Battery cell housing made from aluminum alloy strip with high recycled content
The use of a specific aluminum alloy composition in battery cell housings addresses the limitations of AA3003 by achieving high recycling rates and improved mechanical and electrical properties, enhancing the performance and sustainability of battery cell housings.
Patent Information
- Application Number
- JP2024520697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-05
- Filing Date
- 2022-10-05
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing battery cell housings made from aluminum alloy AA3003 lack high recycling rates and do not meet the requirements of strength, electrolyte stability, and electrical and thermal conductivity, which are essential for modern applications, particularly in electric mobility and consumer electronics.
An aluminum alloy strip or sheet with specific alloy compositions, including 0.1%≦Si≦0.5%, 0.25%≦Fe≦0.8%, Cu≦0.6%, 0.6%≦Mn≦1.4%, 0.5%≦Mg≦1.5%, Cr≦0.25%, Zn≦0.4%, Ti≦0.2%, and a balance of Al and unavoidable impurities, is used to create battery cell housings, allowing for high recycling rates and improved mechanical and electrical properties.
The new alloy composition achieves high recycling rates, enhanced strength, electrolyte stability, and improved electrical and thermal conductivity, enabling efficient production of battery cell housings with reduced environmental impact and increased energy density.
Smart Images

Figure 2024539845000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery cell housing having an aluminum alloy strip or sheet and the use of the aluminum alloy strip or sheet for manufacturing a battery cell housing. [Background technology]
[0002] Battery cells are used in a wide variety of technical applications to supply electrical consumers with electrical energy. Fields of application for battery cells are, for example, in electric mobility, in particular electric cars, electric bicycles and electric scooters, in consumer electronics, in particular laptop computers, tablet computers, mobile phones, digital cameras and camcorders, or in energy technology, in particular battery storage, to name just a few. To form a battery module or battery system, several battery cells are often connected in series or parallel. However, there are also applications in which a single battery cell is used as the energy source.
[0003] Battery cells can be fundamentally differentiated into primary batteries, which can only be discharged once and cannot be repeatedly charged, and secondary batteries, which can be repeatedly charged. The necessary electrochemical processes providing the functionality of a battery cell can be implemented with a wide variety of different materials, both in primary and secondary batteries. Examples of primary batteries in this context are alkaline-manganese batteries, zinc-carbon batteries, nickel-oxyhydroxide batteries or lithium-iron sulfide batteries, to name just a few. Examples of secondary batteries are lithium-ion batteries, sodium-ion batteries, nickel-cadmium batteries, nickel-metal hydride batteries or nickel-zinc batteries, to name just a few.
[0004] For many years, lithium-ion secondary batteries have been increasingly used, especially in the field of electric mobility and consumer electronics, due to their relatively high gravimetric and volumetric energy density. Like other types of battery cells, lithium-ion secondary batteries have a battery cell housing, which forms the external shape of the battery cell and encloses a cavity that contains, among other things, the anode material, the cathode material and the electrolyte. A distinction may be made between different designs of battery cell housings. A cylindrical battery cell housing has essentially the shape of a cylinder. If the height of the cylinder is greater than its diameter, it is called a circular battery, otherwise a button battery. A battery cell housing of prismatic design has essentially the shape of a prism, in particular a rectangular parallelepiped. Another variant is the pouch design, where the battery cell housing essentially has the shape of a pocket or pouch.
[0005] Due to the high demands on strength and mechanical stability as well as on electrochemical stability against the electrolyte acting corrosively on the battery cell housing, cylindrical battery cell housings have been generally manufactured up to now from nickel-plated steel in particular. However, increasing cell formats, such as the increasing replacement of type 18650 circular cells by type 21700 circular cells in the field of electric mobility and the expected future replacement of type 21700 circular cells by type 46800 circular cells, are imposing higher demands on electrical and thermal conductivity due to the generation of larger amounts of heat that need to be dissipated. Potential aluminum materials must moreover meet the high demands on the strength of the housing material.
[0006] The use of aluminum alloys for cylindrical battery cell housings is already known, but is limited to the aluminum alloy AA3003. As an example of this, reference may be made to US Pat. No. 5,399,323. On the other hand, for prismatic battery cell housings the aluminum alloy AA3003 is standard, but its use in the field of prismatic cell housings is also limited to this alloy.
