Lithium iron phosphate cathode material containing carbon powder
Agglomerated particles with a porous carbon matrix and embedded LMP particles address the challenges of LFP cathodes by improving conductivity and capacity, enabling efficient and sustainable lithium-ion batteries for commercial use.
Patent Information
- Application Number
- JP2024519929
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-01
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Conventional lithium iron phosphate (LFP) cathode materials face challenges such as high production costs, environmental impact from toxic waste, and poor performance due to uneven carbon coatings and crystallographic defects, which hinder their scalability and efficiency in lithium-ion batteries.
The development of agglomerated particles comprising porous carbon matrix particles with embedded lithium metal phosphate (LMP) particles, formed through a method involving the use of a polyamic acid gel that is pyrolyzed to create a conductive carbon matrix, reducing particle size and preventing crystal growth, while utilizing environmentally friendly chemistry.
This approach enhances the electrical conductivity and charge capacity of LFP electrodes, achieving high-rate performance and extended cycle life, making them suitable for commercial applications like electric vehicles, while being cost-effective and environmentally friendly.
Smart Images

Figure 2024536298000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a continuation of U.S. Provisional Patent Application No. 63 / 381777, filed November 1, 2022, U.S. Provisional Patent Application No. 63 / 381771, filed November 1, 2022, U.S. Provisional Patent Application No. 63 / 381694, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381687, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381681, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381672, filed October 31, 2022, U.S. This application claims priority to and the benefit of U.S. Provisional Patent Application No. 63 / 381,666, U.S. Provisional Patent Application No. 63 / 416,996, filed October 18, 2022, U.S. Provisional Patent Application No. 63 / 378,756, filed October 7, 2022, U.S. Provisional Patent Application No. 63 / 352,571, filed June 15, 2022, U.S. Provisional Patent Application No. 63 / 336,640, filed April 29, 2022, and U.S. Provisional Patent Application No. 63 / 326,353, filed April 1, 2022, each of which is incorporated by reference in its entirety herein.
[0002] The present disclosure relates to improved cathode materials for lithium-ion batteries. In particular, the present disclosure relates to porous carbon matrix materials including carbon aerogels doped with cathode materials and methods for their manufacture. [Background technology]
[0003] One of the most common forms of rechargeable batteries is the lithium-ion battery (LIB). LIBs are widely used in a variety of applications, ranging from portable electronics to automobiles. LIBs are a type of battery in which lithium ions move from the anode to the cathode during discharge and from the cathode to the anode during a charging cycle (recharging). Traditionally, the anode of a LIB is made of graphite and / or alloy materials (e.g., Si), or oxides (e.g., Li4Ti5O 12), and lithium ions are inserted within the graphite layers during the charging cycle, providing energy storage. LIB cathode materials are typically oxide compounds of nickel, cobalt, or manganese ("NCM") or aluminum. NCM cathode materials are interesting because they have high charge capacities (approximately 200 milliamp hours per gram (mAh / g)) compared to other types of cathode materials. However, these materials can be expensive to prepare and can be harmful to the environment because expensive ores must be obtained and processed to provide the necessary precursors, producing toxic waste during the process.
[0004] Recently, LFP (LiFePO4) has emerged as one of the most promising cathode materials for lithium-ion batteries (LIBs), eliminating conflict metals such as nickel and cobalt that are widely used in non-LFP LIBs (e.g., NMC chemistries). However, the main challenge for this material lies in its cost / performance in large-scale production, especially the cost of raw materials and manufacturing processes. LFP materials that perform well in batteries (i.e., approach a theoretical capacity of 170 milliampere-hours per gram (mA / g) and experience minimal capacity loss for at least 500 or 1000 charging cycles) can be produced from a variety of precursors using a variety of techniques. However, these techniques can generate wastewater, requiring expensive and energy-intensive treatment techniques.
[0005] On the other hand, low-cost (and low-quality) LFPs (herein "LC-LFPs") can be economically produced from iron oxide (minerals), but their performance is inferior. The inferior performance of some types of LFPs can be attributed to uneven or poor quality carbon coating of the particles (thereby increasing the internal electrical resistance of the material) and / or crystallographic defects that inhibit lithium ion mobility. Both electron transfer resistance and ion transfer resistance are positively correlated with particle size. Therefore, optimizing the performance of LFP electrodes, especially for use in lithium ion batteries (LIBs), involves reducing the particle size of the LFP to below 1 micron.
[0006] Optimizing the performance of LFP electrodes may also involve reducing crystalline defects through annealing. However, particle size reduction techniques and high temperature treatment are incompatible because high temperature treatment induces undesirable crystal growth in the (desirable) small particles of LFP. Undesirable crystal growth results in electronically isolated zones within the cathode particles that reduce access to lithium (Li) ions and reduce charge capacity. Therefore, conductive surface coatings and particle level engineering using advanced polymer and carbon technologies are required to target high performance LFP electrodes suitable for LIB work.
[0007] Therefore, the present disclosure seeks to meet the need in the art for high performance LFP materials produced from low cost starting materials while overcoming the above-mentioned shortcomings in conventional materials and methods. Summary of the Invention
[0008] The present technology is generally directed to agglomerated particles including porous carbon matrix particles and a plurality of cathode material particles, as well as a method for preparing the cathode material within a conductive carbon matrix. The method generally includes providing a slurry of the cathode material particles in a solution of an organogel precursor material suitable for subsequent gelation to form an organogel (e.g., a polyimide or polyamic acid gel), gelling the organogel precursor material, thereby forming an organic matrix in the form of a wet organogel, and drying the wet organogel. The dried organogel (aerogel, xerogel, or aerogel-like) is then pyrolyzed to form a porous carbon matrix material doped with particles of the cathode material.
[0009] Various solid and liquid phase methods for forming lithium iron phosphate materials have been reported, see, for example, U.S. Patent Application Publication No. 2011 / 0110838 to Wang et al., U.S. Patent Application Publication No. 2008 / 0099720 to Huang et al., U.S. Patent Application Publication No. 2010 / 0065787 and U.S. Patent Application Publication No. 2011 / 0091772 to Mishima et al., U.S. Patent No. 7,988,879 to Park et al. and U.S. Patent No. 7,060,238 to Saidi et al., European Patent Application Publication No. 1,921,698 to Dong, and International Patent Application Publication No. WO2004 / 092065 to Barker et al.
[0010] LFP alone has low electrical conductivity, and it is known in the art to provide additional carbon (i.e., LFP / C) to obtain the required electrical conductivity. Previously reported methods provide LFP cathode materials that include carbon, for example, but the carbon is typically added using carbon particles (e.g., carbon black) or by pyrolysis of a mixture of LFP precursors and sugar molecules. None of these prior methods of introducing carbon into the cathode material provide a conductive matrix comparable to that provided according to the methods disclosed herein.
[0011] The disclosed products and methods can use LFP from any source, including low cost / low quality LFP (LC-LFP) materials, as the starting material, making the disclosed products and methods cost-effective. Additionally, the products and methods disclosed herein overcome the poor performance of such materials by providing a porous carbon matrix in which LFP particles are at least partially embedded, thereby providing the carbon necessary for improved electrical conductivity. The amount of carbon present in the final material can be tailored to the minimum amount required for electrical conductivity, thereby maximizing the amount of LFP, the component that stores charge in the final battery.
[0012] The formation of the disclosed carbon matrix by pyrolysis is carried out herein at a temperature high enough to pyrolyze the polymer (e.g., polyamic acid, polyimide, or combinations thereof) of the organogel into carbon while simultaneously preventing undesirable crystal growth in the LFP particles. Without wishing to be bound by theory, it is believed that at least partially embedding the LFP particles within the pores of the carbon matrix particles prevents this potential crystal growth that would otherwise reduce the charge capacity of the battery cell.
[0013] Additionally, the methods disclosed herein generally utilize environmentally friendly chemistry, and where non-aqueous solvents are used, the solvents can be recycled, resulting in an overall low environmental impact from the methods.
[0014] In one aspect, an agglomerated particle is provided that includes a matrix particle comprising porous carbon and a plurality of cathode material particles at least partially embedded within the matrix particle.
[0015] In some embodiments, the plurality of cathode material particles comprises lithium metal phosphate (LMP) particles.
[0016] In some embodiments, the metal (M) of the LMP is selected from the group consisting of Fe, Mn, V, and a combination of Fe and Mn.
[0017] In some embodiments, the matrix particles have a particle size between 100 nm and 20 microns, or between 1 and 10 microns.
[0018] In some embodiments, at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 250 nm, or less than 150 nm.
[0019] In some embodiments, the matrix particles have an internal specific surface area corresponding to the internal pores of 50 m 2 / g ~ 150m 2 / gram.
[0020] In some embodiments, at least a portion of the internal surface area is configured to be accessible to the electrolyte.
[0021] In some embodiments, the matrix particles comprise an aerogel or a xerogel.
[0022] In some embodiments, the xerogel aerogel is formed as one or more beads or a monolith.
[0023] In some embodiments, the aerogel or xerogel is derived from an organogel comprising a polyimide, a polyamic acid, or a combination thereof.
[0024] In some embodiments, the aerogel or xerogel is a carbonized organogel.
[0025] In some embodiments, the matrix particles have a pore structure that includes a fibrillar morphology.
[0026] In some embodiments, the fibrillar morphology comprises struts of carbonized material having widths in the range of about 2 to about 10 nm.
[0027] In some embodiments, the matrix particles have a substantially uniform pore size distribution.
[0028] In some embodiments, the matrix particles have an average pore size of about 1 to about 50 nm, or about 5 to about 25 nm.
[0029] In some aspects, the matrix particles include pores, at least some of the pores configured to accommodate the cathode material particles.
[0030] In some embodiments, the weight ratio of carbon in the matrix material to the cathode material is less than 30:70, less than 10:90, or less than 5:95.
[0031] In another aspect, a method is provided for preparing an agglomerated particle comprising a porous carbon matrix particle and a plurality of cathode material particles at least partially embedded within the matrix particle, the method comprising: (a) preparing an aqueous solution of a salt of a polyamic acid; (b) mixing particles of cathode material with an aqueous solution of a salt of a polyamic acid; (c1) gelling the mixture of step (b) to form an organogel comprising dispersed cathode material particles and drying the organogel of step (c1) to form a dried intermediate; or (c2) drying the mixture of step (b) to form a dried intermediate; (d) carbonizing the dried intermediate to form agglomerated particles.
[0032] In some embodiments, preparing the aqueous solution of a salt of a polyamic acid comprises: mixing a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; and reacting the components to obtain a solution of a salt of the polyamic acid.
[0033] In some embodiments, the mixing comprises: dissolving a water soluble diamine in water to form an aqueous diamine solution; adding a water soluble carbonate or bicarbonate to an aqueous diamine solution; adding a tetracarboxylic dianhydride to an aqueous solution of a diamine and a water-soluble carbonate or bicarbonate to form a solution; and stirring the solution at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days.
[0034] In some embodiments, the mixing comprises: dissolving a water soluble diamine in water to form an aqueous diamine solution; adding a tetracarboxylic dianhydride to an aqueous diamine solution to form a suspension; stirring the suspension at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days; adding a water soluble carbonate or bicarbonate to the suspension; and stirring the suspension at a temperature in the range of about 4 to about 60° C. for a period in the range of about 1 hour to about 4 days to obtain an aqueous solution of the salt of the polyamic acid.
[0035] In some embodiments, the mixing comprises: adding, either simultaneously or in rapid succession, a water-soluble diamine, a tetracarboxylic dianhydride, and a water-soluble carbonate or bicarbonate to water; and stirring the resulting mixture at a temperature in the range of about 4 to about 60° C. for a period in the range of about 1 hour to about 4 days to obtain an aqueous solution of a polyamic acid salt.
[0036] In some embodiments, the water soluble carbonate or bicarbonate comprises a lithium, sodium, potassium, ammonium, or guanidinium cation. In some embodiments, the water soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidinium carbonate, and combinations thereof.
[0037] In some embodiments, the water-soluble carbonate or bicarbonate is a carbonate and the molar ratio of the water-soluble carbonate to the diamine is from about 1 to about 1.4, or the water-soluble carbonate or bicarbonate is a bicarbonate and the molar ratio of the water-soluble bicarbonate to the diamine is from about 2 to about 2.8.
[0038] In some embodiments, the molar ratio of the tetracarboxylic dianhydride to the diamine is from about 0.9 to about 1.1.
[0039] In some embodiments, the tetracarboxylic dianhydride is selected from the group consisting of biphthalic dianhydride (BPDA), benzophenone tetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), naphthyl tetracarboxylic dianhydride, perylene tetracarboxylic dianhydride, and pyromellitic dianhydride (PMDA).
[0040] In some embodiments, the diamine is 1,3-phenylenediamine, 1,4-phenylenediamine, or a combination thereof. In some embodiments, the diamine is 1,4-phenylenediamine.
[0041] In some embodiments, the concentration range of the polyamic acid salt in the aqueous solution is from about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid. 3 It is.
[0042] In some embodiments, drying the organogel or intermediate comprises: Optionally washing or solvent exchanging the organogel or intermediate; exposing the organogel or intermediate to elevated temperature conditions, freeze-drying the organogel or intermediate, or contacting the organogel or intermediate with supercritical fluid carbon dioxide.
[0043] In some embodiments, the porous carbon matrix comprises an aerogel or a xerogel.
[0044] In some embodiments, the carbonization is carried out at a temperature of at least about 650° C. under an inert atmosphere.
[0045] In some embodiments, the cathode material particles comprise at least one lithium metal phosphate (LMP), where the metal (M) is selected from iron, manganese, vanadium, and combinations of iron and manganese.
[0046] In some embodiments, the cathode material particles comprise or consist essentially of LiFePO4.
[0047] In some embodiments, the cathode material is ground before or during step (b).
[0048] In some embodiments, milling comprises milling using a roller mill, a planetary ball mill, or a bead agitator mill, optionally with at least one grinding media selected from alumina, zirconia, and stainless steel.
[0049] In some embodiments, the grinding comprises dispersing the cathode material in a liquid phase optionally selected from water, ethanol, isopropanol, ethylene glycol, acetone, or mixtures thereof, and wet-grinding the cathode material.
[0050] In some embodiments, the milling comprises dispersing the cathode material in an aqueous solution of a salt of a polyamic acid and wet-milling the cathode material during step (b) to obtain cathode material particles.
[0051] In some embodiments, step (b) comprises mixing for a period and under conditions sufficient to disperse the cathode material in the aqueous solution.
[0052] In some embodiments, the organogel comprises a polyimide and the gelling in step (c1) comprises adding a gelling initiator to convert the polyamic acid to a polyimide. In some embodiments, the gelling initiator is acetic anhydride.
[0053] In some embodiments, the gelling of the mixture in step (c1) is carried out in a mold to form a wet gel monolith.
[0054] In some embodiments, the method further comprises breaking the wet gel monolith into a plurality of pieces prior to drying.
[0055] In some embodiments, the method further comprises: (e) grinding the dried material of step (c1).
[0056] In some embodiments, the milling produces particles having an average particle size D50 of less than about 50 microns.
[0057] In some embodiments, step (c1) further comprises, after adding the gelation initiator, mixing the aqueous solution of the salt of the polyamic acid with a water-immiscible liquid to form an emulsion.
[0058] In some embodiments, the gelation initiator is acetic anhydride.
[0059] In some embodiments, mixing to form the emulsion is carried out for about 1 to about 30 minutes, or about 4 to about 15 minutes.
[0060] In some embodiments, the organogel comprises a polyamic acid, and the gelling in step (c1) comprises adding a gelling initiator to convert a salt of the polyamic acid to a polyamic acid organogel, and the gelling initiator is an acid. In some embodiments, the acid is a carboxylic acid. In some embodiments, the carboxylic acid is acetic acid.
[0061] In some embodiments, the method further comprises, between steps (b) and (c1), combining the mixture of step (b) with a water-immiscible liquid to form an emulsion.
[0062] In some embodiments, mixing is carried out for up to about 10 minutes, or from about 1 to about 3 minutes.
[0063] In some embodiments, the mixing is performed using a homogenizer, hi some embodiments, the homogenizer is operated at a speed of at least 1000 rpm, for example, from about 1000 to about 9000 rpm.
[0064] In some embodiments, the water-immiscible liquid is selected from the group consisting of mineral spirits, hexane, heptane, kerosene, octane, toluene, other hydrocarbons, and combinations thereof, hi some embodiments, the water-immiscible liquid is mineral spirits.
[0065] In some embodiments, the water-immiscible liquid further comprises a surfactant dissolved therein, hi some embodiments, the surfactant is present in a concentration of about 1-2% by weight of the water-immiscible liquid.
