Small crystals SSZ-41, their synthesis and uses

JP2024511577A5Active Publication Date: 2024-10-08CHEVRON USA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023555597
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-03-15
Filing Date
2022-03-14
Publication Date
2024-10-08
Estimated Expiration
2042-03-14

AI Technical Summary

Technical Problem

Existing synthesis methods for SSZ-41 molecular sieves face challenges in producing low silica-to-alumina molar ratios without significant impurity phases, particularly for MTW framework-type materials, due to aluminum being a crystallization inhibitor, which affects catalyst activity and selectivity.

Method used

A novel synthesis method for zincoaluminosilicate molecular sieves with an SSZ-41 framework structure is developed, using a reaction mixture comprising FAU framework zeolite, zinc and lithium sources, a specific structure-directing agent, and seeds, under sodium-free conditions, to achieve small crystal sizes and improved catalyst performance.

Benefits of technology

The method produces SSZ-41 molecular sieves with high aluminum concentrations and small crystal aggregates, enhancing catalyst activity and selectivity for organic transformation reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for producing small crystal, high aluminum content zincoaluminosilicate crystalline materials having an SSZ-41 framework structure is disclosed. Compositions produced according to the method and uses thereof are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Application No. 63 / 160,979, filed March 15, 2021, the disclosure of which is incorporated herein by reference.

[0002] Field This disclosure relates to small crystal size SSZ-41 molecular sieves, their synthesis, and use as adsorbents and catalysts for organic conversion reactions. [Background technology]

[0003] Molecular sieves are a commercially important class of materials with specific chemical compositions that have a unique crystal structure with a distinct pore structure that is revealed by a distinctive X-ray diffraction (XRD) pattern. The crystal structure defines the cavities and pores that are characteristic of a particular type of molecular sieve.

[0004] A conventional preparation method using crystalline molecular sieve SSZ-41 and α,ω-di(N-methylpiperidine) polymethylene dicationic compound and α,ω-di(1,4-diazabicyclo[2.2.2]octane) polymethylene dicarboxylic acid compound as structure directing agents is taught by U.S. Pat. No. 5,591,421.

[0005] SSZ-41 materials are useful as catalysts in a variety of organic transformation reactions In such applications, activity and / or selectivity are generally found to be improved when the molecular sieve product has a low silica to alumina molar ratio and small crystal size. Unfortunately, aluminum can be a crystallization inhibitor for some zeolites, including SSZ-41 materials, so it is difficult to produce low silica to alumina molar ratios by most existing synthetic routes without significantly generating impurity phases, especially MTW framework-type materials.

[0006] In accordance with the present disclosure, it has been discovered that SSZ-41 can be produced at higher aluminum concentrations than previously exemplified, and further, that products comprised of agglomerates of small crystals of SSZ-41 having a low silica to alumina molar ratio have been found to have improved activity and selectivity as isomerization catalysts compared to catalysts prepared from conventional SSZ-41. Summary of the Invention

[0007] In a first aspect, there is provided a zincoaluminosilicate molecular sieve having a framework structure of SSZ-41 and an average crystallite size of 500 nm or less.

[0008] In a second aspect, there is provided a method for synthesizing a zincoaluminosilicate molecular sieve having a framework structure of SSZ-41, comprising: (1) forming a reaction mixture comprising (a) an FAU framework-type zeolite, (b) a zinc source, (c) a structure directing agent (Q) comprising 1,1'-(1,4-butanediyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane] dication, (d) a lithium source, (e) a hydroxide ion source, (f) water, and (g) seeds; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form zincoaluminosilicate molecular sieve crystals, wherein the reaction mixture is sodium free or substantially sodium free.

[0009] In a third aspect, a process is provided for converting a feedstock comprising organic compounds to conversion products, the process comprising: (i) contacting the feedstock with a catalyst comprising a zincoaluminosilicate molecular sieve having a framework structure of SSZ-41 and an average crystal size of 500 nm or less under organic compound conversion conditions to produce an effluent comprising conversion products; and (ii) recovering the converted products from the effluent. [Brief description of the drawings]

[0010] [Figure 1]1 shows the powder X-ray diffraction (XRD) pattern of the as-synthesized product of Example 1.

