Secondary batteries and battery packs

The secondary battery design with a non-Faradaic specific capacitance of 50-250 nF/g and optimized resistance, along with a sulfur-containing additive, addresses the challenge of balancing energy density and high-speed charging by enhancing ion-electronic conduction and reducing charge transfer resistance, resulting in improved performance and cycle life.

JP2024539842AActive Publication Date: 2024-10-31SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024519894
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-26
Filing Date
2022-12-22
Publication Date
2024-10-31
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Existing secondary batteries struggle to balance high energy density with high-speed charging performance, particularly in electric vehicles, due to limitations in ion-electronic conduction and charge transfer resistance.

Method used

The secondary battery design includes a negative electrode sheet with a non-Faradaic specific capacitance of 50-250 nF/g, optimized resistance (4≦0.1×Cdl-R≦24 mΩ), porosity of 20-40%, and a sulfur-containing additive in the electrolyte to enhance ion-electronic conduction and reduce charge transfer resistance.

Benefits of technology

This configuration improves the charging ratio performance, current density, and energy density of the secondary battery, ensuring excellent dynamic and cycle performance, enabling high-speed charging without compromising battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539842000007
    Figure 2024539842000007
  • Figure 2024539842000008
    Figure 2024539842000008
  • Figure 2024539842000009
    Figure 2024539842000009
Patent Text Reader

Abstract

The present application discloses a secondary battery and a battery pack, in which a negative electrode active material layer is disposed on a current collector of a negative electrode sheet, the negative electrode active material layer including a negative electrode active material, and the non-Faraday specific capacity of the negative electrode sheet is set to 50 nF / g to 250 nF / g, thereby ensuring the number of electrochemically active sites on the surface of the negative electrode sheet, favoring the contact between the negative electrode sheet and an electrolyte, accelerating the speed of ion-electron conduction, and reducing the resistance of charge transfer, effectively improving the charging rate performance of the secondary battery, and improving the current density of the negative electrode sheet, thereby improving the energy density of the secondary battery, thereby providing the secondary battery with excellent kinetic performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application bearing application number 202211179117.1 and titled "Secondary Battery and Battery Pack" filed with the China Patent Office on September 26, 2022, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to the field of battery technology, and in particular to secondary batteries and battery packs. [Background technology]

[0003] With the rapid development of electric vehicles and digital electronic products, secondary batteries with higher power density, energy density and suitable for fast charging and discharging are required for application in the electric vehicles and related electronic products fields. For electric vehicles, the energy density and charging time of secondary batteries, such as lithium-ion batteries, are two important technical indicators. The adoption of high-capacity batteries can achieve the maximum driving distance, but has a great impact on fast charging performance.

[0004] Therefore, it is necessary to provide a secondary battery that can achieve both high energy density and high-speed charging performance. Summary of the Invention [Problem to be solved by the invention]

[0005] The present application provides a secondary battery and a battery pack, in which the non-faradayian specific capacitance of the negative electrode sheet is 50nF / g-250nF / g, thereby ensuring the number of electrochemically active sites on the surface of the negative electrode sheet, which is favorable for the contact between the negative electrode sheet and the electrolyte, accelerating the ion-electron conduction speed, reducing the resistance of charge transfer, and effectively improving the charging rate performance of the secondary battery, and also improving the current density of the negative electrode sheet, thereby improving the energy density of the secondary battery, so that the secondary battery has excellent kinetic performance and cycle performance, and has good application prospects. [Means for solving the problem]

[0006] A first aspect of the present application provides a secondary battery, the secondary battery including a positive electrode sheet, an electrolyte, and a separator, and further including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including graphite, wherein the non-Faraday specific capacity of the negative electrode sheet is Cdl nF / g, and 50≦Cdl≦250.

[0007] In some embodiments, the negative electrode active material layer has a resistance of R mΩ, where 4≦0.1×Cdl-R≦24.

[0008] In some embodiments, the numerical range for R is 1≦R≦15.

[0009] In some embodiments, the porosity P of the negative electrode sheet is 20% to 40%.

[0010] In some embodiments, the coating weight of the negative electrode active material layer on one surface of the negative electrode current collector is CW mg / cm 2 and 7≦CW≦12.

[0011] In some embodiments, the bulk density of the negative electrode active material is 1 g / cm 3 ~2.5g / cm 3 It is.

[0012] In some embodiments, the negative electrode active material has a granular dispersity of 1.5-5.

[0013] In some embodiments, the electrolyte comprises a sulfur-containing additive, the sulfur-containing additive comprising at least one of Formulas (1)-(5). [ka]

[0014] In some embodiments, the sulfur-containing additive is A % based on the weight of the electrolyte, where 0.05≦Cdl×A %≦12.5.

[0015] In some embodiments, the sulfur-containing additive is A %, based on the weight of the electrolyte, where 0.01≦A≦5.

[0016] In addition, a second aspect of the present application further provides a battery pack, which includes the above-mentioned secondary battery. Effect of the Invention

[0017] Provided is a secondary battery and a battery pack, in which a negative electrode active material layer is disposed on a current collector of a negative electrode sheet, the negative electrode active material layer including a negative electrode active material, and the non-Faraday specific capacity of the negative electrode sheet is 50 nF / g to 250 nF / g, thereby ensuring the number of electrochemically active sites on the surface of the negative electrode sheet, favoring the contact between the negative electrode sheet and an electrolyte, accelerating the speed of ion-electron conduction, and reducing the resistance of charge transfer, thereby effectively improving the charging rate performance of the secondary battery, and improving the current density of the negative electrode sheet, thereby improving the energy density of the secondary battery, thereby providing the secondary battery with excellent kinetic performance and cycle performance, and having good application prospects. [Brief description of the drawings]

[0018] [Figure 1] This is a cyclic voltammogram of the negative electrode sheet produced in Example 1 of the present application at a scan rate of 0.1 mv / s. [Diagram 2] 1 is a linear scan voltammogram of the negative electrode sheet produced in Example 1 of the present application at a potential range of 2.6 V to 2.7 V and a scan rate of 0.1 mv / s. [Diagram 3] 1 is a fitting curve showing a scatter diagram of scan rate-current density for the negative electrode sheet produced in Example 1 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present application provides a secondary battery and a battery pack, and in order to more clearly and embody the objectives, technical ideas, and effects of the present application, the present application will be described in more detail below by way of examples with reference to the drawings. It should be understood that the specific examples described in the present specification are merely for the purpose of illustrating the present application, and are not intended to limit the present application.

[0020] In one example of the present application, a secondary battery is provided, the secondary battery including a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte, and a housing.

[0021] I, negative electrode sheet

[0022] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, and the negative electrode active material includes graphite.

