Thermoplastic resin composition, its method of manufacture and molded article containing same
The thermoplastic resin composition addresses flow mark issues in ASA resins by combining specific copolymers and resins, enhancing fluidity and weather resistance while improving appearance quality.
Patent Information
- Application Number
- JP2024508552
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-13
- Filing Date
- 2023-07-03
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-07-03
AI Technical Summary
Traditional ASA resins struggle with flow marks during molding, which are appearance defects caused by uneven resin flow, and existing methods to mitigate these issues are either difficult to implement or ineffective.
A thermoplastic resin composition comprising specific ratios of acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymers with varying particle sizes, a heat-resistant resin, and ultra-high molecular weight SAN resins, optimized to enhance fluidity and suppress flow marks.
The composition achieves improved fluidity and weather resistance while effectively preventing flow marks, ensuring excellent appearance quality in molded products.
Smart Images

Figure 2024539814000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0131044 dated October 13, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated as part of this specification.
[0002] The present invention relates to a thermoplastic resin composition, a production method thereof, and a molded article containing the same. More specifically, the present invention relates to a thermoplastic resin composition which is excellent in fluidity and weather resistance and which suppresses the occurrence of flow marks and thus has excellent appearance quality, a production method thereof, and a molded article containing the same. [Background technology]
[0003] Acrylate-styrene-acrylonitrile graft copolymer (hereinafter referred to as "ASA resin") has weather resistance, aging resistance, chemical resistance, and processability, and has a wide range of uses, so it is used in a wide range of fields such as automobiles, leisure goods, construction materials, gardening goods, and building materials.
[0004] Recently, there has been a significant increase in customer preferences for molded products with excellent natural coloring properties in consideration of aesthetic design. However, when conventional ASA resins are injection molded into the shape of a desired product, the occurrence of flow marks, one of various appearance defects, has been increasing. As a result, there is an increasing demand for ASA resins that can eliminate this problem and have improved appearance quality.
[0005] Flow marks refer to striped appearance defects that appear when the flow of a resin composition is non-uniform within a mold during molding.
[0006] Flow marks that appear during injection molding can be of irregular thickness, record type, or wavy stripes like tiger stripes; particularly in ASA injection molded products, gaps occur due to differences in solidification speed within the resin composition as the molten resin cools on the surface of the mold, or when the fluidity of the resin composition is unstable, differences in transfer occur on the contact surface with the mold, resulting in wavy stripe type flow marks with repeated stripes on the appearance.
[0007] Generally, in order to improve the occurrence of flow marks, there is a method of increasing the injection temperature and speed, but this method has a drawback that it is difficult to apply because the injection conditions are not standardized. In addition, there is a method of optimizing the thickness and position of the gate, but this method has a drawback that it is difficult to apply because the mold design is also not standardized.
[0008] Another method is to add internal and external lubricants to ASA resin to improve the flow properties of the resin. However, this method has limitations because not only is the improvement effect not obvious, but low molecular weight substances such as lubricants volatilize during injection processing and over the long term end up depositing in the mold. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent Publication No. 10-2022-0000554 Summary of the Invention [Problem to be solved by the invention]
[0010] In order to solve the problems of the conventional techniques as described above, an object of the present invention is to provide a thermoplastic resin composition which is excellent in flowability and weather resistance, and which prevents deterioration of surface properties that may occur during molding and has excellent appearance quality.
[0011] Another object of the present invention is to provide a molded article produced from the thermoplastic resin composition.
[0012] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]
[0013] In order to achieve the above object, the present invention provides I) a thermoplastic resin composition comprising 100 parts by weight of a base resin including (A-1) an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle size of 400 to 600 nm, (A-2) an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle size of 30 to 200 nm, (B) a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol, and (C) an aromatic vinyl compound-vinyl cyan compound copolymer having a weight-average molecular weight of 50,000 to 70,000 g / mol; and (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight-average molecular weight of 1,000,000 to 10,000,000 g / mol.
[0014] II) In the above I), when the weight percentages of (A-1), (A-2), (B) and (C) are a, b, c and d, respectively, the following formula 1 can be satisfied.
[0015] [Formula 1] a≦d <b≦c (In the above formula, a is an integer of 5 to 20, b is an integer of 26 to 35, c is an integer of 35 to 60, and d is an integer of 6 to 25.)
[0016] III) In the above I) or II), the base resin may be contained in a weight ratio of (A-1):(A-2):(B):(C) of 1:2-3:4-5:1-2.
[0017] IV) In the above I) to III), the aromatic vinyl compound-vinyl cyan compound copolymer (D) may have an intrinsic viscosity (IV, 25° C.) of 10 dL / g or more.
[0018] V) In the above I) to IV), the aromatic vinyl compound-vinyl cyan compound copolymer (D) has a bulk density of 0.1 to 0.5 g / cm 3 may be also possible.
[0019] VI) In the above I) to V), the aromatic vinyl compound-vinyl cyan compound copolymer (D) may have a weight average molecular weight of more than 1,000,000 g / mol.
[0020] VII) In the above I) to VI), the (D) aromatic vinyl compound-vinyl cyan compound copolymer may contain 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound.
[0021] VIII) In the above I) to VII), the total amount of (A-1) and (A-2) may be 40% by weight or less, based on 100% by weight of the total content of all components constituting the base resin.
[0022] IX) In the above I) to VIII), the heat-resistant resin (B) may contain 60 to 80% by weight of an α-methylstyrene monomer and 20 to 40% by weight of a vinyl cyan compound.
[0023] X) In the above I) to IX), the (A-1) acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may contain 40 to 60% by weight of acrylate rubber, 25 to 45% by weight of aromatic vinyl compound, and 5 to 20% by weight of vinyl cyan compound, based on a total of 100% by weight.
[0024] XI) In the above I) to X), the (A-2) acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may contain 40 to 60% by weight of acrylate rubber, 25 to 45% by weight of aromatic vinyl compound, and 5 to 20% by weight of vinyl cyan compound, based on a total of 100% by weight.
[0025] XII) In the above I) to XI), the (C) aromatic vinyl compound-vinyl cyan compound copolymer may contain 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound.
[0026] XIII) The present invention also provides (A-1) 5 to 20% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 400 to 600 nm; (A-2) 20 to 40% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 30 to 200 nm, (B) 30 to 60% by weight of a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol, and (C) 100 parts by weight of a base resin containing 5 to 30% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer having a weight average molecular weight of 50,000 to 70,000 g / mol; (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol; The thermoplastic resin composition is characterized in that the base resin is contained in a weight ratio of (A-1):(A-2):(B):(C) of 1:2-3:4-5:1-2.
[0027] XIV) In the above XIII), the thermoplastic resin composition can satisfy the condition of the following mathematical formula 3.
