MXene compounds having novel crystal forms and a process for producing MAX phase type compounds for synthesizing said MXene compounds

A two-step chemical attack and spark plasma sintering process on MAX phase precursors produces MXene compounds with uniform size distribution and improved interconnectivity, addressing the limitations of existing MXene production methods.

JP2024537923AActive Publication Date: 2024-10-16AISIN CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024543594
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-10-04
Publication Date
2024-10-16
Estimated Expiration
2042-10-04

AI Technical Summary

Technical Problem

Existing MXene compounds exhibit significant dispersion in particle shape and size, limiting interconnectivity and insertion rates during crystal assembly, and achieving uniform particle size distribution is challenging.

Method used

The production of MXene compounds involves a two-step chemical attack process on MAX phase precursors, combined with spark plasma sintering to create porous pellets with defined crystal shapes and sizes, ensuring a uniform size distribution and improved interconnectivity.

Benefits of technology

This method results in MXene compounds with a uniform particle size distribution and enhanced interconnectivity, facilitating better insertion rates and assembly of thin sheets with controlled morphology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537923000001_ABST
    Figure 2024537923000001_ABST
Patent Text Reader

Abstract

The present invention provides a process for producing MXene compounds having a novel crystalline morphology and a MAX phase type compound for synthesizing said MXene compounds. The present invention relates firstly to an MXene compound having the advantage of having a predominantly plate-like crystalline morphology, which can be obtained from a MAX phase precursor obtained by a spark plasma sintering process of insulating powder mixtures, and a process for producing said MXene compounds. The present invention also relates to a MAX phase type compound obtained by a spark plasma sintering process of insulating powder mixtures. The present invention also relates to a process for synthesizing MXene compounds from said precursors, and to an MXene compound obtained by this process having the advantage of having a predominantly plate-like crystalline morphology.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to lamellar MXene compounds synthesized from precursors referred to as MAX phases.

[0002] The present invention relates to a process for producing MAX phase type compounds, MAX phase type compounds obtained by said process, an apparatus for carrying out said process, as well as a novel type of MXene compound and related manufacturing process thereof. [Background technology]

[0003] The MXene compound was discovered in 2011 (Non-Patent Document 1). This compound is n+1 X n wherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, and X is C or N; alternatively, M n+1 X n T x where T corresponds to a terminal group selected from O, OH, F or any other halogen group, and S or any other chalcogen group. This compound is described and characterized in US Pat. No. 5,399,433.

[0004] MXenes are lamellar compounds, i.e., two-dimensional materials (2D), that can be exfoliated to form single sheets with a thickness of about 1 nm, with repeat units having the structures MXM, MXMXM, or MXMXMX, where n is 1, 2, or 3, respectively.

[0005] These materials have many applications, especially due to their lamellar structure, electrical conductivity and / or propensity to insert and desorb species in the interlayer space. The MXene that has been most studied for this purpose is Ti3C2T x It has the formula:

[0006] While most of the literature focuses on MXene after delamination, some papers, including Non-Patent Document 2, have used scanning electron microscope images (SEM) to reveal the shape of MXene particles before delamination. These particles are bulk particles with no well-defined geometric shape. They also show a wide dispersion in both size and shape. The structure of these particles may lead to limited conductive properties and may also limit the intercalation rate of other species within the crystals. For example, it can be assumed that there is low interconnectivity between the crystals when assembled to make thin layers useful for various applications. Also, due to the large dispersion in particle size and shape, thin sheets with uniform size distribution after delamination cannot be easily obtained (useful for some applications), and therefore additional size selection operations are required.

[0007] In known methods, these MXene compounds are synthesized from precursors commonly referred to as "MAX phase type compounds" or "MAX phase compounds". These MAX phase compounds are n+1 AX n where n is 1, 2 or 3, M and X are the same as for MXene, and A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb. MAX phase compounds have a similar structure to MXene, but with the addition of M n+1 X n They further comprise the element A, which is present in the form of layers between the repeating units. To produce MXenes, the element A is chemically removed from the MAX phase type precursor. In most cases, MAX phase precursors in which A is aluminum are preferred, and a related method consists of chemically attacking the MAX precursor with an aqueous acid solution containing hydrofluoric acid. This results in the formation of M n+1 X n Aluminum is removed from the space between the repeat units, forming the terminal group T xIn most cases, T is -F, -OH or =O and is bonded to the element M located on the outside of the repeat unit. The MAX precursor is pre-milled to ensure a good yield of the chemical attack. After the chemical attack, the product is washed and centrifuged several times to remove excess reagents used in the attack and soluble by-products such as AlF3. If the aim is to obtain single sheets (2D) of MXene instead of three-dimensional particles, an additional delamination step may be performed. One variant of the attack process with a hydrofluoric acid solution is to use a mixed solution of a fluoride salt, typically Li, and a strong acid, typically HCl, as described in the above-mentioned non-patent document 2.

[0008] Regarding the synthesis of MAX phase precursors, the most widespread process for producing MXene, especially of the formula Ti3AlC2, is to mix a mixture of carbide or nitride powder of metal M (such as MC or MN), metal A (such as Al), and metal M in a tube furnace under a flow of inert gas. n+1 AX n The main goal is to provide the elements in the amounts necessary to reach the stoichiometric amount. In the particular case of Ti3AlC2, the reaction mixture is composed of TiC, Al and Ti powders. The aluminum in the starting mixture may be in slight excess of the stoichiometry. Mixing of the three elements (e.g. Ti, Al and C) is usually avoided because the reaction is highly exothermic and there is a risk of explosion. The use of a tube furnace under a flow of inert gas requires several hours of heating up to temperatures on the order of 1300°C to 1500°C, as well as several hours at the maximum temperature. There are other synthesis processes, some of which rely on higher pressures and / or more difficult to control conditions and / or use other reaction mixtures.