[0023] The negative electrode sheet is a single-sided sheet or a double-sided sheet, and when the negative electrode sheet is a single-sided sheet, the negative electrode active material layer is disposed on one surface of the negative electrode current collector, and when the negative electrode sheet is a double-sided sheet, the negative electrode active material layer is disposed on both surfaces of the negative electrode current collector. The negative electrode sheet can have a single-sided negative electrode sheet region and a double-sided negative electrode sheet region at the same time.

[0024] The non-Faraday specific capacity Cdl of the negative electrode sheet is as follows:

[0025] The non-faradaic specific capacity of the negative electrode sheet is Cdl nF / g, and the numerical range of Cdl is 50≦Cdl≦250. Specifically, Cdl may be any of 50, 70, 80, 140, 160, 180, 200, 205, 210, and 250, or any two of them. The faradaic reaction in a battery is a process in which the oxidation state of the active material changes and the charge passes through the double charge layer and moves through the electrode interface to the inside of the active material. The non-faradaic reaction is a reaction in which the charge is stored and released by the physical adsorption and desorption of ions on the electrode surface without causing charge transfer through the electrode interface. The non-faradaic specific capacity value Cdl nF / g indicates the number of electrochemically active sites in the negative electrode sheet. Within a certain range, increasing Cdl increases the number of electrochemically active sites, which is favorable for the contact between the negative electrode active material and the electrolyte, and is favorable for accelerating the ion-electron conduction rate, reducing the resistance of charge transfer, and effectively improving the charge multiplier performance of the secondary battery. In some embodiments, when 80≦Cdl≦250 and the non-Faraday specific capacity value of the negative electrode sheet is within the above range, the overall performance of the secondary battery is further improved.

[0026] In some embodiments, when 80≦Cdl≦200 and the non-Faraday specific capacity value of the negative electrode sheet is within the above range, the overall performance of the secondary battery is well balanced and the overall performance of the secondary battery is better.

[0027] The resistance R of the negative electrode active material layer is as follows.

[0028] In some embodiments, the relationship between R and Cdl is 4≦0.1×Cdl-R≦24. When the negative electrode sheet satisfies the above relationship, the ion transport path of the negative electrode sheet is shorter, and the electrochemical reaction is promoted, thereby realizing a high-power discharge performance. In addition, when the negative electrode sheet satisfies the above relationship, the electrolyte wettability, surface resistance, and high-power charge and discharge performance of the negative electrode sheet are all in an appropriate state, and the expansion of the negative electrode sheet during the cycle process can also be reduced.

[0029] In some embodiments, the relationship between R and Cdl is 4≦0.1×Cdl-R≦14. When the negative electrode sheet satisfies the above relationship, the internal structure of the negative electrode sheet can be further optimized, and the overall performance of the secondary battery can be improved.

[0030] In some embodiments, the resistance of the negative electrode active material layer is R mΩ, and R is in the range of 1≦R≦15. Specifically, R may be any of 1, 3, 4, 6, 8, 10, 12, and 15, or any two of them. The electronic conduction characteristics mainly affect the multiplication performance of the secondary battery, and important factors affecting the conductivity of the negative electrode sheet of the secondary battery include the interface state between the negative electrode current collector and the negative electrode active material layer, the distribution state of the conductive agent, the contact state between the granules, etc., and the material performance of the negative electrode sheet can be optimized by adjusting the sheet resistance of the negative electrode sheet (the resistance of the negative electrode active material layer).

[0031] In some embodiments, the range of R is 2≦R≦11. If the value of R is within this range, the conductive network inside the negative electrode sheet is more complete, and the overall performance of the secondary battery is better. In addition, in order to realize high-speed charging of the secondary battery, one of the important techniques is to enable the secondary battery to accept a larger charging current, and for this purpose, it is necessary to sufficiently reduce the polarization resistance of the battery itself. In this application, the resistance R of the negative electrode active material layer of the negative electrode sheet is limited to 1mΩ≦R≦15mΩ, and 4≦0.1×Cdl-R≦24, that is, by sufficiently reducing the sheet resistance, the polarization resistance of the secondary battery itself is sufficiently reduced, and the number of active sites of the electrochemical reaction is within a preferred range, so that the overall performance of the secondary battery is better.

[0032] In the examples of the present application, the method for testing the resistance R of the negative electrode active material layer is as follows.

[0033] The negative electrode sheet has an area of ​​1540.25 mm 2The negative electrode sheet is cut into a circular sheet, and the cut negative electrode sheet is placed at the center of the probe of a sheet resistance measuring instrument, and then the negative electrode sheet is tested using the sheet resistance measuring instrument to obtain the measured resistance of the negative electrode active material layer of the negative electrode sheet. The selected 10 negative electrode sheet samples are each measured using the sheet resistance measuring instrument, and the average resistance of the negative electrode active material layer of the obtained 10 measured negative electrode sheets is calculated to obtain the resistance of the negative electrode active material layer.

[0034] The porosity P of the negative electrode sheet is as follows:

[0035] In some embodiments, the porosity P of the negative electrode sheet is 20% to 40%, and specifically, P may be any of 20%, 25%, 28%, 30%, 35%, 40%, or any two of them. The more the porosity of the negative electrode sheet is within the above range and the more the pore structure, the more the contact area between the electrode and the electrolyte can be improved, the shorter the transport path of lithium ions can be, the faster the wetting of the electrolyte can be achieved, the smoother the charge transport path can be provided at the solid-liquid interface, the lower the diffusion barrier can be, the faster the lithium ions can be absorbed and released on the surface of the negative electrode material can be, the faster the reaction kinetics can be, the less the polarization of the negative electrode surface can be, the more uniform the current distribution can be, and the more negative electrode active materials can simultaneously absorb and release Li when charging at a high rate. + By adopting the above-mentioned method, it can effectively avoid the lithium deposition on the negative electrode surface, and at the same time provide sufficient active sites for electrochemical reaction in the electrochemical process, accelerate the non-Faraday reaction process of the negative electrode, and favor the transmission of electrons and ions between the solid phase and the liquid phase, thereby improving the kinetics of the electrochemical reaction, and ultimately improving the multiplication performance of the material.

[0036] The porosity of the negative electrode sheet is P=(V1-V2) / V1×100%, where V1 is the apparent volume of the sample and V2 is the actual volume of the sample. The test method can refer to GB / T33052-2016 Porosity Measurement Method.

[0037] The coating weight CW of the negative electrode active material layer is as follows.

