Injectable polyhydroxy fatty acid ester microspheres and method for producing same

The production method for polyhydroxy fatty acid ester microspheres addresses aggregation and adhesion issues by using an organic solvent and hyaluronic acid aqueous phase, resulting in high-yield, dispersible, and injectable microspheres with biocompatibility and long-term filling effects.

JP2024537278AActive Publication Date: 2024-10-10BEIJING JOYINERA BIOMATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024521747
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-12
Filing Date
2022-09-27
Publication Date
2024-10-10
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

Conventional methods for producing polyhydroxy fatty acid ester microspheres for biodegradable fillers face issues with aggregation and adhesion, leading to difficulties in dispersibility and injectability, which can cause needle clogging and require frequent injections.

Method used

A method involving dissolving PHA material in an organic solvent to create an oil phase and hyaluronic acid in water to form an aqueous phase, followed by dropping the oil phase into the aqueous phase under stirring, then evaporating the solvent and drying to produce microspheres, which improves dispersibility and injectability.

Benefits of technology

The method achieves high yields of microspheres with excellent dispersibility, avoiding aggregation, and ensures easy injection without needle clogging, while maintaining biocompatibility and achieving long-term filling effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to the field of biomedicine technology, and specifically discloses injectable polyhydroxy fatty acid ester (PHA) microspheres and a method for preparing the same. The method for preparing the polyhydroxy fatty acid ester injectable microspheres includes: a) dissolving a PHA material in an organic solvent to obtain an oil phase; b) dissolving hyaluronic acid in water to obtain an aqueous phase; and c) dropping the oil phase into the aqueous phase under stirring conditions, and after the dropping is completed, continuing the stirring to volatilize the organic solvent, and then performing solid-liquid separation and drying to obtain PHA microspheres, and the order of steps a) and b) is not limited. The above method of the present invention can increase the dispersibility of PHA microspheres, and the obtained microspheres can be quickly dispersed in water, and the microspheres have a perfect shape, are independent of each other, and do not have agglomeration phenomenon, so that clogging of the needle tip can be avoided, and it is easy to inject them as a filler later. In addition, PHA microspheres have excellent biocompatibility and can achieve a long-term filling effect without causing rejection.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of biopharmaceutical technology, in particular to injectable polyhydroxy fatty acid ester microspheres and a method for preparing the same. [Background technology]

[0002] (CROSS REFERENCE TO RELATED APPLICATIONS) This invention claims priority to a Chinese patent application, application number 202111187296.9, entitled "Injectable polyhydroxy fatty acid ester microspheres and their manufacturing method", filed with the State Intellectual Property Office of China on October 12, 2021, the entire contents of which are incorporated herein by reference.

[0003] As humans age or are affected by certain diseases, the muscle and collagen tissues of the human body will undergo a certain degree of functional deterioration, causing problems such as skin depression and gastric reflux. Therefore, various fillers have been invented to fill the sunken skin and stimulate muscle and collagen regrowth through foreign bodies. However, the filling effect of these substances is only maintained for a short time as fillers, and they need to be injected frequently to maintain the filling effect. In order to achieve a long-term filling effect, attempts have been made to use non-biodegradable materials such as polyvinyl alcohol (PVA) and polymethyl methacrylate (PMMA) as fillers. Although the filling effect of these fillers can be maintained for an obvious longer time, if these materials remain in the body for too long, they will release harmful substances, which will cause a series of side reactions and harm the health of the human body.

[0004] In recent years, biodegradable polymer materials have come into people's sights. These materials are non-toxic to the human body and do not cause rejection reactions. They can be gradually decomposed and excreted from the body along with the human body's metabolism. By adjusting parameters such as the molecular weight of the materials, the decomposition time can be extended from one week to several years.

[0005] Polyhydroxy fatty acid esters, abbreviated as PHA, are natural polymeric biomaterials, intracellular polyesters synthesized from microorganisms. PHA is currently one of the most ideal biomedical materials because of its good biocompatibility and biodegradability. PHA has good cytocompatibility with cells in the body, cells can grow well on such stents, and such stents can be decomposed into CO2 and H2O. To facilitate injection, people usually make it into microspheres so that it can be injected through a needle. Due to the presence of human phagocytes, the diameter of the microspheres is usually 20 microns or more, but if the microspheres are too large, they may clog the needle tip or cause skin rupture. Therefore, the size of the microspheres used for injection is usually 60 microns or less.

[0006] Conventionally, when PHA materials are made into injectable microspheres, a polyvinyl alcohol (PVA) aqueous solution is usually used as the aqueous phase, and the microspheres are produced by the emulsification method or the microflow control method. However, the microspheres produced by such a process tend to aggregate and adhere to each other, and tend to become large lumps, which makes it difficult to inject the microspheres, and greatly hinders their application as fillers for biodegradable materials. Therefore, a new method for producing microspheres is urgently needed to solve the problem of aggregation and adhesion of microspheres. Summary of the Invention

[0007] Therefore, the object of the present invention is to provide a polyhydroxy fatty acid ester microsphere and a method for producing the same, which can effectively improve the dispersibility of the polyhydroxy fatty acid ester microsphere, overcome the problem of aggregation and adhesion of the microsphere, and effectively improve the absorbability and injectability of the polyhydroxy fatty acid ester microsphere.

