixed and precrystallized as a cement suspension, while the remaining portion is mixed directly, for example together with the aggregates, in a concrete mixer. This is particularly advantageous in the context of the method according to the invention, in contrast to the prior art.
[0057] To achieve improved early strength, it is not necessary to pretreat the entire amount of cement, which makes more water available for the premix process (a higher w / c ratio of the suspension can be chosen), saves energy and advantageously reduces the dimensions of the required machinery.
[0058] Furthermore, according to the invention there is provided a method for producing concrete, in particular using an apparatus according to the invention, comprising the following steps: i) preparing a cement suspension in a cement premixer; ii) stirring the cement suspension in a crystallization tank for a predetermined residence time; and iii) transferring the cement suspension after a predetermined residence time to a concrete mixer.
[0059] The most important measure for improving early strength is the residence time, which corresponds to the residence time or crystallization time of the premix suspension in the crystallization tank. The residence time depends on the concrete manufacturing process (mixing time, amount of concrete per hour, concrete composition) and the desired strength increase.
[0060] Crystallization tank (or storage / holding / retention tank) is a vessel where the suspension is stored under continuous agitation / circulation for a predetermined period of time (0.5-6 hours). After the residence time, the suspension is dumped into a concrete mixer. Residence time or residence time corresponds to the time that the activated suspension remains in the crystallization tank under continuous agitation or circulation.
[0061] Advantageously, the first crystallization tank has an outlet opening into the inlet of the concrete mixer or into the second (or third, fourth, ...) crystallization tank. The device further comprises an adjusting member arranged at the outlet of the first crystallization tank and / or at the inlet of the concrete mixer. The device may also comprise a first evaluation and / or control unit, which is equipped to operate the adjusting member for partial or complete emptying of the first crystallization tank after a residence time of 0.5-6 hours of the cement suspension in the first crystallization tank.
[0062] Further, the cement premixer may comprise a treatment vessel having a treatment chamber, wherein at least one ultrasonic probe extends at least partially into the treatment chamber, the ultrasonic probe emitting ultrasonic waves, the emitted ultrasonic waves or ultrasonic signals being measured, for example, by an evaluation and / or control unit, at a power of 25-250 W / cm. 2 and an amplitude of 15 to 500 μm.
[0063] In addition, during the production of concrete, a first portion of cement can be added to the cement premixer and a second portion of cement can be added to the concrete mixer, which is particularly advantageous in terms of energy.
[0064] The proportion of cement thus pretreated is preferably 5 to 95%, preferably 10 to 25%, of the total cement content.
[0065] Control or setting of the preferred residence time set point of the cement suspension in the crystallization tank can be performed as a function of a given time at a given temperature, which provides better control over the quality of the cement suspension since crystallization is temperature dependent.
[0066] For better and more comprehensive transfer, the transfer of the cement suspension to the concrete mixer can be carried out in batches.
[0067] The stirring speed of the first and further crystallization tanks, respectively, and / or the inflow and / or outflow of the cement suspension into the first or further crystallization tanks, respectively, can be controlled by a sensor and / or a sensor array. For this purpose, one or more temperature sensors, ultrasonic sensors for determining the ultrasonic transit time, and / or sensors for torque detection can preferably be used to monitor the quality of the cement suspension, in particular its concentration.
[0068] By temperature regulation, the temperature of the cement suspension in the first or further crystallization tank can be adjusted to a temperature between 10 and 45° C., and below 20° C., in particular between 10 and 20° C., allowing a more suitable storage.
[0069] The crystallization time or residence time as well as the emergency drainage time can be set depending on the temperature and / or the above mentioned measured variables.
[0070] The cement suspension can be charged into the concrete mixer, preferably only after a residence time of 1-8 hours. The transfer of the cement suspension into the concrete mixer is carried out according to a given protocol.
[0071] The water / cement ratio (w / c) of the cement suspension may advantageously be between 0.5 and 2. The residence time is selected depending on the reaction rate of the cement. The times indicated above are optimal for the residence time specifications mentioned above.
[0072] The pre-storage time of the cement suspension before transfer to the concrete mixer can be advantageously in practice between 1 and 8 hours.
[0073] Particularly preferably, the aforementioned w / c ratios as well as the resting period can be combined with an ultrasonic treatment of the cement suspension as described above.