[0038] In some embodiments, the coating weight of the negative electrode active material layer on one surface of the negative electrode current collector is CW mg / cm 2 and 7≦CW≦12, specifically, CW may be any one of 7, 9, 9.5, 10, 11, and 12, or a range consisting of any two of these numbers. When the non-Faraday specific capacitance value Cdl of the negative electrode sheet is 50 to 250 nF / g and the coating weight of the negative electrode active material layer is in the above range, it is ensured that the electrolyte can be sufficiently diffused into the negative electrode sheet while ensuring the energy density of the negative electrode, thereby reducing excessive consumption of the electrolyte for film formation and excessive consumption of lithium ions, and reducing polarization in the thickness direction of the negative electrode sheet, preventing lithium deposition on the negative electrode surface during high-speed charging, and ensuring the cycle life and initial efficiency of the secondary battery. When the coating weight of the negative electrode active material layer is 7 mg / cm 2 ~12mg / cm 2 Within this range, the transition distance of the lithium ions in the negative electrode sheet is relatively short, which reduces the charge transfer resistance and is favorable for improving the power performance of the battery, while at the same time improving the current density of the sheet and the energy density of the battery.

[0039] In addition, a change in coating weight changes the physical contact between the granules in the negative electrode active material layer, and the pores between the granules in the negative electrode active material layer. Since a non-Faradaic reaction is a reaction in which ions are physically adsorbed and desorbed on the electrode surface to release electric charge, the pores between the granules in the negative electrode active material layer change, affecting the magnitude of the non-Faradaic specific capacitance Cdl.

[0040] Coating weight of negative electrode active material layer = (weight of negative electrode sheet - weight of negative electrode current collector) / area of ​​negative electrode sheet. If the tested negative electrode sheet is coated on both sides, the area of ​​the negative electrode sheet is twice the area of ​​the sample.

[0041] The bulk density of the negative electrode active material is as follows.

[0042] In some embodiments, the bulk density of the negative electrode active material in the negative electrode active material layer is 1 g / cm 3 ~2.5g / cm 3 Specifically, it may be any one of 1, 1.5, 1.8, 2.0, 2.2, and 2.5, or a range consisting of any two of these numbers. The bulk density can represent the average density of a stack of loose granules, including pores inside and outside the granules and voids between the granules, and means the density obtained by dividing the powder mass by the volume of the container in which the powder occupies. The bulk density can be adjusted to a predetermined range depending on the particle size of the raw material, the firing conditions, etc. The bulk density value indicates the uniformity of the negative electrode active material granules. The more uniform the negative electrode active material granules are, the greater the porosity of the negative electrode sheet will be, thereby improving the liquid phase diffusion ability of lithium ions and favoring the progress of non-Faraday reactions in the battery. Increasing the non-Faraday specific capacity Cdl of the negative electrode sheet will increase the number of electrochemically active sites, which is favorable for the contact between the negative electrode active material and the electrolyte, accelerating the speed of ion-electron conduction, reducing the resistance of charge transfer, and effectively improving the charging rate performance of the secondary battery.

[0043] For the bulk density test of the negative electrode active material, reference can be made to GB / T31057.1-2014 Granular Material Physical Property Test Part 1 Bulk Density Measurement.

[0044] The granular dispersity of the negative electrode active material is as follows.

[0045] In some embodiments, the granular dispersion of the negative active material is 1.5 to 5, and may be any of 1.5, 1.8, 2.0, 2.2, 2.5, 2.7, 3.0, 3.2, 3.5, 3.8, 4.0, 4.2, 4.5, 4.8, and 5, or any two of them. The granular dispersion can represent the degree of dispersion of various particle size components, and the dispersion affects the dispersion effect of the powder material during the stirring process, and the obtained slurry has excellent uniformity and stability and is not easily settled, and can effectively adjust the uniformity of the coating weight of the negative electrode sheet, strengthen the stability of the negative electrode sheet, and further adjust the non-Faraday process, improve the transmission efficiency of lithium ions between the positive and negative electrodes, and improve the multiplication performance of the secondary battery.

[0046] In some embodiments, the granular dispersity of the negative electrode active material is 1.5 to 3.5. When the granular dispersity of the negative electrode active material is in this range, the uniformity of the negative electrode slurry is improved, the apparent performance of the formed negative electrode sheet is more excellent, and the overall performance of the secondary battery is more excellent.

[0047] The granular dispersity of the negative electrode active material can be measured using a laser particle size analyzer, and is expressed as the granular dispersity of the negative electrode active material=(Dv99−Dv10) / Dv50.

[0048] The test method for the non-Faraday specific capacitance value Cdl is as follows.

[0049] In some embodiments, referring to FIGS. 1 to 3, a method for testing the non-Faraday specific capacitance value Cdl of a negative electrode sheet includes the following steps.

[0050] In S1, the step of confirming the non-Faraday potential range, the negative electrode sheet is assembled into a half cell (abbreviated as button cell) to perform a cyclic voltammogram (CV) test, where the voltage range is 0.005-3.0V and the scan rate is 0.1-1mV / s. FIG. 1 shows the cyclic voltammogram of the negative electrode sheet at a scan rate of 0.1mV / s. Referring to FIG. 1, the cyclic voltammogram includes two curves, and the two curves only represent two scans at the same scan rate. Since the first cycle is irreversible, the peak positions of the two cycles are different, while the non-Faraday potential range is the flat section of the curve, i.e., in the range of 1.5V-3V.

[0051] In step S2, the cathodic scanning step of the non-Faraday section, a potential range was selected from the potential range of 1.5V to 3V confirmed in step S1 to perform a linear scan voltammogram (LSV) test, and the scanning direction was from high potential to low potential to collect a voltage-current curve. Here, the selected potential range was 2.6 to 2.7V, and the scanning rate was 0.05-5mV / s. Figure 2 shows the linear scan voltammogram at a scanning rate of 0.1mV / s.

[0052] Furthermore, select the median U V in the potential range of 2.6 to 2.7 V at a scan rate of 0.1 mV / s, obtain the corresponding current value U = 2.65, and calculate the current density value J1 according to the corresponding active material mass, in units of A / g. Select the current values ​​corresponding to the median U at different scan rates within the scan rate range of 0.05 to 5 mV / s, calculate different current density values, and obtain a scatter diagram of scan rate-current density.

[0053] In step S3, the non-Faraday specific capacitance value calculation step, a linear function is obtained by fitting based on the scatter diagram of the scanning speed-current density collected in step S2, and the slope K of the linear function is the non-Faraday specific capacitance value Cdl of the negative electrode sheet in the cathode scanning direction.

[0054] The button battery was assembled as follows. The negative electrode sheet was dried, cut into small circular sheets, weighed, and then transferred to a vacuum oven, dried at 100°C for 8 hours, and then transferred to a glove box filled with argon gas again to assemble the half cell. The assembly method is a common assembly method in the art. The non-Faraday potential range was confirmed using a cyclic Voltammogram curve, and the current value was measured using a linear scanning Voltammogram curve in the potential range to calculate the non-Faraday specific capacitance value Cdl.

