Plate-shaped nuclear fuel element and its manufacturing method
The nuclear fuel element design with a harder frame material mitigates 'dogbone' effects, enhancing the structural integrity and containment of fissile material during rolling and irradiation.
Patent Information
- Application Number
- JP2024523386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-19
- Filing Date
- 2022-10-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-17
AI Technical Summary
Existing plate-shaped nuclear fuel elements face issues with 'dogbone' effects during rolling, which can lead to localized thinning of the cladding and potential release of fissile material, necessitating reworking.
A plate-shaped nuclear fuel element design featuring a frame made of a harder cladding material than the cover plate, which limits deformation and minimizes the 'dogbone' effect during rolling.
The design effectively reduces the risk of cladding thinning, ensuring secure containment of fissile material and maintaining structural integrity during processing and irradiation.
Smart Images

Figure 2024538193000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of nuclear fuel elements, in particular plate-shaped nuclear fuel elements, for example for use as primary targets or as nuclear fuel for research reactors. [Background technology]
[0002] The plate-shaped nuclear fuel elements may be placed, for example, in a nuclear reactor to be irradiated, for example to obtain fission products for instrument calibration for use in nuclear medicine or biology, or to provide neutrons for research applications.
[0003] Uranium-containing plate-shaped nuclear fuel elements can be used to recover molybdenum-99 (hereinafter referred to as "Mo99"), which is a standard beta emitter and can therefore serve as a source of technetium-99, which is used, for example, for instrument calibration, and in particular the metastable nuclear isomer of technetium-99 (Tc99m), which is used as a radioactive tracer in nuclear medicine and biology.
[0004] It is possible to provide a plate-shaped nuclear fuel element comprising a plate-shaped core of fissile material sealed within a cladding covering edges and faces of the core, The fissile material may comprise a uranium alloy and the cladding may be made of aluminium or an aluminium alloy.
[0005] It is possible to manufacture such plate-shaped nuclear fuel elements by using the "picture-in-frame" technique, in which a core made of a rectangular plate of fissile material of uniform thickness is fitted into an opening in a frame, and cover plates are placed on opposite sides of the frame in such a way that the frame containing the core is sandwiched between the cover plates. This sandwich structure is then rolled, in particular hot rolled. During the rolling process, the cover plates are fixed to the frames, sealing the core and forming the plate-shaped nuclear fuel element.
[0006] Rolling reduces the thickness of the nuclear fuel element and increases its length. Rolling can create a so-called "dog bone" effect, which increases the thickness of the core at the ends of the core and causes a corresponding decrease in the thickness of the cover plates.
[0007] However, it is desirable to minimize the thickness of the cladding to prevent the release of fissile material during processing and irradiation. If the cladding becomes too thin locally, especially due to the dogbone effect, it may be necessary to rebut the nuclear fuel elements.
[0008] Several proposals have been made to limit the dog-bone effect.
[0009] GB 1 094 505 proposes providing inserts between the fissile core and the cover plate at the ends of the core.
[0010] French patent FR 1 210 887 proposes providing the fissile core as a uranium-aluminium alloy (U-Al) with the addition of one element selected from the group consisting of silicon (Si), titanium (Ti), germanium (Ge), zirconium (Zr) and tin (Sn). [Prior art documents] [Patent documents]
[0011] [Patent Document 1] British Patent No. 1094505 [Patent Document 2] French Patent No. 1210887 Summary of the Invention [Problem to be solved by the invention]
[0012] One of the aims of the present invention is to propose a plate-shaped nuclear fuel element which makes it possible to reduce the risk of the dog-bone effect. [Means for solving the problem]
[0013] To achieve this object, the invention proposes a plate-shaped nuclear fuel element comprising a core and cladding made of fissile material, the cladding comprising a frame defining a central opening for accommodating the core and two cover plates sandwiching the frame and the core, the frame being made of a metallic first cladding material and the cover plates being made of a metallic second cladding material, the first cladding material having a hardness strictly higher than the hardness of the second cladding material.
[0014] The frame made of the first cladding material, which exhibits a higher hardness than the second cladding material of the cover plate, is more resistant to deformation than the cover plate, so that during rolling of the nuclear fuel element, the nuclear fuel element is less deformed in the area of the ends of the core, thus limiting the appearance of the dog-bone effect.