[0028] [Formula 3] 380≦flow index×die swell ratio×spiral×content of processing aids≦1400 (In the above formula 3, the flow index is a value (unit: g / 10 min) measured at 220°C and a load of 10 kg according to ASTM D1238 for the thermoplastic resin composition, the die swell ratio is a value calculated by the following formula 4, the spiral is the length (unit: cm) of a test piece injected using a spiral die (2.0T) under conditions of an injection temperature of 300°C, a die temperature of 80°C, and a pressure of 500 kgf using an injection molding machine (Engel, Victory 80), and the content of the processing aid is the amount (parts by weight) of the (D) copolymer used based on 100 parts by weight of the total amount of the base resin and the aromatic vinyl compound-vinyl cyan compound copolymer.)
[0029] [Formula 4] Die swell ratio = D ex / D0 (In the above formula 4, D0 is the diameter of the die, 2 mm, and D ex is the diameter (unit: mm) of the extrusion test piece extruded at 220°C and a load of 10 kg using a fluidity tester (Melt Indexer, MI) with a die diameter of 2 mm (D0).
[0030] XV) In the above XIII) to XIV), the formula 3 can satisfy the range of 400 to 1300.
[0031] XVI) In the above XIII) to XV), the flow index may be 6.7 to 13.2 g / 10 min.
[0032] XVII) In any of XIII) to XVI), the die swell ratio may be 1.31 to 1.54.
[0033] XVIII) In any of XIII) to XVII), the spiral may be 21.1 to 24.4 cm.
[0034] The present invention also relates to XIX) a polymerizable composition comprising (A-1) 5 to 20% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 400 to 600 nm, (A-2) 20 to 40% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 30 to 200 nm, (B) 30% by weight of a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol, and (C) 20% by weight of a heat-resistant resin having a weight-average molecular weight of 20,000 to 30,000 g / mol. (C) 100 parts by weight of a base resin containing 5 to 60% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 70,000 g / mol; and (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol; The base resin is contained in a weight ratio of (A-1):(A-2):(B):(C) of 1:2-3:4-5:1-2.
[0035] The present invention also provides XX) a molded article comprising the above-mentioned thermoplastic resin composition. Effect of the Invention
[0036] According to the present invention, there is an effect of providing a thermoplastic resin composition which has fluidity and weather resistance equal to or greater than those of conventional ASA resins, and which has excellent appearance quality by suppressing the occurrence of flow marks.
[0037] Therefore, the thermoplastic resin composition according to the present invention can be widely used, particularly in the field of automotive exterior parts, and specifically, can be used as a material for side mirror housings, radiator grilles, or pillars. [Brief description of the drawings]
[0038] [Figure 1]Photographs were taken to observe the presence or absence of flow marks on the surfaces of injection test pieces measuring 40 mm x 200 mm produced in Example 1 and Comparative Examples 1, 3, and 5, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] The thermoplastic resin composition of the present invention, its production method and molded articles containing the same will be described in detail below.
[0040] The inventors have confirmed that when two or more graft copolymers containing acrylate rubbers having different average particle sizes are combined with a heat-resistant resin, a low molecular weight SAN resin, and an ultra-high molecular weight SAN resin, etc., by adjusting the composition ratio, etc., a synergistic effect is created by combining these components, which results in excellent fluidity and weather resistance, as well as suppressing the occurrence of flow marks and improving appearance quality. Based on this, the inventors have continued their research and have completed the present invention.
[0041] The thermoplastic resin composition according to the present invention will be described in detail as follows.
[0042] The thermoplastic resin composition according to the present invention is characterized by comprising 100 parts by weight of a base resin including (A-1) an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 400 to 600 nm, (A-2) an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 30 to 200 nm, (B) a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol, and (C) an aromatic vinyl compound-vinyl cyan compound copolymer having a weight-average molecular weight of 50,000 to 70,000 g / mol; and (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight-average molecular weight of 1,000,000 to 10,000,000 g / mol.
[0043] In this case, the ASA resin composition has the same or higher fluidity and weather resistance as the conventional ASA resin composition, and also has the effect of suppressing the occurrence of flow marks and thus providing excellent appearance quality.
[0044] Hereinafter, the thermoplastic resin composition of the present invention will be described in detail with respect to each component.
[0045] (A-1) Acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing acrylate rubber having an average particle size of 400 to 600 nm The acrylate rubber of the graft copolymer (A-1) may have, for example, an average particle size of 420 to 550 nm, preferably 450 to 520 nm, and more preferably 450 to 500 nm. Within this range, the effect of excellent mechanical strength such as impact strength is achieved.
[0046] In this description, the average particle size can be measured using dynamic light scattering, and in particular, it is measured as an intensity value in Gaussian mode using a particle size analyzer (product name: Nicomp380, manufacturer: PSS). At this time, as a specific measurement example, 0.1g of latex with a total solid content of 35-50% by weight is prepared by diluting it 1,000-5,000 times with distilled water, and the measurement method is automatic dilution and measurement with a flow cell, the measurement mode is dynamic light scattering / intensity 300KHz / intensity-weighted Gaussian analysis, and the setting values are a temperature of 23°C, a measurement wavelength of 632.8nm, and a channel width of 10μsec.
[0047] The (A-1) graft copolymer may be, for example, 5 to 20% by weight, preferably 7 to 20% by weight, and more preferably 7 to 15% by weight, based on the total weight of the base resin. Within this range, the fluidity and weather resistance are equal to or greater than those of conventional ASA resin compositions, and the die swell ratio is excellent, thereby suppressing the occurrence of flow marks and providing excellent appearance quality.
[0048] The (A-1) graft copolymer, for example, contains 40 to 60% by weight of acrylate rubber, 25 to 45% by weight of aromatic vinyl compound, and 5 to 20% by weight of vinyl cyan compound, and preferably contains 45 to 55% by weight of acrylate rubber, 30 to 40% by weight of aromatic vinyl compound, and 10 to 15% by weight of vinyl cyan compound. Within these ranges, the copolymer has the effect of exhibiting excellent mechanical strength such as impact strength.
[0049] In this description, a polymer comprising a certain compound means a polymer polymerized containing that compound, where the units in the polymerized polymer are derived from that compound.
[0050] In the present description, the alkyl acrylate compound may be, for example, an alkyl acrylate having an alkyl group with 1 to 15 carbon atoms, preferably one or more selected from the group consisting of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylbutyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, hexyl acrylate, heptyl acrylate, n-pentyl acrylate, and lauryl acrylate, more preferably an alkyl acrylate containing a chain alkyl group with 1 to 4 carbon atoms, and even more preferably butyl acrylate.
[0051] In the present description, the aromatic vinyl compound may be, for example, one or more selected from the group consisting of styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, ethylstyrene, isobutylstyrene, t-butylstyrene, o-bromostyrene, p-bromostyrene, m-bromostyrene, o-chlorostyrene, p-chlorostyrene, m-chlorostyrene, vinyltoluene, vinylxylene, fluorostyrene, and vinylnaphthalene, preferably one or more selected from the group consisting of styrene and α-methylstyrene, and more preferably styrene. In this case, the aromatic vinyl compound has an appropriate fluidity, and therefore has the effect of excellent processability and excellent mechanical properties such as impact resistance.