[0066] In some embodiments, the method further comprises separating the organogel beads formed in step (c1) prior to drying, hi some embodiments, the separating comprises decanting the water-immiscible liquid and optionally recycling the water-immiscible liquid.
[0067] In some embodiments, the beads have an average size ranging from about 5 to about 30 microns.
[0068] In some embodiments, the method further comprises washing the gel beads with water, a C1-C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.
[0069] In some embodiments, at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 250 nm, or less than 150 nm.
[0070] In some embodiments, the drying step (c2) is spray drying.
[0071] In yet another aspect, there is provided an agglomerated particle comprising porous carbon matrix particles and a plurality of cathode material particles at least partially embedded within the matrix particles, the agglomerated particle being obtained or obtainable by the methods disclosed herein.
[0072] In some embodiments, the weight ratio of carbon in the matrix material to the cathode material is less than 30:70, less than 10:90, or less than 5:95.
[0073] In yet another aspect, there is provided an electrode comprising the agglomerated particles disclosed herein.
[0074] In yet another aspect, there is provided an energy storage device comprising the agglomerated particles disclosed herein. In some aspects, the energy storage device is a Li-ion battery.
[0075] The present disclosure includes, but is not limited to, the following aspects.
[0076] Embodiment 1: An agglomerated particle comprising a matrix particle comprising porous carbon and a plurality of cathode material particles at least partially embedded within said matrix particle.
[0077] Example 2. The agglomerated particle of example 1, wherein the plurality of cathode material particles comprises lithium metal phosphate (LMP) particles.
[0078] Embodiment 3: The agglomerated particle of embodiment 1 or 2, wherein the metal (M) of the LMP is selected from the group consisting of Fe, Mn, V, and a combination of Fe and Mn.
[0079] Embodiment 4: The agglomerated particle of any one of embodiments 1 to 3, wherein the matrix particles have a particle size of from 100 nm to 20 microns, or from 1 to 10 microns.
[0080] Embodiment 5: The agglomerated particle of any one of Embodiments 1-4, wherein at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 250 nm.
[0081] Embodiment 6: The agglomerated particle of any one of Embodiments 1-5, wherein at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 150 nm.
[0082] Aspect 7: The matrix particles have an internal specific surface area of 50 m 2 / g ~ 150m 2 7. The agglomerated particle of any one of the preceding embodiments, wherein the agglomerated particle weight is 1 / gram.
[0083]
[0023] Embodiment 8: The agglomerated particle of any one of embodiments 1-7, wherein at least a portion of the internal specific surface area is configured to be accessible to an electrolyte.
[0084]
[0023] Example 9: The agglomerated particle of any one of Examples 1-8, wherein the matrix particle comprises an aerogel or a xerogel.
[0085] Example 10: The agglomerated particle of example 9, wherein the xerogel aerogel is formed as one or more beads or a monolith.
[0086] Example 11: The agglomerated particle of any one of Examples 9-10, wherein the aerogel or xerogel is derived from an organogel comprising a polyimide, a polyamic acid, or a combination thereof.
[0087] Example 12: The agglomerated particle of any one of Examples 9-11, wherein the aerogel or xerogel is a carbonized organogel.
[0088] Example 13: The agglomerated particle of any one of Examples 1 to 12, wherein the matrix particles have a pore structure that includes a fibrillar morphology.
[0089] Example 14. The agglomerated particle of example 13, wherein the fibrillar morphology comprises struts of carbonized material having widths in the range of about 2 to about 10 nm.
[0090] Example 15: The agglomerated particle of any one of Examples 1-14, wherein the matrix particles have a substantially uniform pore size distribution.
[0091] Embodiment 16: The agglomerated particle of any one of embodiments 1 to 15, wherein the matrix particle has an average pore size of from about 1 to about 50 nm, or from about 5 to about 25 nm.
[0092] Example 17 The agglomerated particle of any one of Examples 1-16, wherein the matrix particles include pores, at least a portion of the pores configured to accommodate the cathode material particles.
[0093]
[0041] Example 18: The agglomerated particle of any one of Examples 1-17, wherein a weight ratio of carbon in the matrix material to the cathode material is less than 30:70, less than 10:90, or less than 5:95.
[0094] Aspect 19: A method of preparing an agglomerated particle comprising a porous carbon matrix particle and a plurality of cathode material particles at least partially embedded within the matrix particle, comprising the steps of: (a) preparing an aqueous solution of a salt of a polyamic acid; (b) mixing particles of cathode material with an aqueous solution of a salt of the polyamic acid; (c1) gelling the mixture of step (b) to form an organogel comprising dispersed cathode material particles and drying the organogel of step (c1) to form a dried intermediate; or (c2) drying the mixture of step (b) to form a dried intermediate; (d) carbonizing said dried intermediate to form said agglomerated particles.
[0095] Aspect 20. Preparing the aqueous solution of a salt of the polyamic acid comprises: mixing a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; and reacting the components to obtain a solution of a salt of the polyamic acid.
[0096] Aspect 21: The mixing dissolving a water soluble diamine in water to form an aqueous diamine solution; adding said water-soluble carbonate or bicarbonate to said aqueous diamine solution; adding a tetracarboxylic dianhydride to an aqueous solution of the diamine and the water-soluble carbonate or bicarbonate to form a solution; 21. The method of embodiment 20, comprising stirring the solution at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days.
[0097] Aspect 22: The mixing dissolving a water soluble diamine in water to form an aqueous diamine solution; adding a tetracarboxylic dianhydride to the aqueous diamine solution to form a suspension; stirring the suspension at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days; adding said water soluble carbonate or bicarbonate to said suspension; and stirring the suspension at a temperature in the range of about 4 to about 60° C. for a period in the range of about 1 hour to about 4 days to obtain an aqueous solution of a salt of the polyamic acid.
[0098] Aspect 23: The mixing adding, either simultaneously or in rapid succession, a water-soluble diamine, a tetracarboxylic dianhydride, and a water-soluble carbonate or bicarbonate to water; and stirring the resulting mixture at a temperature in the range of about 4 to about 60° C. for a period in the range of about 1 hour to about 4 days to obtain an aqueous solution of the polyamic acid salt.
[0099] Aspect 24: The method of any one of aspects 19 to 23, wherein the water-soluble carbonate or bicarbonate comprises a lithium, sodium, potassium, ammonium, or guanidinium cation.
[0100] Aspect 25: The method of any one of aspects 19 to 24, wherein the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidinium carbonate, and combinations thereof.
[0101] Aspect 26: The method of any one of aspects 19 to 25, wherein the water-soluble carbonate or bicarbonate is a carbonate and the molar ratio of the water-soluble carbonate to the diamine is from about 1 to about 1.4, or the water-soluble carbonate or bicarbonate is a bicarbonate and the molar ratio of the water-soluble bicarbonate to the diamine is from about 2 to about 2.8.
[0102] Aspect 27 The method of any one of aspects 19 to 26, wherein the molar ratio of the tetracarboxylic dianhydride to the diamine is from about 0.9 to about 1.1.
[0103] Aspect 28: The method of any one of aspects 19 to 27, wherein the tetracarboxylic dianhydride is selected from the group consisting of biphthalic dianhydride (BPDA), benzophenone tetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), naphthalyl tetracarboxylic dianhydride, perylene tetracarboxylic dianhydride, and pyromellitic dianhydride (PMDA).
[0104] Aspect 29: The method of any one of aspects 19 to 28, wherein the diamine is 1,3-phenylenediamine, 1,4-phenylenediamine, or a combination thereof.
[0105] Example 30: The method of any one of Examples 19 to 29, wherein the diamine is 1,4-phenylenediamine.
[0106] Aspect 31: The concentration range of the polyamic acid salt in the aqueous solution is about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid. 3 The method according to any one of aspects 19 to 30, wherein
[0107] Aspect 32: Drying the organogel or intermediate comprises: Optionally washing or solvent exchanging the organogel or intermediate; 32. The method of any one of aspects 19-31, comprising exposing the organogel or intermediate to elevated temperature conditions, freeze-drying the organogel or intermediate, or contacting the organogel or intermediate with supercritical fluid carbon dioxide.
[0108] Example 33: The method of any one of examples 19-32, wherein the porous carbon matrix comprises an aerogel or a xerogel.
[0109] Example 34: The method of any one of Examples 19 to 33, wherein the carbonization is carried out under an inert atmosphere at a temperature of at least about 650° C.
[0110] Example 35. The method of any one of Examples 19 to 34, wherein the cathode material particles comprise at least one lithium metal phosphate (LMP), and the metal (M) is selected from iron, manganese, vanadium, and combinations of iron and manganese.
[0111] Example 36: The method of any one of examples 19-35, wherein the cathode material particles comprise, or consist essentially of, LiFePO4.
[0112]
[0041] Example 37. The method of any one of Examples 19-36, wherein the cathode material is ground before or during step (b).
[0113] Aspect 38: The method of aspect 37, wherein the grinding comprises grinding using a roller mill, a planetary ball mill, or a bead agitator mill, optionally using at least one grinding medium selected from alumina, zirconia, and stainless steel.
[0114] Aspect 39: The method of aspect 37 or 38, wherein the grinding comprises dispersing the cathode material in a liquid phase optionally selected from water, ethanol, isopropanol, ethylene glycol, acetone, or a mixture thereof, and wet-grinding the cathode material.
[0115] Aspect 40: The method of any one of aspects 37 to 39, wherein the milling comprises dispersing the cathode material in an aqueous solution of a salt of the polyamic acid and wet-milling the cathode material during step (b) to obtain cathode material particles.
[0116]
[0046] Example 41. The method of any one of Examples 19-40, wherein step (b) comprises mixing for a period and under conditions sufficient to disperse the cathode material in the aqueous solution.
[0117] Aspect 42: The method of any one of aspects 19 to 41, wherein the organogel comprises a polyimide, and the gelling in step (c1) comprises adding a gelling initiator to convert the polyamic acid to the polyimide.
[0118] Aspect 43: The method of aspect 42, wherein the gelation initiator is acetic anhydride.
[0119]
[0046] Aspect 44: The method of any one of aspects 19 to 43, wherein the gelling of the mixture in step (c1) is carried out in a mold to form a wet gel monolith.
[0120]
[0046] Aspect 45: The method of aspect 44, further comprising breaking the wet gel monolith into a plurality of pieces prior to said drying.
[0121] Example 46: The method of any one of examples 19 to 45, further comprising: (e) grinding the dried material of step (c1).
[0122] Aspect 47: The method of aspect 46, wherein the grinding produces particles having an average particle size D50 of less than about 50 microns.
[0123] Aspect 48: The method of any one of aspects 19 to 43, wherein step (c1) further comprises, after adding the gelation initiator, mixing the aqueous solution of the salt of the polyamic acid with a water-immiscible liquid to form an emulsion.
[0124] Aspect 49: The method of aspect 48, wherein the gelation initiator is acetic anhydride.
[0125] Embodiment 50: The method of any one of embodiments 48 to 49, wherein the mixing to form the emulsion is performed for about 1 to about 30 minutes, or about 4 to about 15 minutes.
[0126] Aspect 51: The method of any one of aspects 19 to 41, wherein the organogel comprises a polyamic acid, and the gelling in step (c1) comprises adding a gelation initiator to convert a salt of the polyamic acid into a polyamic acid organogel, and the gelation initiator is an acid.
[0127] Example 52: The method of example 51, wherein the acid is a carboxylic acid.
[0128] Embodiment 53: The method of embodiment 52, wherein the carboxylic acid is acetic acid.
[0129] Embodiment 54: The method of any one of embodiments 51 to 53, further comprising between steps (b) and (c1), mixing the mixture of step (b) with a water-immiscible liquid to form an emulsion.
[0130] Aspect 55: The method of aspect 54, wherein the mixing is performed for up to about 10 minutes, or from about 1 to about 3 minutes.
[0131] Embodiment 56: The method of embodiment 54 or 55, wherein said mixing is performed using a homogenizer.
[0132] Aspect 57: The method described in aspect 56, wherein the homogenizer is operated at a speed of at least 1000 rpm, for example from about 1000 to about 9000 rpm.
[0133] Aspect 58: The method of any one of aspects 48-50 or 54-57, wherein the water-immiscible liquid is selected from the group consisting of mineral spirits, hexane, heptane, kerosene, octane, toluene, other hydrocarbons, and combinations thereof.
[0134] Aspect 59: The method of aspect 58, wherein the water-immiscible liquid is mineral spirits.
[0135] Embodiment 60: The method of any one of embodiments 48-50 or 54-59, wherein the water-immiscible liquid further comprises a surfactant dissolved therein.
[0136] Aspect 61: The method of aspect 60, wherein the surfactant is present at a concentration of about 1 to 2% by weight relative to the water-immiscible liquid.
[0137] Embodiment 62: The method of any one of embodiments 48 to 61, further comprising separating the beads of the organogel formed in step (c1) before drying.
[0138] Aspect 63: The method of aspect 62, wherein separating comprises decanting the water-immiscible liquid and optionally recycling the water-immiscible liquid.
[0139] Example 64: The method of example 62 or 63, wherein the beads have an average size in the range of about 5 to about 30 microns.
[0140] Aspect 65: The method of any one of aspects 62 to 64, further comprising washing the gel beads with water, a C1 to C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.
[0141] Example 66: The method of any one of Examples 19 to 65, wherein at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 250 nm, or less than 150 nm.
[0142] Aspect 67: The method of any one of aspects 19 to 66, wherein the drying step (c2) is spray drying.
[0143] Example 68: An agglomerated particle comprising porous carbon matrix particles and a plurality of cathode material particles at least partially embedded within the matrix particles, the agglomerated particle obtained by or obtainable by the method of any one of examples 19-67.
[0144]
[0046] Aspect 69: The agglomerated particle of aspect 68, wherein a weight ratio of carbon in the matrix material to cathode material is less than 30:70, less than 10:90, or less than 5:95.
[0145] Embodiment 70: An electrode comprising the agglomerated particles of any one of embodiments 1-18 or 68-69.
[0146] Embodiment 70: An energy storage device comprising the agglomerated particles of any one of embodiments 1-18 or 68-69.
[0147] Example 71: The energy storage device of example 70, which is a Li-ion battery.
[0148] To provide an understanding of aspects of the present technology, reference is made to the accompanying drawings, which are not necessarily drawn to scale. These aspects are illustrated in the accompanying drawings by way of example and not by way of limitation. It should be noted that references to "an" or "one" aspect in this disclosure do not necessarily refer to the same aspect, but rather mean at least one. [Brief description of the drawings]
[0149] [Figure 1] FIG. 1 is a schematic diagram illustrating a method 100 for producing agglomerated particles according to one or more non-limiting embodiments of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram illustrating a further method 200 for producing agglomerated particles according to one or more non-limiting embodiments of the present disclosure. [Diagram 3] FIG. 3 is a schematic diagram illustrating yet another method 300 for producing agglomerated particles according to one or more non-limiting embodiments of the present disclosure. [Figure 4] FIG. 4 is a schematic diagram illustrating another method 400 for producing agglomerated particles according to one or more non-limiting embodiments of the present disclosure. [Figure 5A] FIG. 5A is a schematic diagram of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 5B] FIG. 5B is a schematic diagram of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 6] FIG. 6 is a schematic diagram of an agglomerated particle 600 according to one or more non-limiting embodiments of the present disclosure. [Figure 7] FIG. 7 is a schematic diagram of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 8A] FIG. 8A is a scanning electron micrograph of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 8B] FIG. 8B is a scanning electron micrograph of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 8C] FIG. 8C is a scanning electron micrograph of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 8D] FIG. 8D is a scanning electron micrograph of an agglomerated particle according to one or more non-limiting embodiments of the present disclosure. [Figure 9] FIG. 9 is a first cycle charge / discharge voltage profile including agglomerated particles according to one or more non-limiting embodiments of the present disclosure. [Figure 10] FIG. 10 is a chart showing rate performance including agglomerated particles according to one or more non-limiting embodiments of the present disclosure. [Figure 11] FIG. 11 is a chart showing volume loss with agglomerated particles according to one or more non-limiting embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0150] In the following description, for purposes of explanation, numerous specific details are set forth in order to provide a thorough understanding. One or more aspects may be practiced without these specific details. Features described in one aspect may be combined with features described in another aspect. In some instances, well-known structures and devices are described in block diagram form in order to avoid unnecessarily obscuring the present invention.
