ETHYLBENZENE DEHYDROGENATION CATALYST, PREPARATION METHOD THEREOF, AND USE THEREOF

A catalyst with a high CeO2(100) exposed crystal plane area, composed of Fe2O3, K2O, CeO2, MoO3, and CaO, addresses the inefficiencies of existing catalysts by maintaining high activity and stability under low steam/ethylbenzene ratios, enhancing styrene production efficiency and reducing energy costs.

JP2024536466APending Publication Date: 2024-10-04CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024521820
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-11
Filing Date
2022-10-11
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing ethylbenzene dehydrogenation catalysts are less active and less stable under low steam/ethylbenzene ratios, leading to inefficient styrene production with high energy consumption and increased production costs.

Method used

A catalyst comprising Fe2O3, K2O, CeO2, MoO3, and CaO, with a high proportion of CeO2(100) exposed crystal plane area, prepared through a method involving mixing sources, adding an alkaline solution, shaping, and firing, to enhance activity and stability.

Benefits of technology

The catalyst exhibits high activity and stability under low steam/ethylbenzene ratios, maintaining performance for over 1000 hours with improved styrene selectivity and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536466000001_ABST
    Figure 2024536466000001_ABST
Patent Text Reader

Abstract

The present invention relates to an ethylbenzene dehydrogenation catalyst, its preparation method and its use. The catalyst comprises Fe2O3, K2O, CeO2, MoO3 and CaO, and the exposed crystal face area of ​​CeO2(100) accounts for more than 60% of the total exposed crystal face area of ​​CeO2. The catalyst of the present invention is used in the reaction to prepare styrene by dehydrogenating ethylbenzene at a low water ratio, and has high activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] [Technical field] The present invention relates to an ethylbenzene dehydrogenation catalyst, in particular a catalyst for the dehydrogenation of ethylbenzene to prepare styrene at low steam / ethylbenzene ratios, and a process for preparing the same, as well as uses thereof.

[0002] [Background technology] Styrene is an important bulk chemical raw material, mainly used as an important raw material in the synthetic rubber and plastics industries. Styrene has a wide range of applications and occupies an important position in the national economy.

[0003] At present, there are two main routes for producing styrene from ethylbenzene in the world: one is catalytic dehydrogenation of ethylbenzene to produce hydrogen gas and styrene, and the other is co-oxidation of PO / SM. Catalytic dehydrogenation of ethylbenzene has always been the main technological route for producing styrene, and its production capacity accounts for more than 85% of the total styrene production capacity.

[0004] The dehydrogenation of ethylbenzene is a strong endothermic reversible reaction that increases the number of molecules. High temperature and low pressure are suitable for this reaction. In industry, a large amount of hot steam is usually introduced to facilitate the production of the target product, styrene. Steam plays many important roles in the reaction, such as providing the heat required for the reaction; reducing the partial pressure of ethylbenzene and promoting the chemical balance toward styrene; removing the carbon deposited on the catalyst surface by the steam shift reaction; and oxidizing the catalyst surface to maintain catalytic activity. However, using a large amount of superheated steam as the dehydrogenation medium consumes a lot of energy in the process, generates a large amount of condensed water, and generates a lot of costs for the process equipment, resulting in high production costs. Therefore, the ethylbenzene dehydrogenation process aims to achieve a higher styrene yield at a lower steam / ethylbenzene ratio (also called the "water ratio", i.e., the mass ratio of steam to ethylbenzene in the feed). Operating at a low steam / ethylbenzene ratio is one of the important measures for energy saving and consumption reduction. It is urgent for styrene companies to develop styrene catalysts suitable for low steam / ethylbenzene ratios and improve catalytic activity, selectivity, and stability to save energy and reduce consumption in styrene production facilities and reduce production costs.

[0005] Most of the existing styrene catalysts are Fe-K-Ce, with Fe-K oxide as the main catalyst and Ce as the main promoter, and also contain Mg, Mo, W, and Ca oxides as structural stabilizers and electronic assistants. In the ethylbenzene dehydrogenation catalysts with low steam / ethylbenzene ratios disclosed so far, methods for improving the structural stability of the catalyst and methods for modifying the surface properties of the catalyst are mainly used to improve the stability, activity, and selectivity of the catalyst under the condition of low steam / ethylbenzene ratio.

[0006] CN106582678A discloses that based on Fe-K-Ce-W catalyst, oxides of Ba, Sn, and rare earths (Sm, Eu, Gd) are introduced to stabilize the active phase of the catalyst, so as to realize high activity and high stability of the catalyst under the condition of low steam / ethylbenzene ratio.

[0007] CN1981929A discloses that, based on the Fe-K-Ce-W catalyst system, at least two light rare earth oxide additives other than cerium (at least two of La, Pr, Nd, and Sm) are added, and at the same time, at least one metal oxide of Ca oxide, Mg oxide, Ba oxide, B oxide, Sn oxide, Pb oxide, Cu oxide, Zn oxide, Ti oxide, Zr oxide, and Mo oxide is added, thereby improving the stability and activity of the low K catalyst under the condition of low steam / ethylbenzene ratio.

[0008] Today's styrene production technology is developing in the direction of large-scale equipment and comprehensive energy utilization. The development of ethylbenzene dehydrogenation catalysts that are suitable for operation under low steam / ethylbenzene ratio conditions and have higher activity, selectivity and better stability has always been the direction of researchers' efforts.

[0009] Summary of the Invention One of the technical problems that the present invention aims to solve is the problem existing in the existing ethylbenzene dehydrogenation technology, which is that the catalyst has low activity and poor stability under the condition of low steam / ethylbenzene ratio, therefore, a novel ethylbenzene dehydrogenation catalyst for preparing styrene is provided, which has high activity and high stability for ethylbenzene dehydrogenation reaction under the condition of low steam / ethylbenzene ratio.

[0010] The second technical problem that the present invention aims to solve is to provide a method for preparing an ethylbenzene dehydrogenation catalyst for preparing styrene, which corresponds to solving the first technical problem.

[0011] The third technical problem that the present invention aims to solve is to provide the use of an ethylbenzene dehydrogenation catalyst for preparing styrene, which corresponds to the solution of the first technical problem in the production of styrene by ethylbenzene dehydrogenation at a low steam / ethylbenzene ratio.

[0012] In order to solve the above first technical problem, the technical solutions adopted by the present invention are as follows: A first aspect of the present invention provides a catalyst, the catalyst may comprise Fe2O3, K2O, CeO2, MoO3 and CaO; and an area of ​​exposed crystal faces in CeO2(100) accounts for 60% or more of a total area of ​​exposed crystal faces of CeO2.

