Polyimide film having high dimensional stability and method for producing same
By controlling the expansion coefficient ratio using specific dianhydride and diamine components, the polyimide film achieves both thermal and moisture stability, addressing the dimensional instability issues in existing films, suitable for flexible laminates and electronics.
Patent Information
- Application Number
- JP2024525721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-01
- Filing Date
- 2022-10-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-31
AI Technical Summary
Existing polyimide films face challenges in achieving both high thermal dimensional stability and moisture dimensional stability, with existing methods often prioritizing one over the other, leading to unpredictable dimensional changes due to humidity variations.
The ratio of hygroscopic expansion coefficient to thermal expansion coefficient is controlled to be between 0 and 2.5, using specific dianhydride and diamine components, such as biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, and paraphenylenediamine, to enhance both thermal and moisture stability.
The resulting polyimide film exhibits excellent thermal and moisture dimensional stability, suitable for flexible metal foil laminates and electronic components, with controlled dimensional changes under varying environmental conditions.
Smart Images

Figure 2024538306000001 
Figure 2024538306000002 
Figure 2024538306000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide film having high dimensional stability, and more particularly to a polyimide film having high dimensional stability against both heat and moisture, and a method for producing the same. [Background technology]
[0002] Polyimide (PI) is a polymeric material based on imide rings, which have excellent chemical stability along with a rigid aromatic main chain, and has the highest levels of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials. Polyimide films have been attracting attention as a material for a variety of electronic devices that require the above-mentioned properties. An example of a microelectronic component to which polyimide films are applied is a flexible thin circuit board having a high degree of circuit integration so as to accommodate the trend toward lighter and smaller electronic products. Polyimide films are particularly widely used as insulating films for thin circuit boards.
[0003] The thin circuit board generally has a structure in which a circuit including a metal foil is formed on an insulating film, and such a thin circuit board is broadly called a flexible metal foil clad laminate (Flexible Metal Foil Clad Laminate), and when a thin copper plate is used as the metal foil, it is more narrowly called a flexible copper clad laminate (FCCL). Examples of methods for producing flexible metal foil laminates include (i) a casting method in which polyamic acid, a precursor of polyimide, is cast or coated onto a metal foil and then imidized, (ii) a metallizing method in which a metal layer is directly formed on a polyimide film by sputtering, and (iii) a lamination method in which a polyimide film and a metal foil are bonded together by heat and pressure via a thermoplastic polyimide. In particular, the metallizing method is a method for producing flexible metal foil laminates by sputtering a metal such as copper on a polyimide film having a thickness of, for example, 20 to 38 μm, and sequentially depositing a tie layer and a seed layer. This method is advantageous in forming ultra-fine circuits with a circuit pattern pitch of 35 μm or less, and is widely used to manufacture flexible metal foil laminates for COF (chip on film).
[0004] Polyimide films used in flexible metal foil laminates using the metallizing method must have high dimensional stability. Usually, dimensional stability is measured by thermal dimensional stability represented by the thermal expansion coefficient, but dimensional stability against moisture represented by the hygroscopic expansion coefficient, which is no less important than thermal dimensional stability, is becoming increasingly important. That is, there is an increasing demand for polyimide films that are excellent in both thermal dimensional stability and moisture dimensional stability. However, when a polyimide film is actually designed to have a structure with a low thermal expansion coefficient and high thermal dimensional stability, a problem of low moisture dimensional stability has arisen. Therefore, there is a strong demand for a polyimide film that is capable of achieving both high thermal dimensional stability and high dimensional stability against moisture. The matters described in the above background art are intended to aid in understanding the background of the invention, and may include matters that are not prior art already known to those having ordinary skill in the art to which this technology pertains. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Republic of Korea Patent Publication No. 2021-0057936 Summary of the Invention [Problem to be solved by the invention]
[0006] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a polyimide film which simultaneously has high dimensional stability against both heat and moisture. However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0007] In order to achieve the above object, one aspect of the present invention is a method for manufacturing a thermoplastic elastomer having a ratio of expansion coefficients represented by the following formula 1, which is more than 0 and 2.5 or less: A polyimide film is provided. <Expression 1> Expansion coefficient ratio = Hygroscopic expansion coefficient (ppm / RH%) / Thermal expansion coefficient (ppm / ℃) Another aspect of the present invention is a method for producing a laminate comprising: A flexible metal foil laminate is provided. Yet another aspect of the present invention includes a flexible metal foil laminate, Provide electronic components. Effect of the Invention
[0008] The present invention provides a polyimide film having excellent thermal dimensional stability and moisture dimensional stability by controlling the composition ratio and reaction ratio of dianhydride and diamine components. Such polyimide films are applicable to various fields requiring polyimide films with excellent dimensional stability, such as flexible metal foil laminates produced by a metallizing method or electronic parts including such flexible metal foil laminates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that corresponds to the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to explain his / her invention in the best possible way. Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not fully represent the technical ideas of the present invention, and that there may be various equivalents and modifications that can replace them at the time of this application. In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0010] As used herein, "dianhydride acid" is intended to include precursors or derivatives thereof which may not technically be dianhydrides but which nevertheless must react with a diamine to form a polyamic acid which is then converted back to a polyimide. As used herein, "diamine" is intended to include its precursors or derivatives. Although these may not technically be diamines, they should nevertheless react with the dianhydrides to form polyamic acids which are then converted back to polyimides. Whenever an amount, concentration, or different value or parameter is given herein as a range, a preferred range or a list of upper and lower preferred values, it should be understood to specifically disclose all ranges formed by any pair of any upper range limit or preferred value, and any lower range limit or preferred value, regardless of whether a range is otherwise disclosed.
