Thermoplastic resin composition, its method of manufacture and molded article containing same
The thermoplastic resin composition addresses the limitations of recycled resins by using a specific core-shell structure and matrix resin blend, ensuring superior physical properties and environmental sustainability.
Patent Information
- Application Number
- JP2024508737
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-14
- Filing Date
- 2023-07-24
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-07-24
AI Technical Summary
Existing thermoplastic resin compositions face challenges in incorporating recycled resins due to issues with moldability, mechanical rigidity, appearance quality, flexibility, chemical resistance, and thermal stability, which are inferior to virgin resins, limiting their use in large quantities.
A thermoplastic resin composition comprising an alkyl acrylate rubber core with an aromatic vinyl compound-vinyl cyanide compound copolymer shell and a matrix resin containing recycled polystyrene and polyarylene oxide, optimized for particle size, molecular weight, and composition ratios to enhance physical properties.
The composition achieves excellent moldability, impact strength, tensile strength, heat resistance, and colorability while being environmentally friendly, allowing for the use of recycled resins without compromising performance.
Smart Images

Figure 2024539815000001 
Figure 2024539815000002 
Figure 2024539815000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0136778 filed on October 21, 2022 and Korean Patent Application No. 10-2023-0091902 refiled on July 14, 2023 based thereon, and all contents disclosed in the documents of the Korean patent application are incorporated as part of this specification.
[0002] The present invention relates to a thermoplastic resin composition, a method for producing the same, and a molded article containing the same. The present invention relates to a thermoplastic resin composition which has excellent physical properties such as moldability, impact strength, tensile strength, heat resistance, and colorability, and is advantageous in that it contains recycled resins and is therefore environmentally friendly, a method for producing the same, and a molded article containing the same. [Background technology]
[0003] Acrylonitrile-butadiene-styrene resin (hereinafter referred to as "ABS resin") based on conjugated diene rubber has been used in a variety of fields due to its excellent moldability, mechanical properties and appearance characteristics. However, because it is based on butadiene rubber, which has chemically unstable unsaturated bonds, it has problems such as poor weather resistance and easily ages when exposed to ultraviolet rays. As a possible alternative material, an acrylate compound-styrene-acrylonitrile copolymer (hereinafter referred to as "ASA resin"), which has excellent weather resistance, has been proposed.
[0004] ASA resin has excellent weather resistance, aging resistance and chemical resistance, as well as moldability, rigidity, impact resistance and processability, so it is widely used in a variety of fields, regardless of indoor or outdoor use, such as electrical and electronic parts, building materials, automotive interior and exterior materials, ships and leisure goods.
[0005] On the other hand, plastics, which are consumed in large quantities in modern society due to their convenience, do not decompose naturally, so there is a gradual increase in demand for waste disposal and utilization methods. In addition, there is a trend toward making the use of recycled resins mandatory as part of environmental regulations.
[0006] However, recycled resins age due to impact, abrasion, heat, UV rays, humidity, high and low temperature environments during the manufacturing, consumption and disposal processes, and are contaminated by the inflow of foreign matter, resulting in problems such as inferior moldability, mechanical rigidity, appearance quality, flexibility, chemical resistance and thermal stability compared to newly polymerized virgin resins. Therefore, unless a small amount of recycled resin is used, even mixing it with virgin resin is insufficient to solve these problems.
[0007] Therefore, there is an urgent need to develop a recycled resin composition that contains a certain level of recycled resin and yet exhibits physical properties that are applicable to existing plastic material fields. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent No. 10-1271250 Summary of the Invention [Problem to be solved by the invention]
[0009] In order to solve the problems of the conventional techniques as described above, an object of the present invention is to provide a thermoplastic resin composition which contains recycled resins and is therefore environmentally friendly, and which has excellent moldability, impact strength, tensile strength, heat resistance and colorability, a method for producing the same, and a molded article produced from the same.
[0010] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]
[0011] In order to achieve the above object, the present invention provides a rubber composition comprising: (A) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer including an alkyl acrylate rubber core having an average particle size of 60 to 200 nm and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the alkyl acrylate rubber core; and (B) a matrix resin, the copolymer shell of the graft copolymer (A) comprises, relative to a total of 100% by weight, 85 to 99% by weight of an aromatic vinyl compound and 1 to 15% by weight of a vinyl cyan compound, and has a weight average molecular weight of 100,000 to 400,000 g / mol; The thermoplastic resin composition is characterized in that the (B) matrix resin contains 50 to 90% by weight of recycled polystyrene and 8 to 50% by weight of polyarylene oxide, relative to a total of 100% by weight of the matrix resin.
[0012] The thermoplastic resin composition may preferably contain 20 to 60% by weight of the graft copolymer (A) and 40 to 80% by weight of the matrix resin (B), relative to 100% by weight in total of the graft copolymer (A) and the matrix resin (B).
[0013] The (A) graft copolymer may preferably comprise 40 to 70% by weight of the alkyl acrylate rubber core and 30 to 60% by weight of the copolymer shell, with the total being 100% by weight.
[0014] The (A) graft copolymer may preferably contain a polymer seed containing one or more compounds selected from the group consisting of alkyl (meth)acrylates, aromatic vinyl compounds, and vinyl cyan compounds. In this case, the (A) graft copolymer may preferably contain 1 to 20% by weight of the polymer seed, 35 to 65% by weight of the alkyl acrylate rubber core, and 30 to 60% by weight of the copolymer shell.
[0015] The recycled polystyrene may preferably include any one selected from the group consisting of recycled non-expanded polystyrene, recycled expanded polystyrene, and a mixture thereof.
[0016] The recycled polystyrene may preferably have a weight average molecular weight of 100,000 to 350,000 g / mol.
[0017] The (B) matrix resin may further preferably contain virgin general purpose polystyrene (GPPS). In this case, the matrix resin may contain 50 to 90% by weight of recycled polystyrene, 8 to 45% by weight of polyarylene oxide, and 1 to 30% by weight of virgin general purpose polystyrene.
[0018] The (B) matrix resin may further contain, for example, an aromatic vinyl compound-vinyl cyan compound copolymer, preferably an aromatic vinyl compound-vinyl cyan compound copolymer containing 75 to 95% by weight of an aromatic vinyl compound and 5 to 25% by weight of a vinyl cyan compound. In this case, the (B) matrix resin may contain 1 to 15% by weight of the aromatic vinyl compound-vinyl cyan compound copolymer relative to a total of 100% by weight of the (B) matrix resin.
[0019] The thermoplastic resin composition may preferably contain (C) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer including an alkyl acrylate rubber core having an average particle size of more than 200 nm and not more than 500 nm, and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the alkyl acrylate rubber core. In this case, the content of the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may be 0.1 to 12 parts by weight based on 100 parts by weight in total of the graft copolymer (A) and the matrix resin (B).
[0020] The thermoplastic resin composition may preferably contain 0.1 to 7 parts by weight of (D) a light stabilizer based on 100 parts by weight in total of the (A) graft copolymer and the (B) matrix resin.
[0021] The thermoplastic resin composition may preferably have a heat distortion temperature (HDT) of 82° C. or higher, measured under a load of 18.5 kgf in accordance with ASTM D 648.
[0022] The thermoplastic resin composition preferably has a tensile strength of 400 kgf / cm2 measured at a speed of 50 mm / min according to ASTM D 638. 2 It may be more than that.
[0023] The present invention also provides a method for producing a thermoplastic resin composition, comprising the steps of kneading and extruding (A) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer including an alkyl acrylate rubber core having an average particle size of 60 to 200 nm and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the alkyl acrylate rubber core, and (B) a matrix resin, under conditions of 180 to 300°C and 100 to 400 rpm, wherein the copolymer shell of the (A) graft copolymer contains, relative to its total 100% by weight, 85 to 99% by weight of an aromatic vinyl compound and 1 to 15% by weight of a vinyl cyan compound and has a weight average molecular weight of 100,000 to 400,000 g / mol, and the (B) matrix resin contains, relative to its total 100% by weight, 50 to 90% by weight of recycled polystyrene and 8 to 50% by weight of a polyarylene oxide.
[0024] The present invention also provides a molded article comprising the thermoplastic resin composition. Effect of the Invention
[0025] According to the present invention, by incorporating recycled resin into an ASA-based resin composition, it is possible to provide a thermoplastic resin composition which is environmentally friendly and at the same time has excellent moldability, impact strength, tensile strength, heat resistance and colorability, a production method thereof, and a molded article produced therefrom. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The thermoplastic resin composition of the present invention, its production method and molded articles will be described in detail below.
[0027] The present inventors have been researching how to produce an environmentally friendly ASA-based resin composition containing recycled resin, while at the same time ensuring physical properties at a level that can replace existing virgin ASA resin-based compositions or higher. They have found that by adjusting the size and composition of the rubber core and shell of the virgin ASA resin that is partially added, and the composition ratio of recycled resin to virgin resin, etc., physical properties such as moldability, impact strength, and heat resistance are greatly improved. Based on this, they have continued their research and have completed the present invention.
[0028] The thermoplastic resin composition of the present invention comprises (A) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer including an alkyl acrylate rubber core having an average particle size of 60-200 nm and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the alkyl acrylate rubber core, and (B) a matrix resin, wherein the copolymer shell of the graft copolymer (A) comprises 85-99% by weight of an aromatic vinyl compound and 1-15% by weight of a vinyl cyan compound relative to the total of 100% by weight, and has a weight average molecular weight of 100,000-400,000 g / mol, and the matrix resin (B) comprises 50-90% by weight of recycled polystyrene and 8-50% by weight of a polyarylene oxide relative to the total of 100% by weight, and in this case, the inclusion of recycled resins provides the effect of being environmentally friendly and excellent in moldability, impact strength, tensile strength, heat resistance and colorability.
[0029] In this description, the component ratio of a copolymer or resin may refer to the content of units constituting the copolymer, or the content of monomers added during polymerization of the copolymer.
[0030] In this description, a polymer comprising a certain compound means a polymer polymerized containing that compound, where the units in the polymerized polymer are derived from that compound.
