Solid acid alkylation catalyst and its preparation and use

The synthesis of MWW structural molecular sieves using low-toxic organic amines and seed crystals addresses the deactivation and cost issues of conventional catalysts, providing a stable and cost-effective solid acid alkylation catalyst with improved performance in alkylation reactions.

JP2024545459AActive Publication Date: 2024-12-06PETROCHINA CO LTD

Patent Information

Application Number
JP2024534763
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-08
Filing Date
2022-12-13
Publication Date
2024-12-06
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Conventional alkylation catalysts, such as L acid catalysts like AlCl3 and B acid catalysts like HF, H2SO4, face issues with deactivation due to carbon accumulation and environmental hazards, while macroporous molecular sieves suffer from channel clogging and high manufacturing costs, necessitating the development of a more stable and cost-effective solid acid catalyst.

Method used

A method for synthesizing MWW structural molecular sieves using low-toxic and inexpensive organic amines as template agents, combined with seed crystals, to form interlayer hydrogen bonds, resulting in a solid acid alkylation catalyst with improved stability and catalytic activity.

Benefits of technology

The synthesized catalyst exhibits high alkylation catalyst activity, reduced environmental impact, and lower production costs, with enhanced stability and selectivity in alkylation reactions, isomerization, and decomposition reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545459000001_ABST
    Figure 2024545459000001_ABST
Patent Text Reader

Abstract

The present invention provides a solid acid alkylation catalyst and its preparation method and use, the preparation method includes the steps of: S1: mixing aluminum source, water, alkali source, template agent, silicon source and seed crystal to form gel, carrying out crystallization reaction to obtain MWW structure molecular sieve (wherein the template agent is composed of main template agent and sub-template agent with a molar ratio of 0.5-20:1); S2: calcining the MWW structure molecular sieve obtained in S1 to remove template agent, then carrying out ammonium exchange, and calcining again to obtain H type molecular sieve; S3: mixing the H type molecular sieve obtained in S2 with inorganic oxide and nitric acid solution, kneading and molding to obtain solid acid alkylation catalyst. The present invention uses the method of seed crystal and two kinds of template agents to cooperate in crystallization, directly synthesizing MWW structure molecular sieve without using hexamethyleneimine, piperidine, homopiperazine, and further obtaining solid acid alkylation catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid acid catalyst, and in particular to a solid acid alkylation catalyst and its preparation method and use. [Background technology]

[0002] Alkylation is a very important reaction in the petrochemical industry, among which the alkylation reaction between aromatic hydrocarbons and olefins to produce alkyl-substituted aromatic hydrocarbons is a very important reaction. The usual catalysts can be divided into L acid catalyst and B acid catalyst. L acid catalyst is anhydrous AlCl 3 The main representative is HF, H. It has the advantages of being cheap, having high catalytic activity, and being technologically mature. However, the production process generates a large amount of aluminum-containing waste liquid, and there are too many side reactions, so the catalyst is currently almost completely eliminated from the market. 2 SO 4 and H 3 PO 4 However, because the reaction of long carbon chain olefins is prone to deactivation due to carbon accumulation in the catalyst, the use of liquid acids is currently focused mainly on the alkylation reaction of long chain olefins (carbon number > 8). 2 SO 4 Due to the strong corrosiveness of , the requirements for equipment materials are very high, and the production process also involves the discharge of various waste materials, which results in very high environmental costs, so there is a strong need to develop solid acid catalysts.

[0003] The 12-ring macropore molecular sieve has a strong channel internal diffusion performance, which is effective in alleviating the problem of rapid catalyst deactivation caused by channel clogging, but the conventional 12-ring macropore molecular sieve, such as octahedral zeolite and beta zeolite, is prone to deactivation due to the blocking of the channels inside the crystal by large molecules. In the conventional technology, different types of 12-ring macropore molecular sieves are used as the main active components of the catalyst, and the diffusion performance is further improved by modifying the molecular sieve, but there are still problems such as complicated manufacturing costs, the presence of highly corrosive halogens, and the deterioration of the stability of the molecular sieve.

[0004] The MWW molecular sieve has a very typical two-dimensional sheet-like morphology, and the sheet-like structure is formed by stacking several basic monolayers, and a unique channel structure is also formed, mainly including two-dimensional sinusoidal 10-membered ring channels in the ab-axis plane and 12-membered ring supercage structures and semi-supercage structures along the c-axis direction. The opening size of the 10-membered ring channel is 0.41nm×0.51nm, and it is distributed outside the supercage structure. The size of the 12-membered ring supercage is 0.71nm×0.71nm×1.82nm, and it communicates with six identical supercages in the surrounding ab-axis plane through the 10-membered ring. The size of the semi-supercage distributed on the surface of the sheet layer is 0.71nm×0.71nm×0.8nm, and its open 12-membered opening is very favorable for the diffusion of reactants, and it has excellent catalytic reaction performance for large molecule reactions, and is widely applied in reaction processes such as alkylation.