[0011] [Diagram 2] 1A and 1B show scanning electron micrograph (SEM) images of conventional SSZ-41 (large particle SSZ-41) and the as-synthesized SSZ-41x product of Example 1.

[0012] [Diagram 3] 1 is a plot of conversion or yield versus temperature for n-decane conversion over Pd / SSZ-41x catalyst.

[0013] [Figure 4] 1 is a plot of product yield versus conversion for n-decane conversion over Pd / SSZ-41x catalyst.

[0014] [Diagram 5] 1 is a plot of methylnonane isomer distribution versus conversion for n-decane conversion over Pd / SSZ-41x catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] definition As used herein, the term "zeolite" refers to an aluminosilicate molecular sieve having a framework composed of alumina and silica (ie, repeating tetrahedral units of SiO4 and AlO4).

[0016] The term "zincoaluminosilicate" refers to a molecular sieve having a framework composed of zinc, alumina, and silica (ie, repeating ZnO4, AlO4, and SiO4 tetrahedral units).

[0017] As used herein, the term "framework type" has the meaning set forth in "Atlas of Zeolite Framework Types" by Ch. Baerlocher, LBMcCusker and DH Olson (Elsevier, 6th revised edition, 2007).

[0018] The term "as-synthesized" refers to the molecular sieve in its state after crystallization and prior to removal of the structure directing agent.

[0019] The term "SiO2 / Al2O3 molar ratio" is sometimes abbreviated as "SAR."

[0020] The term "SSZ-41x" refers to a zincoaluminosilicate molecular sieve having the structure of SSZ-41 and characterized by having an average crystallite size of less than or equal to 500 nm.

[0021] Molecular sieve synthesis A zincoaluminosilicate molecular sieve having an SSZ-41 framework structure can be synthesized by (1) forming a reaction mixture comprising (a) an FAU framework-type zeolite, (b) a zinc source, (c) a structure directing agent (Q) comprising 1,1'-(1,4-butanediyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane] dication, (d) a lithium source, (e) a hydroxide ion source, (f) water, and (g) seeds; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form zincoaluminosilicate molecular sieve crystals, wherein the reaction mixture is sodium free or substantially sodium free.

[0022] The reaction mixture may have a composition, in molar ratios, within the ranges set forth in Table 1. [Table 1] wherein Q comprises a 1,1'-(1,4-butanediyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane] dication.

[0023] The FAU framework-type zeolite can be zeolite Y. The FAU framework-type zeolite can be an ammonium-form zeolite or a hydrogen-form zeolite (e.g., NH4 + - Forms of Zeolite Y and H + The FAU framework type zeolite may be a zeolite Y-form (FAU framework type zeolite). The FAU framework type zeolite may have a SiO2 / Al2O3 molar ratio of at least 12 (e.g., 12-500, or 12-100, or 30-500, or 30-100, or 60-80). The FAU framework type zeolite may comprise two or more zeolites. Typically, the two or more zeolites are Y zeolites having different silica to alumina molar ratios. Examples of suitable aluminosilicate zeolites include Y zeolites CBV720, CBV760, and CBV780 available from Zeolyst International, and Y zeolites HSZ-HUA385 and HSZ-HUA390 available from Tosoh. The FAU framework type zeolite may be used as the sole or primary source of silicon and aluminum in the reaction mixture.

[0024] The FAU framework-type zeolite can be a zinc-exchanged zeolite (e.g., zinc-exchanged zeolite Y), where the zeolite can also be the source of zinc metal for the reaction mixture. "Zinc-exchanged zeolite" refers to an aluminosilicate zeolite in which zinc metal is disposed on the surface and / or within the cages and / or pores of the aluminosilicate zeolite. It does not refer to an aluminosilicate in which the zinc metal is within the aluminosilicate framework.

[0025] Additionally or alternatively, the zinc source may be a zinc salt of an organic or inorganic acid. Exemplary zinc salts include zinc formate, zinc acetate, zinc citrate, zinc chloride, zinc bromide, zinc nitrate, and zinc sulfate.

[0026] Sources of lithium include lithium hydroxide and other lithium salts, especially lithium halides such as lithium chloride.

