Modified bismaleimide prepolymer, resin composition and use of resin composition

JP2024539527AActive Publication Date: 2024-10-29SHENGYI TECH SUZHOU +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023542749
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-11
Filing Date
2023-03-31
Publication Date
2024-10-29
Estimated Expiration
2043-03-31

AI Technical Summary

Benefits of technology

【0025】 本発明で提供される1つ又は複数の技術的解決手段は、少なくとも以下の技術効果又は利点を有する。 本発明で提供される変性ビスマレイミドプレポリマーは、ビスマレイミド化合物と異なるアミノ当量のアミノ有機シリコーン樹脂との反応によって、ビスマレイミド化合物の反応性及び脆性が改善され、また、アミノ有機シリコーン樹脂とビスマレイミド化合物の質量を制御することで、樹脂組成物のレオロジー反応ウィンドウが効果的に調節され、樹脂組成物の圧着において反応が速すぎるため基材にシワ又は白い模様という欠陥が発生するリスクが低減される。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539527000001_ABST
    Figure 2024539527000001_ABST
Patent Text Reader

Abstract

The present invention provides a modified bismaleimide prepolymer, a resin composition and its use, the modified bismaleimide being obtained by reacting a prepolymer bismaleimide compound with an aminoorganic silicone resin A and an aminoorganic silicone resin B, wherein the amino equivalent Ea A is the amino equivalent Ea of the amino organic silicone resin B B Unlike the above, the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (5 to 80): 100. In the present invention, the reactivity of the bismaleimide compound is improved, and the rheological properties in high temperature lamination are controlled when the modified bismaleimide prepolymer is used in the field of substrate materials such as package substrates.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of electronic materials, in particular to modified bismaleimide prepolymers, resin compositions containing modified bismaleimide prepolymers, and uses of the resin compositions. [Background technology]

[0002] In recent years, electronic devices have been developed toward smaller size and higher performance, and printed circuit boards have been continuously improved in wiring density and integration, which has resulted in higher requirements for the heat resistance and reliability of copper-clad boards. In particular, in semiconductor package boards, warping occurs due to the difference in thermal expansion coefficient between the chip and the organic substrate during package assembly.

[0003] Bismaleimide resin cured products have excellent properties such as high temperature resistance, humidity and heat resistance, high elastic modulus, low CTE, and high strength, and are particularly suitable for use as matrix resins for IC package substrates and substrate-like PCBs. However, they also have disadvantages such as high brittleness and poor processability, which limit their large-scale use.

[0004] In the prior art, in order to improve the above problems present in the cured product of bismaleimide resin, silicone rubber powder is introduced into bismaleimide resin, and the introduction of silicone rubber powder can improve the water absorption and toughness of the cured product of bismaleimide resin to a certain extent, but silicone rubber powder has low density, is prone to aggregation, and has low dispersibility, so it floats to the upper layer of the bismaleimide resin adhesive liquid, causing phase separation, and causing problems such as interlayer delamination in the cured product of bismaleimide resin. In addition, there is a prior art in which silicone oil is directly added to bismaleimide resin, but if the silicone oil does not react completely during lamination of the cured product, it is very likely to seep out of the system, which affects production processability and seriously affects the overall performance of the final cured product. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a modified bismaleimide prepolymer, a resin composition containing a modified bismaleimide prepolymer, and use of the resin composition. The modified bismaleimide prepolymer is modified by reaction of a bismaleimide compound with an amino organic silicone resin having a different amino equivalent, and by controlling the masses of the amino organic silicone resin and the bismaleimide compound, the problem of high brittleness of the bismaleimide resin is improved, the reactivity of the bismaleimide resin and the rheological properties of the resin during high temperature lamination are effectively controlled, and the processing performance of the resin composition is improved. [Means for solving the problem]

[0006] In order to achieve one of the above objects of the invention, one embodiment of the present invention provides a silicone rubber composition obtained by reacting a bismaleimide compound with an aminoorganic silicone resin A and an aminoorganic silicone resin B, the aminoorganic silicone resin A having an amino equivalent Ea A is the amino equivalent Ea of the amino organic silicone resin B B The present invention provides a modified bismaleimide prepolymer, in which the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (5 to 80):100, unlike the above.

[0007] As a further improvement of one embodiment of the present invention, the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (20-50):100.

[0008] As a further improvement of one embodiment of the present invention, the mass ratio of the amino organic silicone resin A to the amino organic silicone resin B is 1:(2-30).

