Thermoformable boron-based ceramic materials and their use in thermal management

The alignment of hexagonal boron nitride particles in a boron oxide matrix through tape casting and thermoforming addresses the challenge of fabricating complex ceramic composites for thermal management, achieving superior thermal conductivity and mechanical strength in electronic devices.

JP2024536758AInactive Publication Date: 2024-10-08NORTHEASTERN UNIV (US)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024516599
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-15
Filing Date
2022-09-14
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods struggle to fabricate complex, thin, and lightweight ceramic matrix composites (CMCs) that maximize heat transfer while maintaining electrical insulation, mechanical strength, and toughness, particularly for thermal management in high-density electronic devices.

Method used

A method involving tape casting and vibration processes to align hexagonal boron nitride particles with a parallel-oriented plate-like crystal structure in a boron oxide matrix, followed by thermoforming to create ceramic composite materials with controlled microstructures, allowing for the production of thin, lightweight, and complex shapes.

Benefits of technology

The process enables the fabrication of ceramic composites with high thermal conductivity and mechanical robustness, suitable for thermal management applications without the need for significant post-processing, outperforming conventional materials in heat transfer and mechanical resilience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536758000001_ABST
    Figure 2024536758000001_ABST
Patent Text Reader

Abstract

In a method for producing ceramic composite parts, a ceramic composite preform is provided, which has ceramic particles with platelet crystal morphology formed within a ceramic matrix. The preform is heated to a temperature above the melting or softening temperature of the ceramic matrix, and a load is applied to deform the preform, which is then thermoformed in a mold to form a ceramic composite body of a desired shape. This process is used to fabricate precisely shaped ceramic composites and devices containing them. These materials and devices may be used for thermal management of electronic components and other heat generating structures, etc.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing ceramic composite articles that provides ceramic composite preforms having ceramic particles with platelet crystal structures formed within a ceramic matrix. The process is used to fabricate precisely shaped ceramic composites and devices containing them that are used in the thermal management of electronic components and other heat generating structures.

[0002] [CROSS-REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of 35 U.S.C. § 119(e) to U.S. Provisional Application No. 63 / 397,931, filed August 15, 2022, entitled "Thermoformable Boron-Based Ceramic Materials and Uses in Thermal Management," U.S. Provisional Application No. 63 / 289,132, filed December 13, 2021, entitled "Thermoformable Boron-Based Ceramic Materials and Uses in Thermal Management," and U.S. Provisional Application No. 63 / 244,223, filed September 14, 2021, entitled "Thermoformable Boron-Based Ceramic Materials and Uses in Thermal Management," all of which are incorporated herein by reference. [Background technology]

[0003] Next-generation high-density electronics, such as 5G cellular devices, long-range communications, and computer processing chips, are increasingly limited in performance by the inability to manage heat, rather than the capabilities of current devices. Thermal management systems are becoming a bottleneck for innovation, especially in electronic applications with small design envelopes or where reduced weight is required. These systems are driving demands for higher power, higher frequencies, and longer duty cycles. Additionally, with component miniaturization and increased packing density, heat fluxes are approaching levels found in nuclear reactors.

[0004] The field of ceramic matrix composites (CMCs) continues to expand as next generation materials, especially for applications in the automotive, aerospace, and electronics industries. As one example, these materials may be used as dielectric thermal sealants to absorb or spread heat from topographical surfaces in printed circuit boards or other high density electronic devices, including power inverters.

[0005] Several methods are available to create the complex shapes in ceramics required for such thermal management applications, including injection molding, machining, and 3D printing. Thermoforming is an industrial process used to produce complex shell-like structures from shaping thin sheets of material, called blanks or preforms, by heated compression molding. Thermoforming processes typically use polymer and metallic materials for applications such as disposable plates, toys, and automotive interior panels.

[0006] Phononic conductors incorporated into ceramic matrix composites (CMCs) have been investigated to provide electrical insulation while maintaining both thermal conductivity and mechanical strength and toughness. The main drawback of these phononic CMCs is that they are difficult to fabricate and machine into complex, thin, and lightweight shapes that maximize heat transfer. Summary of the Invention [Problem to be solved by the invention]

[0007] The techniques described herein provide processes for manufacturing materials and devices, such as ceramic composite compacts and thermal management devices produced by such processes. The techniques may overcome the difficulty of fabricating complex shapes from ceramic matrix composites (CMCs) into thin, lightweight geometries that can maximize heat transfer. The techniques employ tape casting and vibration processes that result in highly oriented and infiltrated microstructures that allow for thermoforming of these ceramic composites. The thermal management materials and devices so produced allow for electrical insulation while maintaining both good thermal conductivity and robust mechanical strength and toughness. Methods are also described for providing thermal management of systems, such as thermal management of circuit boards.

[0008] In some embodiments, the ceramic composite material comprises a boron-based ceramic material in which hexagonal boron nitride (hBN) particles with a parallel-oriented platelet crystal structure are embedded in a boron oxide matrix. This technology allows the fabrication of hBN-based ceramic composite preforms that can be thermoformed using manufacturing processes previously only used for thermoplastics and sheet metal. Several systematic studies have been conducted to present the ceramic composite material and the process for producing the material.

[0009] This technology can also be summarized in the following list of items: 1. A method for producing a ceramic composite compact, the method comprising: (a) providing a preform having a first structure and having two opposing surfaces, the preform comprising a ceramic matrix composite material, the material including ceramic particles within the ceramic matrix having a platelet grain structure aligned parallel to a thickness direction extending between the two opposing surfaces of the first structure; (b) thermoforming the preform, which comprises the steps of: (i) heating the preform in the mold to a temperature above the melting or softening temperature of the ceramic matrix, and preferably below the melting or decomposition temperature of the ceramic particles; and (ii) applying a load to the mold, thereby transforming the first configuration of the preform within the mold to a second configuration to form a ceramic composite compact; (c) cooling the ceramic composite compact in the mold; and (d) removing the ceramic composite compact from the mold;

[0010] 2. The method according to claim 1, wherein the step of providing a preform comprises: (a-1) providing a slurry including a plurality of said ceramic particles in a polymer binder; (a-2) vibrating the slurry to provide a suspension in which the slurry is fluidized; (a-3) forming the slurry into a layer on a stage or within a preform mold so that the ceramic particles are aligned in parallel; (a-4) solidifying the polymer binder to form a solid green body containing the ceramic particles maintained in parallel alignment; (a-5) debinding the solid green body at a temperature first at which the polymer binder decomposes, leaving a ceramic body comprising the ceramic matrix and the ceramic particles; and (a-6) sintering the ceramic body at a second temperature, higher than the first temperature, whereby the ceramic particles remain parallel aligned in the ceramic matrix.

[0011] 3. The method according to item 2, wherein in step (a-6) the ceramic particles are partially oxidized.

[0012] 4. The method of claim 2 or 3, wherein the slurry provided in (a-1) further comprises one or more photoinitiators and one or more diluents mixed with the ceramic particles and the polymer binder, and wherein the slurry flows under shear stress.

[0013] 5. The method according to any one of items 2 to 4, wherein the polymer binder is selected from the group consisting of polymerizable resins, epoxies, melt-melting thermoplastics, and solvent-based thermoplastics.

[0014] 6. The method of claim 5, wherein the polymerizable resin comprises an acrylate, a methacrylate, a polymethylmethacrylate, a thiolene resin, an epoxy resin, a thermoplastic polymer, a wax, a methylcellulose, a phenolic resin, a polyvinyl acetate, a polyvinyl alcohol, or a raw rubber adhesive.

[0015] 7. The method according to any one of items 2 to 6, wherein in the solidifying step (a-4), solidifying the polymer binder comprises solidifying the polymer binder at a curing temperature to form a solid green body.

[0016] 8. The method according to any one of items 2 to 7, wherein the polymer binder is an oxygen-donating material, and in the solidification step (a-4), the polymer binder donates oxygen for seeding the oxidation process in the ceramic particles.

[0017] 9. The method according to any one of items 2 to 8, wherein the step (a-3) of forming the slurry into the layer comprises tape casting the slurry onto the stage or depositing the slurry into the preform mold.

[0018] 10. The method according to any of items 2 to 9, wherein the step (a-2) of vibrating the slurry occurs before the step of forming a slurry in the bed, during the step (a-3) of forming the slurry in the bed, after the step (a-3) of forming the slurry in the bed, or a combination thereof.

[0019] 11. The method according to any one of items 2 to 10, wherein the step (a-2) of vibrating the slurry and the step (a-3) of forming the slurry into a layer are repeated multiple times to form the sheet.

[0020] 12. The method according to any one of items 2 to 11, wherein the polymer binder is a photopolymerizable resin, and the step (a-4) of hardening the polymer binder comprises irradiating the slurry with ultraviolet or visible light.

[0021] 13. The method according to any of the preceding items, wherein in the thermoforming step (b), the temperature to which the preform is heated is below the decomposition and / or evaporation temperature of the ceramic matrix.

[0022] 14. The method according to any of the preceding items, wherein in the thermoforming step (b), the preform is heated to a temperature of about 400°C to about 1000°C, or about 500°C to about 700°C.

[0023] 15. The method according to any of the preceding items, wherein in the step (b)(ii) of applying the load, the load stress is in the range of about 50 kPa to about 100 MPa, or about 500 kPa to 5 MPa.

[0024] 16. The method of any of the preceding items, wherein in the thermoforming step (b), the mold comprises a lower portion having a negative surface and an upper portion having a positive surface, and the load is applied to the preform through the upper portion of the mold.

[0025] 17. The method of any preceding item, wherein in the thermoforming step (b), the mold includes a negative surface and a positive surface, each surface including at least one surface feature having a feature size of about 1 mm or less in any dimension.

[0026] 18. The method of claim 17, wherein the features have a size of about 200 μm or less in any dimension.

[0027] 19. The method of any preceding claim, wherein in the thermoforming step (b), the mold has a maximum draw ratio of feature height to feature width of about 1:1.

[0028] 20. The method of any of the preceding claims, wherein the ceramic particles comprise oxides, nitrides, carbides, sulfides, fluorides, or combinations thereof in flake form.

[0029] 21. The method of any preceding claim, wherein the ceramic particles are hexagonal boron nitride, hexagonal aluminum nitride, aluminum oxide, molybdenum disulfide, clay, cesium oxide, graphene, flaky ferrite, calcium phosphate flakes, zirconia flakes, silica flakes, or combinations thereof.

[0030] 22. The method of any of the preceding items, wherein the ceramic matrix comprises boron oxide, silicon dioxide, glass flake, silver coated glass flake, lithium oxide-silica mixture, magnesium oxide-silica mixture, or combinations thereof.

[0031] 23. A method according to any of the preceding items, wherein the ceramic matrix comprises a glassy material or glassy-ceramic material mixture having a softening phase or melting temperature within the operating temperature range of the material forming the mould and below the melting or decomposition temperature of the ceramic particles.

[0032] 24. The method described in any of the preceding items, wherein the ceramic particle concentration in the ceramic composite compact is about 30% by weight to about 90% by weight, and the ceramic matrix concentration is about 10% by weight to about 70% by weight.