[0008] The present invention provides a method for producing injectable polyhydroxy fatty acid ester microspheres, comprising the steps of: a) dissolving a PHA material in an organic solvent to obtain an oil phase; b) dissolving hyaluronic acid in water to obtain an aqueous phase; c) adding the oil phase dropwise to the aqueous phase under stirring conditions, and after the addition is completed, continuing the stirring to volatilize the organic solvent, and then performing solid-liquid separation and drying to obtain PHA microspheres; The steps a) and b) are not limited in order in the production method.

[0009] Preferably, the molecular weight of the hyaluronic acid is 5 to 500 KDa. Preferably, the mass concentration of hyaluronic acid in the aqueous phase is 0.01% to 1% (w / v). Preferably, in the step c), the volume ratio of the oil phase to the water phase is 1:(10 to 200). Preferably, in the oil phase, the mass concentration of the PHA material is 2.5% to 10% (w / v); The organic solvent is one or more selected from the group consisting of dichloromethane, chloroform, and ethyl acetate.

[0010] Preferably, the molecular weight of the PHA material is 10 to 100 KDa. Preferably, the PHA material is a natural or non-natural polyhydroxy fatty acid ester; The natural or unnatural polyhydroxy fatty acid esters include, but are not limited to, one or more of PHB, PHBV, PHBHHx, P34HB, PHBVHHx, PHHx, and PHO.

[0011] Preferably, the stirring speed is 100 to 500 rpm. Preferably, the stirring is performed by a magnetic stirrer; after the dropwise addition of the oil phase is completed, the stirring is continued for 4 hours or more. The present invention further provides injectable polyhydroxy fatty acid ester microspheres prepared by the preparation method described in the above technical solution.

[0012] In the manufacturing method of the present invention, PHA material is dissolved in an organic solvent to prepare an oil phase, and hyaluronic acid aqueous solution is used as the aqueous phase. The aqueous phase solution is stirred while the oil phase is gradually added to the aqueous phase, and the stirring is continued to volatilize the organic solvent, and then solid-liquid separation and drying are performed to produce PHA microspheres. The above method of the present invention can increase the dispersibility of PHA microspheres, and the obtained microspheres can be quickly dispersed in water, and the microspheres have a perfect shape, are independent of each other, and do not have agglomeration phenomenon, so that clogging of the needle tip can be avoided, and it is easy to inject them as a filler later. At the same time, the polyhydroxy fatty acid ester microspheres obtained by the present invention have excellent absorbability and injectability. And the PHA microspheres have excellent biocompatibility, and can achieve long-term filling effect without causing rejection.

[0013] Experimental results show that the manufacturing method provided by the present invention has the following beneficial effects: (1) High microsphere yield: The microsphere yield is 70% or more. (2) Good dispersibility: The PHA microspheres obtained by the present invention can be dispersed in water by proper mixing, and after standing, the microspheres show good dispersibility in water, do not exhibit layer separation phenomenon, do not float on the top layer of water, do not deposit on the bottom of water, and are uniformly dispersed in the water body to form a uniform dispersion. After air-drying the dispersion, the microspheres are observed to have a perfect shape, are independent of each other, have no aggregation phenomenon, and the particle size of all or most of the microsphere particles is 60 μm or less, which can meet the demand for injection. (3) Good suction property: When the dispersion is sucked into a syringe, the suction rate of the microspheres is 85% or more, showing excellent suction property. (4) Good injectability: The injected dispersion was collected by pressing the syringe, and the injection rate of the microspheres was calculated. The injection rate of the microspheres reached 88% or more, indicating excellent injectability. [Brief description of the drawings]

[0014] In the following, in order to more clearly explain the technical means in the embodiments of the present invention or the prior art, the drawings used in the following description of the embodiments or the prior art will be briefly described. However, the drawings in the following description are only embodiments of the present invention, and those skilled in the art can obtain other drawings based on the drawings provided without performing creative work.

[0015] [Figure 1] FIG. 1 is an optical microscope photograph of the injectable PHBHHx microspheres obtained in Example 1. [Diagram 2] FIG. 1 is a light microscope photograph of the injectable PHBVHHx microspheres obtained in Example 2. [Diagram 3] 1 is a light microscope photograph of the injectable PHB microspheres obtained in Example 3. [Figure 4] 1 is a light microscope photograph of the injectable PHBV microspheres obtained in Example 4. [Diagram 5] FIG. 1 is a light microscope photograph of the injectable P34HB microspheres obtained in Example 5. [Figure 6] FIG. 1 is a schematic diagram showing the dispersion stability of the microspheres obtained in Examples 1 to 5 and Comparative Examples 1 to 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention provides a method for producing injectable polyhydroxy fatty acid ester microspheres, comprising the steps of: a) dissolving a PHA material in an organic solvent to obtain an oil phase; b) dissolving hyaluronic acid in water to obtain an aqueous phase; c) adding the oil phase dropwise to the aqueous phase under stirring conditions, and after the addition is completed, continuing the stirring to volatilize the organic solvent, and then performing solid-liquid separation and drying to obtain PHA microspheres; The steps a) and b) are not limited in order in the production method.

[0017] In the manufacturing method of the present invention, PHA material is dissolved in an organic solvent to prepare an oil phase, and hyaluronic acid aqueous solution is used as the aqueous phase. The aqueous phase solution is stirred while the oil phase is gradually added to the aqueous phase, and the stirring is continued to volatilize the organic solvent, and then solid-liquid separation and drying are performed to produce PHA microspheres. The above method of the present invention can increase the dispersibility of PHA microspheres, and the obtained microspheres can be quickly dispersed in water, and the microspheres have a perfect shape, are independent of each other, and do not have agglomeration phenomenon, so that clogging of the needle tip can be avoided, and it is easy to inject them as a filler later. At the same time, the polyhydroxy fatty acid ester microspheres obtained by the present invention have excellent absorbability and injectability. And the PHA microspheres have excellent biocompatibility, and can achieve long-term filling effect without causing rejection.