[0005] MWW structure molecular sieves can be subdivided into several varieties according to the lamination method of the basic monolayer, including MCM-22(P) molecular sieve, which is mainly hydrogen bond between monolayers, MCM-49 molecular sieve, which is oxygen bridge bond between monolayers, MCM-36 molecular sieve, which forms column support structure between layers, MCM-56 molecular sieve, which is randomly laminated between layers, ITQ-2 molecular sieve with monolayer structure, etc. Among them, MCM-22(P) molecular sieve is relatively special, and after calcining and dehydrating the silanol group between layers to form oxygen bridge bond, MCM-22 molecular sieve (the crystal structure is the same as MCM-49 molecular sieve) can be obtained, and MCM-36 molecular sieve can be produced through swelling and column support, and ITQ-2 molecular sieve can be produced through swelling and layer peeling, so MCM-22(P) molecular sieve has good modification potential.

[0006] The template agents for direct induction synthesis of MWW molecular sieves generally include hexamethyleneimine, piperidine, and homopiperazine. Among them, hexamethyleneimine is the most widely used, but it has the disadvantages of being easily volatile, flammable, and highly toxic. Piperidine is a chemical that is prone to producing toxic substances and is difficult to obtain. Homopiperazine is expensive and difficult to apply. Therefore, it is very important to develop a cheap and green method for synthesizing MWW molecular sieves.

[0007] In [Synthesis and Application Research of MCM-22 Molecular Sieve [D]. Dalian. Dalian Institute of Chemical Physics, Chinese Academy of Sciences. 2006.], hexamethyleneimine and cyclohexylamine were used as double template agents to synthesize MCM-22 molecular sieve, effectively reducing the amount of hexamethyleneimine used. CN02145233.4 discloses a method for synthesizing MCM-22 molecular sieve by using pentamethyleneimine, hexamethyleneimine or heptamethyleneimine as template agent and recycling the mother liquor, effectively reducing the amount of template agent used. CN201310538868.2 discloses a method for synthesizing MCM-22 molecular sieve by using hexamethyleneimine and cyclohexylamine as double template agents. CN201110216909.7 discloses a method for synthesizing MCM-22 family molecular sieves using acidified hexamethyleneimine template agent and refluxing the template agent. [Microporous and Mesoporous Materials.2019, 276:192-200.] realized the induction synthesis of MCM-49 molecular sieves in cooperation with seed crystals and cyclohexylamine, but due to the special nature of MWW structure molecular sieves, it was found that the synthesis could not be achieved directly using seed crystals. By adding seed crystals and then cyclohexylamine, it was possible to support the 10-membered ring channel to construct a complete MCM-49 molecular sieve, but the hydrogen bond spacing between the basic layers could not be achieved. Until now, there has been no precedent for synthesizing MCM-22 molecular sieves without using hexamethyleneimine, piperidine, or homopiperazine, so the preparation of MCM-22 inevitably had problems caused by the template agent. Summary of the Invention

[0008] In order to solve the above technical problems, the present invention provides a solid acid alkylation catalyst and its preparation method and use, which is a method of using seed crystals and two kinds of template agents in cooperation to assist crystallization, without using hexamethyleneimine, piperidine, or homopiperazine, to directly synthesize MWW molecular sieve, and then obtain a solid acid alkylation catalyst. S1: mixing an aluminum source, water, an alkali source, a template agent, a silicon source and a seed crystal to form a gel, and then carrying out a crystallization reaction to obtain an MWW molecular sieve; S2: calcining the MWW molecular sieve obtained in S1 to remove the template, then carrying out ammonium exchange and calcining again to obtain H-type molecular sieve; S3: Mixing the H-type molecular sieve obtained in S2 with inorganic oxide and inorganic acid solution, kneading and shaping, drying and calcining to obtain a solid acid alkylation catalyst; A method for producing a solid acid alkylation catalyst, comprising: The template agent is composed of a main template agent and a sub-template agent in a molar ratio of 0.5-20:1. The main template agent is cyclohexylamine, and the sub-template agent is diisopropylamine, di-n-butylamine, diisobutylamine, 1,4-diazabicyclo[2.2.2]octane, 1,6-hexanediamine, N,N,N,N-tetramethyl-1,6-hexanediamine (CAS No. 111-18-2, molecular formula C 10 H 24 N 2 The present invention provides a method for producing a solid acid alkylation catalyst comprising at least one of:

[0009] In the manufacturing method of the present invention, both the main template agent and the sub-template agent are low-toxicity and inexpensive organic amines. Here, the main template agent can cooperate with the seed crystal to realize the construction of the molecular sieve base layer structure, and the sub-template agent can be a catalyst in which the N atom is sp 3 Hybrid aliphatic amines are used, and the nitrogen atom sp 3 The hybrid orbital forms interlayer hydrogen bonds with the silanol groups on the surface of the single-layer structure through the vacant orbital holes, and the process of forming hydrogen bonds does not affect the overall crystallization effect of the molecular sieve. Therefore, in some embodiments, the MWW molecular sieve obtained by the above preparation method has interlayer hydrogen bonds formed between the silanol groups and the subtemplate agent.

[0010] The production method of the present invention can synthesize a molecular sieve having an MWW structure having hydrogen bonds between layers without using hexamethyleneimine, piperidine, or homopiperazine, by utilizing the synergistic effects of the main template agent, sub-template agent, and seed crystals.