[0009] As a further refinement of one embodiment of the present invention, both the amino organosilicone resin A and the amino organosilicone resin B also include the following structure:

[0010] [ka]

[0011] In the formula, R and R′ are C1 to C5 alkyl groups, and m is an integer of 1 to 30.

[0012] In a further improvement of one embodiment of the present invention, the side chains in said amino organosilicone resin A and / or said amino organosilicone resin B contain at least one amino group.

[0013] As a further improvement of one embodiment of the present invention, the terminals in the aminoorganosilicone resin A and / or the aminoorganosilicone resin B contain at least one amino group.

[0014] One embodiment of the present invention comprises, by weight: (a) 30 to 100 parts of a modified bismaleimide prepolymer; (b) 3 to 50 parts of a cyanate resin; (c) 5 to 60 parts of an elastomer; wherein the modified bismaleimide prepolymer is the modified bismaleimide prepolymer described above.

[0015] As a further improvement of one embodiment of the present invention, the cyanate resin is selected from one or more of bisphenol A cyanate resin, bisphenol F cyanate resin, bisphenol S type cyanate resin, bisphenol E type cyanate resin, bisphenol M type cyanate resin, double bond-containing cyanate resin, phosphorus-containing cyanate resin, phenol type cyanate resin, biphenyl type cyanate resin, naphthalene ring type cyanate resin, dicyclopentadiene type cyanate resin.

[0016] As a further improvement of one embodiment of the present invention, the cyanate resin is a naphthalene type cyanate resin or / and a phenol type cyanate resin as shown in the following structure:

[0017] [ka]

[0018] Here, R6 is a hydrogen atom, a methyl group, or an ethyl group, and n2 is an integer of 1 to 10.

[0019] [ka]

[0020] Here, n is an integer from 1 to 10.

[0021] In a further refinement of an embodiment of the present invention, the elastomer is selected from at least one of a styrene-based elastomer, a methacrylate-based elastomer, and an organosilicone-based elastomer.

[0022] A further improvement of one embodiment of the present invention further includes a silane coupling agent and a dispersing agent.

[0023] As a further improvement of one embodiment of the present invention, the silane coupling agent is an epoxy silane coupling agent, the dispersant is a phosphate ester-based dispersant and / or a modified polyurethane-based dispersant, and the weight ratio of the silane coupling agent to the dispersant is 2:1 to 10:1.

[0024] One embodiment of the present invention further provides the use of the resin composition described above for prepregs, laminates, insulating thin films, insulating boards, copper-clad boards, circuit boards and electronic devices. Effect of the Invention

[0025] One or more technical solutions provided in the present invention have at least the following technical effects or advantages: In the modified bismaleimide prepolymer provided by the present invention, the reactivity and brittleness of the bismaleimide compound are improved by reacting the bismaleimide compound with an amino organic silicone resin having a different amino equivalent. In addition, by controlling the mass of the amino organic silicone resin and the bismaleimide compound, the rheological reaction window of the resin composition can be effectively adjusted, and the risk of defects such as wrinkles or white patterns occurring on the substrate due to too fast a reaction during compression of the resin composition can be reduced. [Brief description of the drawings]

[0026] [Figure 1] FIG. 2 is a rheology curve diagram of Example 2 of the present invention and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will be described in detail below in conjunction with specific embodiments, but these embodiments do not limit the present invention, and any changes to reaction conditions, reactants or raw material amounts made by those skilled in the art based on these embodiments are within the protection scope of the present invention.

[0028] The embodiment of the present invention is obtained by reacting a bismaleimide compound with an aminoorganic silicone resin A and an aminoorganic silicone resin B, and the amino equivalent Ea A is the amino equivalent Ea of amino organic silicone resin B B The present invention provides a modified bismaleimide prepolymer, in which the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (5 to 80):100, unlike the above.

[0029] Preferably, the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (20-50:100).

[0030] Furthermore, the mass ratio of the amino organic silicone resin A to the amino organic silicone resin B is 1:(2 to 30).

[0031] The specific reaction between the bismaleimide compound, the amino organic silicone resin A, and the amino organic silicone resin B is as follows. First, the bismaleimide compound is reacted with aminoorganic silicone resin A at 60-90°C for 0.5-1.5 hours, and then the temperature is raised to 90-130°C, and aminoorganic silicone resin B is added and the reaction is continued for 0.5-2 hours.