[0055] The negative electrode current collector is as follows.

[0056] In some embodiments, the negative current collector includes, but is not limited to, a metal foil, a metal cylinder, a roll of metal tape, a metal sheet, a metal thin film, a metal sheet mesh, a stamping metal, a metal foam, and the like. In some embodiments, the negative current collector is a metal foil. In some embodiments, the negative current collector is an aluminum foil or a copper foil. As used herein, the term "copper foil" includes copper alloy foil.

[0057] In some embodiments, the negative electrode current collector is a conductive resin, hi some embodiments, the conductive resin comprises a film obtained by evaporating copper onto a polypropylene film.

[0058] The negative electrode active material layer is as follows.

[0059] The negative electrode active material layer may be a single layer or multiple layers, and each of the multiple layers may include the same or different negative electrode active materials. The negative electrode active material is any material that can reversibly absorb and release metal ions, such as lithium ions. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being deposited on the negative electrode sheet during charging.

[0060] In some embodiments, the thickness of the negative electrode active material layer refers to the thickness of the negative electrode active material layer coated on one side of the negative electrode current collector. In some embodiments, the thickness of the negative electrode active material layer on one side is 15 μm or more. In some embodiments, the thickness of the negative electrode active material layer on one side is 20 μm or more. In some embodiments, the thickness of the negative electrode active material layer on one side is 30 μm or more. In some embodiments, the thickness of the negative electrode active material layer on one side is 150 μm or less. In some embodiments, the thickness of the negative electrode active material layer on one side is 120 μm or less. In some embodiments, the thickness of the negative electrode active material layer on one side is 100 μm or less. In some embodiments, the thickness of the negative electrode active material layer is within a range consisting of any two of the above numbers. When the thickness of the negative electrode active material layer is within the above range, the electrolyte can penetrate to the vicinity of the interface of the negative electrode current collector, improving the charge and discharge characteristics of the secondary battery at high current density. At the same time, the volume ratio of the negative electrode current collector to the negative electrode active material can be set within an appropriate range to ensure the capacity of the secondary battery.

[0061] In some embodiments, the negative electrode active material layer includes a negative electrode active material, a conductive agent, an adhesive, and a dispersant.

[0062] The negative electrode active material is as follows.

[0063] In some embodiments, the negative electrode active material comprises one or more of synthetic graphite, natural graphite, soft carbon, hard carbon, amorphous carbon, carbon nanotubes, and mesocarbon microspheres.

[0064] The conductive agent is as follows:

[0065] In some embodiments, the conductive agent comprises one or more of carbon black, graphite, carbon fiber, carbon nanotubes, or graphene, preferably carbon black.

[0066] The adhesive is as follows:

[0067] The adhesive improves adhesion between the negative electrode active materials. The type of adhesive is not particularly limited as long as it is a material that is stable against the electrolyte and the solvent used in manufacturing the electrodes. In some embodiments, the adhesive includes sodium carboxymethylcellulose and styrene butadiene rubber.

[0068] The dispersants are as follows:

[0069] In some embodiments, the dispersant comprises diethylhexanol, which is an environmentally friendly organic compound, has low price, wide supply source, low surface tension, and is easy to be adsorbed and spread on the liquid surface. The material is subjected to mechanical force shear and friction, and there is also internal friction between the granules. Under the action of various forces, the raw material granules tend to be highly dispersed, making the slurry more uniform, with good dispersion effect, and the thickness of the produced dry sheet is uniform, avoiding problems such as wrinkles that affect the performance of electrical performance, strengthening the stability of the sheet, improving the transmission efficiency between the positive and negative electrodes of lithium ions, reducing electrochemical polarization, and accelerating non-Faraday reaction processes, and meeting the requirements of the power battery's multiplication performance and cycle life.

[0070] II, electrolyte

[0071] In some embodiments, the electrolyte comprises a sulfur-containing additive, the sulfur-containing additive comprising at least one of Formulas (1)-(5). [ka]

[0072] The content of the sulfur-containing additive is A%, based on the mass of the electrolyte, and 0.05≦Cdl×A%≦12.5, preferably 0.01≦A≦5. Specifically, A may be any one of 0.1, 0.5, 0.7, 1, 1.5, 1.8, 2.2, 2.7, 3, and 4, or a range consisting of any two of these numbers. When the non-Faraday specific capacity of the negative electrode sheet is 50nF / g-250nF / g and the electrolyte contains a sulfur-containing additive, the sulfur-containing additive has high stability and high ionic conductivity, and the interface film formed by the sulfur-containing additive is mainly composed of organic sulfide, so that the impedance is low, the lithium ion conduction ability is improved, and the life of the secondary battery is extended, the side reaction of the electrolyte component itself and the reaction between the electrolyte and the negative electrode material are reduced, the lithium ion transfer rate is improved, the resistance of the SEI film is reduced, and the resistance of the secondary battery is reduced, the polarization phenomenon is reduced, the charge and discharge efficiency is improved, and the internal short circuit of the secondary battery caused by lithium deposition on the negative electrode sheet is avoided. The cooperation of the negative electrode sheet and the electrolyte is favorable to improving the cycle performance of the battery. The appropriate content of the sulfur-containing additive improves the lithium ion conduction efficiency, accelerates the non-Faraday reaction process, and improves the ability to charge at a high rate. In some embodiments of the present application, 0.1≦A≦4. In some embodiments of the present application, 0.5≦A≦3. When the mass percentage of the sulfur-containing additive is within the above range and the non-Faraday specific capacity of the negative electrode sheet is 50 nF / g to 250 nF / g, an electrochemical reaction occurs between the two, the protective film formed is complete, and the film has appropriate density, which reduces the polarization phenomenon and improves the cycle performance of the secondary battery.

[0073] The lithium salts are as follows:

[0074] In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate, lithium organoborate, lithium perchlorate, and sulfonimide type lithium salt. The content of the lithium salt is not particularly limited as long as it does not impair the effect of the present application.

[0075] III. Positive electrode sheet

[0076] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.

[0077] The positive electrode active material layer is as follows.

[0078] The positive electrode active material layer may be a single layer or multiple layers, and each of the multiple negative electrode active material layers may contain the same or different positive electrode active materials. The positive electrode active material is any material that can reversibly absorb and release metal ions, such as lithium ions.

[0079] In some embodiments, the positive electrode active material includes one or more of lithium manganate, lithium iron phosphate (LFP), and ternary materials.

[0080] In some examples, the active cathode material can include a ternary material, and the ternary material can include lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide.