[0011] Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range. In the polyimide film according to an embodiment of the present invention, the ratio of the expansion coefficients represented by the following Formula 1 may be more than 0 and not more than 2.5. <Expression 1> Expansion coefficient ratio = Hygroscopic expansion coefficient (ppm / RH%) / Thermal expansion coefficient (ppm / ℃) Preferably, the ratio of the expansion coefficients represented by the formula 1 may be 1.0 or more and 2.5 or less. A polyimide film having a value of more than 2.5 in the above formula 1 has a large dimensional change due to moisture and a small dimensional change due to heat, so that it may be difficult to predict the dimensional change of the polyimide film. That is, if the humidity changes due to a change in the surrounding environment, the range of dimensional change of the polyimide film becomes large, so that it may be difficult to control the dimension due to heat.
[0012] In one embodiment, the polyimide film may have a thermal expansion coefficient of 1 ppm / ° C. or more and 7 ppm / ° C. or less, and a hygroscopic expansion coefficient of 3 ppm / RH % or more and 10 ppm / RH % or less. Preferably, the thermal expansion coefficient is 5.5 ppm / °C or less, and the hygroscopic expansion coefficient is 9 ppm / RH% or less, and more preferably, the thermal expansion coefficient is 5.0 ppm / °C or less, and the hygroscopic expansion coefficient is 8 ppm / RH% or less.
[0013] In one embodiment, the polyimide film is obtained by an imidization reaction of a polyamic acid solution including a dianhydride component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), oxydiphthalic anhydride (ODPA), and benzophenonetetracarboxylic dianhydride (BTDA), and a diamine component including two or more selected from the group consisting of paraphenylenediamine (PPD), m-tolidine, oxydianiline (ODA), and 1,3-bisaminophenoxybenzene (TPE-R). The polyimide film is obtained by imidizing a polyamic acid solution containing a dianhydride component consisting of two or more selected from the group consisting of biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, and benzophenonetetracarboxylic dianhydride, and a diamine component including two or more selected from the group consisting of paraphenylenediamine, m-tolidine, and oxydianiline.
[0014] On the other hand, based on 100 mol% of the total content of the dianhydride acid components, the content of the biphenyltetracarboxylic dianhydride may be 60 mol% or less, the content of the pyromellitic dianhydride may be 40 mol% or more and 60 mol% or less, and the content of the benzophenonetetracarboxylic dianhydride may be 60 mol% or less. Preferably, the content of the pyromellitic dianhydride may be less than 53 mol % and the content of the benzophenone tetracarboxylic dianhydride may be 50 mol % or less, based on 100 mol % of the total content of the dianhydride acid components.
[0015] In addition, based on 100 mol% of the total content of the diamine components, the content of the paraphenylenediamine may be 50 mol% or more and 95 mol% or less, the content of the m-tolidine may be 55 mol% or less, and the content of the oxydianiline may be 25 mol% or less. Preferably, based on 100 mol% of the total content of the diamine components, the content of the paraphenylenediamine may be 55 mol% or more and 90 mol% or less, the content of the m-tolidine may be 50 mol% or less, and the content of the oxydianiline may be 20 mol% or less. In addition, when paraphenylenediamine and m-tolidine are used as the diamine components, the content of the paraphenylenediamine may be 50 mol % or more and 70 mol % or less, and the content of the m-tolidine may be 30 mol % or more and 45 mol % or less, based on 100 mol % of the total content of the diamine components.