[0052] In the present description, the vinyl cyanide compound may be, for example, one or more selected from the group consisting of acrylonitrile, methacrylonitrile, ethyl acrylonitrile, and isopropyl acrylonitrile, and is preferably acrylonitrile.
[0053] The (A-1) graft copolymer may be prepared, for example, by emulsion polymerization, in which case it has the effect of being excellent in mechanical strength such as impact strength.
[0054] The emulsion polymerization is not particularly limited as long as it is an emulsion polymerization commonly performed in the technical field to which the present invention pertains, and a specific example thereof may be an emulsion graft polymerization method.
[0055] (A-2) Acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing acrylate rubber having an average particle size of 30 to 200 nm The acrylate rubber of the graft copolymer (A-2) may have, for example, an average particle size of 30 to 200 nm, preferably 50 to 180 nm, more preferably 70 to 150 nm, and even more preferably 70 to 120 nm. Within this range, excellent impact strength and gloss can be imparted to the final thermoplastic resin composition.
[0056] The (A-2) graft copolymer may be, for example, 26 to 35% by weight, preferably 28 to 35% by weight, and more preferably 28 to 33% by weight, based on the total weight of the base resin. Within this range, the fluidity and weather resistance are equal to or greater than those of conventional ASA resin compositions, and the die swell ratio is excellent, so that the occurrence of flow marks is suppressed, resulting in excellent appearance quality.
[0057] The (A-2) graft copolymer, for example, contains 40 to 60% by weight of acrylate rubber, 25 to 45% by weight of aromatic vinyl compound, and 5 to 20% by weight of vinyl cyan compound, and preferably contains 45 to 55% by weight of acrylate rubber, 30 to 40% by weight of aromatic vinyl compound, and 10 to 15% by weight of vinyl cyan compound. Within these ranges, the effect of excellent gloss and impact strength is achieved.
[0058] The (A-2) graft copolymer may be produced by, for example, emulsion polymerization, in which case, it has the effect of providing excellent impact strength and gloss.
[0059] The emulsion polymerization is not particularly limited as long as it is an emulsion polymerization commonly performed in the technical field to which the present invention pertains, and a specific example thereof may be an emulsion graft polymerization method.
[0060] The weight ratio (A-1:A-2) of the graft copolymer (A-1) to the graft copolymer (A-2) may be preferably 1:2 or more, more preferably 1:2 to 3, and even more preferably 1:2.5 to 1:3. Within this range, there are advantages in that the fluidity and weather resistance are equal to or greater than the same, and the occurrence of flow marks is suppressed, thereby improving the appearance quality.
[0061] In the present invention, the weight ratio of A to B means the weight ratio of A:B.
[0062] The total amount of the (A-1) graft copolymer and the (A-2) graft copolymer may be preferably 40% by weight or less, more preferably 10 to 40% by weight, and even more preferably 25 to 40% by weight, based on 100% by weight of the total content of all components constituting the base resin. Within this range, there are advantages in that the fluidity and weather resistance are equal to or higher, and the occurrence of flow marks is suppressed, thereby improving the appearance quality.
[0063] (B) a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol The heat-resistant resin (B) may have a weight average molecular weight of, for example, preferably 50,000 to 150,000 g / mol, more preferably 70,000 to 140,000 g / mol, and even more preferably 90,000 to 130,000 g / mol. Within this range, the heat-resistant resin has the effect of being excellent in heat resistance, etc.
[0064] In this description, unless otherwise specified, the weight average molecular weight can be measured using GPC (gel permeation chromatography, water breeze), and as a specific example, it can be measured as a relative value to a standard PS (standard polystyrene) sample through GPC using THF (tetrahydrofuran) as an eluent. In this case, as a specific measurement example, the solvent is THF, the column temperature is 40°C, the flow rate is 0.3 ml / min, the sample concentration is 20 mg / ml, the injection amount is 5 μl, the column model is 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B Guard (50×4.6 mm), the measuring device is an Agilent 1200 series system, the refractive index detector is an Agilent G1362 RID, the RI temperature is 35°C, the data is processed by Agilent ChemStation S / W, and the test method (Mn, Mw and PDI) can be measured under the conditions of OECD TG 118.
[0065] The (B) heat-resistant resin may be, for example, 35 to 60% by weight, preferably 35 to 55% by weight, and more preferably 38 to 52% by weight, based on the total weight of the base resin. Within this range, the impact resistance, heat resistance, and hardness are maintained at the same levels, while the fluidity and die swell ratio are excellent, so that the occurrence of flow marks is suppressed and the appearance quality is improved.
[0066] In the present description, the heat-resistant resin is not particularly limited as long as it is a polymer generally referred to as a heat-resistant resin in the technical field to which the present invention belongs. Specifically, it may mean a polymer containing a monomer having a higher glass transition temperature (polymer basis) than a styrene monomer, i.e., a heat-resistant monomer.
[0067] The heat-resistant resin (B), for example, may include at least one heat-resistant monomer selected from the group consisting of an α-methylstyrene-based monomer and a maleimide-based monomer, and preferably an α-methylstyrene-based monomer. In this case, the heat-resistant resin (B) has an excellent balance between heat resistance and physical properties.
[0068] The maleimide monomer may be, for example, one or more selected from the group consisting of maleimide and derivatives thereof, and preferably one or more selected from the group consisting of maleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-isobutylmaleimide, Nt-butylmaleimide, N-laurylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(4-chlorophenyl)maleimide, 2-methyl-N-phenylmaleimide, N-(4-bromophenyl)maleimide, N-(4-nitrophenyl)maleimide, N-(4-hydroxyphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-carboxyphenyl)maleimide, and N-benzylmaleimide.
[0069] The α-methylstyrene-based monomer may be, for example, at least one selected from the group consisting of α-methylstyrene and its derivatives, in which case there is an effect of excellent heat resistance.
[0070] In the present description, a derivative of a certain compound may preferably be a compound in which one or more of its hydrogen atoms have been substituted with a substituent such as an alkyl group having 1 to 10 carbon atoms, a halogen group, or the like.
[0071] The heat-resistant resin (B) preferably contains 60 to 80% by weight of an α-methylstyrene monomer and 20 to 40% by weight of a vinyl cyan compound, and more preferably contains 65 to 75% by weight of an α-methylstyrene monomer and 25 to 35% by weight of a vinyl cyan compound. In this case, the heat-resistant resin has excellent heat resistance and mechanical properties.
