Electrical Wire and Cable for Space Applications

JP2024513982A5Inactive Publication Date: 2024-10-25AXON CABLE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023562799
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-04-13
Filing Date
2022-04-11
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing manufacturing processes for silver-plated copper or copper alloy conductors used in space applications suffer from degradation of the silver coating due to thermal and mechanical stresses, leading to poor performance in oxidation and corrosion resistance tests like the A&B test and polysulfide test.

Method used

The process involves electrolytic deposition of silver using pulsed current with reversal (PCR) to optimize nucleation and growth of the silver layer, ensuring a uniform and dense coating, which is then subjected to controlled conditions to enhance resistance to oxidation and corrosion.

Benefits of technology

The resulting silver-plated conductors exhibit improved resistance to oxidation and corrosion, achieving better performance in A&B tests and polysulfide tests, even with reduced silver layer thickness, thus meeting the stringent requirements of space applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to a process for producing a silver-plated copper or copper alloy blank wire having a silver layer thickness of 1.5 μm to 15 μm, comprising a step of electrolytic deposition of silver on a copper or copper alloy blank wire, the electrolytic deposition being carried out in a silver plating bath under specific electrolytic conditions with a pulsed current with reversal. The invention also relates to a silver-plated copper or copper alloy blank wire obtainable by said process, a process for producing a silver-plated copper or copper alloy strand, a strand obtainable by said process, a silver-plated conductor and an electromagnetic shielding layer comprising a silver-plated strand, an electric wire comprising a silver-plated conductor, and an electric cable comprising an electric wire, and uses thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to electrical wires and cables including copper or copper alloy conductors coated with a silver layer and having enhanced oxidation and corrosion resistance. In particular, these wires and cables may be used for space applications. [Background technology]

[0002] ESCC (European Space Components Coordination) standard N3901 (May 2013) specifies electrical wire and cable types for space applications.

[0003] These wires and cables are hereinafter referred to as SPC wires and cables because either the central core or the electromagnetic shield is made of a copper or copper alloy conductor coated with a silver layer, hereinafter referred to as an SPC (Silver-plated Copper) conductor.

[0004] In order to classify electrical conductors according to their section, the standardization practice of AWG (American Wire Gauge) has been established in the ASTM B258 standard (April 2002). This standard clearly defines how conductors are constructed in terms of the number of strands. The SPC conductor of the present invention also complies with this standard.

[0005] Unlike the primary applications where SPC conductors are coated with a minimum of 1 μm of silver according to the ASTM B298 standard (December 2017), the ESCC-3901 standard also specifies a minimum silver coating thickness of 2 μm for all SPC conductors. The reason for this doubling of the silver thickness is related to the requirements of space applications where protection of electrical and electronic systems against corrosion is crucial.

[0006] For that reason, the ESCC-3901 standard imposes the Antony & Brown control test, hereafter referred to as the A&B test, on the SPC conductors contained in SPC wires and cables to guarantee the quality of the silver coating. As subject to the ECSS-Q-ST-70-20C standard (July 2008), this A&B test is essentially a corrosion test to determine the level of resistance of the SPC conductors to the so-called “red plague” corrosion, which can be interpreted as the oxidation of copper. As detailed in the standard, in this test, a 20 mm sample of the SPC conductor, from which the insulation has been removed, is placed in a container where a high-oxygen atmosphere is permeated with a continuous oxygen flow. The assembly is exposed to a temperature of 58°C for 240 hours, i.e. 10 full days. After this test, a microscopic examination is performed at 20x magnification and the oxidation state of the sample is determined by assigning it a code setting of six levels, as set forth in Table 1 below.

[0007] [Table 1]

[0008] The standard imposes strict sanctions on any sample of code 4 and 5, in other words having severe defects of corrosion due to oxidation of copper or copper alloys.

[0009] Given the duration of the A&B test, in practice another test is used, called polysulfide, which is shorter in duration so that control tests can be carried out during the manufacture of the SPC conductor. The polysulfide test, subject of the ISO 10308 standard (January 2006), consists of immersing the SPC conductor in a sodium polysulfide solution for 30 seconds, followed by rinsing and drying it. An examination with a binocular microscope (un examen binoculaire) is then carried out at a magnification of 10 times. The test is considered good when no corrosion spots are observed on the conductor (resistance to oxidation).

[0010] The manufacture of SPC wire and cable typically involves several steps.

[0011] The first step is the electrolytic plating (or electrolytic deposition) of silver, more frequently called silvering, on round wires, called copper or copper alloy blanks. The process is continuous and is sometimes called "reel-to-reel". More precisely, several wires (plusieurs fils), as cathodes, pass through an electrolytic silvering bath, to which a pure silver anode is attached. During the process, a generator sends a direct current between the anode and the cathode. This current creates an electrolysis that, on the one hand, dissolves the silver anode and, at the same time, on the other hand, allows the deposition of a silver coating on the passing wire.

[0012] The second step is called trefilage and consists of reducing the diameter of the cold silver wire by mechanical force. A machine called a wiredrawing machine, which contains a set of 5 to 30 dies, is used to gradually reduce the diameter, as required. The drawn silver wires are called SPC strands and are used to make either SPC conductive strands or SPC electromagnetic shields (braided or spiral).

[0013] The third step, called toronnage, is the implementation of the SPC conductor itself: using a machine called a "toronnage machine", the correct number of SPC strands are assembled according to one of the construction modes specified in the ASTM B258 standard.

[0014] The fourth step, called isolation, consists of placing a layer of dielectric around the SPC conductor core to obtain an SPC electric wire. The dielectric materials used here are generally based on polytetrafluoroethylene (PTFE), ethylene tetrafluoroethylene (ETFE) and polyimide, all certified to the ESCC 3901 standard. The processing is carried out either by extrusion for PTFE and ETFE, or by taping for PTFE and polyimide in the form of tapes. In some cases, these SPC wires are coated with a thin finishing layer, sometimes called coating, based on polyimide, to give them additional functions, for example coloring. Generally, the application of a solid finishing layer is carried out with a polyimide liquid, using one or more passes in an oven at 250 ° C to 500 ° C, if necessary.

[0015] The fifth step, called assemblage, consists of twisting several electric wires (plusieurs: 2 to 4 wires) into a bundle by twisting to obtain a subset of SPC electric wires.

[0016] The sixth step, called braiding or winding, consists of implementing a layer of SPC strands around a subset of the electrical wires. This braided or wound layer, often called the shielding layer, forms a protective screen against electromagnetic interference.