[0151] I. Overview This disclosure describes LMP-carbon composites in which nanoscale particles of LMP are at least partially embedded within porous carbon particles or beads having an average particle size of 0.5 to 20 microns. As used herein, "LMP" refers to "lithium metal phosphates," including LFP ("lithium iron phosphate," where the metal "M" is iron), LMFP ("lithium iron manganese phosphate," where the metal "M" is a solid solution of manganese and iron), and LVP ("lithium vanadium phosphate," where the metal "M" is vanadium), as well as mixtures thereof, as described herein. In this agglomerated particle configuration, the particles of LMP are physically separated from one another by being embedded in the carbon matrix, which allows kinetically favorable access of the electrolyte to the LMP, supporting high charge and discharge rates without significant loss of capacity.
[0152] In principle, LMPs obtained through any synthesis approach can be ground and used to produce the disclosed LMP-doped carbon aerogel or xerogel composites. However, for cost and scalability optimization, LMPs may be made through the lowest cost implementation, in one example, synthesizing LFPs from iron oxide (hematite), phosphoric acid, lithium carbonate, and a carbon source by solid-state carbothermal reduction. Such as-produced low-cost (and low-quality) LFPs (herein "LC-LFPs") have submicron particle sizes and perform very poorly (e.g., about 20 mAh / g compared to a theoretical specific capacity of 169.9 mAh / g) when used as cathodes in half-cells. Grinding the aforementioned LC-LFPs can increase the capacity to about 80 mAh / g, which is still less than half the theoretical capacity. For example, grinding the same LFPs for several hours increases the capacity to 78 mAh / g, which is significantly higher than the as-produced LC-LFPs, indicating the inhibiting effect of large particle size on the cathode capacity. Despite the four-fold increase, this capacity is still too low for use in many commercial applications, especially transportation applications (e.g., electric vehicles).
[0153] According to the present disclosure, it has surprisingly been found that the battery performance of LC-LFP can be significantly improved when the LC-LFP is embedded in a porous carbon matrix, such as a carbon aerogel or xerogel, in various form factors including monoliths and microbeads. The disclosed LFP-carbon aerogel composite beads show an additional 50% increase in the practical capacity of the LFP compared to the crushed LFP alone, such that capacities of over 145 mAh / g are achievable, whereas the same LFP in pre-carbon agglomerate form may have capacities of less than 100 mAh / g, or even less than 70 mAh / g. A second unexpected advantage is that the agglomerated particle cathode exhibits high rate performance (80% capacity retention at 1C compared to C / 20). As a third advantage, the LFP-doped agglomerated particle cathode exhibits excellent cycle life, with no capacity loss after 500 cycles at 1C charge / discharge rate in a half cell composed of a metallic lithium anode.
[0154] Overall, the newly developed processes to improve the performance of LC-LFPs can be summarized by the following key features and advantages: (1) high specific capacity LFP-carbon aerogel microcomposite beads are obtained from low-cost LC-LFP materials, (2) high rate performance is achieved compared to commercial LFPs, (3) excellent capacity retention is achieved even at high rate cycling, (4) the carbon aerogel used in the LFP / carbon aerogel materials is cost-effective and its production is environmentally friendly, and (5) a new class of LFP materials is developed for diverse applications.
[0155] To produce the disclosed agglomerated particles, LFP produced from any source, including low-cost or bulk LC-LFP, is mixed with a solution of a suitable salt of a polyamic acid to form a slurry. The advantage of this method is that the viscosity of the polyamic acid salt solution is sufficient to keep the particles of LFP in suspension, resulting in good dispersion of the LFP particles throughout the gel and the final product formed. The LFP can be milled to reduce particle size before or after mixing with the aqueous solution, and the LFP can be further processed into various forms, such as solid monolithic or microbead composites of LFP particles in a polymer matrix. In a variation of the microbead composite, microdroplets of aqueous polyamic acid solution containing the LFP suspension become the dispersed phase in a two-phase emulsion and are gelled during dispersion with a suitable gelling initiator (e.g., an acid anhydride such as acetic anhydride, an acid such as acetic acid, or an acid precursor such as acetic anhydride). The resulting gel microbeads can be dried to LFP-doped polyimide or polyamic acid aerogel or xerogel beads, which can be carbonized to LFP-doped carbon aerogel or xerogel microbeads.
[0156] The preparation of monolithic LFP-doped carbon aerogel microcomposites is as described above, except that instead of an emulsification step, a wet suspension and gelation initiator are introduced into a mold to form a monolithic wet organogel. After the gel is dried to form an aerogel or xerogel, the aerogel or xerogel can be ground into a powder form and then pyrolyzed to form agglomerated particles containing a carbon matrix. Alternatively, the slurry is not gelled, but instead spray dried to form a powder containing LFP particles and polymer, which can be pyrolyzed again to form a carbon matrix. The agglomerated particles limit undesirable crystallite growth of the LFP during the carbonization / pyrolysis step, providing a high performance cathode with fast ion and electron transfer rates.
[0157] In a first general method of the disclosure, a slurry of LMP (where M can be Fe, Mn / Fe, or V) and an aqueous solution of polyamic acid salt are contacted with a gelation initiator (such as an anhydride) and the gelation solution is emulsified with a water-immiscible liquid to obtain beads of polyimide gel, which are separated, washed, and dried to form LMP-doped aerogel or xerogel beads. In an alternative emulsification process described herein, the slurry is first emulsified to form liquid beads, which are then gelled using a gelation initiator (such as an acid or anhydride) to form wet gel polyamic acid and / or polyimide beads. Again, these beads are separated, washed, and dried. Third, the emulsification step can be avoided and the slurry can be gelled in a mold using a gelation initiator (such as an acid or anhydride) to form a monolithic wet organogel (polyamic acid and / or polyimide). This monolith can be crushed into particles and then dried to form an aerogel or xerogel.
[0158] To prepare the LFP-doped carbon aerogel microcomposite beads described herein, commercially available low-cost (and low-performance) LC-LFP was ball-milled and incorporated into polyimide or polyamic acid microspheres using an emulsion gelation process. The microspheres were dried to yield low-cost LFP-doped polyimide or polyamic acid xerogels or aerogels, which were carbonized / annealed to form LFP-doped carbon aerogels or xerogels.
[0159] One or more aspects described and / or claimed herein may not be included in this summary section.
[0160] II. Definition The following definitions are provided for terms used in this disclosure: This application uses the terms defined below unless a different meaning is required by the context of the text in which the term appears.
[0161] The articles "a" and "an" are used herein to refer to one or more (i.e., at least one) of the grammatical object of the article. The term "about" is used throughout this specification to describe and account for small variations. For example, the term "about" can refer to ±10% or less or ±5% or less, such as ±2% or less, ±1% or less, ±0.5% or less, ±0.2% or less, ±0.1% or less, or ±0.05% or less. All numerical values herein are modified by the term "about", whether or not expressly stated. Values modified by the term "about" are, of course, inclusive of the specific value. For example, "about 5.0" must include 5.0.
[0162] Within the context of the present disclosure, in some instances, the term "framework" or "framework structure" refers to a network of nanoscale and / or microstructural elements, such as fibrils, struts, and / or colloidal particles, that form the solid structure of a gel or aerogel. The structural elements that make up the framework structure have at least one characteristic dimension (e.g., length, width, diameter) of about 100 angstroms or less. In the example of a pyrolytic or carbonized aerogel, the term "framework" or "framework structure" may refer to an interconnected network of linear fibrils, nanoparticles, a co-continuous network (e.g., a network that transitions between fibrillar and globular morphologies, having aspects of both transitional structures), or a combination thereof. In some instances, the linear fibrils, nanoparticles, or other structural elements can be linked together (in some instances at nodes) to form a framework that defines pores.
[0163] As used herein, the terms "aerogel" and "aerogel material" refer to a solid object, regardless of shape or size, that includes a framework of interconnected solid structures, with a corresponding network of interconnected pores integrated within that framework, and that contains a gas, such as air, as a dispersed interstitial medium. Thus, regardless of the drying method used, an aerogel is an open, non-fluid colloidal or polymeric network that is expanded throughout its entire volume by a gas, and is formed by removing all of the expansion agent (e.g., solvent) from a corresponding wet gel without substantial volume loss or network compression.
[0164] Generally, aerogels have one or more of the following physical and structural characteristics: (a) an average pore size in the range of about 2 nm to about 100 nm; (b) a porosity of about 60% or more; (c) a porosity of about 1, about 10, or about 20 to about 100 or about 1000 m. 2Specific surface area in g / g. Typically, such properties are measured using nitrogen adsorption porosimetry tests and / or helium pycnometry. It can be appreciated that the inclusion of additives such as reinforcing materials or electrochemically active species, e.g., silicon or lithium iron phosphate, can reduce the porosity or specific surface area of the resulting aerogel composite. Densification can also reduce the porosity of the resulting aerogel composite.
[0165] Aerogel materials may also be further characterized by additional physical properties, such as (d) a pore volume of about 2.0 mL / g or more, preferably about 3.0 mL / g or more, (e) a density of about 0.50 g / cc or less, preferably about 0.25 g / cc or less, and (f) at least 50% of the total pore volume containing pores having a pore size between 2 and 50 nm, although characterization of a compound as an aerogel material need not require the compound to meet these additional properties. References herein to "aerogel" include any aerogel or other open-cell porous material that can be characterized as an aerogel, xerogel, cryogel, ambigel, microporous material, etc., regardless of material (e.g., polyimide, polyamic acid, or carbon), unless otherwise indicated.
[0166] In some embodiments, the gel material may be specifically referred to as a xerogel. As used herein, the term "xerogel" refers to a type of aerogel that includes an open, non-fluid colloidal or polymeric network that is formed by removing all swelling agents from a corresponding wet gel without taking any precautions to avoid substantial volume loss or retard compaction. Xerogels typically include a compact structure. Xerogels undergo significant volume loss during atmospheric drying, generally resulting in a porosity of about 40% or less.
[0167] The term "carbon aerogel" or "carbon xerogel" as used herein refers to a porous carbon-based material. Some non-limiting examples of carbon aerogels and xerogels include carbonized aerogels and xerogels, such as carbonized polyimide gels. The term "carbonization" in the context of aerogels and xerogels refers to an organogel (e.g., polyimide) that has undergone pyrolysis to decompose or convert the organogel composition to at least substantially pure carbon. As used herein, the term "pyrolyze" or "pyrolysis" or "carbonization" refers to the heat-induced decomposition or conversion of an organic matrix to pure or substantially pure carbon.
[0168] Monolithic aerogel materials are distinguished from particulate aerogel materials. The term "particulate aerogel materials" refers to aerogel materials in which the majority (by weight) of the aerogel contained in the aerogel material is in the form of particulates, particles, granules, beads, or powders that may be bound together (i.e., via a binder, such as a polymeric binder) or compressed together, but there is no interconnected aerogel nanostructure between the individual particles. Collectively, aerogel materials in this form are considered to have a powder or particulate morphology (as opposed to a monolithic morphology). It should be noted that, although individual particles of a powder have a unitary structure, individual particles are not considered monolithic herein. Incorporation of aerogel powders into electrochemical cells typically involves preparation of a paste or slurry from the powder, casting onto a substrate and drying, and may optionally include calendaring.
[0169] Within the context of the present disclosure, the term "binderless" or "binder-free" (or derivatives thereof) refers to a material that is substantially free of a binder or adhesive to bind the materials together. For example, a monolithic nanoporous carbon material does not contain a binder since its framework is formed as a single continuous interconnected structure. Advantages of not containing a binder include avoiding the effects of binders on electrical conductivity, pore volume, etc. On the other hand, aerogel particles require a binder to bind them together to form a larger functional material, but such larger materials are not considered to be monolithic herein. Furthermore, the term "binder-free" does not exclude the use of a binder altogether. For example, a monolithic aerogel according to the present disclosure can be secured to another monolithic aerogel or non-aerogel material by placing a binder or adhesive on a major surface of the aerogel material. Thus, a binder is used to create a laminated composite and provide electrical contact to a current collector, but the binder does not function to maintain the stability of the monolithic aerogel framework itself.
[0170] As used herein, the term "gelation" or "gel transition" refers to the formation of a wet gel from a polymer system, such as a polyimide or polyamic acid as described herein. At some point during the reaction or process described herein for gelation (defined as the "gel point"), the sol loses fluidity. In this context, gelation progresses from an initial sol state (e.g., a solution of a salt of a polyamic acid), through a highly viscous dispersion state, until the dispersion solidifies and the sol gels (gel point), resulting in a wet gel (e.g., a polyimide or polyamic acid gel). Notably, such definitions of gelation and gel point are simplified and do not take into account the possibility of fluidity under stress, such as the thixotropic behavior of a particular gel. In some aspects, gelation is induced by the addition of a suitable gelation initiator. In other aspects, gelation can be induced by removing the solvent, for example from a solution containing a salt of a polyamic acid. As described herein, such solvent removal can be achieved by a variety of drying techniques, including but not limited to spray drying.
[0171] As used herein, the term "wet gel" refers to a gel in which the mobile interstitial phase within the network of interconnected pores is composed primarily of a liquid phase, such as a conventional solvent or water, a liquefied gas, such as liquid carbon dioxide, or a combination thereof. Aerogels typically require the initial creation of a wet gel, followed by processing and extraction to replace the mobile interstitial liquid phase within the gel with air or another gas. Examples of wet gels include, but are not limited to, alcogels, hydrogels, ketogels, carbonogels, and any other wet gels known to those of skill in the art.
[0172] As used herein, the term "mean / average particle size" is synonymous with D50, meaning that half of the population of particles have a particle size greater than this point and half have a particle size less than this point. Particle size can be measured by laser light scattering or microscopic techniques. Unless otherwise indicated, average particle sizes reported herein are obtained by visual interpretation of SEM images using a calibrated scale bar and image processing software (such as ImageJ). Multiple particles are measured randomly, the results are averaged, and the standard deviation is calculated. Laser diffraction particle size analysis is used for secondary particles and aggregates.
[0173] As used herein, the term "positive electrode" is used synonymously with cathode. Similarly, the term "negative electrode" is used synonymously with anode.
[0174] Within the context of this disclosure, the term "conductivity" refers to a measurement of a material's ability to conduct electric current or other ability to allow electrons to flow through or within a material. Conductivity is specifically measured as the electrical conductivity / susceptance / admittance of a material per unit size of the material. It is usually recorded as S / m (Siemens / meter) or S / cm (Siemens / centimeter). The conductivity or resistivity of a material can be measured by methods known in the art, including, but not limited to, in-line four-point resistivity (using the dual configuration test method of ASTM F84-99). Within the context of this disclosure, unless otherwise stated, conductivity measurements are taken according to ASTM F84 (resistivity (R) measurements obtained by dividing voltage (V) by current (I)). In certain embodiments, the materials of the present disclosure have a conductivity of about 10 S / cm or more, 20 S / cm or more, 30 S / cm or more, 40 S / cm or more, 50 S / cm or more, 60 S / cm or more, 70 S / cm or more, 80 S / cm or more, or a range between any two of these values.
[0175] Within the context of this disclosure, the term "capacity" refers to the amount of specific energy or charge that a battery can store. Capacity is specifically measured as the discharge current that a battery can deliver over time per unit mass. It is usually recorded as ampere-hours or milliampere-hours per gram of total electrode mass, i.e., Ah / g or mAh / g. For example, a battery with a capacity of 1 Ah can deliver a current of 1 ampere for 1 hour and 0.5 amperes for 2 hours. Thus, 1 ampere-hour (Ah) corresponds to 3,600 coulombs of charge. Similarly, the term "milliampere-hour (mAh)" also refers to the unit of storage capacity of a battery, which is 1 / 1,000 of an ampere-hour. The capacity of a battery (especially the cathode) can be determined by methods known in the art, including, but not limited to, applying a fixed constant current load to a fully charged battery until the voltage of the battery reaches a discharge end voltage value, multiplying the constant current by the time to reach the discharge end voltage to obtain the discharge capacity, and dividing the discharge capacity by the weight or volume of the electrode material. Within the context of this disclosure, unless otherwise specified, capacity measurements are obtained according to this method. Unless otherwise specified, capacity is reported at cycle 10 of the battery.