[0072] The heat-resistant resin (B) may be, as a preferred example, an α-methylstyrene-vinyl cyanide compound copolymer, or, as a more preferred example, an α-methylstyrene-acrylonitrile copolymer, which has the advantages of being excellent in heat resistance, suppressing the occurrence of flow marks, and providing excellent appearance quality.
[0073] The heat-resistant resin (B) preferably has a glass transition temperature of 110 to 150° C., more preferably 110 to 140° C., and within this range, it has the effect of providing excellent heat resistance and the like.
[0074] In this description, the glass transition temperature (Tg) can be measured using a Differential Scanning Calorimetry (DSC) in accordance with ASTM D 3418. As a specific measurement example, it can be measured using a Q100 DSC manufactured by TA Instruments at a heating rate of 10° C. / min.
[0075] The heat-resistant resin (B) may be produced by, for example, solution polymerization or bulk polymerization, in which case there is an effect of excellent heat resistance and flowability.
[0076] The solution polymerization and bulk polymerization are not particularly limited as long as they are solution polymerization and bulk polymerization methods commonly used in the technical field to which the present invention pertains.
[0077] (C) Aromatic vinyl compound-vinyl cyanide compound copolymer having a weight average molecular weight of 50,000 to 70,000 g / mol The (C) copolymer may preferably have a weight average molecular weight of 50,000 to 70,000 g / mol, more preferably 55,000 to 70,000 g / mol, and even more preferably 55,000 to 65,000 g / mol, and within this range, the occurrence of flow marks is suppressed, and the appearance quality is excellent. If the weight average molecular weight exceeds the range, as will be seen from Comparative Example 7 described later, the melt index decreases and the processability is poor.
[0078] The (C) copolymer may be, for example, 6 to 25% by weight, preferably 6 to 22% by weight, and more preferably 8 to 22% by weight, based on the total weight of the base resin. Within this range, the impact resistance, heat resistance, and hardness are maintained at the same levels, while the fluidity and die swell ratio are excellent, so that the occurrence of flow marks is suppressed and the appearance quality is improved.
[0079] The copolymer (C) may, for example, contain an aromatic vinyl compound and a vinyl cyan compound. In this case, there are advantages in that the impact resistance is excellent and the occurrence of flow marks is suppressed.
[0080] As a preferred example, the aromatic vinyl compound-vinyl cyan compound copolymer may contain 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound, more preferably 60 to 80% by weight of an aromatic vinyl compound and 20 to 40% by weight of a vinyl cyan compound, and even more preferably 70 to 75% by weight of an aromatic vinyl compound and 25 to 30% by weight of a vinyl cyan compound. In this case, there is an advantage that the fluidity and die swell ratio are excellent, and thus the occurrence of flow marks is suppressed.
[0081] The types of the aromatic vinyl compound and the vinyl cyan compound contained in the copolymer (C) may be within the same category as the types of the aromatic vinyl compound and the vinyl cyan compound contained in the graft copolymer (A-1) described herein.
[0082] The copolymer (C) may be produced by, for example, suspension polymerization, emulsion polymerization, solution polymerization or bulk polymerization, and in this case, it has the effect of being excellent in heat resistance and fluidity.
[0083] The suspension polymerization, emulsion polymerization, solution polymerization and bulk polymerization are not particularly limited as long as they are suspension polymerization, emulsion polymerization, solution polymerization and bulk polymerization methods commonly used in the technical field to which the present invention pertains.
[0084] In this description, in addition to the above-mentioned (C) copolymer, it is preferable to avoid the use of a methacrylate-aromatic vinyl compound-vinyl cyanide compound copolymer, since this can eliminate flow marks that tend to occur on the surface of the injected product while fully realizing fluidity and weather resistance properties, but the present invention is not limited thereto.
[0085] (D) Aromatic vinyl compound-vinyl cyanide compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol The (D) copolymer may preferably have a weight average molecular weight of 3,000,000 to 8,000,000 g / mol, more preferably 4,000,000 to 7,000,000 g / mol, and even more preferably 4,000,000 to 5,000,000 g / mol. Within this range, the occurrence of flow marks is suppressed, resulting in excellent appearance quality.
[0086] The (D) copolymer may be, for example, 0.5 to 4 parts by weight, preferably 0.7 to 3.7 parts by weight, more preferably 0.9 to 3.5 parts by weight, even more preferably 0.9 to 3.2 parts by weight, and particularly preferably 1 to 3 parts by weight, based on 100 parts by weight of the base resin. Within this range, there is an effect that the fluidity is excellent and the occurrence of flow marks is suppressed, resulting in excellent appearance quality.
[0087] The (D) copolymer may be, for example, a crosslinked aromatic vinyl compound-vinyl cyan compound copolymer, which has the advantages of excellent impact resistance and suppressing the occurrence of flow marks.
[0088] The crosslinked aromatic vinyl compound-vinyl cyan compound copolymer may, for example, be a mixture containing an aromatic vinyl compound and a vinyl cyan compound, and at least one polyfunctional compound selected from the group consisting of polyfunctional mercaptan compounds and polyfunctional acrylic monomers. In this case, it has the advantages of excellent impact resistance and suppressing the occurrence of flow marks.
[0089] As a preferred example, the crosslinked aromatic vinyl compound-vinyl cyan compound copolymer may contain 0.01 to 5 parts by weight of a polyfunctional mercaptan compound and 0.005 to 5 parts by weight of a polyfunctional acrylic monomer with respect to 100 parts by weight of a mixture containing 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound, and more preferably, 0.01 to 5 parts by weight of a polyfunctional mercaptan compound and 0.005 to 5 parts by weight of a polyfunctional acrylic monomer with respect to 100 parts by weight of a mixture containing 60 to 80% by weight of an aromatic vinyl compound and 20 to 40% by weight of a vinyl cyan compound. It may comprise 0.5 to 3 parts by weight of a mercaptan compound and 0.05 to 3 parts by weight of a polyfunctional acrylic monomer, and more preferably, it may comprise 0.5 to 3 parts by weight of a polyfunctional mercaptan compound and 0.05 to 3 parts by weight of a polyfunctional acrylic monomer per 100 parts by weight of a mixture containing 70 to 75% by weight of an aromatic vinyl compound and 20 to 30% by weight of a vinyl cyan compound. In this case, since the fluidity and die swelling ratio are excellent, there is an advantage that the occurrence of flow marks is suppressed.
[0090] As another preferred example, the (D) copolymer may contain 0.01 to 5 parts by weight of a polyfunctional mercaptan compound based on 100 parts by weight of a mixture containing 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound. In this case, there is an advantage that the fluidity and die swell ratio are excellent, and therefore the occurrence of flow marks is suppressed.
[0091] As yet another preferred example, the (D) copolymer may contain 0.005 to 5 parts by weight of a polyfunctional acrylic monomer based on 100 parts by weight of a mixture containing 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound. In this case, there is an advantage that the fluidity and die swell ratio are excellent, and therefore the occurrence of flow marks is suppressed.