[0033] 25. The method according to any of the preceding items, wherein the ceramic particles in the ceramic composite compact have a diameter of about 1 μm to about 100 μm, or about 5 μm to about 45 μm, and a thickness that is about 3 to about 100 times smaller than the diameter.

[0034] 26. The method of any of the preceding items, wherein the preform has a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to 3 mm.

[0035] 27. The method of any of the preceding items, wherein the ceramic composite compact has a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to about 3 mm.

[0036] 28. The method of any preceding claim, wherein the ceramic particles comprise phononic crystal particles.

[0037] 29. The method of any of the preceding items, wherein the lateral bonds between layers of the ceramic particles in the preform are sufficiently weak to permit sliding of the ceramic particles when subjected to a load in the thermoforming step (b)(ii).

[0038] 30. The method of any preceding claim, wherein the ceramic composite compact has an in-plane thermal conductivity transverse to a thickness dimension, the in-plane thermal conductivity being greater than the through-plane thermal conductivity.

[0039] 31. The method of any of the preceding items, wherein the ceramic composite compact has an in-plane thermal conductivity of about 5 W / mK to about 100 W / mK, or about 10 W / mK to about 40 W / mK, transverse to the thickness dimension, at ambient temperature.

[0040] 32. The method of any of the preceding paragraphs, wherein the ceramic composite compact is configured as a thermal management device, a heat sink or heat spreader for a printed circuit board, a heat exchanger, a cold plate, a low loss dielectric RF component, a radome, a power inverter, a solar cell, a neutron shield, a high temperature heat shield, a satellite satellite, an encapsulant, or a heat shield for a medical device.

[0041] 33. A method of fabricating a thermal management device for a heat generating component, the method comprising: (a) providing a mold configured to fit at least a portion of the heat generating component; (b) forming a ceramic composite body according to any of the methods in the preceding paragraphs using the mold provided in step (a) to produce a thermal management device; Includes.

[0042] 34. The method according to item 33, further comprising: (c) fitting the ceramic composite compact into the heat generating component or a part thereof; The method comprising:

[0043] 35. The method of claim 33 or 34, wherein the heat generating component is a printed circuit board, a central processing unit, a high density electronic platform, an electronic chassis, an RF device, an RF or phased antenna array, a low loss dielectric RF component, a radome, a power inverter, a solar cell, a neutron shield, a cube satellite, or a medical device.

[0044] 36. A method of fabricating a thermal management device, the method comprising: (a) providing a design for a heat generating component or portion thereof requiring thermal management; (b) fabricating a preform mold designed to fit a first structure complementary to the heat generating component or portion thereof; (c) fabricating a mold designed to fit a second structure complementary to the second structure, the second structure being more precisely complementary to the heat generating component or portion thereof than the first structure; (d) fabricating a preform using a preform mold, wherein said preform has said first structure and has two opposing surfaces, wherein said preform comprises a ceramic matrix composite material, said material comprising ceramic particles within said ceramic matrix, wherein said ceramic particles have a platelet grain structure aligned parallel to a thickness direction extending between said two opposing surfaces; (e) thermoforming the preform in the mold to provide a thermal management device in the second configuration, said thermoforming comprising: (i) heating the preform in the preform mold to a temperature above the melting or softening temperature of a ceramic matrix; Including, (ii) applying a load to the preform mold, thereby transforming the first configuration of the preform within the mold to a second configuration to form a thermal management device; (f) cooling the thermal management device within the mold; and (g) removing the thermal management device from within the mold; The method comprising:

[0045] 37. The method of claim 36, wherein in step (a), the design includes a negative geometry of the heat-generating component or portion thereof, provided by a three-dimensional computer-aided design model of the heat-generating component or portion thereof or by a three-dimensional scan of the heat-generating component or portion thereof.

[0046] 38. The method of claim 36 or 37, wherein step (b) comprises fabricating the preform mold and / or the mold from a metallic material by an additive manufacturing process or a machining process based on a three-dimensional computer-aided design model of a design of the heat generating component or part thereof.

[0047] 39. The method of claim 38, wherein the additive manufacturing process is a three-dimensional printing process, a stereolithography process, a direct write process, a fused deposition process, or a thermal or laser selective sintering process.

[0048] 40. An apparatus for thermal management of a heat generating component, the apparatus being fabricated by a method according to any of the preceding items.

[0049] 41. An apparatus for thermal management of a heat generating component, said apparatus comprising: A body comprising a ceramic matrix composite material, the material including a plurality of ceramic particles within a ceramic matrix, the body including two opposing surfaces, the ceramic particles having a platelet crystal structure arranged in parallel alignment transversely through a thickness direction extending between the two opposing surfaces; and the body is formed with at least one deformation to accommodate a surface shape of the component, and the parallel alignment of the platelet crystal structure matches at least one dimension of the at least one deformation. The method.

[0050] 42. The apparatus of claim 41, wherein the ceramic particles are hexagonal boron nitride, boron oxide, hexagonal aluminum nitride, aluminum oxide, molybdenum disulfide, clay, cesium oxide, graphene, flaky ferrite, calcium phosphate flakes, zirconia flakes, silica flakes, or combinations thereof.

[0051] 43. The device of claim 41 or 42, wherein the ceramic matrix comprises boron oxide, silicon dioxide, glass flakes, silver-coated glass flakes, lithium oxide-silica mixtures, magnesium oxide-silica mixtures, or combinations thereof.

[0052] 44. The device according to any one of items 41 to 43, wherein the ceramic particle concentration in the ceramic matrix composite material of the main body is about 30% by weight to about 90% by weight, and the ceramic matrix concentration in the ceramic matrix composite material of the main body is about 10% by weight to about 70% by weight.

[0053] 45. The device according to any one of items 41 to 44, wherein the ceramic particles in the ceramic matrix composite of the body have a diameter of about 1 μm to about 100 μm, or about 5 μm to about 45 μm, and a thickness that is about 3 to about 100 times smaller than the diameter.

[0054] 46. ​​The device according to any one of items 41 to 45, wherein the body has a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to 3 mm.

[0055] 47. The device according to any one of items 41 to 46, wherein the ceramic particles include phononic crystal particles.

[0056] 48. The apparatus of any of items 41-47, wherein the body has an in-plane thermal conductivity transverse to the thickness dimension that is greater than the through-plane thermal conductivity.

[0057] 49. The device according to any one of items 41 to 48, wherein the body has an in-plane thermal conductivity transverse to the thickness dimension of about 5 W / mK to about 100 W / mK, or about 10 W / mK to about 40 W / mK, at ambient temperature. [Brief description of the drawings]

[0058] [Figure 1] 1A-1F show a step of providing a preform in a process for producing a ceramic composite material. [Figure 1A] The left is a schematic diagram of a slurry containing ceramic particles in a polymerizable resin being deposited on a stage, and the right is a schematic diagram of the slurry on the stage being subjected to vibration to fluidize the particles in the resin. [Figure 1B]1 is a schematic diagram showing a slurry being tape cast onto a first structure in the form of a thin sheet or layer exhibiting parallel aligned particles. [Figure 1C] 1 shows a micrograph illustrating particle alignment during tape casting. [Figure 1D] 1 is a schematic diagram of curing the slurry in the first structure to polymerize the resin. [Figure 1E] 1 is a schematic embodiment of an apparatus suitable for vibrating, tape casting, and curing a preform. [Figure 1F] The next step is to sinter the cured preform to form a fully sintered preform. [Diagram 2] 2A-2B show steps for thermoforming a preform including a ceramic composite material. [Figure 2A] Diagram A shows two fully sintered preforms on the left and one fully sintered preform on the right placed into a two-part thermoforming mold. [Figure 2B] On the left side is shown the result of applying a load to the top of the mold to compress the preform within the mold, and on the right side is the deformed ceramic matrix composite being removed from the mold. [Diagram 3] 1 is a schematic representation of phononic conduction of aligned particles in a matrix. [Figure 4] 1 is a series of scanning electron micrographs showing particle alignment based on particle size. [Figure 5A] 1 is a schematic diagram of the photopolymerization step. [Figure 5B] 1 is a graph of cure depth versus energy for various particle concentrations and various particle sizes. For the 12 μm particle system, a layer thickness of approximately 250 μm was cured in 15 seconds, giving a cure time of 22.5 seconds per layer. [Figure 6A] 1 is a schematic diagram of the sintering step. [Figure 6B]The change in atomic composition of carbon (C), boron (B), oxygen (O), and nitrogen (N) during sintering of sintered hBN, a green body of 54 vol.% Ebecryl 230, and sintered 54 vol.% Ebecryl 230 is shown. [Figure 7A] 1 is a schematic representation of a preform microstructure that allows for in-plane flow during the thermoforming process. [Figure 7B] 1 is a schematic representation of a preform microstructure that allows for in-plane flow during the thermoforming process. [Figure 8A] 1 shows a phase diagram under a loading pressure of ∼0.5 kPa for determining feature size based on temperature during thermoforming. [Figure 8B] 1 illustrates a schematic of a mold showing the identification of feature width, height, and length. [Figure 9] The fine feature mold and the upper and lower mold halves of the ceramic composite compact molded at 500°C, 600°C, and 700°C are shown. [Figure 10A] Two examples of rough shaped molds are shown, the left one with 90° steps and a maximum step height of 5 mm, and the right one with a fillet of 1 mm radius, with ceramic composite compacts molded at 500 °C in each mold. At 500 °C, the boron-based ceramic composite was able to mold even the most aggressive steps (5.8 mm wide, 5 mm deep, 90° sharp bends) without tearing. Notably, this sample was also able to pick up the shape of the mold surface from the 3D printing process. [Figure 10B] 1 shows a broken edge of a thermoformed heat sink formed in a large feature mold. [Figure 10C] 1 shows scanning electron micrographs (SEM) of samples deformed in a large feature mold. [Figure 11] 1 is a schematic diagram of a deep-draw die for thermoforming the preform. [Figure 12A] 1 is a diagram of a process for fabricating a thermal management device for a printed circuit board. [Figure 12B] 1 is a diagram of a process for fabricating a thermal management device for a printed circuit board. [Figure 12C]1 is a diagram of a process for fabricating a thermal management device for a printed circuit board. [Figure 13] Figure 1 shows graphs of flexural strength (i), strain (ii), and resistance (iii) of molded ceramic matrix composites and commercial boron nitride based all-ceramic material without microstructural control at dwell times of 4 and 6 hours. [Figure 14] Graph of deformation of a boron-based ceramic preform measured in a simply loaded bending case (see inset) at high temperature (Tm=450°C). The deflection was recorded after a 10 minute dwell time and was found to follow a linear trend with a yield point associated with a load of 0.015 N. [Figure 15] 1 is a graph showing the maximum drawing ratio and estimated stress measured at temperatures from 500° C. to 700° C. and die sizes. [Figure 16A] 1 shows the steps of performance testing of a hot-formed boron-based ceramic composite heat spreader. [Figure 16B] The steps of performance testing of thermoformed boron-based ceramic composite heat spreaders are shown. 1) A 3D model of a Raspberry Pi (RPi) PCB was used to create a relief mold for encasing the chipset on the PCB surface. The height variation of the created positive relief of the RPi is displayed in the shaded key. 2) Both the positive and negative design relief molds were 3D metal printed. Here, Inconel 625 was selected to withstand the thermal stress from the thermoforming process. 3) The preform sheet made by the process shown in Figure 1A-1F was placed between the negative (bottom) and positive (top) relief molds in an oven at 500 °C. After a dwell time of 10 minutes, the positive (top) relief mold was pressed down onto the preform. The mold was then removed from the oven and allowed to cool. The thermoformed ceramic composite could then be removed. 4) The thermoformed ceramic composite was post-processed with a wire saw and the formed patterns were cut into the final shapes used in the tests. [Figure 17A] 1 is a graph of temperature versus time for a prior art control heat sink, a prior art metal heat sink, and a thermoformed heat sink. [Figure 17B] 1 is a graph of temperature change per height versus time on a logarithmic scale for a prior art metal heat sink and a thermoformed heat sink. [Figure 18A] The positive and negative mold halves are open to reveal a cast of a human face with the mold shown in a closed position. [Figure 18B] Shown is a human face mold and a ceramic composite compact formed within the mold (shown between two mold parts). [Figure 19] 1 shows several deep-draw dies used to form the ceramic composite materials described herein. [Figure 20A] A) XRD plot of the sample before the decomposition process showing the presence of hBN and B2O3, and [Figure 20B] B) XRD plot of the sample after digestion showing only hBN peaks present in the sample, confirming successful digestion. [Figure 21] 1 shows an array of samples with different drawing depths in a deep drawing process. [Figure 22A] 1 is a graph of average surface temperature versus time for a prior art metal heat sink and a thermoformed ceramic composite heat sink. [Figure 22B] FIG. 22B shows a thermal image of the heat sink of FIG. 22A. [Figure 23] This experimental apparatus heats the bottom of a sintered hBN sample, which is loaded with a weight on top, with a propane torch. [Figure 24] Shows the thermoforming process steps using a U-shaped mold.