[0027] Preferably, the reaction mixture is sodium-free or substantially sodium-free. The term "substantially free" means that the indicated substance is not intentionally added to the composition, or is preferably not present at analytically detectable levels. This is meant to include compositions in which the specified substance is present only as an impurity of one of the intentionally added substances. For example, a "substantially sodium-free" composition may refer to a composition containing 0.005% or less, 0.002% or less, and / or 0.001% or less sodium by weight. Applicants have discovered that the presence of sodium can cause various impurities in the final product. For example, if SSZ-41 is synthesized in the presence of sodium cations, ZSM-12 (MTW) ​​can be an impurity in the final product.

[0028] The hydroxide ion source can be lithium hydroxide. The structure directing agent can also be used to provide the hydroxide ions.

[0029] The structure directing agent (Q) comprises 1,1'-(1,4-butanediyl)bis-4-aza-1-azoniabicyclo[2.2.2]octane dication (DABCO-diquat-4) of the following structure (1): [ka]

[0030] Suitable sources of Q are the hydroxide, chloride, bromide, and / or other salts of diquaternary ammonium compounds.

[0031] The reaction mixture also contains seeds, typically SSZ-41 from a previous synthesis, desirably in an amount of 0.1-20 wt. % (e.g., 0.5-10 wt. %) based on the total weight of SiO2 in the reaction mixture. Seeding can be advantageous in improving the selectivity of SSZ-41x and / or shortening the crystallization process.

[0032] It is noted that the components of the reaction mixture can be provided from multiple sources, or two or more reaction components can be provided by a single source, and the reaction mixture can be prepared in either a batch or continuous manner.

[0033] Crystallization of the desired molecular sieves from the above reaction mixture can be carried out in a suitable reaction vessel, such as, for example, a polypropylene jar or Teflon-lined or stainless steel autoclave, under either static, tumbling or stirred conditions, at a temperature between 100° C. and 200° C. (e.g., 130° C. and 180° C.) for a time sufficient for crystallization to occur at the temperature used, such as about 1 day to 14 days (e.g., 3 days to 10 days). Crystallization is typically carried out under pressure in an autoclave such that the reaction mixture is subjected to autogenous pressure.

[0034] Once the desired molecular sieve crystals have formed, the solid product can be separated from the reaction mixture by standard mechanical separation techniques such as centrifugation or filtration. The recovered crystals are washed with water and dried for a few seconds to a few minutes (e.g., 5 seconds to 10 minutes for flash drying) or for a few hours (e.g., 4 hours to 24 hours for oven drying at 75°C to 150°C) to obtain the as-synthesized molecular sieve crystals. The drying step can be carried out under vacuum or at atmospheric pressure.

[0035] As a result of the crystallization process, the recovered crystalline molecular sieve product contains within its pores at least a portion of the structure directing agent used in its synthesis.

[0036] The as-synthesized molecular sieve may be heat-treated, ozone-treated, or otherwise treated to remove some or all of the directing agent used in its synthesis. Removal of the directing agent may be accomplished using a heat treatment (e.g., calcination) in which the as-synthesized material is heated in an atmosphere selected from air, nitrogen, or mixtures thereof at a temperature sufficient to remove some or all of the directing agent. For convenience, atmospheric pressure is required for the heat treatment, although subatmospheric pressures may also be used. The heat treatment may be performed at a temperature of at least 370° C. (e.g., 400-700° C.) for at least 1 minute, typically for no more than 20 hours (e.g., 1-8 hours).

[0037] To the extent desired, any extraframework metal cations (e.g., Li+) in the molecular sieve can be replaced by ion exchange with other cations according to techniques well known in the art. Replacement cations include metal ions, hydrogen ions, hydrogen precursors (e.g., ammonium ions), and mixtures thereof.

[0038] Molecular sieve characterization In its as-synthesized and anhydrous forms, the SSZ-41x molecular sieves can have a chemical composition, in molar ratios, within the ranges shown in Table 2. [Table 2] wherein Q comprises a 1,1'-(1,4-butanediyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane] dication.

[0039] The crystals of the SSZ-41x molecular sieve can have an average crystal size of 500 nm or less. Typically, the crystals can have an average crystal size in the range of 50-500 nm (e.g., 50-250 nm, or 75-500 nm, or 75-250 nm). Conventional SSZ-41 usually has an average crystal size of at least 1 micron.