[0007] US Pat. No. 5,399,433 discloses a high-strength battery housing made of a composite material having a plastic outer layer and an aluminium foil made of aluminium alloys of type AA8079, 1N30, AA8021, AA3003, AA3004, AA3104 or AA3105.
[0008] The same aluminium alloys are known from US Pat. No. 5,399,323, which suggests that aluminium alloys of type AA3003 are preferably used.
[0009] US Pat. No. 5,399,433 focuses on the strength and wettability of the battery housing and proposes the use of aluminum alloys of the types AA3003, AA3203, AA3004, AA3104, AA3005 or AA3105.
[0010] None of the aforementioned documents address the issue of recyclability taking into account the requirements for strength, electrolyte stability and electrical and thermal conductivity of the battery cell housing.
[0011] However, sustainability requirements, which have increased greatly in recent years, are calling for the production of battery cell housings with as small a CO2 footprint as possible. The most effective way is to reduce the use of energy-intensive primary aluminum by increasing the use of recycled materials, also called secondary aluminum. Secondary aluminum is obtained by melting aluminum scrap. In the case of aluminum scrap, a distinction is made between pre-consumer and post-consumer scrap. Pre-consumer scrap is waste generated during the production of semi-finished or final products made from aluminum or aluminum alloys in the wide variety of possible processes. Pre-consumer scrap may be further divided into internal process scrap, such as sprues, offcuts, swarf, production leftovers or production rejects, which is unavoidably generated within the process of producing aluminum strip or sheet on the one hand, and external process scrap, such as perforation scrap, swarf or production rejects, which is unavoidably generated in the further processing to form the final product on the other hand. Post-consumer scrap is the final product that has completed its entire life cycle and becomes waste after it has been used. It does not matter whether it has been used by an end user, meaning that it may have been used, for example, in an industrial or commercial facility. Examples of post-consumer wrap include food packaging, especially beverage cans, window frames, lithographic printing plate carriers, cable cores and automotive components.
[0012] According to international standards, the alloy composition of the aluminum alloy AA3003 used so far for battery cell housings is relatively restricted, for example with respect to the standard alloy elements copper, magnesium, chromium, zinc and titanium. Therefore, the use of this alloy requires the use of a high proportion of primary aluminum, which in turn prevents the achievement of high recycling rates. Prior art battery cell housings made from the aluminum alloy AA3003 therefore need to be improved with respect to their sustainability.
[0013] Against this background, the object of the present invention is to provide a battery cell housing with an aluminum alloy strip or sheet which makes it possible to achieve high recycling rates and at the same time meets the requirements of the battery cell housing, in particular with regard to strength, electrolyte stability and electrical and thermal conductivity.
[0014] A further object of the present invention is to provide a corresponding use of the aluminum alloy strip or sheet for manufacturing a battery cell housing. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] U.S. Patent No. 6,258,480(B1) [Patent Document 2] US Patent No. 2006 / 093908(A1) [Patent Document 3] Korean Patent Application No. 2016 005673(A) [Patent Document 4] Patent Publication No. 2015-125886(A) Summary of the Invention [Means for solving the problem]
[0016] According to a first teaching of the present invention, the aforementioned object of the battery cell housing having an aluminum alloy strip or sheet is achieved by providing the aluminum alloy strip or sheet with the following properties in weight percent: 0.1%≦Si≦0.5%, 0.25%≦Fe≦0.8%, Cu≦0.6%, 0.6%≦Mn≦1.4%, 0.5%≦Mg≦1.5%, Cr≦0.25%, Zn≦0.4%, Ti≦0.2%, The balance is Al and incidental impurities of not more than 0.05% individually and not more than 0.15% in total. This is achieved by having an aluminum alloy with alloying components.
[0017] Surprisingly, the inventors have found in testing that battery cell housings with aluminum alloy strip or sheet according to the invention meet the corresponding requirements, in particular with regard to strength, electrolyte stability and electrical and thermal conductivity. Above all, it has been surprisingly found that the electrolyte stability and weldability are not or are not significantly reduced compared to the already known alloy AA3003. At the same time, the battery cell housings according to the invention are suitable for achieving high recycling rates due to the specified copper and magnesium content of the aluminum alloy. This applies in particular to the use of UBC scrap (UBC: used beverage cans), i.e. beverage cans made of an aluminum alloy that has a significant content of magnesium and copper and is suitable for producing the aluminum alloy of the aluminum strip or sheet of the battery cell housing. All of the aforementioned advantages are achieved by the alloy composition of the aluminum alloy strip or sheet of the battery cell housing. The aluminum alloy can also be recycled well itself, since it further contains only standard alloying elements, so that the battery cell housings according to the invention can be easily added to existing scrap recycling operations.