[0009] Although prior to the first synthesis of MXene, in Non-Patent Document 3 the authors synthesized a MAX phase precursor by spark plasma sintering (SPS) using a mixture of TiC, Ti, Al and about 20% Si relative to Al. The mixture was fed into a graphite sample holder, typical of an SPS apparatus, and a product was obtained in the form of a very compact pellet with no porosity. This lack of porosity makes the synthesis of MXene from the abovementioned MAX phase precursor difficult and takes a long time, since in the prior art, for a reasonable synthesis rate of the MXene compound, the MAX precursor needs to have a powder morphology of sub-millimeter size, and this powder is difficult to obtain from a compact pellet. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2021 / 177712 [Non-patent literature]

[0011] [Non-Patent Document 1] Naguib et al. Adv. Master. 23, 4248, 2011 [Non-Patent Document 2] Alhabeb et al. Chem. Mater. 29, 7633, 2017 [Non-Patent Document 3] Zhou et al., J. Mater. Scie. 40, 2099, 2005 Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention therefore aims to produce MXene compounds with a smaller dispersion in particle shape and size than in the prior art, which makes it possible, in particular, to increase the rate of seed insertion within each crystal and to ensure better interconnectivity between these crystals during the assembly of the crystal layers, as well as to obtain, via delamination, sheets with a more uniform particle size distribution than those reported in the prior art.

[0013] The present invention also relates to the preparation of MAX phase precursors and associated manufacturing processes which ensure in particular the obtaining of the above-mentioned MXene compounds. [Means for solving the problem]

[0014] To this end, the present invention provides n+1 X n T x where n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, X is C or N and T corresponds to an end group selected from O, OH, F or any other halogen group, and S or any other chalcogen group, characterized in that the majority are in the form of crystals having a general plate shape, the plate having two opposing parallel surfaces of a defined length L separated by a defined height H, and The length of the plate-shaped crystal is 1 μm to 15 μm; The height H of the plate-shaped crystal is 0.2 μm to 1 μm, and The compound is characterized in that the flattened aspect ratio of the plate-shaped crystal, defined by the ratio of the length L to the height H, is 5 to 50.

[0015] The compounds of the invention may also comprise any of the following features, taken individually or according to all possible technical combinations: Ti3C2T x It has the formula: M n+1 AX nwherein n is 1, 2 or 3; M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta; A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb; and X is C or N; in the form of pellets having a porosity of more than 30%, preferably more than 40%, and having a stoichiometric element ratio M / X within a relative error of less than ±0.5%; It is obtained from a MAX phase type precursor compound. The MAX phase type precursor compound has the formula Ti3AlC2. Most of the above MAX phase type precursor compounds have morphologies exhibiting the following two types of grain cross sections. a rectangular flat cross-section having a length of 1 μm to 20 μm and a height of 0.5 μm to 2 μm, and / or Rounded corners and flat cross section with diagonal length of 1μm to 20μm.

[0016] The present invention also relates to the above-mentioned M n+1 X n T x The present invention relates to a process for producing a compound having the general formula:

[0017] Furthermore, the present invention relates to the above-mentioned M n+1 X n T x 2. A process for producing a compound of the general formula: mixing the precursor powders; placing the powder mixed in the above step into a closed container made of insulating ceramic material housed in the hollow chamber; performing a spark plasma sintering operation; obtaining pellets of said MAX phase type compound; The present invention relates to a process comprising at least

[0018] The process of the invention may also include any of the following features, considered individually or according to all possible technical combinations: The container is alumina-based. The powder is not in contact with the two punches, is not directly exposed to the applied electric current, and is insulated from the applied pressure, which are applied during the spark plasma sintering operation. The spark plasma sintering operation includes at least one thermal cycle applying a heating rate of more than 60° C. / min. The above thermal cycle is A first ramp of increasing the temperature to 550°C to 700°C at a ramp rate of greater than 60°C / min and holding for 2 to 15 minutes; A second heating step in which the temperature is increased to 1400°C to 1500°C at a heating rate of more than 60°C / min and held for 5 to 15 minutes; Includes. The process includes two steps of chemically attacking the MAX phase precursor compound with aqueous acid.

[0019] The present invention also relates to the above-mentioned M n+1 X n T x a spark plasma sintering apparatus for carrying out a process for the manufacture of a MAX precursor compound for use in a process for the manufacture of a compound of the general formula:

[0020] Furthermore, the present invention relates to a spark plasma sintering apparatus having a graphite die and two graphite punches that define a hollow chamber, n+1AX n wherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb, and X is C or N, mixing the powders; placing the powder mixed in the above step into a closed container made of insulating ceramic material housed in the hollow chamber; performing a spark plasma sintering operation; obtaining pellets of said MAX phase type compound; The present invention relates to a process comprising at least

[0021] The spark plasma sintering process of the invention may also comprise the following optional features, considered individually or according to all possible technical combinations: The container is alumina-based. The powder is not in contact with the two punches, is not directly exposed to the applied electric current, and is insulated from the applied pressure, which are applied during the spark plasma sintering operation. The spark plasma sintering operation includes at least one thermal cycle applying a heating rate of more than 60° C. / min. The above thermal cycle is A first ramp of increasing the temperature to 550°C to 700°C at a ramp rate of greater than 60°C / min and holding for 2 to 15 minutes; A second heating step in which the temperature is increased to 1400°C to 1500°C at a heating rate of more than 60°C / min and held for 5 to 15 minutes; Includes.

[0022] The present invention also provides M n+1 AX nwherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb, and X is C or N, which is obtained by the spark plasma sintering process as described above, is in the form of pellets with a porosity of more than 30%, preferably more than 40%, and has a stoichiometric elemental ratio M / X within a relative error of less than ±0.5%.