[0176] As used herein, the term "battery cycle life" refers to the number of complete charge / discharge cycles that a battery can perform before its nominal capacity falls below 80% of its initial rated capacity. Cycle life can be affected by various factors that are not significantly affected over time, such as the mechanical strength of the underlying substrate, the connectivity of particles within the cathode material, and the maintenance of interconnectivity in the carbon matrix. It is noted that it is a surprising aspect of certain embodiments of the present invention that these factors are relatively unchanged over time in practice. Cycle life can be measured by methods known in the art, including, but not limited to, cycle testing, in which a battery cell is subjected to repeated charge / discharge cycles at a given current rate and operating voltage. Within the context of the present disclosure, cycle life measurements are obtained according to this method unless otherwise specified. In certain embodiments of the present disclosure, an energy storage device, such as a battery, or an electrode thereof has a cycle life of about 25 cycles or more, 50 cycles or more, 75 cycles or more, 100 cycles or more, 200 cycles or more, 300 cycles or more, 500 cycles or more, 1000 cycles or more, or a range between any two of these values.
[0177] The term "substantially," as used herein, unless otherwise indicated, means the majority of the characteristic, amount, etc. referred to in relation to a particular context (e.g., substantially pure, substantially identical, etc.), e.g., greater than about 95%, greater than about 99%, greater than about 99.9%, greater than 99.99%, or even 100%.
[0178] Although reference may be made herein to "LFPs," the teachings herein are applicable more generally to cathode materials, particularly lithium metal phosphates (LMPs) where the metal may be selected from iron (i.e., LFPs, LiFePO4), vanadium, manganese, or a combination of iron and manganese. The LMPs discussed herein may comprise, consist of, or consist essentially of a single lithium metal phosphate (e.g., LFP) or a mixture thereof (e.g., particles of LFP and LVP, where V=vanadium). Alternatively, or in combination, the LFP materials described herein may be LiFe 1-x Mn x It may also be a continuous solid solution containing a mixture of transition metals such as PO4 (0≦x≦1). The term "LFP" should not be construed as being limited to only iron-containing LFPs, but is used interchangeably with "LMP" + carbon coating.
[0179] III. Aerogel Synthesis As discussed above in the Overview, the present disclosure is directed to LMP-carbon composite particles and their synthesis. These materials, useful for lithium ion battery cathode materials, are referred to herein as "agglomerated particles" or equivalently agglomerated or composite microbeads. Composite particles can be formed by synthesizing LMP particles or obtaining pre-synthesized (e.g., via commercial routes) LMP particles and combining the LMP particles with organogel precursors.
[0180] The methods disclosed herein generally utilize polyamic acid and polyimide wet gels that can be prepared without the use of organic solvents and without the use of organic (e.g., amine) bases. References herein to the preparation of polyamic acid and polyimide wet gels "without the use of organic bases" mean that no carbon-based alkaline substances such as amines are utilized to solubilize the preformed polyamic acid in water or to solubilize the polyamic acid in situ as it is formed (i.e., by reaction of a diamine with a tetracarboxylic dianhydride). For the avoidance of doubt, references to "organic bases" do not include carbonates and bicarbonates, nor do they include carbonates and bicarbonates that contain nitrogen-containing cationic species (such as ammonium or guanidinium).
[0181] Reference herein to an aqueous solution means that the solution is substantially free of organic solvents. The term "substantially free" as used herein with respect to organic solvents means that no organic solvents have been intentionally added and that no organic solvents are present in more than trace amounts. For example, in certain embodiments, the aqueous solution can be characterized as containing less than 1% organic solvent by volume, or less than 0.1% by volume, or less than 0.01% by volume, or even 0% organic solvent by volume. These aqueous-based methods are advantageous in reducing material and waste disposal costs and reducing potential safety and environmental hazards.
[0182] A. Preparation of Polyamic Acid and Polyimide Gel and Aerogel Materials under Aqueous Conditions Utilized herein are methods for preparing polyamic acid and polyimide gel materials under aqueous conditions. The methods generally involve preparing an aqueous solution of a polyamic acid salt without the use of an organic base, followed by converting the polyamic acid salt to a polyamic acid gel or aerogel material, a polyimide gel or aerogel material, or a corresponding carbon aerogel material. Each of these materials and the corresponding method(s) are further described herein below.
[0183] In one embodiment, the method includes providing a polyamic acid and mixing the polyamic acid with a water-soluble carbonate or bicarbonate in water, thereby providing a solution of a salt of the polyamic acid. In such an embodiment, the polyamic acid is a preformed polyamic acid, either a purchased commercially available material or a material prepared from a suitable diamine and a tetracarboxylic anhydride according to conventional known techniques, such as preparation in an organic solvent solution. Suitable preformed polyamic acids are as described below for in situ synthesized polyamic acids. Suitable water-soluble carbonates or bicarbonates are further described below.
[0184] Alternatively, the polyamic acid can be prepared in situ. Thus, in another embodiment, an aqueous solution of a polyamic acid salt is prepared by reacting a water-soluble diamine with a tetracarboxylic dianhydride in the presence of a water-soluble carbonate or bicarbonate. Generally, the diamine is reacted with the tetracarboxylic dianhydride in the presence of the carbonate or bicarbonate to form the polyamic acid salt. Thus, the method includes mixing a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water, and reacting the components to obtain a solution of the polyamic acid salt. The polyamic acid salt contains anionic carboxylic acid groups charge-compensated by cations from the carbonate or bicarbonate, and the polyamic acid salt is water-soluble. Each of the components utilized in the method (e.g., water-soluble diamine, tetracarboxylic dianhydride, water-soluble carbonate or bicarbonate, etc.) is further described below.
[0185] The order of addition of the various components may vary. For example, in some embodiments, the mixing includes dissolving a water-soluble diamine in water to form an aqueous diamine solution, adding a water-soluble carbonate or bicarbonate to the aqueous diamine solution, adding a tetracarboxylic dianhydride to the aqueous solution of the diamine and the water-soluble carbonate or bicarbonate to form a solution, and stirring the solution at a temperature ranging from about 15 to about 60° C. for a period ranging from about 1 hour to about 4 days.
[0186] In some embodiments, the combining includes dissolving a water-soluble diamine in water to form an aqueous diamine solution, adding a tetracarboxylic dianhydride to the aqueous diamine solution to form a suspension, stirring the suspension at a temperature in the range of about 15 to about 60° C. for a period in the range of about 1 minute to about 24 hours, adding a water-soluble carbonate or bicarbonate to the suspension, and stirring the suspension at a temperature in the range of about 15 to about 60° C. for a period in the range of about 1 hour to about 4 days to obtain an aqueous solution of a polyamic acid salt.
[0187] In some embodiments, the mixing comprises adding, simultaneously or in rapid succession, the water-soluble diamine, the tetracarboxylic dianhydride, and the water-soluble carbonate or bicarbonate to water and stirring the resulting mixture at a temperature ranging from about 15 to about 60° C. for a period ranging from about 1 hour to about 4 days to obtain an aqueous solution of the polyamic acid salt.
[0188] A non-limiting general reaction sequence is shown in Scheme 1. In some cases, the reactions are carried out generally according to Scheme 1, and the reagents and products have structures according to the formulae in Scheme 1. Scheme 1. Formation of aqueous solutions of salts of polyamic acids by reaction of monomers in the presence of water-soluble carbonates or bicarbonates. [ka]
[0189] The diamines disclosed herein are generally described as "water-soluble diamines". As used herein, the term "water-soluble diamines" means that the diamines have a significant solubility in water such that synthetically useful concentrations of the diamines are obtained under the conditions utilized in the disclosed methods. For example, diamines suitable for use in the disclosed methods may have a solubility in water at 20°C of at least about 0.01 g per 100 mL, at least about 0.1 g per 100 mL, at least about 1 g per 100 mL, or at least about 10 g per 100 mL.
[0190] In some embodiments, a combination of two or more diamines can be used. A combination of diamines can be used to optimize the properties of the gel material. In some embodiments, a single diamine is used.
[0191] Referring to Scheme I, the structure of the diamine can vary. In some embodiments, the diamine has a structure according to Formula I, where Z is aliphatic (i.e., alkylene, alkenylene, alkynylene, or cycloalkylene) or aryl, each as described herein above. In some embodiments, Z is an alkylene, such as a C2-C12 alkylene or a C2-C6 alkylene. In some embodiments, the diamine is a C2-C6 alkane diamine, such as, but not limited to, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, and ethylenediamine. In some embodiments, the C2-C6 alkylene of the alkane diamine is substituted with one or more alkyl groups, such as methyl.
[0192] In some embodiments, Z is aryl. In some embodiments, the aryl diamine is 1,3-phenylenediamine, methylene dianiline, 1,4-phenylenediamine (PDA), or a combination thereof. In some embodiments, the diamine is 1,3-phenylenediamine. In some embodiments, the diamine is 1,4-phenylenediamine (PDA).
[0193] Continuing with reference to Scheme 1, a tetracarboxylic dianhydride is added. In some embodiments, two or more tetracarboxylic dianhydrides are added. A combination of tetracarboxylic dianhydrides can be used to optimize the properties of the gel material. In some embodiments, a single tetracarboxylic dianhydride is added. The structure of the tetracarboxylic dianhydride can vary. In some embodiments, the tetracarboxylic dianhydride has a structure according to Formula II, where L comprises an alkylene group, a cycloalkylene group, an arylene group, or a combination thereof, each as described herein above. In some embodiments, L comprises an arylene group. In some embodiments, L comprises a phenyl group, a biphenyl group, or a diphenyl ether group. In some embodiments, the tetracarboxylic dianhydride of Formula II has a structure selected from one or more structures provided in Table 1. [Table 1-1] [Table 1-2]
[0194] In some embodiments, the tetracarboxylic dianhydride is selected from the group consisting of pyromellitic dianhydride (PMDA), biphthalic dianhydride (BPDA), oxydiphthalic dianhydride (ODPA), benzophenonetetracarboxylic dianhydride (BTDA), ethylenediaminetetraacetic dianhydride (EDDA), 1,4,5,8-naphthalenetetracarboxylic dianhydride, and combinations thereof. In some embodiments, the tetracarboxylic dianhydride is PMDA.
[0195] The methods disclosed herein utilize water-soluble carbonates or bicarbonates. The water-soluble carbonates or bicarbonates may vary. As used herein, the term "water-soluble" with respect to a salt means that the carbonate or bicarbonate has a significant solubility in water such that a synthetically useful concentration of carbonate or bicarbonate anion is obtained under the conditions utilized in the disclosed methods. For example, a water-soluble carbonate or bicarbonate suitable for use in the disclosed methods may have a solubility in water at 20°C of at least about 0.1 g per 100 mL, at least about 1 g per 100 mL, or at least about 10 g per 100 mL.
[0196] As used herein, the term "carbonate or bicarbonate" refers to an alkaline substance that contains a carbonate or bicarbonate anion, and specifically excludes alkaline substances that contain a carbon-hydrogen covalent bond (i.e., organic bases, including but not limited to alkylamines, arylamines, and heteroaromatic amines). Water-soluble carbonates or bicarbonates suitable for use in the disclosed methods can be further described as non-nucleophilic, meaning that the carbonates or bicarbonates do not participate in chemical reactions by donating an electron pair other than as a proton acceptor.
[0197] In certain embodiments, the water-soluble carbonate or bicarbonate is a carbonate. In other particular embodiments, the water-soluble carbonate or bicarbonate is a bicarbonate. With continued reference to Scheme 1, the water-soluble carbonate or bicarbonate has the general formula M2CO3 or MHCO3, where M is a cationic species having a valence of +1.
[0198] In some embodiments, the cationic species M comprises or is an ammonium ion, a guanidinium ion, or an alkali metal ion. In some embodiments, the cationic species M comprises lithium, sodium, potassium, ammonium, guanidinium, or a combination thereof. In some embodiments, the cationic species M is lithium. In some embodiments, the cationic species M is sodium. In some embodiments, the cationic species M is potassium. In some embodiments, the cationic species M is ammonium (NH4 + In some embodiments, the cationic species M is guanidinium (NH2-C(=NH2 + )-NH2).
[0199] Particularly suitable water-soluble carbonates and bicarbonates include alkali metal carbonates and bicarbonates. In some embodiments, the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and combinations thereof. In some embodiments, the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate.
[0200] In some embodiments, the water soluble carbonate or bicarbonate is selected from the group consisting of ammonium carbonate, ammonium bicarbonate, guanidinium carbonate, and combinations thereof.
[0201] The amount of water-soluble carbonate or bicarbonate salt added may vary and may depend, for example, on the stoichiometry of the particular salt used. For example, one of ordinary skill in the art will recognize that it depends on the charge associated with the particular anionic species (carbonate or bicarbonate) present in the salt. For example, sodium bicarbonate (NaHCO3) contains one equivalent of base (bicarbonate ion, HCO3) that can react with one proton each. -) and one equivalent of sodium ion for each molar equivalent of sodium bicarbonate. In contrast, sodium carbonate (Na2CO3) provides two equivalents of base (carbonate ion, CO3) that can react with two equivalents of protons from each repeat unit of the polyamic acid. 2- ) to provide two equivalents of sodium ion for each molar equivalent of sodium carbonate.
[0202] The amount of water-soluble carbonate or bicarbonate can be expressed as a molar ratio relative to other reactants (e.g., diamine). The molar ratio of water-soluble carbonate or bicarbonate to diamine may need to be optimized for each set of reactants and conditions. In some embodiments, the molar ratio is selected to maintain the solubility of the polyamic acid. In some embodiments, the molar ratio is selected to avoid any precipitation of the polyamic acid. In some embodiments, the molar ratio of water-soluble carbonate or bicarbonate to diamine ranges from about 1 to about 4, or from about 2 to about 3. In some embodiments, the molar ratio is from about 1.0, about 1.1, about 1.2, about 1.3, about 1.4, or about 1.5 to about 1.6, about 1.7, about 1.8, about 1.9, or about 2.0. In some embodiments, the molar ratio of the water-soluble carbonate or bicarbonate to the diamine is about 2.0 to about 2.6, e.g., about 2.0, about 2.1, about 2.2, about 2.3, about 2.4, about 2.5, or about 2.6. Without wishing to be bound by any particular theory, it is believed that in some exemplary embodiments, at least enough base is required to enable neutralization (i.e., to form salts) of substantially all of the free carboxylic acid groups of the polyamic acid. In some embodiments, the amount of water-soluble carbonate or bicarbonate utilized is an amount that neutralizes substantially all of the carboxylic acid groups present in the polyamic acid formed during the reaction.
[0203] In some embodiments, the water-soluble salt is a carbonate, such as lithium carbonate, sodium carbonate, potassium carbonate, ammonium carbonate, or guanidinium carbonate, and the molar ratio of carbonate ion to diamine is from about 1.0 to about 1.3.
[0204] In some embodiments, the water-soluble carbonate or bicarbonate is a bicarbonate, such as lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, or ammonium bicarbonate, and the molar ratio of bicarbonate ion to diamine is from about 2.0 to about 2.6.
[0205] In some embodiments, the amount of water-soluble carbonate or bicarbonate present can be expressed relative to the carboxylic acid groups of the polyamic acid formed during the reaction or otherwise present in the reaction mixture. In some embodiments, the water-soluble carbonate or bicarbonate is a bicarbonate salt, such as lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, or ammonium bicarbonate, and the molar ratio of bicarbonate ions to carboxylic acid groups of the polyamic acid is about 2.0. In some embodiments, the water-soluble carbonate or bicarbonate is a carbonate salt, such as lithium carbonate, sodium carbonate, potassium carbonate, or ammonium carbonate, and the molar ratio of carbonate ions to carboxylic acid groups of the polyamic acid is about 1.0.
[0206] The relative amounts of diamine and dianhydride present can be expressed as a molar ratio. The molar ratio of diamine to dianhydride can vary depending on the desired reaction time, reagent structure, and desired material properties. In some embodiments, the molar ratio is about 0.1 to about 10, such as about 0.1, about 0.5, or about 1 to about 2, about 3, about 5, or about 10. In some embodiments, the ratio is about 0.5 to about 2. In some embodiments, the ratio is about 1 (i.e., stoichiometric), such as about 0.9 to about 1.1. In certain embodiments, the ratio is about 0.99 to about 1.01.
[0207] The molecular weight of the polyamic acid can vary based on the reaction conditions (e.g., concentration, temperature, reaction time, nature of the diamine and dianhydride, etc.). The molecular weight is based on the number of polyamic acid repeat units, as indicated by the value of the integer "n" for the structure of Formula III in Scheme 1. The specific molecular weight range of the polymeric material produced by the disclosed method can vary. In general, the reaction conditions described above can be modified to obtain a gel with desired physical properties without specific consideration of molecular weight. In some embodiments, a proxy value for molecular weight is provided in the viscosity of the polyamic acid salt solution, which is determined by variables such as temperature, concentration, molar ratio of reactants, and reaction time.