[0059] Detailed Description The technology described herein provides a method for producing ceramic composite compacts in a variety of geometries useful in applications such as thermal management. The technology provides ceramic composites with textured microstructures that allow the material to be shaped into complex geometries from a fully sintered ceramic preform through a heating and forming process. The technology provides thermoforming of ceramic composites by utilizing the melting temperature difference between the ceramic matrix and the aligned ceramic filler particles in the matrix. The controlled alignment of the microstructure during processing contributes to deformation by grain sliding between the matrix-particle interfaces. The composite ceramic material can exhibit typical ceramic properties and is sufficiently ductile at relatively low temperatures to solidify into the formed geometry without fracture.

[0060] Ceramics tend not to undergo melting transitions at moderate temperatures due to their covalently bonded atomic structure. In contrast, as described herein, glassy ceramics such as boron oxide (BO) can be formed using molding and compaction processes with well-defined shapes due to their amorphous nature and lower melting temperature (450°C for BO). The present technique uses glassy ceramic matrix solutions with high particle filler (inclusion) concentrations. These composites have an amorphous ceramic matrix with embedded anisotropic filler particles that can be thermally conductive. In some embodiments, hexagonal boron nitride (hBN) is the preferred filler particle. Boron oxide is a glassy ceramic material that forms as an oxide layer on boron nitride when ambient temperatures reach 1000°C. Thus, boron nitride can be partially oxidized to form robust glassy-ceramic composites that can withstand substantial thermal shock in addition to having large deformations above the melting temperature of the BO matrix. The oxide acts as a binder between the hBN particles, providing a reinforced structure for the part after sintering. Furthermore, the amorphous oxide matrix is ​​significantly weaker than the boron nitride particles, allowing for a toughened structure for the ceramic. With boron oxide as a binder, highly oriented hBN particles can form a thermally permeated network.

[0061] Thus, the present technology provides ceramic composites that can be thermoformed into a variety of configurations. Moreover, the processes described herein can be extended beyond in situ oxide glass formation to other ceramic matrix composites that are thermoformable and capable of sustaining thermal cycling in a range of extreme environment applications.

[0062] An embodiment of a process for manufacturing a thermal management device from a ceramic matrix composite (CMC) can be described with reference to FIGS. 1A-2B. In a first step, a preform including a ceramic composite material, a material including ceramic particles in a ceramic matrix, is provided. The ceramic particles have a platelet or flake-like morphology. The preform can be comprised of a first structure having two opposing surfaces, such as a sheet or layer having a thickness between the two opposing surfaces. The first structure can have an in-plane direction perpendicular to the thickness direction and a through-plane direction parallel to the thickness direction. The ceramic particles having the platelet or flake-like structure can be arranged with an orientation parallel to the in-plane direction. In some embodiments, the parallel orientation of the particles can be substantially parallel to the through-plane direction, for example, within 10%, within 5%, within 2%, within 1%, or within 0.5%.

[0063] More specifically, a plurality of ceramic particles and a polymer binder are mixed to form a slurry, which is then deposited in layers on a surface, such as on a stage or in a mold. (FIG. 1A) In some embodiments, the slurry can be tape cast onto a stage. In some embodiments, the slurry can be deposited onto the surface of a mold. The slurry is vibrated on the surface to form a suspension in which the ceramic particles are aligned parallel to each other and aligned laterally through the thickness. The vibration promotes fluidization, and the particles are aligned by shear simultaneously with tape casting. (FIGS. 1A, 1B, 1C) In some embodiments, shear alignment improves at thinner thicknesses. In some embodiments, shear alignment improves with a higher particle size to thickness ratio α, where α=D / h, where D is the two-dimensional particle size and h is the height of the tape cast layer.

[0064] In some embodiments, the vibration can be applied in a direction parallel to the thickness or through-plane direction of the layers of the preform. In some embodiments, the vibration can be applied in one or more directions parallel to the in-plane direction of the preform. In some embodiments, the vibration can be applied in one or more of any three-dimensional direction. The vibration can be applied before, during, or after tape casting, or a combination thereof.

[0065] The polymer binder is solidified to form a solid green body of ceramic particles maintained in parallel alignment. In some embodiments, the polymer binder is a polymerizable resin, and the preform is heated to a first temperature to cure the polymerizable resin and form a solid green body with ceramic particles maintained in parallel alignment. (FIG. 1D) In ​​some embodiments, the resin is cured by exposure to ultraviolet radiation, visible radiation, or a combination thereof. In some embodiments, the slurry can be deposited in multiple layers in a lamination process where each layer can be subjected to vibration, tape casting, and curing. This helps provide layer-by-layer particle alignment. An embodiment of an apparatus that can be used to vibrate the slurry, tape cast, and provide curing by exposing to appropriate radiation using a digital light projector (DLP) is illustrated in FIG. 1E. This apparatus can be used to build up the material into multiple layers. In some embodiments, the nominal particle size can be at least about 1 μm. In some embodiments, the nominal particle size can be at least about 300 nm. In some embodiments, the particle size may be about 5 μm, about 12 μm, or about 45 μm. In some embodiments, the layer thickness may be at least about 30 μm. In some embodiments, the layer thickness may be at least about 30 μm to about 3 mm. In some embodiments, the layer thickness may be about 100 μm, about 500 μm, about 1 mm, about 2 mm, or about 3 mm. In some embodiments, the dimensional tolerance may be 20%, 10%, 5%, 1%, or 0.5%.

[0066] The solid green body is then sintered at a second temperature (FIG. 1F) that is higher than the first temperature to partially oxidize the ceramic particles and provide a fully sintered body with the ceramic particles aligned parallel within the ceramic matrix. In some embodiments, seeding with oxygen from the polymer binder burned out in the curing step can provide homogenous oxidation during the sintering process. In some embodiments, the polymer used in the slurry to produce the preform does not need to be photosensitive such that if the polymer is of a sufficiently oxygen-rich formulation, the trapped excess oxygen can be used as a catalyst during the sintering process. In some embodiments, a glassy-ceramic additive can be seeded throughout the slurry mixture to form a glassy matrix with or without the use of a sintering-assisted process with an oxygen-rich polymer.

[0067] Next, referring to FIGS. 2A-2B, the preform is placed in a mold for thermoforming to produce a ceramic composite compact having a desired three-dimensional structure. In some embodiments, the mold can have two halves that provide a positive mold or mold surface with one or more convex curves and a negative mold or mold surface with one or more concave curves. In some embodiments, the mold surface can include one or more steps. The two mold halves have a geometric offset from each other so that the preform can be pressed between the two mold halves. In some embodiments, the mold can be formed by an additive manufacturing process, such as 3D printing, from a metallic material that can withstand the forming temperatures. Suitable metallic materials include Inconel, an austenitic nickel-chromium based superalloy, and 304 stainless steel. The preform in the mold is heated to a temperature above the melting or softening temperature of the ceramic matrix. A load is applied to the mold, causing the preform to deform within the mold. In some embodiments, the load is applied to the preform through the positive mold. Aligning the ceramic particles in the microstructure of the preform allows for in-plane flow of the particles during the thermoforming process. The ceramic composite compact is cooled and removed from the mold. In some embodiments, the ceramic composite compact can be thermoformed from the flat sintered sheet in less than 15 minutes. In some embodiments, the ceramic composite compact can be thermoformed from the flat sintered sheet in less than 10 minutes. In some embodiments, the ceramic composite compact can be thermoformed from the flat sintered sheet in less than 10 minutes. In some embodiments, in the thermoforming step, the preform is heated to a temperature of about 400°C to about 1000°C. In some embodiments, in the thermoforming step, the preform is heated to a temperature of about 500°C to about 700°C.

[0068] In some embodiments, hexagonal boron nitride (hBN) can be selected as the ceramic particles and boron oxide (BO) can be selected as the ceramic matrix, as described above, although it will be understood that the process embodiments can be used with other ceramic particles and matrix materials. The oriented platelet grains of hBN are efficient for in-plane phononic transport due to their atomic structure consisting of covalent bonds between boron and nitrogen atoms in a honeycomb structure. These honeycomb atomic sheets are laterally bound by weak π bonds, which increases lateral phononic scattering. (Figure 3) The thermal anisotropy of hBN dictates that the thermal behavior of the phononic material is determined by the underlying microstructure, including the orientation and percolation of the hBN grains.

[0069] To achieve the desired particle orientation and infiltration throughout the ceramic composite, vibration-assisted casting methods can align high volume fractions of hBN particles in polymer green bodies (as much as 60% by volume in some embodiments). High loadings of hBN particles suspended in liquid binder resins (such as photopolymers or epoxies) behave as Herschel-Buckley fluids and require shear in the form of vibration to flow effectively. Furthermore, these dense particle suspensions are subjected to vibrational energy during the tape casting process, which fluidizes and shear-aligns the in-plane hBN to an even higher degree. Figure 4 shows micrographs of aligned hBN particles in a 250 μm layer with nominal particle sizes of 5 μm, 12 μm, and 45 μm from left to right. The larger diameter particles provide better alignment and act as directors for the smaller particles in the polydisperse particle system.