[0092] The types of the aromatic vinyl compound and the vinyl cyan compound contained in the copolymer (D) may be within the same category as the types of the aromatic vinyl compound and the vinyl cyan compound contained in the graft copolymer (A-1) described herein.
[0093] The polyfunctional mercaptan compound may be, for example, one or more selected from the group consisting of trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptoacetate), trimethylolpropane tris(4-mercaptobutanate), trimethylolpropane tris(5-mercaptopentanate), trimethylolpropane tris(6-mercaptohexanate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(4-mercaptobutanate), pentaerythritol tetrakis(5-mercaptopentanate), and pentaerythritol tetrakis(6-mercaptohexanate).
[0094] The polyfunctional acrylic monomer may be, for example, at least one selected from the group consisting of ethylene dimethacrylate, diethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, and allyl acrylate.
[0095] The copolymer (D) may be produced by emulsion polymerization, bulk polymerization, or suspension polymerization, and preferably by emulsion polymerization, which has the advantage of producing a uniform ultra-high molecular weight resin.
[0096] thermoplastic resin composition As an example, the thermoplastic resin composition may satisfy the following formula 1 when the weight percentages of (A-1), (A-2), (B) and (C) are a, b, c and d, respectively. In this case, the thermoplastic resin composition has an advantage of being excellent in fluidity and die swell ratio, thereby suppressing the occurrence of flow marks.
[0097] [Formula 1] a≦d <b≦c
[0098] Here, a may be an integer from 5 to 20, an integer from 7 to 20, an integer from 7 to 15, or an integer from 7 to 12.
[0099] Here, b may be an integer from 26 to 35, an integer from 28 to 35, an integer from 26 to 32, or an integer from 28 to 32.
[0100] Here, c may be an integer from 35 to 60, an integer from 35 to 55, an integer from 38 to 55, or an integer from 38 to 52.
[0101] Here, d may be an integer from 6 to 25, an integer from 8 to 25, an integer from 6 to 20, an integer from 8 to 20, or an integer from 8 to 15.
[0102] As a specific example, the thermoplastic resin composition can satisfy the following mathematical formula 1-1. In this case, there is an effect that the balance of physical properties is excellent and no flow marks are generated, resulting in excellent appearance quality.
[0103] [Formula 1-1] a <d<b<c
[0104] Here, a may be an integer from 5 to 20, an integer from 7 to 20, an integer from 7 to 15, or an integer from 7 to 12.
[0105] Here, b may be an integer from 26 to 35, an integer from 28 to 35, an integer from 26 to 32, or an integer from 28 to 32.
[0106] Here, c may be an integer from 35 to 60, an integer from 35 to 55, an integer from 38 to 55, or an integer from 38 to 52.
[0107] Here, d may be an integer from 6 to 25, an integer from 8 to 25, an integer from 6 to 20, an integer from 8 to 20, or an integer from 8 to 15.
[0108] As an example, the thermoplastic resin composition may satisfy the following formula 2 when the weights of (A-1), (A-2), (B) and (C) are a, b, c and d, respectively. In this case, the thermoplastic resin composition has an advantage of being excellent in fluidity and die swell ratio, thereby suppressing the occurrence of flow marks.
[0109] [Formula 2] 0.3≦[(a+b) / (c+d)]<0.8
[0110] Here, a may be an integer from 5 to 20, an integer from 7 to 20, an integer from 7 to 15, or an integer from 7 to 12.
[0111] Here, b may be an integer from 26 to 35, an integer from 28 to 35, an integer from 26 to 32, or an integer from 28 to 32.
[0112] Here, c may be an integer from 35 to 60, an integer from 35 to 55, an integer from 38 to 55, or an integer from 38 to 52.
[0113] Here, d may be an integer from 6 to 25, an integer from 8 to 25, an integer from 6 to 20, an integer from 8 to 20, or an integer from 8 to 15.
[0114] As a specific example, the thermoplastic resin composition can satisfy the following formula 2-1. In this case, there is an effect that the balance of physical properties is excellent and no flow marks are generated, resulting in excellent appearance quality.
[0115] [Formula 2-1] 0.3≦[(a+b) / (c+d)]≦0.75
[0116] Here, a may be an integer from 5 to 20, an integer from 7 to 20, an integer from 7 to 15, or an integer from 7 to 12.
[0117] Here, b may be an integer from 26 to 35, an integer from 28 to 35, an integer from 26 to 32, or an integer from 28 to 32.
[0118] Here, c may be an integer from 35 to 60, an integer from 35 to 55, an integer from 38 to 55, or an integer from 38 to 52.
[0119] Here, d may be an integer from 6 to 25, an integer from 8 to 25, an integer from 6 to 20, an integer from 8 to 20, or an integer from 8 to 15.
[0120] As a preferred example, the thermoplastic resin composition can satisfy the following formula 2-2. In this case, there is an effect that the balance of physical properties is excellent and no flow marks are generated, resulting in excellent appearance quality.
[0121] [Formula 2-2] 0.3≦[(a+b) / (c+d)]≦0.7
[0122] Here, a may be an integer from 5 to 20, an integer from 7 to 20, an integer from 7 to 15, or an integer from 7 to 12.
[0123] Here, b may be an integer from 26 to 35, an integer from 28 to 35, an integer from 26 to 32, or an integer from 28 to 32.
[0124] Here, c may be an integer from 35 to 60, an integer from 35 to 55, an integer from 38 to 55, or an integer from 38 to 52.
[0125] Here, d may be an integer from 6 to 25, an integer from 8 to 25, an integer from 6 to 20, an integer from 8 to 20, or an integer from 8 to 15.
[0126] When the thermoplastic resin composition described herein simultaneously satisfies the above-mentioned formula 1 and formula 2, it is more preferable since it has the advantage that the fluidity and weather resistance are equal to or similar to those of conventional ASA resin compositions, and at the same time, it has an excellent die swelling ratio and thus suppresses the occurrence of flow marks.
[0127] When the thermoplastic resin composition described herein satisfies the conditions of the following mathematical formula 3, it has the advantage that the fluidity and weather resistance are equivalent to or similar to those of conventional ASA resin compositions, and at the same time, it has an excellent die swell ratio, thereby suppressing the occurrence of flow marks.
[0128] [Formula 3] 380≦flow index×die swell ratio×spiral×content of processing aids≦1400 (In the above formula 3, the flow index is a value (unit: g / 10 min) measured at 220° C. and a load of 10 kg for the thermoplastic resin composition, the die swell ratio is a value calculated by the following formula 4, the spiral is the length (unit: cm) of a test piece injected using a spiral die (2.0T) under conditions of an injection temperature of 300° C., a die temperature of 80° C., and a pressure of 500 kgf using an injection molding machine (Engel, Victory 80), and the content of the processing aid is the amount (parts by weight) of the (D) copolymer used based on 100 parts by weight of the total amount of the base resin and the aromatic vinyl compound-vinyl cyan compound copolymer.)