[0032] Preferably, at least one of aminophenol, carboxylic acid, and carboxylic anhydride is added in an amount of 0.1 to 10 parts by weight during the reaction, and any of the phenolic hydroxyl group, carboxyl group, and acid anhydride group in the aminophenol, carboxylic acid, or carboxylic anhydride reacts with the bismaleimide compound, thereby improving the reactivity.

[0033] Furthermore, the amino equivalent Ea of the amino organic silicone resin A A is 100g / mol≦Ea A ≦500g / mol, and the amino equivalent Ea of amino organic silicone resin B B The amino equivalent is 500g / mol <Ea B ≦1600 g / mol.

[0034] Preferably, the absolute value of the difference in amino equivalent between the organosilicone resin A and the organosilicone resin B is 100 g / mol to 600 g / mol.

[0035] Both aminoorganosilicone resin A and aminoorganosilicone resin B also contain the following structure:

[0036] [ka]

[0037] In the formula, R and R′ are C1 to C5 alkyl groups, and m is an integer of 1 to 30.

[0038] Furthermore, at least one amino group is contained in the side chain in the amino organosilicone resin A and / or the amino organosilicone resin B.

[0039] Furthermore, the terminal of the amino organic silicone resin A and / or the amino organic silicone resin B contains at least one amino group.

[0040] Furthermore, the bismaleimide compound may be selected from at least one of the following structures:

[0041] [ka]

[0042] [ka]

[0043] [ka]

[0044] [ka]

[0045] Here, R2 is a hydrogen atom, a methyl group, or an ethyl group, R1 is a methylene group or an ethylene group, and n is an integer of 1 to 10.

[0046] [ka]

[0047] [ka]

[0048] Here, n is an integer from 1 to 10.

[0049] [ka]

[0050] Here, n is an integer from 1 to 10.

[0051] [ka]

[0052] Here, n is an integer from 1 to 10.

[0053] [ka]

[0054] [ka]

[0055] Here, R is a hydrogen atom, a methyl group, or an ethyl group, and n is an integer of 1 to 10.

[0056] The present invention comprises, by weight: (a) 30 to 100 parts of a modified bismaleimide prepolymer; (b) 3 to 50 parts of a cyanate resin; (c) 5 to 60 parts of an elastomer; wherein the modified bismaleimide prepolymer is the modified bismaleimide prepolymer described above.

[0057] Further, the cyanate resin is selected from one or more of bisphenol A type cyanate resin, bisphenol F type cyanate resin, bisphenol S type cyanate resin, bisphenol E type cyanate resin, bisphenol M type cyanate resin, double bond-containing cyanate resin, phosphorus-containing cyanate resin, phenol type cyanate resin, biphenyl type cyanate resin, naphthalene ring type cyanate resin, and dicyclopentadiene type cyanate resin.

[0058] Preferably, the cyanate resin is a naphthalene ring type cyanate resin or / and a phenol type cyanate resin represented by the following structure:

[0059] [ka]

[0060] Here, R6 is a hydrogen atom, a methyl group, or an ethyl group, and n2 is an integer of 1 to 10.

[0061] [ka]

[0062] Here, n is an integer from 1 to 10.

[0063] Furthermore, the elastomer is selected from at least one of a styrene-based elastomer, a methacrylate-based elastomer, and an organic silicone-based elastomer.

[0064] Among them, the styrene-based elastomer is selected from H1041, H1043, H1051, H1052, H1053, H1221, P1500, P2000, M1911 or M1913 manufactured by Asahi Kasei Corporation of Japan, and 8004, 8006, 8076, 8104, V9827, 2002, 2005, 2006, 2007, 2104, 7125, 4033, 4044, 4055, 4077 or 4099 manufactured by Kuraray Co., Ltd.

[0065] The methacrylates are selected from M51, M52, M22 or D51N from Arkema, LA-2330 from Kuraray, SG-P3 series or SG-80 series from Nagase.

[0066] The organic silicone elastomer may be selected from X-40-2670, R-170S, X-40-2705, X-40-2701, KMP-600, KMP-605, and X-52-7030 manufactured by Shin-Etsu Chemical Co., Ltd., and AY-42-119, EP-2600, EP-2601, EP-2720, TMS-2670, EXL-2315, and EXL-2655 manufactured by Dow Co., Ltd.