[0015] In specific embodiments, the nuclear fuel element comprises one or more of the following optional features, either individually or in any technically feasible combination: - said hardness of the first cladding material is strictly lower than the hardness of the core; the first cladding material is an aluminum alloy or a zirconium alloy; the first cladding material is an aluminum-magnesium alloy; - the first cladding material is an AG4 or AG5 aluminum-magnesium alloy; - the second cladding material is an aluminum alloy or a zirconium alloy; - the second cladding material is an aluminum-magnesium alloy; - the second cladding material is AG3 aluminum-magnesium alloy; - the fissile material contains at least one uranium alloy; - the fissile material contains a uranium-silicon alloy, a uranium-molybdenum alloy, a uranium-aluminum alloy, a uranium-zirconium alloy, or a combination thereof; -Fissile material is U 3 S 2 Made of; - The uranium content of the fissile material is 2.5 gU / cm 3 Above, specifically, strictly 4.8 gU / cm 3 Super; - The uranium content of the fissile material is 6.5 gU / cm 3 Less than 5.3 gU / cm 3 is less than.
[0016] The present invention also relates to a method for producing a plate-shaped nuclear fuel element as defined above, comprising the steps of: - providing a core, a frame having an opening and a cover plate; - inserting a core into an opening in the frame; - covering a frame housing the core with two cover plates in such a way that the cover plates sandwich the frame and the core; - rolling the sandwich structure so that the cover plate is fixed to the frame, the core being sealed within the cladding defined by the frame and the cover plate; The present invention also relates to a method comprising the steps of:
[0017] The invention and its advantages will be better understood on reading the following description, given purely as a non-limiting example and with reference to the accompanying drawings, in which: [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a front view of a plate-shaped nuclear fuel element. [Diagram 2] FIG. 2 is a cross-sectional view of the nuclear fuel element taken along II-II of FIG. 1. [Diagram 3] FIG. 3 illustrates the sealing of the core of the nuclear fuel element shown in FIGS. 1 and 2 into the cladding. [Figure 4] FIG. 3 illustrates the sealing of the core of the nuclear fuel element shown in FIGS. 1 and 2 into the cladding. [Diagram 5] 1 illustrates a cross-section of a nuclear fuel element taken with an optical microscope. [Figure 6] 1 illustrates a cross-section of a nuclear fuel element taken with an optical microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The nuclear fuel element 2 illustrated in FIG. 1 is intended to be used, for example, as a primary target in a nuclear reactor or as nuclear fuel for a research reactor for the purpose of obtaining neutrons.
[0020] The nuclear fuel elements 2 are plate-shaped. They have a length of, for example, approximately 150 mm for primary targets and up to approximately 1000 mm for use as nuclear fuel for research reactors, a width of, for example, 40-90 mm and a thickness of, for example, approximately 1 mm-3 mm. With a view to obtaining a cylindrical nuclear fuel product, the plate-shaped fuel elements 2 are, for example, rolled and welded, usually with a diameter of approximately 20-50 mm, for example 30 mm.
[0021] As can be seen in FIG. 2, the nuclear fuel element 2 includes a core 4 of fissile material that is sealed within a cladding 6 .
[0022] The core 4 is surrounded in a sealing manner by the cladding 6. The cladding 6 prevents the fissile material of the core 4 from migrating out of the cladding 6. The cladding 6 also retains the fission products produced during irradiation of the nuclear fuel elements 2.
[0023] The fissile material includes, for example, uranium. The uranium content of the fissile material is preferably 2.5 gU / cm 3 More than or equal to 4.8 gU / cm, preferably exactly 4.8 gU / cm 3 The uranium content of the fissile material is, for example, 6.5 gU / cm 3 The following, especially 5.3 gU / cm 3 The following is the result.
[0024] The uranium contained in the fissile material is, for example, low enriched uranium (LEU). LEU is the isotope U in uranium. 235 is less than 20% by weight, for example about 19.75% by weight.
[0025] The fissile material contains, for example, a uranium alloy, in particular a uranium alloy selected from the group consisting of a uranium-silicon alloy, a uranium-molybdenum alloy, a uranium-aluminium alloy and a uranium-zirconium alloy or mixtures thereof.
[0026] In a specific embodiment, the fissile material comprises a single uranium alloy, particularly a uranium alloy selected from the group consisting of uranium-silicon alloy, uranium-molybdenum alloy, uranium-aluminum alloy and uranium-zirconium alloy.
[0027] In a preferred embodiment, the uranium contained in the fissile material of the core 4 is U 3 S 2 Provided as.
[0028] The cladding 6 includes a frame 8 having an opening 10 to accommodate the core 4, and two cover plates 12 mounted on opposite sides of the frame 8 such that the frame 8 and the core 4 housed within the central opening 10 are sandwiched between the cover plates 12.
[0029] The frame 8 is made of a first cladding material and the cover plate 12 is made of a second cladding material that is different from the first cladding material.