[0023] The MAX phase type compounds of the present invention may also comprise any of the following features, considered individually or according to all possible technical combinations: It has the formula Ti3AlC2. Most have morphologies exhibiting two types of particle cross sections: a rectangular flat cross-section having a length of 1 μm to 20 μm and a height of 0.5 μm to 2 μm, and / or Rounded corners and flat cross section with diagonal length of 1μm to 20μm.

[0024] Furthermore, the present invention relates to a spark plasma sintering apparatus for carrying out the above-mentioned spark plasma sintering process of the present invention, comprising a graphite die and two graphite punches defining a hollow chamber, which also comprises an enclosure made of insulating ceramic material, e.g. alumina, located within said hollow chamber and capable of receiving a powder mixture during the application of said spark plasma sintering process and maintaining said powder mixture insulated from direct exposure to applied electric current and from applied pressure, wherein said electric current and said pressure are applied during said spark plasma sintering operation.

[0025] Further, the present invention relates to a method for producing a n+1 X nwherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, and X is C or N, characterized in that it is produced from the above-mentioned inventive MAX phase type compound and / or is obtained by the above-mentioned inventive spark plasma sintering process.

[0026] Advantageously, M n+1 X n wherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, X is C or N and T corresponds to an end group selected from O, OH, F or any other halogen group, and S or any other chalcogen group, predominantly in the form of crystals having a general plate shape, the plate having two opposing parallel surfaces of a defined length L separated by a defined height H, and The length of the plate-shaped crystal is 1 μm to 15 μm; The height H of the plate-shaped crystal is 0.2 μm to 1 μm, and The flattened aspect ratio of the plate-shaped crystal, defined by the ratio of the length L to the height H, is 5-50.

[0027] More advantageously, the compound is Ti3C2T x It has the formula:

[0028] Finally, the present invention provides n+1 X n The present invention relates to a process for producing such a compound having the general formula:

[0029] Advantageously, the inventive MAX phase type precursor compound is as described above and / or is obtained by the inventive spark plasma sintering process as described above.

[0030] Other characteristics and advantages of the invention will become apparent from the following non-limiting description, given by way of example with reference to the accompanying drawings, in which: [Brief description of the drawings]

[0031] [Figure 1] FIG. 1 is a schematic diagram of an apparatus of the present invention used to carry out the spark plasma sintering process (SPS) of the present invention to produce a MAX phase type precursor of the present invention. [Figure 2A] 1 is a scanning electron microscope (SEM) photograph of a cross section of a pellet of the Max phase precursor of the present invention obtained by the spark plasma sintering process of the present invention, taken at a magnification of 600. The pellet is coarsely ground. [Figure 2B] 1 is a scanning electron microscope (SEM) photograph taken at a magnification of 2500 times of a cross section of a pellet of the Max phase type precursor of the present invention obtained by the spark plasma sintering process of the present invention. The pellet is coarsely ground. [Figure 3A] 1 is a scanning electron microscope (SEM) photograph of a prior art MAX phase precursor taken at 600x magnification. [Figure 3B] 1 is a scanning electron microscope (SEM) photograph of a prior art MAX phase type precursor taken at 2500x magnification. [Figure 4A] 1 is a scanning electron microscope (SEM) photograph taken at a magnification of 600 times of an MXene compound of the present invention obtained from a MAX phase type precursor of the present invention by a chemical attack process of the present invention. The precursor in pellet form was coarsely ground. [Figure 4B] 1 is a scanning electron microscope (SEM) photograph taken at a magnification of 2500 times of an MXene compound of the present invention obtained from a MAX phase type precursor of the present invention by a chemical attack process of the present invention. The precursor in pellet form was coarsely ground. [Figure 4C] 1 is a scanning electron microscope (SEM) photograph taken at a magnification of 4500 times of an MXene compound of the present invention obtained from a MAX phase type precursor of the present invention by a chemical attack process of the present invention. The precursor in pellet form was coarsely ground. [Figure 5A]1 is a scanning electron microscope (SEM) photograph taken at a magnification of 600 times of an MXene compound of the present invention having a formula of Ti3C2Tx obtained from a MAX phase type precursor of the present invention by a chemical attack process of the present invention. The precursor in pellet form was pulverized. [Figure 5B] 1 is a scanning electron microscope (SEM) photograph taken at a magnification of 2500 times of an MXene compound of the present invention having a formula of Ti3C2Tx obtained from a MAX phase type precursor of the present invention by a chemical attack process of the present invention. The precursor in pellet form was pulverized. [Figure 5C] 1 is a scanning electron microscope (SEM) photograph taken at a magnification of 4500 times of an MXene compound of the present invention having a formula of Ti3C2Tx obtained from a MAX phase type precursor of the present invention by a chemical attack process of the present invention. The precursor in pellet form was pulverized. [Figure 6] FIG. 1 is an X-ray diffraction diagram of an MXene compound of the present invention having the formula Ti3C2Tx, where the boxed areas correspond to the broadening of low intensity peaks. [Figure 7A] FIG. 3C is a scanning electron microscope (SEM) photograph taken at 600x magnification of an MXene-type compound obtained by applying two chemical attacks according to the present invention to the prior art MAX phase precursor of FIGS. 3A and 3B. [Figure 7B] FIG. 3C is a scanning electron microscope (SEM) photograph taken at 2500x magnification of an MXene-type compound obtained by applying two chemical attacks according to the present invention to the prior art MAX phase precursor of FIG. 3A and FIG. 3B. [Figure 7C] FIG. 4 is a scanning electron microscope (SEM) photograph taken at 4500x magnification of an MXene-type compound obtained by applying two chemical attacks according to the present invention to the prior art MAX phase precursor of FIGS. 3A and 3B. [Figure 8] 1 is an energy dispersive X-ray (EDX) spectrum of an MXene compound of the present invention having the formula Ti3C2Tx. [Figure 9] FIG. 1 is an energy dispersive X-ray (EDX) spectrum of an MXene compound obtained from a prior art MAX phase precursor. [Figure 10] FIG. 2C is an X-ray diffraction diagram of the MAX phase compound of the present invention shown in FIG. 2A and FIG. 2B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] The present invention relates primarily to MXene compounds obtainable from the MAX phase precursors of the present invention, as well as processes for producing MXene compounds, including the inventive process and associated apparatus for producing the MAX phase precursors.