[0067] Furthermore, the resin composition further contains 0.01 to 5 parts by weight of a catalyst, which is at least one of an imidazole catalyst, a pyridine catalyst, and an organometallic salt catalyst.Preferably, the catalyst is at least one of 4-dimethylaminopyridine, 2-methylimidazole, 2-methyl-4-ethylimidazole, 2-phenylimidazole, modified imidazole, and zinc caprylate.

[0068] The modified imidazole is as shown in the following structure:

[0069] [ka]

[0070] In the formula, R3, R4, R5 and R6 are the same or different and are each a methyl group, an ethyl group or a tert-butyl group; B is a methylene group, an ethylene group, a dimethylmethylene group, a sulfide group or a sulfonyl group; and P200F50 manufactured by JER can be used.

[0071] [ka]

[0072] In the formula, R3, R4, R5 and R6 are the same or different and each is a methyl group, an ethyl group or a tert-butyl group; A is a methylene group, an ethylene group, a dimethylmethylene group, a sulfide group, a sulfonyl group or an aromatic hydrocarbon group; G8009L manufactured by Daiichi Kogyo can be used.

[0073] Furthermore, the resin composition further contains 20 to 200 parts by weight of a filler. The filler includes an inorganic filler, an organic filler, and a composite filler. Among them, the inorganic filler is selected from at least one of fused silica, crystalline silica, spherical silica, hollow silica, aluminum hydroxide, aluminum oxide, talc powder, aluminum nitride, boron nitride, silicon carbide, barium sulfate, barium titanate, strontium titanate, calcium carbonate, calcium silicate, mica, and glass fiber powder. The organic filler is selected from at least one of polytetrafluoroethylene powder, polyphenylene sulfide powder, and polyethersulfone powder.

[0074] Preferably, the filler is spherical silica, aluminum oxide or aluminum hydroxide, more preferably spherical silica.

[0075] The content of the filler is preferably 30 to 150 parts by weight.

[0076] Furthermore, the filler is surface-treated with a silane coupling agent, and the silane coupling agent is at least one of an amino silane coupling agent, a carbon-carbon double bond-containing silane coupling agent, or an epoxy silane coupling agent. Preferably, the silane coupling agent is selected from one or more of Shin-Etsu Chemical Co., Ltd.'s product number KBM-573, Dow Corning Co., Ltd.'s product number Z-6883, Shin-Etsu Chemical Co., Ltd.'s product number KBM-1003, and Shin-Etsu Chemical Co., Ltd.'s product number KBM-1403.

[0077] Furthermore, the resin composition further contains a silane coupling agent and a dispersant, the silane coupling agent is an epoxy silane coupling agent, the dispersant is a phosphate ester and / or a modified polyurethane, and the weight ratio of the silane coupling agent to the dispersant is 2:1 to 10:1.

[0078] Furthermore, the resin composition further contains 5 to 50 parts by weight of a flame retardant, based on 100 parts by weight of the resin composition. The flame retardant is selected from a bromine-based flame retardant, a phosphorus-based flame retardant, a nitrogen-based flame retardant, an organic silicone flame retardant, an organic metal salt flame retardant, and the like.

[0079] Preferably, the flame retardant is selected from phosphazenes with product numbers SPB-100, modified phosphazenes with product numbers BP-PZ, PP-PZ, SPCN-100, SPV-100 and SPB-100L, all of which are manufactured by Nippon Otsuka Chemical Co., Ltd.

[0080] In addition, a dye may be further added to the resin composition, and a fluorescent dye or a black dye may be selected. The fluorescent dye may be specifically a pyrazoline-based compound. The black dye may be specifically a liquid or powdered carbon black, a pyridine complex, an azo complex, a quinone-based compound, zirconium nitride, titanium oxide, titanium nitride, black talc powder, cobalt chromium chromium metal oxide, azine or phthalocyanine, etc.

[0081] The present invention further provides the use of the above resin composition for prepreg, laminate, insulating thin film, insulating plate, circuit board and electronic device, the specific description is as follows:

[0082] The present invention further provides a prepreg comprising a reinforcing material and the aforementioned resin composition. The prepreg can be produced by dissolving the resin composition in a solvent to form an adhesive liquid, immersing the reinforcing material in the adhesive liquid, removing the reinforcing material from the immersion, and baking and drying the reinforcing material at 100 to 180°C for 1 to 15 minutes.

[0083] Here, the solvent is selected from at least one of acetone, butanone, toluene, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, benzene, toluene, xylene, and cyclohexane.