[0018] Step a) Dissolving the PHA material in an organic solvent to obtain an oil phase In the present invention, the type of the PHA material, i.e., polyhydroxy fatty acid ester, is not particularly limited, and may be any of the fifth generation PHA commercial products commonly used in the art.Specifically, it is a natural or unnatural polyhydroxy fatty acid ester, more specifically, it is one or more of PHB (i.e., 3-hydroxybutyric acid ester), PHBV (i.e., copolymer of hydroxybutyric acid ester and hydroxyvaleric acid ester), PHBHHx (i.e., P3HB-co-3HHx, copolymer of 3-hydroxybutyric acid and 3-hydroxycaproic acid), P34HB (i.e., P3HB-co-4HB, copolymer of 3-hydroxybutyric acid and 4-hydroxybutyric acid), PHBVHHx (i.e., copolymer of 3-hydroxybutyric acid, 3-hydroxycaproic acid and 3-hydroxyvaleric acid), PHHx (i.e., polyhydroxycaproic acid ester) and PHO (i.e., polyhydroxycaprylic acid ester). In the present invention, the molecular weight of the PHA material is preferably 10-100 KDa. In some embodiments of the present invention, the molecular weight is 10-30 KDa, 20-100 KDa, or 10-100 KDa. The average molecular weight of the PHA material is preferably 15-80 KDa. In some embodiments of the present invention, the average molecular weight is 15 KDa, 40 KDa, 50 KDa, or 80 KDa.

[0019] In some embodiments of the present invention, the PHA material is PHBHHx, has a molecular weight of 20-100 KDa, and has a molecular weight average of 50 KDa. In other some embodiments of the present invention, the PHA material is PHBVHHx, has a molecular weight of 20-100 KDa, and has a molecular weight average of 50 KDa. In other some embodiments of the present invention, the PHA material is PHB, has a molecular weight of 20-100 KDa, and has a molecular weight average of 80 KDa. In other some embodiments of the present invention, the PHA material is PHBV, has a molecular weight of 20-100 KDa, and has a molecular weight average of 40 KDa. In other some embodiments of the present invention, the PHA material is P34HB, has a molecular weight of 10-30 KDa, and has a molecular weight average of 15 KDa.

[0020] In the present invention, the organic solvent is preferably one or more of dichloromethane, chloroform, and ethyl acetate. In the present invention, there is no particular limitation on the origin of the organic solvent, and it may be a commercially available product.

[0021] In the present invention, the mass concentration (w / v) of the organic solution obtained by dissolving the PHA material in an organic solvent is preferably 2.5% to 10%. In some embodiments of the present invention, the mass concentration is 2.5%, 5%, or 10%. In the present invention, the organic solution obtained by dissolving the PHA material in an organic solvent is used as an oil phase.

[0022] Step b) Dissolving hyaluronic acid in water to obtain an aqueous phase In the present invention, the molecular weight of the hyaluronic acid, i.e., HA, is preferably 5 to 500 KDa. In some embodiments of the present invention, the molecular weight is 5 to 100 KDa, 10 to 200 KDa, or 100 to 500 KDa. In the present invention, the average molecular weight of the hyaluronic acid is preferably 50 to 300 KDa. In some embodiments of the present invention, the average molecular weight is 50 KDa or 300 KDa.

[0023] In some embodiments of the present invention, the hyaluronic acid has a molecular weight of 5 to 100 KDa and an average molecular weight of 50 KDa. In some other embodiments of the present invention, the hyaluronic acid has a molecular weight of 10 to 200 KDa and an average molecular weight of 50 KDa. In some other embodiments of the present invention, the hyaluronic acid has a molecular weight of 100 to 500 KDa and an average molecular weight of 300 KDa.

[0024] In the present invention, the water is preferably distilled water or deionized water, and more preferably distilled water. In the present invention, the mass concentration (w / v) of the aqueous solution in which hyaluronic acid is dissolved in water is preferably 0.01% or more and 1% or less. In some embodiments of the present invention, the mass concentration is 0.5%, 5%, or 10%. In the present invention, the aqueous solution in which hyaluronic acid is dissolved in water is used as the aqueous phase. Conventionally, PHA microspheres have been produced using an aqueous solution of polyvinyl alcohol (PVA) as the aqueous phase, but the obtained PHA microspheres tend to aggregate and adhere in water, making it difficult to disperse them quickly. On the other hand, in the present invention, the use of an aqueous solution of hyaluronic acid as the aqueous phase improves the dispersibility of the PHA microspheres, and the obtained microspheres can be dispersed quickly in water, and the microspheres have a perfect shape, are independent of each other, and do not aggregate, so that clogging of the needle can be avoided and they can be easily injected as a filler later. At the same time, the polyhydroxy fatty acid ester microspheres obtained in the present invention have excellent absorbability and injectability. And, the PHA microspheres have excellent biocompatibility and can achieve a long-term filling effect without causing rejection. In the present invention, there is no restriction on the order of the above steps a) and b).