[0040] Crystal size is based on individual crystals (including twins) but does not include crystal aggregates. Crystal size is the length of the longest diagonal of a three-dimensional crystal. Direct measurements of crystal size can be made using microscopy techniques such as SEM and transmission electron microscopy (TEM). For example, measurements by SEM involve the examination of the morphology of a material at high magnification (usually 1000× to 10,000×). SEM techniques can be performed by distributing a representative portion of molecular sieve powder on a suitable mount so that the individual particles are reasonably evenly spread across the field of view at 1000× to 10,000× magnification. From this population, a statistically significant sample of random individual crystals (e.g., 50-200) is examined and the longest diagonal of the individual crystals is measured and recorded. (Particles that are clearly large polycrystalline aggregates should not be included in the measurement.) Based on these measurements, the arithmetic mean of the sample crystal size is calculated.

[0041] As conventionally synthesized, for example as taught by U.S. Pat. No. 5,591,421, the molecular sieve SSZ-41 has a powder X-ray diffraction (XRD) pattern which, for the synthetic form of the molecular sieve, includes at least the peaks listed in Table 3 below, and for the calcined form of the molecular sieve, includes at least the peaks listed in Table 4 below. [Table 3] [Table 4]

[0042] The X-ray diffraction data reported herein were collected by standard techniques using copper K-α radiation. The determination of the parameter 2-θ is subject to both human and mechanical errors, which, when combined, result in an uncertainty of approximately ±0.10° in each reported value of 2-θ. It is understood that the values ​​of d-spacing, when converted to values ​​corresponding to d-spacing using Bragg's law, have a corresponding deviation determined based on ±0.10 degrees 2θ. The relative intensity of a line, I / Io, represents the ratio of the peak intensity to the intensity of the most intense line above background. Relative intensities are given the following symbols: VS=very strong (>60), S=strong (≧40 and ≦60), M=medium (≧20 and <40), and W=weak (<20).

[0043] It is known that certain lines in the X-ray pattern of molecular sieves tend to broaden as the relevant dimension of the molecular sieve crystal decreases, so that adjacent lines begin to overlap, thereby appearing as only partially resolved peaks, or as unresolved broad peaks.

[0044] Applicants have discovered that the novel synthesis methods described herein can produce SSZ-41x molecular sieves with high phase purity, i.e., SSZ-41x molecular sieves with phase purity of 95% to 99% or greater as determined, for example, by Rietveld XRD analysis. As used herein, the term "phase purity" with respect to a molecular sieve means the amount (e.g., by weight) of a single crystalline phase of the molecular sieve relative to the total weight of all phases (crystalline and amorphous) in the molecular sieve material. Thus, although other crystalline phases may be present in the SSZ-41x molecular sieve, the SSZ-41x molecular sieve comprises at least 95% by weight (e.g., at least 97%, or at least 98%, or at least 99%, or at least 99.9%) of SSZ-41x as the predominant crystalline phase, with the weight percentage of SSZ-41x being provided relative to the total weight of the molecular sieve crystalline phases present in the composition. Examples of other crystalline phases that may be present as impurities may include faujasite undissolved (FAU) and / or MTW framework type material.

[0045] Industrial Applicability The SSZ-41x materials described herein can be used as adsorbents or catalysts to facilitate one or more of a wide variety of organic compound conversion processes. Examples of chemical conversion processes that are effectively catalyzed by the SSZ-41x materials described herein, alone or in combination with one or more other catalytically active substances (including other crystalline catalysts), include those that require a catalyst with acid activity. Examples of organic conversion processes that may be catalyzed by the SSZ-41x materials described herein include cracking, hydrocracking, disproportionation, alkylation, oligomerization, and isomerization.

[0046] As with many catalysts, it may be desirable to combine SSZ-41x materials with another material that is resistant to the temperatures and other conditions used in organic conversion processes. Such materials include active and inactive materials, synthetic or naturally occurring zeolites, and inorganic materials such as clays, silica and / or metal oxides such as alumina. The latter may be naturally occurring or in the form of gelatinous precipitates or gels that include mixtures of silica and metal oxides. The use of materials in combination with SSZ-41 (i.e., combined with or present with SSZ-41 during the synthesis of new crystals that are active) tends to alter the conversion and / or selectivity of the catalyst in certain organic conversion processes. Inert materials suitably serve as diluents to control the amount of conversion in a given process so that products can be obtained in an economical and orderly manner without employing other means to control the reaction rate. These materials can be incorporated into natural clays (e.g., bentonite and kaolin) to improve the crush strength of the catalyst under commercial operating conditions. These materials (i.e., clays, oxides, etc.) act as binders for the catalyst. Since it is desirable to prevent the catalyst from breaking down into powder in commercial applications, it is desirable to provide a catalyst with good crush strength. These clay and / or oxide binders are typically used solely for the purpose of improving the crush strength of the catalyst.