[0070] After tape casting, the suspension is exposed to UV light to polymerize the photosensitive resin and fix the oriented hBN particles into a solid green body. In some embodiments, the material is exposed to UV-A and visible UV light with a peak wavelength of 405 nm. The hBN platelets are translucent to visible light (see FIG. 5A). Photodynamic characterization can explain the relationship between particle concentration and particle size to cure depth. For example, as particle concentration increases, in some embodiments above 30 volume % for hBN particles, cure depth can be more constrained. As particle size decreases, cure depth also decreases, which is related to light scattering effects as the particles become smaller. In some embodiments, a layer thickness of ∼250 μm and hBN particle size of 12 μm can be cured in 22.5 seconds (see FIG. 5B). In some embodiments, a multilayer preform with a thickness of 1 mm and hBN particle size of 12 μm can be fully cured within an hour.

[0071] With reference to FIG. 6A, these polymer green bodies can be sintered at atmospheric pressure in an oxygenated environment to grow a matrix of boron oxide that replaces the polymer matrix and encapsulates the hBN. An oxygen-rich acrylate system can be selected to promote uniform growth of boron oxide throughout the thickness of the green body. The material is placed in a sintering furnace and the temperature is raised to a first temperature (FIG. 6A, step (i)). The two-step sintering process begins with a debinding (polymer burnout) stage (step (ii)) that traps and leaves behind about 0.3 at% oxygen (shown in yellow EDX overlay above the SEM image) in some embodiments from the polymer, which has an affinity for boron and acts as a seeding agent for the oxidation process. The sintering temperature is then raised to 1050° C. to partially oxidize the hBN (FIG. 6A, step (iii)). The trapped oxygen enhances and homogenizes the oxidation rate of hBN throughout the part (again shown in EDX overlay), resulting in a white all-ceramic part described as a preform or blank. In some embodiments, the material can be sintered at 1050° C. for 6 hours in dry air under atmospheric conditions, utilizing the oxidation of hBN to produce approximately 40 vol.% B2O3 that acts as a secondary binder when the polymer is burned out of the system. FIG. 6B shows the change in atomic composition of carbon, boron, nitrogen, and oxygen elements for sintered hBN, 54 vol.% Ebecryl 230 green body, and sintered 54 vol.% Ebecryl 230.

[0072] The orientation of the hBN in the microstructure of the preform allows for in-plane flow during the thermoforming process. (FIG. 7A, FIG. 7B) Thermoforming begins by first placing the preform on the negative mold surface of a two-part mold, heating the system above the melting temperature Tm of B2O3 (450°C), and dwelling for a sufficient time for the sample and mold to reach equilibrium temperature, in some embodiments 10 minutes. The boron oxide (B2O3) melts and the material behaves again as a viscous, particle-packed Bingham pseudoplastic, exhibiting a yield stress that prevents flow until an adequate load is applied. A mold compressive load is then applied for an appropriate time (in some embodiments, at least 10 minutes or at least 15 minutes) to overcome the yield stress of the partially fluid all-ceramic and induce deformation. The mold is removed from the oven and allowed to cool. The deformed ceramic can then be removed from the mold, resulting in complex, thin, and lightweight parts. Thus, these hBN ceramic materials can be thermoformed by applying sufficient heat, pressure, and dwell time. In some embodiments, the heating may be in the range of 500-700°C. In some embodiments, the pressure may be in the range of 50 kPa-100 MPa. In some embodiments, the pressure may be in the range of 500 kPa-5 MPa. In some embodiments, the residence time in the mold may be at least 10 minutes. In some embodiments, the residence time in the mold may be less than 10 minutes. In some embodiments, the residence time in the mold may be less than 5 minutes or less than 1 minute. In some embodiments, the majority of the time in the mold is spent bringing the mold and preform up to the desired temperature. In some embodiments, the dimensional tolerances may be 20%, 10%, 5%, 1%, or 0.5%.

[0073] The moldability of the preform may depend on the temperature. With reference to FIG. 8A, increasing the temperature during thermoforming may result in the formation of finer feature sizes of the material. At low temperatures and high viscosity, the material may get stuck in mechanical interlocking regions where the material does not fully resolve the features. As the temperature increases, a transition to groove contact regions allows finer features to be resolved. As the temperature increases further, the material becomes bonded regions with fully resolved features. Within the bonded regions, the formed ceramic composite material may adhere to the surface of the mold and may require high temperature demolding to remove the molded part. In some embodiments, the phase diagram (FIG. 8A) can assist in the expected feature sizes at a given temperature from the feature sizes that can be formed based on different temperatures. With the identified thermoforming regions, the mold can be designed, for example, with full bond contact regions in some embodiments. FIG. 8B is a schematic of a mold identifying the width, height, and length features as used herein. Feature width is the width between the mold features, where the mold features create rugged features on the molded material. Feature height is the depth to which the material can be molded into the mold features. The feature length is the dimension spanning the die. In some embodiments, the die can have a maximum draw ratio of about 1:1, where the draw ratio is defined as the feature height to the feature width.

[0074] Figure 9 shows a mold with fine feature sizes. Finer feature formation may require lower viscosity, which can be achieved by increasing the temperature. For example, a ceramic material with a liquid matrix of boron oxide will have a decrease in viscosity as the temperature increases above the Tm of B2O3. The decrease in viscosity of B2O3 with increasing temperature has been confirmed by Pei-Ching Li, et al, who derived the activation flow energy, , for melting B2O3. As the temperature increases, the energy required to induce flow decreases. This fact can be exploited to increase the thermoforming resolution of parts with finer features. At temperatures just above the Tm of B2O3, 500°C, ℃At low temperatures, thermoforming of hBN ceramic material preforms is possible for feature widths greater than 2 mm, and is limited to features less than 5 mm wide. Features less than 2 mm at 500 °C are not resolved due to the inhibiting activation energy (characterized as the mechanical interlocking region). At 600 °C, finer features can be resolved by lowering the transition in the groove contact region to a feature size of 1.6 mm. At 600 °C, feature sizes 1.6 mm wide and greater are fully formed (characterized as the groove contact region). At 700 °C, more flow is permitted and feature widths down to 0.6 mm are resolved (characterized as the bonded region). Within the bonded region, the formed all-ceramic may adhere to the mold surface, requiring high temperature demolding to remove the formed part. Further increases in temperature are limited by oxidation of the ceramic particles, e.g., BN over 1000 °C at longer times, and the vaporization temperature of the oxide matrix at shorter times, e.g., 1375 °C for boron oxide. The oriented hBN microstructure plays a role in the formation process due to the ability of aligned particles to flow over one another, whereas isotopically aligned systems cause localized particle jamming due to steric hindrance.

[0075] FIG. 10A shows two embodiments of a die with rough features and a ceramic composite compact formed at 500° C. in each die. The die on the left has many 90° steps. The die on the right has a step with a 1 mm radius fillet. In some embodiments, the rough features die can be used to thermoform ceramic preforms with hBN platelet grains at a low temperature of 500° C. with a feature size of 5.8 mm wide. In some embodiments, the preform can withstand 90° bends in 5 mm steps without failure. In some embodiments, three-dimensional parts can be formed with a feature resolution of 200 μm.

[0076] Figure 10B shows the fracture edge of a thermoformed heat sink formed in a large feature mold, showing grains formed in the deformation and aligned grains following the curved section, and Figure 10C shows an SEM of a sample deformed in a large feature mold, showing that the large deformation is smooth at the surface level and the curved surface is free of surface delamination or cracks.

[0077] In some embodiments, a deep draw mold can be employed. See FIG. 11. The mold can include a base or pull guide that provides a negative mold surface, a male mold that provides a positive mold surface, and a male mold guide for aligning the male mold with the base. In some embodiments, a maximum draw ratio of 1:1 feature depth to width can be employed.

[0078] In some embodiments, passive thermoforming techniques can be employed, and in some embodiments, active thermoforming techniques can be employed, generally depending on the type and design of the mold. Passive thermoforming is placing the ceramic composite preform between two mold halves and placing the mold in an oven at temperature to set. No additional load is required as the weight of the top mold is enough load to form the ceramic. This approach may be suitable for simple U molds (described in Example 1) and Raspberry Pi molds (described in Example 2). Active thermoforming is a method of forming the material by applying a load to the top mold. This is useful when the surface shape of the top mold is complex and may jam when the mold is sliding into the molding position. Active forming may be suitable for rough feature molds, fine feature molds, face molds (which can be considered as fine feature molds), and deep draw molds, as described herein. A high temperature release agent (Hi-Temp 1800 Mold Release, Slide, Wheeling IL) can be applied to the mold to prevent sticking and sample damage when removing the part after molding is complete.

[0079] In some embodiments, the ceramic particles can be hexagonal boron nitride, boron oxide, hexagonal aluminum nitride, aluminum oxide, molybdenum disulfide, clay, cesium oxide, graphene, flaked ferrite, calcium phosphate flakes, zirconia flakes, silica flakes. In some embodiments, the ceramic particles can be flaked one or more of oxides, nitrides, carbides, sulfides, and fluorides.

[0080] In some embodiments, the ceramic matrix can be boron oxide, silicon dioxide, glass flake, silver coated glass flake, or a lithium oxide-silica mixture. In some embodiments, the ceramic matrix can be a glassy material or glassy ceramic material mixture that has a softening phase or melting temperature within the operating temperature range of the material forming the mold and below the melting or decomposition temperature of the ceramic particles.

[0081] In some embodiments, the ceramic particle concentration in the ceramic composite compact may be about 30% by weight to about 90% by weight, and the ceramic matrix concentration may be about 10% by weight to about 70% by weight.

[0082] The ceramic particles in the ceramic composite compact may have a diameter of about 1 μm to about 100 μm, or about 5 μm to about 45 μm, and a thickness of about 3 to less than about 100 times the diameter. In some embodiments, the preform may have a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to 3 mm. In some embodiments, the ceramic composite compact may have a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to 3 mm.

[0083] In some embodiments, the casting process can be scaled up to roll-to-roll or large-scale sheet manufacturing, including large format vibratory platforms. In some embodiments, the process can form or be integrated into a production line for manufacturing multiple parts. The thermoforming process also exhibits repeatability and reliability under a variety of load and temperature conditions. In some embodiments, the tolerances on the dimensions and other parameters described herein can be 20%, 10%, 5%, 1%, or 0.5%.

[0084] In some embodiments, this technique may provide a process that provides thermal management of devices such as heat generating circuit boards. With reference to FIGS. 12A-12C, in one embodiment, a circuit board requiring thermal management is 3D scanned. From the scan, a positive and negative thermoforming mold is manufactured using an additive manufacturing process, such as 3D printing. The mold may be created using other metal processing processes, including subtractive processes such as machining. The mold may be made from metal or other materials that can withstand the forming temperatures of the thermoforming process. The negative mold half has a geometric offset from the positive mold half, allowing the ceramic preform to be compressed between the two mold halves. The ceramic preform with aligned microstructures made as described herein is heated and compressed inside the mold as described herein. In some embodiments, the thermoformed ceramic structure may be coated with a water protective coating. Suitable coatings include spray-on glass, siloxane-based coatings, PTFE spray, dip coating with epoxy or silicone, spray with epoxy or silicone, oil-based paint, and other commercially available barrier coatings. This structure can be cooled, removed from the mold, and pressed onto a circuit board to distribute heat generated by the electronics to the circuit board for use as a thermal management solution. In some embodiments, the thermal management device employed as a heat sink can provide a heat transfer rate of 10° C. / mm, compared to the 1° C. / mm rate achieved by prior art metal heat sinks. This process can be repeated multiple times, potentially hundreds or thousands of times, to produce thermal management devices for multiple circuit boards during the manufacturing process.