[0208] The temperature at which the reaction is carried out can vary. A suitable range is generally from about 4°C to about 100°C. In some embodiments, the reaction temperature is from about 15 to about 60°C, e.g., about 20, about 25, about 30, about 35, about 40, about 45, about 50, about 55, or about 60°C. In some embodiments, the temperature is from about 15 to about 25°C. In some embodiments, the temperature is from about 50 to about 60°C.
[0209] The reaction is allowed to proceed for a period of time, generally until all available reactants (e.g., diamine and dianhydride) have reacted with each other. The time required for the reaction to reach completion may vary depending on the structure, concentration, and temperature of the reagents. In some embodiments, the reaction time is from about 1 minute to about 1 week, e.g., from about 15 minutes to about 5 days, from about 30 minutes to about 3 days, or from about 1 hour to about 1 day. In some embodiments, the reaction time is from about 1 hour to about 12 hours.
[0210] The concentration of the polyamic acid salt in the aqueous solution can vary. For example, in some embodiments, the concentration of the polyamic acid salt in the aqueous solution ranges from about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid. 3 It is.
[0211] B. Polyamic acid (PAA) and polyimide (PI) gel In some embodiments, the method further comprises converting the aqueous solution of the polyamic acid salt to the corresponding polyamic acid gel. Generally, the method of converting the polyamic acid salt solution to the corresponding polyamic acid gel comprises acidifying the polyamic acid salt solution to convert the polyamic salt to a polyamic acid and phase separating the polyamic acid as a wet organogel. Acidification to form the polyamic acid generally follows Scheme 2.
[0212] The method of acidification may vary. For example, in some embodiments, the polyamate salt solution is added to an acid solution, where the acidification of the polyamate salt solution is rapid. Alternatively, the polyamate salt solution may be acidified by adding an acid to the polyamate salt solution. In some embodiments, the polyamate salt solution may be acidified gradually or slowly using conditions or techniques known to those skilled in the art.
[0213] The acid used may vary. For example, mineral or organic acids may be utilized. For example, suitable acids include, but are not limited to, carboxylic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, or acetic acid. Alternatively, acid precursors, meaning materials that generate acids under certain conditions, may be utilized. One non-limiting example of such an acid precursor is acetic anhydride, which upon contact with water and hydrolysis liberates acetic acid. Scheme 2. Formation of polyamic acid gel by reaction of polyamic acid salt with acid [ka]
[0214] In some embodiments, the polyamic acid wet gels prepared as disclosed herein, or the corresponding aerogels described below, contain residual carbonate or bicarbonate(s). Generally, the residual amounts are trace, but the carbonate or bicarbonate and / or associated counter cations (e.g., alkali metal ions, guanidinium ions, etc.) can be detected by analytical methods known to those of skill in the art.
[0215] The resulting polyamic acid gel material can then be dried to form a polyamic acid aerogel. Methods for acidifying and forming polyamic acid gel materials are described, for example, in International Patent Application Publication No. WO2022125835, which is incorporated herein in its entirety. Drying methods to form the corresponding aerogels are further described below.
[0216] In some embodiments, the method further comprises forming a polyimide aerogel from an aqueous solution of a polyamic acid salt. In general, the method comprises imidizing a polyamic acid salt to form a polyimide gel and drying the polyimide gel to form a polyimide aerogel. Methods for imidizing an aqueous solution of a polyamic acid salt are described, for example, in International Patent Application No. PCT / US2021 / 062706 (incorporated herein in its entirety), and suitable methods are also described further below. The corresponding drying method for forming a polyimide aerogel is further described below.
[0217] In some embodiments, imidizing the polyamic acid salt comprises thermally imidizing the corresponding polyamic acid. Irradiation of the wet gel polyamic acid material with microwave frequency energy is one particularly suitable thermal treatment. Compared to conventional heating that relies on slow heat conduction, microwave heating allows for rapid and efficient energy transfer. Thus, microwave heating is particularly suitable for carrying out the thermal imidization reaction of the present invention. In general, the power and time of microwave frequency irradiation are sufficient to convert a significant portion of the amide and carboxyl groups of the polyamic acid to imide groups. As used herein in connection with converting amide and carboxyl groups to imide groups, "significant portion" means that more than 90% of the amide and carboxyl groups are converted to imide groups, for example 95%, 99%, 99.9%, 99.99%, or even 100%.
[0218] In other embodiments, imidizing the polyamic acid salt comprises performing chemical imidization, which comprises adding a gelation initiator to an aqueous solution of a salt of a polyamic acid to form a gelling mixture ("sol"), and allowing the gelling mixture to gel (e.g., in a mold, or poured onto a sheet, or in a variety of other formats such as beads). In such embodiments, the gelation initiator is added to initiate and promote imidization to form a polyimide wet gel from the polyamic acid salt.
[0219] The structure of the gelation initiator may vary, but generally it is at least partially soluble in the reaction solution while having minimal reactivity with aqueous solutions, and is an effective reagent for reacting with the carboxylic acid groups of the polyamic acid salt and promoting imidization of the carboxyl and amide groups of the polyamic acid. One example of a suitable type of gelation initiator is a carboxylic acid anhydride, such as acetic anhydride, propionic anhydride, etc. In some embodiments, the gelation initiator is acetic anhydride.
[0220] In some embodiments, the amount of gelation initiator may vary based on the amount of tetracarboxylic dianhydride or polyamic acid. For example, in some embodiments, the gelation initiator is present in various molar ratios with the tetracarboxylic dianhydride. In some embodiments, the gelation initiator is present in various molar ratios with the polyamic acid. The molar ratio of the gelation initiator to the tetracarboxylic dianhydride or polyamic acid may vary depending on the desired reaction time, the reagent structure, and the desired material properties. In some embodiments, the molar ratio is about 2 to about 10, for example, about 2, about 3, about 4, or about 5 to about 6, about 7, about 8, about 9, or about 10. In some embodiments, the ratio is about 2 to about 5.
[0221] The temperature at which the gelling reaction proceeds can vary, but is generally less than about 50°C, for example, from about 10 to about 50°C, or from about 15 to about 25°C.
[0222] The gelation conditions described above (both acidification and imidization) are general and are intended to be non-limiting with respect to the manner in which gelation is performed. For example, one skilled in the art will recognize the various permutations in which monoliths or beads (including microbeads) may be prepared. For example, contemplated herein are forming monoliths by pouring the gelation mixture into a mold, forming beads of various sizes by dripping or spraying a polyamic acid salt solution into an acidic receiving solution, or forming micron-sized beads of polyamic acid or polyimide gel in an emulsion.
[0223] In some embodiments, polyimide wet gels prepared as disclosed herein, or the corresponding aerogels described below, contain residual carbonate or bicarbonate(s). Generally, the residual amounts are trace, but the carbonate or bicarbonate and / or associated counter cations (e.g., alkali metal ions, guanidinium ions, etc.) can be detected by analytical methods known to those skilled in the art.
[0224] C. Polyamic acid and polyimide aerogels As described herein above, in some embodiments, the method further comprises converting the polyamic acid salt to an aerogel material via the corresponding polyamic acid or polyimide wet gel. Generally, the formation of the aerogel comprises drying the wet gel in one or more stages. In some embodiments, the wet gel (polyamic acid or polyimide) is aged. After aging, the resulting wet gel material can be collected (e.g., removed from the mold) and first washed or solvent exchanged with water to remove unreacted organic salts or acids, and then the primary reaction solvent (i.e., water) present in the wet gel can be replaced in a suitable secondary solvent. Such secondary solvents should be miscible with supercritical fluid carbon dioxide (CO2) and include linear alcohols having one or more aliphatic carbon atoms, diols having two or more carbon atoms, or branched alcohols, cyclic alcohols, alicyclic alcohols, aromatic alcohols, polyols, ethers, ketones, cyclic ethers, or derivatives thereof. In some embodiments, the secondary solvent is water, a C1-C4 alcohol (e.g., methanol, ethanol, propanol, isopropanol, or n-, iso-, or sec-butanol), acetone, tetrahydrofuran, ethyl acetate, acetonitrile, supercritical fluid carbon dioxide (CO2), or a combination thereof. In some embodiments, the secondary solvent is ethanol.
[0225] Once the wet gel has been formed and processed, an extraction method, including processing and extraction techniques, can then be used to at least partially extract the liquid phase of the wet gel from the wet gel material to form an aerogel material (i.e., "drying"). Liquid phase extraction plays an important role in engineering the properties of aerogels, such as porosity and density, and related properties, such as thermal conductivity, among other factors. In general, aerogels are obtained when the liquid phase is extracted from the wet gel in a manner that causes low shrinkage in the porous network and solid framework of the wet gel. The wet gel can be dried using various techniques to obtain an aerogel or xerogel. In an exemplary embodiment, the wet gel material can be dried at ambient pressure, under vacuum (e.g., by freeze drying), under subcritical conditions, or under supercritical conditions to form the corresponding dried gel (e.g., an aerogel, such as a xerogel).
[0226] In some embodiments, it may be desirable to reduce the surface area of the dried gel. If a reduction in surface area is desired, the aerogel can be fully or partially converted into a xerogel with various porosities. The high surface area of the aerogel can be reduced by forcing some of the pores to collapse. This can be done, for example, by soaking the aerogel in a solvent such as ethanol or acetone for a period of time, or by exposing the aerogel to a solvent vapor. The solvent is then removed by drying at ambient pressure.
[0227] Aerogels are typically formed by removing a liquid mobile phase from a wet gel material at temperatures and pressures near or above the critical point of the liquid mobile phase. Once the critical point is reached (near critical) or exceeded (supercritical, i.e., the pressure and temperature of the system are at or above the critical pressure and critical temperature, respectively), a new supercritical phase appears in the fluid, distinct from the liquid or vapor phase. The solvent can then be removed without introducing liquid-vapor interfaces, capillary forces, or any of the associated mass transfer limitations typically associated with receding liquid-vapor boundaries. Furthermore, the supercritical phase is generally more miscible with organic solvents, thus allowing for better extraction. Co-solvents and solvent exchange are also commonly used to optimize the supercritical fluid drying process.
[0228] When evaporation or extraction occurs below the supercritical point, capillary forces generated by the evaporation of the liquid can cause shrinkage and pore collapse within the gel material. Maintaining the mobile phase near or above the critical pressure and temperature during the solvent extraction process mitigates the adverse effects of such capillary forces. In certain aspects of the present disclosure, the use of near-critical conditions just below the critical point of the solvent system may allow for the production of aerogels or compositions with sufficiently low shrinkage to produce a commercially viable end product.
[0229] A variety of techniques can be used to dry the wet gel to provide an aerogel. In an exemplary embodiment, the wet gel material can be dried at ambient pressure, subcritical conditions, or supercritical conditions.
[0230] Both room temperature and high temperature processes can be used to dry the gel material at ambient pressure, in some embodiments, a slow atmospheric drying process can be used in which the wet gel is exposed to air in an open container for a period of time sufficient to remove the solvent, for example ranging from a few hours to a few weeks, depending on the solvent, amount of wet gel, exposed surface area, size of the wet gel, etc.
[0231] In another embodiment, the wet gel material is dried by heating. For example, the wet gel material can be heated in a convection oven for a period of time to evaporate most of the solvent (e.g., ethanol). After partial drying, the gel can be left at ambient temperature to completely dry for a period of time, e.g., hours to days. This drying method produces a xerogel. Notably, according to the present disclosure, wet gels in monolithic form crack when dried, whereas wet gels in bead form have a lower target density Td (e.g., Td=0.05 g cm). 3 ) It was found that the particles retained their spherical shape even when in solution.
[0232] In some embodiments, the wet gel material is dried by freeze drying. "Freeze drying" or "lyophilizing" refers to a low temperature process for removing solvent, which involves freezing the material (e.g., wet gel material), reducing the pressure, and then removing the frozen solvent by sublimation. Because water is an ideal solvent for removal by freeze drying, and because water is the solvent in the methods disclosed herein, freeze drying is particularly suited to aerogel formation from the disclosed polyimide wet gel materials. This drying method produces cryogels, which may closely resemble aerogels.
[0233] Both supercritical and subcritical drying can be used to dry the wet gel material. In some embodiments, the wet gel material is dried under subcritical or supercritical conditions. In an exemplary embodiment of supercritical drying, the gel material can be placed in a high pressure vessel to extract the solvent with supercritical CO2. After removing the solvent, e.g., ethanol, the vessel can be held above the critical point of CO2 for a period of time, e.g., about 30 minutes. After supercritical drying, the vessel is depressurized to atmospheric pressure. Generally, an aerogel is obtained by this process.
[0234] In an exemplary embodiment of subcritical drying, the gel material is dried using liquid CO2 at room temperature at pressures ranging from about 800 psi to about 1200 psi. This operation is faster than supercritical drying; for example, the solvent (e.g., ethanol) can be extracted in about 15 minutes. Generally, aerogels are obtained by this process.
[0235] Several additional aerogel extraction techniques are known in the art, including various approaches using supercritical fluids to dry the aerogel, as well as atmospheric drying techniques. For example, U.S. Patent No. 6,670,402 teaches the injection of supercritical (as opposed to liquid) carbon dioxide into an extractor that is preheated and prepressurized to substantially supercritical conditions or above to extract the liquid phase from the gel via rapid solvent exchange, thereby producing an aerogel.
[0236] In some embodiments, supercritical CO2 conditions are used to extract the liquid phase from the wet gel.
[0237] IV. LFP-Aerogel Agglomerate Particles A. Exemplary process flow for agglomerated particle synthesis 1, 2, 3, and 4 are flow diagrams illustrating some methods according to non-limiting embodiments of the present disclosure. According to FIG. 1, in one embodiment, method 100 is used to synthesize agglomerated particles with embedded LMP particles. In step 102, an aqueous solution of polyamic acid salt is prepared and mixed with cathode material particles in step 104. In step 106, a gelation initiator, such as an acid or an acid anhydride, is added to the mixture to initiate organogel formation to form a polyamide organogel. In step 108, the gelling mixture from step 106 is emulsified to form beads before the gel formation is complete, and the beads are separated and washed in step 110 after gelation. The beads can then be dried in step 112 to form aerogel or xerogel beads with embedded LMP. The beads are then carbonized in step 114 to form the agglomerated particles of the present disclosure.
[0238] Alternatively, according to method 200 of Figure 2, an aqueous solution of polyamic acid salt is prepared in step 202 and mixed with particles of cathode material in step 204. A gelation initiator, such as an acid anhydride, is added to the mixture in step 206 and a gel is formed from the mixture in a mold in step 208. The monolithic gel formed in step 208 is crushed in step 210 and optionally dried in step 212 to form an aerogel or xerogel powder. The powder is carbonized in step 214 to form agglomerated particles according to the present disclosure in the form of a powder.
[0239] 3 illustrates a further alternative method 300 for forming agglomerated particles in the form of beads according to the present disclosure. According to this process 300, an aqueous solution of polyamic acid salt is prepared in step 302 and mixed with particles of cathode material in step 304. The mixture is emulsified in step 306, and then a gelling initiator such as an acid is added in step 308 to gel the emulsion. The formed gel beads are separated in step 310, washed, and then dried in step 312 to form aerogel or xerogel beads with embedded cathode material particles. These beads are then carbonized in step 314 to form agglomerated particles according to the present disclosure.
[0240] A further alternative is shown in Figure 4, which is labeled Process 400. In this embodiment, in step 402, an aqueous solution of polyamic acid salt is prepared. In step 404, particles of cathode material are mixed. In step 406, the mixture is dried, for example by spray drying, to form intermediate xerogel beads and / or powder. The intermediate xerogel beads and / or powder are then carbonized in step 408 to form agglomerated particles according to the present disclosure.
[0241] B.LFP synthesis As described herein, the LMP (M=metal, also referred to as "LFP") materials discussed herein can comprise, consist of, or consist essentially of a single lithium metal phosphate (e.g., an LFP where "F" is iron), or a mixture thereof (e.g., particles of LFP and LVP, where V=vanadium). Alternatively, or in combination, the LFP materials described herein can comprise LiFe 1-x Mn x It may also be a continuous solid solution containing a mixture of transition metals such as LiMePO4 (0≦x≦1). If the metal is Fe or Mn, the formula is LiMePO4. If the metal is V, the formula is Li3V2(PO4)3.
[0242] The present disclosure can utilize LFPs from any source, including commercial sources, and LMPs, including coarse-grained, low-cost LFPs ("LC-LFPs") that have large particle size and poor electrochemical performance, although for purposes of illustration, a general method for synthesizing LMPs is provided.