[0033] The present invention also relates to a first innovative process and associated apparatus for producing a MAX phase precursor, which is subsequently used to produce the MXene compounds of the present invention according to a second innovative manufacturing process.

[0034] The process for producing MAX phase precursors, particularly but not exclusively, having the formula Ti3AlC2, is based on the known spark plasma sintering (SPS) technique.

[0035] 1, and in a known manner, this process involves the use of an apparatus 1 comprising a graphite die 2 defining a hollow chamber 4 and lower 3a and upper 3b punches. This single configuration corresponds to SPS equipment widely sold and used to perform this sintering technique.

[0036] In the present invention, the device 1 further comprises a closed hollow vessel 5, which is housed in the hollow chamber 4 and is composed of a hollow cylinder 6 made of a high temperature resistant and chemically neutral insulating material, and a disk-shaped lower 7a and upper 7b cover made of the same material and attached to both ends of the hollow cylinder 6. For example, the hollow cylinder 6 and the covers 7a, 7b can be made of alumina or another insulating ceramic material. The powder mixture used for the synthesis of the MAX phase precursor is placed in the alumina hollow vessel 5, and then the known operations of applying a vacuum and increasing the temperature are applied. After cooling, a cylindrical pellet is obtained.

[0037] To synthesize a MAX phase precursor with the composition Ti3AlC2, commercially available titanium, aluminum and titanium carbide powders are used and mixed in an agate mortar. To mix the three components more finely, the mixture is passed through a ball mill. The composition of the Ti:Al:TiC mixture can be stoichiometric (element ratios of 1:1:2, respectively, within a relative error of less than ±0.5%), but it is preferred to have a slight excess of aluminum, in particular an element ratio of 1:1.1:2, respectively. That is, the element ratio Ti / C is stoichiometric within a relative error of less than ±0.5%.

[0038] With the hollow cylinder 6 and its lower cover 7a already in place, the powder mixture is loaded into the hollow alumina container 5 of the apparatus of FIG. 1. The powder is compacted within the hollow container 5, after which the upper cover 7b of the container 5 and the graphite upper punch 3b are placed in place. After applying the vacuum, a thermal cycle is performed which includes a rapid temperature ramp (about 15-30 minutes) to a temperature of about 1400°C-1600°C, more specifically 1450°C, over a period of 5-15 minutes. More typically, the ramp rate is greater than 60°C / min. More specifically, the thermal cycle includes a first ramp to a temperature of 550°C-700°C at a rate of greater than 60°C / min and held for 2-15 minutes, followed by a second ramp to a temperature of 1400°C-1500°C at a rate of greater than 60°C / min and held for 5-15 minutes.

[0039] A cylindrical porous pellet is obtained, and as shown below, this porosity is essential for the synthesis of MXene compounds.

[0040] The synthesis of MAX phase precursors was tested using the prior art SPS technique (without the alumina hollow container) as detailed in Comparative Example 1. In these tests, the powder mixture was loaded into an assembly formed by a graphite die and punch. According to XRD analysis, these tests yielded a mixture of MAX phases with other peaks of unidentified crystalline phases. The strong presence of titanium carbide TiC was also confirmed. The pellets were also very dense, compact and not porous. They were difficult to crush and difficult to perform chemical attack.

[0041] These differences between the MAX phase precursors obtained by known SPS techniques and the MAX phase precursors obtained by the process and apparatus of the present invention may be due to several factors. Using conventional SPS techniques, additional reactions of the powder mixture with the carbon of the graphite assembly may occur. Additionally or additionally, the powder mixture is subjected to high pressures of the same magnitude as those applied to the graphite punch. Also additionally, an electric current is passed through the powder reaction mixture, which may cause the phenomenon of electromigration of one of the components.

[0042] Thus, in contrast to the usual use of SPS equipment, in the present invention the powder mixture is not in contact with graphite, is not directly exposed to applied current and is insulated from applied pressure, which allows obtaining innovative MAX phase precursors in the form of porous pellets, enabling the synthesis of MXene compounds with specific crystal configurations, as shown below.

[0043] The second process of the invention is a process for the synthesis of MXene compounds by chemical attack of the MAX phase precursor obtained by the process of the invention described above. The chemical attack is carried out using an aqueous solution of hydrofluoric acid. More specifically, an aqueous solution of hydrofluoric acid formed in situ is used, more specifically a mixture of a fluoride salt such as lithium fluoride and a strong acid such as hydrochloric acid, with a concentration of fluorine species less than 5M.

[0044] In the present invention, at least two chemical attacks are carried out, each additional attack step consisting of recovery of the product and a new attack with a hydrofluoric acid solution.

[0045] Most of the crystals are flat, especially Ti3C2T xThe resulting MXene compound has the formula: These plates have two parallel planes and the flattened aspect ratio, defined as the ratio of the plate's length L to its height H, is between 5 and 50, with an average of about 10. The crystal size distribution is relatively uniform, with the majority of crystals having lengths between 1 micron and 15 microns and heights H between 0.2 microns and 1 micron. The distribution and flattened aspect ratio are assessed by counting the distances measured in scanning electron microscope (SEM) images and by measurements on SEM images, respectively.