[0025] Step c) Dropping the oil phase into the aqueous phase under stirring conditions, and after the dropwise addition is completed, continuing the stirring to volatilize the organic solvent, and then performing solid-liquid separation and drying to obtain PHA microspheres. In the present invention, after the oil phase and the aqueous phase are obtained, the aqueous phase is stirred, and the oil phase is slowly dropped into the aqueous phase under this stirring condition. Here, the stirring is performed by a magnetic stirrer. The stirring speed is 100 to 500 rpm, and typically and non-limitingly, the stirring speed can be 100 rpm, 200 rpm, 300 rpm, 400 rpm, or 500 rpm. The volume ratio of the oil phase to the aqueous phase is preferably 1:(10 to 200). In some embodiments of the present invention, the volume ratio is 1:10, 1:20, 1:50, 1:100, 1:150, or 1:200.

[0026] After the oil phase is all dropped, the stirring process preferably includes first continuing stirring to form an emulsion, and then continuing stirring to volatilize the organic solvent. In the process of continuing stirring, the stirring is performed by a magnetic stirrer, and the stirring speed is 100 to 500 rpm, and in some embodiments of the present invention, the stirring speed is 400 rpm. In the process of continuing stirring, the stirring is performed by a magnetic stirrer, and the stirring speed is 100 to 500 rpm, and typically and non-limitingly, the stirring speed can be 100 rpm, 200 rpm, 300 rpm, 400 rpm, or 500 rpm. The time for which the stirring is continued is preferably 4 hours or more, and more preferably 4 to 6 hours. In some embodiments of the present invention, the time for which the stirring is continued (to volatilize the organic solvent) after forming the emulsion is 4 hours, 5 hours, or 6 hours. In the present invention, there is no particular limitation on the temperature at which the oil phase is dropped and stirred, and the temperature may be room temperature, specifically 10 to 37°C, and preferably 25°C.

[0027] Stirring is continued until the solvent is completely evaporated, and then solid-liquid separation is carried out. In the present invention, there is no particular limitation on the method of solid-liquid separation, and any conventional method well known to those skilled in the art, such as filtration, may be used. After the solid-liquid separation, the water is removed by drying. In the present invention, the drying is preferably performed by first freezing and then lyophilization. In the present invention, the drying temperature is -80 to -20°C; the freezing temperature is preferably -80 to -20°C, and the lyophilization temperature is preferably -60 to -40°C. In some embodiments of the present invention, the freezing temperature is preferably -80 to -40°C and the time is preferably 6 to 12 hours; and the lyophilization temperature is preferably -40°C and the time is 24 hours. After the above drying process, PHA microspheres are obtained.

[0028] The present invention further provides PHA microspheres prepared by the preparation method described in the above technical solution. In the manufacturing method of the present invention, PHA material is dissolved in an organic solvent to prepare an oil phase, and hyaluronic acid aqueous solution is used as the aqueous phase. The aqueous phase solution is stirred while the oil phase is gradually added to the aqueous phase, and the stirring is continued to volatilize the organic solvent, and then solid-liquid separation and drying are performed to produce PHA microspheres. The above method of the present invention can increase the dispersibility of PHA microspheres, and the obtained microspheres can be quickly dispersed in water, and the microspheres have a perfect shape, are independent of each other, and do not have agglomeration phenomenon, so that clogging of the needle tip can be avoided, and it is easy to inject them as a filler later. At the same time, the polyhydroxy fatty acid ester microspheres obtained by the present invention have excellent absorbability and injectability. And the PHA microspheres have excellent biocompatibility, and can achieve long-term filling effect without causing rejection.

[0029] As a result of the experiment, the following was found: (1) The production method provided by the present invention has a microsphere yield of 70% or more. The PHA microspheres obtained by the present invention can be dispersed in water by proper mixing, and after standing, the microspheres show good dispersibility in water, do not exhibit layer separation, do not float on the top layer of water, do not deposit on the bottom of water, and are uniformly dispersed in the water body to form a uniform dispersion. After air-drying the dispersion, the microspheres are observed to have a perfect shape, are independent of each other, have no aggregation phenomenon, and the particle size of all or most of the microsphere particles is 60 μm or less, which can meet the requirements for injection. (2) A disposable 1 mL syringe was fitted with a needle with an inner diameter of 0.5 mm and a length of 19.7 mm (i.e., the needle of a regular 1 mL syringe) to serve as the aspiration rate detection device, and 1 mL of microsphere dispersion (microsphere dry weight 0.1 g, designated M0) was used as the experimental sample. All of the microsphere dispersion was aspirated at once, and the microspheres that could be aspirated into the syringe tube were taken out and freeze-dried, with the mass being M1, and the aspiration rate was defined as [M1 / M0] x 100%. When the above microsphere dispersion was aspirated with the above syringe, the aspiration rate of the microspheres was 85% or more, indicating excellent aspiration properties. (3) A disposable 1 mL syringe was equipped with a needle with an inner diameter of 0.5 mm and a length of 19.7 mm (i.e., the needle of a conventional 1 mL syringe) to serve as the aspiration rate detection device, and 1 mL of microsphere dispersion (microsphere dry weight 0.1 g, designated as M0) was used as the experimental sample. 1 mL of the microsphere dispersion was injected into the syringe tube from the rear of the syringe, and all of the microsphere dispersion was injected at once. The microspheres that could be injected outside the syringe tube through the needle were collected and freeze-dried, and the mass was designated as M2, and the injection rate was defined as (M2 / M0) × 100%. The injected dispersion was collected by pressing the syringe, and the injection rate of the microspheres was calculated. As a result, the injection rate of the microspheres reached 88% or more, demonstrating excellent injectability.