[0084] The reinforcing material is at least one selected from natural fibers, organic synthetic fibers, organic fabrics, and inorganic fabrics. Preferably, glass fiber cloth is used as the reinforcing material. Of the glass fiber cloths, it is preferable to use open filament fiber cloth or plain weave fiber cloth. The glass fiber cloth is preferably E glass fiber cloth, S glass fiber cloth, or Q glass fiber cloth.

[0085] In addition, when glass fiber cloth is used as the reinforcing material, the glass fiber cloth is chemically treated with a coupling agent to improve the interfacial bond between the resin composition and the glass fiber cloth. The coupling agent is preferably an epoxy silane coupling agent or an amino silane coupling agent to provide high water resistance and heat resistance.

[0086] An embodiment of the present invention further provides a laminate including one of the above prepregs and a metal foil provided on at least one surface of the prepreg, or including a combination sheet obtained by stacking a plurality of the above prepregs on one another, and a metal foil provided on at least one surface of the combination sheet.

[0087] The laminate is manufactured by the following method. Either one or both surfaces of one prepreg are covered with metal foil, or at least two prepregs are stacked to form a combined sheet, one or both surfaces of the combined sheet are covered with metal foil, and the combined sheet is subjected to hot-press molding to obtain a metal foil laminate. The hot-press pressure conditions are 0.2-2 MPa and 150-250°C for 2-4 hours.

[0088] Preferably, the metal foil is selected from copper foil or aluminum foil, and the thickness of the metal foil is 5 microns, 8 microns, 12 microns, 18 microns, 35 microns or 70 microns.

[0089] An embodiment of the present invention further provides an insulating board comprising at least one of the prepregs described above.

[0090] An embodiment of the present invention further provides a thin insulating film comprising a carrier film and the aforementioned resin composition applied thereon, the thin insulating film having a significantly improved thermal index.

[0091] The insulating thin film is produced by the following method: the aforementioned resin composition is dissolved in a solvent to form an adhesive liquid, the adhesive liquid is then applied onto a carrier film, and the carrier film to which the adhesive liquid has been applied is heated and dried to obtain an insulating thin film.

[0092] The aforementioned solvent is selected from at least one of acetone, butanone, toluene, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, benzene, toluene, xylene, and cyclohexane.

[0093] The carrier film is selected from at least one of a PET film, a PP film, a PE film, and a PVC film.

[0094] An embodiment of the present invention further provides a circuit board including one or more of the prepreg, laminate, insulating plate, and insulating thin film described above.

[0095] An embodiment of the present invention further provides an electronic device including the aforementioned circuit board, in which the heat resistance of the circuit board is greatly improved, so that the safety of the electronic device is significantly improved.

[0096] The technical solutions of the present application are further illustrated below in conjunction with some specific synthesis examples and comparative examples.

[0097] Synthesis Example 1 Modified bismaleimide prepolymer Y1 In a beaker, 100 g of bismaleimide resin (BMI-2300, manufactured by Yamato Chemical Co., Ltd.) and 10 g of aminoorganic silicone resin A (amino equivalent weight 450 g / mol, DOWSIL TMBY 16-853) and an appropriate amount of organic solvent are added, and the mixture is reacted at 80°C for 60 minutes. The temperature is raised to 100°C, and 25 g of aminoorganic silicone resin B (amino equivalent weight 800 g / mol, X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd.) is added, the reaction is continued for 90 minutes, and the mixture is discharged to obtain modified bismaleimide prepolymer Y1.

[0098] Synthesis Example 2 Modified bismaleimide prepolymer Y2 100 g of bismaleimide resin (MIR-3000, manufactured by Nippon Kayaku Co., Ltd.), 5 g of amino organic silicone resin A (amino equivalent 430 g / mol, KF-8010, manufactured by Shin-Etsu Chemical Co., Ltd.) and an appropriate amount of organic solvent are added to a beaker, and the mixture is reacted at 80°C for 60 minutes. The temperature is then raised to 100°C, and 30 g of amino organic silicone resin B (amino equivalent 800 g / mol, X-22-161A, manufactured by Shin-Etsu Chemical Co., Ltd.) is added. The reaction is continued for 90 minutes, and the mixture is discharged to obtain a modified bismaleimide prepolymer Y2.