[0013] In the above technical solution, the main reduction peak position in H2-TPR may be located at 570-620°C.

[0014] In the above technical solution, the catalyst may include the following components in mass fractions based on the total mass of the catalyst: (a) 60%-85% Fe2O3; (b) 6%-14% K2O; (c) 6%-14% CeO2; (d) 0.5%-5% MoO3; (e) 0.3%-7% CaO.

[0015] In the above technical solution, preferably, the catalyst may contain Na2O with a mass fraction of 0.01% to 2.0%.

[0016] In the above technical solutions, the catalyst may also contain other metal oxides, such as TiO2, with a mass fraction of 0.01%-2.0%.

[0017] In the above technical solution, preferably, the area of ​​the exposed crystal planes in CeO2(100) may be 70% or more of the total area of ​​the exposed crystal planes of CeO2; for example, but not limited to, 70%, 75%, 80%, 85%, 87%, 90%, 92%, 95%, 97%, 99% etc. of the total area of ​​the exposed crystal planes of CeO2.

[0018] In the above technical solution, the main reduction peak position in H2-TPR of the catalyst may be located at 570 to 620°C; the main reduction peak position in H2-TPR of the catalyst may be, for example, 570°C, 580°C, 585°C, 590°C, 595°C, 600°C, 605°C, 610°C, 615°C, 620°C, etc., but is not limited thereto.

[0019] In order to solve the second technical problem above, the technical solutions adopted by the present invention are as follows: A second aspect of the present invention provides a method for preparing an ethylbenzene dehydrogenation catalyst as described above, comprising the steps of: a step of uniformly mixing an Fe source, a Ce source, a Mo source, a Ca source, an optional first K source, and an optional pore-forming agent, followed by adding an alkaline solution to allow a static reaction, forming, and calcining to produce a catalyst; Here, the K2O in the catalyst may be derived from the first K source and / or the alkaline solution.

[0020] In the above technical solution, the alkaline solution can be an aqueous solution of potassium hydroxide and / or sodium hydroxide, preferably an aqueous solution of sodium hydroxide and potassium hydroxide. When the alkaline solution is an aqueous solution of sodium hydroxide and potassium hydroxide, the mass ratio of sodium hydroxide as Na2O to potassium hydroxide as K2O is preferably 1:2-23. The concentration of OH groups in the alkaline solution can be 1 mol / L-8 mol / L. In the preparation method of the catalyst, the alkaline solution is used in an amount sufficient for the cerium source to dissolve in the liquid phase required for the reaction.

[0021] In the above technical solution, the K2O in the catalyst can be derived from the first K source and / or the alkaline solution, and preferably, the K2O in the catalyst can be at least partially derived from the alkaline solution. Preferably, at least 50% of the K2O in the catalyst can be derived from the K-containing alkaline solution, and the remaining part is derived from the first K source. Instead of using the first K source, the K2O in the catalyst can also be entirely derived from the K-containing alkaline solution.

[0022] In the above technical solution, the Fe source can be added in the form of oxide Fe2O3. The Fe source is preferably selected from iron oxide red and / or iron oxide yellow, more preferably a composition of iron oxide red and iron oxide yellow, and the mass ratio of iron oxide red as Fe2O3 to iron oxide yellow as Fe2O3 can be 1.0-3.5:1. The first K source can be added in the form of a potassium salt; the potassium salt can be any one or more of potassium carbonate, potassium nitrate, and potassium bicarbonate. The Ce source can be added in the form of a cerium salt; the cerium salt can be cerium nitrate. The Mo source can be added in the form of a molybdenum salt or oxide; the molybdenum salt can be ammonium molybdate. The calcium source can be added in the form of an oxide or hydroxide. The pore former can be any one or more of activated carbon, graphite, sodium carboxymethylcellulose, and polystyrene microspheres. The pore former can be added in an amount of 0-5% by mass relative to the catalyst. In the preparation method of the catalyst, the Fe source, the Ce source, the Mo source, the Ca source, the first K source and the pore-forming agent can all be added in the form of solid-phase powder.

[0023] In the above technical solution, the raw material further includes a Ti source; the Ti source can be uniformly mixed and added with the Fe source, the Ce source, the Mo source, the Ca source, optionally the first K source, and optionally the pore-forming agent. The Ti source can be added in the form of a titanium salt or oxide; the titanium salt can be either one or both of titanium tetrachloride or titanium tetrabromide.

[0024] In the above technical solutions, the mixing can be carried out using conventional mechanical stirring methods.

[0025] In the above technical solution, the condition of the static reaction may include a static reaction at 120 to 180°C for 12 to 48 hours. The vessel used for the reaction is preferably an autoclave. The pressure during the static reaction is not particularly limited, and is, for example, 2 to 20 atm.

[0026] In the above technical solution, the molding can be extrusion molding, and the molded body can be particles with a diameter of 2-5 mm and a length of 3-10 mm. If the material after reaction cannot meet the molding conditions, it can remove part of the moisture by evaporation or other methods, or add an appropriate amount of moisture before molding.

[0027] In the above technical solution, the firing temperature can be 600-1000°C, and the firing time can be 2-8 hours.

[0028] In the above technical solution, the preferred calcination conditions include, but are not limited to, two-stage calcination, for example, calcination at 600-800° C. for 2-4 hours, followed by calcination at 900-1000° C. for 2-4 hours. The calcination can be carried out in a muffle furnace.

[0029] In the above technical solution, the molded sample can be dried first before firing. The drying temperature can be 50-200°C, and the drying time can be 1-24 hours.

[0030] In order to solve the third technical problem, the third aspect of the present invention provides a use of the above ethylbenzene dehydrogenation catalyst in producing styrene by dehydrogenating ethylbenzene.

[0031] In the above technical solution, the use of the ethylbenzene dehydrogenation catalyst in styrene production is suitable for ethylbenzene dehydrogenation with a steam / ethylbenzene ratio of less than or equal to 2.0, preferably 1.3-2.0.

[0032] In the above technical solution, the use of the ethylbenzene dehydrogenation catalyst in the production of styrene is suitable for ethylbenzene dehydrogenation at a low steam / ethylbenzene ratio; the low steam / ethylbenzene ratio is below 1.3, preferably 0.7-1.3.

[0033] In said technical solution, said use includes contacting a feed gas containing ethylbenzene with the above-mentioned catalyst of the present invention in the presence of steam to carry out a dehydrogenation reaction to produce a styrene-containing product.