[0047] Natural clays that can be composited with SSZ-41x materials include the montmorillonite and kaolin families, including sub-bentonites, kaolins commonly known as Dixie, McNamee, Georgia, and Florida clays, or others whose primary mineral components are halloysite, kaolinite, dickite, nacrite, or anaxite. Such clays can be used as originally mined, or after initial calcination, acid treatment, or chemical modification. Binders useful for composites with SSZ-41x also include inorganic oxides, such as silica, zirconia, titania, magnesia, beryllia, alumina, and any combination thereof.

[0048] In addition to the above materials, SSZ-41x can be composited with porous matrix materials such as silica-alumina, silica-magnesia, silica-zirconia, silica-thoria, silica-beryllia, silica-titania, and ternary compositions such as silica-alumina-thoria, silica-alumina-zirconia, silica-alumina-magnesia, and silica-magnesia-zirconia.

[0049] The relative proportions of SSZ-41x and inorganic oxide matrix can vary widely, with the SSZ-41x content ranging from 1 to 90 wt % (e.g., 2 to 80 wt %) of the composite. EXAMPLES

[0050] The following illustrative examples are intended to be non-limiting.

[0051] Example 1 A Teflon liner was charged with 0.036 g anhydrous LiOH, 0.10 g zinc acetate dihydrate, 0.44 g Zeolyst CBV760 Y zeolite (SAR=60), 0.22 g Tosoh 390HUA Y zeolite (SAR=500), as-synthesized SSZ-41 seeds (based on 3% of the other two FAU materials as the silica source), 3 mM DABCO-diquat-4 dihydroxide, and water. The total of the SDA solution and additional water was 5.6 g. All aluminum in the reaction mixture was provided by the two FAU materials. The liner was then capped, sealed in a 23 mL autoclave, and heated in a convection oven at tumbling conditions (43 rpm) at 150 °C for 6-8 days. The solids were then separated by centrifugation, washed with deionized water, and dried in a 95 °C oven.

[0052] Figure 1 shows the powder XRD of the as-synthesized product, consistent with the product being SSZ-41x. The powder XRD pattern of the product shows the broad characteristics of a material with very small crystallites.

[0053] SEM images of conventional SSZ-41 (large particle SSZ-41) and as-synthesized SSZ-41x products are shown in Figures 2A and 2B, respectively.

[0054] The as-synthesized product had an aluminum content of 1.04 wt.% (SAR=84) as measured by inductively coupled plasma-atomic emission spectroscopy (ICP-AES).

[0055] The as-synthesized material was then calcined in air by placing a thin bed of material in a calcination dish and heating in a muffle furnace from room temperature to 120°C at a rate of 1°C / min and holding at 120°C for 2 hours. The temperature was then increased at a rate of 1°C / min to 540°C and held at 540°C for 5 hours. The temperature was again increased at 1°C / min to 595°C and held at 595°C for 5 hours. The material was then cooled to room temperature.

[0056] The calcined material was converted to the ammonium form by heating in an ammonium nitrate solution (typically 1 g NH4NO3 / 1 g zeolite in 10 mL H2O at 85°C for at least 3 hours). The material was then filtered. This was repeated twice for a total of three exchanges. Finally, the material was washed with deionized water to a conductivity of less than 100 μS / cm and dried in air at 85°C.

[0057] The acid site density was characterized using n-propylamine temperature programmed desorption (TPD) and found to be 312.64 μmol H+ / g.

[0058] Analysis by nitrogen physical adsorption showed that the micropore volume in the t-plot was 0.1207 cm 3 / g, the external surface area of ​​the t-plot is 122.04 m 2 / g, BET surface area is 383.05m 2 / g, total pore volume is 0.933 cm 3 / g.