[0011] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably, in the gel of S1, SiO 2 and Al 2 O 3 the molar ratio of the aluminum source as an alkali metal oxide to the template agent is 1:0.005-0.05:0.03-0.50:0.1-0.75; Seed crystals on a dry basis and SiO 2 The mass ratio of the silicon source to the silicon oxide is 0.01-0.25:1.

[0012] In the above-mentioned method for preparing a solid acid alkylation catalyst, preferably, in S1, the seed crystal is a molecular sieve having an MWW topology structure.

[0013] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably in S1, the seed crystals include MCM-22 molecular sieve or MCM-49 molecular sieve from which a template agent has not been removed. The seed crystals preferably include MCM-22 molecular sieve from which a template agent has not been removed, and the molecular sieve has interlayer hydrogen bonds. The use of the seed crystals in the above-mentioned production process is advantageous for obtaining a molecular sieve with an MWW structure having interlayer hydrogen bonds and similar to the MCM-22 molecular sieve structure.

[0014] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably, in S1, the silicon source includes at least one of silica sol, solid silica gel, white carbon, and water glass.

[0015] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably, in S1, the alkali source includes sodium hydroxide and / or potassium hydroxide.

[0016] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably, in S1, the aluminum source includes at least one of sodium metaaluminate, aluminum sulfate, aluminum oxide, and pseudoboehmite.

[0017] In the above-mentioned method for preparing a solid acid alkylation catalyst, preferably, in S1, the crystallization reaction is carried out at a temperature of 120-170° C. for a reaction time of 12-120 h.

[0018] In the above-mentioned method for preparing a solid acid alkylation catalyst, preferably, S1 specifically includes the steps of mixing an aluminum source, water, an alkali source, a main template agent, and a sub-template agent to obtain an intermediate solution, slowly adding a silicon source to the intermediate solution and mixing uniformly, and then adding seed crystals and mixing to form a gel, and carrying out a crystallization reaction to obtain the MWW molecular sieve. The above-mentioned order of synthesis is advantageous for uniform dispersion of each raw material and promotion of crystallization reaction. The main template agent and the sub-template agent are added after the aluminum source, which contributes to the aluminum source being completely dissolved and uniformly dispersed in the solution. The seed crystals are added after the silicon source is slowly added, which improves the uniformity and stability of the reaction system, and avoids the problem of the silicon source being rapidly added and then forming a colloid with the aluminum source, which causes the reaction system to be non-uniformly dispersed.

[0019] The MWW molecular sieve obtained in the present invention S1 has interlayer hydrogen bonds and is similar to the structure of MCM-22 molecular sieve when it is not calcined (the template agent is not removed), so it can be regarded as a precursor of MCM-22 molecular sieve (which can be written as MCM-22(P) molecular sieve). The MWW molecular sieve of the present invention has good modification potential, for example, it can produce MCM-36 molecular sieve through swelling and column support, and ITQ-2 molecular sieve through swelling and layer peeling. The present invention's research has found that MCM-49 molecular sieve does not have interlayer hydrogen bonds and cannot be swollen and peeled, while MCM-22 molecular sieve prepared using a normal template agent (hexamethyleneimine) and MWW molecular sieve provided by the present invention both have interlayer hydrogen bonds, so these two molecular sieves both have the ability of swelling and layer peeling. Compared with the MCM-22 molecular sieve prepared by the conventional template agent (hexamethyleneimine), the MWW molecular sieve provided by the present invention is less difficult to peel off, specifically, the pH of the alkaline environment required for peeling is closer to neutral, which indicates that the interlayer hydrogen bond strength of the MWW molecular sieve provided by the present invention is more suitable than that of the MCM-22 molecular sieve. When the molecular sieve is column-supported or peeled off, it is more advantageous to maintain the integrity of the molecular sieve sheet crystal structure, improve the stability of the molecular sieve, and reduce the loss of catalytic active sites, and therefore it is advantageous to improve the catalytic activity and stability when the molecular sieve is applied to reactions such as alkylation, isomerization, or cracking.

[0020] In the above-mentioned method for preparing a solid acid alkylation catalyst, preferably, in S2, the two calcinations are each carried out in an air atmosphere, the calcination temperature is independently 490-590° C., and the calcination time is independently 0.5-72 h.

[0021] In the above-mentioned method for preparing a solid acid alkylation catalyst, preferably, in S2, the ammonium exchange is carried out in an ammonium nitrate solution, the concentration of the ammonium nitrate solution is 0.1-10 mol / L, the ammonium exchange temperature is 30-120° C., and the ammonium exchange time is 0.5-72 h.

[0022] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably, in S3, the mass ratio of the H-type molecular sieve to the inorganic oxide is 10-95:5-90.

[0023] In the above-mentioned method for producing a solid acid alkylation catalyst, the inorganic oxide in S3 preferably includes at least one of aluminum oxide, pseudoboehmite, boehmite, and aluminum hydroxide.

[0024] In the above-mentioned method for producing a solid acid alkylation catalyst, preferably, in S3, the inorganic acid solution includes at least one of a nitric acid solution, a phosphoric acid solution, a hydrochloric acid solution, and a sulfuric acid solution. In the present invention, the inorganic acid solution is used to emulsify an inorganic oxide to form a binder.