[0034] In the above technical solutions, the water can be preheated to steam before entering the reactor and thoroughly mixed with the feed gas.

[0035] In the above technical solution, the temperature of the dehydrogenation reaction can be 570-640°C.

[0036] In the above technical solution, the pressure of the dehydrogenation reaction can be 20-100 kPa absolute pressure.

[0037] In the above technical solution, the weight hourly space velocity of ethylbenzene is 0.2-2.0h -1 It can be said that:

[0038] In addition, the present disclosure also includes the following technical solutions: 1. A catalyst comprising Fe, K, Ce, Mo and Ca, and optionally Na; and wherein the area of ​​exposed crystal faces in CeO2(100) is 43% or more, for example 50% or more, preferably 60% or more, more preferably 70% or more, for example 70%, 75%, 80%, 85%, 87%, 90%, 92%, 95%, 97%, 99%, etc., of the total area of ​​exposed crystal faces of CeO2.

[0039] In particular, the area of ​​exposed crystal faces is measured by a characterization method using a high angle dark field scanning transmission electron microscope (HAADF-STEM), such as a FEI Titan Cubed Themis G2 300 double spherical aberration corrected transmission electron microscope; The ratio of the area of ​​exposed crystal planes in CeO2(100) to the total area of ​​exposed crystal planes of CeO2 of the catalyst sample is obtained by collecting and calculating based on HAADF-STEM morphological photographs and the geometric structure characteristics of the catalyst, and at least 100 HAADF-STEM morphological photographs are collected; for each photograph, the area of ​​each exposed crystal plane of CeO2 is obtained, and the area of ​​the maximum exposed crystal plane is taken as the basic standard, and one or more crystal planes having an "exposed crystal plane area" higher than "0.001 × the maximum exposed crystal plane area" are selected, and the total area of ​​the one or more exposed crystal planes is taken as the total area of ​​exposed crystal planes of CeO2, and the ratio is calculated; the ratio is averaged and used as the ratio of the area of ​​exposed crystal planes in CeO2(100) to the total area of ​​exposed crystal planes of CeO2 of the catalyst sample.

[0040] For example, when observing a slice of a HAADF-STEM morphology image of a catalyst sample, the CeO2(100) crystal face is the most exposed. In addition to CeO2(100), only each of CeO2(110), CeO2(111), and CeO2(311) has an exposed crystal face area that is greater than [0.001 × the exposed crystal face area of ​​CeO2(100)], and the sum of the exposed crystal face areas of CeO2(100), CeO2(110), CeO2(111), and CeO2(311) is taken as the total exposed crystal face area of ​​CeO2, and the ratio is calculated to determine the ratio of the exposed crystal face area of ​​CeO2(100) to the total exposed crystal face area of ​​CeO2 in this morphology photograph; in this way, at least 100 HAADF-STEM morphology photographs of the catalyst sample are collected and calculated, and the obtained average value is taken as the ratio of the exposed crystal face area of ​​CeO2(100) to the total exposed crystal face area of ​​CeO2 in the catalyst sample.

[0041] 2. The catalyst according to technical solution 1, wherein Fe and K are present in the form of (K2O)x(Fe2O3)y, where x:y=1:1 to 1:11.

[0042] 3. A catalyst, the composition of which is calculated as oxides and includes Fe2O3, K2O, CeO2, MoO3, and CaO; A catalyst, characterized in that the area of ​​exposed crystal faces in CeO2(100) accounts for 43% or more, for example 50% or more, preferably 60% or more, and more preferably 70% or more of the total area of ​​exposed crystal faces of CeO2.

[0043] 4. The catalyst according to any one of the above technical solutions, characterized in that the main reduction peak position in H2-TPR of the catalyst is located at 570°C to 620°C, for example, 570°C, 580°C, 585°C, 590°C, 595°C, 600°C, 605°C, 610°C, 615°C, or 620°C.

[0044] 5. The catalyst according to any one of the above technical solutions, characterized in that it comprises the following components, in mass fractions based on the total mass of the catalyst: (a) 60%-85% Fe2O3; (b) 6%-14% K2O; (c) 6%-14% CeO2; (d) 0.5%-5% MoO3; (e) 0.3%-7% CaO.

[0045] 6. The catalyst according to technical solution 5, characterized in that it contains 0.01%-2.0% Na2O, in mass fraction based on the total mass of the catalyst.

[0046] 7. The catalyst according to technical solution 5, characterized in that it contains 0.01%-2.0% Na2O and further contains 0.01%-2.0% other metal oxides, such as TiO2, in mass fractions based on the total mass of the catalyst.

[0047] 8. The catalyst according to any one of the preceding technical solutions, characterized in that it is used in ethylbenzene dehydrogenation, preferably in ethylbenzene dehydrogenation at low steam / ethylbenzene ratios.

[0048] 9. A method for preparing the catalyst according to any one of the above technical solutions, characterized in that it comprises the following steps: a step of uniformly mixing an Fe source, a Ce source, a Mo source, a Ca source, an optional first K source, and an optional pore-forming agent, followed by adding an alkaline solution to allow a static reaction, forming, and calcining to produce a catalyst; wherein the KO in the catalyst is derived from a first K source and / or an alkaline solution, e.g., at least 50% of the KO in the catalyst is derived from a K-containing alkaline solution, with the remaining portion being derived from the first K source; or, instead of using the first K source, all of the KO in the catalyst is derived from a K-containing alkaline solution.

[0049] 10. The alkaline solution is an aqueous solution of potassium hydroxide and / or sodium hydroxide, preferably an aqueous solution of sodium hydroxide and potassium hydroxide, and the mass ratio of sodium hydroxide as Na2O to potassium hydroxide as KO is preferably 1:2-23; the concentration of OH groups in the alkaline solution is 1 mol / L-8 mol / L; and / or The preparation method according to technical solution 9, characterized in that the alkaline solution is an aqueous solution of sodium hydroxide and potassium hydroxide, and the mass ratio of sodium hydroxide as Na2O to potassium hydroxide as K2O is preferably 1:2-23.

[0050] 11. The preparation method according to technical solution 9 or 10, characterized in that at least a part of the KO in the catalyst is derived from the alkaline solution; preferably, at least 50% of the KO in the catalyst is derived from the K-containing alkaline solution, and the remaining part is derived from the first K source.

[0051] 12. The preparation method according to any one of technical solutions 9 to 11, characterized in that: the raw material further includes a Ti source; the Ti source is uniformly mixed and added with the Fe source, the Ce source, the Mo source, the Ca source, optionally the first K source, and optionally the pore-forming agent; the Ti source is added in the form of a titanium salt or an oxide; and the titanium salt is preferably either one or both of titanium tetrachloride or titanium tetrabromide.