[0129] [Formula 4] Die swell ratio = D ex / D0 (In the above formula 4, D0 is the diameter of the die, 2 mm, and D ex is the diameter (unit: mm) of the extrusion test piece extruded at 220°C and a load of 10 kg using a fluidity tester (Melt Indexer, MI) with a die diameter of 2 mm (D0).
[0130] The formula 3 preferably satisfies the range of 400 to 1300. In this case, there are effects that the fluidity and weather resistance are excellent, the occurrence of flow marks is suppressed, and the appearance quality is excellent.
[0131] The thermoplastic resin composition is, for example, measured by measuring the diameter (D ex) and the die swell ratio calculated by the above formula 4 is 1.3 to 1.57, preferably 1.3 to 1.55, and more preferably 1.3 to 1.54. Within this range, there are effects that the impact resistance and fluidity are excellent, the occurrence of flow marks is suppressed, and the appearance quality is excellent.
[0132] For example, the thermoplastic resin composition is injected into a spiral mold (2.0T) using an injection molding machine (Engel, Victory 80) under conditions of an injection temperature of 300°C, a mold temperature of 80°C, and a pressure of 500 kgf, and the spiral length of a test piece is 21.1 cm or more, preferably 21.1 to 24.4 cm. Within this range, the thermoplastic resin composition has an excellent balance of physical properties and does not generate flow marks, resulting in excellent appearance quality.
[0133] The thermoplastic resin composition has, for example, a flow index of 6.7 g / 10 min or more, preferably 6.7 to 13.2 g / 10 min, as measured at 220° C. under 10 kg for 10 minutes in accordance with ASTM D1238. Within this range, the composition has an excellent balance of physical properties while preventing the occurrence of flow marks, resulting in excellent appearance quality.
[0134] The thermoplastic resin composition has, for example, a Charpy impact strength of 9 kJ / m, measured at 23° C. using a test piece having a thickness of 4 mm in accordance with ISO 179. 2 More than 10 kJ / m 2 More preferably, 10 to 15 kJ / m 2 , and more preferably 10.5 to 13 kJ / m 2 Within this range, there is an effect that the physical properties are well balanced and no flow marks are generated, resulting in excellent appearance quality.
[0135] For example, the thermoplastic resin composition was injected into a test piece of 40 mm x 200 mm using an injection machine (Engel 120MT) under conditions of an injection temperature of 240°C, a holding pressure of 50 bar, and an injection speed of 80 mm / s, and no flow marks were observed on the surface. In this case, the thermoplastic resin composition has an excellent balance of all physical properties and an improved appearance quality.
[0136] According to another embodiment of the present disclosure, the thermoplastic resin composition comprises (A-1) 5 to 20% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 400 to 600 nm, (A-2) 20 to 40% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 30 to 200 nm, (B) 30 to 60% by weight of a heat-resistant resin having a weight average molecular weight of 50,000 to 150,000 g / mol, and (C) 20 to 40% by weight of a heat-resistant resin having a weight average molecular weight of 50,000 to 150,000 g / mol. and (C) 100 parts by weight of a base resin containing 5 to 30% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 70,000 g / mol; and (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol; and the base resin may be contained in a weight ratio of (A-1):(A-2):(B):(C) of 1:2-3:4-5:1-2.
[0137] The thermoplastic resin composition may further contain, for example, 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, and more preferably 0.1 to 3 parts by weight, of one or more selected from the group consisting of lubricants, antioxidants, ultraviolet stabilizers, UV stabilizers, fluorescent brighteners, chain extenders, pigments, dyes, antibacterial agents, processing aids, metal deactivators, smoke suppressants, inorganic fillers, glass fibers, antifriction agents, and antiwear agents, based on 100 parts by weight of the base resin. In this case, there is an effect that the required physical properties are well realized without decreasing the inherent physical properties of the thermoplastic resin composition described herein.
[0138] Method for producing thermoplastic resin composition One example of the method for producing a thermoplastic resin composition according to the present invention is to mix (A-1) 5 to 20% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 400 to 600 nm, (A-2) 20 to 40% by weight of an acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an acrylate rubber having an average particle size of 30 to 200 nm, (B) a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol, and (C) a heat-resistant resin having a weight-average molecular weight of 100,000 g / mol. The method is characterized in that it comprises a step of kneading and extruding 100 parts by weight of a base resin containing (A) 30-60% by weight of a resin having a viscosity of 1000 nm or less, and (B) 5-30% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000-70,000 g / mol, and (C) 0.5-4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 1,000,000-10,000,000 g / mol, under conditions of 200-300°C and 100-500 rpm. In this case, the fluidity and weather resistance are equal to or higher than those of conventional ASA resin compositions, and the die swelling ratio is excellent, so that the occurrence of flow marks is suppressed and the appearance quality is excellent.
[0139] The method for producing the thermoplastic resin composition has all the technical features of the thermoplastic resin composition described above, and therefore, the description of the overlapping parts will be omitted.
[0140] The step of producing pellets using the extrusion kneader may be preferably performed at 200-300°C with a standard of 25-75 phi, more preferably at 210-260°C with a standard of 20-70 phi, within which stable extrusion is possible and kneading effect is excellent. At this time, the temperature is the temperature set in the cylinder, and phi means the outer diameter (unit: mm).
[0141] The extrusion kneader is not particularly limited as long as it is an extrusion kneader that is commonly used in the technical field to which the present invention pertains, and may be preferably a twin-screw extrusion kneader.
[0142] Molded product The molded article described herein is characterized by containing, as an example, the thermoplastic resin composition described herein. In this case, compared with conventional ASA resin compositions, the molded article has the effect of having equal or greater fluidity and weather resistance, and also has excellent appearance quality with the occurrence of flow marks being suppressed.
[0143] The method for producing a molded article described herein is characterized by including a step of injecting pellets produced by the method for producing a thermoplastic resin composition under conditions of an injection temperature of 200 to 300°C, an injection pressure of 60 to 100 bar, and a holding pressure of 30 to 65 bar. In such a case, there is an advantage that an injection molded article with high impact strength can be easily produced.
[0144] The injection temperature is preferably 220 to 280° C., more preferably 230 to 270° C., and within this range, there is an advantage that injection molded articles requiring complex designs can be easily produced.
[0145] The injection pressure is preferably 70 to 90 bar, more preferably 75 to 85 bar, and within this range, there is an advantage that injection molded articles requiring complex designs can be easily produced.
[0146] The above-mentioned holding pressure may be preferably 35 to 60 bar, more preferably 40 to 55 bar, and within this range, there is an advantage that injection molded products requiring complex designs can be easily produced.
[0147] The molded article may be used in automotive exterior applications, including side mirror housings, radiator grilles, or filters.
