Surface treatment method for rare earth magnetic powder, extruded rare earth magnetic material and its manufacturing method

The surface treatment method for rare earth magnetic powders, involving weak oxidation, phosphatization, and coupling, addresses the oxidation susceptibility of these powders, resulting in improved magnetic properties and stability through a more robust protective film.

JP2024539777AInactive Publication Date: 2024-10-31HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022542205
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-27
Filing Date
2021-11-05
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Rare earth magnetic powders, particularly those with fine particle sizes, are highly susceptible to oxidation during the granulation process, leading to poor magnetic properties and potential ignition, and existing surface treatments like coupling and phosphoric acid complex solutions fail to form stable protective films effectively.

Method used

A surface treatment method involving weak oxidation with a specific pH-adjusted weak acid solution, followed by phosphatization and coupling with a silane coupling agent, enhances the formation of a complete and stable phosphide film on the magnetic powder surface, improving oxidation resistance and magnetic properties.

Benefits of technology

The method significantly improves the oxidation resistance and magnetic properties of rare earth magnetic materials, ensuring high performance and stability during injection granulation by forming a more complete phosphide film and coupling protective layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539777000001
    Figure 2024539777000001
  • Figure 2024539777000002
    Figure 2024539777000002
  • Figure 2024539777000003
    Figure 2024539777000003
Patent Text Reader

Abstract

The present invention provides a surface treatment method for rare earth magnetic powder, an extruded rare earth magnetic material and a manufacturing method thereof. The surface treatment method includes the following steps: Step S1: Add the rare earth magnetic powder to a weak acid solution to perform a weak oxidation treatment on the surface of the rare earth magnetic powder, and form a weakly oxidized magnetic powder, where the weak acid in the weak acid solution is an inorganic weak acid with an acidity coefficient pKa value of more than 4.5 and / or an organic weak acid with an acidity coefficient of more than 1.0; Step S2: Use a phosphorizing solution to perform a phosphorization treatment on the weakly oxidized magnetic powder to form a phosphorized magnetic powder; Step S3: Mix the phosphorized magnetic powder with a coupling agent to perform a coupling treatment on the phosphorized magnetic powder, and then dry to obtain a surface-treated rare earth magnetic powder. The present invention solves the problem that the rare earth magnetic powder in the prior art has poor oxidation resistance, resulting in poor magnetic properties of the extruded rare earth magnetic material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of rare earth permanent magnets, in particular to a surface treatment method for rare earth magnetic powder, an extruded rare earth magnetic material and a method for producing the same. [Background technology]

[0002] Injection magnets are made by melt blending organic polymer resins and magnetic powders and extruding them into granules. Commonly used polymer resins include polyamide PA6, PA66, PA12, PA11, PA612 series, as well as polyphenylene sulfide PPS and polyether ether ketone PEEK, which have higher temperature resistance. Magnetic powders include low-performance ferrite (FeO) and high-performance rare earth magnetic powders such as neodymium iron boron (Nd-Fe-B), samarium iron nitrogen (Sm-Fe-N), and samarium cobalt (Sm-Co). With the development of the market, the requirements for performance and product miniaturization are becoming higher, and the demand for injected rare earth magnetic materials is becoming greater.

[0003] However, unlike ferrite powder, rare earth magnetic powder itself belongs to alloy powder, and requires a relatively high temperature in the granulation process, so that the magnetic powder is very easily oxidized, which significantly reduces the performance.

[0004] Especially rare earth powders with fine powder particle size, such as anisotropic SmFeN powder. In the milling process, in order to improve the magnetic properties of anisotropic SmFeN powder, manufacturers often cause the existence of a lot of fine powder by adjusting the powder particle size, and the particle size of these fine powders is often crushed to 1-2 μm, and these powders are very easy to oxidize, and at the same time, they may even spontaneously ignite in exposed high-temperature air.

[0005] Therefore, in order to manufacture high-performance extruded rare earth magnet materials, it is generally necessary to first perform surface treatment on the rare earth magnetic powder, which provides a protective layer on the surface of the magnetic powder, reduces oxidation during the processing of the magnetic powder, and protects its magnetic properties. At present, many companies use the coupling treatment method to treat the surface of the magnetic powder, which can improve the binding with the binder PA or PPS, and protect the magnetic powder inside the binder from oxidation after the binder dissolves and coats the magnetic powder in the twin-screw extruder, but there is a high possibility that the magnetic powder will be oxidized before the binder completely coats the magnetic powder.

[0006] Chinese patent CN201510454107.8 also mentions a method of treating rare earth SmFeN magnetic powder by immersing the magnetic powder in a coupling agent and phosphoric acid complex solution. The phosphoric acid solution can form a certain phosphorus film on the powder surface, thereby improving the high temperature resistance of the magnetic powder and protecting the magnetic powder from oxidation during the granulation process. The phosphoric acid forms phosphate crystal nuclei on the active points of the magnetic powder surface, which then continue to grow and form a stable phosphorus film.