[0030] In order to better understand the present invention, preferred embodiments of the present invention will be described below based on examples. However, it should be understood that these descriptions are intended to further illustrate the features and advantages of the present invention and are not intended to limit the scope of the claims of the present invention.

[0031] Example 1 1 g of PHBHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 5-100 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of both solutions was 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at -80°C for 6 hours) and then freeze-dried (freeze-dried at -40°C for 24 hours) to remove water, and injectable PHBHHx microspheres were obtained.

[0032] From the amount of PHBHHx material added and the amount of PHBHHx microspheres obtained, the yield of injectable PHBHHx microspheres was calculated to be 93%. The PHBHHx microspheres after freeze-drying treatment can be dispersed in water by dissolving them in water and mixing them appropriately. After air-drying the water, they were observed under an optical microscope, and the results are shown in Figure 1, which is an optical microscope image of the injectable PHBHHx microspheres obtained in Example 1. It was found that the microspheres obtained have good dispersibility and are spherical or elliptical. The particle size was detected by a particle sizer to be 1 to 50 μm.

[0033] Example 2 1 g of PHBVHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 10-200 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 4 hours. The resulting solution was then first frozen (frozen at -40 °C for 12 hours) and then freeze-dried (freeze-dried at -40 °C for 24 hours) to remove water, and injectable PHBVHHx microspheres were obtained.

[0034] The yield of the obtained injectable PHBVHHx microspheres is 91%. The PHBVHHx microspheres after freeze-drying can be dispersed in water by dissolving in water and mixing appropriately. After air-drying, the microspheres are observed under an optical microscope, and the results are shown in FIG. 2, which is an optical microscope image of the injectable PHBVHHx microspheres obtained in Example 2. It can be seen that the obtained microspheres have good dispersibility and are spherical or elliptical. The particle size is 4 to 50 μm as detected by a particle sizer.

[0035] Example 3 1 g of PHB (molecular weight 20-100 KDa, average molecular weight 80 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 100-500 KDa, average molecular weight 300 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by continuing to stir at this speed for 6 hours. The resulting solution was then first frozen (frozen at -40°C for 12 hours) and then freeze-dried (freeze-dried at -40°C for 24 hours) to remove water, and injectable PHB microspheres were obtained.

[0036] The yield of the obtained injectable PHB microspheres is 92%. The freeze-dried PHB microspheres can be dispersed in water by dissolving them in water and mixing them appropriately. After air-drying, the microspheres are observed under an optical microscope. The results are shown in FIG. 3, which is an optical microscope image of the injectable PHB microspheres obtained in Example 3. It can be seen that the microspheres obtained have good dispersibility and are spherical or elliptical. The particle size is 2 to 55 μm as detected by a particle sizer.

[0037] Example 4 1 g of PHBV (molecular weight 20-100 KDa, average molecular weight 40 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 5-100 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at -40°C for 12 hours) and then freeze-dried (freeze-dried at -40°C for 24 hours) to remove water, and injectable PHBV microspheres were obtained.

[0038] The yield of the obtained injectable PHBV microspheres is 90%. The PHBV microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing them appropriately. After air-drying, the microspheres are observed under an optical microscope, and the results are shown in FIG. 4, which is an optical microscope image of the injectable PHBV microspheres obtained in Example 4. It can be seen that the obtained microspheres have good dispersibility and are spherical or elliptical. The particle size is 1 to 52 μm as detected by a particle sizer.

[0039] Example 5 1 g of P34HB (molecular weight 10-30 KDa, average molecular weight 15 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 5-100 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by continuing to stir at this speed for 5 hours. The resulting solution was then first frozen (frozen at -40°C for 12 hours) and then freeze-dried (freeze-dried at -40°C for 24 hours) to remove water, and injectable P34HB microspheres were obtained.

[0040] The yield of the obtained injectable P34HB microspheres is 90%. The P34HB microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing appropriately. After air-drying, the microspheres are observed under an optical microscope, and the results are shown in FIG. 5. FIG. 5 is an optical microscope image of the injectable P34HB microspheres obtained in Example 5, and it can be seen that the obtained microspheres have good dispersibility and are spherical or elliptical. The particle size of the microspheres detected by a particle sizer is 5-100 μm, of which 68% have a particle size of 1-60 μm, that is, the particle size of the majority of the particles is 60 μm or less.

[0041] Example 6: Different oil phase concentrations 0.5g, 1g, and 2g of PHBHHx (molecular weight 20-100KDa, average molecular weight 50KDa) were dissolved in 20mL of dichloromethane to prepare organic solutions with final concentrations of 2.5% (w / v), 5% (w / v), and 10% (w / v), which were used as the oil phase. Hyaluronic acid (molecular weight 5-100KDa, average molecular weight 50KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at −80°C for 6 h) and then lyophilized (lyophilized at −40°C for 24 h) to remove water, resulting in injectable PHBHHx microspheres.

[0042] The yields of the obtained injectable PHBHHx microspheres are 90%, 93%, and 89%, respectively. The PHBHHx microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing appropriately. After air-drying, the microspheres were observed under an optical microscope, and the microspheres obtained were found to have good dispersibility and to be spherical or elliptical. The particle sizes detected by a particle sizer were 0.4-20 μm, 1-50 μm, and 1-80 μm, respectively (83% of the particles had a particle size of 1-60 μm).

[0043] Example 7: Different volume ratios of oil and water phases 1 g of PHBHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 5-100 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of both solutions was 1:10, 1:50, and 1:200, respectively. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; further stirring was continued for 5 hours at this speed to remove the organic solvent. The resulting solution was then first frozen (frozen at −80°C for 6 h) and then lyophilized (lyophilized at −40°C for 24 h) to remove water, resulting in injectable PHBHHx microspheres.