[0052] 13. The preparation method according to any one of technical solutions 9 to 12, characterized in that the conditions of the static reaction include static reaction at 120 to 180°C for 12 to 48 hours.

[0053] 14. The calcination temperature is 600 to 1000°C, and the calcination time is 2 to 8 hours; The preparation method according to any one of technical solutions 9-13, characterized in that it uses, for example, two-stage calcination, for example, but not limited to, calcination at 600-800 ° C for 2-4 hours, followed by calcination at 900-1000 ° C for 2-4 hours.

[0054] 15. The preparation method according to any one of technical solutions 9 to 14, characterized in that the calcination is carried out in a muffle furnace.

[0055] 16. The preparation method according to any one of technical solutions 9 to 15, characterized in that before firing the molded sample, it first undergoes a drying process in which the drying temperature is 50 to 200 ° C and the drying time is 1 to 24 hours.

[0056] 17. The preparation method according to any one of technical solutions 9 to 16, characterized in that the reaction is carried out under pressure, for example, at 2 to 20 atm (gauge pressure).

[0057] 18. The Ce source is added in the form of a cerium salt, for example the Ce source is cerium nitrate; and / or The Fe source is added in the form of an oxide, Fe2O3, for example, the Fe source is preferably selected from iron oxide red and / or iron oxide yellow, more preferably a composition of iron oxide red and iron oxide yellow, wherein the mass ratio of iron oxide red as Fe2O3 to iron oxide yellow as Fe2O3 is 1.0-3.5:1; and / or The first K source is added in the form of a potassium salt; the potassium salt is any one or more of potassium carbonate, potassium nitrate, and potassium bicarbonate; and / or The Mo source is added in the form of a molybdenum salt or oxide; the molybdenum salt is ammonium molybdate; and / or The calcium source is added in the form of an oxide or hydroxide; Optionally, the pore former is any one or more of activated carbon, graphite, sodium carboxymethylcellulose, and polystyrene microspheres, and the pore former is added in an amount of 0-5% based on the mass of the catalyst; Optionally, in the method for preparing the catalyst, the Fe source, the Ce source, the Mo source, the Ca source, the first K source, and the pore-forming agent are all added in the form of solid-phase powders. The preparation method according to any one of technical solutions 9 to 17, characterized in that

[0058] 19. Use of a catalyst according to any one of technical solutions 1-8 or prepared by a preparation method according to any one of technical solutions 9-18 in the production of styrene by ethylbenzene dehydrogenation.

[0059] 20. The use according to technical solution 19, characterized in that the catalyst is suitable for ethylbenzene dehydrogenation at a low steam / ethylbenzene ratio; the low steam / ethylbenzene ratio is less than or equal to 1.3, preferably 0.7-1.3.

[0060] 21. The use according to technical solution 19, characterized in that the catalyst is suitable for the production of styrene with a steam / ethylbenzene ratio of ≦2.0.

[0061] 22. The use includes a step of contacting a feed gas containing ethylbenzene with the catalyst in the presence of steam to carry out a dehydrogenation reaction to produce a styrene-containing product; The water is preheated to steam before entering the reactor and thoroughly mixed with the feed gas; The temperature of the dehydrogenation reaction is 570 to 640°C; The pressure of the dehydrogenation reaction is an absolute pressure of 20 to 100 kPa; The weight hourly space velocity of ethylbenzene is 0.2 to 2.0 h -1 The use according to any one of technical solutions 19 to 21, characterized in that:

[0062] Compared with the existing technology, the present invention has great advantages and excellent effects, specifically as follows: 1. During the dehydrogenation of ethylbenzene, after H is incorporated into the ethylbenzene molecule, the surface of the catalyst is covered with H and the surface is reduced. In order to restore the reaction activity, it is necessary to remove H2. The active phase potassium ferrite of the Fe-K-Ce-Mo type catalyst has a low removal rate of H2 on the surface, which limits the reaction activity of the catalyst. The H on the surface of the active phase of the catalyst can be transferred to the CeO2 surface by the promotion of water to quickly form H2 and leave the catalyst surface, which reduces the reaction energy barrier, promotes the reaction, and improves the catalytic activity of the catalyst. Through research, the inventors have found that the reaction performance of the Fe-K-Ce-Mo type ethylbenzene dehydrogenation catalyst is greatly related to its surface structure. Different exposed crystal faces of CeO2 will cause significant differences in the dehydrogenation activity and stability of the catalyst. As a result of further research, the inventors have found that the higher the ratio of the exposed crystal face area of ​​CeO2(100) (especially when it is over 60%), the more the reoxidation of the active sites of the catalyst in the ethylbenzene dehydrogenation reaction is promoted, and the higher the reduction temperature of the catalyst in cooperation with the auxiliary, resulting in good activity and stability of the catalyst.

[0063] 2. In the present invention, the inventors have found through research that, in preparing the Fe-K-Ce-Mo type ethylbenzene dehydrogenation catalyst, by controlling the alkalinity of the system and the wet reaction conditions, on the one hand, the surface of the prepared catalyst has a high proportion of exposed crystal faces of CeO2 (100). On the other hand, this preparation method promotes the interaction between the auxiliary components and the active components, and improves the stability of the crystal structure in the catalyst. Compared with the traditional dry method, this preparation method is more conducive to improving the catalytic performance of the ethylbenzene dehydrogenation catalyst. The catalyst preparation method is simple, the obtained catalyst has the advantages of high activity, high styrene selectivity, and the performance of the catalyst is stable after 1,000 hours of operation.

[0064] 3. The catalyst of the present invention is used in the ethylbenzene dehydrogenation reaction to prepare styrene. Under the conditions of low steam / ethylbenzene ratio to high steam / ethylbenzene ratio, especially low steam / ethylbenzene ratio, it has high activity, high selectivity and high stability, and has good technical effect.

[0065] Using the technical solution of the present invention, in an isothermal fixed bed, the absolute pressure is 70 kPa, the liquid hourly space velocity is 1.0 h -1 The activity of the catalyst of the present invention is evaluated at a temperature of 620°C, a steam / ethylbenzene ratio of 0.8 (wt) (a reduction from the commonly used ratio of 2.0 (wt)), and a conversion rate of >75%. Even after 1,000 hours of operation, the catalytic activity is stable and the conversion rate does not change significantly. This shows that the catalyst of the present invention has high activity and high stability when used in the dehydrogenation reaction of ethylbenzene to prepare styrene, especially when the steam / ethylbenzene ratio is low, and has good technical effects.