[0085] The processes and materials described herein can provide many advantages over conventional ceramic manufacturing processes and prior art ceramic materials. The techniques described herein can be used to produce dielectric ceramic materials that can conform to complex surfaces, withstand large stresses without failure, and have high thermal conductivity while being electrically insulating. The techniques can be used to rapidly form thin-walled, complex shapes of ceramic materials at low temperatures without significant use of post-processing or machining techniques. There is no need for design trade-offs due to shrinkage, relaxation, or post-machining of the part because the preform is already fully sintered before the thermoforming step. Traditional ceramic processing is costly due to the tools and expertise required to perform the processing. Prior art advanced manufacturing processes typically require near-net-shape processing to account for shrinkage or deformation during final sintering, for example. Machining typically results in micro-cracks that prevent the formation of the desired material properties.

[0086] Ceramic composite materials can exhibit improved properties such as thermal shock resistance, mechanical strength and toughness compared to prior art materials such as commercially available hBN. The thermal management performance of the materials as heat sinks or heat spreaders can show improvement when compared to prior art metallic heat sink and heat spreader devices.

[0087] The processes and apparatus described herein can provide thermal management for a variety of heat generating applications with both suitable thermal conductivity and electrical resistivity. In contrast, prior art metal heat exchangers can provide good thermal conductivity but have poor electrical resistivity, making them unsuitable for many electrical and radio frequency (RF) systems where short circuit failures may occur. Prior art carbon fiber and graphite filled composites exhibit similar thermal management behavior to metals. Prior art polymers and composites can improve electrical resistivity but have poor thermal conductivity.

[0088] The materials, products, and manufacturing processes described herein can provide solutions for a variety of thermal management solutions and other applications requiring complex geometries of thin ceramics. The devices and materials formed by the processes described herein can be used in heat exchangers, cold plates, printed circuit boards, high performance CPUs, high density electronic platforms, electronic chassis systems, RF devices, RF and phased antenna arrays, low loss dielectric RF components, radomes, power inverters, solar cells, neutron shielding, high temperature heat shielding, heat shields for cube satellites, encapsulants, medical devices, and laminates with complex surface geometries.

[0089] The process and products can be used in industries such as aerospace, defense, renewable energy, clean energy, environmental, electric vehicle (EV), transportation and medical device industries. The process can be integrated into other manufacturing processes developed to design and mold custom ceramic heat spreaders with complex geometries tailored specifically for specific electronic devices.

[0090] The first observation of thermoforming was made during an experiment comparing the thermal shock potential of a commercially available sintered hBN sheet (3 in. x 5 in. x 1 / 16 in. hBN sheet, McMaster-Carr), which exploded during application of a thermal shock, with a ceramic composite preform containing aligned hBN particles, according to the techniques described herein, but without catastrophic reaction. Both materials, with different compositions, contained only hBN and B2O3. When tested by placing a load on top of the sample and heating a propane torch underneath it, the ceramic composite in the preform began to deform and dropped to the floor. The material was intact and permanently deformed. The same experiment was repeated to verify, with different shapes being deformed depending on the position of the flame (Figure 23).

[0091] A thermoforming processing method was then tested, showing that above the melting temperature of the matrix, the material could be formed into complex shapes without failing at a critical load. A U-shaped mold was created to test the processing method, confirming that the forming process was repeatable and controllable (Figure 24).

[0092] In one example, hexagonal boron nitride (hBN) was selected as the phononic ceramic particles and boron oxide was selected as the ceramic matrix. The general process for creating preforms or coupons is divided into three steps: 1) material compounding, 2) curing and bakeout, and 3) sintering. A concentrated ceramic slurry (54 vol%) is mixed with commercially available hBN, an oxygen donating polymer, a photoinitiator, and a diluent to achieve a slurry rheology that flows only under shear stress. Here, the oxygen donating polymer, photoinitiator, and diluent are as follows: acrylate resin (70 vol%, density 1.15 g / cm3), ... 3 , EBECRYL230, Allnex), isobornyl acrylate (30% by volume, density 0.986 g / cm 3 , IBOA, Sigma-Aldrich) was added as a reactive diluent, and two photoinitiators (0.1 vol%, 1-hydroxycyclohexyl phenyl ketone 99%, and phenylbis(2,4,6-trimethylbenzyl)phosphine oxide 97%, Sigma-Aldrich) were added in a 1:1 ratio. Finally, hBN, 12 μm platelets (54 vol%, PT-120 hBN, Momentive) were added at a volumetric concentration relative to the resin. In this case, additional solvent was required to produce a uniform paste that would flow under shear conditions. Ethanol (8 vol%, Sigma-Aldrich) was added to further reduce the viscosity of the mixture, creating a slurry with reduced loading for a time. The material was then homogenized in a speed mixer (DAC 150.1 FVZ-K, FlackTek Inc) at 1500 RPM for 2 minutes. The final product yielded a slurry that behaved as a Hershel-Buckley fluid, in that it did not deform until a shear stress was applied.

[0093] To achieve exceptional particle orientation and infiltration throughout the CMC, the vibration-assisted casting method described herein was employed to align a high volume fraction (60 vol%) of hBN particles in the polymer green body. High loadings of hBN particles suspended in a liquid photosensitive resin behave as Herschel-Buckley fluids, requiring shear in the form of vibration to flow effectively. Furthermore, these dense particle suspensions were subjected to vibrational energy during the tape casting process, resulting in even higher fluidization and shear alignment of the in-plane hBN (as described above with respect to Figures 1A-1C). After tape casting, the suspension was exposed to UV light to polymerize the photosensitive resin and fix the oriented hBN particles into the solid green body (as described above with respect to Figure 1D).

[0094] These polymer green bodies were then pressureless sintered in an oxygenated environment to grow a matrix of boron oxide that replaced the polymer matrix and encapsulated the hBN. An oxygen-rich acrylate system was selected to promote uniform growth of boron oxide throughout the thickness of the green bodies. The two-stage sintering process (described above) began with a debinding (polymer burn-off) stage that left approximately 0.3 at% trapped oxygen from the polymer, which has an affinity for boron, and acted as a seed for the oxidation process. The hBN was then partially oxidized by increasing the sintering temperature to 1050 °C. The trapped oxygen enhanced and homogenized the oxidation rate of the hBN throughout the part, resulting in a brilliantly white all-ceramic part described as a preform or blank.

[0095] The orientation of hBN in the preform microstructure also allowed for in-plane flow during the thermoforming process. Specifically, when a boron-based all-ceramic preform was placed into a negative mold and heated above 450 °C, the boron oxide (BO) melted and the material again behaved as a viscous particle-filled Bingham pseudoplastic, exhibiting a yield stress that prevented flow until a critical load was applied. Thus, these hBN all-ceramics could be thermoformed by applying sufficient heat (500-700 °C), pressure (described below), and dwell time (>10 min), as exemplified in the molding of a complex all-ceramic human face using a metal 3D-printed Inconel 625 mold (see Figure 2A).

[0096] To understand the thermal properties, the in-plane and through-plane thermal conductivity were measured. Due to the shear alignment of the hBN particles during tape casting, the in-plane thermal conductivity was expected to be higher compared to through-plane. The through-plane thermal conductivity was characterized with ASTM E1461 and found to be 3.52+ / -0.67 W / mK at room temperature. The in-plane thermal conductivity was characterized using the Angstrom method (see Section 2.4, Materials and Methods) and found to be 12.8 W / mK at room temperature. Both of these values ​​are well below the theoretical conductivity of pure hexagonal boron nitride, highlighting the thermal resistance that the boron oxide matrix provides to the detriment of overall electrical conductivity. Nonetheless, these thermal conductivity values ​​make these boron nitride-based all-ceramics useful in the space for dielectrics that can conduct heat, especially when density and high resolution formability are important to the application space.

[0097] To quantify the mechanical robustness of the boron nitride-based all-ceramic preforms, flexural characterization was performed on sintered specimens at three deflections (see Section 2.4, Materials and Methods). Both 4- and 6-hour sintering dwell times were tested, resulting in increasingly robust mechanical properties (Figure 13). The 6-hour sintered sample had a significantly higher flexural strength and a significantly higher flexural strain at break, ε 屈曲=0.78+ / -0.17%, bending elasticity is 0.22+ / -0.037MJ / m 3 And U r =1 / 2σ flex ε flex As a benchmark, a commercial sample (McMaster Carr) of a hot pressed boron nitride based all-ceramic sold for thermal management was purchased and tested in the same manner, resulting in significantly reduced flexural strength, strain at break, and resilience. In particular, the commercial sample was found to lack an oriented microstructure and to have no thermoforming capabilities. Compared to conventional ceramic materials such as the commercial sample, the boron nitride based ceramic materials tested in this example showed superior resilience. This appears to stem from the underlying oriented nacre-like microstructure of these materials. A sintering residence time of 6 hours was used for the remainder of this example.

[0098] The composition of the boron nitride based ceramic composites fabricated and considered herein was expected to be hBN and B2O3 with a moderate amount of porosity due to pressureless sintering and non-optimized fabrication at this stage. To confirm these expectations, the composition was authenticated using a modified Archimedes method in combination with XRD (see Section 2.4, Materials and Methods). The fabricated ceramic composites had a molecular weight of 1.42 + / - 0.10 g / cm 3 and balance hBN and B2O3 contents of 49.8 vol% and 50.2 vol%, respectively. The samples had high porosity contents, calculated to be 37.9 vol%. Nevertheless, these sample compositions exhibited significant mechanical properties as discussed above, and yielded preform "blanks" that could be effectively thermoformed into complex, thin shapes.

[0099] Thermoforming and current shape resolution of ceramic matrix composites. To investigate the relationship of processing structure within thermoformable ceramic composites, the yield strength of these preforms at 500°C was displayed with a simple support structure as shown in (Figure 14). There was no flow under a force of 0.01 N, even though the temperature was above the melting temperature Tm of B2O3 (Tm = 450°C). As the load was increased, the samples deformed with maximum deflection at a force of 0.2 N with a simply supported structure. This behavior supports the hypothesis that these boron-based ceramic composites behaved as Bingham plastics due to their microstructure and composition of the fluid-like matrix, solid loading near 50 vol%, and being a direct analogue of concentrated slurries.