[0031] In this description, the recycled thermoplastic resin is not particularly limited as long as it is generally recognized as a recycled thermoplastic resin in the technical field to which the present invention belongs, as long as it follows the definition of the present invention, and for example, it is a thermoplastic resin recycled from recovered waste plastic, and for example, it means a thermoplastic resin prepared in a usable raw material state after sorting, washing and crushing recovered waste plastic. In addition, if necessary, a material processed into pellets through an extrusion process can be used, and in this case, there is an advantage that additional processing such as purification is not required. Since such a recycled thermoplastic resin has been processed one or more times, it may contain residual additives such as colorants, lubricants and / or release agents.
[0032] In this description, non-recycled thermoplastic resins are contrasted with the recycled thermoplastic resins defined above, and may be prepared by directly polymerizing monomers constituting the thermoplastic resin, or may be a corresponding available product, and may be referred to as a virgin resin, for example.
[0033] Hereinafter, the thermoplastic resin composition of the present invention will be described in detail with respect to each component.
[0034] (A) Alkyl acrylate-aromatic vinyl compound-vinyl cyanide graft copolymer The alkyl acrylate rubber-aromatic vinyl compound-vinyl cyanide compound graft copolymer (hereinafter referred to as "(A) graft copolymer") having an average particle diameter of the rubber core of 60 to 200 nm may be contained in an amount of 20 to 65% by weight or 20 to 60% by weight, preferably 25 to 60% by weight, more preferably 30 to 58% by weight, and even more preferably 35 to 55% by weight, based on 100% by weight of the total of the (A) graft copolymer and the (B) matrix resin. In this case, there are advantages in that the molding processability, impact strength, tensile strength, heat resistance, and colorability are all excellent, along with environmental friendliness.
[0035] For example, the (A) graft copolymer may be contained in an amount of 40 to 58% by weight, preferably 40 to 55% by weight, and more preferably 40 to 50% by weight, relative to 100% by weight of the total of the (A) graft copolymer and the (B) matrix resin. In this case, there are advantages such as further excellent environmental friendliness, moldability, tensile strength, and heat resistance.
[0036] For example, the (A) graft copolymer may be contained in an amount of 45 to 60% by weight, preferably 48 to 60% by weight, and more preferably 50 to 60% by weight, based on 100% by weight of the total of the (A) graft copolymer and the (B) matrix resin. In this case, there is an advantage that the impact strength and colorability are further improved.
[0037] The (A) graft copolymer, for example, has an average particle size of 60 to 200 nm and comprises an alkyl acrylate rubber core containing an alkyl acrylate compound; and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the rubber core and containing an aromatic vinyl compound and a vinyl cyan compound. The copolymer shell may contain 85 to 99% by weight of the aromatic vinyl compound and 1 to 15% by weight of the vinyl cyan compound relative to the total of 100% by weight, and may have a weight average molecular weight of 100,000 to 400,000 g / mol. In this case, even if recycled resin is contained, there is an advantage that all of the moldability, impact strength, tensile strength, heat resistance and colorability are excellent.
[0038] In the present description, the average particle size of the polymer seed, rubber core or graft shell of the graft copolymer is not particularly limited as long as it is measured by a method commonly used in the technical field to which the present invention belongs, including an electron microscope measurement method using SEM, TEM, etc. For example, samples are taken at the time when the preparation of the polymer seed, the preparation of the rubber core and the preparation of the graft shell are completed, and the average particle size can be measured using a dynamic light scattering method. In detail, the intensity value is measured in Gaussian mode using a particle size analyzer (product name: Nicomp380, manufacturer: PSS). In this case, as a specific measurement example, a sample is prepared by diluting 0.1g of latex (total solid content TSC 35-50wt%) 1,000-5,000 times with deionized water or distilled water, i.e., diluting appropriately so as not to deviate significantly from the intensity setpoint of 300kHz, and putting it into a glass tube. The measurement method is auto-dilution and measurement with a flow cell, the measurement mode is dynamic light scattering / intensity 300KHz / intensity-weight Gaussian analysis, and the setting values are a temperature of 23°C and a measurement wavelength of 632.8nm.
[0039] In this description, unless otherwise specified, the weight average molecular weight can be measured using GPC (gel permeation chromatography, water breeze), and as a specific example, it can be measured as a relative value to a standard PS (standard polystyrene) sample through GPC using THF (tetrahydrofuran) as an eluent. At this time, as a specific measurement example, the measurement can be performed under the following conditions: solvent: THF, column temperature: 40°C, flow rate: 0.3 ml / min, sample concentration: 20 mg / ml, injection amount: 5 μl, column model: 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B Guard (50×4.6 mm), equipment name: Agilent 1200 series system, refractive index detector: Agilent G1362 RID, RI temperature: 35°C, data processing: Agilent ChemStation S / W, test method (Mn, Mw and PDI): OECD TG 118.
[0040] In this description, the copolymer (shell) grafted to the rubber (core) can be separated from the rubber (core) by a separation method commonly used in the technical field to which the present invention pertains in order to measure the weight average molecular weight. For example, the sol from which the insoluble matter (gel) has been separated by the method described in the graft ratio measurement method described below can be dissolved in THF solvent to prepare a solution, which can then be filtered through a filter to obtain a filtrate, which can be used as a sample for measuring the weight average molecular weight.
[0041] The (A) graft copolymer may, for example, comprise 40 to 70% by weight of an alkyl acrylate rubber core and 30 to 60% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer shell based on a total of 100% by weight, preferably 40 to 65% by weight of an alkyl acrylate rubber core and 35 to 60% by weight of a copolymer shell, more preferably 42 to 63% by weight of an alkyl acrylate rubber core and 37 to 58% by weight of a copolymer shell, and even more preferably 45 to 60% by weight of an alkyl acrylate rubber core and 40 to 55% by weight of a copolymer shell. In this case, there is an advantage that compatibility with a matrix resin is improved, and excellent effects of improving moldability, impact strength, tensile strength, heat resistance and colorability are obtained.
[0042] The (A) graft copolymer may, for example, comprise: a polymer seed comprising at least one selected from the group consisting of an alkyl (meth)acrylate, an aromatic vinyl compound, and a vinyl cyan compound; an alkyl acrylate rubber core surrounding the polymer seed; and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the rubber core. As a specific example, the (A) graft copolymer may contain, based on its total weight, 1 to 20% by weight of polymer seed, 35 to 65% by weight of alkyl acrylate rubber core, and 30 to 60% by weight of copolymer shell, preferably 2 to 18% by weight of polymer seed, 38 to 63% by weight of alkyl acrylate rubber core, and 30 to 60% by weight of copolymer shell, more preferably 3 to 15% by weight of polymer seed, 40 to 60% by weight of alkyl acrylate rubber core, and 35 to 55% by weight of copolymer shell, and even more preferably 5 to 10% by weight of polymer seed, 40 to 57% by weight of alkyl acrylate rubber core, and 35 to 52% by weight of copolymer shell. In this case, there is an advantage that compatibility with the matrix resin is improved, and excellent effects of improving moldability, impact strength, and gloss are obtained.
[0043] The polymer seed may, for example, comprise an alkyl acrylate, an aromatic vinyl compound, and a vinyl cyan compound, and preferably comprises an alkyl acrylate. In this case, there is an advantage in that the effect of improving moldability, impact strength, tensile strength, heat resistance, and colorability is excellent.
[0044] As another example, the polymer seed may contain one or more selected from the group consisting of alkyl methacrylate, aromatic vinyl compound, and vinyl cyan compound, and preferably may contain aromatic vinyl compound and vinyl cyan compound. As a specific example, based on the total weight of the polymer seed, the polymer seed may contain 50 to 90% by weight of aromatic vinyl compound and 10 to 50% by weight of vinyl cyan compound, preferably 55 to 85% by weight of aromatic vinyl compound and 15 to 45% by weight of vinyl cyan compound, more preferably 60 to 80% by weight of aromatic vinyl compound and 20 to 40% by weight of vinyl cyan compound, and within this range, there is an advantage that the appearance quality such as glossiness and colorability, mechanical properties, and moldability are further excellent.
[0045] The polymer seed of the graft copolymer (A) may have an average particle size of, for example, 40 to 140 nm, preferably 50 to 100 nm, and more preferably 60 to 90 nm. In this case, the average particle size of the polymer seed is smaller than the average particle size of the rubber core surrounding it, and within this range, there is an advantage that the moldability, impact strength, tensile strength, heat resistance, and colorability are further improved.
[0046] The rubber core of the graft copolymer (A) may have an average particle size of, for example, 60 to 200 nm, preferably 65 to 170 nm, more preferably 70 to 150 nm, even more preferably 80 to 120 nm, and preferably 100 to 150 nm. In this case, the average particle size of the rubber core is larger than the average particle size of the polymer seeds when the polymer seeds are contained, and within this range, there is an advantage that the moldability, impact strength, tensile strength, heat resistance and colorability are further improved.
[0047] In this description, the average particle size of the rubber core means the average particle size including the seeds, if the seeds are included.
[0048] The graft shell of the graft copolymer (A) may, for example, comprise 85 to 99% by weight of an aromatic vinyl compound and 1 to 15% by weight of a vinyl cyan compound, preferably 85 to 98% by weight of an aromatic vinyl compound and 2 to 15% by weight of a vinyl cyan compound, more preferably 90 to 98% by weight of an aromatic vinyl compound and 2 to 10% by weight of a vinyl cyan compound, and within these ranges, there are advantages in that the molding processability, impact strength and gloss are further improved.
[0049] The graft shell of the graft copolymer (A) may have a weight average molecular weight of, for example, 100,000 to 400,000 g / mol, preferably 110,000 to 395,000 g / mol, more preferably 120,000 to 350,000 g / mol, and even more preferably 130,000 to 300,000 g / mol. Within this range, there are advantages in that the molding processability, impact strength, and gloss are further improved.
[0050] In this description, alkyl (meth)acrylates can be defined as a range that includes both alkyl acrylates and alkyl methacrylates.
[0051] In the present description, the alkyl acrylate may be, for example, an alkyl acrylate having an alkyl group of 1 to 15 carbon atoms, preferably one or more selected from the group consisting of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylbutyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, hexyl acrylate, heptyl acrylate, n-pentyl acrylate, and lauryl acrylate, more preferably an alkyl acrylate containing an alkyl group having 1 to 4 carbon atoms, even more preferably n-butyl acrylate, 2-ethylhexyl acrylate, or a mixture thereof, and even more preferably butyl acrylate.