[0025] In the above-mentioned method for preparing a solid acid alkylation catalyst, preferably, in S3, the calcination is carried out in an air atmosphere, the calcination temperature is 490-590° C., and the calcination time is 0.5-72 h.

[0026] The present invention also provides a solid acid alkylation catalyst obtained by the above-mentioned method for producing a solid acid alkylation catalyst.

[0027] The present invention also provides use of the solid acid alkylation catalyst obtained by the above-mentioned method for producing a solid acid alkylation catalyst in the alkylation reaction of an aromatic hydrocarbon with an olefin.

[0028] In the above use, the aromatic hydrocarbon is preferably at least one selected from benzene, alkylbenzene, naphthalene, alkylnaphthalene, anthracene, and alkylanthracene, and more preferably at least one selected from benzene, alkylbenzene, naphthalene, and anthracene.

[0029] In the above uses, the olefin is preferably selected from olefins having 2 to 20 carbon atoms, more preferably selected from olefins having 2 to 15 carbon atoms.

[0030] In the above use, the alkylation reaction conditions are preferably: reaction temperature 100-385°C, reaction pressure 0.5-7MPa, mass space velocity 0.1-12h -1 More preferably, the alkylation reaction conditions are a reaction temperature of 120-350° C., a reaction pressure of 0.5-5 MPa, and a mass space velocity of 0.5-10 h -1 This includes being.

[0031] In the above use, the molar ratio of the aromatic hydrocarbon to the olefin is preferably 0.05-200.

[0032] The technical solution provided in the present invention has the following beneficial effects:

[0033] (1) In the solid acid alkylation catalyst provided by the present invention, the catalytically active component H-type molecular sieve is prepared by ammonium exchange from the MWW structure molecular sieve, and the MWW structure molecular sieve realizes the construction of a basic layer structure by the seed crystal and the main template agent, and realizes the construction of interlayer hydrogen bonds by the sub-template agent, and has properties similar to those of MCM-22(P) molecular sieve; (2) The main template agent and the sub-template agent used in the present invention are both organic amines with low toxicity and easy availability, which are low in cost, do not use highly toxic and easily toxic template agents such as hexamethyleneimine, piperidine, homopiperazine, etc., and are low in cost, which reduces the pollution and cost of the preparation method of the solid acid alkylation catalyst, and the obtained solid acid alkylation catalyst has high alkylation catalytic activity and product selectivity, which can greatly improve the operability of the production of MWW molecular sieves, and is of great practical significance. [Brief description of the drawings]

[0034] [Figure 1] 1 is an XRD pattern of a seed crystal. [Diagram 2] This is an SEM image of a seed crystal. [Diagram 3] 1 is an XRD pattern of the MWW molecular sieve synthesized in Example 1. [Figure 4] 1 is a SEM image of the MWW molecular sieve synthesized in Example 1. [Diagram 5] 1 is an XRD pattern of the MWW molecular sieve synthesized in Example 2. [Figure 6] 1 is a SEM image of the MWW molecular sieve synthesized in Example 2. [Figure 7] 1 is an XRD pattern of the molecular sieve synthesized in Comparative Example 1. [Figure 8] 1 is a SEM image of the molecular sieve synthesized in Comparative Example 1. [Figure 9] 1 is an XRD pattern of the molecular sieve synthesized in Comparative Example 3. [Figure 10] 1 is a SEM image of the molecular sieve synthesized in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] In order to make the technical requirements, objectives and beneficial effects of the present invention more clearly understood, the technical solutions of the present invention are described in detail below, but should not be understood as limiting the possible scope of the present invention.

[0036] The raw materials used in the examples of the present invention are as follows.

[0037] Silicon source: Silica sol (SiO 2 content 40%), solid silica gel (SiO 2 Content 95%), White Carbon Black (SiO 2 content 93%), ethyl orthosilicate (purity 98%), Aluminum source: sodium metaaluminate (Al 2 O 3 content 41%), aluminum sulfate (Al 2 O 3 content 15%), aluminum oxide (95%), pseudoboehmite (Al 2 O 3 content 70%), Alkaline source: Sodium hydroxide (99% purity), Potassium hydroxide (99% purity), Main template agent: cyclohexylamine (purity 99%), Subtemplate agent: Diisopropylamine (99% purity), di-n-butylamine (99% purity), diisobutylamine (99% purity), 1,4-diazabicyclo[2.2.2]octane (99% purity), 1,6-hexanediamine (99% purity), N,N,N,N-tetramethyl-1,6-hexanediamine (99% purity), Seed crystal: MCM-22 molecular sieve manufactured by Mobil Corp. The molecular sieve was not calcined to remove the template, and the XRD pattern and SEM image of the surface are shown in Figures 1 and 2, respectively.

[0038] Other: Deionized water.

[0039] The present invention will now be described with reference to specific embodiments and drawings.

[0040] Example 1 This embodiment provides a MWW structure molecular sieve, the preparation method of which is as follows:

[0041] 1.87 g of sodium hydroxide was added to 120 g of deionized water and stirred to dissolve. 2.15 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 9.50 g of cyclohexylamine was added slowly and stirring was continued vigorously for 0.5 h. 6.50 g of diisopropylamine was added slowly and stirring was continued vigorously for 0.5 h. 80 g of silica sol was added slowly and stirring was continued vigorously for 3 h. Available SiO in silica sol 2 Seed crystals were added in an amount of 3% of the mass, and the mixture was stirred vigorously for 1 hour to prepare a crystallized gel. The crystallized gel was crystallized at 140°C for 60 hours. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and dried at 120°C for 4 hours to obtain a MWW molecular sieve.