[0016] The paraphenylenediamine of the present invention is a rigid monomer, and by increasing the content of paraphenylenediamine, the synthesized polyimide has a more linear structure, which contributes to improving the mechanical properties of the polyimide. Furthermore, m-tolidine has a methyl group that exhibits hydrophobicity, and contributes to the low moisture absorption characteristic related to the dimensional stability of the polyimide film against moisture. The polyimide chain derived from the biphenyltetracarboxylic dianhydride of the present invention has a structure called a charge transfer complex (CTC), i.e., a regular linear structure in which an electron donor and an electron acceptor are located close to each other, and intermolecular interactions are strengthened.
[0017] Such a structure has the effect of preventing hydrogen bonding with moisture, thereby reducing the moisture absorption rate and maximizing the effect of reducing the moisture absorption of the polyimide film, which affects the dimensional stability against moisture. In addition, pyromellitic dianhydrides are preferred in that they are dianhydride acid components having a relatively rigid structure and can impart suitable elasticity to the polyimide film. In order for the polyimide film to have excellent dimensional stability, the content ratio of the dianhydride acid is important. For example, as the content ratio of biphenyltetracarboxylic dianhydride decreases, it becomes difficult to expect a low moisture absorption rate due to the CTC structure, and the dimensional stability against moisture also decreases.
[0018] Additionally, biphenyltetracarboxylic dianhydride and benzophenonetetracarboxylic dianhydride contain two benzene rings corresponding to the aromatic moiety, whereas pyromelitic dianhydride contains one benzene ring corresponding to the aromatic moiety. An increase in the content of pyromellitic dianhydride in the dianhydride acid component can be understood as an increase in the imide groups in the molecule when the same molecular weight is used as a standard, and this can be understood as a relative increase in the ratio of imide groups derived from the pyromellitic dianhydride in the polyimide polymer chain compared to the imide groups derived from biphenyltetracarboxylic dianhydride and benzophenonetetracarboxylic dianhydride. In other words, the increase in the pyromellitic dianhydride content is seen as a relative increase in imide groups in the polyimide film as a whole, which leads to a low moisture absorption rate and a high resistance to moisture. Therefore, it is difficult to expect high dimensional stability.
[0019] Conversely, if the content ratio of the pyromellitic dianhydride is decreased, the components having a relatively rigid structure are decreased, and the elasticity of the polyimide film may be decreased below a desired level. For this reason, if the content of the biphenyl tetracarboxylic dianhydride and the benzophenone tetracarboxylic dianhydride exceeds the above range, or if the content of the pyromellitic dianhydride is below the above range, the dimensional stability of the polyimide film may be reduced. Conversely, if the content of the pyromellitic dianhydride exceeds the above range, the dimensional stability of the polyimide film may also be adversely affected. In one embodiment, the ratio of the mol% of the pyromellitic dianhydride to the mol% of the paraphenylenediamine (mol% of pyromellitic dianhydride / mol% of paraphenylenediamine) may be 0.5 or more and 0.8 or less.
[0020] In the present invention, the polyamic acid can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize it; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the dianhydride component to polymerize it; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and the remaining dianhydride component is added successively thereto, so that the diamine component and the dianhydride component are polymerized in substantially equimolar amounts; (4) A method in which a dianhydride component is placed in a solvent, a part of the components in the diamine compound is mixed in a ratio of 95 to 105 mol % relative to the reactive components, and then another dianhydride component is added, followed by the remaining diamine component, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (5) A method of forming a first composition by reacting some diamine components and some dianhydride acid components in a solvent so that one of them is in excess, and forming a second composition by reacting some diamine components and some dianhydride acid components in another solvent so that one of them is in excess, and then mixing the first and second compositions to complete polymerization, in which if the diamine component is in excess when the first composition is formed, the dianhydride acid component is in excess in the second composition, and if the dianhydride acid component is in excess in the first composition, the diamine component is in excess in the second composition, and the first and second compositions are mixed to polymerize so that the total diamine components and dianhydride acid components used in these reactions are substantially equimolar.