[0007] The quality and integrity of the phosphide film are closely correlated with the number of surface active points of the magnetic powder. Simply immersing the magnetic powder in a phosphoric acid solution will result in very weak surface active points, making it difficult to form a stable, high-quality phosphide film. In addition, there is a high risk of the treated rare earth magnetic powder being oxidized in the subsequent high-temperature granulation process.

[0008] Based on the above reasons, it is necessary to provide a new surface treatment method for rare earth magnetic powder so as to have better oxidation resistance and further improve the magnetic properties of the rare earth magnetic material after extrusion. Summary of the Invention [Problem to be solved by the invention]

[0009] The main objective of the present invention is to provide a surface treatment method for rare earth magnetic powder, an extruded rare earth magnetic material, and a manufacturing method thereof, in order to solve the problem that the oxidation resistance of rare earth magnetic powder in the prior art is weak, and therefore the magnetic properties of the extruded rare earth magnetic material are poor. [Means for solving the problem]

[0010] In order to achieve the above-mentioned object, according to one aspect of the present invention, a surface treatment method for rare earth magnetic powder is provided, the method including step S1 of adding rare earth magnetic powder to a weak acid solution to perform a weak oxidation treatment on the surface of the rare earth magnetic powder to form a weakly oxidized magnetic powder, where the weak acid in the weak acid solution is an inorganic weak acid having an acidity coefficient pKa value greater than 4.5 and / or an organic weak acid having an acidity coefficient greater than 1.0, step S2 of performing a phosphorization treatment on the weakly oxidized magnetic powder using a phosphorization liquid to form a phosphorized magnetic powder, and step S3 of mixing the phosphorized magnetic powder with a coupling agent to perform a coupling treatment on the phosphorized magnetic powder, followed by drying to obtain the rare earth magnetic powder after surface treatment.

[0011] Furthermore, the weak acid is one or more of oxalic acid, acetic acid and carbonic acid, preferably, the pH value of the weak acid solution is 5-7, preferably, the pH value of the weak acid solution is adjusted using ethanol, and preferably, the volume ratio of the weak acid solution to the rare earth magnetic powder is 1.5-3:1.

[0012] Furthermore, in step S1, after the rare earth magnetic powder is added to the weak acid solution, first ultrasonic vibration is applied to perform a weak oxidation treatment, and preferably, the power of the first ultrasonic vibration is 1500 to 2500 W and the time is 2 to 5 minutes.

[0013] Furthermore, the phosphorizing solution is a zinc-based or manganese-based phosphorizing solution, and preferably, after the weak oxidation treatment is completed, the phosphorizing solution is directly added to the system containing the weakly oxidized magnetic powder until the pH value of the system reaches 4 to 5, so as to perform the phosphorizing treatment, followed by the second ultrasonic vibration, and preferably, the power of the second ultrasonic vibration is 1000 to 1500 W and the time is 10 to 15 minutes.

[0014] Furthermore, the coupling agent is a silane coupling agent, preferably one or more of KH550, KH560, and KH792. Preferably, after the phosphorization treatment is completed, the coupling agent is directly added to the system containing the phosphorized magnetic powder to perform the coupling treatment, followed by the third ultrasonic vibration. Preferably, the amount of the coupling agent added is 0.5-1% of the weight of the rare earth magnetic powder. Preferably, the power of the third ultrasonic vibration is 1200-2000W, and the time is 10-15min. Preferably, the drying process adopts vacuum drying, and the drying temperature is 70-90°C.

[0015] Furthermore, the rare earth magnetic powder is one or more of homogeneous neodymium iron boron magnetic powder, heterogeneous neodymium iron boron magnetic powder, homogeneous samarium iron nitrogen magnetic powder, heterogeneous samarium iron nitrogen magnetic powder, and samarium cobalt magnetic powder.

[0016] According to another aspect of the present invention, there is further provided a method for producing an extruded rare earth magnetic material, the method including the steps of: employing the above-mentioned surface treatment method to perform a surface treatment on a rare earth magnetic powder; and mixing the surface-treated rare earth magnetic powder with a binder, followed by extrusion granulation to obtain an extruded rare earth magnetic material.

[0017] Furthermore, the binder is one or more of nylon, polyphenylene sulfide, and polyether ether ketone, and preferably the amount of the binder used is 8 to 15% by weight of the rare earth magnetic powder.

[0018] Furthermore, the extrusion granulation process adopts a twin-screw extruder, and the temperature of the extrusion granulation is 200-310°C.

[0019] According to another aspect of the present invention there is further provided an extruded rare earth magnetic material, said material being produced by the above method. Effect of the Invention

[0020] The present invention provides a surface treatment method for rare earth magnetic powder, which is to carry out weak oxidation treatment, phosphorus treatment and coupling treatment on rare earth magnetic powder in sequence. The weak oxidation treatment is the basis of phosphorus treatment and coupling treatment, which can improve the number of active sites on the surface of rare earth magnetic powder, and dissolve the insoluble ferrous iron and iron compound impurities on the surface of rare earth magnetic powder, and convert it into weak acid ferrous iron.