[0081] In some embodiments, the cathode active material comprises lithium nickel cobalt manganese oxide, the molar ratio of elemental nickel, elemental cobalt, and elemental manganese being 1:1:1, in which the content of elemental nickel is greater than or equal to 0.5.

[0082] In some embodiments, the cathode active material comprises lithium nickel cobalt manganese oxide, having a molar ratio of elemental nickel, elemental cobalt, and elemental manganese of 1:1:1, in which the content of elemental nickel is less than or equal to 0.85.

[0083] In some embodiments, the positive electrode active material includes doping elements and / or coating elements, and there is no special requirement for the doping elements and / or coating elements, as long as the positive electrode active material becomes more stable.

[0084] The positive electrode active material further includes a positive electrode conductive agent, a positive electrode adhesive, and a solvent.

[0085] The positive electrode conductive agent is as follows.

[0086] The type of the positive electrode conductive agent is not particularly limited, and any known conductive agent can be used. The positive electrode conductive agent includes, but is not limited to, graphite such as natural graphite and artificial graphite, carbon black such as acetylene black, amorphous carbon such as needle coke, carbon nanotubes, graphene, etc. The above positive electrode conductive agents may be used alone or in any combination.

[0087] The positive electrode adhesive is as follows.

[0088] The type of positive electrode adhesive used in the production of the positive electrode active material layer is not particularly limited, and in the case of a coating method, it is sufficient that the material is soluble or dispersible in the liquid medium used in the production of the electrode. Examples of the positive electrode adhesive may include, but are not limited to, one or more of the following: Resin-based polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, etc.; rubber-like polymers such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, ethylene-propylene rubber, etc.; thermoplastic elastomeric polymers such as styrene-butadiene-styrene block copolymers or their hydrogenated products, ethylene-propylene-diene terpolymer (EPDM), styrene-ethylene-butadiene-ethylene copolymers, styrene-isoprene-styrene block copolymers or their hydrogenated products, etc.; soft resin-like polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, propylene-α-olefin copolymers, etc.; fluoropolymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, polyvinylidene fluoride, polytetrafluoroethylene-ethylene copolymers, etc.; and polymer compositions having ionic conductivity for alkali metal ions (especially lithium ions). The positive electrode adhesives may be used alone or in any combination.

[0089] The solvents are as follows:

[0090] The type of solvent for forming the positive electrode slurry is not limited, and any solvent capable of dissolving or dispersing the positive electrode active material, the positive electrode conductive agent, and the positive electrode adhesive may be used. Examples of the solvent for forming the positive electrode slurry include, but are not limited to, water and a mixture of alcohol and water. Examples of the organic medium include, but are not limited to, diethylenetriamine, N,N-dimethylaminopropylamine, diethyl ether, propylene oxide, tetrahydrofuran (THF), N-methylpyrrolidone (NMP), dimethylformamide, dimethylacetamide, hexamethylphosphoramide, and dimethylsulfoxide.

[0091] The positive electrode current collector is as follows.

[0092] The type of the positive electrode current collector is not particularly limited, and may be any known material suitable for use as a positive electrode current collector. Examples of the positive electrode current collector include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum, carbon materials such as carbon cloth and carbon paper, and composite materials made of polymers and metal layers. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0093] The shape of the positive electrode current collector is not particularly limited. When the positive electrode current collector is a metal material, the shape of the positive electrode current collector includes, but is not limited to, a metal foil, a metal cylinder, a metal tape roll, a metal plate, a metal thin film, a metal plate mesh, a stamping metal, a metal foam, and the like. When the positive electrode current collector is a carbon material, the shape of the positive electrode current collector includes, but is not limited to, a carbon plate, a carbon thin film, a carbon cylinder. In some embodiments, the positive electrode current collector is a metal foil. In some embodiments, the metal foil is in a mesh shape. The thickness of the metal foil is not particularly limited. In some embodiments, the thickness of the metal foil is 1 μm or more, 3 μm or more, or 5 μm or more. In some embodiments, the thickness of the metal foil is 1 mm or less, 50 μm or less, or 20 μm or less. In some embodiments, the thickness of the metal foil is in the range consisting of any two of the above numbers.

[0094] IV, separator

[0095] In order to prevent short circuits, a separator is usually disposed between the positive and negative electrodes, and in this case, the electrolyte of the present invention is usually used by permeating the separator.

[0096] V. Application

[0097] In addition, the present embodiment further provides a battery pack, which includes a secondary battery. Representative applications of the battery pack include, but are not limited to, electric toys, electric tools, battery vehicles, electric vehicles, energy storage devices, ships, spacecraft, etc.

[0098] Hereinafter, the method for producing a secondary battery provided by the present invention will be described based on specific examples.

[0099] Example 1

[0100] The positive electrode sheet was produced as follows.

[0101] A positive electrode slurry was prepared by mixing a positive electrode active material, a positive electrode conductive agent, a positive electrode adhesive, and a solvent. The mass percentage ratio of the positive electrode active material NCM811, the positive electrode conductive agent carbon black, and the positive electrode adhesive polyvinylidene fluoride (PVDF) was 96:2:2, and the solvent was N-methylpyrrolidone (NMP). The obtained positive electrode slurry was uniformly coated on both sides of a positive electrode current collector (aluminum foil), and then dried at 120°C to obtain a positive electrode sheet. The thickness of the positive electrode sheet was adjusted by roll pressing, and its compaction density was 3.5 g / cm. 3 Adjust to.

[0102] The negative electrode sheet was produced as follows.

[0103] First, a negative electrode slurry was prepared. The negative electrode active material in the negative electrode slurry contained artificial graphite, conductive carbon black, sodium carboxymethyl cellulose, styrene-butadiene rubber, and diethylhexanol. The mass ratio of the artificial graphite, conductive carbon black, sodium carboxymethyl cellulose, styrene-butadiene rubber, and diethylhexanol was 96.5:1.2:1.2:1.0:0.1, and the bulk density of the artificial graphite was 1.5 g / cm. 3 , the dispersity is 2.0.