[0017] The seventh step, called the gainage, makes it possible to complete the manufacture of the SPC cable by placing a protective sheath around the subset of shielded wires. The sheath materials are PTFE, ETFE, perfluoroalkoxy (PFA) and polyimide, all certified to the ESCC 3901 standard. Processing is carried out either by extrusion for PTFE, PFA and ETFE, or by taping for PTFE and polyimide in the form of a tape.

[0018] All the manufacturing steps can be summarized as follows: E1: Silver plating on copper or copper alloy base wire => Silver plated base wire E2: Pulling silver-plated wire => SPC strand E3: Assemble SPC strands => SPC conductor E4: Taping or extrusion of dielectric (ETFE, PTFE, polyimide, ...) onto SPC conductor => SPC electric wire E5: Assembling several electric wires (plusieurs) => subset E6: Braid or wrap SPC strands on subset => shielded subset E7: Armoring a shielded subset => SPC cable

[0019] It is known that these manufacturing steps, involving thermal and mechanical stresses, can affect the performance of the silver coating in A&B tests, especially when these manufacturing steps involve traction, twisting, heating, and other movements. The greater the magnitude of these processing parameters (time, force, pressure, temperature, ...), the more the degradation of the performance of the silver coating on the SPC conductors progresses.

[0020] The inventors have surprisingly found that it is possible to mitigate these degradations by modifying step E1 of the process, in other words by using electrolytic deposition of silver with pulsed current with inversion (PCR) instead of direct current (DC). Indeed, unlike electrolytic deposition with DC, where a constant electrolytic current is sent throughout the silver plating by a generator, that under PCR uses a discontinuous and modulated electrolytic current in the form of a series of cathodic pulses at a given frequency, each cathodic pulse being followed by an anodic pulse. The inventors have therefore found that electrolytic plating under PCR, when carried out under well-controlled and therefore precise conditions, can best optimize the nucleation and growth of the electrolytic deposit, and thus improve the performance of SPC conductors in A&B tests. Thus, the process according to the invention makes it possible even to reduce the thickness of the silver layer deposited on the SPC conductor to only 1 μm, while enabling the SPC conductor to have better resistance than conventional SPC conductors (whose silver layer is obtained by DC electrolytic deposition), which in A&B tests had a deposited silver layer thickness of 2 μm. Indeed, the inventors have found that the silver coating produced by PCR has a better crystallization state, being more uniform and denser. Summary of the Invention

[0021] Therefore, the present invention relates to a process for manufacturing a silver-plated copper or copper alloy blank wire having a silver layer thickness of 1.5 μm to 15 μm, advantageously 2 μm to 10 μm, comprising a step of electrolytic deposition of silver (electrolytic plating) onto a copper or copper alloy blank wire, said electrolytic deposition being carried out with pulsed current with reversal (PCR) in a silver plating bath containing 40 g / l to 70 g / l, in particular 40 g / l to 65 g / l, more particularly 45 g / l to 60 g / l silver cyanide (AgCN) and 90 g / l to 150 g / l, in particular 90 g / l to 140 g / l, more particularly 100 g / l to 130 g / l potassium cyanide (KCN), the electrolytic conditions being as follows: Average current density Jm is 1.5A / dm 2 and 15A / dm 2 between 1.78 A / dm and 1.78 A / dm 2 and 10A / dm 2 Specifically, between 1.78 A / dm 2 and 5A / dm 2 Included between the pulse frequency f is comprised between 0.8 Hz and 1.6 Hz, advantageously between 0.8 Hz and 1.4 Hz, in particular 1 Hz, a duty cycle Q between 50% and 80%, advantageously between 55% and 65%, The peak current density of the cathode, Jc, is 3A / dm 2 and 11A / dm 2 Between 5A / dm and 6A / dm 2 and 10A / dm 2 Between, and more specifically, 3A / dm 2 and 8A / dm 2 Between 5A / dm and 6A / dm 2 and 7A / dm 2 Included between The peak anode current density, Ja, is 1A / dm 2 and 5A / dm 2 between 1.28A / dm and 1.28A / dm 2 and 4.2A / dm 2 Between 1.28A / dm and 2.0A / dm 2 and 3.1A / dm2 and, more specifically, between 1.28A / dm 2 and 2.16A / dm 2 Included between the time Tc for maintaining the cathodic pulse is comprised between 0.2 s and 0.8 s, advantageously between 0.55 s and 0.65 s; and The time Ta for maintaining the anodic pulse is comprised between 0.06 s and 0.5 s, advantageously between 0.35 s and 0.45 s.

[0022] Within the meaning of the present invention, the terms "included between" or "including" are inclusive of the limits.

[0023] Within the meaning of the present invention, the term "silver-plated copper or copper alloy blank wire" refers to any round wire that is not directly usable in a conductor and is made of copper or a copper alloy and is coated with a silver layer. In particular, the diameter of the blank wire is comprised between 0.1 mm and 1.5 mm, in particular between 1 mm and 0.2 mm. The copper alloy of the blank wire according to the present invention is any usable copper alloy in blank wire, such as a Cu-Be-Ni alloy, the components of which may be, for example, Be: 0.2% to 0.6%, Ni: 1.4 to 2.2%, Cu: balance, or a Cu-Cr-Zr alloy, the components of which may be, for example, Cr: 0.10 to 1.05%, Zr: 0.01 to 0.105%, Cu: balance, in mass %.

[0024] Within the meaning of the present invention, the terms "electrolytic deposition of silver with pulsed current with reversal" or "electrolytic deposition of silver with PCR" refer to any electrolytic deposition of silver or electrolytic plating of silver or plating of silver, in which a discontinuous and modulated electrolytic current is used in the form of a train of cathodic pulses at a given frequency, each of which is followed by an anodic pulse, whether preceded and / or followed by a rest period, advantageously without a rest period. This PCR mode is shown in FIG. 1 (A / dm as a function of time in seconds). 2is shown diagrammatically in units of current density J), where T represents the period (in seconds), T represents the duration of the cathodic pulse (in seconds), Ta represents the duration of the anodic pulse (in seconds), Tr represents the rest time (in seconds), and J represents the peak cathodic current density (A / dm 2 Ja is the peak anodic current density (A / dm 2 Jm is the average current density (A / dm) over a period T. 2 Units).