[0066] Description of the drawings FIG. 1 is a photograph of the major exposed crystal faces in the HAADF-STEM examination of the catalyst of Example 1; FIG. 2 is a photograph of the main exposed crystal faces in the HAADF-STEM test of the catalyst of Comparative Example 1; FIG. 3 is an H2-TPR diagram of the catalysts of Example 1 and Comparative Example 1.

[0067] Detailed Description The present invention will be further described below through examples, but the scope of protection of the present invention is not limited to the examples.

[0068] In the present invention, the area of ​​exposed crystal faces is measured by a characterization method using a high angle dark field scanning transmission electron microscope (HAADF-STEM), and the measuring device is a FEI Titan Cubed Themis G2 300 double spherical aberration corrected transmission electron microscope. The ratio of the area of ​​exposed crystal faces in CeO2(100) to the total area of ​​exposed crystal faces of CeO2 is obtained by collecting HAADF-STEM morphological photographs of the catalyst sample and calculating. That is, the ratio is the ratio of the area of ​​exposed crystal faces in CeO2(100) observed to the total area of ​​exposed crystal faces of CeO2 observed. The total area of ​​exposed crystal faces of CeO2 is the sum of the areas of exposed crystal faces of CeO2(100), CeO2(110), CeO2(111) and CeO2(311). When the exposed crystal surface of CeO2(100) is observed with a scanning transmission electron microscope, two mutually perpendicular directions,

[0020] and

[0002] , can be confirmed within a plane perpendicular to the observation direction of

[0100] . The distance between these planes is both 260~290 pm, proving that the exposed crystal surface is CeO2(100).

[0069] In the present invention, H2-TPR experiments of catalysts are carried out using an AutoChem II 2920 chemisorption apparatus. 0.1 g of catalyst is weighed and placed in a U-shaped quartz reaction tube. First, it is purged with 30 mL / min of high purity Ar gas at 200 °C for 2 h. Then, hydrogen gas is used as the reducing gas and argon gas is used as the balance gas. A mixed gas of 10% H2 / Ar is introduced at a rate of 30 mL / min. The system is heated to a constant temperature at 10 K / min. The consumption of H2 during the heating process is recorded by a TCD detector. The H2-TPR main reduction peak position is the temperature position corresponding to the strongest peak of the signal in the spectrum.

[0070] In this invention, the catalyst of the invention is evaluated for its performance in dehydrogenating ethylbenzene in an isothermal fixed bed. The process can be briefly described as follows: The reactor is a stainless steel tube with an inner diameter of 1'' and is filled with 50-150 mL of catalyst with a diameter of 3-10 mm. Deionized water and ethylbenzene are fed into the preheating mixer through metering pumps. They are preheated and mixed to become gaseous before entering the reactor. The reactor is heated by an electric heating wire to reach a predetermined temperature. The reactants leaving the reactor are condensed with water and analyzed by gas chromatography.

[0071] The ethylbenzene conversion and styrene selectivity are calculated according to the following equations: Ethylbenzene conversion rate (%) = [ethylbenzene concentration before reaction (wt%) - ethylbenzene concentration after reaction (wt%)] / ethylbenzene concentration before reaction (wt%) × 100%, Styrene selectivity (%) = concentration of styrene produced (wt%) / [ethylbenzene concentration before reaction (wt%) - ethylbenzene concentration after reaction (wt%)] × 100%.

[0072] Example 1 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, ammonium molybdate equivalent to 2.8 parts MoO3, calcium oxide 3.2 parts and polystyrene microspheres 3.05 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a mixed aqueous solution of NaOH equivalent to 0.8 parts Na2O and KOH equivalent to 11.2 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.2 mol / L. This mixed solution was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0073] The abundance ratio of K and Fe in the catalyst of Example 1 is K 1.81 Fe 10.73 O 17 which was determined based on XRD crystalline phase analysis.

[0074] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1, and the test results after 1000 hours of reaction are shown in Table 2.

[0075] Example 2 Iron oxide red equivalent to 36.2 parts Fe2O3, iron oxide yellow equivalent to 26.6 parts Fe2O3, cerium nitrate equivalent to 11.6 parts CeO2, ammonium molybdate equivalent to 4.8 parts MoO3, calcium oxide 5.4 parts, and polystyrene microspheres 2.6 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a mixed aqueous solution of NaOH equivalent to 1.8 parts Na2O and KOH equivalent to 13.6 parts K2O was added, and the OH concentration in the mixed aqueous solution was 6.5 mol / L. The mixture was placed in an autoclave and reacted at 120°C for 48 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0076] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0077] Example 3 Iron oxide red equivalent to 45.6 parts Fe2O3, iron oxide yellow equivalent to 23.8 parts Fe2O3, cerium nitrate equivalent to 13.8 parts CeO2, ammonium molybdate equivalent to 3.6 parts MoO3, and calcium oxide 1.5 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Next, a mixed aqueous solution of NaOH equivalent to 0.9 parts Na2O and KOH equivalent to 10.8 parts K2O was added, and the OH concentration in the mixed aqueous solution was 2.5 mol / L. This mixture was placed in an autoclave and reacted at 170°C for 12 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0078] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0079] Example 4 Iron oxide red equivalent to 48.2 parts Fe2O3, iron oxide yellow equivalent to 34.9 parts Fe2O3, cerium nitrate equivalent to 8.3 parts CeO2, ammonium molybdate equivalent to 1.2 parts MoO3, calcium oxide 0.4 parts, and polystyrene microspheres 4.8 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Next, a mixed aqueous solution of NaOH equivalent to 0.8 parts Na2O and KOH equivalent to 6.2 parts K2O was added, and the OH concentration in the mixed aqueous solution was 2.0 mol / L. This mixed solution was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and 150°C for 4 hours, and then placed in a muffle furnace and calcined at 600°C for 4 hours and 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0080] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0081] Example 5 Iron oxide red equivalent to 52.3 parts Fe2O3, iron oxide yellow equivalent to 28.0 parts Fe2O3, cerium nitrate equivalent to 8.1 parts CeO2, ammonium molybdate equivalent to 0.6 parts MoO3, calcium oxide 2.6 parts, and polystyrene microspheres 2.5 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a mixed aqueous solution of NaOH equivalent to 1.0 part Na2O and KOH equivalent to 7.4 parts K2O was added, and the OH concentration in the mixed aqueous solution was 2.6 mol / L. This mixed solution was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 750°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0082] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0083] Example 6 Iron oxide red equivalent to 50.6 parts Fe2O3, iron oxide yellow equivalent to 20.3 parts Fe2O3, cerium nitrate equivalent to 6.9 parts CeO2, ammonium molybdate equivalent to 3.5 parts MoO3, calcium oxide 6.9 parts, titanium oxide 0.06 parts, and polystyrene microspheres 2.6 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a mixed aqueous solution of NaOH equivalent to 0.6 parts Na2O and KOH equivalent to 11.14 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.1 mol / L. This mixture was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 980°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0084] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0085] Example 7 Iron oxide red equivalent to 54.4 parts Fe2O3, iron oxide yellow equivalent to 16.0 parts Fe2O3, cerium nitrate equivalent to 11.2 parts CeO2, 3.0 parts MoO3, calcium carbonate equivalent to 3.2 parts CaO, and 3.1 parts polystyrene microspheres were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a mixed aqueous solution of NaOH equivalent to 1.6 parts Na2O and KOH equivalent to 10.6 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.0 mol / L. This mixed solution was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 50°C for 12 hours and 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0086] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of 620°C, and steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1. The test results after 1000 hours of reaction are shown in Table 2.