[0046] This process for the preparation of MXene compounds by two chemical attacks has been applied to finely ground MAX phase precursors of the invention as well as to coarsely ground MAX phase precursors of the invention. As shown in detail below, in both cases an improvement in the size distribution of the particles is observed when the MAX phase precursor is finely ground prior to chemical attack, while the bulk morphology of the crystals remains the same in the form of plates as defined above.

[0047] The same preparation process of MXene compounds by two chemical attacks was also applied to a commercial MAX phase precursor for comparison purposes. The morphology of the obtained MXene compounds is quite different from that of the present invention (Comparative Example 2 and Figures 7A, 7B and 7C). These results show that the acquisition of the MXene compounds of the present invention with a plate morphology is related to the specificity of the MAX phase precursor of the present invention. This specificity is believed to induce this special crystalline morphology of the MXene compounds of the present invention, and the subsequent two chemical attacks do not deteriorate this crystalline morphology.

[0048] The morphological features are revealed by visual observation and measurement of multiple crystals in several samples in scanning electron microscope (SEM) images, performed at several points in each sample. To date, to the inventors' knowledge, there are no reliable quantitative techniques to replace imaging for measuring flattened aspect ratio and particle size distribution when the particles cannot be approximated as spherical particles and when their large size makes them difficult to place in suspension.

[0049] Examples of the crystal morphology of the MXene compound of the present invention are shown in Figures 4A, 4B, and 4C. These are Ti3C2T of the present invention having the above-mentioned crystal morphology. x SEM images of the compound are shown at several magnifications.

[0050] The compounds obtained by the process of the present invention are of the "MXene" type, in particular Ti3C2T x That it corresponds to a compound having the composition was confirmed by two techniques: analysis of the crystalline phase by X-ray powder diffraction (XRD) using a Cu Kα radiation source (FIG. 6) and energy dispersive X-ray spectroscopy (EDX) using an EDX detector integrated into the SEM instrument (FIG. 8).

[0051] As shown in FIG. 6, the X-ray diffraction pattern of the MXene compound of the present invention obtained by the above-mentioned process is characterized by a large peak, designated by the reference number 9, located at an angle 2θ of 6.5° to 6.9°. This corresponds to the (hkl)=(002) plane and is the origin of Ti3C2T x The distance between the lamellae of the (002) planes corresponds to the interplanar distance. Peaks at lower densities and higher angles can also be observed. These peaks correspond mainly to replicas of the (002) plane and therefore correspond to multiples of the angle of the main peak.

[0052] Ti3C2T x Elemental analysis of the MXene compound of the present invention having the formula was performed by energy dispersive X-ray (EDX) spectroscopy. With reference to Figure 8, the EDX reveals a composition of Ti and C, with no Al present (no peak at about 1.5 keV, in contrast to the EDX of the MXene compound obtained from the prior art MAX phase precursor shown in Figure 9). This indicates that the main structural unit of the MXene compound having the composition Ti3C2 is Ti3C2, and that the T corresponding to -OH or =O, -F and -Cl groups are present. xThe atomic ratios of the elements forming the end groups to Ti, i.e., Cl / Ti, F / Ti and O / Ti, are on average 0.05, 0.5 and 0.4, respectively, from the quantitative EDX analysis of the samples obtained according to the procedure of Example 2 described below.

[0053] By changing the synthesis or post-treatment conditions, x The composition of the end groups may be different, or one type of end group may be absent, but even in such cases the resulting compound will still be of the MXene type, especially Ti3C2T x It should be noted that in the MXene compound, no aluminum is present. This is in contrast to the case where the chemical attack involves only one step, even if the chemical attack continues for a long time (more than 48 hours) and excess F is still present at the end of the attack step relative to the strong acidic medium and the MAX phase precursor. In this case, a single chemical attack is observed to have an Al / Ti ratio of about 0.01, which corresponds to an Al / Ti ratio of 0.003 to 0.01 in the above-mentioned non-patent document 2. EXAMPLES

[0054] Example 1: Synthesis of MAX phase precursor with composition Ti3AlC2 A spark plasma sintering apparatus was used, marketed by Fuji Electric Industrial Co., Ltd. under the name Dr. Sinter Lab. Jr. (model number: SPS-211Lx). This apparatus was modified according to the invention, as described with reference to FIG. 1, by retaining the graphite die 2 and the two graphite punches 3a and 3b, but adding to the hollow chamber 4 a hollow alumina cylinder 6 and upper 7a and lower 7a alumina disks forming a hollow alumina container 5. The powder mixture described below was placed in the container 5, compressed and kept electrically insulated from the current flowing through the graphite punch and die. The mixture was also kept insulated from the pressure exerted by the punches and kept without contact with the graphite throughout the operation time.

[0055] Commercially available titanium, aluminum and titanium carbide powders were mixed in an agate mortar in elemental ratios of 1:1.1:2 respectively with a total weight of the powder mixture of about 5 g. The mixture was placed in a ball mill with tungsten carbide bowl and balls for 1 hour and 15 minutes and ground at a speed of 300 rpm. 1 g of ground powder was placed in the hollow cylinder 6 with the lower cover 7a already in place in the apparatus. The output was compressed and the upper cover 7b was placed on the top end of the hollow cylinder 6, thereby forming the hollow vessel 5. With the graphite upper punch 3b in place, the entire assembly 1 was placed in the SPS apparatus and a vacuum was applied. The following thermal cycle was applied: 6 minutes ramp to 580°C, 5 minutes hold at 580°C, 12 minutes ramp to 1450°C and 8 minutes hold at 1450°C. Once the thermal cycle is complete, the temperature is rapidly reduced to below 580°C in about 5-10 minutes. A cylindrical porous pellet is obtained. The porosity of the pellets is greater than 30%, in most cases greater than 40%, and in most cases about or greater than 50%, as determined by the difference between the measured volume of the pellet and the volume of the compressed material calculated from the theoretical density and weight of the pellet.