[0059] Examples 2 to 5 For Examples 2-5, the starting materials outlined in Table 5 below were each loaded into a Teflon liner. Zinc-exchanged CBV760 Y zeolite (SAR=60, Zeolyst) was prepared from hydrogen form Y zeolite by ion exchange methods known in the art. The zinc-exchanged material had a zinc content of about 3 wt.%. The liner was then capped and sealed in a 23 mL autoclave and heated in a convection oven at tumbling conditions (43 rpm) at 150°C for 6-8 days. The solids were then separated by centrifugation, washed with deionized water, and dried in an oven at 95°C. The recovered products were characterized by powder XRD. [Table 5]

[0060] Examples 6 to 16 For Examples 6-16, the starting materials outlined in Table 6 below were each loaded into a Teflon liner. The zinc source was zinc acetate dihydrate. The liner was then capped and sealed in a 23 mL autoclave and heated in a convection oven at tumbling conditions (43 rpm) at 150°C for 6-8 days. The solids were then separated by centrifugation, washed with deionized water, and dried in an oven at 95°C. The recovered products were characterized by powder XRD. [Table 6-1] [Table 6-2]

[0061] Example 17 Constraint Index The constraint index is a test for determining the shape-selective catalytic behavior of zeolites. It compares the reaction rates for the cracking of n-hexane and its isomer 3-methylpentane under competitive conditions (see, for example, V. J. Frillette et al., J. Catal. 1981, 67, 218-222).

[0062] Ammonium-exchanged SSZ-41x (NH4 + Catalyst (SSZ-41x) was pelletized at 4-5 kpsi, crushed, and meshed to 20-40. 0.47 g (dry weight measured by TGA at 600 °C) of this catalyst was then loaded into a 3 / 8 inch stainless steel tube lined on both sides of the zeolite bed with catalytically inactive alundum. The reactor tube was heated using an ATS (Applied Test Systems, Inc.) furnace. Helium was introduced into the reactor at 23 mL / min and atmospheric pressure. The catalyst was dehydrated at 482 °C for 2 h. The reactor temperature was then reduced to the preselected reaction temperature (e.g., 427 °C in this example). The helium flow rate was then adjusted to 9.4 mL / min and an equimolar mixed feed of n-hexane and 3-methylpentane was introduced into the reactor at a rate of 0.48 mL / h. The feed was delivered by an ISCO pump. 15 min after feed introduction, online sampling of the products to a gas chromatograph (GC) was started. Constraint index values ​​(including 2-methylpentane) were calculated from the GC data using methods known in the art. Representative results are shown in Table 7. [Table 7]

[0063] The initial conversion with SSZ-41x prepared as described herein is more than double that with conventional SSZ-41, which was prepared according to U.S. Patent No. 5,591,421 and showed 26% conversion after 10 minutes.

[0064] Example 18 Catalyst preparation Ammonium-exchanged SSZ-41x (NH4 + / SSZ-41x) was ion-exchanged in an aqueous solution of palladium nitrate with a pH of about 10 and a Pd loading of 0.5 wt.%. The Pd-exchanged zeolite was washed with deionized water to a conductivity of less than 50 mS / cm and dried. The zeolite was then calcined in air at 482 °C for 3 h.

[0065] Example 19 Hydroconversion of n-decane For catalytic testing, the Pd catalyst of Example 18 was pelletized at 4-5 kpsi, crushed, and meshed to 20-40. 0.50 g of this catalyst (dry weight determined by TGA at 600°C) was then loaded into the center of a 23 in. long by 0.375 in. OD stainless steel reactor tube loaded with catalytically inactive alundum on both sides of the zeolite bed. The reactor tube was heated using an ATS (Applied Test Systems, Inc.) furnace. The catalyst was then heated from room temperature to 232°C for 120 h, held at 232°C for 1 h, heated from 232°C to 316°C for 1 h, held at 316°C for 3.5 h, and preconditioned into downflow hydrogen at atmospheric pressure at a rate of 95 mL / min. It was then cooled to 221°C. The reactor was then pressurized to 1200 psig with a high hydrogen flow rate.