[0074] The proportion of ultrasonically pretreated cement in the concrete may advantageously be between 5 and 95% by weight, ideally between 10 and 25% by weight.
[0075] The stirring speed in the first and / or second crystallization tank and / or the inflow and / or outflow of the cement suspension into the first and / or second crystallization tank can be controlled by a sensor and / or a sensor array. For this purpose, one or more temperature sensors, ultrasonic sensors for determining the ultrasonic transit time and / or sensors for torque detection can be preferably used to monitor the quality of the cement suspension, in particular its concentration.
[0076] Another advantage within the scope of the method is the provision of an intelligent control method and / or device for maintaining a defined suspension quality: a series of sensors in the tank permanently analyzes the suspension properties (in particular temperature, viscosity, density, conductivity, ultrasonic transit time), evaluates them and, based on the sensor measurement data, initiates measures such as adding new suspension and draining old suspension.
[0077] The temperature in the tank is a particularly important factor affecting the quality (=reactivity) of the suspension, which can be advantageously maintained permanently in the desired range by cooling and heating devices, for example by forming a double-walled tank wall as part of the first and / or second crystallization tank, or by a heat exchanger on or inside the crystallization tank.
[0078] In particular, a sensory detection of material-dependent physical measurement variables of the cement suspension located in the first and / or second crystallization tank can be performed.
[0079] Preferably, the inflow and / or outflow rates, the agitation speed and / or the temperature may be controlled based on measurements determined by sensory detection.
[0080] In the following, the concrete manufacturing device according to the invention is explained in more detail on the basis of exemplary embodiments with the aid of the attached drawings, which also contain some features which, when considered individually, can be combined in an obvious way with other exemplary embodiments not shown, the overall exemplary embodiment should not be understood as limiting the scope of protection of the invention in any way. [Brief description of the drawings]
[0081] [Figure 1] FIG. 1 shows a side view of an exemplary embodiment of the apparatus according to the present invention, comprising a cement premixer and first and second crystallization tanks. [Diagram 2] FIG. 2 illustrates a perspective view of the exemplary embodiment of FIG. [Diagram 3] FIG. 3 shows a cross-sectional view along the longitudinal axis of the crystallization tank. [Figure 4] FIG. 4 shows a schematic diagram of conventional concrete production. [Diagram 5] FIG. 5 shows a schematic diagram of concrete production according to one embodiment of the present invention. [Figure 6] FIG. 6 shows a graph of the amount of heat dissipation. [Figure 7] FIG. 7 is a diagram showing the composition of the first concrete mixture. [Figure 8] FIG. 8 is a diagram showing the composition of the second concrete mixture. [Figure 9] FIG. 9 shows the mixing ratio of cement suspension and water. [Figure 10] FIG. 10 is a graph showing the correlation between the onset of clotting and pre-storage time. [Figure 11] FIG. 11 shows the relationship between the pre-storage time of ultrasonically treated cement mortar and the slump flow and slump spread. [Figure 12] FIG. 12 shows the relationship between concrete age and compressive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0082] FIG. 1 shows an apparatus 1 according to the invention, comprising a cement premixer 3 and two crystallization tanks 4 and 5 . An inlet opening 7 is provided above the cement premixer 3 . The cement premixer 3 and the two crystallization tanks 4 and 5 are connected to each other by a machine frame 2 .
[0083] The cement premixer 3 has an ultrasonic probe 6 which extends internally through the wall of the cement premixer. A transfer line is provided between the cement premixer 3 and the two tanks 4 and 5. The transfer line may have regulating members, for example valve devices. The tank 5 has an outlet 10. The crystallization tanks 4 and 5 and the cement premixer 3 each have agitators 7 to 9.
[0084] Figure 2 shows a perspective view of the device of figure 1. Storage levels A, B and C are indicated on which the aforementioned containers are stored.
[0085] Figure 3 discloses further details, for example the crystallization tank 4 has an agitator 8 with a rod 15 and a spirally wound stirring blade 13. The crystallization tank has a cylindrical jacket portion 11 and a curved bottom portion 12.
[0086] A sensor element 17 is arranged in the upper part of the crystallization tank 4, which can be, for example, a temperature sensor. The crystallization tank 4 has an outlet 18 which merges into a transfer line 20. Furthermore, the crystallization tank 4 has an emergency drain 16, via which the tank 4 can be drained in case of an emergency, for example if the cement suspension is overflowing.