[0056] In Figures 2A and 2B the morphology of porous pellets of the MAX phase precursor obtained according to the invention after coarse grinding is shown. These images are compared with the images of a commercial powder of the MAX phase compound in Figures 3A and 3B. A clear difference can be seen between the two compounds. In contrast to the particles bonded together in the case of the precursor of the invention, the MAX phase compound of the prior art is characterized by clusters of particles with a large dispersion of particle sizes (tens of nanometers to tens of micrometers). The images in Figures 3A and 3B are similar to the MAX phase compound as obtained and published in the abovementioned literature.

[0057] Furthermore, as shown in Figure 2B, the MAX phase according to the present invention exhibits joined particles that exhibit a cross section similar to the particle shape of MXene obtained after chemical attack. In particular, many particle cross sections appear to have either rectangular flat cross sections with lengths of 1 μm to 20 μm and heights of 0.5 μm to 2 μm, or rounded corner flat cross sections with rounded outlines with diagonal lengths of 1 μm to 20 μm, depending on the orientation of the cross sections in the crushed section. Since the particles of this MAX phase are not isolated and are joined, these dimensions are rough estimates.

[0058] 10, the X-ray diffraction pattern of the MAX phase compound of the present invention obtained in this example using a Cu Kα radiation source corresponds to the crystalline phase of the Ti3AlC2 compound with the addition of a low intensity peak at an angle 2θ of 36.0° due to a titanium carbide phase contained in the initial powder, which is estimated to be less than 5% by volume of the crystalline phase of the MAX phase compound.

[0059] The EDX spectrum of the MAX phase compound of the present invention reveals the presence of three elements in the composition of the MAX phase, namely titanium, aluminum and carbon, and the absence of impurities such as oxygen or any other element.

[0060] Comparative Example 1: Trial production of MAX phase precursor having the composition Ti3AlC2 in a conventional SPS apparatus The powder mixture described and prepared in Example 1 was loaded into a commercial spark plasma sintering apparatus as in Example 1. In contrast to the apparatus used in Example 1, this apparatus was not modified; the powder was placed in a hollow graphite chamber exposed to electric current and pressure. Several heating parameters were tested, such as maximum hold temperature (1150°C to 1450°C), temperature hold time (8 min to 24 min), and adding an intermediate hold at 650°C. All these tests resulted in very compact pellets that were not porous. Due to their extensive compactness, the pellets were unsuitable for one or more chemical attacks to produce MXene compounds.

[0061] Moreover, the composition of the pellets, as determined by X-ray diffraction analysis, showed a high titanium carbide content to the detriment of the desired Ti3AlC2.

[0062] Further tests were carried out by adding 20 at. % Si relative to Al in the powder mixture (following the example of non-patent document 3). The pellets obtained here were also very compact with no porosity. Also, analysis by X-ray diffraction showed that the product was clearly Ti3(Al) with an additional unidentified phase. 1-x S x )C2.

[0063] Therefore, prior art sintering techniques by spark plasma sintering do not allow for obtaining MAX phase compounds that would allow the subsequent synthesis of MXene compounds.

[0064] Example 2: Ti3C2T from the coarsely ground MAX phase precursor of Example 1 x Preparation of MXene compounds having the formula The porous pellets of Ti3AlC2 obtained in Example 1 were coarsely ground in an agate mortar to clusters of mostly about 1 mm to 2 mm. A first chemical attack was performed using an in situ formed hydrofluoric acid solution. For that purpose, 0.5 g of the MAX phase compound having the formula of Ti3AlC2 obtained in Example 1 was placed in a Teflon centrifuge tube of about 50 mL capacity, to which was added 10 mL of a previously prepared aqueous solution containing 2 M lithium fluoride and 6 M hydrochloric acid. The mixture was left stirring at ambient temperature for 5 minutes using a magnetic stirrer. The tube was placed in a temperature controlled bath at 35°C for about 72 hours with continued stirring.

[0065] After this first challenge, deoxygenated water was added to a level of about 35 mL and centrifuged at 9000 rpm for 10-15 min, after which the supernatant was drained off and the precipitate retained. A second chemical challenge was then performed by pouring 10-20 mL of the same aqueous solution containing 2 M lithium fluoride and 6 M hydrochloric acid onto the precipitate and stirring in a temperature-controlled bath at 35° C. for about 72 h.

[0066] Upon completion of this second chemical attack, a rinse step was performed by adding deoxygenated water (typically 200 mL) with stirring for 5 minutes, followed by centrifugation at 9000 rpm for 10-15 minutes, draining the supernatant and keeping the precipitate. This operation was repeated about five times until the pH of the supernatant was 4.5 or higher. The precipitate was then washed with ethanol in two steps of ethanol rinse and centrifugation, then covered with ethanol and stored. Alternatively, the precipitate can be dried by vacuum heating at temperatures between 40°C and 120°C.

[0067] In this way, Ti3C2T x or more generally, an MXene compound having the formula Ti3C2 is obtained. The crystalline morphology of this compound is shown in Figures 4A, 4B and 4C. It can be seen that the compound is composed of crystals separated from each other in the form of plates with two parallel planes. The flattened aspect ratio (ratio of crystal length L to height H) is between 5 and 50, with an average of about 10. The size distribution of the crystals is relatively uniform, with the crystal length L being between 1 micron and 15 microns, and the height being between 0.2 microns and 1 micron.

[0068] As mentioned above, the X-ray diffraction pattern in FIG. 6 is characterized by a large peak, designated by reference number 9, located at an angle 2θ of 6.5° to 6.9°. This corresponds to the (hkl)=(002) plane and is the origin of Ti3C2T x It corresponds to the interplanar distance between lamellar surfaces consisting of units.