[0052] In the present description, the alkyl methacrylate may be, for example, an alkyl methacrylate having an alkyl group with 1 to 15 carbon atoms, preferably one or more selected from the group consisting of methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylbutyl methacrylate, 2-ethylhexyl methacrylate, and lauryl methacrylate, more preferably an alkyl methacrylate containing an alkyl group with 1 to 4 carbon atoms, and even more preferably methyl methacrylate.
[0053] In the present description, the aromatic vinyl compound may be, for example, one or more selected from the group consisting of styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, ethylstyrene, isobutylstyrene, t-butylstyrene, o-bromostyrene, p-bromostyrene, m-bromostyrene, o-chlorostyrene, p-chlorostyrene, m-chlorostyrene, vinyltoluene, vinylxylene, fluorostyrene, and vinylnaphthalene, and may be preferably styrene.
[0054] In the present description, the vinyl cyanide compound may be, for example, one or more selected from the group consisting of acrylonitrile, methacrylonitrile, ethyl acrylonitrile, and isopropyl acrylonitrile, and may be preferably acrylonitrile.
[0055] The graft copolymer (A) may have a graft ratio of, for example, 20% or more, preferably 20 to 100%, more preferably 25 to 80%, even more preferably 30 to 70%, and even more preferably 30 to 60%. Within this range, the graft copolymer has excellent mechanical properties such as impact resistance and also has excellent weather resistance.
[0056] As a specific measurement example, the graft ratio described herein is obtained by adding 30 g of acetone to 0.5 g of graft copolymer powder, stirring at room temperature at 210 rpm for 12 hours (SKC-6075, Lab Companion), centrifuging the mixture at 18,000 rpm for 3 hours at 0°C using a centrifuge (Supra R30, Hanil Science), and collecting only the insoluble matter (gel) that did not dissolve in acetone. The mixture is then dried at 85°C for 12 hours in a forced circulation method (OF-12GW, Lab Companion), and the weight is measured, and the result can be calculated using the following formula 1.
[0057] [Formula 1] Graft rate (%) = [grafted monomer weight (g) / rubber weight (g)] × 100
[0058] In the above formula 1, the weight (g) of the grafted monomer is the weight (g) of the insoluble matter obtained after dissolving the graft copolymer in acetone and centrifuging the insoluble matter minus the weight (g) of the rubbery matter, and the weight (g) of the rubbery matter is the weight (g) of the rubbery matter theoretically added to the graft copolymer powder.
[0059] The method for producing the graft copolymer (A) may, for example, include the steps of: i) preparing an alkyl acrylate rubber core by adding an alkyl acrylate; and ii) preparing a graft copolymer by adding an aromatic vinyl compound and a vinyl cyanide compound and graft polymerizing them in the presence of the rubber core. In this case, the graft copolymer has advantages in that it has excellent moldability, impact strength, and gloss.
[0060] The method for producing the graft copolymer (A) may preferably include the steps of: i) polymerizing 40 to 70% by weight of an alkyl acrylate with a crosslinking agent, an initiator and an emulsifier to produce a rubber core, based on a total of 100% by weight; and ii) graft polymerizing 30 to 60% by weight of an aromatic vinyl compound and a vinyl cyan compound with a crosslinking agent, an initiator and an emulsifier in the presence of the rubber core to produce a graft copolymer, in which case there are advantages in that the molding processability, impact strength and gloss are all excellent.
[0061] The method for producing the graft copolymer (A) may, for example, include the steps of: i) preparing a polymer seed including at least one selected from the group consisting of an alkyl (meth)acrylate, an aromatic vinyl compound, and a vinyl cyan compound; ii) preparing an alkyl acrylate rubber core including an alkyl acrylate in the presence of the polymer seed; and iii) preparing a graft copolymer by graft polymerization including an aromatic vinyl compound and a vinyl cyan compound in the presence of the rubber core. In this case, the method has the advantage of being excellent in moldability, impact strength, and gloss.
[0062] The method for producing the graft copolymer (A) may preferably include, based on a total of 100% by weight, i) a step of polymerizing 1 to 20% by weight of one or more selected from the group consisting of alkyl (meth)acrylates, aromatic vinyl compounds, and vinyl cyan compounds with an electrolyte, a crosslinking agent, an initiator, and an emulsifier to produce a polymer seed; ii) a step of polymerizing 35 to 65% by weight of alkyl acrylate with a crosslinking agent, an initiator, and an emulsifier in the presence of the polymer seed to produce a rubber core; and iii) a step of graft polymerizing 30 to 60% by weight of aromatic vinyl compounds and vinyl cyan compounds with a crosslinking agent, an initiator, and an emulsifier in the presence of the rubber core to produce a graft copolymer; in this case, there is an advantage that all of the molding processability, impact strength, and glossiness are excellent.
[0063] In this description, the content of a monomer in a polymer may refer to the weight % of the monomer added when the polymer is produced, or the weight % of the unit in the polymer in terms of the monomer.
[0064] The emulsifier used in each of the polymer seed production step (when a polymer seed is included), the rubber core production step, and the copolymer shell production step is not particularly limited as long as it is an emulsifier commonly used in the technical field to which the present invention belongs, and may be, for example, one or more selected from the group consisting of a metal salt of alkyl sulfosuccinate having 12 to 18 carbon atoms or a derivative thereof, an alkyl sulfate ester having 12 to 20 carbon atoms or a derivative thereof, a metal salt of alkyl sulfonate having 12 to 20 carbon atoms or a derivative thereof, a fatty acid soap, and a rosin acid soap.
[0065] The metal salt of alkyl sulfosuccinate having 12 to 18 carbon atoms or a derivative thereof may be preferably at least one selected from the group consisting of dicyclohexyl sulfosuccinate, dihexyl sulfosuccinate, di-2-ethylhexyl sulfosuccinate sodium salt, di-2-ethylhexyl sulfosuccinate potassium salt, dioctyl sulfosuccinate sodium salt, and dioctyl sulfosuccinate potassium salt.
[0066] The alkyl sulfate having 12 to 20 carbon atoms or a derivative thereof may be preferably one or more selected from the group consisting of sodium lauryl sulfate, sodium dodecyl sulfate, sodium dodecylbenzene sulfate, sodium octadecyl sulfate, sodium oleate sulfate, potassium dodecyl sulfate, and potassium octadecyl sulfate.
[0067] The fatty acid soap may preferably be one or more selected from the group consisting of sodium salts or potassium salts of oleic acid, stearic acid, lauric acid, and mixed fatty acids.
[0068] The rosin acid soap may preferably be an abietic acid salt, specifically, a metal abietic acid salt.
[0069] The emulsifier can be used in an amount of, for example, 0.01 to 5 parts by weight, preferably 0.1 to 4 parts by weight, and more preferably 1 to 3 parts by weight, based on a total of 100 parts by weight of the graft copolymer (A).
[0070] The initiator is not particularly limited, but a radical initiator can be preferably used.
[0071] The radical initiator may be, for example, one or more selected from the group consisting of inorganic peroxides, organic peroxides, peroxyketal peroxides, peroxycarbonate peroxides, and azo compounds.
[0072] The inorganic peroxide may preferably be one or more selected from the group consisting of sodium persulfate, potassium persulfate, ammonium persulfate, potassium perphosphate, and hydrogen peroxide.
[0073] Examples of the organic peroxide include t-butyl peroxide, cumene hydroperoxide, p-menthane hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)-hexane, di-t-amyl peroxide, 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy)-cyclohexane, 1,1-di(t-amylperoxide), t-Cyclohexane, ethyl 3,3-di(t-amylperoxy)butyrate, diisopropylbenzene monohydroperoxide, t-amyl hydroperoxide, t-butyl hydroperoxide, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, di-(3,3,5-trimethylhexanoyl)-peroxide, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxy-3,3,5-trimethylhexanoyl, t-amyl peroxyneo Decanoate, t-amyl peroxypivalate, t-amyl peroxy-2-ethylhexanoate, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-amyl peroxy 2-ethylhexyl carbonate, t-butyl peroxy 2-ethylhexyl carbonate, t-butyl peroxy isopropyl monocarbonate, t-butyl peroxymaleate, cumyl peroxy neodecanoate, 1,1,3,3-tetramethylbutyl peroxy neodecanoate, The peroxyalkylene oxide may be one or more selected from the group consisting of 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, di-2-ethylhexyl peroxydicarbonate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, acetyl peroxide, isobutyl peroxide, octanoyl peroxide, dibenzoyl peroxide, dilauroyl peroxide, 3,5,5-trimethylhexanol peroxide, and t-butyl peroxyisobutyrate.
[0074] The peroxyketal peroxide may be preferably one or more selected from the group consisting of 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 1,1-di(t-amylperoxy)cyclohexane, ethyl-3,3-di(t-butylperoxy)butyrate, and ethyl-3,3-di(t-amylperoxy)butyrate.
[0075] The peroxycarbonate peroxide may be preferably at least one selected from the group consisting of dicumylperoxide, di(t-butylperoxy)-m / p-diisopropylbenzene, 2,5-dimethyl-2,5-(t-butylperoxy)hexane, t-butylcumylperoxide, dialkylperoxide such as 2,5-methyl-2,5-(t-butylperoxy)hexyne-3, t-butylperoxy 2-ethylhexyl monocarbonate, and t-butylperoxybenzoate.
[0076] The azo compound may preferably be one or more selected from the group consisting of azobisisobutyronitrile, azobis-2,4-dimethylvaleronitrile, azobiscyclohexanecarbonitrile, and methyl azobisisobutyrate (butyrate).
[0077] In at least one of the steps of preparing the polymer seed (if the polymer seed is included), preparing the rubber core, and preparing the copolymer shell, an oxidation-reduction catalyst may be used together with the initiator to further promote the initiation reaction.
[0078] The oxidation-reduction catalyst may be, for example, one or more selected from the group consisting of sodium pyrophosphate, dextrose, ferrous sulfide, sodium sulfite, sodium formaldehyde sulfoxylate, and sodium ethylenediaminetetraacetate, and may be preferably a mixture of sodium pyrophosphate, dextrose, and ferrous sulfide, but is not limited thereto.
[0079] In at least one of the steps of preparing the polymer seed (if the polymer seed is included), preparing the rubber core, and preparing the copolymer shell, an activator may be used together with the polymerization initiator to promote the initiation reaction of the peroxide.