[0087] The crystallization tank 5 is of a similar design. Both the sensor element 27 and the agitator 9 can be seen. At the bottom 22 there are two drain nozzles 26 and 28, each with a flanged end 24. One of the two drain nozzles again serves as an emergency drain, the other allows transfer to a concrete mixer.
[0088] 4 shows a conventional method 100 for producing concrete. In this process, water 103, cements 104 and 105, additives 102, and optionally binders and admixtures, are mixed with gravel 106, 107 or sand 108 in a concrete mixer 101.
[0089] Those skilled in the art of concrete recognize binders as inorganic or organic substances that can be processed in a plastic state and harden after a certain time, binding other substances, such as aggregates, firmly together. Binders used in the concrete industry are of mineral origin and, with a few exceptions, are obtained from certain rocks by firing and grinding them into a fine powder. When mixed with water, a binder adhesive is first formed. Chemical reactions, and possibly also physical surface forces, can solidify the binder paste into a stone-like state, where any fillers can be bound together.
[0090] Those skilled in the art are also familiar with the terms "admixtures" for concrete or "concrete admixtures". These are substances that are added in small amounts to concrete in finely divided form, e.g., liquid, powder or as granules or pastes, to affect certain properties of the green or hardened concrete by chemical or physical action. Typical admixtures are concrete plasticizers, superplasticizers, air entrainers, sealants, retarders, accelerators, grout aids and / or stabilizers.
[0091] Furthermore, those skilled in the art of concrete are familiar with the term additives or concrete additives. These are finely dispersed substances that are used in concrete to improve or achieve certain properties. Such substances are present as volumetric components in the concrete composition in significantly greater amounts than admixtures. They are therefore also called fillers. According to DIN EN 206-1 and DIN 1045-2, two types of inorganic additives are distinguished: Type I additives are mostly inert additives, such as stone dust or pigments; Type II additives are pozzolans or latent hydraulic additives, such as trass, fly ash or silicate dust.
[0092] Finally, concrete mixtures contain significant proportions of aggregates such as gravel and sand, the particle sizes and proportions of which may vary depending on the type of concrete, and which are sometimes grouped together with other materials under the collective term aggregates.
[0093] The essence of the present invention is now to provide a method to overcome these technical obstacles and still ensure high early strength of concrete, for example by using an ultrasonic premix step.
[0094] In this process, cement 209, water 210 and additives 211 are mixed and ultrasonically activated in a cement premixer 212. The cement suspension is then transferred to a crystallization tank 213 and from there to a concrete mixer 201. Admixtures 202, water 203, cements 204 and 205, as well as gravel 206, 207 and sand 208 may also be fed to the concrete mixer 201 as part of a method 200 according to the invention.
[0095] The invention is based on the fact that there exists a favourable w / c ratio or w / c range for the preparation of cementitious suspensions, where the suspension is sufficiently homogenised and can be activated (e.g. by ultrasound). This favourable w / c ratio lies between 0.5 and 2, depending on the type of cement and admixtures used. Furthermore, the invention is based on the fact that it is not necessary to premix and activate the entire proportion of cement and water to produce a significant increase in early strength.
[0096] In a preferred variant of the invention, the cement suspension provided in the cement premixer is prepared from cement, water and, optionally, admixtures, whereas no additives are provided in the cement suspension.
[0097] This means that part of the cement is put into the premixer for activation and part of the cement is put into the concrete mixer. This can be done by a separate metering device at the premixer (silo + screw conveyor) or in an existing concrete mixing plant by a distributor of cement metering and a screw conveyor from the cement metering to the premixer.
[0098] Furthermore, part of the process according to the invention is that the premixed activated cement suspension is not charged into the concrete mixer immediately after mixing, but is instead conveyed to a resting or crystallization tank stored downstream of the suspension mixer. The capacity of the crystallization tank is approximately the amount of suspension required for one hour of concrete production.