[0069] The EDX spectrum of this same compound (Figure 8) reveals the presence of two major elements in the composition of this MXene-type compound, namely titanium and carbon, as well as the presence of the terminal group T x In particular, it can be seen that there are fluorine, oxygen and chlorine, which may correspond to -F, -Cl, =O or -OH groups. As mentioned above, the EDX spectrum also shows that there is no element Al present, which means that the entire MAX phase precursor has been attacked and no aluminum-containing by-products remain, such as the oxide Al2O3.

[0070] Example 3: Ti3C2T from finely ground MAX phase precursor of Example 1 x Preparation of MXene compounds having the formula The Ti3AlC2 porous pellets obtained in Example 1 were crushed in an agate mortar and then pulverized. The powder was passed through a sieve with a mesh size of 50 μm. This resulted in a powder with a particle size of less than 0.50 μm. The same two chemical attack and rinsing procedures as described in Example 2 were applied.

[0071] The crystal morphology of this compound is shown in Figures 5A, 5B and 5C. It is confirmed that this compound is also composed of crystals separated from each other in the form of a plate with two parallel planes. The flat aspect ratio (ratio of length L to height H of the crystal) is also 5-50, with an average of about 10. The size distribution of the crystals is relatively uniform, with the length L of the crystal being 1 micron to 15 microns and the height H being 0.2 microns to 1 micron. Nevertheless, a strong presence of crystals having a size of about 1 micron or less is confirmed. These crystals are often in bulk shape (height H of the same order as length L) rather than in plate morphology, but most of the crystals are in plate morphology.

[0072] The X-ray diffraction pattern and EDX spectrum are the same as those described in Example 2.

[0073] Comparative Example 2: Ti3C2T from prior art MAX phase precursor Ti3AlC2 x Preparation of MXene compounds having the formula Two batches of a commercially available MAX phase precursor sold under the name Ti3AlC2 were used. Both had the appearance of a fine powder with particle sizes less than about 50 microns. SEM images of these compounds (Figures 3A and 3B) show a heterogeneous distribution of particle sizes ranging from tens of microns to tens of nanometers.

[0074] The same two-step chemical attack and rinsing procedure described in Example 2 was applied to each batch.

[0075] The crystal morphology of the obtained MXene compound is shown in Figures 7A, 7B and 7C. The compound is mainly composed of bulk shaped particles (length on the same order as height) and particle clusters. Only a small number of these particles have platelet morphology. The particle size distribution is very heterogeneous, ranging from tens of microns to tens of nanometers. This morphology was the same for both batches of the MAX phase precursor used. This morphology is also consistent with that reported in the literature.

[0076] The X-ray diffraction patterns of the two MXene compounds obtained are similar to those of the compound of the invention obtained in Example 2. The EDX spectrum (FIG. 9) shows that, as in the case of the compound obtained in Example 2, in addition to the presence of two main elements, namely titanium and carbon, in the composition of this MXene type compound, the terminal group T x It can be seen that in particular fluorine, oxygen and chlorine are present which may correspond to -F, -Cl, =O or -OH groups.

[0077] On the other hand, these spectra also show the presence of aluminum as an impurity, in contrast to the inventive MXene compounds of Examples 2 and 3 (Figure 8). The atomic ratio Al / Ti is estimated to be 0.03-0.04 from EDX spectra acquired on images containing many particles (such as the spectrum in Figure 9). EDX analysis of individual particles shows that aluminum is mainly present as submicrometer particles of aluminum oxide, which is undoubtedly the compound Al2O3.

Claims

1. M n+1 X n T x wherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, X is C or N and T corresponds to an end group selected from O, OH, F or any other halogen group, and S or any other chalcogen group, characterized in that the majority are in the form of crystals having a general plate shape, the plate having two opposing parallel surfaces having a defined length (L) spaced apart by a defined height (H); and The length of the plate-shaped crystals is 1 μm to 15 μm; The height (H) of the plate-shaped crystal is 0.2 μm to 1 μm, and A compound characterized in that the flattened aspect ratio of the plate-shaped crystals, defined by the ratio of the length (L) to the height (H), is 5 to 50.

2. Ti 3 C 2 T x 2. The compound of claim 1 having the formula:

3. M n+1 AX n wherein n is 1, 2 or 3; M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta; A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb; and X is C or N; in the form of pellets having a porosity of more than 30%, preferably more than 40%, and having a stoichiometric element ratio M / X within a relative error of less than ±0.5%; 3. A compound according to claim 1 or 2, characterized in that it is obtained from a MAX phase type precursor compound.

4. The MAX phase type precursor compound is Ti 3 AIC 2 4. The compound of claim 3 having the formula:

5. 5. The compound according to claim 3 or 4, wherein the majority of the MAX phase type precursor compound has a morphology exhibiting two types of grain cross sections: a rectangular flat cross-section having a length of 1 μm to 20 μm and a height of 0.5 μm to 2 μm; and / or A rounded flat cross section having a diagonal length of 1 μm to 20 μm.

6. A process for producing a compound according to any one of claims 1 to 5, comprising two steps of chemical attack of a MAX phase type precursor compound with aqueous acid.

7. A process for producing the compound according to any one of claims 3 to 5, in which the MAX phase type precursor compound is obtained by a spark plasma sintering process in a spark plasma sintering device (1) comprising a graphite mould (2) defining a hollow chamber (4) and two graphite punches (3a, 3b), the spark plasma sintering process comprising: mixing the precursor powders; placing the powder mixed in the previous step in a closed container (5) made of insulating ceramic material housed in the hollow chamber (4); performing a spark plasma sintering operation; obtaining pellets of the MAX phase type compound; A process comprising at least

8. 8. The process according to claim 7, wherein the vessel (5) is alumina-based.