[0021] By carrying out the weak oxidation treatment followed by the phosphorization treatment and coupling treatment, a more complete and higher quality phosphorization film and coupling protective layer can be formed on the surface of the rare earth magnetic powder, so that the treated rare earth magnetic powder has better oxidation resistance, and can protect the rare earth magnetic powder from oxidation before and during the subsequent extrusion granulation with the binder, and the obtained extruded rare earth magnetic material has correspondingly better magnetic properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] In addition, the embodiments and features of the embodiments of the present application may be combined with each other if there is no contradiction. The present invention will be described in detail below with reference to the embodiments.

[0023] As explained in the Background section, the oxidation resistance of the rare earth magnetic powder in the prior art is weak, so the magnetic properties of the rare earth magnetic material after injection are poor.

[0024] In order to solve the above problems, the present invention provides a surface treatment method for rare earth magnetic powder, the method comprising the steps of: Step S1: adding the rare earth magnetic powder to a weak acid solution to perform a weak oxidation treatment on the surface of the rare earth magnetic powder, thereby forming a weakly oxidized magnetic powder, in which the weak acid in the weak acid solution is an inorganic weak acid having an acidity coefficient pKa value of more than 4.5 and / or an organic weak acid having an acidity coefficient of more than 1.0; Step S2 of performing a phosphorization process on the weakly oxidized magnetic powder using a phosphorization liquid to form a phosphorized magnetic powder; and step S3 of mixing the phosphide magnetic powder with a coupling agent so as to subject the phosphide magnetic powder to a coupling treatment, followed by drying to obtain a surface-treated rare earth magnetic powder.

[0025] The present invention provides a surface treatment method for rare earth magnetic powder, which is to carry out weak oxidation treatment, phosphorus treatment and coupling treatment on rare earth magnetic powder in sequence. The weak oxidation treatment is the basis of phosphorus treatment and coupling treatment, which can improve the number of active sites on the surface of rare earth magnetic powder, and dissolve the insoluble ferrous iron and iron compound impurities on the surface of rare earth magnetic powder, and convert it into weak acid ferrous iron.

[0026] The number of active sites is increased, and the number of sites involved in the phosphorization reaction and coupling reaction on the surface of rare earth magnetic powder can be increased, thereby improving the degree of phosphorization in the phosphorization treatment process and making the coupling treatment more complete. The weak acid ferrous iron formed by dissolving impurities such as ferrous iron and iron compounds approaches or remains on the surface of rare earth magnetic powder, which can play a certain role as phosphorization nuclei in the phosphorization process and is also favorable for the growth and formation of the phosphorization film. Both of the above two reasons contribute to improving the integrity and quality of the phosphorization film, and the coupling protection layer is also more complete accordingly.

[0027] Therefore, by carrying out the weak oxidation treatment followed by the phosphorization treatment and coupling treatment, a more complete and higher quality phosphorization film and coupling protective layer can be formed on the surface of the rare earth magnetic powder, thereby providing the treated rare earth magnetic powder with better oxidation resistance, and protecting the rare earth magnetic powder from oxidation before and during the subsequent extrusion granulation with the binder, and the resulting extruded rare earth magnetic material has correspondingly better magnetic properties.

[0028] In addition, compared with the method of mixing phosphorizing solution and coupling agent, the present invention sequentially carries out phosphorizing and coupling treatment after weak oxidation treatment, so that the growth of phosphorizing film is more complete, and the corresponding coupling protective layer is also more complete, which is helpful to improve the oxidation resistance of rare earth magnetic powder. At the same time, this operation is helpful to improve the compatibility and binding force of rare earth magnetic powder with polymer materials in the later kneading and granulation process.

[0029] In short, the surface treatment method provided by the present invention can be used to treat rare earth magnetic powder to significantly improve its oxidation resistance, and accordingly produce extruded rare earth magnetic materials with high performance and high stability.

[0030] The weak acid is an inorganic weak acid having an acidity coefficient pKa value greater than 4.5 and / or an organic weak acid having an acidity coefficient greater than 1.0, which can increase the number of active sites on the surface of the magnetic powder as much as possible without damaging the rare earth magnetic powder itself, and in order to make the weak oxidation treatment more effective, in a preferred embodiment, the weak acid is one or more of oxalic acid, acetic acid and carbonic acid.

[0031] Preferably, the pH value of the weak acid solution is 5-7. Controlling the pH value of the weak acid solution within the above range helps to control the stability of the weak oxidation treatment, and also promotes the weak oxidation treatment more thoroughly, which has a further promoting effect on the growth quality and integrity of the subsequent phosphorus film and coupling protective layer. In addition, in order to more thoroughly disperse and coat the rare earth magnetic powder in the weak acid solution, it is preferable to adjust the pH value of the weak acid solution to 5-7 using ethanol as a pH adjuster. Specific solvents in the weak acid solution include, but are not limited to, one or more of isopropyl alcohol, ethanol, and deionized water.