[0066] The reaction was started at 221 °C, 1200 psig, 0.66 mL / h of n-decane, and 8.3 mL / min of H2 downflow. Feed was provided by an ISCO pump. The reaction temperature was increased to 282 °C in steps of 5.6 °C. Products were analyzed by an online capillary GC approximately once every 60 min. Raw data from the GC was collected by an automated data acquisition / processing system, and the hydrocarbon conversion was calculated from the raw data. Conversion is defined as the amount (mol%) of n-decane that was reacted to produce products other than the feed n-decane (i.e., iso-C10 and cracked products). The iso-C10 yield is expressed as the mole % of the feed n-decane converted to iso-C10 products. The cracked products (less than C10) yield is expressed as the mole percent of the feed n-decane converted to cracked products.

[0067] The results of the hydrocarbon conversion are shown in Figures 3-5. As shown, up to about 50% conversion, the products are more than 80% isomerized C10, mostly single-branched C10 isomers. Furthermore, an isomerization maximum is observed at about 260°C, indicating that the catalyst is highly active.

Claims

1. A zincoaluminosilicate molecular sieve having an SSZ-41 framework structure and an average crystal size of 500 nm or less.

2. SiO in the range of 30 to less than 100 2 / Al 2 O 3 Molar ratio and SiO in the range of 15 to 75 2 2. The zincoaluminosilicate molecular sieve of claim 1 having a molar ratio of ZnO to ZnO.

3. 2. The zincoaluminosilicate molecular sieve of claim 1, wherein said average crystallite size is in the range of 50 nm to 500 nm.

4. 2. The zincoaluminosilicate molecular sieve of claim 1 having a phase purity of at least 95% by weight.

5. 2. The zincoaluminosilicate molecular sieve of claim 1 further comprising within its pores a 1,1'-(1,4-butanediyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane] dication.

6. 1. A method for synthesizing a zincoaluminosilicate molecular sieve having a framework structure of SSZ-41, said method comprising: (1) forming a reaction mixture, the reaction mixture comprising: (a) FAU framework zeolite; (b) a zinc source; (c) a structure directing agent (Q) containing 1,1'-(1,4-butanediyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane] dication; (d) a lithium source; (e) a hydroxide ion source; (f) water, and (g) forming the reaction mixture comprising a seed; (2) subjecting said reaction mixture to crystallization conditions sufficient to form crystals of said zincoaluminosilicate molecular sieve; wherein the reaction mixture contains no more than 0.005%, no more than 0.002%, no more than 0.001% sodium by weight, or is sodium-free.

7. 7. The method of claim 6, wherein the reaction mixture has the following composition in molar ratios: 【Table 1A】

8. 7. The method of claim 6, wherein the reaction mixture has the following composition in molar ratios: 【Table 1B】

9. 7. The method of claim 6, wherein the FAU framework-type zeolite is zeolite Y.

10. 7. The method of claim 6, wherein the zinc source comprises a zinc salt of an organic or inorganic acid, a zinc-exchanged FAU framework-type zeolite, or any combination thereof.

11. 7. The method of claim 6, wherein the lithium source comprises lithium hydroxide, lithium halide, or any combination thereof.

12. The method of claim 6, wherein the seeds comprise a molecular sieve having a framework structure of SSZ-41.

13. The reaction mixture is a mixture of SiO 2 7. The method of claim 6, further comprising adding 0.1 to 20 wt. % of seeds based on the total weight of the mixture.

14. 7. The method of claim 6, wherein the crystallization conditions comprise heating the reaction mixture under autogenous pressure at a temperature in the range of 100° C. to 200° C. for a time period ranging from 1 to 14 days.

15. 1. A process for converting a feedstock comprising organic compounds into a conversion product, the process comprising: (i) contacting said feedstock with a catalyst comprising a zincoaluminosilicate molecular sieve having a framework structure of SSZ-41 and an average crystal size of 500 nm or less under conditions for converting organic compounds to produce an effluent comprising a conversion product; (ii) recovering said conversion products from said effluent.

16. The zincoaluminosilicate molecular weight is in the range of 30 to less than 100 SiO 2 / Al 2 O 3 Molar ratio and SiO in the range of 15 to 75 2 16. The process of claim 15 having a molar ratio of ZnO to ZnO.

17. 16. The process of claim 15, wherein the zincoaluminosilicate molecular sieve has an average crystal size in the range of 50 nm to 500 nm.

18. 16. The process of claim 15, wherein the zincoaluminosilicate molecular sieve has a phase purity of at least 95% by weight.