[0080] The activator is not particularly limited as long as it is an activator commonly used in the technical field to which the present invention pertains.
[0081] The activator may be added in an amount of 0.01 to 3 parts by weight, preferably 0.01 to 1 part by weight, based on 100 parts by weight of the total of the graft copolymer (A). Within this range, there is an advantage that a high degree of polymerization can be achieved.
[0082] The electrolyte may be, for example, KCl, NaCl, KHCO 3 , NaHCO 3 , K 2 CO 3 , Na 2 CO 3 , K.H.S.O. 3 , NaHSO 4 , Na 2 S 2 O 7 , K 3 P 2 O 7 , K 3 PO 4 , Na 3 PO 4 , KOH, NaOH and Na 2 HPO 4 One or more selected from the group consisting of, but not limited to, may be used.
[0083] The electrolyte may be added in an amount of 0.001 to 1 part by weight, preferably 0.01 to 0.5 parts by weight, based on 100 parts by weight of the total of the graft copolymer (A). Within this range, there is an advantage that a high degree of polymerization can be achieved.
[0084] In the present description, unless otherwise defined, the crosslinking agent is not particularly limited as long as it is a crosslinking agent commonly used in the technical field to which the present invention belongs. For example, a compound having an unsaturated vinyl group and capable of acting as a crosslinking agent, or a compound having an unsaturated vinyl group having two or more different reactivities may be used. Specific examples include polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, polypropylene glycol diacrylate, polypropylene glycol dimethacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, divinylbenzene, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, hexane ...
[0043] It is to be noted that the monomer may be one or more selected from the group consisting of, but is not limited to, allyl propoxylate diacrylate, neopentyl glycol dimethacrylate, neopentyl glycol ethoxylate diacrylate, neopentyl glycol propoxylate diacrylate, trimethylolpropane trimethacrylate, trimethylolmethane triacrylate, trimethylpropane ethoxylate triacrylate, trimethylpropane propoxylate triacrylate, pentaerythritol ethoxylate triacrylate, pentaerythritol propoxylate triacrylate, vinyltrimethoxysilane, allyl methacrylate, triallyl isocyanurate, triallylamine, and diallylamine.
[0085] The crosslinking agent can be used in an amount of, for example, 0.01 to 5 parts by weight, preferably 0.01 to 3 parts by weight, and more preferably 0.1 to 1 part by weight, based on a total of 100 parts by weight of the graft copolymer (A).
[0086] In the copolymer shell preparation step, for example, a molecular weight regulator may be used.
[0087] The amount of the molecular weight regulator may be, for example, 0.01 to 2 parts by weight, preferably 0.05 to 2 parts by weight, and more preferably 0.05 to 1 part by weight, based on 100 parts by weight of the total of the graft copolymer (A). Within this range, a polymer having a target molecular weight can be easily produced.
[0088] The molecular weight regulator may be, for example, one or more selected from the group consisting of α-methylstyrene dimer, t-dodecyl mercaptan, n-dodecyl mercaptan, octyl mercaptan, carbon tetrachloride, methylene chloride, methylene bromide, tetraethylthiuram disulfide, dipentamethylenethiuram disulfide, and diisopropylxanthogen disulfide, but is not limited thereto.
[0089] In this description, 100 parts by weight of the graft copolymer means 100 parts by weight of the total weight of the graft copolymer finally obtained, or, since almost all of the monomers added participate in the polymerization, it can conveniently mean the combined weight of all the monomers used in the polymer seed (if the polymer seed is included), the rubber core, and the graft shell, or the combined weight of the monomers added during the preparation of the polymer seed (if the polymer seed is included) and the rubber core, and the monomers added during the preparation of the graft shell, which is 100 parts by weight.
[0090] In this description, % means % by weight unless otherwise specified.
[0091] In the step of preparing the seeds and cores, the monomer may be added in a single batch or continuously, or the two methods may be combined.
[0092] In this description, "continuous addition" means not "adding all at once" and refers to, for example, addition drop by drop, little by little, step by step or continuous flow for 10 minutes or more, 30 minutes or more, 1 hour or more, preferably 2 hours or more within the polymerization reaction time range.
[0093] The (A) graft copolymer may be prepared by, for example, emulsion polymerization, in which case it has the effect of being excellent in chemical resistance, weather resistance, fluidity, tensile strength and impact strength.
[0094] The emulsion polymerization is not particularly limited as long as it is an emulsion polymerization method commonly used in the technical field to which the present invention pertains, and specifically may be emulsion graft polymerization.
[0095] The polymerization temperature during the emulsion polymerization is not particularly limited, but may be, for example, 50 to 85°C, and preferably 60 to 80°C.
[0096] The latex formed after polymerization of the graft copolymer (A) can be obtained in the form of a powder through, for example, a common process such as coagulation, washing, and drying. Specifically, the latex can be prepared in the form of a powder through a process of coagulation at a temperature of 60 to 100°C by adding a metal salt or an acid, aging, dehydration, washing, and drying, but is not limited thereto.
[0097] The graft copolymer (A) may be, for example, a commercially available product as long as it complies with the definition of the present invention.
[0098] (B) Matrix resin The (B) matrix resin may be contained in an amount of, for example, 35 to 80% by weight, or 40 to 80% by weight, preferably 40 to 75% by weight, more preferably 42 to 70% by weight, and even more preferably 45 to 65% by weight, relative to 100% by weight of the total of the (A) graft copolymer and the (B) matrix resin. In this case, by containing a certain level or more of recycled resin, there is an advantage that the molding processability, impact strength, tensile strength, and heat resistance are all excellent while being excellent in environmental friendliness.
[0099] For example, the (B) matrix resin may be contained in an amount of 48 to 60% by weight, preferably 45 to 60% by weight, and more preferably 50 to 60% by weight, relative to 100% by weight of the total of the (A) graft copolymer and the (B) matrix resin. In this case, there are advantages such as further improved environmental friendliness, moldability, tensile strength, and heat resistance.
[0100] For example, the (B) matrix resin may be contained in an amount of 40 to 55% by weight, preferably 40 to 52% by weight, and more preferably 40 to 50% by weight, relative to 100% by weight of the total of the (A) graft copolymer and the (B) matrix resin. In this case, there is an advantage that the impact strength and colorability are further improved.
[0101] The recycled polystyrene refers to a recycled resin of polystyrene (PS), which is a polymer derived from an aromatic vinyl compound.
[0102] The recycled polystyrene may be, for example, a recycled resin derived from a general purpose polystyrene (GPPS) resin and / or a high-impact polystyrene (HIPS) resin. In this case, even if conventional virgin polystyrene is replaced with the recycled resin, there is an advantage that the recycled resin provides physical properties equivalent to or exceeding those of virgin polystyrene.
[0103] The general-purpose polystyrene resin may be, for example, a homopolymer of an aromatic vinyl compound, preferably styrene.
[0104] The high-impact polystyrene resin may be, for example, a rubber-reinforced polystyrene resin containing rubber having an average particle size of 0.1 to 20 μm. The rubber contained in the high-impact polystyrene resin may be, for example, one or more selected from the group consisting of butadiene rubber, isoprene rubber, butadiene-styrene copolymer, and alkyl acrylate rubber.
[0105] The (B) matrix resin may, for example, contain 50 to 90% by weight of recycled polystyrene and 8 to 50% by weight of polyarylene oxide, relative to a total of 100% by weight, and may preferably contain 50 to 85% by weight of recycled polystyrene and 9 to 50% by weight of polyarylene oxide, or 50 to 80% by weight of recycled polystyrene and 10 to 48% by weight of polyarylene oxide, or 50 to 70% by weight of recycled polystyrene and 12 to 47% by weight of polyarylene oxide. Within these ranges, there are advantages in that the molding processability, impact strength, tensile strength and heat resistance are all excellent.
[0106] The (B) matrix resin may, for example, contain 50 to 68% by weight of recycled polystyrene and 25 to 50% by weight of polyarylene oxide, preferably 50 to 67% by weight of recycled polystyrene and 30 to 50% by weight of polyarylene oxide, or 50 to 65% by weight of recycled polystyrene and 35 to 50% by weight of polyarylene oxide, relative to a total of 100% by weight. Within these ranges, there are advantages in that the impact strength, tensile strength, heat resistance and colorability are further improved without deterioration of other physical properties.
[0107] As a specific example, it may contain 50 to 90% by weight of recycled polystyrene and 10 to 50% by weight of polyarylene oxide, preferably 50 to 85% by weight of recycled polystyrene and 15 to 50% by weight of polyarylene oxide, more preferably 52 to 80% by weight of recycled polystyrene and 20 to 48% by weight of polyarylene oxide, and even more preferably 53 to 70% by weight of recycled polystyrene and 30 to 47% by weight of polyarylene oxide. By containing a certain level or more of recycled resin within these ranges, it has the advantages of being environmentally friendly while also being excellent in all of moldability, impact strength, tensile strength, heat resistance and colorability.
[0108] In this description, resins not designated as regenerated or virgin can refer to preferably virgin resins, although both are possible.
[0109] The (B) matrix resin may, for example, contain virgin general-purpose polystyrene. In this case, there are advantages in that the moldability, impact strength, tensile strength and heat resistance are further improved.
[0110] As an example, the (B) matrix resin may contain, based on its total weight, 50 to 90% by weight of recycled polystyrene, 8 to 45% by weight of polyarylene oxide, and 0 to 30% by weight of virgin general-purpose polystyrene. A specific example is 50 to 90% by weight of recycled polystyrene, 8 to 45% by weight of polyarylene oxide, and 1 to 30% by weight of virgin general-purpose polystyrene, preferably 50 to 85% by weight of recycled polystyrene, 10 to 45% by weight of polyarylene oxide, and 2 to 28% by weight of general-purpose polystyrene, more preferably. Preferably, the composition may contain 50 to 75% by weight of recycled polystyrene, 13 to 42% by weight of polyarylene oxide, and 3 to 27% by weight of general-purpose polystyrene, more preferably 50 to 70% by weight of recycled polystyrene, 15 to 40% by weight of polyarylene oxide, and 3 to 27% by weight of general-purpose polystyrene, and even more preferably 50 to 65% by weight of recycled polystyrene, 15 to 40% by weight of polyarylene oxide, and 5 to 25% by weight of general-purpose polystyrene, and within these ranges, there is an advantage that the molding processability and balance of physical properties are further excellent.