[0042] The MWW molecular sieve obtained in this example was analyzed by X-ray diffraction (XRD) and scanning electron microscope (SEM). As shown in Figures 3 and 4, the XRD pattern and SEM image of the MWW molecular sieve were typical peaks characteristic of the MWW structure, and the molecular sieve morphology was a flower cluster of nanosheets.

[0043] The MWW molecular sieve obtained in this example was calcined in an air atmosphere at 540° C., and then the specific surface area and pore size (BET) analysis evaluation were performed. The BET test results are shown in Table 1. In Table 1, S BET is the specific surface area, S mic is the micropore surface area, S ext is the mesopore surface area, V pore is the pore volume, V mic is the micropore volume.

[0044] Example 2 This embodiment provides a MWW structure molecular sieve, the preparation method of which is as follows:

[0045] 1.87 g of sodium hydroxide was added to 120 g of deionized water and stirred to dissolve. 2.50 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 9.00 g of cyclohexylamine was slowly added and stirring was continued vigorously for 0.5 h. 8.00 g of 1,6-hexadiamine was slowly added and stirring was continued vigorously for 0.5 h. 80 g of silica sol was slowly added and stirring was continued vigorously for 3 h. Available SiO in silica sol 2 Seed crystals were added in an amount of 5% of the mass, and the mixture was stirred vigorously for 1 hour to prepare a crystallized gel. The crystallized gel was crystallized at 145°C for 72 hours. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and dried at 120°C for 4 hours to obtain a MWW molecular sieve.

[0046] The MWW molecular sieve obtained in this example was subjected to XRD and SEM analysis. The XRD pattern and SEM image are shown in Fig. 5 and Fig. 6, respectively. The MWW molecular sieve has a typical MWW structure characteristic peak, and the molecular sieve morphology is a flower cluster formed by the accumulation of nanosheets.

[0047] The MWW molecular sieve obtained in this example was calcined in an air atmosphere at 540° C., and then subjected to BET analysis evaluation. The BET test results are shown in Table 1.

[0048] Example 3 This embodiment provides a MWW structure molecular sieve, the preparation method of which is as follows:

[0049] 1.95 g of sodium hydroxide was added to 130 g of deionized water and stirred to dissolve. 2.33 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 9.00 g of cyclohexylamine was added slowly and stirred vigorously for 0.5 h. 9.00 g of 1,4-diazabicyclo[2.2.2]octane was added slowly and stirred vigorously for 0.5 h. 80 g of silica sol was added slowly and stirred vigorously for 3 h. Available SiO in silica sol 2Seed crystals were added in an amount of 5% of the mass, and the mixture was stirred vigorously for 1 hour to prepare a crystallized gel. The crystallized gel was crystallized at 140°C for 72 hours. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and naturally dried in the shade for 48 hours to obtain a MWW molecular sieve.

[0050] The product obtained in this example was analyzed by XRD, SEM and BET (after calcination in air at 540℃), and it was found to have typical MWW structure peaks and the molecular sieve morphology was a flower cluster of nanosheets. The BET test results are shown in Table 1.

[0051] Example 4 This embodiment provides a MWW structure molecular sieve, the preparation method of which is as follows:

[0052] 1.93 g of sodium hydroxide was added to 150 g of deionized water and stirred to dissolve. 1.50 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 12.25 g of cyclohexylamine was added slowly and stirring was continued vigorously for 0.5 h. 8.50 g of N,N,N,N-tetramethyl-1,6-hexanediamine was added slowly and stirring was continued vigorously for 0.5 h. 80 g of silica sol was added slowly and stirring was continued vigorously for 3 h. Available SiO in silica sol 2 Seed crystals were added in an amount of 10% of the mass, and the mixture was stirred vigorously for 1 hour to prepare a crystallized gel. The crystallized gel was crystallized at 140°C for 100 hours. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and dried at 120°C for 4 hours to obtain a MWW molecular sieve.

[0053] The product obtained in this example was analyzed and evaluated by XRD, SEM, and BET (after calcination in an air atmosphere at 540°C), and it was found to have typical MWW structure characteristic peaks and the molecular sieve morphology was a flower cluster formed by the accumulation of nanosheets.

[0054] Example 5 This embodiment provides a MWW structure molecular sieve, the preparation method of which is as follows:

[0055] 2.21 g of sodium hydroxide was added to 175 g of deionized water and stirred to dissolve. 1.25 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 7.55 g of cyclohexylamine was added slowly and stirring was continued vigorously for 0.5 h. 10.50 g of diisobutylamine was added slowly and stirring was continued vigorously for 0.5 h. 80 g of silica sol was added slowly and stirring was continued vigorously for 3 h. Available SiO in silica sol 2 Seed crystals were added in an amount of 15% of the mass, and the mixture was stirred vigorously for 1 hour to prepare a crystallized gel. The crystallized gel was crystallized at 140°C for 120 hours. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and naturally dried in the shade for 48 hours to obtain a MWW molecular sieve.