[0099] This has the advantage that the required volume of the premixer is reduced compared to the variant using the entire amount of cement and water (and possibly sand) for pretreatment. The production and activation of the suspension and its subsequent storage in the crystallization tank has the further advantage that, after a sufficient crystallization time, a quick withdrawal or injection of the suspension is possible as required, and therefore the mixing time can be chosen short. The resting or crystallization period results in a significant increase in early strength, even compared to the variant where the entire calculated available amount of cement and water is premixed and activated. Without the resting period, this potential cannot be achieved. If ultrasound is used for activation in the premix stage, the early strength increases again significantly. Ideally, this resting period lasts from 1 to 8 hours, depending on the type of cement and the composition of the suspension.
[0100] The mixing time of the suspension mixing process in this production process needs to be very short so that the overall mixing time can be short. This is not always guaranteed, especially when the cement suspension is activated by, for example, ultrasound. In the production of large concrete elements (e.g. bridge girders), larger quantities of concrete must be produced in a short time in order to quickly complete the concrete element. This also poses special challenges for the premixing of the cement suspension in the ultrasonic premixer, since the mixing chamber is limited to a certain size in order to effectively apply ultrasound. By producing an "in-stock" of the suspension, these components can also be produced without the associated increase in concrete mixing time.
[0101] Compared to the prior art, the method presented here is characterized by the following novel approaches: · The proportion of cement suspension required for optimum strength development, ideally only 10-25% of the cement proportion is premixed and activated. The premixed and activated cement suspension is then conveyed in stock to a resting or crystallizing tank and left there for a period of time, ideally 1-8 hours, where it is continuously mixed at low shear rates or circulated by pumps. The removal from the crystallization tank is carried out subsequently after this pre-storage time and the concrete mixing time is not extended.
[0102] Thus, the problem of high moisture content of the aggregate can be effectively addressed. The mixing time of the concrete mixing process is not extended. The early strength increases significantly for the same concrete composition. If the crystallization tank is topped up by a further tank of the same size, even very large quantities of concrete can be produced precisely with the activated cement suspension (e.g. ready mixed concrete production).
[0103] In the following, an optimized pre-storage time in the crystallization tank is described.
[0104] FIG. 6 shows the time dependence of the heat release rate in J / gh, which is a calorimetric measurement of Portland cement, designated in the figure as CEM I 52.5 R, measured with and without ultrasonic treatment, designated in the figure as PUS. The onset of the acceleration phase and the maximum heat generation after about 4-5 hours are clearly different.
[0105] The reaction of cement with water follows a specific kinetic pathway. For a typical water-cement ratio of 0.5, the heat release rate curve is shown in Figure 6.
[0106] Patent application DE102020132015.9 proposes the use of pre-storage of an activated cement suspension, which does not interfere with the concrete manufacturing process and yet increases the early compressive strength.
[0107] Further research has shown that increasing the water content of the suspension and / or the time of pre-storage, in some cases significantly, offers process engineering advantages.
[0108] In concrete terms, this means that the time the suspension is added is correlated with the rate of heat release, and the suspension is only administered when the curve exceeds a 1-3 hour resting period and a new increase in heat release (= chemical reaction) is observed. This time varies greatly depending on the materials used (type of cement and superplasticizer as well as water content) and should be determined in advance.
[0109] The preferred parameters of the cement suspension are as follows: - Water / cement ratio (w / c) = 0.5 to 2 -Pre-storage time: 1-8 hours -Percentage of pre-treated cement: 5-95%, ideally 10-25%
[0110] The w / c ratio must be selected so that the rise of the curve (the so-called "acceleration phase") does not take too long (lower w / c ratios) and so that there is no solidification of the material during pre-storage (higher w / c ratios). A suitable w / c ratio for this is around 1.0±0.25, depending on the type of cement and the type and amount of superplasticizer.
[0111] The pre-storage time then depends on the selected w / c ratio and the reactivity of the cement. In order to keep the process engineering effort associated with pre-storage low, a maximum pre-storage time of 4 hours is targeted.
[0112] In this way the early strength can again be significantly increased and the proportion of cement that needs to be premixed and activated can be reduced.
[0113] In an exemplary method sequence, a portion of cement is premixed with water, ultrasonically treated, and then stored for an extended period of time. After storage, the cement suspension is metered into a concrete mixer. As previously mentioned, ultrasonic activation occurs as a result of the sonication. This is achieved using a power range of 25-250 W / cm 2 and ultrasonic amplitudes of 15 to 500 μm.