[0104] The specific method for preparing the negative electrode slurry is as follows: 50% artificial graphite, conductive carbon black, 50% artificial graphite and 70% sodium carboxymethylcellulose are added in sequence to a double planetary mixer, the revolution speed of the stirring tank is 20 r / min, the rotation speed is 800 r / min, and the mixture is mixed at a low speed for 30 min to be uniformly mixed, and a portion of deionized water is added and stirred for 1 h to form a first mixed powder material. After scraping and bottom rotation, the remaining 30% sodium carboxymethylcellulose and deionized water are added to the first mixed powder material, the revolution speed is 25 r / min, the rotation speed is 2500 r / min, and the mixture is stirred at a high speed for 90 min. The vacuum degree during this process is adjusted to -0.085 MPa, and the slurry is dispersed to form a second mixed solution. After scraping and bottom rotation, the adhesive styrene butadiene rubber and 50% diethylhexanol are added to the second mixed solution, the revolution speed is 20 r / min, the rotation speed is 500 r / min, and the mixture is stirred at a low speed for 30 min, and the vacuum is adjusted to -0.085 MPa during this process to form a third mixed solution. Finally, 50% diethylhexanol is added to the third mixed solution, the revolution speed is 10 r / min, the rotation speed is 100 r / min, and the mixture is stirred at a low speed for 30 min, and the vacuum is adjusted to -0.085 MPa during this process to form a fourth mixed solution. Finally, deionized water is added to further adjust the viscosity of the slurry, and the revolution speed is set to 25 r / min, the rotation speed is set to 300 r / min, and the mixture is stirred for 30 min, which is more favorable for uniform dispersion of the slurry. During this process, the vacuum degree is adjusted to -0.085 MPa, and when the viscosity of the slurry is 2000 mPa·s to 3500 mPa·s, the slurry passes the test. The slurry is subjected to defoaming treatment at a rotation speed of 200 r / min, stored, and sieved through a 200 mesh sieve to produce a negative electrode slurry. The produced negative electrode slurry is uniformly coated on one or both sides of the copper foil of the negative electrode current collector, and the density of the coating surface is 9.5 mg / cm. 2 The mixture is then calcined and dried, and then roll-cut to obtain a negative electrode sheet. The calcination temperature is 90°C to 110°C, the drying time is 24 hours, and the porosity P of the negative electrode sheet after roll-pressing is 30%.

[0105] Here, the preparation of the negative electrode slurry is mainly performed by thoroughly mixing the active material and the inactive components, fully exerting the electrochemical performance, including the uniformity of the slurry of the electric sheet, avoiding aggregation and sedimentation, ensuring the adjustable coating weight of the sheet, and the consistency of the active material and the inactive components, ensuring the movement between the positive and negative electrodes of the lithium ion battery, and improving the electrochemical performance of the entire battery.

[0106] The electrolyte was prepared as follows.

[0107] Ethylene carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (EDC) are mixed in a volume ratio of 1:1:1, and then 1 mol / L of LiPF6 is added and mixed uniformly to prepare an electrolyte.

[0108] The secondary battery is manufactured as follows.

[0109] The negative electrode sheet and the positive electrode sheet produced by the above steps are dried, and then wound together with the separator using a winding machine to produce an electric core. The positive electrode aluminum tab and the negative electrode copper-nickel plated tab are welded to the electric core. The welded electric core is then packaged in a pouch-formed aluminum plastic film. The separator is made of PP film, and a secondary battery is produced through injection, chemical formation and volume control.

[0110] The non-Faraday specific capacitance value Cdl test of the negative electrode sheet is as follows.

[0111] Step 1: Disassemble the secondary battery in a glove box, obtain the sheet of the negative electrode overhang area, soak it in dimethyl carbonate (DMC) solution, cut it, and then assemble it with a metallic lithium sheet and a button half cell, or cut the negative electrode sheet that is not assembled into a battery, and then assemble it with a metallic lithium piece and a button half cell.

[0112] Step 2: Conduct a CV test on the button half-cell in the voltage range of 0.005 V to 3.0 V, with a scan rate of 0.1 mV / s, and ensure that the non-Faraday potential range is 2.6 V to 2.7 V.

[0113] Step 3: Then, LSV test was performed from 2.7V to 2.6V, and the scan rates were 0.1mV / s, 0.2mV / s, 0.5mV / s, 1mV / s, and 2mV / s, respectively. The median potential range of 2.65V was selected to obtain the corresponding current values ​​of -4.32E-07A, -5.50E-07A, -1.15E-06A, -2.08E-06A, and -3.80E-06A. Based on the corresponding mass of active material of 0.02175g, the current density values ​​of -1.25E-05A / g, -2.08E-05A / g, -4.75E-05A / g, -8.87E-05A / g, and -1.64E-04A / g were calculated.

[0114] Step 4: Based on the scan rate and current density values ​​obtained in step 3, a scatter plot of scan rate-current density is made and fitted to obtain a linear function, the slope of the linear function is -8E-05, that is, the non-Faraday specific capacitance Cdl of the negative electrode sheet in the cathode scan direction is 80 nF / g.

[0115] Here, the negative electrode sheet overhang region refers to the portion of the negative electrode sheet that protrudes from the positive electrode sheet in the longitudinal and transverse directions.

[0116] Example 2

[0117] In Example 2, a secondary battery is produced by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0118] Coating weight of negative electrode sheet CW mg / cm 2 7mg / cm 2 The porosity P of the negative electrode sheet is 25%, the resistance R mΩ of the negative electrode active material layer is 3 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 140 nF / g.

[0119] Example 3

[0120] In Example 3, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0121] Coating weight of negative electrode sheet CW mg / cm 2 12mg / cm 2 The porosity P of the negative electrode sheet is 25%, the resistance R mΩ of the negative electrode active material layer is 15 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 200 nF / g.

[0122] Example 4

[0123] In Example 4, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0124] Coating weight of negative electrode sheet CW mg / cm 2 9mg / cm 2 The porosity P of the negative electrode sheet is 20%, the resistance R mΩ of the negative electrode active material layer is 1 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 250 nF / g.

[0125] Example 5

[0126] In Example 5, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0127] Coating weight of negative electrode sheet CW mg / cm 2 9mg / cm 2 The porosity P of the negative electrode sheet is 40%, the resistance R mΩ of the negative electrode active material layer is 8 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 50 nF / g.

[0128] Example 6

[0129] In Example 6, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0130] Coating weight of negative electrode sheet CW mg / cm 2 12mg / cm 2 The porosity P of the negative electrode sheet is 25%, the resistance R mΩ of the negative electrode active material layer is 15 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 200 nF / g.

[0131] Example 7

[0132] In Example 7, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0133] Coating weight of negative electrode sheet CW mg / cm 2 10.5mg / cm 2 The porosity P of the negative electrode sheet is 26%, the resistance R mΩ of the negative electrode active material layer is 12 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 230 nF / g.

[0134] Example 8

[0135] In Example 8, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0136] Coating weight of negative electrode sheet CW mg / cm 2 9mg / cm 2 The porosity P of the negative electrode sheet is 20%, the resistance R mΩ of the negative electrode active material layer is 2 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 250 nF / g.

[0137] Example 9

[0138] In Example 9, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0139] Coating weight of negative electrode sheet CW mg / cm 2 10mg / cm 2 The porosity P of the negative electrode sheet is 40%, the resistance R mΩ of the negative electrode active material layer is 2 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 50 nF / g.