[0025] The relationship between these separate parameters corresponds to the following equation:

number

[0026] Also, the duty cycle Q (in %) is defined as the ratio of the time allocation of the cathode pulse Tc to the period T, according to the following formula:

number

number

[0027] The process according to the invention makes it possible to coat the blank wire with a continuous silver layer having a thickness of between 1.5 μm and 15 μm, advantageously between 2 μm and 10 μm.

[0028] In an advantageous embodiment, the process is a continuous process. Thus, as cathodes, a number of blank wires, in particular at least three blank wires, more advantageously five blank wires, run through the electrolytic silver plating bath, where a pure silver anode is attached. During the process, a generator, for example of the type Harlor PE86CB-20-10-50S, sends a discontinuous modulated current between the cathode and the anode in the form of a series of cathode pulses at a given frequency, each of which is followed by an anodic pulse. This current generates an electrolysis, which on the one hand allows the dissolution of the silver anode and, at the same time, on the other hand, the deposition of a silver coating on the running blank wire.

[0029] Advantageously, the electrolytic silver plating bath is an aqueous electrolytic bath containing silver cyanide and potassium cyanide. It may also contain additives such as a brightener additive, advantageously at a concentration between 10 ml / l and 50 ml / l, in particular 19 ml / l. The electrolytic bath is a high-speed bath, advantageously at a flow rate of 3 A / dm 2 It can be processed with.

[0030] The wire running speed may be 4.0 m / min.

[0031] The invention further relates to a silver-plated copper or copper alloy blank wire obtainable by the process of the invention, with a silver layer thickness of 1.5 μm to 15 μm, advantageously 2 μm to 10 μm. This silver blank wire can be distinguished from conventional silver blank wires (obtained by electrolytic deposition of silver with direct current) by using very sophisticated analytical means, such as transmission electron microscopy TEM combined with grazing incidence X-ray diffraction. Indeed, the silver coating produced by PCR has a better crystallization state, is more uniform and dense. The blank wire is specifically as described above.

[0032] Advantageously, the silver-plated copper or copper alloy blank wire according to the invention has no defects or, if any, only minor defects in the A&B test according to ECSS-Q-ST-70-20C standard (July 2008), in particular it has a code of 0, 1, 2 or 3, more particularly a code of 0, 1 or 2, even more particularly a code of 0 or 1, even more particularly a code of 0 in the A&B test according to ECSS-Q-ST-70-20C standard.

[0033] Advantageously, the silver-plated copper or copper alloy blank wire according to the invention has no defects in the polysulphurization test according to the ISO 10308 standard (January 2006), in particular in the more severe polysulphurization test in which the quenching time of the wire in a sodium polysulphide solution is extended to 20 minutes.

[0034] Advantageously, the silver-plated copper or copper alloy blank wire according to the invention has good adhesion in an adhesion test consisting of wrapping the wire around itself 5-6 times and then inspecting it under a binocular microscope at a magnification of 10. The adhesion is considered to be good only if no cracks or delamination are detected on the silver coating.

[0035] In particular, the diameter of the silver wire according to the invention is comprised between 0.1 mm and 1.5 mm.

[0036] The invention further relates to a process for producing silver-plated copper or copper alloy strands having a silver layer thickness of 1 μm to 1.5 μm, comprising the step of drawing a blank wire of silver-plated copper or copper alloy according to the invention.

[0037] The drawing step according to the invention makes it possible to reduce the diameter of the silver blank wire according to the invention, which is advantageously carried out cold, advantageously at room temperature, in particular by mechanical force, for example using a machine called a wire drawing machine, which may comprise, as required, a set of 5 to 30 dies, advantageously by reducing the diameter of the blank wire by at least 6.6% (ratio of the final diameter of the strand to the diameter of the blank wire), advantageously obtaining a strand with a diameter comprised between 0.063 mm and 0.254 mm.

[0038] The invention further relates to silver-plated copper or copper alloy strands having a silver layer thickness of 1 μm to 1.5 μm, in particular 1 μm to 1.4 μm, more particularly 1.1 μm to 1.3 μm. Advantageously, the silver-plated strands according to the invention have a diameter comprised between 0.063 mm and 0.254 mm, in particular between 0.079 mm and 0.2 mm, more particularly between 0.1 mm and 0.2 mm.

[0039] It is possible to distinguish these silver-plated strands (or SPC strands) from conventional silver-plated strands (whose silver layer is obtained by electrolytic deposition of silver with a direct current) using very sophisticated analytical tools, such as transmission electron microscopy (TEM) combined with grazing incidence X-ray diffraction. Indeed, the silver coating produced by PCR has a better crystallization state and is more uniform and dense.

[0040] Advantageously, the silver-plated strand according to the invention has no defects or, if any, only minor defects in the A&B test according to the ECSS-Q-ST-70-20C standard (July 2008), in particular it has a code of 0, 1, 2 or 3, more particularly a code of 0, 1 or 2, even more particularly a code of 0 or 1, even more particularly a code of 0 in the A&B test according to the ECSS-Q-ST-70-20C standard.

[0041] Advantageously, the silver-plated strands according to the invention have no defects in the polysulphurization test according to the ISO 10308 standard (January 2006), in particular in the more severe polysulphurization test in which the quenching time of the strands in a sodium polysulphide solution is extended to 20 minutes.

[0042] Advantageously, the silver-plated strand according to the invention has good adhesion in an adhesion test consisting of wrapping the strand around itself 5-6 times and then inspecting it under binocular microscope observation at a magnification of 10. The adhesion is considered to be good only if no cracks or peeling are detected on the silver coating.

[0043] The invention further relates to a silver-plated conductor (or SPC conductor) comprising at least one silver-plated strand according to the invention, advantageously all of whose strands are according to the invention. It is in particular an electrical conductor.

[0044] Advantageously, the conductor according to the invention is a single strand or a multi-strand conductor, advantageously a multi-strand conductor.

[0045] In certain embodiments, the conductor is multi-stranded. It may, for example, comprise 7, 19, 27, 37, 45 and 61 silver-plated strands according to the invention, as well as 7 x 7 silver-plated strands according to the invention. Advantageously, the conductor according to the invention comprises 19 or 37 silver-plated strands according to the invention, and even more advantageously, 19 silver-plated strands according to the invention. Depending on the number of silver-plated strands according to the invention, assemblies according to the ASTM B258 standard (April 2002) can be used, for example, in tordons, concentriques (in particular 19, 61 or 37 silver-plated strands according to the invention), equilays, semi-concentriques, unilays (in particular 19 silver-plated strands according to the invention) or ropelays (in particular 7 x 7 silver-plated strands according to the invention). Advantageously, the electrical conductor comprises 19 silver-plated strands according to the invention assembled concentrically.