[0114] Hydrate nuclei are formed in the suspension, which significantly affects the early strength of the concrete, which can be demonstrated especially by microscopic images.
[0115] The calculated water available for the premix process is often insufficient, so the percentage of cement that is premixed is reduced.
[0116] In concrete with dry aggregate, three main components are distributed as shown in Figure 7. In this case, the water content is low but sufficient for the premix process since a flowable suspension can still be prepared and metered using a superplasticizer.
[0117] If the aggregate is wet, the percentage of aggregate in the volume calculation increases and the percentage of water decreases due to the percentage of moisture bound to the aggregate (see Figure 8). Figures 7 and 8 each show the weighed amounts of each component. The aggregate in Figure 8 is wetter than in Figure 7 and therefore contains more water. The figure only shows the amount of water added in addition to the aggregate by the bar "H2O". "H" and "H2O" should be understood as meaning the same in the drawings.
[0118] Here, there is very little water available for the mixing process, making it very difficult to apply a premix process (if at all). In the case of ultrasonic treatment, high solids concentrations often lead to undesirable side effects such as negative superplasticizer-cement interactions, strong heating, and problems with filling / draining the premix tank.
[0119] Nevertheless, to ensure the advantages of the premix process with ultrasound, a premix and store concept was developed, the essence of which is the use of only a fraction of the available cement (see Figure 9). The suspension produced in this way has a significantly lower solids content, which simplifies the production process compared to variants in which the entire cement is premixed.
[0120] However, the number of hydrate nuclei that can be formed is limited by the amount of cement. This led to the concept of storing or crystallizing the suspension until a sufficient amount of hydrate nuclei are formed to promote hydration. The number of hydrate phases increases with the time of pre-storage. For this purpose, measurements of the onset of setting, i.e. the point at which the hardening process has progressed to the point where the concrete cannot be further processed, are given below.
[0121] FIG. 10 shows the onset of setting of cement mortar with the following parameters: -W / C ratio of mortar = 0.50 -W / C ratio of upstream suspension = 1.0 -Percentage of pretreated cement = 25% - Sonication of suspensions at 20kHz and 60sec / liter
[0122] Figure 10 shows that the onset of clotting (Y-axis) decreases with increasing pre-storage time (X-axis). This behavior is particularly pronounced for the sonicated suspensions (cross-hatched). Without sonication, the decrease in clotting time is less pronounced (dash-hatched).
[0123] In general, the workability is also influenced by the pre-storage. This is determined by the slump flow and the slump spread for the cement. Figure 11 shows the slump flow and the slump spread for the cement mortar already described in figure 10 with cement suspensions of different lengths of time. Here, the extent to which the mortar flows on the table is measured without vibration (slump flow) and with 15 impacts (slump spread). Here, it can be seen that with increasing pre-storage time, both the slump flow and the spread dimension decrease. This means that the workability of the mortar decreases. However, in the first 240 minutes, the decrease is slight, which means that there is no significant change for the concrete. After 240 minutes, a more significant decrease occurs.
[0124] From these results it can be concluded that the ideal pre-storage time for the mortar under consideration is about 240 min, in which case the changes in workability are small and at the same time the early strength increases significantly.
[0125] As for the specific size, the effect can be explained by the following data. Concrete was produced using Portland cement (CEM I 52.5R) with a w / c ratio of 0.47. The concrete was pre-suspended and ultrasonicated for 240 minutes (w / c = 1.0) and then cooled to 0.3 m. 3 The mixture was mixed with a superplasticizer (type: polycarboxylate ether) having a volume of 1000 ml.