[0140] Example 10

[0141] In Example 10, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0142] Coating weight of negative electrode sheet CW mg / cm 2 9.2mg / cm 2 The porosity P of the negative electrode sheet is 30%, the resistance R mΩ of the negative electrode active material layer is 2.5 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 65 nF / g.

[0143] Example 11

[0144] In Example 11, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0145] Coating weight of negative electrode sheet CW mg / cm 2 9.1mg / cm 2 The porosity P of the negative electrode sheet is 25%, the resistance R mΩ of the negative electrode active material layer is 6.3 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 150 nF / g.

[0146] Example 12

[0147] In Example 12, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0148] Coating weight of negative electrode sheet CW mg / cm 2 9.6mg / cm 2 The porosity P of the negative electrode sheet is 30%, the resistance R mΩ of the negative electrode active material layer is 9.5 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 150 nF / g.

[0149] Example 13

[0150] In Example 13, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0151] Coating weight of negative electrode sheet CW mg / cm 2 10mg / cm 2 The porosity P of the negative electrode sheet is 22%, the resistance R mΩ of the negative electrode active material layer is 11 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 150 nF / g.

[0152] Comparative Example 1

[0153] In Comparative Example 1, a secondary battery was fabricated by the method of Example 1, but the other parts were the same as those of Example 1, except for the following differences.

[0154] Coating weight of negative electrode sheet CW mg / cm 2 5mg / cm 2 The porosity P of the negative electrode sheet is 42%, the resistance R mΩ of the negative electrode active material layer is 10 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 260 nF / g.

[0155] Comparative Example 2

[0156] In Comparative Example 2, a secondary battery was fabricated by the method of Example 1, but the other parts were the same as those of Example 1, except for the following differences.

[0157] Coating weight of negative electrode sheet CW mg / cm 2 14mg / cm2 The porosity P of the negative electrode sheet is 18%, the resistance R mΩ of the negative electrode active material layer is 12 mΩ, and the non-Faraday specific capacitance Cdl nF / g of the negative electrode sheet is 45 nF / g.

[0158] The performance test process and test results of the secondary battery according to the embodiment of the present application are as follows.

[0159] (1) Dynamic performance test

[0160] The secondary battery is left at 25°C for 30 minutes, fully charged at xC, fully discharged at 1C, and then fully charged again at xC. The negative electrode sheet is then disassembled and the state of lithium deposition on the surface of the negative electrode sheet is observed. If no lithium is deposited on the surface of the negative electrode, the charge rate xC is increased by 0.1C each time and the test is repeated until lithium is deposited on the surface of the negative electrode. The maximum charge rate of the battery is determined by subtracting 0.1C from the charge rate xC at this time.

[0161] (2) Energy density test

[0162] The secondary battery is left at 25°C for 30 minutes, fully charged at 1C, and fully discharged at 1C, and the actual discharge energy is recorded. The lithium ion battery is weighed on an electronic balance, and the ratio of the actual discharge energy at 1C to the weight is the actual energy density of the secondary battery. Here, if the actual energy density is 80% or less of the target energy density, the actual energy density of the secondary battery is considered to be very low. If the actual energy density is 80% or more and 95% or less of the target energy density, the actual energy density of the secondary battery is considered to be low. If the actual energy density is 95% or more and 105% or less of the target energy density, the actual energy density of the secondary battery is considered to be appropriate. If the actual energy density is 105% or more and 120% or less of the target energy density, the actual energy density of the secondary battery is considered to be high. If the actual energy density reaches 120% of the target energy density, the actual energy density of the secondary battery is considered to be very high.

[0163] (3) Cycle performance test

[0164] A cycle test is performed on the secondary battery by leaving it at 25°C for 30 minutes, discharging at a constant current of 1C, leaving it at rest for 10 minutes, charging at a constant current and constant voltage of 1C, leaving it at rest for 10 minutes, and then fully charging and fully discharging the battery. The capacity retention rate after 1000 cycles is recorded.

[0165] Table 1 shows the performance test results of the secondary batteries according to Examples 1 to 13 and the performance test results of the secondary batteries according to Comparative Examples 1 and 2.

[0166] [Table 1]

[0167] Referring to Table 1, the secondary batteries according to Examples 1 to 13 have excellent dynamic performance, high or very high energy density, and the capacity retention rate of the cycle performance reaches 91% to 96%. As a result, the secondary batteries according to the examples of the present application have high or very high energy density while being fast charged at a high rate, and have excellent cycle performance (the capacity retention rate of the cycle performance reaches 91% to 96%).

[0168] On the other hand, the coating amount of the negative electrode active material layer in Comparative Example 1 was 5 mg / cm 2 The porosity P of the negative electrode sheet was 42%, and the non-Faraday specific capacitance value Cdl of the negative electrode sheet reached 260 nF / g, so that the dynamic performance of the secondary battery according to Comparative Example 1 was deteriorated, the energy density was very low, and the capacity retention rate after the cycle performance test was only 85%. The coating amount of the negative electrode active material layer in Comparative Example 2 was 14 mg / cm 2 The porosity P of the negative electrode sheet was 18%, and the non-Faraday specific capacitance value Cdl of the negative electrode sheet was 260. The secondary battery according to Comparative Example 2 had a high energy density, but the capacity retention rate after the cycle performance test was only 86%, resulting in a decrease in dynamic performance.

[0169] Therefore, in both the secondary batteries according to Comparative Example 1 and Comparative Example 2, it is difficult to maintain a high energy density and excellent cycle performance while performing high-rate charging at a large rate.

[0170] Example 14

[0171] In Example 14, a secondary battery was prepared by the method of Example 1, and the coating weight CW of the negative electrode active material layer was 2 9mg / cm 2 and the porosity P is 35%, but the other parts are the same as in Example 1 except for the following differences.

[0172] The bulk density of the negative electrode active material is 1.5 g / cm 3 The granular dispersity of the negative electrode active material is set to 2, and the non-Faraday specific capacity Cdl nF / g of the negative electrode sheet is set to 200 nF / g.

[0173] Example 15

[0174] In Example 15, a secondary battery was prepared by the method of Example 1, and the coating weight CW of the negative electrode active material layer was 2 9mg / cm 2 and the porosity P is 35%, but the other parts are the same as in Example 1 except for the following differences.

[0175] The bulk density of the negative electrode active material is 1 g / cm 3 The granular dispersity of the negative electrode active material is set to 1.5, and the non-Faraday specific capacity Cdl nF / g of the negative electrode sheet is set to 240 nF / g.

[0176] Example 16

[0177] In Example 16, a secondary battery was prepared by the method of Example 1, and the coating weight CW of the negative electrode active material layer was 2 9mg / cm 2 and the porosity P is 35%, but the other parts are the same as in Example 1 except for the following differences.