[0018] According to the invention, the silicon content of the aluminum alloy is in the range of 0.1 wt%≦Si≦0.5 wt%. In one embodiment of the battery cell housing according to the invention, the silicon content of the aluminum alloy is in the range of 0.2 wt%≦Si≦0.4 wt%, preferably 0.2 wt%≦Si≦0.35 wt%. Combined with the iron and manganese content according to the invention in the specified amounts, a silicon content of 0.1 wt%≦Si≦0.5 wt% results in dense particles of the quaternary α-Al(Fe,Mn)Si phase, which is particularly distributed relatively uniformly. These precipitated particles remove the iron and manganese from the solid solution without adversely affecting other properties such as the corrosion behavior, i.e. electrolyte stability or formability, thus increasing both the strength of the aluminum alloy and its electrical and thermal conductivity. A silicon content of less than 0.1 wt% results in reduced precipitation of the α-Al(Fe,Mn)Si phase, which may reduce the electrical and thermal conductivity due to the dissolved manganese. Furthermore, the absence of the α-Al(Fe,Mn)Si phase adversely affects tool wear. A silicon content of more than 0.5 wt.% can result in the formation of the Mg2Si phase when combined with magnesium, which adversely affects the solid solution hardening of magnesium. The silicon content passage of the aforementioned embodiment of 0.2 wt.%≦Si≦0.4 wt.%, preferably 0.2 wt.%≦Si≦0.35 wt.%, represents an ideal compromise between high strength and high electrical and thermal conductivity.
[0019] According to the invention, the iron content of the aluminum alloy is in the range of 0.25%≦Fe≦0.8% by weight. In one embodiment of the battery cell housing according to the invention, the iron content of the aluminum alloy is in the range of 0.3%≦Fe≦0.7% by weight, preferably 0.4%≦Fe≦0.7% by weight. When combined with the manganese content according to the invention in the specified amount, an iron content of 0.25%≦Fe≦0.8% by weight leads to the formation of the Al6(Mn,Fe) phase, which, as already explained above, when combined with the silicon and manganese content according to the invention in the specified amount leads to the precipitation of particles of the quaternary α-Al(Fe,Mn)Si phase. Iron in this case contributes to reducing the solubility of manganese in aluminum, so that more manganese is bound in the intermetallic phase, which has a positive effect on the electrical and thermal conductivity. Furthermore, the intermetallic phase influences the recovery and recrystallization processes and improves the thermal stability of the mechanical properties. An iron content of more than 0.8 wt.% promotes the formation of coarse intermetallic phases that may reduce formability in deep drawing processes. On the other hand, an iron content of less than 0.25 wt.% overly limits the tolerance of the present aluminum alloy to iron-based scrap, since conventional scrap grades generally have a significant proportion of iron. Overly limiting the iron content may therefore prevent the achievement of high recycling rates. Thus, the iron content passage of the aforementioned embodiment of 0.3 wt.%≦Fe≦0.7 wt.%, preferably 0.4 wt.%≦Fe≦0.7 wt.%, represents an ideal combination of recyclability, use of a high proportion of recycled material, thermal stability, electrical and thermal conductivity, and formability.
[0020] According to the invention, the copper content of the aluminum alloy is in the range Cu≦0.6 wt.%. In one embodiment of the battery cell housing according to the invention, the copper content of the aluminum alloy is in the range Cu≦0.3 wt.%, preferably 0.1 wt.%≦Cu≦0.2 wt.%. The fact that a copper content of up to 0.6 wt.% is permitted results in an increased tolerance of the aluminum alloy to copper-containing aluminum alloy scrap, which facilitates the achievement of a high proportion of recycled material in the manufacture of the battery housing. However, since an excessively high copper content may adversely affect the corrosion properties, according to the invention the copper content is limited to at most 0.6 wt.% in order to achieve a sufficiently high electrolyte stability. For improved electrolyte stability and sufficiently high electrical and thermal conductivity, the copper content in the aforementioned embodiment is limited to 0.3 wt.%. However, the presence of copper also causes an increase in the strength of the aluminum alloy due to solid solution hardening, which is only noticeable above a content of 0.1 wt.%. Thus, the preferred range of 0.1 wt.%≦Cu≦0.2 wt.% represents a compromise between high strength, sufficiently high electrical and thermal conductivity as well as improved electrolyte stability and sufficient recycling tolerance.