[0087] Example 8 Iron oxide red equivalent to 37.5 parts Fe2O3, iron oxide yellow equivalent to 35.1 parts Fe2O3, cerium nitrate equivalent to 11.9 parts CeO2, ammonium molybdate equivalent to 2.1 parts MoO3, calcium carbonate equivalent to 3.3 parts CaO, and activated carbon equivalent to 3.5 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until it was homogenous. Next, a mixed aqueous solution of NaOH equivalent to 1.5 parts Na2O and KOH equivalent to 8.6 parts K2O was added, and the OH concentration in the mixed aqueous solution was 2.8 mol / L. This mixture was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 100°C for 4 hours and 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0088] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0089] Example 9 Iron oxide red equivalent to 40.0 parts Fe2O3, iron oxide yellow equivalent to 32.5 parts Fe2O3, cerium nitrate equivalent to 10.6 parts CeO2, ammonium molybdate equivalent to 2.1 parts MoO3, calcium carbonate equivalent to 2.9 parts CaO, and 3.2 parts graphite were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until it was homogenous. Next, a mixed aqueous solution of NaOH equivalent to 0.5 parts Na2O and KOH equivalent to 11.4 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.5 mol / L. This mixed solution was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 120°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0090] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0091] Example 10 Iron oxide red equivalent to 50.5 parts Fe2O3, iron oxide yellow equivalent to 19.7 parts Fe2O3, cerium nitrate equivalent to 12.0 parts CeO2, 2.6 parts MoO3, 3.5 parts calcium oxide, and 3.2 parts hydroxymethylcellulose were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Next, a mixed aqueous solution of NaOH equivalent to 1.1 parts Na2O and KOH equivalent to 10.6 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.4 mol / L. This mixed solution was placed in an autoclave and allowed to react at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 180°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0092] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0093] Example 11 Iron oxide red equivalent to 50.9 parts Fe2O3, iron oxide yellow equivalent to 23.4 parts Fe2O3, cerium nitrate equivalent to 11.2 parts CeO2, ammonium molybdate equivalent to 1.8 parts MoO3, calcium carbonate equivalent to 2.7 parts CaO, and 3.2 parts graphite were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Next, a mixed aqueous solution of NaOH equivalent to 0.5 parts Na2O and KOH equivalent to 9.5 parts K2O was added, and the OH concentration in the mixed aqueous solution was 2.9 mol / L. This mixed solution was placed in an autoclave and allowed to react at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 200°C for 2 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0094] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0095] Example 12 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, potassium nitrate equivalent to 9.6 parts K2O, ammonium molybdate equivalent to 2.8 parts MoO3, calcium oxide 3.2 parts, and polystyrene microspheres 3.05 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Next, a mixed aqueous solution of NaOH equivalent to 0.8 parts Na2O and KOH equivalent to 1.6 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.2 mol / L. This mixture was placed in an autoclave and allowed to react at 140°C for 20 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and 900°C for 2 hours to obtain a finished catalyst. The catalyst composition is shown in Table 1.

[0096] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of 620°C, and steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1. The test results after 1000 hours of reaction are shown in Table 2.

[0097] Example 13 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, potassium carbonate equivalent to 11.2 parts K2O, ammonium molybdate equivalent to 2.8 parts MoO3, calcium oxide 3.2 parts, and polystyrene microspheres 3.05 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, an aqueous NaOH solution equivalent to 0.8 parts Na2O was added, and the OH concentration in the aqueous solution was 3.2 mol / L. The mixture was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven to dry at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace to calcinate at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0098] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0099] Example 14 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, ammonium molybdate equivalent to 2.8 parts MoO3, 3.2 parts calcium oxide, sodium nitrate equivalent to 0.8 parts Na2O, and 3.05 parts polystyrene microspheres were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a KOH aqueous solution equivalent to 11.2 parts K2O was added, and the OH concentration in the aqueous solution was 3.2 mol / L. The mixture was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven to dry at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace to calcinate at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0100] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1, and the test results after 1000 hours of reaction are shown in Table 2.

[0101] Example 15 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, ammonium molybdate equivalent to 2.8 parts MoO3, 3.2 parts calcium oxide, and 3.05 parts polystyrene microspheres were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until it was homogenous. Then, a KOH aqueous solution equivalent to 11.2 parts K2O was added to make the OH concentration in the aqueous solution 3.2 mol / L. The mixture was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were then dried in an oven at 80°C for 4 hours and at 150°C for 4 hours, and then calcined in a muffle furnace at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0102] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1.

[0103] Comparative Example 1 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, potassium carbonate equivalent to 11.2 parts K2O, ammonium molybdate equivalent to 2.8 parts MoO3, 4.0 parts calcium oxide, and 3.05 parts polystyrene microspheres were weighed and added to a mixer with the same amount of water as in Example 1, and the resulting mixture was stirred for 2 hours until it was uniform. The hydroxyl group concentration in the mixed aqueous solution was 0.3 mol / L. The mixture was placed in an autoclave and allowed to stand at 140°C for 20 hours. The mixture was then extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were then dried in an oven at 80°C for 4 hours and at 150°C for 4 hours, and then calcined in a muffle furnace at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The catalyst evaluation method was the same as in Example 1. The test results and catalyst composition are shown in Tables 1 and 2.