[0099] Synthesis Example 3 Modified bismaleimide prepolymer Y3 In a beaker, 100 g of bismaleimide resin (BMI-2300, manufactured by Yamato Chemical Co., Ltd.) and 10 g of aminoorganic silicone resin A (amino equivalent weight 450 g / mol, DOWSIL TM BY 16-853), 1 g of aminophenol and an appropriate amount of organic solvent are added, and the mixture is reacted at 80°C for 60 minutes. The temperature is raised to 100°C, and 25 g of aminoorganic silicone resin B (amino equivalent weight 800 g / mol, X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd.) is added, and the reaction is continued for 90 minutes. The mixture is then discharged to obtain a modified bismaleimide prepolymer Y3.

[0100] Synthesis Example 4 Modified bismaleimide prepolymer Y4 Into a beaker, 100 g of bismaleimide resin (manufactured by Nippon Kayaku Co., Ltd., BMI-2300), 10 g of amino organic silicone resin A (amino equivalent 430 g / mol, manufactured by Shin-Etsu Chemical Co., Ltd., KF-8010), 1 g of aminophenol and an appropriate amount of organic solvent are added, and the mixture is reacted at 80°C for 60 minutes. The temperature is then raised to 100°C, and 25 g of amino organic silicone resin B (amino equivalent 1500 g / mol, manufactured by Shin-Etsu Chemical Co., Ltd., X-22-161B) is further added, the reaction is continued for 100 minutes, and the mixture is discharged to obtain a modified bismaleimide prepolymer Y4.

[0101] Comparative Synthesis Example 1 Modified bismaleimide prepolymer Y5 In a beaker, 100 g of bismaleimide resin (Daiwa Kasei Co., Ltd., BMI-2300) and 35 g of amino organic silicone resin A (amino equivalent weight 450 g / mol, DOWSIL TM BY 16-853) and an appropriate amount of organic solvent are added, and the mixture is reacted at 100°C for 120 minutes, and then discharged to obtain modified bismaleimide prepolymer Y5.

[0102] Comparative Synthesis Example 2 Modified bismaleimide prepolymer Y6 In a beaker, 100 g of bismaleimide resin (MIR-3000, manufactured by Nippon Kayaku Co., Ltd.), 35 g of amino organic silicone resin B (amino equivalent 800 g / mol, X-22-161A, manufactured by Shin-Etsu Chemical Co., Ltd.), 1 g of aminophenol, and an appropriate amount of organic solvent are added, and the mixture is reacted at 100°C for 120 minutes, and then discharged to obtain a modified bismaleimide prepolymer Y6.

[0103] According to the data in Table 1, the corresponding solids are weighed out, and each weighed solid is adjusted with a solvent so that the solid content of the adhesive liquid is 60%. The adhesive liquid is applied to an E-glass fiber cloth, and after it is wetted, it is left in a 160°C air drying oven and baked for 3 to 6 minutes to produce a prepreg.

[0104] The prepreg is cut to 300 x 300 mm, one electrolytic copper foil is placed on each side of the prepreg, stacked into a certain stacking structure, and fed into a vacuum press for pressure bonding to obtain a metal foil laminate (or copper clad laminate). The specific performance test is shown in Table 2.

[0105] [Table 1]

[0106] [Table 2]

[0107] The prepregs and copper-clad laminates produced in all of the above Examples 1 to 5 and Comparative Examples 1 and 2 are subjected to performance tests.

[0108] 1) The glass transition temperature is measured by DMA (thermomechanical analysis) at a heating rate of 10℃ / min. 2) For the PCT 2HR water absorption measurement, three samples of 10 cm x 10 cm and 0.40 mm thickness were taken from which the metal foil on both sides had been removed, dried at 100°C for 2 hours, weighed and designated as W1, and then treated in a pressure cooker tester at 121°C and 2 atm for 2 hours, weighed and designated as W2, and the water absorption was calculated as (W2-W1) / W1 x 100%. 3) X / Y coefficient of thermal expansion (CTE) is measured by TMA (thermomechanical analysis), the heating rate is 10℃ / min, and the test temperature range is 30~100℃. 4) Secondary defects in appearance are tested using the standard method specified in IPC-TM-650, and the presence or absence of defects such as wrinkles and white patterns in the base material is judged by visual inspection or the slice method.

[0109] As can be seen from the above experimental data, Examples 1 to 3 have excellent performance, such as high Tg, low water absorption, low CTE value, and high appearance quality. Among them, Example 1 has a higher Tg value and a lower CTE than Comparative Example 1, and Example 2 has a higher Tg value and a lower CTE than Comparative Example 2.