[0021] According to the invention, the manganese content of the aluminum alloy is in the range of 0.6%≦Mn≦1.4% by weight. In one embodiment of the battery cell housing according to the invention, the manganese content of the aluminum alloy is in the range of 0.8%≦Mn≦1.1% by weight. As already explained above, a manganese content of 0.6%≦Mn≦1.4% by weight or 0.8%≦Mn≦1.1% by weight, combined with the silicon and iron contents in the specified amounts, leads to the precipitation of particles of the quaternary α-Al(Fe,Mn)Si phase as well as the Al6(Mn,Fe) phase. These intermetallic phases hinder the recovery and recrystallization processes and thus improve the thermal stability of the mechanical properties. A manganese content below 0.8% by weight already reduces the increase in strength due to dispersoids and solid solution hardening. Manganese contents below 0.6 wt.% lead to insufficient increase in strength due to dispersoids and solid solution hardening, while manganese contents above 1.1 wt.%, and especially above 1.4 wt.%, promote the formation of coarse intermetallic phases that adversely affect the forming properties in deep drawing processes. Furthermore, manganese contents above 1.1 wt.%, and especially above 1.4 wt.%, significantly reduce the electrical and thermal conductivity of the battery cell housing, resulting in inefficient thermal management.
[0022] According to the invention, the magnesium content of the aluminum alloy is in the range of 0.5 wt%≦Mg≦1.5 wt%. In one embodiment of the battery cell housing according to the invention, the magnesium content of the aluminum alloy is in the range of 0.8 wt%≦Mg≦1.5 wt%, preferably 0.8 wt%≦Mg≦1.2 wt%. The fact that a magnesium content of up to 1.5 wt% is allowed results in an increased tolerance of the aluminum alloy to magnesium-containing aluminum alloy scrap, such as UBC scrap, which further facilitates the achievement of a high proportion of recycled material in the manufacture of the battery cell housing. Furthermore, the presence of magnesium above a content of at least 0.5 wt% leads to an efficient solid solution hardening, which contributes to an increase in cold hardening and thus increases the strength. However, since an excessively high magnesium content has a negative effect on the electrical and thermal conductivity, the magnesium content is limited according to the invention to at most 1.5 wt%. In order to achieve improved mechanical properties, the magnesium content in the aforementioned embodiment is increased to at least 0.8 wt%. The preferred range of 0.8%≦Mg≦1.2% represents a compromise between high strength, good forming behavior and high electrical and thermal conductivity with good recycling tolerance.
[0023] According to the invention, the chromium content of the aluminum alloy is in the range of Cr≦0.25 wt.%. In one embodiment of the battery cell housing according to the invention, the chromium content of the aluminum alloy is in the range of Cr≦0.1 wt.%, preferably Cr≦0.05 wt.%. The fact that a chromium content of up to 0.25 wt.% is allowed results in an increased tolerance of the aluminum alloy to chromium-containing aluminum alloy scrap, which facilitates the achievement of a high proportion of recycled material in the manufacture of the battery cell housing. Furthermore, chromium also has a strength-increasing effect and forms dispersoids. Dispersoids increase the thermal stability and prevent softening due to recrystallization or recovery. However, since an excessively high chromium content can adversely affect the electrical conductivity of the aluminum alloy, the chromium content is limited according to the invention to at most 0.25 wt.%. For improved conductivity with still sufficient recycling tolerance and strength, the chromium content in the aforementioned embodiment is limited to 0.1 wt.%, preferably 0.05 wt.%.