[0044] The yields of the obtained injectable PHBHHx microspheres are 71%, 93%, and 94%, respectively. The PHBHHx microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing appropriately. After air-drying, the microspheres obtained were observed under an optical microscope, and the results showed that the microspheres had good dispersibility and were spherical or elliptical. The particle size was detected by a particle sizer and found to be 1-110 μm (58% of the particles have a particle size of 1-60 μm), 1-50 μm, and 1-50 μm, respectively.

[0045] Example 8: Different stirring methods and rotation speeds 1 g of PHBHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 5-100 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of both solutions was 1:50. Stirring was continued with a magnetic stirrer (rotation speeds of 100 rpm, 400 rpm, and 500 rpm, respectively) and a high-speed homogenizer (rotation speed of 12,000 rpm), respectively, until an emulsion was formed; the organic solvent was removed by further stirring for 5 hours. The resulting solution was then first frozen (frozen at −80°C for 6 h) and then lyophilized (lyophilized at −40°C for 24 h) to remove water, resulting in injectable PHBHHx microspheres.

[0046] The yields of the obtained injectable PHBHHx microspheres are 77%, 93%, 89%, and 99%, respectively. The PHBHHx microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing appropriately. After air-drying the water, the microspheres were observed under an optical microscope, and the microspheres obtained were found to have good dispersibility and to be spherical or elliptical. The particle size was detected by a particle sizer and found to be 5-60 μm, 1-50 μm, 1-45 μm, and 0.1-10 μm (the particle size of the particles is basically 10 μm or less, only 5% of the particles have a particle size of 1-60 μm, and the overall particle size distribution is at the level of 0.1-10 μm). This proves that, compared with the high-speed homogenization stirring method, the use of a magnetic stirrer to stir at an appropriate speed (100-500 rpm) in the present invention is advantageous in obtaining a particle size of microspheres that is more suitable for the human body. Example 9: Different types of oil phase organic solvent

[0047] 1 g of PHBHHx (molecular weight 10-20 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane, chloroform, and ethyl acetate to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 5-100 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at −80°C for 6 h) and then lyophilized (lyophilized at −40°C for 24 h) to remove water, resulting in injectable PHBHHx microspheres.

[0048] The yields of the obtained injectable PHBHHx microspheres are 93%, 92%, and 89%, respectively. The PHBHHx microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing appropriately. After air-drying, the microspheres were observed under an optical microscope, and the microspheres obtained were found to have good dispersibility and to be spherical or elliptical. The particle sizes detected by a particle sizer were 1-52 μm, 1-50 μm, and 1-55 μm, respectively.

[0049] Example 10: Different aqueous phase concentrations 1 g of PHBHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Hyaluronic acid (molecular weight 10-200 KDa, average molecular weight 50 KDa) was dissolved in distilled water to prepare aqueous solutions with final concentrations of 0.01% (w / v), 0.5% (w / v), and 1% (w / v), which were used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at −80°C for 6 h) and then lyophilized (lyophilized at −40°C for 24 h) to remove water, resulting in injectable PHBHHx microspheres.

[0050] The yields of the obtained injectable PHBHHx microspheres are 80%, 93%, and 87%, respectively. The PHBHHx microspheres after freeze-drying can be dispersed in water by dissolving them in water and mixing appropriately. After air-drying, the microspheres were observed under an optical microscope, and the microspheres obtained were found to have good dispersibility and to be spherical or elliptical. The particle sizes detected by a particle sizer were 3-50 μm, 1-50 μm, and 0.7-50 μm, respectively.

[0051] Comparative Example 1 1 g of PHBHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Polyvinyl alcohol (PVA) with an alcohol decomposition degree of 80% was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at -80 °C for 6 hours) and then freeze-dried (freeze-dried at -40 °C for 24 hours) to remove water, and PHBHHx microspheres were obtained.

[0052] Comparative Example 2 1 g of PHBVHHx (molecular weight 20-100 KDa, average molecular weight 50 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Polyvinyl alcohol (PVA) with an alcohol decomposition degree of 80% was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at -80 °C for 6 hours) and then freeze-dried (freeze-dried at -40 °C for 24 hours) to remove water, and PHBVHHx microspheres were obtained.

[0053] Comparative Example 3 1 g of PHB (molecular weight 20-100 KDa, average molecular weight 80 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Polyvinyl alcohol (PVA) with an alcohol decomposition degree of 80% was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by continuing to stir at this speed for 5 hours. The resulting solution was then first frozen (frozen at -80 °C for 6 hours) and then freeze-dried (freeze-dried at -40 °C for 24 hours) to remove water, and PHB microspheres were obtained.

[0054] Comparative Example 4 1 g of PHBV (molecular weight 20-100 KDa, average molecular weight 40 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Polyvinyl alcohol (PVA) with an alcohol decomposition degree of 80% was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by further stirring at this speed for 5 hours. The resulting solution was then first frozen (frozen at -80°C for 6 hours) and then freeze-dried (freeze-dried at -40°C for 24 hours) to remove water, and injectable PHBV microspheres were obtained.