[0021] In one embodiment, a method for producing a polyimide film according to the present invention includes the steps of: (a) a step of producing a polyamic acid by polymerizing a dianhydride component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), oxydiphthalic anhydride (ODPA), and benzophenonetetracarboxylic dianhydride (BTDA) in an organic solvent and a diamine component including two or more selected from the group consisting of paraphenylenediamine (PPD), m-tolidine, oxydianiline (ODA), and 1,3-bisaminophenoxybenzene (TPE-R); (b) imidizing the polyamic acid. In the present invention, the polymerization method of the polyamic acid may be defined as a random polymerization method, and the polyimide film prepared from the polyamic acid of the present invention prepared in the above-mentioned process is preferably applicable in terms of maximizing the effect of the present invention of improving dimensional stability. However, in the above polymerization method, the length of the repeating unit in the polymer chain is relatively short as described above, so that there may be a limit to the excellent properties of the polyimide chain derived from the dianhydride acid component. Therefore, the polymerization method of polyamic acid that can be particularly preferably used in the present invention is the block polymerization method.
[0022] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited, and any solvent that dissolves the polyamic acid can be used, but an amide-based solvent is preferable. Specifically, the organic solvent may be an organic polar solvent, more specifically, an aprotic polar solvent, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as needed. In one example, the organic solvent that can be particularly preferably used is N,N-dimethylformamide or N,N-dimethylacetamide. In addition, in the process for producing the polyamic acid, a filler may be added for the purpose of improving various properties of the film such as sliding properties, thermal conductivity, corona resistance, loop hardness, etc. The filler to be added is not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0023] The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm. If the particle size is below this range, the modifying effect is unlikely to be achieved, whereas if it exceeds this range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced. The amount of the filler to be added is not particularly limited, and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, relative to 100 parts by weight of polyimide.
[0024] If the amount of the filler added is less than this range, the modifying effect of the filler is unlikely to be exhibited, and if the amount exceeds this range, the mechanical properties of the film may be significantly damaged. The method of adding the filler is not particularly limited, and any known method may be used. In the production method of the present invention, the polyimide film is produced by a thermal imidization method and a chemical imidization method. Alternatively, the imidation layer may be produced by a hybrid imidation method in which a thermal imidization method and a chemical imidization method are performed in parallel. The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared dryer. The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600°C, specifically, by heat-treating the gel film at 200 to 500°C, more specifically, by heat-treating the gel film at 300 to 500°C, to imidize the amic acid groups present in the gel film.
[0025] However, even during the process of forming the gel film, a portion of the amic acid (approximately 0.1 mol % to 10 mol %) is imidized, and therefore the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which also falls within the category of the thermal imidization method. In the case of the chemical imidization method, a polyimide film can be produced using a dehydrating agent and an imidization agent by methods known in the art. As an example of the composite imidization method, a polyimide film can be produced by adding a dehydrating agent and an imidization agent to a polyamic acid solution, heating the solution at 80 to 200°C, preferably 100 to 180°C, partially curing and drying the solution, and then heating the solution at 200 to 400°C for 5 to 400 seconds. The present invention provides a flexible metal foil laminate comprising the above-mentioned polyimide film and an electrically conductive metal foil. The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment, the metal foil may be, for example, copper or a copper alloy, stainless steel or an alloy thereof, nickel or a nickel alloy (including alloy 42), aluminum or an aluminum alloy.
[0026] In general flexible metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and are also preferably usable in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer. In the present invention, the thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient functionality depending on the application. The flexible metal foil laminate according to the present invention may have a structure in which a metal foil is laminated on at least one surface of the polyimide film. EXAMPLES
[0027] The functions and effects of the present invention will be described in more detail below through specific manufacturing examples and examples of the present invention, however, these manufacturing examples and examples are presented only as examples of the present invention and do not limit the scope of the invention.
[0028] Manufacturing example: Manufacturing of polyimide film The polyimide film of the present invention can be produced by the following conventional method known in the art: First, the above-mentioned dianhydride acid and diamine component are reacted in an organic solvent to obtain a polyamic acid solution. In this case, the solvent is generally an aprotic polar solvent such as an amide solvent. A solvent such as N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methyl-pyrrolidone, or a combination thereof can be used. The dianhydride and diamine components may be added in the form of powder, lump, or solution. It is preferable to add them in the form of powder at the beginning of the reaction to proceed with the reaction, and then add them in the form of a solution to control the polymerization viscosity.