[0111] The (B) matrix resin may further contain, for example, an aromatic vinyl compound-vinyl cyan compound copolymer (hereinafter referred to as "SAN-based resin") containing 70 to 95% by weight of an aromatic vinyl compound and 5 to 30% by weight of a vinyl cyan compound. In this case, there is an advantage that mechanical rigidity and weather resistance are further improved.
[0112] As a specific example, the SAN-based resin may be contained in an amount of 1 to 15 weight %, preferably 1 to 13 weight %, more preferably 2 to 12 weight %, even more preferably 2 to 10 weight %, and even more preferably 3 to 10 weight %, relative to a total of 100 weight % of the (B) matrix resin. In this case, there is an advantage that the mechanical rigidity and weather resistance are further improved without deteriorating other physical properties.
[0113] The aromatic vinyl compounds contained in the recycled polystyrene and the virgin general-purpose polystyrene may be appropriately selected from the aromatic vinyl compounds mentioned in the copolymer (A), and may be preferably styrene.
[0114] The general-purpose polystyrene may be, for example, a homopolymer of styrene.
[0115] The polystyrene is not particularly limited as long as it is a method generally used in the technical field to which the present invention belongs. As a specific example, an aromatic vinyl compound may be prepared by solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, or a mixture thereof, and the polymerization may be performed by thermal polymerization or in the presence of a polymerization initiator. The polymerization initiator that can be used in the polymerization may be, for example, a peroxide initiator, an azo initiator, or a mixture thereof. The peroxide initiator may be preferably at least one selected from the group consisting of benzoyl peroxide, t-butyl hydroperoxide, acetyl peroxide, and cumene hydroperoxide, and the azo initiator may be preferably azobisisobutyronitrile.
[0116] The recycled polystyrene may include, for example, recycled expanded polystyrene (EPS). The recycled polystyrene may include, for example, recycled non-expanded polystyrene alone; recycled expandable polystyrene alone; or a mixture of recycled non-expanded polystyrene and recycled expandable polystyrene. In this case, there is an advantage that a recycled resin composition having desired physical properties can be provided by using recycled polystyrene regardless of whether the recycled polystyrene is expanded or not.
[0117] As a specific example, the recycled polystyrene may contain 0-100% by weight of recycled non-expanded polystyrene and 0-100% by weight of recycled expandable polystyrene relative to its total 100% by weight. More specifically, the recycled polystyrene may contain 30-80% by weight of recycled non-expanded polystyrene and 20-70% by weight of recycled expandable polystyrene, preferably 40-75% by weight of recycled non-expanded polystyrene and 25-60% by weight of recycled expandable polystyrene, more preferably 45-75% by weight of recycled non-expanded polystyrene and 25-55% by weight of recycled expandable polystyrene relative to its total 100% by weight. Within this range, there is an advantage that the moldability, impact strength, tensile strength and heat resistance are further excellent while containing recycled resin.
[0118] The expanded polystyrene is chemically or physically expanded to contain air inside, providing heat retention and cushioning properties, and is mainly used as a heat-retaining / cushioning packaging material and building insulation material.
[0119] The expandable polystyrene is not particularly limited as long as it is generally recognized as expandable polystyrene in the technical field to which the present invention belongs. As a specific example, when a foaming agent is contained in polystyrene, polystyrene expanded containing 0.2 to 10 wt % of the foaming agent based on the total weight of the polystyrene may be used.
[0120] The foamed polystyrene is not particularly limited as long as it is produced by a method commonly used in the technical field to which the present invention pertains. As a specific example, the foamed polystyrene may be produced by a foaming process containing a melt of a polymer constituting the foamed polystyrene and a foaming agent.
[0121] In the case of the polystyrene foam, for example, a separate volume reduction process may be performed to reduce the expanded volume, or a commercially available volume-reduced product may be used, which has the advantage of being more efficient in production.
[0122] The recycled polystyrene may have a weight average molecular weight of, for example, 100,000 to 400,000 g / mol, preferably 110,000 to 350,000 g / mol, more preferably 130,000 to 300,000 g / mol, and even more preferably 150,000 to 280,000 g / mol. Within this range, the recycled polystyrene has the effect of providing excellent balance of physical properties and impact resistance.
[0123] The recycled polystyrene may have a glass transition temperature of, for example, 80 to 180°C, preferably 85 to 170°C, and more preferably 90 to 160°C. Within this range, the mechanical properties and moldability are further improved.
[0124] In this description, the glass transition temperature (Tg) can be measured, for example, in accordance with ASTM D 3418 using a differential scanning calorimetry (DSC, Q100, manufactured by TA Instruments) at a heating rate of 10° C. / min.
[0125] The recycled polystyrene may have a flow index of, for example, 20 to 60 g / 10 min, preferably 30 to 55 g / 10 min, and more preferably 40 to 50 g / 10 min, as measured at a temperature of 220° C. and under a load of 10 kg in accordance with ASTM D1238. Within this range, the recycled polystyrene has the effect of being excellent in moldability and balance of physical properties.
[0126] As the recycled polystyrene, for example, a commercially available product can be used as long as it complies with the definition of the present invention.
[0127] The weight average molecular weight, glass transition temperature, flow index, etc. of the general-purpose polystyrene may be appropriately selected within the same range as that of the recycled polystyrene.
[0128] The polyarylene oxide may be a recycled or virgin polyarylene oxide, preferably a virgin polyarylene oxide, and may be, for example, a homopolymer or copolymer of aromatic arylene oxide units, preferably polyphenylene oxide (PPO).
[0129] Specific examples of the homopolymer of the aromatic arylene oxide unit include poly(2,6-dimethyl-1,4-phenylene oxide), poly(2,6-diethyl-1,4-phenylene oxide), poly(2,6-dipropyl-1,4-phenylene) oxide, poly(2-methyl-6-ethyl-1,4-phenylene) oxide, poly(2-methyl-6-propyl-1,4-phenylene oxide), poly(2-ethyl-6-propyl-1,4-phenylene) oxide, poly(2,5-dimethyl-1,4-phenylene oxide), poly( The poly(2,3,6-trimethyl-1,4-phenylene)oxide may include one or more selected from the group consisting of poly(2,3,6-triethyl-1,4-phenylene)oxide, poly(2,6-dimethoxy-1,4-phenylene oxide), poly(2,6-dichloromethyl-1,4-phenylene oxide), poly(2,6-dibromomethyl-1,4-phenylene oxide), and poly(2,6-diphenyl-1,4-phenylene)oxide, and may preferably be poly(2,6-dimethyl-1,4-phenylene oxide).
[0130] The copolymer of aromatic arylene oxide units means a polymer in which a comonomer is copolymerized with an aromatic arylene oxide unit as a main monomer. A specific example thereof may be selected from the group consisting of a copolymer of poly(2,6-dimethyl-1,4-phenylene) oxide and poly(2,3,6-trimethyl-1,4-phenylene) oxide; a copolymer of poly(2,6-dimethyl-1,4-phenylene) oxide and poly(2,3,6-triethyl-1,4-phenylene) oxide; and combinations thereof. A preferred example thereof may be a copolymer of poly(2,6-dimethyl-1,4-phenylene) oxide and poly(2,3,6-trimethyl-1,4-phenylene) oxide.
[0131] The polyarylene oxide may have a number average molecular weight of, for example, 10,000 to 100,000 g / mol, preferably 10,000 to 70,000 g / mol, and more preferably 15,000 to 45,000 g / mol. Within this range, there is an advantage in that the processability and balance of physical properties are further improved.
[0132] In this description, the number average molecular weight, as a specific example, can be calculated as a number average value, although it is measured in the same manner as the weight average molecular weight.
[0133] The polyarylene oxide may have an intrinsic viscosity of, for example, 0.15 to 0.6 dl / g, preferably 0.2 to 0.5 dl / g, more preferably 0.2 to 0.4 dl / g, and even more preferably 0.25 to 0.4 dl / g. Within this range, the composition has the advantage of having a better balance of physical properties, such as mechanical strength and moldability.
[0134] In this description, unless otherwise specified, the intrinsic viscosity can be measured at 25° C. using an Ubbelohde viscometer after dissolving the sample to be measured in chloroform solvent at a concentration of 0.5 g / dl.
[0135] The polyarylene oxide may be produced by, for example, a production method generally applied in the technical field to which the present invention pertains, and commercially available products may also be used as long as they comply with the definition of the present invention.
[0136] The SAN-based resin may be a recycled or virgin SAN-based resin, preferably a virgin SAN-based resin. For example, the SAN-based resin may contain 70 to 95% by weight of an aromatic vinyl compound and 5 to 30% by weight of a vinyl cyan compound, preferably 70 to 90% by weight of an aromatic vinyl compound and 10 to 30% by weight of a vinyl cyan compound, more preferably 80 to 90% by weight of an aromatic vinyl compound and 10 to 20% by weight of a vinyl cyan compound. In this case, there is an advantage that the fluidity and impact strength are further improved without deterioration of other physical properties.
[0137] The aromatic vinyl compound and the vinyl cyan compound contained in the SAN-based resin can be appropriately selected from the ranges of the aromatic vinyl compound and the vinyl cyan compound mentioned in the graft copolymer (A), respectively.
[0138] The SAN-based resin may have a weight average molecular weight of, for example, 70,000 to 200,000 g / mol, preferably 80,000 to 180,000 g / mol, and more preferably 90,000 to 160,000 g / mol. Within this range, there is an advantage that the mechanical strength and weather resistance are further improved.
[0139] The SAN-based resin may be produced by, for example, a production method generally applied in the technical field to which the present invention pertains, and commercially available products may also be used as long as they comply with the definition of the present invention.
[0140] (C) An alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer having a rubber core with an average particle size of more than 200 nm to 500 nm. The thermoplastic resin composition may, for example, comprise an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (hereinafter referred to as "(C) graft copolymer") having an average particle size of more than 200 nm and not more than 500 nm, the alkyl acrylate rubber core comprising an alkyl acrylate compound; and an aromatic vinyl compound-vinyl cyan compound copolymer shell surrounding the alkyl acrylate rubber core, the aromatic vinyl compound and the vinyl cyan compound being included in the copolymer shell. In this case, there is an advantage that the moldability, impact strength, tensile strength and heat resistance are further excellent.