[0056] The product obtained in this example was analyzed by XRD, SEM and BET (after calcination in air at 540℃), and it was found to have typical MWW structure peaks and the molecular sieve morphology was a flower cluster of nanosheets. The BET test results are shown in Table 1.

[0057] Example 6 This embodiment provides a solid acid alkylation catalyst, the preparation method of which is as follows:

[0058] The MWW molecular sieve product of Example 1 was taken, and calcined at 540°C for 5h in air to remove the template, and then ammonium-exchanged in 1mol / L ammonium nitrate solution at 80°C for 2h, and calcined again at 540°C for 4h in air to obtain H-type molecular sieve. 90g of the above H-type molecular sieve and 15g of pseudo-boehmite were mixed uniformly, and 55g of nitric acid solution was slowly added while kneading, and the mixture was band extrusion molded into a cylindrical catalyst with a diameter of 2.0 mm, and then cut into a cylindrical catalyst with a length of 2.5 mm. The catalyst was dried at room temperature for 24 hours, and then calcined at 550℃ for 6 hours to obtain the finished solid acid alkylation catalyst.

[0059] The solid acid alkylation catalyst obtained in this example was applied to the catalytic action of the alkylation reaction of aromatic hydrocarbons with olefins, specifically as follows.

[0060] 2 g of the above solid acid alkylation catalyst was taken and placed in a fixed-bed reactor, and a mixture of benzene and ethylene was introduced. The alkylation reaction conditions were: benzene to ethylene molar ratio 5, reaction temperature 330°C, reaction pressure 1.4 MPa, mass space velocity 2.0 h -1 It was.

[0061] As a result of the reaction, after 500 hours of reaction, the ethylene conversion was 99.99% and the ethylbenzene selectivity was 96.21%.

[0062] Example 7 This embodiment provides a solid acid alkylation catalyst, the preparation method of which is as follows:

[0063] The MWW molecular sieve product of Example 2 was taken, and calcined at 540°C for 5h in air to remove the template, and then ammonium-exchanged in 1mol / L ammonium nitrate solution at 80°C for 2h, and calcined again at 540°C for 4h in air to obtain H-type molecular sieve.

[0064] 90g of the above H-type molecular sieve and 15g of pseudo-boehmite were mixed uniformly, and 55g of nitric acid solution was slowly added while kneading, and the mixture was band extrusion molded into a cylindrical catalyst with a diameter of 2.0 mm, and then cut into a cylindrical catalyst with a length of 2.5 mm. The catalyst was dried at room temperature for 24 hours, and then calcined at 550℃ for 6 hours to obtain the finished solid acid alkylation catalyst.

[0065] The solid acid alkylation catalyst obtained in this example was applied to the catalytic action of the alkylation reaction of aromatic hydrocarbons with olefins, specifically as follows.

[0066] 2 g of the above solid acid alkylation catalyst was taken and placed in a fixed-bed reactor, and a mixture of benzene and propylene was introduced. The reaction conditions were: benzene to propylene molar ratio 4, reaction temperature 150°C, reaction pressure 2.5 MPa, mass space velocity 3.0 h -1 It was.

[0067] As a result of the reaction, after 300 hours of reaction, the propylene conversion was 99.97% and the isopropylbenzene selectivity was 99.20%.

[0068] Example 8 This embodiment provides a solid acid alkylation catalyst, the preparation method of which is as follows:

[0069] The MWW molecular sieve product of Example 3 was taken, and calcined at 540°C for 5h in air to remove the template, and then ammonium-exchanged in 1mol / L ammonium nitrate solution at 80°C for 2h, and calcined again at 540°C for 4h in air to obtain H-type molecular sieve.

[0070] 90g of the above H-type molecular sieve and 15g of pseudo-boehmite were mixed uniformly, and 55g of nitric acid solution was slowly added while kneading, and the mixture was band extrusion molded into a φ2.0mm cylindrical catalyst, which was then cut into a 2.5mm cylindrical catalyst. The cylindrical catalyst was dried at room temperature for 24h, and then calcined at 550℃ for 6h to obtain the finished solid acid alkylation catalyst.

[0071] The solid acid alkylation catalyst obtained in this example was applied to the catalytic action of the alkylation reaction of aromatic hydrocarbons with olefins, specifically as follows.

[0072] 2 g of the above solid acid alkylation catalyst was taken and placed in a fixed-bed reactor, and a mixture of benzene and n-dodecene was introduced. The reaction conditions were: benzene to n-dodecene molar ratio 15, reaction temperature 150°C, reaction pressure 3.0 MPa, mass space velocity 2.0 h -1 It was.

[0073] As a result of the reaction, after 300 hours of reaction, the n-dodecene conversion was 99.97% and the 2-alkylbenzene selectivity was 42.01%.

[0074] Comparative Example 1 This comparative example provides a molecular sieve, the preparation method of which is as follows:

[0075] 1.95 g of sodium hydroxide was added to 130 g of deionized water and stirred to dissolve. 2.33 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 9.00 g of cyclohexylamine was added slowly and stirring was continued vigorously for 0.5 h. 80 g of silica sol was added slowly and stirring was continued vigorously for 3 h. Available SiO in silica sol 2 The amount of seed crystals added is 5% by mass of the available SiO in the silica sol. 2 The mixture was 5% by mass and stirred vigorously for 1 hour. A crystallized gel was prepared. The crystallized gel was crystallized at 140°C for 72 hours. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and naturally dried in the shade for 48 hours to obtain a molecular sieve.