[0024] According to the invention, the zinc content of the aluminum alloy is in the range of Zn≦0.4 wt.%. In one embodiment of the battery cell housing according to the invention, the zinc content of the aluminum alloy is in the range of 0.02 wt.%≦Zn≦0.25 wt.%, preferably 0.04 wt.%≦Zn≦0.25 wt.%. The fact that a maximum zinc content of 0.4 wt.% is permitted results in an increased tolerance of the aluminum alloy to zinc-containing aluminum alloy scrap, which further facilitates the achievement of a high recycling rate. Zinc also has a strength-increasing effect. However, an excessively high zinc content reduces the weldability, electrical and thermal conductivity, and corrosion resistance of the aluminum alloy, so according to the invention the zinc content is limited to at most 0.4 wt.%. In the aforementioned embodiment, the zinc content is adjusted within the passage of 0.02 wt.%≦Zn≦0.25 wt.%, preferably 0.04 wt.%≦Zn≦0.25 wt.%, so that an optimal compromise between high strength, good weldability and good electrolyte stability with recycling tolerance remaining good is achieved.
[0025] According to the invention, the titanium content of the aluminum alloy is in the range of Ti≦0.2 wt.%. In one embodiment of the battery cell housing according to the invention, the titanium content of the aluminum alloy is in the range of 0.005 wt.%≦Ti≦0.1 wt.%, preferably 0.005 wt.%≦Ti≦0.05 wt.%. The fact that a maximum titanium content of 0.2 wt.% is permitted results in an increased tolerance of the aluminum alloy to titanium-containing aluminum alloy scrap, which facilitates the achievement of a high proportion of recycled material in the manufacture of the battery cell housing. However, an excessively high titanium content can adversely affect the forming properties of the aluminum alloy and significantly reduce the electrical and thermal conductivity, so that the titanium content is limited to at most 0.2 wt.% according to the invention. Conversely, titanium above a content of 0.005 wt.% improves grain refinement when casting the aluminum alloy. In order to achieve good grain refinement together with good formability, sufficiently high electrical and thermal conductivity and sufficient recycling tolerance, the titanium content in the aforementioned embodiments is therefore adjusted within the range of 0.005 wt.%≦Ti≦0.1 wt.%, preferably 0.005 wt.%≦Ti≦0.05 wt.%.
[0026] In addition to the above-mentioned alloying components, the balance of the aluminum alloy of the battery cell housing according to the invention consists of aluminum and unavoidable impurities. Avoidable impurities are alloying components that are not intentionally added but are inevitably contained in the aluminum alloy due to production. According to the invention, the content of each unavoidable impurity is limited to 0.05% by weight, and the content of all unavoidable impurities is limited to 0.15% by weight in total. This ensures that the unavoidable impurities do not adversely affect or have a significant adverse effect on the properties of the aluminum alloy, for example by the formation of undesirable phases.
[0027] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy has a proportion of recycled material of at least 50% by weight, preferably at least 70% by weight. Due to the above-mentioned high recycling tolerance of the aluminum alloy, it is possible to achieve a high recycling rate of at least 50% by weight, preferably at least 70% by weight, for the battery cell housing according to the invention. The associated energy savings allow the production of the battery cell housing with the smallest possible CO2 footprint and improved sustainability. In particular, the aluminum alloy of the battery cell housing according to the invention has a proportion of post-consumer scrap of at least 50% by weight, preferably at least 70% by weight. The use of post-consumer scrap is particularly CO2-efficient, so that a particularly large reduction in the CO2 footprint can be achieved thereby. Additionally or alternatively, by using pre-consumer scrap, in particular by using internal process scrap and / or external process scrap, a proportion of recycled material of at least 50% by weight, preferably at least 70% by weight, is achieved. In the internal process scrap, the composition and amount of the individual alloys are generally very well known, so that the alloy composition resulting from the melting of the internal process scrap can be well determined. Although external process scrap is less well defined in terms of its composition than internal process scrap and may require further processing, it occurs in large proportions, for example in the manufacture of drilled parts, so that recycling is economically and sustainability relevant. By recycling external process scrap, the demand for primary metals can be reduced, which lowers the overall CO2 balance.
[0028] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet has a strain hardening state of type H1X. In particular, these are the states H12, H14, H16, H18 and H19 familiar to the person skilled in the art. Preferably, the aluminum alloy strip or sheet has the strain hardening state H18 or H19. The aforementioned states, in particular H18 and H19, are characterized by a particularly high mechanical stability, so that a particularly high strength can be provided for the battery cell housing.