[0100] To understand the temperature dependence of preform formability, fine feature molds (such as those described in Figure 9) were tested at elevated temperatures to establish contact regions (Figure 8B) corresponding to flow characteristics. At these elevated temperatures, the ceramic composite had a liquid matrix of boron oxide that decreased in viscosity as the temperature increased above the Tm of B2O3. At a lower temperature of 500 °C, just above the Tm of B2O3, thermoforming of hBN ceramic composite preforms was possible for feature widths greater than 2 mm and was limited to features less than 5 mm wide. Features less than 2 mm at 500 °C were not resolved due to inhibitory activation energies (characterized as mechanical interlocking regions). For 600 °C, finer features could be resolved by lowering the transition in groove contact regions to feature sizes of 1.6 mm. At 600 °C, feature sizes greater than 1.6 mm wide allowed the material to be fully formed (characterized as groove contact regions). At 700 °C, even more flow is possible, resolving feature widths up to 0.6 mm (characterized as bonded regions). Within the bonded regions, the molded ceramic composite can adhere to the mold surface, necessitating high-temperature demolding to remove the molded part. Further increases in temperature were limited by the oxidation of BN above 1000 °C at longer times and the evaporation temperature of the oxide matrix at 1375 °C at shorter times. The oriented hBN microstructure is believed to play a role in the forming process due to the ability of aligned grains to flow past each other, such that isotopically aligned systems cause localized grain jamming due to steric hindrance. Using the step mold shown in Figure 10, ceramic composite preforms were successfully thermoformed with feature sizes as wide as 5.8 mm at temperatures as low as 500 °C. Here, the preforms were able to withstand 90° bends in 5 mm steps without failure. The thermoforming process demonstrated repeatability and reliability under a variety of load and temperature conditions.

[0101] To further characterize the capabilities of this manufacturing process, a systematic forming study using deep-draw dies as in Figure 11 characterized the success of various draw ratios (defined as the depth of the feature relative to its width). The dies were designed with a maximum draw ratio that varied with sample size, with maximum pin lengths ranging from 1.6 mm to 6.93 mm, and the maximum possible draw ratio was 2.32 for each die size. The results revealed a dependence of die size on the maximum draw ratio that the preform could withstand across temperatures before tearing (Figure 15). A clear upper limit near a draw ratio of 1.0 was observed independent of temperature and die size. This limit also represents a threshold for deep drawing, which is likely a function of sheet thickness, die preparation, and die process, and can be further optimized to find the limits of this process. Lower forming temperatures require higher pressures for thermoforming, which coincides with the activation energy of flow in the molten B2O3 matrix. When the maximum achievable draw ratio was exceeded, tearing of the preform was observed. The higher temperatures of 700°C allowed for thermoforming under smaller compressive stresses, but generally resulted in preforms with lower viscosities and susceptibility to tearing. Surprisingly, drawing ratios of greater than 1.0 have been demonstrated, and forming results using this method are classified as deep drawing. Deep drawing is an aggressive area of ​​thermoforming that also poses significant challenges for certain thermoplastic polymers and metals.

[0102] Performance testing for thermal management applications The application of thermoforming of ceramic composites to thermal management applications was demonstrated through in situ performance testing. Specifically, the entire thermoforming process described herein was applied to the fabrication of a short-run all-ceramic heat spreader for a custom-made printed circuit board (PCB). With reference to Figures 16A and 16B, the process was explored using a Raspberry Pi (RPi) circuit board as the PCB with an internal thermocouple to track the operating temperature. First, a mold was designed from a 3D CAD model of the PCB and metal 3D printed from Inconel 625. The phononic ceramic composite preform was thermoformed at the bonding contact area (500°C for these feature sizes). After light post-processing, the thermoformed material was pressed onto the PCB and set using a small amount of thermal paste to minimize the thermal impedance of the connection and allow robustness to device handling.

[0103] To evaluate performance, the PCB was fully throttled for 10 minutes using a custom program to allow the processor chip to reach its maximum steady-state temperature (see Section 2.4, Materials and Methods). Comparisons were made with the as-received PCB, a PCB additionally provided with a metal heat sink package for cooling, and the thermoformed ceramic composite heat spreader described herein. The metal heat sink package provided by the supplier featured a parallel fin aluminum heat sink required to contain a 9.07 mm thick spatial envelope compared to the 0.68 mm thick ceramic composite heat spreader. In a comparable test, the internal temperature of the processor chip was evaluated using internal thermocouples, showing that the ceramic composite heat spreader (maximum temperature 52.9 °C) performed better than the larger aluminum heat sink package (maximum temperature 56.8 °C), both of which offered cooling advantages over the as-received system (maximum temperature 60.5 °C) (Figure 17A).

[0104] Additionally, the surface temperature of the PCB in all three cases was measured with a FLIR camera and showed similar results. To highlight the performance of the low-profile conformal all-ceramic heat spreaders, we plotted the cooling effect of each thermal management solution on the system as received normalized by the required geometric envelope thickness (in °C / mm) (Figure 17B). When the cooling effect (measured by the drop in temperature compared to the as-received control) of the ceramic composite heat spreader and the metal heat sink were normalized by the thickness of the thermal management solution, the all-ceramic thermoformed heat spreader outperformed the metal heat sink by more than 10 years on a semi-log plot scale. When the geometric envelope of the thermal management solution must be minimized, this normalization shows that the thermoformed all-ceramic heat spreader outperformed the current prior art metal heat sink by 10 years on a semi-log performance plot. Additionally, these ceramic composite heat sinks are made of a strong dielectric, which helps them to use closer contact with the electrical connectors in the PCB and move heat more effectively.

[0105] Material Composition The general process for creating preforms and coupons is divided into three steps: 1) compounding of materials, 2) curing and bakeout, and 3) sintering. A concentrated ceramic slurry (54 vol%) is mixed together with commercially available hBN, oxygen donating polymer, photoinitiator, and diluent to achieve a slurry rheology that flows only under shear stress. In this example, the oxygen donating polymer, photoinitiator, and diluent are as follows: acrylate resin (70 vol%, density 1.15 g / cm3); 3 , EBECRYL230, Allnex), isobornyl acrylate (30% by volume, density 0.986 g / cm 3, IBOA, Sigma-Aldrich) was added as a reactive diluent, and two photoinitiators (0.1 vol%, 1-hydroxycyclohexyl phenyl ketone 99%, and phenylbis(2,4,6-trimethylbenzyl)phosphine oxide 97%, Sigma-Aldrich) were added in a 1:1 ratio. Finally, hBN, 12 μm platelets (54 vol%, PT-120 hBN, Momentive) were added at a volumetric concentration relative to the resin. In this case, additional solvent was required to produce a uniform paste that would flow under shear conditions. Ethanol (8 vol%, Sigma-Aldrich) was added to further reduce the viscosity of the mixture, creating a slurry with reduced loading for a time. The material was then homogenized in a speed mixer (DAC 150.1 FVZ-K, FlackTek Inc) at 1500 RPM for 2 minutes. The final product yielded a slurry that behaved as a Hershel-Buckley fluid, in that it did not deform until a shear stress was applied.

[0106] Preform Manufacturing Process Preform fabrication was completed by applying vibration and surface shear forces from the casting blade to spread a thin layer (200 μm) for photopolymerization. This process was repeated six times until a thickness of approximately 1.2 mm was reached. The vibrating tape casting system utilizes vibration to reduce viscosity and fluidize the material system. The vibration of the modified stage was generated by a single-axis vibrator (JT-51B vibrator, Jintai) and was initially increased until fluid motion was observed, and then vibration was set at that level for the remainder of the test. After fluidizing the slurry with oscillatory shear, the casting blade thinned the material into a sheet of user-defined thickness, and after the vibration was turned off, the binder was cured by UV exposure using a 405 nm DLP UV projector (PRO4500, Wintech Digital System Technology Corp.) (see Figures 1A-1D).

[0107] The limitations of this process were that layer thicknesses could fall below 100 μm due to delamination during the sintering process, and could not exceed 20 times the grain size to obtain reasonable grain alignment. Additionally, single layer samples could be processed using translucent sheets. Here, a 0.25 inch thick piece of glass was used to force the fluid during vibration and spread it into a planar mold. Once the material was spread, it was exposed to a 405 nm UV lamp and placed on top of the glass to create a green body. Pressing combined with vibration created a squeeze-flow type environment where the streamlines formed perpendicular to the force of the press plate created a shear flow that forced the grains into a preferred direction, aligning the grains using the same shear force mechanism as a casting blade. The negative planar mold was made of glass or clear acrylic to allow light to reach the sides of the sample during curing. The negative space was a rectangle no larger than 80 mm by 60 mm to allow all the material to fit under the curing light, and the top was a square sheet of 0.25 inch glass that was used to force the material into the negative space when the vibration was on. A limitation of this process was the curing time. For example, layers made of 12 μm hBN particles with a particle size dependence of thickness 1-1.5 mm were cured for at least 60 minutes, whereas layers from the DLP printing process took 1-2 minutes per layer depending on the layer thickness. After curing, the ethanol was baked out of the samples in a 60 °C oven for over 2 hours, further hardening the green bodies as the ethanol evaporated. These samples were then ready to be sintered.

[0108] The sintering profile was: 1 hour ramp to 60°C, 20 minute dwell, 1 hour 500°C ℃ The resin was burned off and the temperature was increased to 1050°C for 1 hour. ℃The temperature was raised to 0.25°C and held for 6 hours to allow the B2O3 to form a secondary binder. The samples were then naturally cooled to room temperature for handling. Of note, with either method, measuring the dimensions of the cast sheet allows for shrinkage due to polymer burn-off during sintering to be taken into account. Shrinkage was tested by tracking the dimensional change of rectangular samples in the green and sintered states and was found to be 12.4 + / - 0.37% in the X-axis, 11.4 + / - 3.85% in the Y-axis, and 19.6 + / - 3.21% in the Z-axis (through the plane). The shrinkage was anisotropic, likely due to the in-plane orientation of the hBN grains which reduced the in-plane shrinkage. In this example, shrinkage was addressed by scaling up the dimensions of the green bodies with these corresponding shrinkage rates so that the sintered parts exhibited the desired dimensions. Additionally, limiting the adhesion between the cured coupon and the surface was useful to avoid tearing during sample removal. This was achieved by applying Kapton tape to the bottom of the casting surface in both processes, and by coating the sheet glass with a release agent in the press casting process.

[0109] Mold design and manufacturing Molds were designed to demonstrate the bending, stretching, conforming capabilities, and resolution of the process and materials. Each mold was designed in SolidWORKS (Dassault Systems, France) and fabricated using Inconel 625 filament with a Markforged metal 3D printing and sintering system (Markforged, MA). Inconel was selected to sustain repeated heating and cooling cycles during the thermoforming process. Five types of molds were prepared: 1) a coarse-featured mold (Figure 10) that helped define the bend angles and large step shapes possible at the 500°C minimum forming temperature; 2) a 100 ℃A fine feature mold (Figure 9) to study the different flow regimes as the temperature increases from 500°C to 700°C in the first step; 3) a human face mold (Figures 2A, 18A, 18B) to demonstrate multiple feature resolution in a single sheet; 4) several deep drawing molds (Figure 19) to perform the traditional deep drawing process used in metals and authenticate the current thermoforming resolutions possible, as well as 5) a Raspberry Pi mold (Figure 16A) to study the performance of the thermoformed material as an all-ceramic morphology-tunable heat spreader.