[0046] Advantageously, the conductor according to the invention is obtained by twisting (or assembling) silver-plated strands according to the invention.

[0047] Advantageously, the silver plated conductor (or SPC conductor) according to the present invention has no defects or only minor defects, if any, in the A&B test according to ECSS-Q-ST-70-20C standard (July 2008), in particular it has code 0, 1, 2 or 3, more particularly code 1 or 2, even more particularly code 1, in the A&B test according to ECSS-Q-ST-70-20C standard.

[0048] Advantageously, the silver-plated conductor according to the invention has no defects in the polysulphurization test according to the ISO 10308 standard (January 2006), in particular in the more severe polysulphurization test in which the quenching time of the conductor in a sodium polysulphide solution is extended to 20 minutes.

[0049] Advantageously, the silver-plated conductor according to the invention has good adhesion in an adhesion test consisting of wrapping the conductor around itself 5-6 times and then inspecting it under binocular microscope observation at a magnification of 10. The adhesion is considered to be good only if no cracks or peeling are detected on the silver coating.

[0050] The invention additionally relates to an electromagnetic shielding layer (mesh or spiral) comprising at least one silver-plated strand according to the invention, advantageously all of the strands being according to the invention, and is in particular intended for electric cables.

[0051] Advantageously, the shielding layer according to the invention is obtained by helical assembly (or winding) of silver-plated strands according to the invention.

[0052] The invention additionally relates to an electric wire (or SPC electric wire) comprising a silver-plated conductor according to the invention. The electric wire further comprises an insulating layer. The insulating material used to produce the insulating layer is a dielectric material, in other words it does not conduct electricity. The main function of the dielectric is to maintain the electrical insulation performance between the main conductor of the cable and the conductive elements (at earth potential) during a given period of time and in a given environment.

[0053] Advantageously, all the materials of the insulating layers are certified to the ESCC 3901 standard (May 2013). Advantageously, the insulating layers of the electric wire according to the invention comprise polytetrafluoroethylene (PTFE), ethylene tetrafluoroethylene (ETFE) and / or polyimide, in particular polyimide and / or PTFE, and said layers are advantageously produced by extrusion or taping, such as by extrusion for PTFE and ETFE or by taping for PTFE and polyimide in the form of a tape. PTFE can also be fritted, for example by a passage in an oven at a temperature comprised between 380°C and 475°C, in order to give it optimized mechanical, thermal and dielectric properties.

[0054] The insulating layer is advantageously obtained by taping, for example by applying one or more tapes, in particular 1 For example, polyimide tape produced at 150°C, or 2 Multiple polyimide tapes having a minimum overlap of 51% and produced at, for example, 150°C; or 3 A plurality of tapes, specifically a first PTFE tape, specifically 56 μm thick, followed by a second polyimide tape, specifically 25 μm thick, followed by a third PTFE tape, specifically 50 μm thick, all with, for example, a 50% overlap. It may be composed of:

[0055] Advantageously, the electric wire according to the invention further comprises a finishing layer on the insulating layer, in particular based on polyimide, in order to give the wire a complementary function, for example coloring. Generally, application of the finishing layer is carried out with a polyimide liquid, optionally using one or more passes, in particular three passes, in an oven at 250° C. to 500° C.

[0056] Electrical wires according to the invention are illustrated, for example, in FIGS.

[0057] As an example, in Figure 2, a conductor (1) according to the invention, of type SPC26-19x0.102C, is covered by two continuous polyimide tapes (2,3) produced at a temperature of 150°C and with a minimum overlap of 51%, where 26 denotes AWG26 and 19x0.102C denotes a structure of 19 concentric SPC strands according to the invention, with a diameter of 0.102 mm. The finishing polyimide layers (4,5,6) are applied by passing the taped wire three times in a polyimide-based liquid, followed by placing it in an oven at 250°C. The wire thus produced has, on average, a diameter of 0.80 mm and a linear mass (masse lineaire) of 2.00 g / m.

[0058] In Fig. 3, a conductor (1) according to the invention, of type SPC22-19x0.160C, is coated with a polyimide tape (2) produced at a temperature of 150°C, where 22 denotes AWG22 and 19x0.160C denotes the structure of 19 concentric SPC strands according to the invention, with a diameter of 0.160 mm. The finishing polyimide layer (3,4,5) is applied by passing the taped wire three times in a polyimide-based liquid, followed by placing it in an oven at 250°C. The wire thus produced has, on average, a diameter of 1 mm and a linear mass of 4.15 g / m.

[0059] In Fig. 4, a conductor (1) according to the invention, of type SPC22-19x0.160C, is successively coated with three tapes (2,3,4), namely a first tape (2) of PTFE with a thickness of 56 μm, followed by a second polyimide tape (3) with a thickness of 25 μm, and then a third PTFE tape (4) with a thickness of 50 μm, all with an overlap of 50%, where 22 denotes AWG22 and 19x0.160C denotes the structure of 19 concentric SPC strands according to the invention, with a diameter of 0.160 mm. In practice, two separate taping processes are carried out, each followed by a pass in a furnace at 475 °C, in order to properly frit the PTFE. The wire thus produced has, on average, a diameter of 1.21 mm and a linear mass of 5.45 g / m.

[0060] Advantageously, the conductor of the electric wire according to the invention (or SPC electric wire) has no defects or, if any, only minor defects in the A&B test according to the ECSS-Q-ST-70-20C standard (July 2008), in particular it has code 0, 1, 2 or 3, more particularly code 1 or 2, even more particularly code 1 in the A&B test according to the ECSS-Q-ST-70-20C standard.

[0061] Advantageously, the conductor of the electric wire according to the invention does not have any defects in the polysulphurization test according to the ISO 10308 standard (January 2006), in particular in the more severe polysulphurization test in which the quenching time of the insulation-stripped conductor in a sodium polysulphide solution is extended to 20 minutes.

[0062] The electric wire according to the invention may have a diameter comprised between 0.4 mm and 3.0 mm, advantageously between 0.5 mm and 1.5 mm.

[0063] The electric wire according to the invention is thus advantageously obtained by taping or extruding a dielectric onto the silver-plated conductor according to the invention, followed, optionally, by the addition of a finishing layer.