[0029] The resulting polyamic acid solution is mixed with an imidization catalyst and a dehydrating agent and applied to a support. Examples of the catalyst used include tertiary amines (e.g., isoquinoline, β-picoline, pyridine, etc.), and examples of the dehydrating agent include, but are not limited to, anhydrous acids. In addition, examples of the support used include, but are not limited to, glass plates, aluminum foils, circular stainless steel belts, stainless steel drums, etc. The film coated on the support is gelled on the support by dry air and heat treatment. The gelled film is separated from the support and heat treated to complete drying and imidization. After the heat treatment, the film is heat treated under a certain tension to remove residual stress inside the film generated during the film formation process.
[0030] Specifically, 500ml of DMF was added to a reactor equipped with a stirrer and nitrogen inlet / outlet pipes while injecting nitrogen, and the temperature of the reactor was set to 30°C, after which biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), benzophenonetetracarboxylic dianhydride (BTDA), paraphenylenediamine (PPD), m-tolidine, and oxydianiline (ODA) were added in the adjusted composition ratio and in the specified order and completely dissolved. Thereafter, the temperature of the reactor was raised to 40°C under a nitrogen atmosphere, and stirring was continued for 120 minutes to produce polyamic acid with a primary reaction viscosity of 1,500cP. The polyamic acid thus produced was stirred so that the final viscosity became 100,000 to 120,000 cP. The catalyst and dehydrating agent were added to the prepared final polyamic acid with the adjusted contents, and then a polyimide film was produced using an applicator.
[0031] Examples and Comparative Examples As shown in Table 1 below, the contents of the dianhydride acid component and the diamine component in Examples 1 to 5 and Comparative Examples 1 to 7 were adjusted to produce polyimide films according to the Production Examples. [Table 1] The coefficient of thermal expansion (CTE), coefficient of hydroscopic expansion (CHE), and ratio of coefficients of expansion (CHE / CTE) of the prepared polyimide film were measured and are shown in Table 2 below. [Table 2]
[0032] (1) Measurement of thermal expansion coefficient The coefficient of thermal expansion (CTE) was measured using a TA thermomechanical analyzer, model Q400. The polyimide film was cut to a width of 4 mm and a length of 20 mm, and then heated from room temperature to 400°C at a rate of 10°C / min under a nitrogen atmosphere while applying a tension of 0.05 N. The temperature was then increased from room temperature to 400°C at a rate of 10°C / min, and then cooled again at a rate of 10°C / min to measure the slope in the range from 50°C to 200°C. The measured thermal expansion coefficient is the average value of the thermal expansion coefficients in the MD and TD directions of the polyimide film.
[0033] (2) Measurement of hygroscopic expansion coefficient The coefficient of moisture expansion (CHE) was measured by adjusting the humidity to 3% RH with a minimum load applied so as not to loosen the polyimide film (approximately 1 g for a 25 mm x 150 mm sample), allowing the sample to absorb moisture until it was completely saturated, and then measuring the dimensions.The humidity was then adjusted to 90% RH, and the sample was allowed to absorb moisture until it was saturated, and the dimensions were measured.From these two results, the dimensional change rate was measured at a humidity of 90% RH per a relative humidity difference of 87%. The measured moisture expansion coefficient is the average value of the moisture expansion coefficients in the MD and TD directions of the polyimide film. As a result of the measurements, the polyimide films of Examples 1 to 5 exhibited the following characteristics: the ratio of the expansion coefficients was 0 or more and 2.5 or less, the thermal expansion coefficient was 1 ppm / °C or more and 7 ppm / °C or less, and the moisture expansion coefficient was 3 ppm / RH% or more and 10 ppm / RH% or less. In contrast, in Comparative Example 1, which contained only one type of paraphenylenediamine as the diamine component, the thermal expansion coefficient was very low compared to the hygroscopic expansion coefficient, and the ratio of the expansion coefficients was very large. Moreover, in Comparative Example 2, in which only biphenyltetracarboxylic dianhydride and paraphenylenediamine were used as the dianhydride acid component and diamine component, respectively, the thermal expansion coefficient value was large.
[0034] On the other hand, in Comparative Example 3, which contained only one type of pyromellitic dianhydride as the dianhydride acid component, the values of the hygroscopic expansion coefficient and the thermal expansion coefficient all became large. Furthermore, in Comparative Examples 4 and 5, which contained only one type of oxydianiline as the diamine component, the values of the hygroscopic expansion coefficient and the thermal expansion coefficient all became very large. On the other hand, compared to Examples 2 and 3, which had the same dianhydride acid components and content ratios and diamine components, Comparative Examples 6 and 7, in which the contents of m-tolidine and paraphenylenediamine were adjusted, showed significantly reduced thermal expansion coefficient values and increased expansion coefficient ratios, respectively. Therefore, the polyimide films of Examples 1 to 5 produced within the appropriate range of the present application were excellent in both thermal dimensional stability and dimensional stability against moisture, but it was confirmed that when the appropriate range of the present application is exceeded, it is difficult to achieve both thermal dimensional stability and dimensional stability against moisture.