[0030] The first cladding material has a hardness strictly higher than that of the second cladding material, and preferably strictly lower than that of the core 4 (ie the hardness of the fissile material).
[0031] As explained below, the method for manufacturing the nuclear fuel element 2 may comprise hot rolling, for example at a temperature between 300°C and 600°C, in particular between 350°C and 450°C.
[0032] In a temperature range of 300°C to 600°C, in particular in a temperature range of 350°C to 450°C, the first cladding material has a Vickers hardness (HV) of, for example, 40 to 70 HV, the second cladding material has a Vickers hardness of, for example, 30 to 60 HV, and / or the core 4 has a Vickers hardness of, for example, 50 to 100 HV.
[0033] As described below, the method for manufacturing the nuclear fuel element 2 may include cold rolling, which is performed at room temperature.
[0034] At room temperature, the first cladding material has a Vickers hardness (HV) of, for example, 50-100 HV, the second cladding material has a Vickers hardness of, for example, 30-70 HV, and / or the core 4 has a Vickers hardness of, for example, 100 HV or more.
[0035] The first cladding material and the second cladding material are, for example, metallic materials.
[0036] Each of the first and second cladding materials may generally be any type of metallic material used in nuclear reactors, i.e. an aluminium alloy, for example EN AW-1050A, EN AW-6061, EN AW-5754, EN AW-5083, EN AW-5019 or AlFeNi, a zirconium alloy, for example Zircaloy-2, Zircaloy-4 or a Zr-Nb alloy, a Ni-based alloy, for example Alloy600, or a stainless steel, for example AISI 304L or AISI 316L.
[0037] The first cladding material is for example an aluminium-magnesium alloy (Al-Mg), in particular EN AW-5083 also known as AG4 or EN AW-5019 also known as AG5.
[0038] The second cladding material is for example an aluminium-magnesium alloy, in particular EN AW-5754, also known as AG3, which contains for example about 3% by weight of magnesium.
[0039] As illustrated in FIGS. 3 and 4, the method for manufacturing the nuclear fuel element 2 includes the following steps: - providing a core 4, a frame 8 and a cover plate 12; - inserting the core 4 into the opening 10 of the frame 8; - a step of placing the cover plate 12 so as to sandwich the frame 8 for storing the core 4 between the cover plate 12 (see FIG. 4 ); - rolling the sandwich structure formed by the frame 8 and the core 4 housed between the cover plates 12 such that the cover plates 12 are fixed to the frame 8, the core 4 being sealed in the cladding 6 defined by the frame 8 and the cover plates 12 (see arrow R in Figure 4).
[0040] In a first substep, the uranium and each other constituent of the fissile material of the uranium alloy are melted in a furnace, for example an arc furnace, an induction furnace or a resistance furnace. If present, the above-mentioned additional elements may be added to the melt in this first substep.
[0041] In a second substep, the melt is poured into a mold to form an ingot.
[0042] In a third substep, the ingot is crushed to obtain a uranium alloy powder. Advantageously, the powder particles have an average size of less than 100 μm, for example between 40 μm and 70 μm. To determine the powder grain size, advantageously, laser grain size distribution can be used according to the NF ISO 13320 standard.
[0043] In a fourth substep, the powder is compressed to obtain a compact having, for example, the shape of a parallelepiped, advantageously having a width approximately equal to the final width of the core 4 in the nuclear fuel product 1.
[0044] The porosity of the compact is advantageously determined by weighing it first in air and then in water. During the latter measurement, the compact is completely immersed in water without any air bubbles being present on the suspension mechanism or on the compact. Since the theoretical density of the fissile material is then known, the porosity can be calculated.
[0045] Alternatively, in order to shorten the duration of the treatment and / or reduce the amount of residual porosity, the sintering substep can be carried out at a temperature between 400° C. and 900° C., advantageously under high pressure of between 200 and 1000 bar.
[0046] As an alternative to the fourth and fifth sub-steps, the powder may be cold sprayed onto the surface, preferably onto the surface of the cladding 6, advantageously at a temperature of 300-500° C. The cold spray method results in a dense and high quality deposit.
[0047] As an alternative to the second to fifth sub-steps, the powder may be cast directly in a mould having the size of the core 4, the additional elements, if any, being added in the first sub-step.
[0048] To allow for the sealing of the core 4 by the cladding 6, the core 4 is placed in a central opening 10 of a frame 8. The opening 10 has a contour that matches the contour of the core 4. The core 4 has, for example, a rectangular contour. The frame 8 extends along the sides of the core 4.