[0055] Comparative Example 5 1 g of P34HB (molecular weight 10-30 KDa, average molecular weight 15 KDa) was dissolved in 20 mL of dichloromethane to prepare an organic solution with a final concentration of 5% (w / v), which was used as the oil phase. Polyvinyl alcohol (PVA) with an alcohol decomposition degree of 80% was dissolved in distilled water to prepare an aqueous solution with a final concentration of 0.5% (w / v), which was used as the aqueous phase. While stirring the aqueous phase at a speed of 400 rpm with a magnetic stirrer, the oil phase was slowly dropped into the aqueous phase under stirring, and the volume ratio of the two solutions was set to 1:50. Stirring was continued at a speed of 400 rpm with a magnetic stirrer to form an emulsion; the organic solvent was removed by continuing to stir at this speed for 5 hours. The resulting solution was then first frozen (frozen at -80°C for 6 hours) and then freeze-dried (freeze-dried at -40°C for 24 hours) to remove water, and P34HB microspheres were obtained.

[0056] Example 11: Measurement of Microsphere Stability 0.01 g of each of the microspheres produced in Examples 1 to 5 and Comparative Examples 1 to 5 was collected, dispersed in 1 mL of distilled water, and placed in a 5 mL glass bottle. The mixture was quickly mixed and then allowed to stand.

[0057] After leaving it for 30 minutes, the dispersion state of each microsphere in water was observed. As a result, as shown in FIG. 6, FIG. 6 is a diagram showing the dispersion stability of the microspheres obtained in Examples 1 to 5 and Comparative Examples 1 to 5 (the 10 containers from left to right correspond to the samples of Examples 1 to 5 and Comparative Examples 1 to 5, respectively). It was found that the PHBHHx microspheres, PHBVHHx microspheres, PHB microspheres, PHBV microspheres and P34HB microspheres in Examples 1 to 5 all had good dispersibility, no layer separation phenomenon was observed, and the microspheres were uniformly dispersed in the water body. The PHBHHx microspheres, PHBVHHx microspheres, PHB microspheres, PHBV microspheres and P34HB microspheres in Comparative Examples 1 to 5 did not have water dispersibility, and all of them exhibited serious layer separation phenomenon, and the microspheres were floating on the upper layer of the water. This proves that in the present invention, the use of an aqueous hyaluronic acid solution as the aqueous phase material significantly improves the dispersibility and stability of the microspheres compared to the use of an aqueous polyvinyl alcohol solution.

[0058] Example 12: Measurement of the attractiveness of microspheres A disposable 1 mL syringe was equipped with a needle with an inner diameter of 0.5 mm and a length of 19.7 mm (i.e., the needle of a conventional 1 mL syringe) to serve as an injection rate detection device, and 1 mL of microsphere dispersion (microsphere dry weight 0.1 g, denoted as M0) was used as an experimental sample. 0.1 g of the microspheres produced in Examples 1 to 5 and Comparative Examples 1 to 5 were each collected, dispersed in 1 mL of distilled water, and placed in a glass bottle. After rapid mixing, a microsphere dispersion was formed. 1 mL of the dispersion was aspirated into the syringe, and the microspheres aspirated into the syringe were each freeze-dried. The ratio of the mass of the microspheres aspirated into the syringe (M1) to the mass of the total microspheres (M0) was defined as the microsphere aspiration rate (M1 / M0) x 100%.

[0059] As a result, the suction rates of PHBHHx microspheres, PHBVHHx microspheres, PHB microspheres, PHBV microspheres and P34HB microspheres in Examples 1 to 5 are 95%, 93%, 91%, 90% and 85%, respectively. The suction rates of PHBHHx microspheres, PHBVHHx microspheres, PHB microspheres, PHBV microspheres and P34HB microspheres in Comparative Examples 1 to 5 are 10%, 13%, 11%, 9% and 6%, respectively. This shows that the suction rates of the microballs in Examples 1 to 5 are much higher than those in Comparative Examples 1 to 5. This proves that in the present invention, the suction property of the microspheres is significantly improved when a hyaluronic acid aqueous solution is used as the aqueous phase material, rather than when a polyvinyl alcohol aqueous solution is used.

[0060] Example 13: Determination of the injectability of microspheres A disposable 1 mL syringe was equipped with a needle with an inner diameter of 0.5 mm and a length of 19.7 mm (i.e., a needle of a conventional 1 mL syringe) to serve as an injection rate detection device, and 1 mL of microsphere dispersion (microsphere dry weight 0.1 g, designated as M0) was used as the experimental sample. 0.1 g of the microspheres prepared in Examples 1 to 5 and Comparative Examples 1 to 5 was collected, dispersed in 1 mL of distilled water, and placed in a glass bottle. After rapid mixing, a microsphere dispersion was formed. The dispersion was completely injected into 1 mL of the syringe, and the injected dispersion was collected by pressing the syringe, and the microsphere mass (M2) of the injected dispersion was freeze-dried, and the percentage of the total microsphere mass (M0) was calculated, which was defined as the microsphere injection rate (M2 / M0) x 100%.

[0061] As a result, the injection rates of PHBHHx microspheres, PHBVHHx microspheres, PHB microspheres, PHBV microspheres and P34HB microspheres in Examples 1 to 5 are 91%, 92%, 90%, 90% and 88%, respectively. The injection rates of PHBHHx microspheres, PHBVHHx microspheres, PHB microspheres, PHBV microspheres and P34HB microspheres in Comparative Examples 1 to 5 are 7%, 11%, 13%, 8% and 4%, respectively. This shows that the injection rates of the microspheres in Examples 1 to 5 are much higher than those in Comparative Examples 1 to 5. This proves that in the present invention, the injection property of the microspheres is significantly improved when a hyaluronic acid aqueous solution is used as the aqueous phase material, rather than when a polyvinyl alcohol aqueous solution is used.