[0064] By way of example, a process for manufacturing an electrical wire according to the invention may comprise the following successive steps: a- electrolytic deposition of silver on a copper or copper alloy blank wire, the electrolytic deposition being carried out in a silver plating bath containing 40 g / l to 70 g / l of silver cyanide and 90 g / l to 150 g / l of potassium cyanide with a pulsed current with reversal, the electrolytic conditions being as described above; b- Stretching the silver-plated copper or copper alloy obtained in step a), c- twisting (or assembling) the silver-plated strands obtained in step b), d- Taping or extrusion of a dielectric onto the conductor obtained in step c), followed, optionally, by application of a finishing layer.

[0065] The invention further relates to an electric cable (or an SPC electric cable) comprising at least one electric wire according to the invention, advantageously all of whose electric wires are according to the invention.

[0066] In particular, the electric cable according to the invention comprises a shielding layer, in particular a metallic shielding layer, and a sheath.

[0067] Shielding layers help to combat the problems caused by electromagnetic interference. A wide variety of shielding layer designs and configurations exist. This layer can be, in particular, woven, in the form of sheets, in the form of a combination of sheets and braids, or wound in a spiral shape (this layer can be particulate and wound in a spiral shape, in a combination of wires and wires and wound in a spiral shape).

[0068] Advantageously, the shielding layer of the electric cable according to the invention is constituted by an assembly of shielding strands according to the invention, in particular in a spiral or braided form, which advantageously results in a shielding layer according to the invention.

[0069] Advantageously, the sheath comprises polytetrafluoroethylene, ethylenetetrafluoroethylene, perfluoroalkoxy and / or polyimide, in particular perfluoroalkoxy, polyimide and / or PTFE, and said sheath is advantageously produced by extrusion or taping, such as by extrusion for perfluoroalkoxy, PTFE and ETFE, or by taping for PTFE and polyimide in tape form. PTFE can be fritted, for example by passing in an oven at a temperature comprised between 380°C and 475°C, to give it optimized mechanical, thermal and dielectric properties. The sheath is advantageously obtained by taping and can for example be composed of one or more tapes, in particular two tapes, such as a first polyimide tape followed by a second PTFE tape, all having for example a 25% overlap. It can also advantageously be obtained by extrusion of PFA.

[0070] An electrical cable according to the invention is illustrated, for example, in FIGS.

[0071] 5, by way of example, four electric wires according to the invention are each composed of a conductor according to the invention (1) of type SPC22-19x0.160C and a polyimide tape (2, 3). A subset of the four electric wires according to the invention is covered with a helical shielding layer of silver-plated strands according to the invention (5) of type SPC36-01x0.127, then with a polyimide tape (6) with an overlap of 25% and a PTFE tape (7) also with an overlap of 25%, followed by a passage in an oven at 380° C. to frit the PTFE tape. The cables thus produced have, on average, a diameter of 3.10 mm and a linear mass of 26.0 g / m.

[0072] As an example, in Fig. 6, two electric wires according to the invention are each made up of a conductor according to the invention of type SPC22-19x0.160C insulated successively by three tapes: a first PTFE tape 56 μm thick, followed by a second polyimide tape 25 μm thick, followed by a third PTFE tape 50 μm thick, all with a 50% overlap. A subset (1) of the two electric wires according to the invention is covered by an electromagnetic shielding layer (2) obtained by braiding silver-plated strands according to the invention of type SPC40-01x0.079, followed by a PFA sheath (3) obtained by extrusion. The cables thus produced have, on average, a diameter of 3.27 mm and a linear mass of 21.1 g / m.

[0073] Advantageously, the conductor of the electric cable according to the invention (or of the SPC electric cable) has no defects or, if any, only minor defects in the A&B test according to the ECSS-Q-ST-70-20C standard (July 2008), in particular it has code 0, 1, 2 or 3, more particularly code 2 or 3, in the A&B test according to the ECSS-Q-ST-70-20C standard.

[0074] Advantageously, the conductor of the electric cable according to the invention does not have any defects in the polysulphurization test according to the ISO 10308 standard (January 2006), in particular in the more severe polysulphurization test in which the quenching time of the insulation-stripped conductor in a sodium polysulphide solution is extended to 20 minutes.

[0075] The electric cable according to the invention may have a diameter comprised between 1.00 mm and 10.0 mm, advantageously between 2.0 mm and 5.0 mm, more advantageously between 0.5 mm and 4 mm, in particular between 0.5 mm and 1.5 mm.

[0076] The electric cable according to the invention (or the SPC electric cable) is advantageously obtained as a result by a process comprising the following successive steps: assembling a plurality of electric wires according to the invention to obtain a subset; assembling, on the subset, silver-plated strands according to the invention to obtain a shielded subset (specifically a shielding layer on the subset); The shielded subset is then exteriorized.

[0077] By way of example, a process for manufacturing an electrical cable according to the invention may comprise the following successive steps: a- electrolytic deposition of silver on a copper or copper alloy blank wire, the electrolytic deposition being carried out in a silver plating bath containing 40 g / l to 70 g / l of silver cyanide and 90 g / l to 150 g / l of potassium cyanide with a pulsed current with reversal, the electrolytic conditions being as described above; b- drawing the silver-plated copper or copper alloy blank wire obtained in step a); c- twisting (or assembling) the silver-plated strands obtained in step b), d- Taping or extrusion of a dielectric onto the conductor obtained in step c), followed, optionally, by the addition of a finishing layer; e) - Assembling the electric wires obtained in step d), f- assembly of the silver-plated strands obtained in step b) on the subset obtained in step e); g-- Sheathing the shielded subset obtained in step f).

[0078] Finally, the invention relates to the use of an electric wire according to the invention or of an electric cable according to the invention in the aerospace field.