[0032] The amount of the weak acid solution added may be any amount sufficient to sufficiently cover the rare earth magnetic powder, and in order to further improve the treatment effect, in a preferred embodiment, the volume ratio of the weak acid solution to the rare earth magnetic powder is 1.5 to 3:1.

[0033] As mentioned above, the weak oxidation treatment can also dissolve the ferrous iron and iron compound impurities on the surface of the rare earth magnetic powder and turn them into weak acid ferrous iron. These weak acid ferrous irons function as phosphorization nuclei to some extent in the process of phosphorization treatment, but in order to fully exert this function, in a preferred embodiment, in step S1, the rare earth magnetic powder is added to the weak acid solution and then subjected to the first ultrasonic vibration so as to perform the weak oxidation treatment. The ultrasonic vibration can make the weak acid ferrous iron more uniformly distributed on the surface of the weakly oxidized magnetic powder, which further makes the growth of the phosphorization film more uniform and complete, and also helps to improve the efficiency of the phosphorization treatment.

[0034] At the same time, the magnetic powder is lightly rubbed during the ultrasonic vibration, which can further improve the shape of the magnetic powder at a micro level, making it closer to a sphere, thereby improving the fluidity of the subsequent product, improving the orientation of the extruded product, and further improving the magnetic properties of the extruded rare earth magnetic material. Preferably, the power of the first ultrasonic vibration is 1500-2500W, and the time is 2-5min. At this power and time, the above functions are more fully exerted. The preferred power is 2000W.

[0035] In a preferred embodiment, the phosphide solution is a zinc-based or manganese-based phosphide solution (purchased from Ersm). By adopting the above phosphide solution, the weakly oxidized magnetic powder can be subjected to a more thorough phosphide treatment, and the quality of the formed phosphide film is higher, more complete and more stable. More preferably, a zinc-based phosphide solution (e.g. Ersm BW-231 special zinc-manganese phosphide solution) is adopted as the phosphide solution.

[0036] In order to improve the effect of the phosphorization process, in a preferred embodiment, after the weak oxidation treatment is completed, the phosphorization solution is directly added to the system containing the weakly oxidized magnetic powder until the pH value of the system reaches 4-5, and then the second ultrasonic vibration is performed to perform the phosphorization treatment. In a specific implementation process, there is no break between the second ultrasonic vibration treatment and the first ultrasonic vibration treatment, and the phosphorization solution can be added and the phosphorization treatment can be performed in such a continuous vibration state, which is more effective. Preferably, the power of the second ultrasonic vibration is 1000-1500W, and the time is 10-15min, and the more preferred power is 1500W.

[0037] The above coupling agent can be of the commonly used type in the field, and preferably, the coupling agent is a silane coupling agent. The silane coupling agent can form a better coupling protective film on the surface of the phosphorized magnetic powder, which can further improve the fusion between the magnetic powder and the binder in the subsequent injection granulation process with the binder, so that the material distribution is more uniform, and the magnetic properties of the final material are better. More preferably, the coupling agent is one or more of KH550, KH560, and KH792.

[0038] In order to improve the effect of coupling treatment, in a preferred embodiment, after the phosphorization treatment is completed, a coupling agent is directly added to the system containing the phosphorized magnetic powder, so as to carry out coupling treatment, and then the third ultrasonic vibration is carried out. In the specific implementation process, there is no break between the third ultrasonic vibration and the second ultrasonic vibration, and the coupling treatment can be carried out in such a continuous vibration state, and the formed coupling protective layer is more uniform and complete.

[0039] Preferably, the amount of coupling agent added is 0.5-1% of the weight of the rare earth magnetic powder. It is advantageous to control the amount of coupling agent used within the above range and distribute it sufficiently on the surface of the phosphorized magnetic powder, thereby improving the oxidation resistance of the magnetic powder and the fusion between the binder in the injection process, so that the material finally obtained by granulation has better magnetic properties and stability. Preferably, the power of the third ultrasonic vibration is 1200-2000W, the time is 10-15min, and the preferred power is 1500W. Preferably, the drying process adopts vacuum drying, and the drying temperature is 70-90°C.

[0040] The above-mentioned surface treatment method of the present invention is applicable to many types of rare earth magnetic powder, including but not limited to one or more of homogeneous neodymium iron boron magnetic powder (Nd-Fe-B), heterogeneous neodymium iron boron magnetic powder (Nd-Fe-B), homogeneous samarium iron nitrogen magnetic powder (Sm-Fe-N), heterogeneous samarium iron nitrogen magnetic powder (Sm-Fe-N), and samarium cobalt magnetic powder (Sm-Co).

[0041] According to another aspect of the present invention, there is further provided a method for producing an extruded rare earth magnetic material, which includes the steps of: using the above-mentioned surface treatment method to perform surface treatment on a rare earth magnetic powder; and mixing the surface-treated rare earth magnetic powder with a binder, followed by extrusion granulation to obtain an extruded rare earth magnetic material. The surface treatment method provided by the present invention can be used to treat the rare earth magnetic powder, which can significantly improve its oxidation resistance, and can protect the rare earth magnetic powder from oxidation before and during the subsequent extrusion granulation with the binder, thereby producing an extruded rare earth magnetic material with high performance and high stability.