[0243] LFPs can be synthesized from metal oxide precursor materials. For M=Fe, natural or artificial Fe2O3 is chosen as the precursor for reasons of cost, availability, and low toxicity. For M=Mn, the precursor can be either MnO, Mn2O3, MnO2, or a combination thereof. For M=V, the precursor can be either VO3, VO2, VO5, or a combination thereof. If the average oxidation state of the precursor metal oxide is greater than 2.0 for Mn and Fe precursors and 3.0 for V precursors (i.e., all of those described in this paragraph except MnO and VO3), a carbon source is required during LFP synthesis to quantitatively and stoichiometrically reduce the metal to the Me(II) oxidation state.
[0244] The choice of carbon source will vary depending on the various polymer sources, such as synthetic polymers (polyarylamides, polyimides, polyamides, polybenzoxazines (PBO), phenol-formaldehyde, RF, polyvinylpyrrolidone, polyethylene oxide, polyethylene), biopolymers (starch, cellulose), modified biopolymers (alginate, cellulose acetate, carboxymethylcellulose [CMC], sucrose-citrate polyester), biomass, or simple mono- or disaccharides (sucrose, glucose, fructose).
[0245] In the case of LiMnPO4, which is synthesized from MnO as a precursor, extensive reduction with a carbon source is not necessary due to the Mn(II) oxidation state. In such cases, thickening agents such as CMC or alginic acid can be added up to 0.5% (by weight relative to MnO) to keep the components in suspension throughout the drying process and provide additional protection against accidental oxidation during the heating step (e.g., due to O2 leakage or impurities in the carrier gas).
[0246] In either case, an appropriate amount of carbon source is added so that the residual carbon content of the bulk LMP is 0.1-3 wt %, depending on the carbon source selected.
[0247] A typical LMP synthesis proceeds as follows: 85% H3PO4, HO (1:1 to 10:1 weight ratio to oxide source), Li2CO3, metal oxide, and carbon source / thickener are added to a reaction vessel in any order such that the molar ratio of Li:Fe:P is 1:1:1. Mixing can be accomplished using a variety of techniques, including overhead mechanical mixing, high speed blade mixers, ultrasonic mixers, and recirculating mixers, with mixing times ranging from 15 minutes to 10 hours.
[0248] Drying can be done in a variety of formats, including hot plates, air ovens, forced hot gas dryers (air or N2), conveyor belt ovens, vacuum ovens, tumble dryers, or combinations of the above. Drying temperatures range from room temperature to 200°C.
[0249] The dried LMP is then heat treated at temperatures ranging from 300 to 1000 °C, and various heating methods can be used, for example, conventional furnaces (convection / conduction), microwave furnaces or induction furnaces. Heating times vary from a few minutes to a few hours depending on the heating method. Short heating times are used in microwave and induction heating, while longer heating times are used in conventional furnaces. Heating and cooling rates can be from 1 to 1000 °C / min depending on the heating method.
[0250] The furnace atmosphere can be static or dynamic, either by gas flow or vacuum. In the case of gas flow, inert (Ar or N2) or reducing (H2-Ar or H2-N2 with 5-10% mol hydrogen content) gas mixtures can be used at flow rates of 10 mL / min to 10 L / min per kg of reaction charge. When a reducing atmosphere is present, the amount of reducing C required is proportionally less.
[0251] Heating can also be carried out in air with provisions to minimize O2 leakage into the reaction mixture, such as a muffle furnace under a nitrogen purge or a sealed furnace with an inert or reducing gas blanket. In such cases, an oxygen scavenger, such as carbon felt, can be used above the reaction charge to minimize oxidation of the LMP / C.
[0252] C.LMP grinding Grinding of LMPs to reduce particle size can be carried out in a variety of mills, such as roller mills, planetary ball mills or high speed bead agitator mills, using grinding media such as alumina, zirconia, and stainless steel. Grinding times can vary from a few minutes (high energy mills) to several hours (low energy mills). Rotation can vary from 60 to 10,000 rpm depending on the method.
[0253] Milling can be carried out in a dry or wet mode. For the wet milling method, the bulk LMP powder is dispersed in a liquid phase selected from water, ethanol, isopropanol, ethylene glycol, acetone, or mixtures thereof. The weight ratio of liquid / solids can vary from 0.5:1 to 10:1. The weight ratio of grinding media (balls or rings) to solids can vary from 5:1 to 100:1.
[0254] Milling can be carried out in air or under an inert gas atmosphere, in static (batch) or dynamic (flow) mode, with single or multiple circuit passes. In the case of wet milling, the resulting milled slurry can be used directly for mixing with the polyamic acid salt, or it can be dried according to one of the methods described above, i.e., using a hot plate, air oven, forced hot gas dryer (air or N2), conveyor belt oven, vacuum oven, tumble dryer, or a combination thereof, at a drying temperature ranging from ambient temperature (e.g., about 20°C) to 200°C. The dispersant can be recycled and reused as required. In the case of wet milling, milling can be carried out with or without surfactants. The surfactants can vary from 0.1 to 5% by weight relative to the solid bulk LMP loading.
[0255] After milling, the desired average particle size of the LMPs is less than 250 nm, for example less than 150 nm, with reference to D50 as described herein.
[0256] D. Dispersion of LMPs into gel precursors The aqueous solution of the polyamic acid salt is prepared as described above. Any of the methods described herein can be used to prepare the aqueous solution of the polyamic acid salt as the first step of the disclosed method. For example, the polyamic acid salt can be prepared in situ from a suitable diamine and a tetracarboxylic dianhydride in water as described herein, or the polyamic acid can be prepared separately in a non-aqueous solvent (e.g., dimethylformamide or dimethylacetamide) and dissolved in water using a water-soluble carbonate or bicarbonate as described herein. The inventors have found that, among the methods disclosed herein, particularly advantageous results are obtained when a guanidinium carbonate or bicarbonate salt and / or a lithium carbonate or bicarbonate salt is used to form the aqueous solution of the polyamic acid salt.
[0257] Dispersion of the nanoscale LMPs in the gel precursor solution (i.e., the aqueous solution of the polyamic acid salt) can be accomplished using a variety of methods, such as a high speed mixer, a high shear mixer, a ball mill, or a rotary mixer. The solid-liquid mix ratio, polymer solution concentration, choice of polymer chemistry, and mixing conditions are described in the Examples. In general, the mixing conditions are selected based on several factors, including the scale, type of organogel, its concentration, etc. In general, mixing is performed for a period and under conditions sufficient to disperse the LMP materials in the gel precursor solution.
[0258] For example, in some embodiments, mixing is performed at a speed of at least about 500 rpm, e.g., about 500 to about 5000 rpm. In some embodiments, mixing is performed at a higher speed, e.g., about 1000 to about 9000 rpm, e.g., using a homogenizer. In particular, such high speed mixing is utilized when the method includes forming an emulsion to produce an organogel in the form of beads having the LMP dispersed therein. In some embodiments, mixing is performed for a period ranging from about 1 minute to about 30 minutes, e.g., about 1 minute to about 3 minutes, about 4 minutes to about 15 minutes, or about 5 minutes to about 10 minutes. One of ordinary skill in the art will recognize that mixing speed and mixing time can vary depending on the desired degree of dispersion / emulsification desired.
[0259] In accordance with the present disclosure, it has been found that the viscosity of the gel precursor plays a role in providing particularly advantageous agglomerated particles. In particular, the density of the gel precursor solution should be sufficient to keep the nanoscale LMP particles dispersed and separated from one another such that they remain separated from one another in the resulting organogel. 3 A concentration of (mass of polymer precursor solute per gram of water) can be particularly advantageous for providing adequate dispersion of the LMP particles.
[0260] It is also possible to mill bulk LMP powders in aqueous polyamic acid salt solutions, in which case the "milling" and "dispersion" steps are integrated and no separate dispersion is required, since the polyelectrolyte nature of the polyamic acid solution has a high affinity to wet the oxide-terminated surfaces of the milled LMP particles.
[0261] The disclosed method includes mixing a cathode material containing an LMP (e.g., iron, manganese, vanadium, combinations thereof) into an aqueous solution of a polyamic acid salt to form a slurry. The slurry is later gelled and then dried to form an aerogel or xerogel. The amount of LMP included in the slurry depends on the target ratio of LMP to aerogel in the final product. The LMP can be obtained from any source as described above, preferably from a low-cost source (LC-LFP), but in the context of this disclosure, it is important to add the LMP to form a slurry of nanoscale particles. These can be obtained by milling bulk LMP materials, for example by reducing the average particle size of a commercial product from the micron scale to the submicron and nanoscale.
[0262] Milling can be carried out using wet or dry processes. In a dry milling process, the powder is added to a vessel along with milling media. The milling media typically include zirconium oxide (yttrium stabilized), silicon carbide, silicon oxide, quartz, or stainless steel balls or rods. The particle size distribution of the resulting milled material is controlled by the energy applied to the system and by matching the particle size of the starting material to the size of the milling media. However, dry milling is an inefficient and energy-consuming process. Wet milling is similar to dry milling, in which a milling liquid is added. The advantage of wet milling is that the energy consumption to achieve the same results is 15-50% lower than dry milling. An additional advantage of wet milling is that the milling liquid can protect the milled material from oxidation. Wet milling can also produce finer particles and has been found to result in less particle agglomeration. Thus, in some embodiments, the method includes wet milling.
[0263] Wet milling can be performed using a variety of liquid components. In other embodiments, the grinding liquid or components contained in the grinding liquid are selected to provide a desired surface chemical functionalization of the particles (e.g., LFP particles) during or after grinding. The grinding liquid or components contained in the grinding liquid can also be selected to control the chemical reactivity or crystal morphology of the particles (e.g., LFP particles). In exemplary embodiments, the grinding liquid or components contained in the grinding liquid can be selected based on compatibility or reactivity with downstream materials, processing steps, or applications of the particles (e.g., LFP particles). For example, the grinding liquid or components contained in the grinding liquid can be compatible with, useful in, or identical to a liquid or solvent used in the process of forming or producing an organic or inorganic aerogel material. In yet another embodiment, the grinding liquid can be selected such that the grinding liquid or components contained in the grinding liquid produce a coating on the LFP particle surface, or on intermediate species such as aliphatic or aromatic hydrocarbons, or by cross-linking or producing cross-functional compounds that react with the organic or inorganic aerogel materials.
[0264] In some embodiments, the solvent or mixture of solvents used for wet milling can be selected to control the chemical functionalization of the particles during or after milling. In some embodiments, the LMP can be conveniently milled in situ in the solution of polyamic acid salt used to form the gel in the disclosed method. In this particular embodiment of the method, it is not necessary to perform a separate step of dispersing the milled LMP particles in the solution of polyamic acid salt, since this is already accomplished in the milling process. The polyamic acid solution can wet the oxide-terminated surfaces of the milled LMP particles and achieve excellent uniform dispersion of the LMP particles in the slurry.
[0265] E. Gelation to Form Organogel Processes for forming organogels by gelling aqueous solutions of polyamic acid salts are described herein in the section entitled "Preparation of Polyamic Acid and Polyimide Gel Materials Under Aqueous Conditions," and any of these methods can be used to form gels of the present disclosure from aqueous slurries of polyamic acid salt solutions and LMPs. Processes 1, 2, and 3 below can be configured for the synthesis of aerogel and / or xerogel microbeads. Aerogels and / or xerogel microbeads can be selected for production in these processes by adjusting the processing temperature, solvent, solvent evaporation rate, reaction rate, drying rate, and other factors to maintain the porosity of the wet gel or reduce the porosity of the wet gel (e.g., via pore collapse during drying).
[0266] i. Process 1: Polyimide (PI) gel beads Uniformly disperse the nanosized LMPs obtained by milling into an appropriate amount (depending on the targeted LMP / C aerogel ratio) of aqueous polyamic acid salt using a high-speed mixer at 1000-5000 rpm for 5-15 min.
[0267] Acetic anhydride is added to the resulting slurry as a gelation initiator, the mixture is poured into an aqueous immiscible medium (i.e., a dispersion medium such as mineral spirits, hexane, heptane, kerosene, octane, or other hydrocarbons), and the mixture is emulsified (using a homogenizer) at high speed (1000-9000 rpm). During this process, micron-sized (5-30 μm) LMP / PI wet gel beads are formed. The emulsification process continues for 4-15 minutes.
[0268] Synthesis of LMP / PI wet gel beads can be carried out in the presence or absence of a surfactant. If a surfactant is used, it is dissolved (1-2 wt%) in the immiscible dispersion medium prior to addition of the acidified LMP / polyamic acid salt solution slurry.
[0269] The dispersion medium is separated from the beads mainly by decantation. The dispersion medium is recyclable. The LMP / PI gel beads are washed several times with ethanol to remove traces of dispersion medium. The LMP / PI gel beads are then converted to LMP / PI aerogel or xerogel beads by drying.
[0270] ii. Process 2: Polyamic acid (PAA) gel beads For LMP / PAA bead synthesis, pour the above slurry into a non-aqueous, water-immiscible dispersion medium (mineral spirits, hexane, heptane, kerosene, octane, or other hydrocarbons) and emulsify (using a homogenizer) at high speed (1000-9000 rpm). After mixing for 1-3 minutes (during this time micron-sized (5-30 μm) liquid beads are formed from the aqueous slurry), add acetic acid or acetic anhydride to the mixture (while mixing) to induce gelation of the formed beads.
[0271] LMP / PAA bead synthesis can be carried out in the presence or absence of a surfactant. When a surfactant is used, it is dissolved in the dispersion medium (1-2 wt%) before adding the LMP / polyamic slurry. The dispersion medium is separated from the beads mainly by decantation. The dispersion medium is recyclable. The LMP / PAA gel beads are washed several times with ethanol to remove traces of the dispersion medium. The LMP / PAA gel beads are subsequently converted to LMP / PAA aerogel or xerogel beads by drying.
[0272] iii. Process 3: Polyimide (PI) gel monolith The nanosized LMPs from milling are uniformly dispersed in an appropriate amount (depending on the targeted LMP / C aerogel ratio) of polyamic acid salt aqueous solution using a high-speed mixer at 1000-5000 rpm for 5-15 min. The resulting slurry is gelled by adding an appropriate amount of acetic anhydride while mixing (using mechanical, magnetic, or other mixing means). The wet monolith gel (LMP / PI) can be milled into small gel chunks (mm size) prior to supercritical drying (to form aerogels) or conventional atmospheric drying (to form xerogels).
[0273] The resulting LMP / PI aerogel (or xerogel) material can be further ground into a powder consisting of micron-sized particles (<50 μm) using a low-energy grinder. Overall, the average particle size D50 of the beads or particles produced by processes 1, 2 and 3 is advantageously between 0.5 and 20 microns, preferably between about 1 micron and 10 microns, e.g. 5 microns. Particle sizes below 1 micron are considered to be easier to disperse in the liquid binder / carbon additive during electrode casting and easier to cast as a uniform thickness film by blade casting techniques, resulting in more reproducible air densities required for anode / cathode pairing, but have certain drawbacks (too small makes working difficult due to dust, static electricity, etc., generally leads to lower tap density of the powder (shape dependent), and lower energy density). In contrast, particle sizes above 10 microns are difficult to cast uniformly, leading to variations in the air capacity of the electrode, and also have a grainy / rough appearance that can cause holes in the separator during cell assembly and stack pressure application.
[0274] F. Spray drying The following process has been found experimentally to produce primarily xerogel microbeads. In an alternative method according to the present disclosure, the aqueous solution of polyamic acid salt is not subjected to the gelation process described above. Instead, LMP particles are dispersed in an aqueous solution of polyamic acid salt as described above, and the resulting slurry is spray dried using techniques known in the art. This involves atomizing the slurry while heating to produce small droplets that have a relatively large surface area and dry quickly. This results in beads of dry droplets that contain cathode material particles and polymer. By controlling the nozzle of the spray drying apparatus and the relative flow rates of the feed (slurry) and drying gas, agglomerated particles having a size of 5-30 μm can be obtained. The agglomerated particles thus formed contain particles of cathode material at least partially encapsulated by polymer from the solution.
[0275] G. Carbonization In some embodiments, the method further comprises converting the organogel (e.g., polyamic acid or polyimide aerogel) to an isomorphous carbon aerogel, the conversion comprising pyrolyzing the respective aerogel under suitable conditions. Thus, in some embodiments, the method further comprises pyrolyzing (e.g., carbonizing) the polyamic acid or polyimide aerogel disclosed herein, which means heating the aerogel at a temperature and for a time sufficient to convert substantially all of the organic material to carbon. As used herein in relation to pyrolysis, "substantially all" means that more than 95% of the organic material is converted to carbon, e.g., 99%, or 99.9%, or even 100% of the organic material is converted to carbon. Pyrolysis of the organic aerogel converts the aerogel to an isomorphous carbon aerogel whose physical properties (e.g., porosity, surface area, pore size, diameter, etc.) are substantially retained in the corresponding carbon aerogel.