[0062] From the above experimental results, it is found that the manufacturing method provided by the present invention has the following beneficial effects: (1) High microsphere yield: The microsphere yield is 70% or more. (2) Good dispersibility: The PHA microspheres obtained by the present invention can be dispersed in water by proper mixing, and after standing, the microspheres show good dispersibility in water, do not exhibit layer separation phenomenon, do not float on the top layer of the water, do not deposit on the bottom of the water, and are uniformly dispersed in the water body to form a uniform dispersion. After air-drying the dispersion, the microspheres are observed to have a perfect shape, are independent of each other, have no aggregation phenomenon, and the particle diameter of all or most of the microsphere particles is 60 μm or less, which can meet the demand for injection. (3) Good suction property: When the dispersion is sucked into a syringe, the suction rate of the microspheres is 85% or more, showing excellent suction property. (4) Good injectability: The injected dispersion was collected by pressing the syringe and the injection rate of the microspheres was calculated. The injection rate of the microspheres reached 88% or more, indicating excellent injectability.

[0063] The principles and embodiments of the present invention have been described above using specific examples. However, the description of the above examples is merely intended to aid in the understanding of the method of the present invention and its core ideas, and includes the best mode, as well as the method of manufacturing and using any device or system and performing any combination. It should be noted that those skilled in the art may make some improvements and modifications to the present invention without departing from the principles of the present invention, and these improvements and modifications are also included in the scope of protection of the claims of the present invention. The scope of protection of the present invention is indicated by the claims and may include other examples that may come to mind by those skilled in the art. It is clear that various modifications or alterations may be made within the scope of the claims, provided that these other embodiments are similar to the components described in the claims or include equivalent components that are not substantially different from the wording of the claims, and it is understood that these also belong to the technical scope of the present invention.

Claims

1. 1. A method for producing polyhydroxy fatty acid ester (PHA) microspheres, comprising: a) dissolving a PHA material in an organic solvent to obtain an oil phase; b) dissolving hyaluronic acid in water to obtain an aqueous phase; c) adding the oil phase to the aqueous phase under stirring conditions, and after the addition is completed, continuing the stirring to volatilize the organic solvent, and then performing solid-liquid separation and drying to obtain PHA microspheres; Including, The steps a) and b) are not limited in order, wherein the molecular weight of the PHA material is 10-100 KDa; In the oil phase, the mass concentration of the PHA material is 2.5% to 10%, The molecular weight of the hyaluronic acid is 5 to 500 KDa; In the aqueous phase, the mass concentration of hyaluronic acid is 0.01% to 1%. A manufacturing method comprising:

2. In the step c), the volume ratio of the oil phase to the aqueous phase is 1:(10 to 200); The method according to claim 1 .

3. The organic solvent is one or more selected from the group consisting of dichloromethane, chloroform, and ethyl acetate. The method according to claim 1 .

4. The average molecular weight of the PHA material is 15 to 80 KDa; The method according to claim 1 .

5. the PHA material is PHBHHx, has a molecular weight of 20-100 KDa, and has an average molecular weight of 50 KDa; or the PHA material is PHBVHHx, has a molecular weight of 20-100 KDa, and has an average molecular weight of 50 KDa; or the PHA material is PHB, has a molecular weight of 20-100 KDa, and has an average molecular weight of 80 KDa; or the PHA material is PHBV and has a molecular weight of 20-100 KDa and an average molecular weight of 40 KDa; or The PHA material is P34HB, has a molecular weight of 10-30 KDa, and has a molecular weight average of 15 KDa; The method according to claim 1 .

6. The average molecular weight of the hyaluronic acid is 50 to 300 KDa. The method according to claim 1 .

7. The hyaluronic acid has a molecular weight of 5 to 100 KDa and an average molecular weight of 50 KDa; or The hyaluronic acid has a molecular weight of 10 to 200 KDa and an average molecular weight of 50 KDa, or The hyaluronic acid has a molecular weight of 100 to 500 KDa and an average molecular weight of 300 KDa. The method according to claim 1 .

8. The stirring speed is 100 to 500 rpm; The method according to claim 1 .

9. The stirring is performed by a magnetic stirrer; After the dropwise addition of the oil phase is completed, the stirring is continued for 4 hours or more. The method according to claim 1 .

10. After the dropwise addition of the oil phase is completed, the stirring is continued for 4 to 6 hours. The method according to claim 9 .

11. The stirring temperature is 10 to 37°C. The method according to claim 1 .

12. The drying is performed by first freezing and then freeze-drying; The freezing temperature is −80 to −20° C., and the freeze-drying temperature is −60 to −40° C.; The method according to claim 1 .

13. Polyhydroxy fatty acid ester microspheres produced by the method according to any one of claims 1 to 12.

14. The particle size of the polyhydroxy fatty acid ester microspheres is 60 μm or less, and / or The polyhydroxy fatty acid ester microspheres have an absorption rate of 85% or more, and / or The injectability of the polyhydroxy fatty acid ester microspheres is 88% or more; The polyhydroxy fatty acid ester microsphere according to claim 13 .

Citation Information

Patent Citations

  • Nanocapsules with a polymer shell

    EP2664324A1

  • Slowly releasing fine particle agent and production thereof

    JP1989156912A

  • Sustained release preparation

    JP1992235926A

  • Dispersion composition and method for producing dispersion composition

    JP2010222293A

  • Microparticles and nanoparticles having negative surface charges

    US20160310426A1