[0042] The binder may be nylon such as nylon 6, nylon 12, nylon 11, nylon 66, or may be a material such as polyphenylene sulfide (PPS) or polyether ether ketone (PEEK) having excellent temperature resistance, and these materials may be used alone or in combination. Preferably, the amount of binder used is 8 to 15% of the weight of the rare earth magnetic powder.

[0043] In a preferred embodiment, the extrusion granulation process employs a twin screw extruder, and the temperature of the extrusion granulation is 200-310°C.

[0044] According to another aspect of the present invention, there is further provided an extruded rare earth magnetic material, which is produced by the above-mentioned method. Due to the excellent oxidation resistance of the rare earth magnetic powder after surface treatment, the extruded rare earth magnetic material has better magnetic properties and stability.

[0045] The beneficial effects of the present invention will be further described below in combination with specific examples.

[0046] Example 1 In this example, the raw materials and the weight parts of the raw materials are as follows: Rare earth magnetic powder: homogeneous NdFeB magnetic powder (Magkun Magnetic Company 15-9 magnetic powder, 92 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Binder: Nylon 12 powder (Japan Ube Nylon, 7.5 parts), The process steps are as follows: 0.01mol / L oxalic acid in isopropyl alcohol solution was dissolved in anhydrous ethanol, and the pH value was adjusted to 5 to form a weak acid solution, into which rare earth magnetic powder was added. The weak acid solution could completely cover the magnetic powder, and the volume ratio of the weak acid solution to the magnetic powder was 1.5:1. The ultrasonic vibration was turned on, the power was controlled to 2000W, and the treatment was continued for 5 minutes to form a system containing weakly oxidized magnetic powder.

[0047] To the above system, Elsom's BW-231 zinc-based phosphide solution was added, the amount added was based on the pH value, the pH value was adjusted to 4, ultrasonic vibration was continued, the power was controlled to 1500W, and the treatment was carried out for 15 minutes to form a system containing phosphide magnetic powder.

[0048] Next, a coupling agent was added to the system, which was then subjected to ultrasonic vibration with the power controlled to 1500 W. After 10 minutes, the system was vacuum dried at 80° C. for 5 hours to obtain surface-treated rare earth magnetic powder.

[0049] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 200 to 220°C, and a high-performance extruded rare earth magnetic material was obtained.

[0050] According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.58T, Hcj=737KA / m, (BH)m=52KJ / m 3 The melt index was 306 g / 10 min.

[0051] Example 2 In this example, the raw materials and the weight parts of the raw materials are as follows: Rare earth magnetic powder: homogeneous NdFeB magnetic powder (Magkun Magnetic Company 15-9 magnetic powder, 90 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Binder: PPS powder (Japan Tosoh 100#, 9.5 parts), The process steps are as follows: 0.01 mol / L oxalic acid in isopropyl alcohol solution was dissolved in anhydrous ethanol, and the pH value was adjusted to 7 to form a weak acid solution, into which rare earth magnetic powder was added. The weak acid solution could completely cover the magnetic powder, and the volume ratio of the weak acid solution to the magnetic powder was 2:1. The ultrasonic vibration was turned on, the power was controlled to 2000W, and the treatment was continued for 5 minutes to form a system containing weakly oxidized magnetic powder.

[0052] To the above system, Elsom's BW-231 zinc-based phosphide solution was added, the amount added was based on the pH value, the pH value was adjusted to 5, ultrasonic vibration was continued, the power was controlled to 1500W, and the treatment was carried out for 15 minutes to form a system containing phosphide magnetic powder.

[0053] Next, a coupling agent was added to the system, which was then subjected to ultrasonic vibration with the power controlled to 1500 W. After 10 minutes, the system was vacuum dried at 80° C. for 5 hours to obtain surface-treated rare earth magnetic powder.

[0054] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 290 to 310°C, and a high-performance extruded rare earth magnetic material was obtained.

[0055] According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.54T, Hcj=709KA / m, (BH)m=49KJ / m 3 The melt index was 183 g / 10 min.

[0056] Example 3 In this example, the raw materials and the weight parts of the raw materials are as follows: Rare earth magnetic powder: isomeric Sm2F 17 Nx magnetic powder (D 50 2.5μm, 91 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Binder: Nylon 12 powder (Japan Ube Nylon, 8.5 parts), The process steps are as follows: 0.01 mol / L oxalic acid in isopropyl alcohol solution was dissolved in anhydrous ethanol, and the pH value was adjusted to 7 to form a weak acid solution, into which rare earth magnetic powder was added. The weak acid solution could completely cover the magnetic powder, and the volume ratio of the weak acid solution to the magnetic powder was 3:1. The ultrasonic vibration was turned on, the power was controlled to 2000W, and the treatment was continued for 5 minutes to form a system containing weakly oxidized magnetic powder.