[0141] The (C) graft copolymer may be included in an amount of, for example, 0 to 12 parts by weight, specifically, 0.1 to 12 parts by weight, preferably 0.5 to 10 parts by weight, more preferably 1 to 10 parts by weight, and even more preferably 2 to 8 parts by weight, based on 100 parts by weight in total of the (A) graft copolymer and the (B) recycled polystyrene. Within this range, there is an advantage that the fluidity and glossiness are excellent without deteriorating other physical properties.
[0142] The average particle size of the alkyl acrylate rubber core contained in the (C) graft copolymer may be, for example, more than 200 nm and not more than 500 nm, preferably 205 to 500 nm, more preferably 210 to 490 nm, even more preferably 250 to 450 nm, and even more preferably 300 to 430 nm. In this case, there is an advantage that the moldability, impact strength, tensile strength, and heat resistance are all excellent.
[0143] The (C) graft copolymer may, for example, contain 30 to 70% by weight of the alkyl acrylate rubber core and 30 to 70% by weight of the aromatic vinyl compound-vinyl cyan compound copolymer shell relative to its total weight, preferably 35 to 65% by weight of the alkyl acrylate rubber core and 35 to 65% by weight of the aromatic vinyl compound-vinyl cyan compound copolymer shell, more preferably 40 to 60% by weight of the alkyl acrylate rubber core and 40 to 60% by weight of the aromatic vinyl compound-vinyl cyan compound copolymer shell, in which case there are advantages in that all of the moldability, impact strength, tensile strength and heat resistance are excellent.
[0144] The aromatic vinyl compound-vinyl cyan compound copolymer shell contained in the graft copolymer (C) may, for example, comprise 50 to 99% by weight of the aromatic vinyl compound and 1 to 50% by weight of the vinyl cyan compound, preferably 60 to 90% by weight of the aromatic vinyl compound and 10 to 40% by weight of the vinyl cyan compound, more preferably 65 to 80% by weight of the aromatic vinyl compound and 20 to 35% by weight of the vinyl cyan compound. In this case, there are advantages in that all of the moldability, impact strength and gloss are excellent.
[0145] The alkyl acrylate, aromatic vinyl compound, and vinyl cyanide compound contained in the graft copolymer (C) can be appropriately selected from the ranges mentioned for the graft copolymer (A).
[0146] The graft copolymer (C) can be produced, for example, by a production method commonly applied in the technical field to which the present invention pertains, and commercially available products can also be used as long as they comply with the definition of the present invention.
[0147] (D) Light stabilizers The thermoplastic resin composition may contain, for example, a (D) light stabilizer. As a specific example, the light stabilizer may be contained in an amount of 0.1 to 7 parts by weight, preferably 0.3 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, and even more preferably 1 to 2 parts by weight, based on 100 parts by weight in total of the (A) graft copolymer and the (B) matrix resin. Within this range, there is an advantage that the weather resistance is further improved without deteriorating other physical properties.
[0148] The (D) light stabilizer may, for example, include at least one selected from the group consisting of triazine-based compounds, benzophenone-based compounds, benzotriazole-based compounds, indole-based compounds, quinolinone-based compounds, benzoate-based compounds, cyanoacrylate-based compounds, and amine-based compounds. Preferably, the (D) light stabilizer may be a benzotriazole-based ultraviolet absorber or an amine-based compound. In this case, there is an effect that the physical properties are well balanced and the light resistance is further improved.
[0149] Examples of the triazine-based ultraviolet absorber include 2,4-diphenyl-6-(2-hydroxy-4-methoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,6- Diphenyl-4-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-dodecyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-benzyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy -4-butoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-dodecyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-benzyloxyphenyl)-1,3,5-triazine, 2 ,4,6-tris(2-hydroxy-4-ethoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-butoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-propoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-methoxycarbonylpropyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-ethoxycarbonylethyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-(1-(2-ethoxyhexyloxy)-1-oxopropan-2-yloxy)phenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-ethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-propoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-butoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-butoxyphenyl)-1,3,5-triazine, toxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-hexyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-octyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-dodecyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-benzyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-benzyloxyphenyl)-1,3,5-triazine, -methyl-4-ethoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-butoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-propoxyethoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-methoxycarbonylpropyloxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-ethoxycarbonylethyloxyphenyl)-1,3,5-triazine )-1,3,5-triazine, 2,4,6-tris(2-hydroxy-3-methyl-4-(1-(2-ethoxyhexyloxy)-1-oxopropan-2-yloxy)phenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-N-octyloxyphenyl)-1,3,5-triazine, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(2-(2-ethylhexanoyloxy)ethoxy)phenol.
[0150] Examples of the benzophenone-based ultraviolet absorber include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxytrihydridolate benzophenone, 2-hydroxy-4-dodecyloxy-benzophenone, 2-hydroxy-4-octadecyloxy-benzophenone, 2,2'-dihydroxy-4- The compound may be one or more selected from the group consisting of methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, and 4,4'-bis(diethylamino)benzophenone.
[0151] Examples of the benzotriazole-based ultraviolet absorber include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-2'-hydroxy-3',2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 5'-bis(α,α-dimethylbenzyl)phenyl-benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butyl-phenyl)-benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butyl-phenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butyl-phenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amyl)-benzotriazole, 2-(2'-hydroxy The compound may be one or more selected from the group consisting of 2-(2-hydroxy-3',5'-di-tert-amylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(3",4",5",6"-tetrahydrophthalimidomethyl)-5'-methylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-pentylphenyl), 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] and 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol, and preferably 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol.
[0152] The indole-based ultraviolet absorber may be, for example, 2-[(1-methyl-2-phenyl-1H-indol-3-yl)methylene]propanedinitrile.
[0153] The quinolinone ultraviolet absorber may be, for example, 4-hydroxy-3-[(phenylimino)methyl]-2(1H)-quinolinone.
[0154] The benzoate-based ultraviolet absorber may be, for example, one or more selected from the group consisting of 2,4-di-t-butylphenyl-3',5'-di-t-butyl-4'-hydroxybenzoate, 2,6-di-t-butylphenyl-3',5'-di-t-butyl-4'-hydroxybenzoate, n-hexadecyl-3,5-di-t-butyl-4-hydroxybenzoate, and n-octadecyl-3,5-di-t-butyl-4-hydroxybenzoate.
[0155] The cyanoacrylate-based UV absorber may be, for example, 2'-ethylhexyl-2-cyano-3,3-diphenylacrylate, ethyl-2-cyano-3-(3',4'-methylenedioxyphenyl)-acrylate, or a mixture thereof.
[0156] The amine-based UV absorber may be, for example, a hindered amine light stabilizer (HALS), and preferably is 1,1-bis(2,2,6,6-tetramethyl-4-piperidyl)succinate, bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, or bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate. , bis(1,2,2,6,6-pentamethyl-4-piperidyl)-N-butyl-3,5-di-tert-butyl-4-hydroxybenzyl malonate, condensation products of 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-hydroxypiperidine with succinic acid, linear or cyclic condensation products of N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)hexamethylenediamine with 4-tert-octylamino-2,6-dichloro-1,3,5-triazine, tris(2,2 ,6,6-tetramethyl-4-piperidyl)nitrilotriacetate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, 1,1'-(1,2-ethanediyl)-bis(3,3,5,5-tetramethylpiperazinone), 4-benzoyl-2,2,6,6-tetramethylpiperidine, 4-stearyloxy-2,2,6,6-tetramethylpiperidine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)hexamethyl linear or cyclic condensation products of hexanediamine with 4-morpholino-2,6-dichloro-1,3,5-triazine, reaction products of 7,7,9,9-tetramethyl-2-cycloundecyl-1-oxa-3,8-diaza-4-oxospiro-[4,5]decane with epichlorohydrin, and poly[[6-(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino], and preferably bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate.
[0157] thermoplastic resin composition The thermoplastic resin composition contains the graft copolymer (A) and the matrix resin (B). In this case, by containing recycled resin, the thermoplastic resin composition has the advantages of being environmentally friendly and having excellent moldability, impact strength, tensile strength, heat resistance, and colorability.
[0158] As an example, the thermoplastic resin composition may include the (A) graft copolymer, the (B) matrix resin, and one or more selected from the group consisting of the (C) graft copolymer and the (D) light stabilizer. In this case, there is an advantage that the molding processability, impact strength, and glossiness are further excellent.
[0159] As an example, the thermoplastic resin composition may contain, relative to 100 parts by weight in total of the (A) graft copolymer and the (B) matrix resin, 0 to 12 parts by weight or 0.1 to 12 parts by weight of the (C) graft copolymer; and 0 to 7 parts by weight or 0.1 to 7 parts by weight of the (D) light stabilizer. In this case, by containing recycled resin, there are advantages that it is environmentally friendly and has excellent moldability, impact strength, tensile strength, heat resistance, and colorability.
[0160] The thermoplastic resin composition may have a heat distortion temperature (HDT) of 82° C. or more, preferably 82 to 120° C., more preferably 82 to 115° C., and even more preferably 83 to 110° C., as a specific example, 87 to 110° C. or 88 to 105° C., as measured under a load of 18.5 kgf in accordance with ASTM D 648. Within this range, there is an advantage that the heat resistance is further improved without deterioration of other physical properties.
[0161] The thermoplastic resin composition has, for example, a tensile strength of 400 kgf / cm2 measured at room temperature and at a speed of 50 mm / min according to ASTM D 638. 2 or more, preferably 400 to 530 kgf / cm 2 , more preferably 400 to 520 kgf / cm 2 , and more preferably 400 to 510 kgf / cm 2 A specific example is 405 to 520 kgf / cm 2 , or 410~510kgf / cm 2 Within this range, there is an advantage that the tensile strength is further improved without deteriorating other physical properties.
[0162] The thermoplastic resin composition may, for example, have a flow index of 6 g / 10 min or more, preferably 6 to 30 g / 10 min, more preferably 6 to 25 g / 10 min, and even more preferably 6 to 22 g / 10 min, measured in accordance with ASTM D1238 at a temperature of 230° C. under a load of 10 kg. Within this range, there is an advantage that the molding processability is further improved without any deterioration in other physical properties.