[0076] The molecular sieve obtained in this comparative example was subjected to XRD and SEM analysis evaluation. As a result, the XRD pattern and SEM image, as shown in Figures 7 and 8, respectively, showed that the molecular sieve had a characteristic peak of a typical MWW structure, and could be subdivided into MCM-49 molecular sieves, and the morphology of the molecular sieve was a regular accumulation of nanosheets.

[0077] The molecular sieve obtained in this comparative example was calcined in an air atmosphere at 540° C., and then subjected to BET analysis evaluation. The BET test results are shown in Table 1.

[0078] Based on the test results, comparing Comparative Example 1 with Example 3, when seed crystals and cyclohexylamine are used as template agents, a pure MWW molecular sieve with high crystallinity can be directly synthesized and can be subdivided into MCM-49 molecular sieve. However, since cyclohexylamine cannot form interlayer hydrogen bonds, this method can only be applied to the synthesis of MAM-49 molecular sieve and cannot synthesize other kinds of MWW molecular sieves. [Table 1]

[0079] On the other hand, in Example 1, diisopropylamine was added, so the nitrogen atom sp 3 The hybridized electron holes and the hydrogen in the interlayer silanol groups formed hydrogen bonds, which made the molecular sieve product more similar to the properties of MCM-22(P) molecular sieve, reduced the number of depositions of the basic layer, reduced the thickness of the molecular sieve sheet layer, increased the total surface area and external surface area, and changed the deposition morphology of the molecular sieve.

[0080] Comparative Example 2 This comparative example provides a catalyst made from the molecular sieve of Comparative Example 1, and its preparation method is as follows:

[0081] The molecular sieve of Comparative Example 1 was calcined at 540°C for 5 h in an air atmosphere to remove the template, and then ammonium-exchanged in a 1 mol / L ammonium nitrate solution at 80°C for 2 h, and calcined again at 540°C for 4 h in an air atmosphere to obtain an H-type molecular sieve.

[0082] 90g of the above H-type molecular sieve and 15g of pseudo-boehmite were mixed uniformly, and 55g of nitric acid solution was slowly added while kneading, and the mixture was band extrusion molded into a φ2.0mm cylindrical catalyst, which was then cut into a 2.5mm cylindrical catalyst. The cylindrical catalyst was dried in the shade at room temperature for 24 hours, and then calcined at 550℃ for 6 hours to obtain a finished catalyst.

[0083] The solid acid alkylation catalyst obtained in this comparative example was applied to the catalyst for the alkylation reaction of aromatic hydrocarbons with olefins, as follows.

[0084] 2 g of the above catalyst was taken and placed in a fixed-bed reactor, and a mixture of benzene and n-dodecene was introduced. The reaction conditions were: benzene to n-dodecene molar ratio 15, reaction temperature 150°C, reaction pressure 3.0 MPa, mass space velocity 2.0 h -1 As a result of the reaction, after 100 hours of reaction, the olefin conversion was 76.32% and the 2-alkylbenzene selectivity was 45.03%.

[0085] Comparing Comparative Example 2 with Example 8, when the MCM-49 molecular sieve was used to prepare an alkylation catalyst for the reaction of benzene with n-dodecane, the thickness of the molecular sieve was larger than that of the MCM-22 molecular sieve, so that the number of surface catalytic active sites exposed per unit mass of catalyst was reduced, and the catalyst was blocked and inactivated more quickly during the reaction, shortening the catalyst life.

[0086] Comparative Example 3 This comparative example provides a molecular sieve, the preparation method of which is as follows:

[0087] 1.87 g of sodium hydroxide was added to 120 g of deionized water and stirred to dissolve. 2.15 g of sodium metaaluminate was added and stirred to dissolve. Stirring was continued vigorously for 1 h. 19.0 g of hexamethyleneimine was slowly added and stirring was continued vigorously for 0.5 h to obtain an intermediate solution.

[0088] 80g of silica sol was slowly added to the intermediate solution and stirred vigorously for 3h to prepare a crystallized gel. The crystallized gel was crystallized at 155℃ for 60h. After the crystallization was completed, the temperature was lowered to room temperature. The product was washed with deionized water, filtered, and dried at 120℃ for 4h to obtain a molecular sieve product.

[0089] The molecular sieve obtained in this comparative example was subjected to XRD and SEM analysis. The XRD pattern and SEM image are shown in Figures 9 and 10, respectively. The molecular sieve product had a typical MWW structure characteristic peak and could be subdivided into MCM-22 molecular sieve, and the molecular sieve morphology was nanosheet stacked.

[0090] The hexamethyleneimine used in this comparative example is a typical template agent for preparing MCM-22 molecular sieve. This method can obtain pure MCM-22 molecular sieve, but the template agent is used in a large amount, and the template agent is expensive and highly toxic.