[0057] To the above system, Elsom's BW-231 zinc-based phosphide solution was added, the amount added was based on the pH value, the pH value was adjusted to 5, ultrasonic vibration was continued, the power was controlled to 1500W, and the treatment was carried out for 15 minutes to form a system containing phosphide magnetic powder.

[0058] Next, a coupling agent was added to the system, which was then subjected to ultrasonic vibration with the power controlled to 1500 W. After 10 minutes, the system was vacuum dried at 80° C. for 5 hours to obtain surface-treated rare earth magnetic powder.

[0059] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 200 to 220°C, and a high-performance extruded rare earth magnetic material was obtained.

[0060] According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.64T, Hcj=725KA / m, (BH)m=65KJ / m 3 The melt index was 142 g / 10 min.

[0061] Example 4 In this example, the raw materials and the weight parts of the raw materials are as follows: Rare earth magnetic powder: isomeric Sm2F 17 Nx magnetic powder (D 50 2.5μm, 89 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Binder: PPS powder (Japan Tosoh 100#, 10.5 parts), The process steps are as follows: 0.01mol / L oxalic acid in isopropyl alcohol solution was dissolved in anhydrous ethanol, and the pH value was adjusted to 6 to form a weak acid solution, into which rare earth magnetic powder was added. The weak acid solution could completely cover the magnetic powder, and the volume ratio of the weak acid solution to the magnetic powder was 1.5:1. The ultrasonic vibration was turned on, the power was controlled to 2000W, and the treatment was continued for 5 minutes to form a system containing weakly oxidized magnetic powder.

[0062] To the above system, Elsom's BW-231 zinc-based phosphide solution was added, the amount added was based on the pH value, the pH value was adjusted to 5, ultrasonic vibration was continued, the power was controlled to 1500W, and the treatment was carried out for 15 minutes to form a system containing phosphide magnetic powder.

[0063] Next, a coupling agent was added to the system, and the system was subjected to ultrasonic vibration with the power controlled to 1500 W. After 10 minutes, the system was vacuum dried at 80° C. for 5 hours to obtain surface-treated rare earth magnetic powder.

[0064] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 290 to 310°C, and a high-performance extruded rare earth magnetic material was obtained.

[0065] According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.59T, Hcj=695KA / m, (BH)m=59KJ / m 3 The melt index was 108 g / 10 min.

[0066] Example 5 The only difference from Example 1 is that acetic acid is used as a weak acid and KH560 is used as a silane coupling agent. According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.58T, Hcj=726KA / m, (BH)m=52KJ / m 3 The melt index was 312 g / 10 min.

[0067] Example 6 The only difference from Example 1 is that carbonic acid is used as a weak acid and KH792 is used as a silane coupling agent. Based on the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.59T, Hcj=724KA / m, (BH)m=53KJ / m 3 The melt index was 300 g / 10 min.

[0068] Example 7 The only difference from Example 1 is as follows: The pH value of the weak acid solution is adjusted to 7 with ethanol, the volume ratio of the weak acid solution to the rare earth magnetic powder is 3:1, the power of the first ultrasonic vibration is 1500W, and the treatment is performed for 2 minutes; Add zinc-based phosphide liquid to the system containing weakly oxidized magnetic powder, adjust the pH value to 5, continue ultrasonic vibration, control the power to 1000W, and process for 10 minutes to form a system containing phosphide magnetic powder; Next, a coupling agent was added to the system, and the amount of the coupling agent added was 0.5% of the weight of the rare earth magnetic powder. The system was subjected to ultrasonic vibration and the power was controlled to 2000 W. After 15 minutes, the system was vacuum dried at 90°C for 5 hours to obtain surface-treated rare earth magnetic powder.

[0069] According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.59T, Hcj=753KA / m, (BH)m=53KJ / m 3 The melt index was 275 g / 10 min.

[0070] Example 8 The only difference from Example 1 is as follows: The pH value of the weak acid solution is adjusted to 6 with ethanol, the volume ratio of the weak acid solution to the rare earth magnetic powder is 2:1, the power of the first ultrasonic vibration is 2500W, and the treatment is performed for 4 minutes; Add zinc-based phosphide liquid to the system containing weakly oxidized magnetic powder, adjust the pH value to 5, continue ultrasonic vibration, control the power to 1500W, and process for 15 minutes to form a system containing phosphide magnetic powder; Next, a coupling agent was added to the system. The amount of the coupling agent added was 1% of the weight of the rare earth magnetic powder. The system was subjected to ultrasonic vibration and the power was controlled to 1200 W. After 15 minutes, the system was vacuum dried at 90°C for 7 hours to obtain surface-treated rare earth magnetic powder.

[0071] According to the test standard related to IEC60404-8-1, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.58T, Hcj=706KA / m, (BH)m=51KJ / m 3The melt index was 328 g / 10 min.