[0104] Comparative Example 2 Iron oxide red equivalent to 39.6 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 21.0 parts CeO2, ammonium molybdate equivalent to 2.8 parts MoO3, calcium oxide 3.2 parts, and polystyrene microspheres 3.05 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until homogeneous. Then, a mixed aqueous solution of NaOH equivalent to 0.8 parts Na2O and KOH equivalent to 11.2 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.2 mol / L. This mixed solution was placed in an autoclave and reacted at 140°C for 20 hours. Then, after adjusting the moisture content, the above mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and at 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0105] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1, and the test results after 1000 hours of reaction are shown in Table 2.

[0106] Comparative Example 3 Yellow iron oxide equivalent to 71.5 parts of Fe2O3 was weighed out and mixed with an aqueous solution of cerium nitrate equivalent to 10.5 parts of CeO2, and then mixed with an aqueous KOH solution equivalent to 11.2 parts of K2O, so that the OH concentration in the mixed aqueous solution was 1.5 mol / L. The resulting paste was dried at 150°C for 2 hours and then fired at 850°C for 2 hours.

[0107] The calcined product was ground, mixed with an aqueous suspension of 2.8 parts MoO3, 3.2 parts calcium oxide, sodium carbonate equivalent to 0.8 parts Na2O, and 3.05 parts polystyrene microspheres, extruded into strips, pelletized to obtain pellets of 3 mm diameter and 6 mm length, dried in an oven at 80°C for 4 hours and at 150°C for 4 hours, and then calcined in a muffle furnace at 650°C for 2 hours and at 900°C for 2 hours to obtain the finished catalyst. The composition of the catalyst is shown in Table 1.

[0108] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1, and the test results after 1000 hours of reaction are shown in Table 2.

[0109] Comparative Example 4 Iron oxide red equivalent to 50.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, potassium carbonate equivalent to 10.64 parts K2O, NaOH equivalent to 0.8 parts Na2O, ammonium molybdate equivalent to 2.8 parts MoO3, calcium oxide 3.2 parts, and polystyrene microspheres 3.05 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until it was uniformly mixed. Then, deionized water was added, and the resulting mixture was stirred for another 0.5 hours, extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were dried in an oven at 80°C for 4 hours and at 150°C for 4 hours, and then calcined in a muffle furnace at 800°C for 4 hours to produce a semi-finished catalyst. Next, potassium carbonate equivalent to 0.56 parts of KO was dissolved in water, and the semi-finished catalyst was impregnated with this solution with an OH concentration of 0.1 mol / L for 2 hours, then dried in an oven at 80°C for 4 hours and at 150°C for 4 hours, and calcined in a muffle furnace at 650°C for 2 hours and at 900°C for 2 hours to obtain a finished catalyst. The composition of the catalyst is shown in Table 1.

[0110] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1, and the test results after 1000 hours of reaction are shown in Table 2.

[0111] Comparative Example 5 Iron oxide red equivalent to 47.1 parts Fe2O3, iron oxide yellow equivalent to 21.4 parts Fe2O3, cerium nitrate equivalent to 10.5 parts CeO2, praseodymium nitrate equivalent to 3.0 parts Pr2O3, ammonium molybdate equivalent to 2.8 parts MoO3, calcium oxide 3.2 parts, and polystyrene microspheres 3.05 parts were weighed and added to a mixer, and the resulting mixture was stirred for 2 hours until it was homogenous. Next, a mixed aqueous solution of NaOH equivalent to 0.8 parts Na2O and KOH equivalent to 11.2 parts K2O was added, and the OH concentration in the mixed aqueous solution was 3.2 mol / L. This mixture was placed in an autoclave and allowed to react at 140°C for 20 hours. Then, after adjusting the moisture content, the mixture was extruded and pelletized to obtain pellets with a diameter of 3 mm and a length of 6 mm, which were placed in an oven and dried at 80°C for 4 hours and 150°C for 4 hours, and then placed in a muffle furnace and calcined at 650°C for 2 hours and 900°C for 2 hours to obtain a finished catalyst. The catalyst composition is shown in Table 1.

[0112] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 0.8 (wt). The test results after 100 hours of reaction are shown in Table 1, and the test results after 1000 hours of reaction are shown in Table 2.

[0113] [Table 1] JPEG2024536466000003.jpg196169

[0114] [Table 2]

[0115] 100 mL of catalyst was placed in the reactor, and the absolute pressure was 70 kPa and the liquid hourly space velocity was 1.0 h -1 The performance evaluation was carried out under the conditions of a temperature of 620°C and a steam / ethylbenzene ratio of 2 (wt). The test results after 100 hours of reaction are shown in Table 3.

[0116] [Table 3]

[0117] From FIG. 1, FIG. 2 and FIG. 3, it can be seen that the main exposed crystal plane of CeO2 in the catalyst of Example 1 is the CeO2(100) crystal plane. The main exposed crystal plane of CeO2 in the catalyst of Comparative Example 1 is the CeO2(111) crystal plane, and the CeO2(111) crystal plane accounts for 52% of the total area of ​​exposed crystal planes of CeO2. The main reduction peak position in H2-TPR of the catalyst of Example 1 is 576°C, which is significantly higher than the main reduction peak position in H2-TPR of the catalyst of Comparative Example 1, which is 545°C. Combining the results of Tables 1 and 2, it can be seen that the catalyst of the present invention has high activity and good stability. In addition, even after the dehydrogenation reaction was carried out for a long period of 1000 hours, the ethylbenzene conversion rate did not decrease significantly.

[0118] Although the preferred embodiments of the present invention have been described in detail above, the present invention is not limited thereto. Within the scope of the technical idea of ​​the present invention, various simple modifications can be made to the technical solutions of the present invention, including combining various technical features in other suitable ways. These simple modifications and combinations should also be considered as the disclosure of the present invention, and all belong to the protection scope of the present invention. [Brief description of the drawings]

[0119] [Figure 1] FIG. 1 is a photograph of the main exposed crystal faces in the HAADF-STEM examination of the catalyst of Example 1. [Diagram 2] FIG. 2 is a photograph of the main exposed crystal faces in the HAADF-STEM test of the catalyst of Comparative Example 1. [Diagram 3] FIG. 3 is an H2-TPR diagram of the catalysts of Example 1 and Comparative Example 1.

Claims

1. The composition is calculated as oxide, Fe 2 O 3 , K 2 O, CeO 2 , MoO 3 and CaO; CeO 2 The area of ​​the exposed crystal plane in (100) is CeO 2 occupying 43% or more, for example 50% or more, preferably 60% or more, and more preferably 70% or more of the total area of ​​exposed crystal faces of said catalyst.