[0148] In describing the thermoplastic resin composition, its production method, and molded articles described herein, other conditions, equipment, etc. that are not explicitly described can be appropriately selected within the range commonly used in the art, and it is clearly stated that there are no particular limitations.
[0149] Below, preferred examples are presented to aid in understanding the present description. However, the following examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications also fall within the scope of the appended claims.
[0150] [Example] The materials used in the following examples and comparative examples are as follows. *(A-1) Graft copolymer: ASA graft copolymer containing 50% by weight of acrylate rubber with an average particle size of 400 to 600 nm, 13% by weight of acrylonitrile, and 37% by weight of styrene (LG Chemical's product name D927) *(A-2) Graft copolymer: ASA graft copolymer containing acrylate rubber with an average particle size of 30 to 200 nm (LG Chemical's product name D100) *(A-3) Graft copolymer: ASA graft copolymer containing 40% by weight of acrylate rubber with an average particle size of 300 to 600 nm, 15% by weight of acrylonitrile, and 45% by weight of styrene (LG Chemical's product name D928) *(B) Heat-resistant resin (α-methylstyrene 71% by weight, acrylonitrile 29% by weight, weight average molecular weight 80,000 to 100,000 g / mol, bulk-polymerized heat-resistant SAN resin, LG Chem product name 200UH) *(C-1) Aromatic vinyl compound-vinyl cyanide compound copolymer (weight average molecular weight 60,000 g / mol, suspension polymerization branched SAN resin (long chain branched SAN), product name EMI-200 by Find Blend Co.) *(C-2) Aromatic vinyl compound-vinyl cyanide compound copolymer (weight average molecular weight 80,000-120,000 g / mol, LG Chem product name S95RF) *(D) Ultra-high molecular weight SAN resin (styrene-acrylonitrile copolymer with 75% by weight of styrene, 25% by weight of acrylonitrile, and a weight average molecular weight of 2,000,000 to 5,000,000 g / mol, product name ZB-869 of Zibo Huaxing Additives Co., Ltd.)
[0151] Examples 1 to 3 and Comparative Examples 1 to 8 The ingredients and contents shown in Tables 1 and 2 below were put into a twin screw extruder, kneaded and extruded at a cylinder temperature of 240°C to produce pellets. The flow index of the produced pellets was measured. As additives, 0.3 wt% each of a lubricant and a UV stabilizer was added.
[0152] Thereafter, the mixture was injected at an injection temperature of 250° C. using an injection machine (Engel 120MT) to prepare test pieces for measuring physical properties.
[0153] [Test example] The properties of the test pieces prepared in Examples 1 to 3 and Comparative Examples 1 to 8 were measured by the following methods, and the results are shown in Tables 1 and 2 and FIG.
[0154] Measurement method *Flow index (g / 10 min): Measured at 220°C and 10 kg for 10 minutes in accordance with ASTM D1238.
[0155] *Charpy impact strength (kJ / m 2 ):Measured at 23°C on 4 mm thick test pieces in accordance with ISO 179.
[0156] * Die swell ratio: The diameter (D) of an extrusion sample extruded at 220°C and a load of 10 kg using a fluidity tester (Melt Indexer, MI) with a die diameter (D0) of 2 mm. ex ) was measured and calculated using the following formula 4. [Formula 4] Die swell ratio = D ex / D0 (In the above formula 4, D ex is the diameter of the extruded sample (mm), and D0 is the diameter of the die (mm).
[0157] *Spiral (unit: cm): Using an injection molding machine (Engel, Victory 80), the length of the test piece injected using a spiral mold (1.5T) was measured under the conditions of an injection temperature of 250°C, a mold temperature of 60°C, and a pressure of 500 kgf.
[0158] *Occurrence of flow marks: Using an injection machine (Engel 120MT), test pieces measuring 40mm x 200mm were injected under conditions of an injection temperature of 250°C, a holding pressure of 50bar, and an injection speed of 90mm / s. The test pieces were visually inspected for the occurrence of flow marks and rated as follows. Flow marks appear as V-shaped wavy patterns. ×: No flow marks on the surface △: Fine flow marks appear on the surface ○: Flow marks appear partially on the surface ◎: A large number of flow marks occur on the surface.
[0159] *Flow mark parameter: When the weight percentages of (A-1), (A-2), (B) and (C) are a, b, c and d, respectively, it is judged whether the following formula 1 is satisfied, and if it is satisfied, it is indicated with ○, and if it is not satisfied, it is indicated with ×. For reference, the mark ○ is related to the suppression of the occurrence of flow marks. [Formula 1] a≦d <b≦c
[0160] *Appearance quality parameter: The values calculated by the following Equation 3 are shown in the following Tables 1 and 2. For reference, when the value is within the range of 380 to 1400, it is determined that the balance of physical properties and appearance quality are excellent. [Formula 3] 380≦flow index×die swell ratio×spiral×content of processing aids≦1400
[0161] [Table 1]
[0162] [Table 2] (In Tables 1 and 2, the contents of (A-1), (A-2), (A-3), (B), (C-1) and (C-2) are in weight percent based on the total weight of these, and the content of (D) is in parts by weight based on 100 parts by weight of the total weight of (A-1), (A-2), (A-3), (B), (C-1) and (C-2).)
[0163] As shown in Tables 1 and 2, in comparison with Comparative Examples 1 to 9, Examples 1 to 3 according to the present invention have the same or higher Charpy impact strength, excellent flow index and die swell ratio, and suppressed occurrence of flow marks, and it was confirmed that they simultaneously satisfy the appropriate ranges of the above-mentioned Formula 1 and Formula 3.
[0164] Specifically, in Comparative Example 1, which does not contain (C) SAN resin and (D) ultra-high molecular weight SAN resin, the flow index was low, resulting in poor processability, the die swell ratio and spiral length were low, and a large number of flow marks occurred, so that the appropriate ranges of Equation 1 and Equation 3 were not satisfied.
[0165] In addition, in Comparative Examples 2 and 3, which did not contain (D) ultra-high molecular weight SAN resin, the die swell ratio was low and (C) flow marks occurred partially or in large quantities depending on the amount of SAN resin used, and the appropriate range of Equation 3 was not satisfied.
[0166] In addition, (C) Comparative Examples 4 and 5, which did not contain SAN resin, had a low flow index, which reduced processability and slightly reduced spiral length. (D) Depending on the amount of ultra-high molecular weight SAN resin used, fine or partial flow marks occurred, and the appropriate ranges of Equation 1 and Equation 3 were not satisfied.
[0167] In addition, in Comparative Example 6, which contained the SAN resin (C) that was outside the appropriate molecular weight range, the die swell ratio was low and flow marks occurred, so that the appropriate range of Equation 3 was not satisfied.
[0168] In addition, in Comparative Example 7, which contained the graft copolymer (A) having a rubber with a medium diameter larger than the small diameter, the die swell ratio was low, the spiral length was outside of 24.4 cm, and poor injection moldability occurred, and the appropriate range of Equation 3 was not satisfied.