[0091] Comparing the XRD results of the molecular sieve products of Examples 1-5 with those of Comparative Example 3, it can be seen that the molecular sieves of Examples 1-5 have a structure similar to that of MCM-22 molecular sieve, which further proves that the molecular sieve prepared by the present invention S1 has interlayer hydrogen bonds.

Claims

1. S1: mixing an aluminum source, water, an alkali source, a template agent, a silicon source and a seed crystal to form a gel, and then carrying out a crystallization reaction to obtain a MWW-structure molecular sieve; S2: calcining the MWW molecular sieve obtained in S1 to remove the template, then carrying out ammonium exchange and calcining again to obtain an H-type molecular sieve; S3: Mixing the H-type molecular sieve obtained in S2 with an inorganic oxide and an inorganic acid solution, kneading and shaping the mixture, drying and calcining the mixture to obtain a solid acid alkylation catalyst; A method for producing a solid acid alkylation catalyst, comprising: The template agent comprises a main template agent and a sub-template agent in a molar ratio of 0.5-20:1, the main template agent being cyclohexylamine, and the sub-template agent being at least one of diisopropylamine, di-n-butylamine, diisobutylamine, 1,4-diazabicyclo[2.2.2]octane, 1,6-hexanediamine, and N,N,N,N-tetramethyl-1,6-hexanediamine.

2. In the gel of S1, SiO 2 and a silicon source as Al. 2 O 3 the molar ratio of the aluminum source as an alkali metal oxide to the template agent is 1:0.005-0.05:0.03-0.50:0.1-0.75; Seed crystals on a dry basis and SiO 2 2. The method for producing a solid acid alkylation catalyst according to claim 1, wherein the mass ratio of the silicon source to the catalyst is 0.01-0.25:

1.

3. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S1, the seed crystal is a molecular sieve having a MWW topology structure.

4. 2. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S1, the seed crystals comprise unremoved MCM-22 molecular sieve or MCM-49 molecular sieve, preferably unremoved MCM-22 molecular sieve.

5. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S1, the silicon source comprises at least one of silica sol, solid silica gel, white carbon, and water glass.

6. The method for producing a solid acid alkylation catalyst according to claim 1, wherein in S1, the alkali source comprises sodium hydroxide and / or potassium hydroxide.

7. The method for producing a solid acid alkylation catalyst according to claim 1, wherein in S1, the aluminum source comprises at least one of sodium metaaluminate, aluminum sulfate, aluminum oxide, and pseudoboehmite.

8. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S1, the crystallization reaction is carried out at a temperature of 120-170° C. for a reaction time of 12-120 h.

9. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S2, the two calcinations are each carried out under an air atmosphere, the calcination temperature is independently 490-590° C., and the calcination time is independently 0.5-72 h.

10. 2. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S2, the ammonium exchange is carried out in an ammonium nitrate solution, the concentration of the ammonium nitrate solution is 0.1-10 mol / L, the ammonium exchange temperature is 30-120° C., and the ammonium exchange time is 0.5-72 h.

11. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S3, the mass ratio of the H-type molecular sieve to the inorganic oxide is 10-95:5-90.

12. In S3, the inorganic oxide includes at least one of aluminum oxide, pseudoboehmite, boehmite, and aluminum hydroxide; The method for preparing a solid acid alkylation catalyst according to claim 1, wherein the inorganic acid solution preferably comprises at least one of a nitric acid solution, a phosphoric acid solution, a hydrochloric acid solution, and a sulfuric acid solution.

13. The method for preparing a solid acid alkylation catalyst according to claim 1, wherein in S3, the calcination is carried out under an air atmosphere, the calcination temperature is 490-590° C., and the calcination time is 0.5-72 h.

14. A solid acid alkylation catalyst obtained by the method for producing a solid acid alkylation catalyst according to any one of claims 1 to 13.

15. Use of a solid acid alkylation catalyst obtained by the method for producing a solid acid alkylation catalyst according to any one of claims 1 to 13 in an alkylation reaction of an aromatic hydrocarbon with an olefin.

16. 16. The use according to claim 15, wherein the aromatic hydrocarbon is at least one selected from benzene, alkylbenzene, naphthalene, alkylnaphthalene, anthracene, alkylanthracene, preferably at least one of benzene, alkylbenzene, naphthalene, anthracene.

17. The use according to claim 15, wherein the olefin is selected from olefins having 2 to 20 carbon atoms, preferably from olefins having 2 to 15 carbon atoms.

18. The alkylation reaction conditions are: reaction temperature 100-385°C, reaction pressure 0.5-7MPa, mass space velocity 0.1-12h -1 The use according to claim 15, comprising

19. The alkylation reaction conditions are: reaction temperature 120-350°C, reaction pressure 0.5-5MPa, mass space velocity 0.5-10h -1 The use according to claim 18, comprising

20. The use according to claim 15, wherein the molar ratio of the aromatic hydrocarbon to the olefin is 0.05-200.

Citation Information

Patent Citations

  • A method of synthesizing a MWW-structure molecular sieve

    CN105439166A

  • Single-layer MWW molecular sieve as well as preparation method and application thereof

    CN112551539A

  • Treatment of acid catalysts

    US20030004056A1

  • Rejuvenating deactivated molecular sieve

    US20080015402A1

Cited By

  • Solid acid catalyst for Friedel-Crafts reaction as well as preparation method and application of solid acid catalyst