[0276] The time and temperature required for pyrolysis can vary. In some embodiments, the polyimide aerogel is exposed to a processing temperature of about 600° C. or higher, such as about 600° C., about 650° C., about 700° C., about 750° C., about 800° C., about 850° C., about 900° C., or about 950° C., or a range between any two of these values, for carbonization of the aerogel. Generally, pyrolysis is carried out under an inert atmosphere to prevent combustion of the organic or carbonaceous materials. Suitable atmospheres include, but are not limited to, nitrogen, argon, or combinations thereof. In some embodiments, pyrolysis is carried out under nitrogen.
[0277] The agglomerated particles produced by the above methods, including, for example, aerogels, xerogels, or spray-dried particles, are further carbonized as described above. This requires heating the material for a time sufficient to convert substantially all of the organic material (polymer) to carbon. As described above, pyrolysis (carbonization) can be carried out at a variety of temperatures, from above 650°C to 1000°C. In accordance with the present disclosure, it has been found that a temperature of 800°C can be particularly advantageous for pyrolyzing the disclosed agglomerated particles. Higher temperatures can be used when pyrolyzing aerogels or xerogels that do not have embedded cathode material. However, for cathode materials such as the lithium metal phosphate particles described herein, there is a risk that as the temperature increases, undesired crystallization of the LMP material may form, which can lead to reduced electrochemical performance. However, in accordance with the present disclosure, it has been found that the porous nature of the polymer network surrounding the LMP in the agglomerated particles inhibits these undesired changes in crystal structure. Thus, in accordance with the present disclosure, carbonization can be carried out at temperatures of about 650°C to about 1000°C, or 650°C to about 800°C. Carbonization times may vary depending on the temperature used; for example, carbonization at about 800°C may be carried out for 5-10 hours, e.g., 8 hours, while carbonization at lower or higher temperatures may require longer or shorter times, respectively, for maximum carbonization (i.e., all of the organogel is converted to carbon).
[0278] According to the present disclosure, it is possible to tailor the amount of carbon in the final agglomerated particles. For example, in some embodiments, it is desirable to prepare agglomerated particles with a carbon percentage suitable for use in Li-ion batteries, where the amount of carbon is sufficient to provide the necessary conductivity for the LMP without creating too much dead space / dead mass in the final battery to hold a charge. Commercially available LFP-carbon materials may contain about 3% carbon, and therefore about 97% LFP.
[0279] The percentage of carbon in the agglomerate particles can be calculated using the following formula:
number
[0280] As an example, 50 g of organogel precursor with a concentration of 0.05 g per gram of solution and a carbonization yield of 0.4 is used with 10 g of LMP, resulting in agglomerated particles with 9% C and 91% LMP. The above formula only calculates the carbon resulting from carbonization of the polymer gel. There may be additional residual carbon from the LMP synthesis process, which also contributes to the carbon in the agglomerated particles. This is expected to be a maximum of about 4%, and less than 1% (e.g., 0.5%).
[0281] H.Material properties A representation of an agglomerated particle 500 according to the present disclosure is shown in Figures 5A and 5B. The particle 500 is substantially spherical and porous, as shown in Figure 5A, which is a perspective view and shows visible pores 512, 520 on the surface of the particle. Also evident from Figure 5A is the presence of partially embedded LFP particles 508 that protrude to some extent within the core 504 of the particle 500.
[0282] Figure 5B is a cross-sectional view through dotted line XX in Figure 5A and shows the same empty surface pores 520 and empty interior pores 516. Figure 5B also shows occupied interior pores 528 containing fully embedded LFP particles 532. Figure 5B also shows LFP particles 524 that are partially embedded and therefore protruding through the surface of agglomerate particle 500.
[0283] In general, the agglomerated particles of the present disclosure are substantially spherical particles with a diameter of 50 mm or less. 2 / g or more than 100m 2The beads have a high internal surface area that may exceed 100 nm / g. The size of the beads may be 0.5 to 50 μm, 5 to 30 μm, or 1 to 10 μm. The pore size of the agglomerated particles may be about 1 to 50 nm, for example about 10 to about 20 nm.
[0284] The agglomerated particles (e.g., in the form of beads) include particles of cathode material (e.g., including LMP) that are at least partially embedded in a porous carbon matrix, in other words, some of the cathode material (e.g., LMP) particles are completely embedded within the matrix particles, while other cathode material (e.g., LMP) particles protrude from or above the surface of the matrix particles.
[0285] The cathode material (e.g., LMP) particles that are at least partially embedded in the porous carbon matrix are separated from one another by the porous carbon network, meaning that while the cathode material (e.g., LMP) particles may be in close proximity, they are generally not in direct contact with one another (i.e., not adjacent to one another).
[0286] 6 shows a schematic of an agglomerated particle 600 according to the present disclosure having a carbon network 604 surrounding LFP particles 608. While FIG. 6 is merely illustrative, it can again be seen that the LFP particles 608 are held apart by the carbon network 604, with some LFP particles being fully embedded within the particle 600 while other LFP particles are partially embedded and visible on the surface of the particle 600.
[0287] The carbon matrix may have a fibril structure, i.e., a structure that includes fibrils as described above. There may be a hierarchy of carbon fibrils within the matrix. FIG. 7 shows the carbon network 604 of FIG. 7 in more detail. As shown in FIG. 7, the carbon network 704 branches into fibrils 712 at the surface of the LMP particle 708. In some embodiments, the fibrils 721 that are in contact with the LFP surface may be thinner and more dense than those that are not in contact with the LFP particle. Without wishing to be bound by theory, it is believed that the thinner and more dense fibrils at the surface of the LMP particle help coat the surface of the LFP particle and improve electrical conductivity.
[0288] Figures 8A-8D include four scanning electron micrographs of agglomerate particles according to the present disclosure. Figures 8A and 8B show agglomerate particles with a 75:25 LFP:carbon mass ratio, while Figures 8C and 8D show a 90:10 LFP:carbon mass ratio. Magnification is 10,000X for Figures 8A and 8C and 50,000X for Figures 8B and 8D. Similar to the schematics of Figures 5A and 5B, the SEMs of Figures 8A-8D show substantially spherical agglomerate particles with embedded LFP particles visible on the surface.
[0289] I. Electrochemical properties The agglomerated particles of the present disclosure surprisingly function as very high performance cathode materials with fast ion and electron transfer rates, due at least in part to the well-separated LFP particles in the conductive carbon matrix and the avoidance of undesirable LFP crystal growth upon carbonization of the gel.
[0290] The starting LC-LFP material used in this disclosure may have a capacity of about 20 mAh / g. After grinding, this capacity may improve slightly to about 80 mAh / g. The agglomerated particles containing LFP particles of the present disclosure can achieve capacities in excess of 140 mAh / g, up to about 160 mAh / g.
[0291] As discussed above, in existing prior art LFP materials, it is common to add small amounts of carbon to improve the conductivity of the poorly conductive LFP materials. The amount of carbon should be minimized because the carbon addition represents dead space, i.e., mass in the battery cell that cannot hold a charge. Thus, commercially available LFP-C materials may contain approximately 3% carbon. The agglomerated particles of the present disclosure can be produced with different amounts of carbon, such as 10% or less, 5% or less, 3% or less carbon, by varying the amount of carbon precursor (polymer) during production, as discussed above, with the remainder being LMP.
[0292] Experiments have shown that the agglomerated particles of the present disclosure can have a total capacity (normalized to the mass of LMP and carbon) of about 130 mAh / g at a charge rate of C / 20, even when containing a relatively large amount of carbon (such as 10%, see e.g., FIG. 9 and discussion herein below), which is close to the charge capacity of the commercially available LFP-C as-is test control. Additionally, the agglomerated particles of the present disclosure have improved first cycle coulombic efficiency (FCE) compared to the control sample.
[0293] For agglomerated particles according to the present disclosure, it is expected that higher capacities of 140 mAh / g or more, e.g., 150-160 mAh / g, will be achieved by having a lower amount of carbon since, as described herein above, reducing the carbon content reduces the dead mass.
[0294] The agglomerated particles of the present disclosure have excellent capacity retention. When used as a cathode material, the agglomerated particles retain capacity very well as the C-rate increases, with half cells showing over 80% capacity retention at a C-rate of 1C. In contrast, the control LFP particles lose about 50% capacity at 1C, i.e., only 50% charge retention.
[0295] The agglomerated particles of the present disclosure also exhibit extremely good cycle life: the materials of the present invention show no capacity loss even after hundreds of charging cycles, whereas prior art products are expected to lose approximately 75% of their initial capacity in a direct comparison.
[0296] The agglomerated particles of the present disclosure further demonstrate an increase in the actual capacity of LFP of over 50% compared to simply crushed LFP, resulting in greater than 145 mAh / g capacity being achievable for LFP materials even when starting from lower quality, lower performance, and less expensive bulk LFP. A further unexpected advantage of the agglomerated particles is the high rate performance of at least 80% capacity retention at 1C compared to C / 20. Third, the materials of the present disclosure exhibit excellent cycle life with no capacity loss after 300 cycles at 1C charge / discharge rate in half cells with metallic lithium anodes.
[0297] Experimental Example Two examples of the synthesis of LFP / carbon aerogel materials according to the present disclosure are described.
[0298] J.LC-LFP synthesis 100 g of starting material LC-LFP was prepared as follows: 51.9 g of bulk iron oxide (Fe2O3) was stirred in 200 ml of water for 30 minutes. 74.94 g of phosphoric acid (85%) was added to the slurry and mixed for 30 minutes. 25.22 g of Li2CO3 was then added stepwise to the mixture. The resulting slurry was mixed for an additional hour.
[0299] Separately, a polyamate salt solution was prepared by dissolving 1,4-phenylenediamine (PDA, 14.86 g) in 808 g water, followed by the addition of triethylamine (TEA: 33.44 g, 46.09 mL, 2.4:1 mole / mol ratio to PDA or PMDA) and PMDA (pyromellitic dianhydride 29.97 g, 0.138 mol, 1:1 mole / mol ratio to PDA). A 75.0 g portion of the resulting aqueous polyamate solution was added to the inorganic mixture (as a carbon source for Fe2O3 reduction) and mixed vigorously. The resulting slurry was heated to 130 °C with mixing to remove water. Once completely dried, the LFP precursor solid was ground into a fine powder and then heat treated at 800 °C for 8 h under inert gas. The resulting LFP exhibited primary particle sizes in the range of 1-10 μm and a low specific capacity of 20 mAh / g. The LC-LFP was ball milled for 10 hours to reduce the particle size to less than 500 nm before being used in the LFP / carbon aerogel synthesis according to the present disclosure. After ball milling, the specific capacity of the ground LFP was improved to about 80 mAh / g.
[0300] II.LFMnP(Fe:Mn=2:1) synthesis Step 1: Preparation of mixed oxide precursor. Ferrous sulfate (FeSO4.7H2O, 90.6 g) and manganese sulfate (MnSO4.H2O, 27.5 g) were dissolved in deionized water and mixed for 30 min. This solution was added dropwise to an oxalic acid solution (90.0 g in 500 mL H2O) to give the mixed metal oxalate, Fe 2 / 3 Mn 1 / 3 C2O4.2H2O was formed immediately. After the addition was complete, the precipitate was filtered and washed multiple times with water. After drying, the solid was calcined in an air oven at 350 °C for 1 h, pulverized, and oxidatively decomposed to produce the mixed oxide spinel MnFe2O4. Separately, a polyamate salt solution was prepared by dissolving PDA (14.86 g) in 808 g water, followed by the addition of triethylamine (TEA: 33.44 g, 46.09 mL, 2.4:1 mol / mol ratio to PDA or PMDA) and PMDA (29.97 g, 0.0.138 mol, 1:1 mol / mol ratio to PDA).
[0301] Step 2: Preparation of LFMnP. The mixed oxides obtained in step 1 were ground to a fine powder and stirred in 200 mL of water for 30 min. Phosphoric acid (85%, 56.3 g) was added to this suspension and the mixture was mixed for 30 min. Li2CO3 (19.0 g) was then added stepwise to the mixture, followed by 37.5 g of the above polyamate solution to the oxide-inorganic mixture (as a carbon source for the reduction of ferric iron) and the mixture was mixed vigorously. The resulting slurry was heated to 130 °C with mixing to remove the solvent (water). The dried mixed oxide precursor was ground to a fine powder and heated at 800 °C under inert gas for 8 h.
[0302] III.LVP synthesis Bulk LVP was prepared as follows: Vanadium(V) oxide (VO, 29.6 g) was stirred in 100 mL water for 30 min. To this suspension was added phosphoric acid (85%, 56.30 g) and the mixture was mixed for 30 min. LiCO (18.9 g) was then added stepwise to the mixture. The resulting slurry was mixed for 1 h. Separately, a polyamate salt solution was prepared by dissolving PDA (14.86 g) in 808 g water, followed by the addition of triethylamine (TEA: 33.44 g, 46.09 mL, 2.4:1 mole / mol ratio to PDA or PMDA) and PMDA (29.97 g, 0.138 mol, 1:1 mole / mol ratio to PDA). A 75.0 g portion of the above polyamate solution was added to the inorganic mixture (as a carbon source for the reduction of VO) and the slurry was vigorously mixed. The new slurry was heated to 130° C. with mixing to remove the solvent (water). The dried LVP precursor was ground to a fine powder and heated at 800° C. under inert gas for 8 hours.
[0303] IV. Aqueous preparation of LFP / micron-sized carbon aerogel beads at different weight ratios Micron-sized LFP / polyamic acid gel beads were prepared by gelation of an aqueous solution of the lithium salt of polyamic acid in emulsion. The target density of the polyamic precursor solution was approximately 0.05 g / cm. 3was prepared by dissolving PDA (14.86 g) in 808 g of water, followed by the addition of lithium carbonate (12.13 g, 1.2:1 mole / mol ratio to PDA or PMDA) and stirring the mixture for 5-15 min. PMDA (29.97 g, 0.138 mol, 1:1 mole / mol ratio to PDA) was added to the mixture and the mixture was stirred at room temperature for 24-48 h. The resulting aqueous carbonate solution of polyamic acid had a viscosity of approximately 400-500 cP at room temperature.
[0304] Two different materials (with weight ratios of LFP / micron-sized carbon aerogel beads of 75 / 25 and 90 / 10) were prepared by the sol-gel method. The synthesis procedure started with dispersing ground LC-LFP in the previously prepared polyamic precursor solution. The amount used was determined based on the carbon yield of the polyimide aerogel after carbonization (~43%), the LFP carbon ratio, and the amount of LC-LFP used. For the sample with the nominal 75 / 25 ratio, 6 g of LC-LFP was mixed with 100 g of polyamic precursor solution, and for the sample with the nominal 90 / 10 ratio, 6 g of LC-LFP was mixed with 40 g of polyamic precursor solution.
[0305] The LC-LFP / polyamic precursor solution mixture was mixed for 5 min at 2500 rpm using a high shear mixer in the presence of 2.5 mm zirconia beads (10 g beads for 50 g mixture) to ensure better dispersion of the LFP in the polyamic precursor solution in the resulting slurry.
[0306] Acetic anhydride (3.21 g, 2.97 mL, 4.3 mole / mole ratio to PMDA in polyamic acid for 75 / 25 material, or 1.28 g, 1.19 mL, 4.3 mole / mole ratio to PMDA in polyamic acid for 90 / 10 material) was added to the resulting LFP / polyamic slurry and magnetically stirred for 60 seconds. At the end of that period, the precursor solution was poured into the immiscible phase under shear using a Ross mixer at 4000 rpm. The immiscible phase was prepared by dissolving 8.35 g of surfactant (Hypermer® H70) in 500 mL of mineral spirits. The precursor solution was added to the mineral spirits phase in a 1:4 v / v ratio. After stirring under high shear for 4-5 minutes, the mixture was removed from the Ross mixer and allowed to stand for 1-3 hours.
[0307] The low density phase (mineral spirits solution) was decanted. The gel beads were recovered by vacuum filtration and solvent exchanged with ethanol three times. The ethanol exchanged (washed) gel beads were dried using supercritical CO2 and are referred to as 75 / 25 and 90 / 10 LFP / PI aerogel beads.
[0308] To carbonize the aerogel materials, heat treatment of the two materials was carried out at 800° C. for 8 h under nitrogen flow using a heating gradient and cooling rate of 5° C. / min and 1° C. / min, respectively.