[0110] Thermoforming Process After the oven was heated to the desired temperature (500°C, 600°C, and 700°C), the mold was placed in a box furnace (KSL 1200X, MTI Corp.). The melting temperature of boron oxide is 450°C. The temperature was heated 50°C above the melting temperature to reduce the viscosity in the melt and allow forming. It was observed that forming was not possible before 500°C. An increase in temperature was necessary to provide finer features, but with the current mold, temperatures above 700°C were not required to achieve fine features. Once the oven was heated, the mold and sample were inserted into the oven and allowed to equilibrate for 10 minutes. After the dwell time, the oven was opened and the top of the mold was pressed to induce forming. The mold was then removed from the oven and the part was removed from the mold.

[0111] Material yield characterization at forming temperature To understand the fundamentals of the force required to induce forming, the yield force was characterized. This was completed with the same heating process at 500 °C with a precise mass load acting as the loading force, except a rectangular envelope was placed on top of the two steel blocks. The mass was increased from 1 g to 20 g. The increasing mass was placed on top of the sample and allowed to infiltrate for 10 minutes at 500 °C. After the infiltration time, the door was opened and a ruler was placed on the side of the oven to take pictures for post-processing in ImageJ. Each image was then processed to measure the deflection of the sample. In each case, the samples were continuously loaded, imaged, and measured with the incremental mass for all three samples until the sample was fully deformed under the loading conditions.

[0112] Three-point deflection test The mechanisms were tested using a three-point deflection setup (Instron, Norwood, MA). The fixture span was 10 mm long with a pointed fixture. The extension rate was set at 10 mm / min with a 500 N load cell. All mechanically tested parts were at least 40 mm x 12.5 mm x 1 mm (l, w, t). All samples were lightly sanded with 220 grit sandpaper to smooth the surface and eliminate small surface defects from the printing process prior to all mechanical testing.

[0113] Thermal Conductivity Measurement To measure thermal conductivity, different methods were used for in-plane and through-plane properties. In both cases, the specific heat capacity was measured using differential scanning calorimetry (Netzsch DSC 204) according to ASTM E1269. For through-plane thermal conductivity, the through-plane thermal diffusivity was measured according to the laser flash method of ASTM E1461 (Netzsch LFA 447 as instructed by Netzsch). The diameter of the samples was 10 mm and the thickness was 0.9 mm. For the in-plane thermal conductivity, the in-plane thermal diffusivity was determined by the Angstrom method. Briefly, the samples were clamped between two bonded heater wires connected to a sinusoidally oscillating DC power source with a frequency of 0.002 Hz and an amplitude of 2.1 W. The opposite ends of the samples were placed 1 mm on an aluminum billet. The thermocouples were placed at distances of 5 mm and 10.8 mm from the heat source, and the setup was sealed to minimize convection fluctuations. After about 3 hours of measurement, the temperature profile was fitted to a sine wave and the corresponding amplitude and phase shift were extracted. The in-plane diffusivity is α = L 2 The thermal profile was calculated as 0.091 cm / (2Δtln(M / N)), where L is the distance between the thermocouples, Δt is the time shift between the temperature profiles, and M and N are the amplitudes measured by the thermocouples closer and further from the heat source, respectively. This analysis revealed that the thermal profile was 0.091 cm for the boron nitride-based ceramic composites described herein. 2An in-plane thermal diffusivity of 1.0 kV / s and an associated in-plane thermal conductivity of 12.8 W / mK were obtained. Furthermore, the method was confirmed to accurately measure known samples (e.g., copper, borosilicate glass).

[0114] Composition analysis of boron nitride-based all-ceramics To measure the composition of the all-ceramics, a modified Archimedes method was combined with XRD to authenticate the composition. The composition of three rectangular block samples was measured by measuring the volume with a vernier caliper and the mass with a precision balance (ATY224, Shimadzu). The samples were completely dissolved in hot water (60 °C) sufficient to remain below the solubility limit, leaving the insoluble hBN particles in the boric acid aqueous solution, and the slurry was filtered through a 0.45 μm nylon filter to remove the hBN particles. The pre-weighed filter was dried overnight in an oven at 60 °C and weighed to measure the mass of hBN. The removal of B2O3 was confirmed by small angle X-ray diffraction (SAXS) measurements (ULTIMA IV, Rigaku) ​​(Figures 20A and 20B). The measured mass of hBN and the original sample mass provided the mass percentage of hBN and B2O3 in each sample. The masses were 2.1 g / cm for hBN and B2O3, respectively. 3 and 2.46 g / cm 3 Finally, knowing the relative volume percentages of hBN and B2O3 in combination with the original part densities allowed the calculation of the volume percentage of air.

[0115] Deep drawing Similar to the yield property evaluation method described above, deep drawing was completed by heating the oven to 500°C, 600°C, and 700°C and testing the drawing properties of the material using a specific die designed for the process (Figure 19). The drawing process was proceeded with precision ingots (20g, 50g, 100g, 200g, 500g) to induce deformation. The die assembly with the drawing male die and preform was loaded into the oven at temperature and allowed to infiltrate for 10 minutes before applying the ingot. After 10 minutes, the door was opened and the ingot was placed on the drawing male die for approximately 10 seconds before being removed. The above method was accomplished to control the flow process by the load and achieve the highest possible drawing depth under the selected load. After removing the ingot, the die assembly was removed from the oven, the sample was measured, and it was returned to the die for further drawing. This process was repeated, increasing the load until tearing occurred. At this point, the sample was considered to have failed. Examples of drawn and torn samples can be seen in Figure 21. Once the drawing threshold was exceeded, the first face tear occurred at the curved end, at which point the top of the sample sheared off upon further pressing. It can also be observed that once the top was removed, the wall of the part thinned, visible in the small diameter formed specimen. This indicates that material extrusion was occurring as opposed to pure drawing. This was also evident as the diameter of the material did not change during this deep drawing process.

[0116] Deep drawing, in particular, is a broad category that encompasses many different molds, so these are designed to allow flexibility for testing if one mold design proves more successful than another. To that end, the molds were designed to test three geometric parameters: diameter size, male mold length, and male mold radius, as well as a permutation of forming curvatures. The base deep drawing mold is composed of three parts: the male mold, the base, and the male mold guide. The male mold is the positive mold, the base is the negative mold, and the male mold guide is a passive element that helps align the pin with the base cavity and keeps the material from unnecessarily deforming during the process. Note that in the orientation of Figure 11, the male mold is inserted into the base cavity through the guide hole, and the guide hole is aligned by the guide pin and the fillet corners of both the base and guide hole parts to ensure they are properly assembled. The deep drawing process is as follows: the ceramic material is inserted between the base and guide parts. The pin is then pressed down to draw the material into the base cavity. A gap of at least 1.2 mm exists between all positive and negative die interfaces to account for the space occupied by the material. Three common sizes of die were tested to determine the continuity between scale-ups. Based on the smallest deep-draw die, the other two were scaled up by a factor of two and three, respectively. The pin length for each die was selected using R=d / D, the ratio of the pin depth d to the pin diameter D when the pin is inserted into the die. Pins with lengths that satisfied ratios of 1.0, 1.5, and 2.0 were manufactured and tested for each die size category.

[0117] The main variables in deep drawing of all-ceramics are the melt temperature of the matrix, the force F of the pull pin, the strain rate of the pull pin, the male die diameter, the preform diameter, the clearance between the base hole and the pin diameter, the pin tip radius, the corner radius of the base hole, the surface roughness of the die, the contact force between the guide die and the material, and the lubrication between all contacting surfaces. The deep drawing die was tested at graded high temperature release up to 800 °C. In all tests, the diameter of the samples was measured before and after the test. It was observed that the diameter of the samples did not change during the deep drawing process. Therefore, only the extrusion of the material occurred, and no actual drawing occurred. This may be due to the very rough surface of the printed die. Other variables may have also caused the premature failure. It was also observed that as the temperature increased, the load required for deformation decreased significantly. This was expected because as the temperature increased, the reduction in the matrix activation energy required for flow to occur decreased. However, an interesting trend between die sizes showed that as the punch diameter decreased, the drawing ratio also decreased. This is most likely due to the clearance between the male die diameter and the base hole. The material limit was met with a maximum value of pin to sample tear of 1:1 ratio. Also, the best samples using the small die do not exceptionally exceed 110% drawing depth ratio.

[0118] Raspberry Pi Stress Testing and FLIR Imaging Running Programs To evaluate the thermal management potential of these thermoformed ceramic materials, they were tested using a simple Raspberry Pi PCB as a proof of concept. Two separate methods were applied to measure the internal thermocouple and external surface temperatures. The internal thermocouple and custom software measured the CPU core temperature under various load conditions. The load profile was set to idle for 30 seconds, throttled for 10 minutes, and then back to idle for 2.5 minutes.

[0119] Data Processing During the time profile, the temperature was monitored every second and the data was saved to a text file for post processing. Once the data was collected, it was transferred to Excel for calculations and then to OriginPro plotting software for data visualization. The data was analyzed by plotting the raw data to understand the difference in cooling capacity between each heat sink and normalizing by the height of each heat sink to promote the benefits of the low-profile design of the thermoformed heat sinks.

[0120] FLIR Imaging Referring to Figures 22A and 22B, the surface temperatures were measured with a FLIR EST230 infrared camera. To control the emissivity between the metal and ceramic surfaces, both were coated with a dry carbon spray coating following the same protocol as the laser flash method of ASTM E1416. Three coats were applied to each heat sink. Each coating was allowed to dry for 10 minutes between coats. The FLIR camera recorded and plotted the data live. The data was then extracted and post-processed in plotting software, and a live plotting movie was created using Matlab.

[0121] Figure 22A shows the heat sinks carbon coated to ensure that the emissivity value of 0.96 is the same for both materials. The plotted surface temperatures show the same 4°C difference as the internal thermocouple data described herein. In Figure 22B, a FLIR thermal still image shows the thermal profile of each heat sink and a scale bar representing the temperature spectrum of the image.

[0122] As used herein, "consisting essentially of" allows for the inclusion of materials or steps that do not materially affect the basic and novel characteristics of the claim. Any reference to the term "comprising" herein may be replaced with "consisting essentially of" or "consisting of," particularly in describing a component of a composition or in describing an element of a device.

[0123] The present technology has been described in conjunction with certain preferred embodiments and aspects, and it is to be understood that the present technology is not limited to the construction, operation, precise materials or precise details of the embodiments or aspects shown and described, and that various modifications, substitutions of equivalents, changes in composition, and other modifications to the embodiments and aspects disclosed herein will be apparent to those skilled in the art.

[0124] US Pat. No. 10,834,854 is incorporated herein by reference in its entirety.

Claims

1. 1. A method for producing a ceramic composite compact, the method comprising: (a) providing a preform having a first structure and having two opposing surfaces, said preform comprising a ceramic matrix composite material comprising ceramic particles within a ceramic matrix, said ceramic particles having a platelet crystal structure arranged in parallel alignment transverse to a thickness direction extending between two opposing surfaces of said first structure; (b) thermoforming the preform, which comprises the steps of: (i) heating the preform in the mold to a temperature above the melting or softening temperature of the ceramic matrix, and preferably below the melting or decomposition temperature of the ceramic particles; and (ii) applying a load to the mold, thereby transforming the first configuration of the preform within the mold to a second configuration to form a ceramic composite compact; (c) cooling the ceramic composite compact in the mold; and (d) removing the ceramic composite compact from the mold.