[0072] Comparative Example 1 The raw materials and the weight parts of the raw materials in this comparative example are as follows: Rare earth magnetic powder: homogeneous NdFeB magnetic powder (Magkun Magnetic Company 15-9 magnetic powder, 92 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Phosphoric acid: 0.5 parts, Binder: Nylon 12 powder (Japan Ube Nylon, 7 parts), The process steps are as follows: The silane coupling agent and phosphoric acid were dissolved in an appropriate amount of anhydrous ethanol, and the rare earth magnetic powder was added thereto. The amount of anhydrous ethanol used was such that the magnetic powder could be completely coated, and the volume ratio of the anhydrous ethanol to the magnetic powder was 1.5:1. The rare earth magnetic powder was then added to the solution and thoroughly stirred to mix uniformly, and then vacuum dried at 80°C for 5 hours to obtain the rare earth magnetic powder after surface treatment.

[0073] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 200 to 220° C., and an extruded rare earth magnetic material was obtained.

[0074] According to the relevant test standards, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.56T, Hcj=716KA / m, (BH)m=48KJ / m 3 The melt index was 264 g / 10 min.

[0075] Comparative Example 2 The raw materials and the mass percentages of the raw materials in this comparative example are as follows: Rare earth magnetic powder: homogeneous NdFeB magnetic powder (Magkun Magnetic Company 15-9 magnetic powder, 90 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Phosphoric acid: 0.5 parts, Binder: PPS powder (Japan Tosoh 100#, 9 parts), The process steps are as follows: The silane coupling agent and phosphoric acid were dissolved in an appropriate amount of anhydrous ethanol, and the rare earth magnetic powder was added thereto. The amount of anhydrous ethanol used was enough to completely cover the magnetic powder, and the volume ratio of the anhydrous ethanol to the magnetic powder was 2:1. The rare earth magnetic powder was then added to the solution and thoroughly stirred to mix uniformly, and then vacuum dried at 80°C for 5 hours to obtain the rare earth magnetic powder after surface treatment.

[0076] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 290 to 310° C., and an extruded rare earth magnetic material was obtained.

[0077] According to the relevant test standards, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.51T, Hcj=674KA / m, (BH)m=46KJ / m 3 The melt index was 152 g / 10 min.

[0078] Comparative Example 3 The raw materials and the weight parts of the raw materials in this comparative example are as follows: Rare earth magnetic powder: isomeric Sm2F 17 Nx magnetic powder (D 50 2.5μm, 91 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), Phosphoric acid: 0.5 parts, Binder: Nylon 12 powder (Japan Ube Nylon, 8 parts), The process steps are as follows: The silane coupling agent and phosphoric acid were dissolved in an appropriate amount of anhydrous ethanol, and the rare earth magnetic powder was added thereto. The amount of anhydrous ethanol used was enough to completely cover the magnetic powder, and the volume ratio of the anhydrous ethanol to the magnetic powder was 3:1. The rare earth magnetic powder was then added to the solution and thoroughly stirred to mix uniformly, and then vacuum dried at 80°C for 5 hours to obtain the rare earth magnetic powder after surface treatment.

[0079] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 200 to 220° C., and an extruded rare earth magnetic material was obtained.

[0080] According to the relevant test standards, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.58T, Hcj=684KA / m, (BH)m=59KJ / m 3 The melt index was 138 g / 10 min.

[0081] Comparative Example 4 The raw materials and the weight parts of the raw materials in this comparative example are as follows: Rare earth magnetic powder: isomeric Sm2F 17 Nx magnetic powder (D 50 2.5μm, 89 parts), Binder: PPS powder (Japan Tosoh 100#, 10.5 parts), Coupling agent: silane coupling agent (KH550, 0.5 parts), The process steps are as follows: The silane coupling agent and phosphoric acid were dissolved in an appropriate amount of anhydrous ethanol, and the rare earth magnetic powder was added thereto. The amount of anhydrous ethanol used was such that the magnetic powder could be completely coated, and the volume ratio of the anhydrous ethanol to the magnetic powder was 1.5:1. The rare earth magnetic powder was then added to the solution and thoroughly stirred to mix uniformly, and then vacuum dried at 80°C for 5 hours to obtain the rare earth magnetic powder after surface treatment.

[0082] The surface-treated rare earth magnetic powder and a binder were mixed and granulated in a twin-screw extruder. The granulation temperature was set to 290 to 310° C., and an extruded rare earth magnetic material was obtained.

[0083] According to the relevant test standards, the performance test was carried out on the injected rare earth magnetic material sample, and the results were as follows: Br=0.52T, Hcj=625KA / m, (BH)m=52KJ / m 3 The melt index was 117 g / 10 min.

[0084] [Table 1]

[0085] Br, Hcj, and (BH)max are all important indicators of the magnetic properties of permanent magnet materials, and after rare earth permanent magnet materials are oxidized, their performance will decrease, and these indicators will decrease, and the more serious the oxidation, the greater the decrease in these indicators. As can be seen from the above table, the rare earth magnetic powder treated by the surface treatment method in the embodiment of the present invention has significantly improved Br, Hcj, and (BH)max indicators of the extruded rare earth magnetic material, which shows that its oxidation resistance is stronger and the magnetic properties of the extruded rare earth magnetic material are better.