[0163] The thermoplastic resin composition may, for example, have an impact strength of 10 kgf·cm / cm or more, preferably 10 to 30 kgf·cm / cm, more preferably 10 to 25 kgf·cm / cm, and even more preferably 10 to 20 kgf·cm / cm, measured at room temperature at a thickness of 1 / 4" in accordance with ASTM D1238. Within this range, there is an advantage that the impact strength is even more excellent without any deterioration in other physical properties.
[0164] In this description, normal temperature may be a point within the range of 23±3°C.
[0165] The thermoplastic resin composition may have a colorability C / S value of 103 or more, preferably 103 to 120, more preferably 103 to 115, and even more preferably 103 to 110, derived from L and b values measured in accordance with the CIE Lab method. Within this range, there is an advantage that the colorability is further improved without deteriorating other physical properties.
[0166] In this description, the coloring property is measured at a Degree Observer of 10° under a UV D65 light source using an X-lite Color-eye 7000A device according to the CIE Lab method, and the L and b values are obtained in the Reflectance Mode according to the CIE Lab method according to the Munsell System. The measured L and b values are then automatically calculated based on a formula incorporated in the software Propalett Paint / Plastics Formulation Platinum 5.2.5.1. of GretagMacbeth LLC. The C / S value is based on 100, and if it is greater than 100, the coloring property is excellent. The higher the value, the better the coloring property.
[0167] For reference, in the CIE LAB color coordinate system, L is expressed as a number from 0 to 100, with the closer to 0, the blacker it is, and the closer to 100, the whiter it is. The a value indicates the Red-Green value, and the b value indicates the Yellow-Blue value.
[0168] Method for producing thermoplastic resin composition The thermoplastic resin composition of the present invention comprises a step of kneading and extruding (A) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber core having an average particle size of 60-200 nm and an aromatic vinyl compound-vinyl cyan compound copolymer shell, and (B) a matrix resin, under conditions of 180-300°C and 100-400 rpm, the copolymer shell of the graft copolymer (A) containing 85-99% by weight of an aromatic vinyl compound and 1-15% by weight of a vinyl cyan compound relative to its total weight, and having a weight average molecular weight of 100,000-400,000 g / mol, and the matrix resin (B) containing 50-90% by weight of recycled polystyrene and 8-50% by weight of polyarylene oxide relative to its total 100% by weight, in which case the inclusion of recycled resins provides the advantages of being environmentally friendly and excellent in moldability, impact strength, tensile strength, heat resistance and colorability.
[0169] In one example, the kneading and extruding step may include kneading and extruding one or more selected from the group consisting of (A) a graft copolymer, (B) a matrix resin, and (C) a graft copolymer and (D) a light stabilizer. In this case, there are advantages in that the molding processability, impact strength, tensile strength, heat resistance, and colorability are all excellent.
[0170] The kneading and extruding step may be performed, for example, using one or more selected from the group consisting of a single screw extruder, a twin screw extruder, and a Banbury mixer. The composition may be uniformly mixed using the extruder and then extruded to obtain, for example, a pellet-shaped thermoplastic resin composition. In this case, there is an effect of preventing deterioration of mechanical properties and heat resistance and providing excellent appearance quality.
[0171] The kneading and extruding steps may be carried out, for example, at a cylinder temperature of the extruder within a range of 180 to 300°C, preferably 210 to 290°C, and more preferably 220 to 280°C. In this case, there are advantages in that the processing amount per unit time is appropriate, melt kneading is sufficiently carried out, and deterioration of physical properties such as thermal decomposition is prevented.
[0172] The kneading and extrusion may be carried out under conditions where the screw rotation speed is, for example, 100 to 400 rpm, preferably 110 to 350 rpm, and more preferably 120 to 270 rpm. In this case, the processing amount per unit time is appropriate, and therefore, there is an advantage in that the process efficiency is excellent.
[0173] The thermoplastic resin composition may optionally further contain, based on 100 parts by weight of the total of the (A) graft copolymer and the (B) matrix resin, 0.01 to 10 parts by weight, 0.05 to 7 parts by weight, 0.1 to 5 parts by weight, 0.3 to 4.5 parts by weight, or 0.3 to 4 parts by weight of one or more other additives selected from the group consisting of lubricants, heat stabilizers, pigments, release agents, antistatic agents, antibacterial agents, processing aids, smoke suppressants, anti-dripping agents, anti-friction agents, and anti-wear agents, and within this range, there is an advantage that the desired physical properties of the thermoplastic resin composition described herein are well realized without decreasing the intended physical properties.
[0174] The lubricant may be, for example, one or more selected from the group consisting of fatty acid amide compounds, montan waxes, silicone oils, and olefin waxes, preferably olefin waxes, and more preferably polyethylene waxes. In this case, not only are the moldability and mold releasability excellent, but the friction and noise resistance properties can also be further improved.
[0175] The fatty acid amide compound may be, for example, at least one selected from the group consisting of stearamide, behenamide, ethylene bis(stearamide), N,N'-ethylene bis(12-hydroxy stearamide), erucamide, oleamide, and ethylene bis oleamide.
[0176] The montan wax may be, for example, a montan wax, a montan ester wax, or a mixture thereof.
[0177] The silicone oil may be, for example, one or more selected from the group consisting of dimethyl silicone oil, methyl hydrogen silicone oil, ester modified silicone oil, hydroxy silicone oil, carbinol modified silicone oil, vinyl silicone oil, and silicone acrylate.
[0178] The olefin wax may be, by way of example, an oxidized polyethylene wax, a polyethylene wax, a polypropylene wax, or a mixture thereof.
[0179] The heat stabilizer may include, for example, a phenol-based heat stabilizer, a phosphorus-based heat stabilizer, or a mixture thereof, and is preferably a phenol-based heat stabilizer. In this case, it has the effect of preventing oxidation due to heat during the extrusion process and having excellent mechanical properties and heat resistance.
[0180] Examples of the phenol-based heat stabilizer include N,N'-hexane-1,6-diyl-bis[3-(3,5-di-t-butyl-4-hydroxyphenylpropionamide)], pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene-bis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], The tertiary amine may be one or more selected from the group consisting of 3,5-di-t-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, and 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate. In this case, the heat resistance can be significantly improved while maintaining a high balance of physical properties.
[0181] Examples of the phosphorus-based heat stabilizer include triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, and monooctyl diphenyl phosphite. The phosphate group may be one or more selected from the group consisting of bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, stearyl pentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, and trimethyl phosphate.
[0182] The pigment may be an inorganic pigment or an organic pigment.
[0183] The organic pigment may be, for example, one or more selected from the group consisting of perinone-based pigments, anthraquinone-based pigments, perylene-based pigments, phthalocyanine-based pigments, azo-based pigments, indigo-based pigments, dioxazine-based pigments, quinacridone-based pigments, methane-based pigments, quinoline-based pigments, isoindolinone-based pigments, and phthalone-based pigments.
[0184] The inorganic pigment may be, for example, one or more selected from the group consisting of ultramarine pigments, titanium dioxide, zinc sulfide, zinc tetracyclic, iron oxide, and carbon black.
[0185] The release agent may be, for example, at least one selected from the group consisting of glycerin stearate, polyethylene tetrastearate, etc., but is not limited thereto.
[0186] The antistatic agent may be, for example, one or more of anionic surfactants, nonionic surfactants, etc., but is not limited thereto.
[0187] The anti-dripping agent may be, for example, one or more selected from the group consisting of PTFE (polytetrafluoroethylene), a mixture of PTFE and SAN (styrene-acrylonitrile) resin (PTFE / SAN), a mixture of PTFE and PMMA (polymethyl methacrylate) (PTFE / PMMA), polyamide, polysilicon, and TFE-HFP (tetrafluoroethylene-hexafluoropropylene) copolymer, and may be, for example, one or more selected from the group consisting of PTFE / SAN and PTFE / PMMA, more preferably, PTFE / SAN. The PTFE / SAN and PTFE / PMMA may be, for example, a mixture of PTFE and SAN or PMMA at a weight ratio of 1:0.5 to 1.5, and may be, for example, a mixture at a weight ratio of 1:1.
[0188] The antibacterial agent, processing aid, smoke suppressant, antifriction agent, antiwear agent, etc. are not particularly limited as long as they are commonly used in the technical field to which the present invention pertains.
[0189] Molded product The molded article described herein is characterized by containing the thermoplastic resin composition of the present invention. In this case, the molded article has the advantages of being environmentally friendly due to the inclusion of recycled resin, and of being excellent in moldability, impact strength, tensile strength and heat resistance.
[0190] Even though the molded product contains recycled resin, it has physical properties equal to or greater than those of conventional virgin resin-based thermoplastic resins, and thus can be applied without additional processing to various fields where conventional virgin resin-based ASA-based thermoplastic resin compositions are used, such as interior and exterior materials for buildings, interior and exterior materials for automobiles, ships, and leisure and sporting goods.
[0191] As a preferred example, the molded article has a heat distortion temperature (HDT) of 82°C or more measured under a load of 18.5 kgf according to ASTM D 648, a flow index of 6 g / 10 min or more measured under a load of 10 kg at a temperature of 230°C according to ASTM D 1238, an impact strength of 10 kgf cm / cm or more measured at room temperature and at a thickness of 1 / 4" according to ASTM D 256, and a tensile strength of 400 kgf / cm or more measured at room temperature and at a speed of 50 mm / min according to ASTM D 638. 2 As described above, the colorability measured under the above-mentioned conditions is excellent at 103 or more, and therefore has the advantage that it can be applied to fields where excellent moldability, impact strength, tensile strength, heat resistance, and colorability are all required.
[0192] The molded article may be manufactured by a method commonly used in the technical field to which the present invention belongs. For example, the molded article may be manufactured by applying a molding method such as injection molding, injection compression molding, extrusion molding, blow molding, press molding, pressure molding, hot bending molding, compression molding, calendar molding, or rotational molding using a melt kneaded product or pellets of the thermoplastic resin composition according to the present invention as a raw material. In this case, the size, thickness, shape, etc. of the molded article may be appropriately adjusted depending on the purpose of use.
[0193] The molded article may be preferably produced by injecting a molten mixture or pellets of the thermoplastic resin composition according to the present invention using an injector at a barrel temperature of 180 to 300°C. The molded article thus produced has an advantage that it can be applied to fields where gloss, moldability, and impact strength are all required.