[0079] The invention will be better understood on reading the following figures and description of examples, given by way of non-limiting indication. [Brief description of the drawings]

[0080] [Figure 1] FIG. 1 shows a schematic diagram of the PCR mode (electrolytic plating in PCR) according to the present invention. [Diagram 2] FIG. 2 is an example of a structural diagram of an electric wire according to the invention according to the ESCC3901-001-24 standard (May 2013), comprising a conductor according to the invention (1) of type SPC26-19x0.102C, two polyimide tapes (2, 3) and a finishing layer (4, 5, 6). [Diagram 3] FIG. 3 is an example of a construction diagram of an electric wire according to the invention according to the ESCC3901-001-24 standard (May 2013) with a conductor according to the invention (1) of type SPC22-19x0.160C, a polyimide tape (2) and finishing layers (3, 4, 5). [Figure 4] FIG. 4 is an example of a construction diagram of an electric wire according to the invention according to the ESCC3901-018-06 standard (May 2013), comprising a conductor according to the invention (1) of type SPC22-19x0.16C, two PTFE tapes (2, 4) and a polyimide tape (3). [Diagram 5] Figure 5 is an example of a construction diagram of an electric cable according to the invention according to the ESCC 3901-002-70 standard (May 2013) with a subset of four electric wires according to the invention, each of which consists of a conductor according to the invention (1) of type SPC22-19x0.160C and a polyimide tape (2, 3), the subset being covered by a helical shielding layer of silver-plated strands according to the invention (5) of type SPC36-01x0.127, followed by a polyimide tape (6) and a PTFE tape (7). [Figure 6] Figure 6 is an example of a structural diagram of an electric cable according to the invention according to the ESCC 3901-018-53 standard (May 2013) with a subset (1) of two electric wires according to the invention, each of which is made up of a conductor according to the invention of type SPC 22-19x0.160C, insulated successively by three tapes, namely a first PTFE tape with a thickness of 56 μm, followed by a second polyimide tape with a thickness of 25 μm, followed by a third PTFE tape with a thickness of 50 μm, all with a 50% overlap, the subset being covered by an electromagnetic shielding layer (2) obtained by braiding silver-plated strands according to the invention of type SPC 40-01x0.079, followed by a PFA sheath (3) obtained by extrusion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0081] Working Example Examples 1 and 2: SPC conductor according to the invention Silver plating in PCR was carried out in an aqueous electrolytic bath whose components are 100 g / l potassium cyanide KCN, 45 g / l silver cyanide AgCN, and 10 ml / l to 30 ml / l brightener additive, using a Harlor PE86CB-20-10-50S generator capable of modulating electric pulses over a wide range of process parameters. Copper wire with a diameter of 1.2 mm was used as the substrate in the tests (blank wire).

[0082] A polysulfide test, which is more stringent than that of the ISO 10308 standard, was carried out on the obtained SPC conductor. The conductor, whose surface is coated with a metal layer, is immersed in a sodium polysulfide solution for 20 minutes, after which it is washed and dried. An examination with a binocular microscope is then carried out at a magnification of 10 times. When no corrosion spots are observed on the conductor, the test is considered OK.

[0083] An adhesion test as an evaluation criterion was also performed on the obtained silver blank wire. The test consisted of wrapping a silver-plated copper wire around itself 5-6 times and then inspecting it under a binocular microscope at 10x magnification. The adhesion was considered good only if no cracks or delamination were detected on the coating.

[0084] The performance of the obtained SPC conductors in A&B tests according to the ESCC 3901 standard was also evaluated.

[0085] An optical inspection is also performed. For example, under a binocular microscope (Motic SMZ-171) at 50x magnification, the appearance of the conductor is observed: brightness, uniformity, absence of coarse grains. In this case, it is marked as OK.

[0086] The resulting thickness of the silver on the SPC conductor has been measured by an X-ray fluorescence process in a Fischerscope® XULM® type instrument.

[0087] The electrolytic deposition conditions and test results are summarized in Table 2 below.

[0088] [Table 2]

[0089] The results obtained here indicate that for the silver plating bath and range of PCR parameters as described above, relatively satisfactory silver deposition performance is obtained in the polysulfide test and the A&B test.

[0090] Examples 3 and 4: SPC conductors according to the invention using high speed silver plating baths Based on the study of the previous two examples, and for the purpose of adopting it to the silver plating process on an industrial scale, a silver plating bath called a high-speed silver plating bath, the components of which are 130 g / l potassium cyanide KCN, 60 g / l silver cyanide AgCN, and a small amount of additives (10 ml / l to 30 ml / l brightener additives), is used. 2 A silver plating test was performed in PCR using an average density of Jm.

[0091] The same tests were carried out under the same conditions as in the previous examples, and the electrolytic deposition conditions and test results are summarized in Table 3 below.

[0092] [Table 3]

[0093] The results clearly support the feasibility of silver plating in PCR in a faster silver plating bath.

[0094] Example 5: Electrical wire according to the invention An industrial-scale PCR silver plating test was carried out using a reel-to-reel silver plating line. In this case, five copper wires with a diameter of 0.254 mm were simultaneously silver plated in a high-speed silver plating bath similar to those in Examples 3 and 4 above, with the PCR process parameters given in Table 4 below.

[0095] [Table 4]

[0096] It should be noted that the actual silver plating conditions here do not completely match those in the laboratory in Examples 3 and 4 above, since the silver plating line used as an industrial facility has many advantages, in particular allowing for a greater current density and generally resulting in a more uniform coating.

[0097] These silver-plated copper wires are then used to make SPC22-19x0.16C conductors. More specifically, they are first reduced in diameter by drawing in step b) according to the invention (drawing from 0.254 mm to 0.16 mm using 7 drawing dies, i.e. a reduction of 63%), and then assembled by twisting in step c) according to the invention (19 concentric strands of 0.16 mm AWG22). At each step, adhesion tests, visual inspections, and polysulfide tests are performed with final results.

[0098] From this conductor, SPC electric wire according to the ESCC3901-018-06 standard (May 2013) is produced, the structure of which is shown diagrammatically in FIG. 4 below.

[0099] According to the ESCC3901-018-06 standard, the conductor must be successively insulated by three tapes, namely a first PTFE tape with a thickness of 56 μm, followed by a second polyimide tape with a thickness of 25 μm, followed by a third PTFE tape with a thickness of 50 μm, all with a 50% overlap. In practice, to properly frit the PTFE, two separate taping processes (taping I with the first PTFE tape and taping II with the polyimide tape followed by the second PTFE tape) are carried out, each followed by a pass in an oven at 475° C. The fritage of the PTFE is important here, as it can give the PTFE optimized mechanical, thermal and dielectric properties for electrical wires according to the standard.

[0100] As mentioned previously, thermal shock is generally considered to be the main factor in degrading performance in A&B testing of SPC electric wires. The selection of ESCC3901-018-06 wire seemed appropriate to evaluate the improvement that could be brought about by silver plating in PCR, since the manufacture of this wire involves one of the highest temperatures of frittage, the most critical of all SPC electric wires in the ESCC3901 standard.