[0035] In other words, it was confirmed that the polyimide film having excellent dimensional stability due to compatibility between thermal dimensional stability and dimensional stability against moisture and satisfying all of the various conditions applicable to various fields of application is the polyimide film manufactured within the appropriate range of the present application. The examples of the polyimide film and the method for manufacturing the polyimide film of the present invention are merely preferred examples that enable a person having ordinary skill in the art to easily carry out the present invention, and the present invention is not limited to the above-mentioned examples, and the scope of the present invention is not limited by these examples. Therefore, the true technical scope of the present invention must be determined by the technical ideas of the appended claims. In addition, it is obvious to a person skilled in the art that various substitutions, modifications and changes are possible within the scope of the present invention, and it is obvious that the parts that can be easily modified by a person skilled in the art are also included in the scope of the present invention. [Industrial Applicability]
[0036] The present invention provides a polyimide film having excellent thermal dimensional stability and moisture dimensional stability by controlling the composition ratio and reaction ratio of dianhydride and diamine components. Such polyimide films are applicable to various fields requiring polyimide films with excellent dimensional stability, such as flexible metal foil laminates produced by a metallizing method or electronic parts including such flexible metal foil laminates.
Claims
1. The ratio of the expansion coefficients represented by the following formula 1 is more than 0 and 2.5 or less. Polyimide film. <Formula 1> Expansion coefficient ratio = Hygroscopic expansion coefficient (ppm / RH%) / Thermal expansion coefficient (ppm / °C)
2. The thermal expansion coefficient is 1 ppm / °C or more and 7 ppm / °C or less, The moisture absorption expansion coefficient is 3 ppm / RH% or more and 10 ppm / RH% or less. The polyimide film according to claim 1 .
3. 2. The polyimide film according to claim 1, obtained by imidization reaction of a polyamic acid solution containing a dianhydride acid component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), oxydiphthalic anhydride (ODPA), and benzophenonetetracarboxylic dianhydride (BTDA), and a diamine component including two or more selected from the group consisting of paraphenylenediamine (PPD), m-tolidine, oxydianiline (ODA), and 1,3-bisaminophenoxybenzene (TPE-R).
4. The polyamic acid solution is obtained by imidizing a polyamic acid solution containing a dianhydride component consisting of two or more selected from the group consisting of biphenyltetracarboxylic dianhydride, pyromelitic dianhydride, and benzophenonetetracarboxylic dianhydride, and a diamine component containing two or more selected from the group consisting of paraphenylenediamine, m-tolidine, and oxydianiline. The polyimide film according to claim 3.
5. With respect to 100 mol% of the total content of the dianhydride acid components, the content of the biphenyl tetracarboxylic dianhydride is 60 mol% or less, the content of the pyromellitic dianhydride is 40 mol% or more and 60 mol% or less, and the content of the benzophenone tetracarboxylic dianhydride is 60 mol% or less. The polyimide film according to claim 4.
6. the content of the paraphenylenediamine is 50 mol % or more and 95 mol % or less, the content of the m-tolidine is 55 mol % or less, and the content of the oxydianiline is 25 mol % or less, based on 100 mol % of the total content of the diamine components; The polyimide film according to claim 4.
7. The ratio of the mol% of the pyromellitic dianhydride to the mol% of the paraphenylenediamine (mol% of pyromellitic dianhydride / mol% of paraphenylenediamine) is 0.5 or more and 0.8 or less; The polyimide film according to claim 3.
8. A laminate comprising the polyimide film according to any one of claims 1 to 7 and an electrically conductive metal foil. Flexible metal foil laminate.
9. The flexible metal foil laminate of claim 8, Electronic components.
Citation Information
Patent Citations
Novel polyimide copolymer and its production
JP1988314240A
Production of polyimide copolymer film
JP1988314242A
Tetrapolyimide film that incorporates benzophenone tetracarboxylic acid two anhydride
JP1992299885A
Polyimide film and substrate for electric and electronic apparatus using same
JP2001072781A
New polyimide composition and polyimide film
JP2003155344A