[0049] The frame 8 is preferably made integrally from a single continuous piece of material, such as by drilling a plate to provide the openings 10. Alternatively, the frame 8 may include multiple frame parts arranged around the core 4 to define the frame 8 extending along a side of the core 4.
[0050] After the core 4 is placed inside the frame 8, a cover plate 12 is placed on the opposing side of the frame 8 to form a sandwich structure 14 that includes the frame 8 containing the core 4 sandwiched between the two cover plates 12.
[0051] The two cover plates 12 can for example be obtained by folding a sheet as shown in figures 3 and 4. In such a case, the two cover plates 12 are made integrally in a single continuous piece of material. Alternatively, the two cover plates 12 are provided separately.
[0052] In Figure 4, the cladding 6 is sealed by rolling the sandwich structure 14 so that the cover plates 12 are secured to the frame 8. Each cover plate 12 is thus secured at its outer edge to the frame 8 and sealingly closes the frame 8.
[0053] The rolling is, for example, hot rolling, which is preferably carried out at a temperature of 300°C to 600°C, particularly 350°C to 450°C.
[0054] The rolling is preferably carried out along one rolling direction R in one or more passes along this rolling direction R.
[0055] The rolling step brings the core 4 to its final thickness and size and ensures proper sealing of the core 4 within the cladding 6 formed by the frame 8 and the top and bottom plates 12 .
[0056] Optionally, the rolling step comprises cold rolling of the nuclear fuel element 2 after the hot rolling. The cold rolling is carried out at a temperature strictly lower than that during the hot rolling. The cold rolling is preferably carried out at room temperature. The cold rolling is carried out, for example, to adjust the thickness and length of the core 4.
[0057] Optionally, the final planar dimensions of the nuclear fuel element 2 are adjusted by cutting the edges of the nuclear fuel element 2. The cutting is by any cutting technique such as press cutting, water cutting, laser cutting, etc.
[0058] Optionally, the final thickness of the nuclear fuel element 2 is adjusted, for example by machining, chemical etching, or the like.
[0059] Optionally, the nuclear fuel element 2 is subjected to a chemical cleaning according to known processes, for example to degrease the nuclear fuel element.
[0060] When the sandwich structure 14 is rolled in the rolling direction R, waves are formed in the core 4 which tend to propagate along the corresponding sides of the frame 8 towards the edges of the core 4 .
[0061] The appearance of the wave causes at least one of the cladding covers 12 to become excessively thin in contact with the wave, increasing the risk of a "dog-bone" effect occurring, which requires the nuclear fuel element 2 to be rebutted.
[0062] The size of the waves formed in the fissile material of the core 4 during rolling increases if the flow rate of the fissile material decreases, and the flow rate of the fissile material decreases if the density of the fissile material increases.
[0063] Therefore, increasing the uranium content of Core 4 by increasing its density tends to increase the risk of the deleterious dogbone effect occurring.
[0064] However, because the first cladding material of the frame 8 has a hardness strictly greater than that of the second cladding material of the cover plate 12, the frame 8 is more resistant to deformation than the cover plate 12 and therefore tends to limit the size of waves formed in the core 4 during rolling.
[0065] Moreover, the first cladding material of the frame 8, which has a hardness strictly lower than that of the core 4, is less resistant to deformation than the core 4, so that the risk of waves forming in the core 4 during rolling is limited.
[0066] Thus, a frame 8 made of a first cladding material that is harder than the material of the cover plate 12 and less hard than the core 4 can limit the risk of a detrimental dogbone effect occurring even if the uranium content of the core 4 is increased by increasing the density of the core 4.
[0067] The properties of the nuclear fuel element 2 are particularly important for use as a primary target in a nuclear reactor or as nuclear fuel for a research reactor for obtaining neutrons.
[0068] The density of the core 4 and the geometry and composition of the core 4, including the fissile material, are important for neutronics. The cladding material is important for the chemistry of the primary circuit of the reactor.
[0069] An increase in the uranium content in Core 4 with a limited risk of the occurrence of the dog-bone effect can be obtained using materials (fissile material, first cladding material and second cladding material), shapes, dimensions and manufacturing techniques already qualified for use in nuclear reactors.
[0070] Grinding the ingot into powder and subsequent sintering of the powder compacts allows one to obtain excellent homogeneity of the core 4 and to reduce its porosity to the desired level and thus to increase its density and uranium content.
[0071] Direct casting of the core 4 results in a non-porous core 4 .
[0072] Figure 5 shows the U 3 S 2 FIG. 1 illustrates an optical microscope view of a cross section of a first nuclear fuel element 2A having a core 4A made of AG3 and a frame 8A and a cover plate 12A made of the same material, namely AG3, such that the frame 8A and the cover plate 12A have the same hardness.