[0178] The bulk density of the negative electrode active material is 1.8 g / cm3 The granular dispersity of the negative electrode active material is set to 2.5, and the non-Faraday specific capacity Cdl nF / g of the negative electrode sheet is set to 180 nF / g.

[0179] Example 17

[0180] In Example 17, a secondary battery was prepared by the method of Example 1, and the coating weight CW of the negative electrode active material layer was 2 9mg / cm 2 and the porosity P is 35%, but the other parts are the same as in Example 1 except for the following differences.

[0181] The bulk density of the negative electrode active material is 2 g / cm 3 The granular dispersity of the negative electrode active material is set to 3, and the non-Faraday specific capacity Cdl nF / g of the negative electrode sheet is set to 150 nF / g.

[0182] Example 18

[0183] In Example 18, a secondary battery was prepared by the method of Example 1, and the coating weight CW of the negative electrode active material layer was 2 9mg / cm 2 and the porosity P is 35%, but the other parts are the same as in Example 1 except for the following differences.

[0184] The bulk density of the negative electrode active material is 2.2 g / cm 3 The granular dispersity of the negative electrode active material is set to 4, and the non-Faraday specific capacity Cdl nF / g of the negative electrode sheet is set to 100 nF / g.

[0185] Example 19

[0186] In Example 19, a secondary battery was prepared by the method of Example 1, and the coating weight CW of the negative electrode active material layer was 2 9mg / cm 2 and the porosity P is 35%, but the other parts are the same as in Example 1 except for the following differences.

[0187] The bulk density of the negative electrode active material is 2.5 g / cm3 The granular dispersity of the negative electrode active material is set to 5, and the non-Faraday specific capacity Cdl nF / g of the negative electrode sheet is set to 60 nF / g.

[0188] Table 2 shows the performance test results of the secondary batteries according to Examples 14 to 19.

[0189] [Table 2]

[0190] Referring to Table 2, the secondary batteries according to Examples 14 to 19 have dynamic performances of 2C to 4C, and therefore the secondary batteries according to Examples 14 to 19 have high or very high energy density while undergoing high-rate charging and have excellent cycle performance.

[0191] Example 20

[0192] In Example 20, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0193] The sulfur-containing additive shown in formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 0.05%.

[0194] Example 21

[0195] In Example 21, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0196] The sulfur-containing additive shown in formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 0.1%.

[0197] Example 22

[0198] In Example 22, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0199] The sulfur-containing additive shown in formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 0.5%.

[0200] Example 23

[0201] In Example 23, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0202] The sulfur-containing additive shown in formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 1%.

[0203] Example 24

[0204] In Example 24, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0205] The sulfur-containing additive shown in formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 2%.

[0206] Example 25

[0207] In Example 25, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0208] The sulfur-containing additive shown in formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 5%.

[0209] Example 26

[0210] In Example 26, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0211] The sulfur-containing additive represented by formula (3) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 0.1%.

[0212] Example 27

[0213] In Example 27, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0214] The sulfur-containing additive shown in formula (3) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive in the electrolyte is 1%.

[0215] Example 28

[0216] In Example 28, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0217] A combination of formula (3) and formula (4) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive represented by formula (3) in the electrolyte is 0.5%, and the content of the sulfur-containing additive represented by formula (4) in the electrolyte is 0.5%.

[0218] Example 29

[0219] In Example 29, a secondary battery is fabricated by the method of Example 1, but the other parts are the same as those of Example 1, except for the following differences.

[0220] A combination of formula (1) and formula (3) is selected as the sulfur-containing additive in the electrolyte, and the content of the sulfur-containing additive represented by formula (1) in the electrolyte is 0.3%, and the content of the sulfur-containing additive represented by formula (3) in the electrolyte is 0.5%.

[0221] Table 3 shows the performance test results of the secondary batteries according to Examples 14 to 19.

[0222] [Table 3]

[0223] Referring to Table 3, the secondary batteries of Examples 20 to 29 have dynamic performance reaching 2.6C to 4C, and therefore the secondary batteries of Examples 20 to 29 have high or very high energy density while undergoing high-rate charging, and have excellent cycle performance (the capacity retention rate of the cycle performance reaches 94 to 96%).

[0224] The above is a detailed description of the secondary battery and battery pack according to the embodiments of the present application, and the principles and embodiments of the present application are described using specific examples. The above description of the embodiments is for the purpose of helping to understand the technical solutions and their core ideas of the present application. Those skilled in the art should understand that some of the technical features described in the above embodiments may be modified or replaced with equivalents, and such modifications and replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of each embodiment of the present application.

Claims

1. In a secondary battery including a positive electrode sheet, an electrolyte, and a separator, a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including graphite, Here, the non-Faraday specific capacity of the negative electrode sheet is Cdl nF / g, and 50≦Cdl≦250. Secondary battery.

2. The resistance of the negative electrode active material layer is R mΩ, and 4≦0.1×Cdl−R≦24. The secondary battery according to claim 1 .

3. The numerical range of R is 1≦R≦15. The secondary battery according to any one of claims 1 to 2.

4. The porosity P of the negative electrode sheet is 20% to 40%. The secondary battery according to any one of claims 1 to 3.

5. The coating weight of the negative electrode active material layer on one surface of the negative electrode current collector is CW mg / cm 2 and 7≦CW≦12. The secondary battery according to any one of claims 1 to 4.

6. The bulk density of the negative electrode active material is 1 g / cm 3 ~2.5g / cm 3 That is, The secondary battery according to any one of claims 1 to 5.

7. The granular dispersity of the negative electrode active material is 1.5 to 5. The secondary battery according to any one of claims 1 to 6.

8. The electrolyte contains a sulfur-containing additive, and the sulfur-containing additive contains at least one of formulas (1) to (5), 【Chemistry 1】 The secondary battery according to any one of claims 1 to 7.

9. The content of the sulfur-containing additive is A% based on the mass of the electrolyte, and 0.05≦Cdl×A%≦12.5; The secondary battery according to claim 8.

10. The content of the sulfur-containing additive is A% based on the mass of the electrolyte, and 0.01≦A≦5. The secondary battery according to any one of claims 8 to 9.

11. A secondary battery comprising the secondary battery according to any one of claims 1 to 10. Battery pack.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP2006344390A

  • Electrode material for nonaqueous electrolyte battery, electrode for nonaqueous electrolyte battery, nonaqueous electrolyte battery including the same, and battery pack

    JP2017168380A

  • Anode material, anode containing said anode material, and electrochemical device

    JP2021536104A

  • Electrochemical device and electronic device having same

    WO2021128095A1

  • Secondary battery, preparation method therefor, and battery module, battery package and device containing same

    WO2022021273A1