2. 10. The method of claim 1 , wherein the step of providing the preform comprises: (a-1) providing a slurry containing a plurality of said ceramic particles in a polymer binder; (a-2) vibrating the slurry to provide a suspension in which the slurry is fluidized; (a-3) forming the slurry into a layer on a stage or in a preform mold so that the ceramic particles are aligned in parallel; (a-4) solidifying the polymer binder to form a solid green body containing the ceramic particles maintained in parallel alignment; (a-5) debinding the solid green body at a temperature first at which the polymer binder decomposes, leaving a ceramic body comprising the ceramic matrix and the ceramic particles; and (a-6) sintering the ceramic body at a second temperature higher than the first temperature, whereby the ceramic particles remain parallel aligned in the ceramic matrix.

3. The method of claim 2, wherein in step (a-6), the ceramic particles are partially oxidized.

4. 3. The method of claim 2, wherein the slurry provided in (a-1) further comprises one or more photoinitiators and one or more diluents mixed with the ceramic particles and the polymer binder, wherein the slurry flows under shear stress.

5. The method of claim 2 , wherein the polymeric binder is selected from the group consisting of polymerizable resins, epoxies, melt-melted thermoplastics, and solvent-borne thermoplastics.

6. The method of claim 5, wherein the polymerizable resin comprises an acrylate, a methacrylate, a polymethylmethacrylate, a thiolene resin, an epoxy resin, a thermoplastic polymer, a wax, a methylcellulose, a phenolic resin, a polyvinyl acetate, a polyvinyl alcohol, or a rubber adhesive.

7. 3. The method of claim 2, wherein in the solidifying step of (a-4), solidifying the polymer binder comprises curing the polymer binder at a curing temperature to form the solid green body.

8. 3. The method of claim 2, wherein the polymer binder is an oxygen donating material, and in the solidifying step of (a-4), the polymer binder donates oxygen for seeding an oxidation process in the ceramic particles.

9. 3. The method of claim 2, wherein the step (a-3) of forming the slurry into the layer comprises tape casting the slurry onto the stage or depositing the slurry into the preform mold.

10. 3. The method of claim 2, wherein the step (a-2) of vibrating the slurry occurs prior to the step of forming the slurry in the bed, during the step (a-3) of forming the slurry in the bed, after the step (a-3) of forming the slurry in the bed, or a combination thereof.

11. 3. The method of claim 2, wherein the step (a-2) of vibrating the slurry and the step (a-3) of forming the slurry into a layer are repeated multiple times to form the sheet.

12. 3. The method of claim 2, wherein the polymer binder is a photopolymerizable resin, and the step (a-4) of solidifying the polymer binder comprises applying ultraviolet or visible light to the slurry.

13. The method of claim 1 , wherein in said thermoforming step (b), the temperature to which said preform is heated is below the decomposition and / or evaporation temperature of said ceramic matrix.

14. The method of claim 1, wherein in said thermoforming step (b), said preform is heated to a temperature of from about 400°C to about 1000°C, or from about 500°C to about 700°C.

15. 2. The method of claim 1, wherein in the load applying step (b)(ii), the load stress ranges from about 50 kPa to about 100 MPa, or from about 500 kPa to 5 MPa.

16. 2. The method of claim 1, wherein in said thermoforming step (b), said mold comprises a lower portion having a negative surface and an upper portion having a positive surface, and said load is applied to said preform through the upper portion of said mold.

17. 10. The method of claim 1, wherein in said thermoforming step (b), said mold comprises a negative surface and a positive surface, each surface including at least one surface feature having a feature size of about 1 mm or less in any dimension.

18. 20. The method of claim 17, wherein the feature size is less than or equal to about 200 μm in any dimension.

19. 10. The method of claim 1, wherein in the thermoforming step (b), the mold has a maximum draw ratio of feature height to feature width of about 1:

1.

20. The method of claim 1 , wherein the ceramic particles comprise flaked oxides, nitrides, carbides, sulfides, fluorides, or combinations thereof.

21. 2. The method of claim 1, wherein the ceramic particles are hexagonal boron nitride, hexagonal aluminum nitride, aluminum oxide, molybdenum disulfide, clay, cesium oxide, graphene, flaky ferrite, calcium phosphate flakes, zirconia flakes, silica flakes, or combinations thereof.

22. The method of claim 1 , wherein the ceramic matrix comprises boron oxide, silicon dioxide, glass flake, silver coated glass flake, lithium oxide-silica mixture, magnesium oxide-silica mixture, or combinations thereof.

23. 2. The method of claim 1 , wherein the ceramic matrix comprises a glassy material or glassy-ceramic material mixture having a softening phase or melting temperature within the operating temperature range of the material forming the mold and below the melting or decomposition temperature of the ceramic particles.

24. 10. The method of claim 1, wherein the ceramic particle concentration in the ceramic composite compact is from about 30% to about 90% by weight and the ceramic matrix concentration is from about 10% to about 70% by weight.

25. 2. The method of claim 1, wherein the ceramic particles in the ceramic composite compact have a diameter of about 1 μm to about 100 μm, or about 5 μm to about 45 μm, and a thickness of about 3 to about 100 times less than the diameter.

26. The method of claim 1 , wherein the preform has a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to 3 mm.

27. The method of claim 1 , wherein the ceramic composite compact has a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to about 3 mm.

28. The method of claim 1 , wherein the ceramic particles comprise phononic crystal particles.

29. 2. The method of claim 1, wherein lateral bonds between layers of the ceramic particles in the preform are weak enough to permit sliding of the ceramic particles when subjected to the load in thermoforming step (b)(ii).

30. The method of claim 1 , wherein the ceramic composite compact has an in-plane thermal conductivity transverse to the thickness dimension, the in-plane thermal conductivity being greater than the through-plane thermal conductivity.

31. 2. The method of claim 1, wherein the ceramic composite compact has an in-plane thermal conductivity transverse to the thickness dimension of about 5 W / mK to about 100 W / mK, or about 10 W / mK to about 40 W / mK at ambient temperature.

32. 10. The method of claim 1, wherein the ceramic composite compact is configured as a thermal management device, a heat sink or heat spreader for a printed circuit board, a heat exchanger, a cold plate, a low loss dielectric RF component, a radome, a power inverter, a solar cell, a neutron shield, a high temperature heat shield, a cube satellite, an encapsulant, or a heat shield for a medical device.

33. 1. A method of fabricating a thermal management device for a heat generating component, the method comprising: (a) providing a mold configured to fit at least a portion of the heat generating component; and (b) producing a ceramic composite compact according to any one of claims 1 to 32 using the mould provided in step (a) to form a thermal management device; Includes.

34. 34. The method of claim 33 further comprising: (c) fitting the ceramic composite compact into the heat generating component or a part thereof; The method comprising:

35. 34. The method of claim 33, wherein the heat generating component is a printed circuit board, a central processing unit, a high density electronic platform, an electronic chassis, an RF device, an RF or phased antenna array, a low loss dielectric RF component, a radome, a power inverter, a solar cell, a neutron shield, a cube satellite, or a medical device.

36. 1. A method of fabricating a thermal management device, the method comprising: (a) providing a design for a heat generating component or portion thereof requiring thermal management; (b) fabricating a preform mold designed to fit a first structure complementary to the heat generating component or portion thereof; (c) fabricating a mold designed to fit a second structure complementary to the second structure, the second structure being more precisely complementary to the heat generating component or portion thereof than the first structure; (d) fabricating a preform using a preform mold, wherein the preform has the first structure and has two opposing surfaces, wherein the preform comprises a ceramic matrix composite material, the material comprising ceramic particles within the ceramic matrix, the ceramic particles having a platelet grain structure aligned parallel to a thickness direction extending between the two opposing surfaces; (e) thermoforming the preform in the mold to provide a thermal management device in the second configuration, the thermoforming comprising: (i) heating the preform in the preform mold to a temperature above the melting or softening temperature of a ceramic matrix; (ii) applying a load to the preform mold, thereby transforming the first configuration of the preform within the mold to the second configuration to form a thermal management device; Including, (f) cooling the thermal management device within the mold; and (g) removing the thermal management device from within the mold; The method comprising:

37. 37. The method of claim 36, wherein in step (a), the design includes a negative geometry of the heat generating component or portion thereof provided by a three-dimensional computer-aided design model of the heat generating component or portion thereof or by a three-dimensional scan of the heat generating component or portion thereof.

38. 37. The method of claim 36, wherein step (b) comprises fabricating the preform mold and / or the mold from a metallic material by an additive manufacturing or machining process based on a three-dimensional computer-aided design model of a design of the heat generating component or portion thereof.

39. 40. The method of claim 38, wherein the additive manufacturing process is a three-dimensional printing process, a stereolithography process, a direct write process, a fused deposition process, or a thermal or laser selective sintering process.

40. 13. An apparatus for thermal management of a heat generating component, said apparatus being fabricated by the method of claim 1.

41. 1. An apparatus for thermal management of a heat generating component, the apparatus comprising: A body comprising a ceramic matrix composite material, the material including a plurality of ceramic particles within a ceramic matrix, the body including two opposing surfaces, the ceramic particles having a platelet crystal structure aligned transversely and parallel to a thickness direction extending between the two opposing surfaces; and The method of claim 1, wherein the body is formed with at least one deformation to accommodate a surface feature of the part, and the parallel alignment of the platelet crystal structures matches at least one dimension of the at least one deformation.

42. 42. The device of claim 41, wherein the ceramic particles comprise hexagonal boron nitride, boron oxide, hexagonal aluminum nitride, aluminum oxide, molybdenum disulfide, clay, cesium oxide, graphene, flaky ferrite, calcium phosphate flakes, zirconia flakes, silica flakes, or combinations thereof.

43. 42. The device of claim 41, wherein the ceramic matrix comprises boron oxide, silicon dioxide, glass flake, silver coated glass flake, lithium oxide-silica mixture, magnesium oxide-silica mixture, or combinations thereof.

44. 42. The apparatus of claim 41, wherein the ceramic particle concentration in the ceramic matrix composite material of the body is about 30% to about 90% by weight, and the ceramic matrix concentration in the ceramic matrix composite material of the body is about 10% to about 70% by weight.

45. 42. The apparatus of claim 41, wherein the ceramic particles in the ceramic matrix composite of the body have a diameter of about 1 μm to about 100 μm, or about 5 μm to about 45 μm, and a thickness of about 3 to about 100 times less than the diameter.

46. 42. The device of claim 41, wherein the body has a thickness of about 0.05 mm to about 10 mm, or about 0.1 mm to 3 mm.

47. The device of claim 41 , wherein the ceramic particles comprise phononic crystal particles.

48. 42. The apparatus of claim 41, wherein the body has an in-plane thermal conductivity transverse to a thickness dimension that is greater than a through-plane thermal conductivity.

49. 42. The apparatus of claim 41, wherein the body has an in-plane thermal conductivity transverse to the thickness dimension of from about 5 W / mK to about 100 W / mK, or from about 10 W / mK to about 40 W / mK at ambient temperature.