9. 9. The process according to claim 7 or 8, wherein the powder is not in contact with the two punches (3a, 3b), is not directly exposed to applied electric current and is insulated from applied pressure, wherein said electric current and said pressure are applied during the spark plasma sintering operation.

10. The process according to any one of claims 7 to 9, wherein the spark plasma sintering operation comprises at least one thermal cycle applying a heating rate of more than 60°C / min.

11. The thermal cycle comprises: A first ramp to a temperature of 550° C.-700° C. at a ramp rate of greater than 60° C. / min and held for 2-15 minutes, followed by A second heating step of heating to a temperature of 1400° C. to 1500° C. at a heating rate of more than 60° C. / min and holding for 5 to 15 minutes; The process according to any one of claims 7 to 10, comprising:

12. The process according to any one of claims 7 to 10, comprising two steps of chemical attack of said MAX phase type precursor compound with aqueous acid.

13. 13. A spark plasma sintering apparatus for carrying out a process for producing the MAX precursor compound used in the process according to any one of claims 7 to 12, comprising a graphite die (2) and two graphite punches (3a, 3b) defining a hollow chamber (4), characterized in that it also comprises an enclosure (5) made of insulating ceramic material, for example alumina, located within said hollow chamber (4) and capable of receiving a powder mixture during the application of the spark plasma sintering process and keeping said powder mixture isolated from direct exposure to applied electric currents and from applied pressures, said electric currents and said pressures being applied during the spark plasma sintering operation.

14. In a spark plasma sintering apparatus (1) equipped with a graphite die (2) defining a hollow chamber (4) and two graphite punches (3a, 3b), M n+1 AX n wherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb, and X is C or N, mixing the powders; placing the powder mixed in the previous step in a closed container (5) made of insulating ceramic material housed in the hollow chamber (4); performing a spark plasma sintering operation; obtaining pellets of the MAX phase type compound; A process comprising at least

15. 15. The process according to claim 14, wherein the vessel (5) is alumina-based.

16. 16. The process according to claim 14 or 15, wherein the powder is not in contact with the two punches (3a, 3b), is not directly exposed to applied electric current and is insulated from applied pressure, wherein said electric current and said pressure are applied during the spark plasma sintering operation.

17. The process according to any one of claims 14 to 16, wherein the spark plasma sintering operation comprises at least one thermal cycle applying a heating rate of more than 60°C / min.

18. The thermal cycle comprises: A first ramp to a temperature of 550° C.-700° C. at a ramp rate of greater than 60° C. / min and held for 2-15 minutes, followed by A second heating step of heating to a temperature of 1400° C. to 1500° C. at a heating rate of more than 60° C. / min and holding for 5 to 15 minutes; 20. The process of claim 17, comprising:

19. M n+1 AX n MAX phase type compound having the general formula: where n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, A is selected from Al, Si, P, S, Ga, Ge, As, Cd, In, Sn, Tl and Pb, and X is C or N, obtainable by the process according to any one of claims 14 to 18, in the form of pellets having a porosity of more than 30%, preferably more than 40%, and having a stoichiometric elemental ratio M / X within a relative error of less than ±0.5%.

20. Ti 3 AIC 2 20. The MAX phase type compound of claim 19 having the formula:

21. 21. The MAX phase type compound according to claim 19 or 20, having a morphology that predominantly exhibits the following two types of grain cross-section: a rectangular flat cross-section having a length of 1 μm to 20 μm and a height of 0.5 μm to 2 μm; and / or A rounded flat cross section having a diagonal length of 1 μm to 20 μm.

22. 19. An apparatus for performing the process according to any one of claims 14 to 18, comprising a graphite die (2) and two graphite punches (3a, 3b) defining a hollow chamber (4), also comprising an enclosure (5) made of insulating ceramic material, e.g. alumina, located within said hollow chamber (4) and capable of receiving the powder mixture during the application of the spark plasma sintering process and keeping the powder mixture isolated from direct exposure to applied electric current and from applied pressure, wherein said electric current and said pressure are applied during the spark plasma sintering operation.

23. M n+1 X n in which n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, and X is C or N, characterized in that it is produced from a MAX phase type compound according to any one of claims 19 to 21 and / or is obtained by a process according to any one of claims 14 to 18.

24. M n+1 X n T x wherein n is 1, 2 or 3, M is selected from Ti, V, Cr, Zr, Nb, Mo, Hf, Sc, Mn, Y and Ta, X is C or N and T corresponds to an end group selected from O, OH, F or any other halogen group, and S or any other chalcogen group, characterized in that the majority are in the form of crystals having a general plate shape, the plate having two opposing parallel surfaces having a defined length (L) spaced apart by a defined height (H); and The length of the plate-shaped crystal is 1 μm to 15 μm; The height (H) of the plate-shaped crystal is 0.2 μm to 1 μm, and The compound according to claim 23, characterized in that the flat aspect ratio of the plate-shaped crystals, defined by the ratio of the length (L) to the height (H), is 5-50.

25. Ti 3 C 2 T x 25. The compound of claim 24 having the formula:

26. 26. A process for producing a compound according to claim 24 or 25, comprising two steps of chemical attack of said MAX phase precursor compound with aqueous acid.

27. A process according to claim 26, wherein the MAX phase type precursor compound is according to any one of claims 18 to 20 and / or is obtainable by a process according to any one of claims 13 to 17.

Citation Information

Patent Citations

  • Preparation method of grain-oriented strontium sodium niobate leadless ferroelectric ceramic

    CN111533556A

  • Overall ordered-local disordered porous ceramic and preparation method thereof

    CN112707738A

  • Energization sintering method

    JP1999012606A

  • High-specific strength magnesium functional material having magnetism

    JP2011243776A

  • Mxene nanosheet and manufacturing method thereof

    US20170088429A1