[0101] A set of manufacturing data for the SPC22-19x0.160C conductor and ESCC3901-018-06 wire, along with the silver thickness and A&B test codes measured at each manufacturing step, are given below in Table 5. The resulting electrical wire has a diameter of 1.21 mm and a linear mass of 5.45 g / m.

[0102] [Table 5]

[0103] The results obtained in the A&B tests for this electrical wire according to the invention, whose silver plating is made from an SPC conductor produced by PCR, are particularly good, whereas the thickness of the silver is only half that of a wire produced by conventional DC.

[0104] Example 6: Electrical cable according to the invention In this example, one of the most sophisticated electrical cables was chosen, allowing better protection against electromagnetic interference, and it is also the most demanding case for A&B testing, taking into account the number of manufacturing steps involved.

[0105] In fact, an electric cable means here a transmission line comprising one or more twisted electric wires, which are then coated with a layer of electromagnetic shielding and then further coated with an insulating sheath, as shown in Comparative Example 4 below. The shielding layer is made by twisting a number of SPC strands, and the sheath is made by extrusion of PFA (perfluoroalkoxy). More specifically, the cable is made according to the ESCC3901-018-53 standard (May 2013), and the following manufacturing steps are carried out:

[0106] A. Silver plating on material wire First, an SPC wire with a diameter of 0.254 mm was produced on a silver plating line different from that used in Example 5, called TS4, whose silver plating bath has the components of those in Examples 3 and 4. The production was carried out at a running speed of 4.0 m / min under the silver plating conditions in PCR shown in Table 6 below.

[0107] [Table 6]

[0108] The thickness of the silver layer on the wire is, on average, 3.66 μm.

[0109] B. Pulling the Silver Wire The resulting SPC wire is stretched from a diameter of 0.254 mm to a diameter of 0.079 mm, i.e. reduced by 31%, and the silver thickness is reduced to an average of 1.14 μm. The SPC strands thus obtained are intended to constitute electromagnetic shields.

[0110] C. Assembly of two electrical wires The two electrical wires produced in Example 5, which correspond to the ESCC3901-018-06 standard (May 2013), are assembled by twisting them together to form a pair, which corresponds to the ESCC3901-018-15 standard (May 2013).

[0111] D. Braided shielding The formed pairs are then electromagnetically shielded by braiding.

[0112] E. Shielded twin extrusion exterior A PFA sheath is carried out by extrusion onto the shielded pairs and an SPC electric cable is obtained according to the ESCC 3901-018-53 standard (May 2013), as shown diagrammatically in FIG.

[0113] A&B tests have been performed at each step of the process, both on the central conductor of the electric wire and on the braided shield of the electric cable. The results obtained are summarized in Tables 7 and 8 below.

[0114] [Table 7]

[0115] [Table 8]

[0116] This example is one of the most sophisticated electrical cables according to the ESCC3901 standard, and in this case it clearly shows that the ESCC3901-018-53 manufactured by the process described herein, using the PCR silver plating technology according to the invention, has a minimum silver thickness of 1.0 μm instead of 2.0 μm, and therefore meets the technical requirements of the ESCC3901 standard, especially in the A&B test.

[0117] Comparative Example 1: Electrical wire, the silver plating of which is carried out with direct current (DC) and has a silver thickness of <2 μm An electric wire made according to the ESCC 3901-001-24 standard, which is usually used for space cabling, has been chosen as a basis for comparison. The corresponding SPC conductor is therefore of type SPC26-19x0.102C, where 26 denotes AWG26 and 19x0.102C denotes a structure of 19 concentric SPC strands with a diameter of 0.102 mm, each strand being coated with silver to an average thickness of 1.35 μm, which average thickness is measured by X-ray fluorescence process on a Fischerscope® type XULM® instrument.

[0118] Silver plating with DC is carried out at 1 A / dm in an aqueous electrolytic bath whose components are 100 g / l potassium cyanide KCN, 10 ml / l to 30 ml / l brightener additive, and 45 g / l silver cyanide AgCN. 2 The electrolysis was carried out under a current density of 0.1.

[0119] Such conductors are used to produce, by taping according to manufacturing step E4, SPC electrical wires according to standard ESCC 3901-001-24.

[0120] More specifically, manufacturing step E4 here includes two sub-steps: the first is the taping of two successive polyimide tapes, carried out at a temperature of 150° C., with a minimum overlap of 51%; the second consists in applying a polyimide finishing layer by passing the taped wire three times in a polyimide-based liquid, followed by placing it in an oven at 250° C. The wire thus produced has, on average, a diameter of 0.80 mm and a linear mass of 2.00 g / m.

[0121] The structure of the SPC wire can be shown diagrammatically in Figure 2. The SPC conductor and the SPC electric wire have been tested by A&B Test at the end of step E3 (stranding) and step E4 (taping), respectively, and have received the resulting codes of 1 and 4, respectively, as shown in Table 9 below.

[0122] [Table 9]

[0123] Although the obtained SPC conductors have good performance in the A&B test, it can be concluded that the SPC electric wire cannot be considered acceptable by the ESCC 3901 standard. The deterioration of the resistance to the A&B test is definitely related to the manufacturing step E4, which involves a combination of mechanical stresses from the taping process and thermal stresses due to successive passes in the furnace.

[0124] Comparative Examples 2-4: Electrical wires and cables, the silver plating of which is carried out with direct current (DC) and has a minimum silver thickness of 2 μm The SPC22-19x0.160 conductors and the SPC36-01x0.127 strands are manufactured with the same DC silver plating as in Comparative Example 1, but with a silver coating having a minimum thickness of 2 μm according to the ESCC 3901 standard. The DC silver plating is carried out under the same conditions as in Comparative Example 1, as is the measurement of the silver thickness. The SPC22-19x0.160C conductor, i.e. made of 19 SPC strands with AWG22 and a diameter of 0.16 mm, is used to make an electric wire according to the ESCC3901-001-26 standard (Comparative Example 2), an electric wire according to the ESCC3901-002-58 standard (Comparative Example 3) and a cable according to the ESCC3901-002-70 standard (Comparative Example 4), while the SPC36-01x0.127 strands with AWG36 and a diameter of 0.127 mm can form a helical shield for the following ESCC3901-002-70 cable.