[0110] In addition, from the rheological curves of Comparative Example 2 and Example 2 in FIG. 1, it can be seen that the rheological window of Example 2 is wider and the minimum melt viscosity is lower, which indicates that the reaction of the resin is slower and contributes to the control of processability.

[0111] It should be understood that although the present specification has been described in terms of embodiments, each embodiment does not include only one independent technical solution, and such description in the specification is merely for the purpose of clarification, and a person skilled in the art should regard the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by a person skilled in the art.

[0112] The above detailed description is merely a specific description of possible embodiments of the present invention, and does not limit the protection scope of the present invention. Any equivalent embodiments or modifications that do not depart from the technical spirit of the present invention shall be included in the protection scope of the present invention.

Claims

1. The amino equivalent of the amino organic silicone resin A is Ea obtained by reacting a bismaleimide compound with an amino organic silicone resin A and an amino organic silicone resin B. A is the amino equivalent Ea of the amino organic silicone resin B B and wherein the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (5 to 80):

100.

2. The modified bismaleimide prepolymer according to claim 1, characterized in that the ratio of the sum of the masses of the amino organic silicone resin A and the amino organic silicone resin B to the mass of the bismaleimide compound is (20 to 50):

100.

3. The modified bismaleimide prepolymer according to claim 1 or 2, characterized in that the mass ratio of the amino organic silicone resin A to the amino organic silicone resin B is 1:(2 to 30).

4. Both the aminoorganosilicone resin A and the aminoorganosilicone resin B also contain the following structure: 【Chemistry 1】 2. The modified bismaleimide prepolymer according to claim 1, wherein R and R' are C1 to C5 alkyl groups, and m is an integer of 1 to 30.

5. 2. The modified bismaleimide prepolymer according to claim 1, wherein a side chain in the aminoorganosilicone resin A and / or the aminoorganosilicone resin B contains at least one amino group.

6. 2. The modified bismaleimide prepolymer according to claim 1, wherein the terminal of said aminoorganosilicone resin A and / or said aminoorganosilicone resin B contains at least one amino group.

7. By weight, (a) 30 to 100 parts of a modified bismaleimide prepolymer; (b) 3 to 50 parts of a cyanate resin; (c) 5 to 60 parts of an elastomer; 2. A resin composition comprising the above-mentioned components, wherein the modified bismaleimide prepolymer is the modified bismaleimide prepolymer according to claim 1.

8. The resin composition according to claim 7, characterized in that the cyanate resin is selected from one or more of bisphenol A type cyanate resin, bisphenol F type cyanate resin, bisphenol S type cyanate resin, bisphenol E type cyanate resin, bisphenol M type cyanate resin, double bond-containing cyanate resin, phosphorus-containing cyanate resin, phenol type cyanate resin, biphenyl type cyanate resin, naphthalene ring type cyanate resin, and dicyclopentadiene type cyanate resin.

9. The cyanate resin is a naphthalene-type cyanate resin or / and a phenol-type cyanate resin represented by the following structure: 【Chemistry 2】 where R6 is a hydrogen atom, a methyl group, or an ethyl group; 2 is an integer from 1 to 10, 【Chemistry 3】 The resin composition according to claim 8, wherein N is an integer of 1 to 10.

10. 8. The resin composition according to claim 7, wherein the elastomer is at least one selected from the group consisting of styrene-based elastomers, methacrylate-based elastomers, and organic silicone-based elastomers.

11. The resin composition according to claim 7, further comprising a silane coupling agent and a dispersant.

12. The resin composition according to claim 11, characterized in that the silane coupling agent is an epoxy silane coupling agent, the dispersant is a phosphate ester-based dispersant and / or a modified polyurethane-based dispersant, and the weight ratio of the silane coupling agent to the dispersant is 2:1 to 10:

1.

13. Use of the resin composition according to claim 7 for prepregs, laminates, insulating thin films, insulating boards, copper-clad boards, circuit boards and electronic devices.

Citation Information

Patent Citations

  • Liquid adhesive for electronic part and adhesive tape using the same

    JP1997176593A

  • Liquid adhesive for electronic part and adhesive tape

    JP1997328665A

  • Thermosetting resin composition, and prepreg, film with resin, laminate, multilayer printed wiring board and semiconductor package using the same