[0086] In addition, different binders have large temperature differences during injection, and magnetic powders produced at different temperatures will have large differences, so the performance differences between the rare earth magnetic powder injection materials produced in the above Examples 1 to 4 are obvious. However, by comparing them with Comparative Examples 1 to 4 respectively, the performance of the injection materials corresponding to the same type of binder or the same type of magnetic powder is obviously improved, which is enough to demonstrate the beneficial effects brought by the surface treatment method of the present invention.

[0087] Fluidity refers to the flow rate of the solution when the product is in a certain molten state and under a certain pressure. The aggregation of magnetic powder or the irregular shape of magnetic powder both affect the fluidity. As can be seen from the above table, the rare earth magnetic powder treated by the surface treatment method in the embodiment of the present invention has a significantly improved melt index of the extruded rare earth magnetic material, the shape of the rare earth magnetic powder is more regular, and the compatibility with the binder after surface treatment is better.

[0088] The above is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Those skilled in the art can make various modifications and changes to the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present application should be included within the protection scope of the present invention.

Claims

1. Step S1 of adding the rare earth magnetic powder to a weak acid solution to form a weakly oxidized magnetic powder so as to perform a weak oxidation treatment on the surface of the rare earth magnetic powder, the weak acid in the weak acid solution being an inorganic weak acid having an acidity coefficient pKa value of more than 4.5 and / or an organic weak acid having an acidity coefficient of more than 1.0; A step S2 of performing a phosphorization process on the weakly oxidized magnetic powder using a phosphorization liquid to form a phosphorized magnetic powder; and step S3 of mixing the phosphorized magnetic powder with a coupling agent so as to subject the phosphorized magnetic powder to a coupling treatment, and then drying the powder to obtain the rare earth magnetic powder after surface treatment.

2. The weak acid is one or more of oxalic acid, acetic acid, and carbonic acid; Preferably, the pH value of the weak acid solution is between 5 and 7; Preferably, the pH value of the weak acid solution is adjusted using ethanol; The surface treatment method according to claim 1, wherein the volume ratio of the weak acid solution to the rare earth magnetic powder is preferably 1.5 to 3:

1.

3. In the step S1, after the rare earth magnetic powder is added to the weak acid solution, a first ultrasonic vibration is applied to perform the weak oxidation treatment; The surface treatment method according to claim 1 or 2, characterized in that the power of the first ultrasonic vibration is preferably 1500 to 2500 W and the duration is preferably 2 to 5 minutes.

4. the phosphorizing solution is a zinc-based phosphorizing solution or a manganese-based phosphorizing solution, Preferably, after the weak oxidation treatment is completed, the phosphorization treatment is carried out by directly adding the phosphorization solution to the system containing the weakly oxidized magnetic powder until the pH value of the system reaches 4 to 5, followed by performing a second ultrasonic vibration; The surface treatment method according to any one of claims 1 to 3, wherein the power of the second ultrasonic vibration is preferably 1000 to 1500 W and the duration is preferably 10 to 15 minutes.

5. The coupling agent is a silane coupling agent, preferably one or more of KH550, KH560, and KH792; Preferably, after the phosphorization treatment is completed, the coupling agent is added directly to the system containing the phosphorized magnetic powder, followed by a third ultrasonic vibration to perform the coupling treatment; Preferably, the amount of the coupling agent added is 0.5 to 1% by weight of the rare earth magnetic powder; Preferably, the power of the third ultrasonic vibration is 1200 to 2000 W and the time is 10 to 15 minutes; The surface treatment method according to claim 4, wherein the drying step is preferably performed by vacuum drying at a drying temperature of 70 to 90°C.

6. The surface treatment method according to any one of claims 1 to 3, characterized in that the rare earth magnetic powder is one or more of homogeneous neodymium iron boron magnetic powder, heterogeneous neodymium iron boron magnetic powder, homogeneous samarium iron nitrogen magnetic powder, heterogeneous samarium iron nitrogen magnetic powder, and samarium cobalt magnetic powder.

7. A step of surface treating a rare earth magnetic powder using the surface treatment method according to any one of claims 1 to 6; and mixing the surface-treated rare earth magnetic powder with a binder, and then extruding and granulating the mixture to obtain an extruded rare earth magnetic material.

8. The manufacturing method according to claim 7, characterized in that the binder is one or more of nylon, polyphenylene sulfide, and polyether ether ketone, and preferably, the amount of the binder used is 8 to 15% by weight of the rare earth magnetic powder.

9. The method according to claim 7, wherein the extrusion granulation process adopts a twin screw extruder, and the temperature of the extrusion granulation is 200-310°C.

10. An extruded rare earth magnetic material, characterized in that it is produced by the production method according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • ε-IRON OXIDE TYPE FERROMAGNETIC POWDER, PROCESS FOR PRODUCING THE SAME, AND ε-IRON OXIDE TYPE FERROMAGNETIC POWDER-CONTAINING COMPOSITION

    JP2018092691A

  • Method for producing rare earth magnetic powder