2. The catalyst, H 2 The catalyst according to claim 1, characterized in that the main reduction peak position in -TPR is located at 570°C to 620°C, for example, 570°C, 580°C, 585°C, 590°C, 595°C, 600°C, 605°C, 610°C, 615°C, or 620°C.

3. 3. The catalyst according to claim 1 or 2, characterized in that it comprises, in mass fractions based on the total mass of the catalyst, the following components: (a) 60% to 85% Fe 2 O 3 ; (b) 6% to 14% K 2 O; (c) 6% to 14% CeO 2 ; (d) 0.5% to 5% MoO 3 ; (e) 0.3% to 7% CaO.

4. 0.01% to 2.0% Na in mass fraction based on the total mass of the catalyst 2 The catalyst according to claim 3, characterized in that it contains O.

5. 0.01% to 2.0% Na in mass fraction based on the total mass of the catalyst 2 O, and 0.01% to 2.0% of other metal oxides, such as TiO 2 The catalyst according to claim 3, characterized in that it comprises:

6. Catalyst according to any one of claims 1 to 5, characterized in that it is used in ethylbenzene dehydrogenation, preferably at low steam / ethylbenzene ratios.

7. The method includes the steps of: uniformly mixing an Fe source, a Ce source, a Mo source, a Ca source, an optional first K source, and an optional pore-forming agent, followed by adding an alkaline solution to react by standing, forming, and calcining to produce the catalyst; Here, K in the catalyst 2 O is derived from the first K source and / or the alkaline solution, for example, K in the catalyst 2 At least 50% of the O is derived from the K-containing alkaline solution, and the remaining portion is derived from the first K source; or 2 Instead of using the first K source, all of O is derived from a K-containing alkaline solution; A process for preparing the catalyst according to any one of claims 1 to 6.

8. The alkaline solution is an aqueous solution of potassium hydroxide and / or sodium hydroxide, preferably an aqueous solution of sodium hydroxide and potassium hydroxide, and 2 Sodium hydroxide as O and K 2 The mass ratio of potassium hydroxide as O is preferably 1:2 to 23; the concentration of OH groups in the alkaline solution is 1 mol / L to 8 mol / L; and / or The alkaline solution is an aqueous solution of sodium hydroxide and potassium hydroxide, 2 Sodium hydroxide as O and K 2 The preparation method according to claim 7, characterized in that the mass ratio of potassium hydroxide as O is preferably 1:2-23.

9. K in the catalyst 2 At least a portion of the O comes from the alkaline solution; preferably, the K in the catalyst 2 9. The method according to claim 7 or 8, characterized in that at least 50% of O comes from the K-containing alkaline solution, and the remaining part comes from the first K source.

10. The preparation method according to any one of claims 7 to 9, characterized in that the raw materials further comprise a Ti source; the Ti source is uniformly mixed and added with the Fe source, the Ce source, the Mo source, the Ca source, optionally the first K source, and optionally the pore-forming agent; the Ti source is added in the form of a titanium salt or an oxide; and the titanium salt is preferably either one or both of titanium tetrachloride or titanium tetrabromide.

11. The preparation method according to any one of claims 7 to 10, characterized in that the static reaction conditions include allowing the static reaction to occur at 120 to 180°C for 12 to 48 hours.

12. The firing temperature is 600 to 1000° C., and the firing time is 2 to 8 hours; The preparation method according to any one of claims 7 to 11, characterized in that a two-stage calcination is used, for example but not limited to, calcination at 600-800°C for 2-4 hours, followed by calcination at 900-1000°C for 2-4 hours.

13. A process according to any one of claims 7 to 12, characterized in that the calcination is carried out in a muffle furnace.

14. The preparation method according to any one of claims 7 to 13, characterized in that before firing the molded sample, a drying step is first performed at a drying temperature of 50 to 200 ° C. and a drying time of 1 to 24 hours.

15. The process according to any one of claims 7 to 14, characterized in that the reaction is carried out under pressure, for example at 2 to 20 atm (gauge pressure).

16. The Ce source is added in the form of a cerium salt, for example the Ce source is cerium nitrate; and / or The Fe source is Fe oxide. 2 O 3 For example, the Fe source is preferably selected from iron oxide red and / or iron oxide yellow, more preferably a composition of iron oxide red and iron oxide yellow, and Fe 2 O 3 Iron oxide red as Fe 2 O 3 and the mass ratio of iron oxide yellow to the cation exchange resin is 1.0 to 3.5:1; and / or The first K source is added in the form of a potassium salt; the first K source is added in the form of a potassium salt; the potassium salt is any one or more of potassium carbonate, potassium nitrate, and potassium bicarbonate; and / or The Mo source is added in the form of a molybdenum salt or oxide; the molybdenum salt is ammonium molybdate; and / or The calcium source is added in the form of an oxide or hydroxide; Optionally, the pore former is any one or more of activated carbon, graphite, sodium carboxymethylcellulose, and polystyrene microspheres, and the pore former is added in an amount of 0-5% based on the weight of the catalyst; Optionally, in the method for preparing the catalyst, the Fe source, the Ce source, the Mo source, the Ca source, the first K source, and the pore-forming agent are all added in the form of solid-phase powder. The process according to any one of claims 7 to 15, characterized in that

17. Use of the catalyst according to any one of claims 1 to 6, or the catalyst prepared by the process according to any one of claims 7 to 16, in the production of styrene by dehydrogenation of ethylbenzene.

18. 18. Use according to claim 17, characterized in that the catalyst is suitable for ethylbenzene dehydrogenation at low steam / ethylbenzene ratios; said low steam / ethylbenzene ratio is less than or equal to 1.3, preferably between 0.7 and 1.

3.

19. 18. Use according to claim 17, characterized in that the catalyst is suitable for the production of styrene with a steam / ethylbenzene ratio of less than or equal to 2.

0.

20. The use includes a step of contacting a feed gas containing ethylbenzene with the catalyst in the presence of steam to carry out a dehydrogenation reaction to produce a styrene-containing product; The water is preheated to steam before entering the reactor and thoroughly mixed with the feed gas; The temperature of the dehydrogenation reaction is 570 to 640° C.; The pressure of the dehydrogenation reaction is 20 to 100 kPa absolute pressure; The weight hourly space velocity of ethylbenzene is 0.2 to 2.0 h -1 The use according to any one of claims 17 to 19, characterized in that

Citation Information

Patent Citations

  • Catalyst for dehydrogenation of alkyl aromatic hydrocarbon and preparation method therefor

    EP3868468A1