[0194] In describing the thermoplastic resin composition, its production method, and molded products, other conditions, equipment, etc. not explicitly described herein can be appropriately selected within the range commonly used in the art, and it is clearly stated that there are no particular limitations.
[0195] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical spirit of the present invention. Naturally, such changes and modifications also fall within the scope of the appended claims.
[0196] [Example] The materials used in the following examples and comparative examples are as follows. (A) ASA graft copolymer: an ASA graft copolymer comprising a butyl acrylate seed polymer; a butyl acrylate rubber core; and a styrene-acrylonitrile copolymer shell; wherein the average particle size of the seed and core particles, the composition and weight average molecular weight of the shell, etc. satisfy the conditions described in Table 1 below (based on the total weight of the (A) ASA graft copolymer, the seed polymer is contained at 7 wt%, the rubber core at 43 wt%, and the copolymer shell at 50 wt%).
[0197] [Table 1] (In Table 1, A-9 does not contain a vinyl cyanide compound, but for the sake of comparison, it is classified as (A) ASA graft copolymer, AN means acrylonitrile, Mw means weight average molecular weight, and the AN content of the shell means the weight % of AN relative to the total weight of the shell.)
[0198] (B) Matrix resin: (B-1) Recycled PS resin (non-foamed PS) with Mw of 240,000 g / mol (B-2) Recycled EPS resin with Mw of 165,000 g / mol (B-3) Virgin GPPS (LG Chem's 25SPI) with Mw of 275,000 g / mol (B-4) PPO: poly(2,6-dimethyl-1,4-phenylene) oxide (LXR035 from Bluestar) having an intrinsic viscosity of 0.32 dl / g and a flow index of 28 g / 10 min measured at 220° C. under a load of 10 kg according to ASTM D1238. (B-5) SAN resin (LG Chem's 82TR SAN) (C) Large particle size ASA resin (LG Chem's SA927) containing a butyl acrylate rubber core with an average particle size of 380-500 nm
[0199] Examples 1 to 13 and Comparative Examples 1 to 10 The above (A) to (C) were mixed in the amounts shown in Table 2 below using a super mixer, and extruded using a twin-screw extruder (screw diameter 26 mm, L / D=40) under extrusion conditions of a cylinder temperature of 260° C. and a screw rotation speed of 200 rpm to prepare pellets.
[0200] The prepared thermoplastic resin composition in pellet form was dried at 80°C for 2 hours or more, and then injection molded in an injector under the conditions of an injector barrel temperature of 230°C, a mold temperature of 60°C, and an injection speed of 30 mm / sec to prepare a test piece for measuring physical properties. The test piece was left at room temperature for 48 hours or more, and then the physical properties were measured.
[0201] [Test example] The physical properties of the specimens prepared in the above examples and comparative examples were measured by the following methods, and the results are shown in Table 3 below. *Flow index (g / 10 min): In accordance with ASTM D1238, the weight (g) of the resin that flowed out after melting for 10 minutes at a temperature of 220°C under a load of 10 kg was measured. *Izod impact strength (kgf cm / cm): Measured at room temperature using 1 / 4" thick injection specimens in accordance with ASTM D256. * Tensile strength (kgf / cm 2 ):Measured at room temperature on 1 / 8" thick ejection specimens at a speed of 50 mm / min in accordance with ASTM D 638. *Heat distortion temperature (℃): HDT was measured under a load of 18.5 kgf in accordance with ASTM D648. *Color strength (C / S): Measured using X-lite Color-eye 7000A under UV D65 light source with Degree Observer 10° according to CIE Lab method. L and b values were obtained in Reflectance Mode according to CIE Lab method according to Munsell System, and C / S (Color Strength) value was calculated based on the formula built into Propalett Paint / Plastics Formulation Platinum 5.2.5.1. software of GretagMacbeth LLC. Here, C / S is based on 100, and the better the color strength, the higher the value.
[0202] [Table 2]
[0203] [Table 3]
[0204] Referring to Tables 1 to 3, in the case of Examples 1 to 13 according to the present invention, even though they contain recycled PS, the flow index, impact strength, tensile strength, heat distortion temperature and colorability were shown to be equal to or higher than those of the comparative examples, and it was confirmed that the molding processability, mechanical rigidity, heat resistance and colorability were all excellent.
[0205] On the other hand, in Comparative Examples 1 to 5 in which ASA was applied in which the average particle size of the alkyl acrylate rubber contained in the (A) graft copolymer, the content of acrylonitrile contained in the copolymer shell, the weight average molecular weight of the copolymer shell, etc. were outside the range of the present invention, it was confirmed that the flow index, impact strength, tensile strength and / or colorability were reduced, and in Comparative Example 6 in which only GPPS was included in the matrix resin instead of PPO, it was confirmed that the mechanical stiffness and heat resistance were significantly reduced. Meanwhile, referring to Comparative Example 9, even if the content of the recycled resin was reduced and the content of ASA was increased without using PPO, it was confirmed that the flowability, tensile strength and heat resistance were poor, and therefore it is not suitable to replace conventional non-recycled resin compositions.
[0206] In addition, Comparative Example 7, which contained an excessive amount of PPO, was confirmed to have deteriorated moldability and colorability, even though the recycled resin content was about 15 wt%, which was about half that of the Examples, and Comparative Example 8, which contained an insufficient PPO content, was confirmed to have deteriorated mechanical rigidity and heat resistance.On the other hand, in Comparative Example 10, although the ratio of recycled resin in the total weight of the composition was at the same level as the Examples, the total content of matrix resin and the ratio of components constituting the matrix resin were outside the range of the present invention, and it was confirmed that the impact strength was significantly reduced.
Claims
1. (A) an alkyl acrylate-vinyl cyanide compound graft copolymer having an alkyl acrylate rubber core having an average particle size of 60 to 200 nm and an aromatic vinyl compound-vinyl cyanide compound copolymer shell; (B) a matrix resin, the copolymer shell of the graft copolymer (A) comprises, based on the total weight of the graft copolymer, 85 to 99% by weight of an aromatic vinyl compound and 1 to 15% by weight of a vinyl cyan compound, and has a weight average molecular weight of 100,000 to 400,000 g / mol; The (B) matrix resin is a thermoplastic resin composition, characterized in that it contains 50 to 90% by weight of recycled polystyrene and 8 to 50% by weight of polyarylene oxide, relative to a total of 100% by weight of the matrix resin.
2. The thermoplastic resin composition according to claim 1, characterized in that it contains 20 to 60% by weight of the graft copolymer (A) and 40 to 80% by weight of the matrix resin (B) relative to 100% by weight in total of the graft copolymer (A) and the matrix resin (B).
3. The thermoplastic resin composition according to claim 1, wherein the (A) graft copolymer comprises 40 to 70% by weight of an alkyl acrylate rubber core and 30 to 60% by weight of a copolymer shell, based on a total of 100% by weight of the graft copolymer.
4. The thermoplastic resin composition according to claim 1, characterized in that the (A) graft copolymer comprises, relative to a total of 100 weight %, 1 to 20 weight % of a polymer seed comprising one or more selected from the group consisting of alkyl (meth)acrylates, aromatic vinyl compounds, and vinyl cyan compounds, 35 to 65 weight % of an alkyl acrylate rubber core, and 30 to 60 weight % of a copolymer shell.
5. The thermoplastic resin composition according to claim 1, wherein the recycled polystyrene includes any one selected from the group consisting of recycled non-expanded polystyrene, recycled expanded polystyrene, and mixtures thereof.
6. The thermoplastic resin composition according to claim 1, wherein the recycled polystyrene has a weight average molecular weight of 100,000 to 350,000 g / mol.
7. The thermoplastic resin composition according to claim 1 , wherein the matrix resin (B) further comprises general-purpose polystyrene.
8. The thermoplastic resin composition according to claim 1, wherein the (B) matrix resin further contains 1 to 15% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer containing 75 to 95% by weight of an aromatic vinyl compound and 5 to 25% by weight of a vinyl cyan compound.
9. The thermoplastic resin composition according to claim 1, characterized in that it comprises (C) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer comprising an alkyl acrylate rubber core having an average particle size of more than 200 nm and not more than 500 nm, and an aromatic vinyl compound-vinyl cyan compound copolymer shell.
10. The thermoplastic resin composition according to claim 9, wherein the graft copolymer (C) is contained in an amount of 0.1 to 12 parts by weight based on 100 parts by weight of the total of the graft copolymer (A) and the matrix resin (B).
11. The thermoplastic resin composition according to claim 1, characterized in that it contains 0.1 to 7 parts by weight of a light stabilizer (D) based on a total of 100 parts by weight of the graft copolymer (A) and the matrix resin (B).
12. The thermoplastic resin composition according to claim 1, characterized in that the thermoplastic resin composition has a heat distortion temperature (HDT) of 82°C or more measured under a load of 18.5 kgf in accordance with ASTM D 648.
13. The thermoplastic resin composition has a tensile strength of 400 kgf / cm2 measured at a speed of 50 mm / min in accordance with ASTM D 638. 2 The thermoplastic resin composition according to claim 1, characterized in that
14. (A) an alkyl acrylate-vinyl cyanide graft copolymer having an alkyl acrylate rubber core with an average particle size of 60 to 200 nm and an aromatic vinyl compound-vinyl cyanide copolymer shell, and (B) a matrix resin, are mixed and extruded under conditions of 180 to 300° C. and 100 to 400 rpm; The method for producing a thermoplastic resin composition is characterized in that the copolymer shell of the graft copolymer (A) contains, relative to its total weight, 85 to 99% by weight of an aromatic vinyl compound and 1 to 15% by weight of a vinyl cyan compound and has a weight average molecular weight of 100,000 to 400,000 g / mol, and the matrix resin (B) contains, relative to its total weight, 50 to 90% by weight of recycled polystyrene and 8 to 50% by weight of polyarylene oxide.
15. A molded article comprising the thermoplastic resin composition according to any one of claims 1 to 13.
Citation Information
Patent Citations
Poly(Phenylene ether) resin composition with excellent light resistance
JP1995258514A
Expandable styrenic resin particle and method for producing the same, styrenic resin expanded particle and styrenic resin expanded and molded product
JP2008156585A
Halogen-free flame-retardant resin composition
JP2019523802A
Thermoplastic resin composition
JP2021503534A
Method of manufacturing resin mold product
WO2004005001A1