[0169] In addition, in Comparative Example 8 in which an excessive amount of (D) ultra-high molecular weight SAN resin was used, a spiral drop occurred and the appropriate range of Equation 3 was not satisfied.
[0170] FIG. 1 below shows the observation of the occurrence of flow marks on the test pieces injected from Example 1, Comparative Examples 1, 3, and 5, respectively. It was confirmed that Example 1 did not generate flow marks and had excellent appearance quality.
[0171] On the other hand, in Comparative Examples 1, 3, and 5, many wavy flow marks occurred on the test pieces, and the appearance quality was deteriorated.
[0172] Considering these results, by adjusting the die swell ratio of a 5-component thermoplastic resin composition containing a graft copolymer containing acrylate rubbers with different average particle sizes, a heat-resistant resin, and a thermoplastic copolymer in different molecular weight ranges, the synergistic effect of the combination of these components can provide excellent fluidity and weather resistance, as well as suppress the occurrence of flow marks and improve appearance quality, making it possible to confirm that the resin composition is suitable for use as an exterior material with excellent product reliability.
Claims
1. 100 parts by weight of a base resin including (A-1) an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 400 to 600 nm, (A-2) an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 30 to 200 nm, (B) a heat-resistant resin having a weight-average molecular weight of 50,000 to 150,000 g / mol, and (C) an aromatic vinyl compound-vinyl cyan compound copolymer having a weight-average molecular weight of 50,000 to 70,000 g / mol; (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol.
2. The thermoplastic resin composition according to claim 1, wherein the weight percentages of (A-1), (A-2), (B) and (C) are a, b, c and d, respectively, and the following mathematical formula 1 is satisfied. [Formula 1] a≦d<b≦c (In the above formula, a is an integer from 5 to 20, b is an integer from 26 to 40, c is an integer from 30 to 60, and d is an integer from 6 to 25.)
3. The thermoplastic resin composition according to claim 1 or 2, characterized in that the base resin is contained in a weight ratio of (A-1):(A-2):(B):(C) of 1:2-3:4-5:1-2.
4. The aromatic vinyl compound-vinyl cyan compound copolymer (D) has an intrinsic viscosity (IV, 25° C.) of 10 dL / g or more and a bulk density of 0.1 to 0.5 g / cm 3 2. The thermoplastic resin composition according to claim 1, characterized in that the weight average molecular weight is greater than 1,000,000 g / mol.
5. The thermoplastic resin composition according to claim 4, wherein the aromatic vinyl compound-vinyl cyan compound copolymer (D) is a copolymer containing 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound.
6. The thermoplastic resin composition according to claim 1, wherein the total amount of (A-1) and (A-2) is 40% by weight or less based on 100% by weight of the total content of all components constituting the base resin.
7. The thermoplastic resin composition according to claim 1, wherein the heat-resistant resin (B) comprises 60 to 80% by weight of an α-methylstyrene monomer and 20 to 40% by weight of a vinyl cyan compound.
8. The thermoplastic resin composition according to claim 1, wherein the (A-1) acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer comprises 40 to 60% by weight of an acrylate rubber, 25 to 45% by weight of an aromatic vinyl compound, and 5 to 20% by weight of a vinyl cyan compound, based on a total of 100% by weight.
9. The thermoplastic resin composition according to claim 1, wherein the (A-2) acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer comprises 40 to 60% by weight of an acrylate rubber, 25 to 45% by weight of an aromatic vinyl compound, and 5 to 20% by weight of a vinyl cyan compound, based on a total of 100% by weight.
10. The thermoplastic resin composition according to claim 1, wherein the aromatic vinyl compound-vinyl cyan compound copolymer (C) comprises 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound.
11. (A-1) 5 to 20% by weight of an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 400 to 600 nm, (A-2) 20 to 40% by weight of an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 30 to 200 nm, (B) 30 to 60% by weight of a heat-resistant resin having a weight average molecular weight of 50,000 to 150,000 g / mol, and (C) 5 to 30% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 70,000 g / mol; and (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol. The base resin is a thermoplastic resin composition, characterized in that the weight ratio of (A-1):(A-2):(B):(C) is 1:2-3:4-5:1-2.
12. The thermoplastic resin composition according to claim 1 or 11, wherein the thermoplastic resin composition satisfies the condition of the following mathematical formula 3. [Formula 3] 380≦flow index×die swell ratio×spiral×content of processing aid≦1400 (In the above formula 3, the flow index is a value (unit: g / 10 min) measured at 220° C. and a load of 10 kg according to ASTM D1238 for the thermoplastic resin composition, the die swell ratio is a value calculated by the following formula 4, the spiral is a length (unit: cm) of a test piece injected using a spiral die (2.0T) under conditions of an injection temperature of 300° C., a die temperature of 80° C., and a pressure of 500 kgf using an injection molding machine (Engel, Victory 80), and the content of the processing aid is the amount (parts by weight) of the (D) copolymer used based on 100 parts by weight of the total amount of the base resin and the aromatic vinyl compound-vinyl cyan compound copolymer.) [Formula 4] Die swell ratio = D ex / D 0 (In the above formula 4, D 0 is the diameter of the die, 2 mm; D ex is the diameter of the die 2 mm (D 0 ) is the diameter (unit: mm) of an extruded test piece extruded at 220°C under a load of 10 kg using a fluidity tester (Melt Indexer, MI).
13. The thermoplastic resin composition according to claim 12, wherein the formula (3) satisfies the range of 400 to 1300, the flow index is 6.7 to 13.2 g / 10 min, the die swell ratio is 1.31 to 1.54, and the spiral is 21.1 to 24.4 cm.
14. (A-1) 5 to 20% by weight of an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 400 to 600 nm, (A-2) 20 to 40% by weight of an acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an acrylate rubber having an average particle diameter of 30 to 200 nm, (B) 30 to 60% by weight of a heat-resistant resin having a weight average molecular weight of 50,000 to 150,000 g / mol. (C) 100 parts by weight of a base resin containing 5 to 30% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 70,000 g / mol; and (D) 0.5 to 4 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 1,000,000 to 10,000,000 g / mol; and kneading and extruding the mixture under conditions of 200 to 300° C. and 100 to 500 rpm, The base resin is contained in a weight ratio of (A-1):(A-2):(B):(C) of 1:2-3:4-5:1-2.
15. A molded article comprising the thermoplastic resin composition according to claim 1 or 11.
Citation Information
Patent Citations
Aqueous dispersion composition and its preparation
JP1982137339A
Thermoplastic resin composition and molded product using the same
KR101974164B1
Thermoplastic resin composition and molded product using same
WO2019190298A1
Thermoplastic resin composition, method for preparing the same, and molding article prepared therefrom
KR1020220000554A