[0309] V. Characteristics and performance of LFP / carbon aerogel Structural and textural properties The 75 / 25 and 90 / 10 materials (figures herein refer to these ratios of LFP / carbon aerogel) have a surface area of 126 m, respectively, as measured by the BET surface area analysis method. 2 / g and 58m 2 / g, which is a relatively high surface area.
[0310] As shown in Figures 8A-8D, SEM micrographs clearly show the sphericity of the agglomerated 75 / 25 material with bead sizes ranging from 1-10 μm and well-dispersed LFP within the carbon aerogel framework. For the LFP / CA 90 / 10 material, the lower amount of PI polymer does not completely contain the LFP agglomerates, resulting in a decrease in sphericity of the microcomposite. Nevertheless, well-separated LFP particles in the porous carbon aerogel are evident.
[0311] Electrochemical performance The LFP-carbon agglomerate particles were cast onto an Al foil current collector and used as the cathode in a coin-cell sized half-cell. For comparison purposes, coin-cells with cathodes containing commercial LFP (purchased from Landt Instruments) were assembled under identical conditions and galvanostatically cycled at various C-rates.
[0312] FIG. 9 shows the voltage profiles and first cycle coulombic efficiency (FCE) of three LFP-carbon agglomerate particles. Clearly, commercial LFP-C provides the highest capacity of 150 mAh / g with FCE slightly lower than 90%. Among the LFP-carbon agglomerate particles, LFP-carbon agglomerate particles 90:10 (LFP:carbon) exhibits higher specific capacity at 130 mAh / g and excellent FCE above 96%. Meanwhile, LFP-carbon agglomerate particles 75:25 exhibits lower specific capacity below 90 mAh / g with FCE slightly higher than 90%. The lower specific capacity and FCE of the high carbon variant of LFP-carbon agglomerate particles is due to the higher carbon content, which contributes to dead mass, higher side reactions, and surface blockage.
[0313] Figure 10 shows the high-rate performance of the LFP-carbon agglomerate particle cathode compared to the commercial LFP. In both LFP-carbon agglomerate particle electrodes, the capacity retention is over 80% as the C-rate increases from C / 20 to 1C, whereas the capacity of the commercial LFP decreases by about 50%. Thus, the LFP-carbon agglomerate particles of the present disclosure have superior high-rate performance.
[0314] Figure 11 shows the cycle life of the LFP-carbon agglomerate particle electrode at 1C cycle rate and compares it with the cycle life of the commercial product. Clearly, the LFP-carbon agglomerate particle electrode has no capacity loss even after 300 cycles, while the commercial sample lost about 75% of its initial capacity over the same period. This demonstrates that the cycle recovery at high rates of the product of the present disclosure is very good.
[0315] Certain U.S. patents, U.S. patent applications, and other materials (e.g., articles) are incorporated by reference in this application. However, the text of such U.S. patents, U.S. patent applications, and other materials is incorporated by reference only to the extent that there is no conflict between such text and the other descriptions and drawings set forth herein. In the event of such a conflict, such conflicting text in the U.S. patents, U.S. patent applications, and other materials incorporated by reference is expressly not incorporated by reference into this patent.
[0316] Further modifications and alternative aspects of the invention will be apparent to those skilled in the art in view of this description. Thus, this description should be interpreted as illustrative only and is intended to teach those skilled in the art the general manner of carrying out the invention. It should be understood that the forms of the invention shown and described herein should be interpreted as examples of embodiments. Elements and materials may be substituted for those shown and described herein, parts and processes may be reversed, and certain features of the invention may be utilized independently, all of which will be apparent to those skilled in the art after having the benefit of this description of the invention. Changes may be made to the elements described herein without departing from the spirit and scope of the invention as set forth in the claims.
[0317] As used in this specification and claims, the terms "comprises" and "comprising" and variations thereof mean that the specified features, steps or integers are included. The terms should not be interpreted as excluding the presence of other features, steps or components. The present invention comprises, consists of, or consists essentially of the features disclosed and claimed.
[0318] The invention may also broadly consist of any combination of the parts, elements, steps, embodiments and / or features referred to or shown herein, individually or collectively, and any two or more of such parts, elements, steps, embodiments and / or features. In particular, one or more features in any of the aspects, embodiments and aspects described herein may be combined with one or more features from any other aspect, embodiment and aspect described herein.
[0319] Protection may be sought for any feature disclosed in any one or more of the publications referenced herein in combination with the present disclosure.
[0320] Although certain exemplary embodiments of the present invention have been described, it is not intended that the appended claims be limited to only those embodiments, and the claims should be construed literally, literal, and / or to encompass equivalents.
Claims
1. matrix particles comprising porous carbon; a plurality of cathode material particles at least partially embedded within the matrix particles; Agglomerate particles containing.
2. The agglomerated particle of claim 1 , wherein the plurality of cathode material particles comprises lithium metal phosphate (LMP) particles.
3. 3. The agglomerated particle of claim 2, wherein the metal (M) of the LMP is selected from the group consisting of Fe, Mn, V, and combinations of Fe and Mn.
4. 4. The agglomerated particle of any one of claims 1 to 3, wherein the matrix particles have a particle size of from 100 nm to 20 microns, or from 1 to 10 microns.
5. The agglomerated particle of any one of claims 1 to 4, wherein at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 250 nm.
6. The agglomerated particle of any one of claims 1 to 5, wherein at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 150 nm.
7. The matrix particles have an internal specific surface area corresponding to the internal pores of 50 m 2 / grams ~ 150m 2 7. The agglomerated particles of any one of claims 1 to 6, wherein the agglomerated particles have a molecular weight of 1 / gram.
8. 8. The agglomerated particle of claim 7, wherein at least a portion of said internal specific surface area is configured to be accessible to an electrolyte.
9. The agglomerated particles of any one of claims 1 to 8, wherein the matrix particles comprise an aerogel or a xerogel.
10. 10. The agglomerated particles of claim 9, wherein the xerogel aerogel is formed as one or more beads or a monolith.
11. 11. The agglomerated particle of claim 9 or 10, wherein the aerogel or xerogel is derived from an organogel comprising a polyimide, a polyamic acid, or a combination thereof.
12. 12. The agglomerated particle of any one of claims 9 to 11, wherein the aerogel or xerogel is a carbonized organogel.
13. 14. The agglomerated particle of any one of claims 1 to 13, wherein the matrix particles have a pore structure that includes a fibril morphology.
14. 14. The agglomerated particle of claim 13, wherein the fibrillar morphology comprises struts of carbonized material having widths in the range of about 2 to about 10 nm.
15. The agglomerated particle of any one of claims 1 to 14, wherein the matrix particles have a substantially uniform pore size distribution.
16. 16. The agglomerated particle of any one of claims 1 to 15, wherein the matrix particles have an average pore size of from about 1 to about 50 nm, or from about 5 to about 25 nm.
17. The agglomerated particle of any one of claims 1 to 16, wherein the matrix particles include pores, at least some of the pores being configured to accommodate the cathode material particles.
18. 18. The agglomerated particle of any one of claims 1 to 17, wherein the weight ratio of carbon in the matrix material to the cathode material is less than 30:70, less than 10:90, or less than 5:
95.
19. 1. A method for preparing an agglomerated particle comprising a porous carbon matrix particle and a plurality of cathode material particles at least partially embedded within the matrix particle, comprising the steps of: (a) preparing an aqueous solution of a salt of a polyamic acid; (b) mixing particles of cathode material with an aqueous solution of a salt of the polyamic acid; (c1) gelling the mixture of step (b) to form an organogel comprising dispersed cathode material particles and drying the organogel of step (c1) to form a dried intermediate; or (c2) drying the mixture of step (b) to form a dried intermediate; (d) carbonizing the dried intermediate to form the agglomerated particles; The method comprising:
20. Preparing an aqueous solution of a salt of the polyamic acid, mixing a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; reacting the components to obtain a solution of a salt of the polyamic acid; 20. The method of claim 19, comprising:
21. The mixing dissolving a water soluble diamine in water to form an aqueous diamine solution; adding said water-soluble carbonate or bicarbonate to said aqueous diamine solution; adding a tetracarboxylic dianhydride to an aqueous solution of the diamine and the water-soluble carbonate or bicarbonate to form a solution; stirring the solution at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days; 21. The method of claim 20, comprising:
22. The mixing dissolving a water soluble diamine in water to form an aqueous diamine solution; adding a tetracarboxylic dianhydride to the aqueous diamine solution to form a suspension; stirring the suspension at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days; adding said water soluble carbonate or bicarbonate to said suspension; stirring the suspension at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days to obtain an aqueous solution of a salt of the polyamic acid; 21. The method of claim 20, comprising:
23. The mixing adding, either simultaneously or in rapid succession, a water-soluble diamine, a tetracarboxylic dianhydride, and a water-soluble carbonate or bicarbonate to water; stirring the resulting mixture at a temperature ranging from about 4 to about 60° C. for a period ranging from about 1 hour to about 4 days to obtain an aqueous solution of the polyamic acid salt; 21. The method of claim 20, comprising:
24. 24. The method of any one of claims 20 to 23, wherein the water-soluble carbonate or bicarbonate comprises a lithium, sodium, potassium, ammonium, or guanidinium cation.
25. 25. The method of any one of claims 20 to 24, wherein the water soluble carbonate or bicarbonate salt is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidinium carbonate, and combinations thereof.
26. the water-soluble carbonate or bicarbonate is a carbonate and the molar ratio of the water-soluble carbonate to the diamine is from about 1 to about 1.4; or the water-soluble carbonate or bicarbonate is a bicarbonate and the molar ratio of the water-soluble bicarbonate to the diamine is from about 2 to about 2.8; The method according to any one of claims 20 to 25.
27. 27. The method of any one of claims 20 to 26, wherein the molar ratio of the tetracarboxylic dianhydride to the diamine is from about 0.9 to about 1.
1.
28. 28. The method of any one of claims 20 to 27, wherein the tetracarboxylic dianhydride is selected from the group consisting of biphthalic dianhydride (BPDA), benzophenone tetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), naphthyl tetracarboxylic dianhydride, perylene tetracarboxylic dianhydride, and pyromellitic dianhydride (PMDA).
29. The method of any one of claims 20 to 28, wherein the diamine is 1,3-phenylenediamine, 1,4-phenylenediamine, or a combination thereof.
30. 30. The method of any one of claims 20 to 29, wherein the diamine is 1,4-phenylenediamine.
31. The concentration range of the polyamic acid salt in the aqueous solution is about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid. 3 The method according to any one of claims 20 to 30, wherein
32. Drying the organogel or intermediate Optionally washing or solvent exchanging the organogel or intermediate; exposing the organogel or intermediate to elevated temperature conditions to freeze-dry the organogel or intermediate or contacting the organogel or intermediate with supercritical fluid carbon dioxide; The method according to any one of claims 19 to 31, comprising:
33. The method of any of claims 19 to 32, wherein the porous carbon matrix comprises an aerogel or a xerogel.
34. The method of any of claims 19 to 33, wherein the carbonization is carried out at a temperature of at least about 650°C under an inert atmosphere.
35. 35. The method of any of claims 19 to 34, wherein the cathode material particles comprise at least one lithium metal phosphate (LMP), the metal (M) being selected from iron, manganese, vanadium, and combinations of iron and manganese.
36. The cathode material particles are LiFePO 4 or consisting essentially of LiFePO 4 The method according to any one of claims 19 to 35, comprising:
37. The method of any of claims 19 to 36, wherein the cathode material is ground before or during step (b).
38. 38. The method of claim 37, wherein the grinding comprises grinding using a roller mill, a planetary ball mill, or a bead agitator mill, optionally using at least one grinding media selected from alumina, zirconia, and stainless steel.
39. 39. The method of claim 37 or 38, wherein the grinding comprises dispersing the cathode material in a liquid phase optionally selected from water, ethanol, isopropanol, ethylene glycol, acetone, or mixtures thereof, and wet-grinding the cathode material.
40. 40. The method of claim 38 or claim 39, wherein the milling comprises dispersing the cathode material in an aqueous solution of a salt of the polyamic acid and wet-milling the cathode material during step (b) to obtain cathode material particles.
41. The method of any of claims 19 to 40, wherein step (b) comprises mixing for a period and under conditions sufficient to disperse the cathode material in the aqueous solution.
42. 42. The method of any of claims 19 to 41, wherein the organogel comprises a polyimide and the gelling in step (c1) comprises adding a gelling initiator to convert the polyamic acid to the polyimide.
43. 43. The method of claim 42, wherein the gelation initiator is acetic anhydride.
44. 44. The method of claim 42 or 43, wherein the gelling of the mixture in step (c1) is carried out in a mold to form a wet gel monolith.
45. 45. The method of claim 44, further comprising breaking the wet gel monolith into a plurality of pieces prior to said drying.
46. 52. The method of claim 50 or 51, further comprising: (e) grinding the dried material of step (c1).
47. 47. The method of claim 46, wherein the milling produces particles having an average particle size D50 of less than about 50 microns.
48. 43. The method of claim 42, wherein step (c1) further comprises, after adding the gelation initiator, mixing the aqueous solution of the salt of the polyamic acid with a water-immiscible liquid to form an emulsion.
49. 49. The method of claim 48, wherein the gelation initiator is acetic anhydride.
50. 50. The method of claim 48 or 49, wherein mixing to form the emulsion is carried out for about 1 to about 30 minutes, or for about 4 to about 15 minutes.
51. 42. The method of any of claims 19 to 41, wherein the organogel comprises a polyamic acid, and the gelling in step (c1) comprises adding a gelling initiator to convert a salt of the polyamic acid into the polyamic acid organogel, and the gelling initiator is an acid.
52. 52. The method of claim 51 , wherein the acid is a carboxylic acid.
53. 53. The method of claim 52, wherein the carboxylic acid is acetic acid.
54. 54. The method of any one of claims 51 to 53, further comprising between steps (b) and (c1) mixing the mixture of step (b) with a water-immiscible liquid to form an emulsion.
55. 55. The method of claim 54, wherein the mixing is carried out for up to about 10 minutes, or from about 1 to about 3 minutes.
56. The method of claims 48-50 or 54-55, wherein the mixing is performed using a homogenizer.
57. 57. The method of claim 56, wherein the homogenizer is operated at a speed of at least 1000 rpm, for example from about 1000 to about 9000 rpm.
58. 58. The method of any of claims 48-50 or 54-57, wherein the water-immiscible liquid is selected from the group consisting of mineral spirits, hexane, heptane, kerosene, octane, toluene, other hydrocarbons, and combinations thereof.
59. 59. The method of claim 58, wherein the water-immiscible liquid is mineral spirits.
60. The method of any of claims 48-50 or 54-59, wherein the water-immiscible liquid further comprises a surfactant dissolved therein.
61. 61. The method of claim 60, wherein the surfactant is present at a concentration of about 1-2% by weight of the water-immiscible liquid.
62. 62. The method of any one of claims 48 to 61, further comprising isolating the organogel beads formed in step (c1) prior to drying.
63. 63. The method of claim 62, wherein the beads have an average size of 5 to 30 microns.
64. 64. The method of claim 62 or 63, wherein separating comprises decanting the water-immiscible liquid and optionally recycling the water-immiscible liquid.
65. 65. The method of any one of claims 62-64, further comprising washing the gel beads with water, a C1-C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.
66. The method of any of claims 19 to 65, wherein at least a portion of the plurality of cathode material particles have an average particle size D50 of less than 250 nm, or less than 150 nm.
67. The method according to any one of claims 19 to 66, wherein the drying step (c2) is spray drying.
68. 68. Agglomerated particles comprising porous carbon matrix particles and a plurality of cathode material particles at least partially embedded within said matrix particles, obtained by or obtainable by the method of any one of claims 19 to 67.
69. 70. The agglomerated particle of claim 68, wherein a weight ratio of carbon in the matrix material to cathode material is less than 30:70, less than 10:90, or less than 5:
95.
70. 70. An electrode comprising the agglomerated particles of any one of claims 1-18 or 68-69.
71. 70. An energy storage device comprising the agglomerated particles of any one of claims 1-18 or 68-69.
72. 72. The energy storage device of claim 71, wherein the energy storage device is a Li-ion battery.
Citation Information
Patent Citations
Making method for nano LiFePO4-carbon composite cathode material
CN101106189A
Lithium iron phosphate / carbon nanometer compound and preparation method and application thereof
CN101630742A
Carbon aerogel network lithium manganese ferric phosphate battery electrode material and preparation method
CN106887586A
Lithium iron phosphate composite positive electrode material, preparation method thereof, lithium-ion battery and capacitor
CN110277541A