[0073] FIG. 6 is an optical microscope view of a cross section of a second nuclear fuel element 2B which differs from that of FIG. 5 only in that the frame 8B is made of AG5 which is harder than the cover plate 12B made of AG3.
[0074] Both the first nuclear fuel element 2A and the second nuclear fuel element 2B were operated under the same conditions and were manufactured using the same manufacturing method, which involves rolling a sandwich structure formed of a core inserted into a frame sandwiched between two cover plates.
[0075] 5 and 6 illustrate that the dog-bone effect appears on a first nuclear fuel element 2A, where the frame 8A and cover plate 12A are made of the same material, and that the dog-bone effect is limited or even avoided in a second nuclear fuel element 2B, where the frame 8A and cover plate 12A are made of different materials, where the material of the frame 8B is harder than the material of the cover plate 12A.
[0076] In particular, the first minimum thickness TA of the cover plate 12A of the first nuclear fuel element 2A is strictly smaller than the second minimum thickness TB of the cover plate 12B of the second nuclear fuel element 2B.
[0077] In this case the first minimum thickness was measured to be 204 μm and the second minimum thickness was measured to be 386 μm. [Explanation of symbols]
[0078] 2. Plate-shaped nuclear fuel elements 4 cores 6. Cladding 8 Frames 10 Opening 12 Cover plate 14 Sandwich structure
Claims
1. 1. A plate-shaped nuclear fuel element (2) comprising a core (4) made of fissile material and a cladding (6), the cladding including a frame (8) defining a central opening (10) for accommodating the core (4) and two cover plates (12) sandwiching the frame (8) and the core (4), the frame (8) being made of a metallic first cladding material and the cover plates (12) being made of a metallic second cladding material, the first cladding material having a hardness strictly greater than that of the second cladding material.
2. 2. A nuclear fuel element according to claim 1, wherein said hardness of the first cladding material is strictly lower than the hardness of the core (4).
3. 3. The nuclear fuel element of claim 1 or 2, wherein the first cladding material is an aluminum alloy or a zirconium alloy.
4. 4. The nuclear fuel element according to claim 1, wherein the first cladding material is an aluminum-magnesium alloy.
5. 5. The nuclear fuel element according to any one of claims 1 to 4, wherein the first cladding material is an AG4 or AG5 aluminium-magnesium alloy.
6. 6. The nuclear fuel element according to claim 1, wherein the second cladding material is an aluminum alloy or a zirconium alloy.
7. The nuclear fuel element according to any one of claims 1 to 6, wherein the second cladding material is an aluminium-magnesium alloy.
8. The nuclear fuel element according to any one of claims 1 to 7, wherein the second cladding material is an AG3 aluminium-magnesium alloy.
9. 9. A nuclear fuel element according to any one of claims 1 to 8, wherein the fissile material comprises at least one uranium alloy.
10. 10. The nuclear fuel element of any one of claims 1 to 9, wherein the fissile material comprises a uranium-silicon alloy, a uranium-molybdenum alloy, a uranium-aluminium alloy, a uranium-zirconium alloy, or a combination thereof.
11. The fissile material is U 3 S 2 11. A nuclear fuel element according to any one of claims 1 to 10, made of
12. The uranium content of the fissile material is 2.5 gU / cm 3 More specifically, strictly 4.8 gU / cm 3 12. A nuclear fuel element according to any one of claims 1 to 11, wherein said nuclear fuel element is greater than 100%.
13. The uranium content of the fissile material is 6.5 gU / cm 3 Less than 5.3 gU / cm 3 13. A nuclear fuel element according to any one of claims 1 to 12, wherein the
14. - providing a core (4), a frame (8) having an opening (10) and a cover plate (12); - inserting the core (4) into the opening (10) of the frame (8); - covering the frame (8) housing the core (4) with two cover plates (12) in such a way that the cover plates (12) sandwich the frame (8) and the core (4); - rolling the sandwich structure so that the cover plate (12) is fixed to the frame (8) and the core (4) is sealed within the cladding (6) defined by the frame (8) and the cover plate (12); A method for producing a plate-shaped nuclear fuel element according to any one of claims 1 to 13, comprising:
Citation Information
Patent Citations
Solid radiation source body
JP2007101439A
Method for producing nuclear fuel products with a high loading of LEU and corresponding nuclear fuel product
US20150340110A1
ELONGATE SiC FUEL ELEMENTS
US20210005334A1
Method of bonding the abutted edges of metal members
US3070880A
Plate-type nuclear fuel element
US3297543A