[0126] Figure 12 shows the evolution of compressive strength over the first 24 hours for concrete produced by the method according to the invention compared to conventionally produced concrete. It can be clearly seen that the concrete samples with pretreated suspension produced by the method according to the invention show significantly higher compressive strength at all measured times. [Explanation of symbols]
[0127] 1...device 2. Machine frame 3. Cement premixer 4, 5: Crystallization tank 6. Ultrasonic probe 7, 8, 9: Stirrer 10...exit 11 Jacket section 12...Bottom 13. Stirring blade 14···- 15 Rod 16...Emergency drain pipe 17 Sensor element 18...exit 19···- 20. Transfer line twenty one···- 22...Bottom twenty three···- 24 Flange end twenty five···- 26...Drain nozzle 27 Sensor element 28...Drain nozzle 100... ways 101: Concrete mixer 102 Additives 103...Water 104, 105: Cement 106, 107: Gravel 108: Sand 201: Concrete mixer 202 Admixtures 203...Wednesday 204, 205: Cement 206, 207: Gravel 208 Sand 209: Cement 210...Wednesday 211...Additives 212 Cement premixer 213 Crystallization tank
Claims
1. An apparatus (1) for producing concrete, comprising: i) a cement premixer (3) for mixing a cement suspension, said premixer having at least one ultrasonic generator for providing said cement suspension; ii) at least one first crystallization tank (4 or 5) for increasing the early strength of the concrete; and iii) a concrete mixer (201) for producing a concrete mixture from the premixed cement suspension by adding aggregates (206-208); An apparatus (1).
2. 2. Apparatus according to claim 1, characterized in that the cement premixer (3), the crystallization tank (4 or 5) and the concrete mixer (201) are arranged with respect to the earth's gravitational field such that the cement suspension can flow by gravity from the cement premixer (3) into the crystallization tank (4 or 5) and from there into the concrete mixer (201).
3. 3. Apparatus according to claim 1 or 2, characterized in that the device (1) comprises an arrangement (17, 27) for detecting a measurement variable for controlling the emergency drainage of the first crystallization tank (4 or 5).
4. 4. The apparatus according to claim 3, characterized in that the apparatus comprises a supply device for supplying a flowable medium as a function of the sensed measurement variable.
5. 5. Apparatus according to any of claims 1 to 4, characterized in that the first crystallization tank (4 or 5) is designed for a volume of cement suspension of at least 2 cubic meters.
6. 6. Apparatus according to any of the preceding claims, characterized in that the first crystallization tank (4 or 5) comprises a heat exchanger arrangement for the temperature control of the cement suspension along the wall of the crystallization tank (4 or 5).
7. 7. Apparatus according to any one of claims 1 to 6, characterized in that the apparatus (1) comprises a cement storage silo having a first portion supply line of cement to the cement premixer (212) and a second portion supply line of cement to the concrete mixer (201), and the apparatus comprises a cement metering machine for metering a first portion amount of cement to the cement premixer (212) and a second portion amount of cement to the concrete mixer (201).
8. 8. Apparatus according to any one of claims 1 to 7, characterized in that the first crystallization tank (4 or 5) comprises sensor elements for measuring the quality of the cement suspension located in the crystallization tank, the sensor elements being a temperature sensor, a torque sensor (viscosity), a conductivity sensor for determining the thermal or electrical conductivity, a sensor for measuring the ultrasonic transit time, a velocity sensor of the ultrasonic waves or a density sensor.
9. 9. The device according to claim 8, characterized in that the device (1) comprises a control unit and / or an evaluation unit for controlling a temperature control device, an inlet valve and / or an outlet valve based on measured values measured by the sensor elements.
10. 10. Apparatus according to any one of claims 1 to 9, characterized in that the apparatus (1) comprises a second crystallization tank (5) between the first crystallization tank (4) and the concrete mixer (201).
11. A method for producing concrete using the apparatus according to any one of claims 1 to 10, i) preparing a cement suspension in a cement premixer (212) using ultrasound; ii) stirring the cement suspension in a crystallization tank (213) for a predetermined residence time. and iii) transferring said cement suspension after a given residence time to a concrete mixer (201). A method comprising:
12. The cement blender (212) comprises a processing space, and the at least one ultrasonic probe (6) projects at least partially into the processing space; The ultrasonic probe (6) emits ultrasonic waves, and the emitted ultrasonic waves have a power of 25 to 250 W / cm 2 and an amplitude of 15 to 500 μm.
13. 13. The method according to claim 11 or 12, characterized in that the control of the residence time is performed as a function of a given time at a given temperature and / or the residence time of the suspension is based on a predetermined heat release.
14. Method according to any of claims 11 to 13, characterized in that the pre-storage time of the cement suspension before transfer to the concrete mixer (201) is between 1 and 8 hours.
15. 15. The method according to any one of claims 11 to 14, characterized in that the proportion of pretreated cement in the concrete is between 5 and 95% by weight.