[0125] The production of ESCC3901-001-26 wire (Comparative Example 2) as illustrated in Figure 2 is obtained by taping a polyimide tape followed by deposition of a polyimide finishing layer. The SPC electric wire thus produced has, on average, a diameter of 1.10 mm and a linear mass of 4.20 g / m.

[0126] The production of SPC electric wire of ESCC3901-002-58 (Comparative Example 3) as illustrated in Figure 3 is obtained by taping a single polyimide tape at 150°C, followed by application of a polyimide finishing layer, followed by two or three passes in an oven at 250°C. The wire thus obtained has, on average, a diameter of 1.00 mm and a linear mass of 4.15 g / m.

[0127] The production of the SPC electric cable ESCC3901-002-70 (Comparative Example 4) as shown in Figure 5 includes three steps: the first is to twist a subset of four ESCC9301-002-58 electric wires, the second is to cover the subset with a helical shield layer of SPC36-01x0.127 strands, and the third is to taping a polyimide tape with 25% overlap and another PTFE tape with 25% overlap over the shielded subset, followed by passing through a 380°C oven to frit the PTFE tape. The cable thus produced has an average diameter of 3.10 mm and a linear mass of 26.0 g / m.

[0128] A&B tests were then performed at the end of stranding and at the end of taping for the conductor of the wire of Comparative Example 2, at the end of drawing, stranding and taping for the conductor of the wire of Comparative Example 3, and at the end of drawing E2 and at the end of sheathing E7 for the cable of Comparative Example 4. The test codes as well as the silver thickness of the conductors are summarized in Table 10 below.

[0129] [Table 10]

[0130] In fact, it can be seen that a silver thickness greater than 2 μm makes it possible to improve resistance to A&B tests, both at the conductor end of manufacture and at the electrical wire end of manufacture.

[0131] The results also seem to indicate that, despite the silver thickness exceeding 2μm on the SPC36-01x0.127 strands, once winding has been performed, the resistance to the A&B test is significantly degraded. In other words, the winding, taping and frittage processes have a strong influence on the resistance of the silver coating to the A&B test, thus justifying the minimum silver thickness of 2μm imposed by the ESCC3901 standard.

[0132] Comparative Examples 5 to 11: The silver plating is produced by PCR, but the conductor is produced by separate electrolysis conditions. Conductors were produced under the same conditions as in Examples 1 and 2, except for the electrolysis conditions, and are summarized in Table 8 below.

[0133] The same tests as those shown in Examples 1 and 2 were performed on the resulting silver plated conductors, and the results are shown in Table 11 below.

[0134] [Table 11]

[0135] The results obtained demonstrate the importance of the electrolysis conditions in order to obtain compliant silver plated conductors.

[0136] Comparative Examples 12 to 13: The silver plating is produced by PCR using a high-speed silver plating bath, but the conductor is produced by separate electrolysis conditions. Conductors were prepared under the same conditions as in Examples 3 and 4, except for the electrolysis conditions, and are summarized in Table 9 below.

[0137] The same tests as those shown in Examples 3 and 4 were performed on the resulting silver plated conductors, and the results are shown in Table 12 below.

[0138] [Table 12]

[0139] The results obtained show that the electrolysis conditions are important in order to obtain compliant silver plated conductors.

Claims

1. 1. A process for producing silver-plated copper or copper alloy blank wire having a silver layer thickness of 1.5 μm to 15 μm, comprising: Electrolytically depositing silver onto a copper or copper alloy blank wire; 1. A process for producing silver-plated copper or copper alloy blank wire, wherein the electrolytic deposition is carried out in a silver plating bath containing 40 g / l to 70 g / l of silver cyanide and 90 g / l to 150 g / l of potassium cyanide, with pulsed current with reversal, and the electrolysis conditions are as follows: Average current density Jm is 1.5A / dm 2 and 15 A / dm 2 and preferably between 1.78 A / dm 2 and 5A / dm 2 Included between The pulse frequency f is between 0.8 Hz and 1.6 Hz, preferably between 0.8 Hz and 1.4 Hz, in particular 1 Hz, the duty cycle Q is comprised between 50% and 80%, advantageously between 55% and 65%, The peak current density Jc of the cathode is 3 A / dm 2 and 11 A / dm 2 and preferably between 5 A / dm 2 and 10 A / dm 2 Included between The peak current density of the anode is 1 A / dm 2 and 5A / dm 2 and preferably between 1.28 A / dm 2 and 4.2 A / dm 2 Included between the time Tc for maintaining the cathodic pulse is comprised between 0.2 s and 0.8 s, advantageously between 0.55 s and 0.65 s; and The time Ta for maintaining the anodic pulse is comprised between 0.06 s and 0.5 s, advantageously between 0.35 s and 0.45 s.

2. A silver-plated copper or copper alloy blank wire obtainable by the process according to claim 1, having a silver layer thickness of between 1.5 μm and 15 μm.

3. 1. A process for producing silver-plated copper or copper alloy strands having a silver layer thickness of 1 μm to 1.5 μm, comprising:

3. A process for producing strands of silver-plated copper or copper alloy comprising the step of drawing the silver-plated copper or copper alloy blank wire of claim 2.

4. Silver-plated copper or copper alloy strands obtainable by the process according to claim 3, having a silver layer thickness of between 1 μm and 1.5 μm.

5. A silver plated conductor comprising at least one silver plated strand according to claim 4, advantageously all of said strands being as defined in claim 4.

6. Electromagnetic shielding layer comprising at least one silver-plated strand according to claim 4, advantageously all of said strands being as defined in claim 4.

7. An electrical wire comprising the silver plated conductor of claim 5.

8. 8. Electric wire according to claim 7, characterized in that its insulating layer comprises polytetrafluoroethylene, ethylenetetrafluoroethylene and / or polyimide, said insulating layer being advantageously produced by extrusion or by taping.

9. An electric cable comprising at least one electric wire according to claim 7, advantageously all of said electric wires being as claimed in claim 7.

10. 10. Electric cable according to claim 9, characterized in that its shielding layer is as claimed in claim 6.

11. 10. Electric cable according to claim 9, characterized in that its sheath comprises polytetrafluoroethylene, ethylenetetrafluoroethylene, perfluoroalkoxy and / or polyimide, said sheath being advantageously produced by extrusion or by taping.

12. Use of the electric wire according to claim 7 or 8 in the field of aerospace.

13. Use of an electric cable according to any one of claims 9 to 11 in the field of aerospace.