[0029] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet has a thickness between 0.1 mm and 2.0 mm. This thickness range essentially fully encompasses the typical wall thickness for a battery cell housing. Reducing the thickness below 0.1 mm reduces the mechanical stability of the battery cell housing too much. Conversely, a thickness of more than 2.0 mm no longer allows efficient use of the material. Furthermore, if the aluminum alloy strip or sheet of the battery cell housing were to have a thickness greater than 2.0 mm, the gravimetric and volumetric energy densities of the battery cell or battery module or battery system would be too low. Preferably, the thickness of the aluminum alloy strip or sheet is between 0.2 mm and 1.5 mm, in particular between 0.35 mm and 1.2 mm.
[0030] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet has an electrical conductivity σ of at least 35% IACS. Thus, compared to previously used battery cell housings made of nickel-plated steel, this electrical conductivity is significantly increased so that faster charging times, lower electrical losses and therefore less heat generation during operation of the battery cell are also achieved. Due to the Wiedemann-Franz law, which states that there is a direct relationship between the electrical and thermal conductivity of metals, the increase in electrical conductivity is further associated with an increased thermal conductivity compared to nickel-plated steel. This allows the waste heat generated during operation of the battery cell to be dissipated more efficiently. Furthermore, a higher thermal conductivity leads to a more uniform temperature distribution inside the cell, which has a positive effect on aging. Thus, an electrical conductivity σ of at least 35% IACS leads to an overall improvement in the performance of the battery cell.
[0031] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet has a yield strength R of at least 180 MPa, preferably at least 220 MPa, in particular at least 250 MPa. p0.2 This allows a high strength to be provided for the battery cell housing. Preferably, the aluminum alloy strip or sheet has the aforementioned yield strength values, for example in state H16, H18 or H19, before its processing to form the battery cell housing. Furthermore, since processing of the aluminum alloy strip or sheet, typically carried out by cold forming, for example deep drawing, is generally associated with an increase in strength, it can be assumed that the specified minimum values for yield strength apply in the same way to the battery cell housing according to the invention in the finished state.
[0032] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet has a tensile strength R of at least 190 MPa, preferably at least 230 MPa, in particular at least 260 MPa.m This also makes it possible to provide high strength for the battery cell housing. Here again, it can also be assumed that the aluminum alloy strip or sheet preferably already has the aforementioned values for tensile strength before its processing to form the battery cell housing, for example in state H16, H18 or H19, which values apply in the same way to the battery cell housing according to the invention in the finished state.
[0033] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet has a yield strength R of at least 200 MPa at a temperature of 100° C. p0.2 Simultaneously or alternatively, the aluminum alloy strip or sheet has a yield strength R of at least 150 MPa at a temperature of 200°C. p0.2 The aforementioned yield strength at 100°C or 200°C may also provide high thermal stability for the battery cell housing, since battery cells are sometimes heated to temperatures significantly higher than room temperature in the event of defects, damage or the effects of improper use. Here again, it may also be assumed that the aluminum alloy strip or sheet preferably already has the aforementioned values for yield strength at 100°C or 200°C prior to its processing to form the battery cell housing, which values apply in the same way to the battery cell housing according to the invention in the finished state.
[0034] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet, prior to its processing to form the battery cell housing, has a wall thickness ratio δ to steel of not more than 1.6, preferably not more than 1.4. The wall thickness ratio δ to steel is determined by the yield strength R of nickel-plated steel strip of type AISI 1020. p0.2、St The yield strength R of the aluminum alloy strip p0.2、Al is determined by dividing by R p0.2、Stis set to a typical value of 350 MPa. To derive the wall thickness ratio δ, the internal pressure loading scenario relevant for a real battery cell housing is considered. For simplicity, the battery cell housing is assumed to be a closed and thin-walled cylinder. On this basis, the calculation of the wall thickness ratio δ for steel is carried out using Barlow's formula σ known from elastostatics: φ =p·R i / s, where σ φ : Stress component in the circumferential direction, p: Internal pressure, R i : inner radius, s: wall thickness, and comparative stress σ by Tresca V、Tresca = σ max -σ min = σ φ -0=p·R i / s, where the design for the load is limited by the onset of flow, i.e., σ V、Tresca ≦R p0.2 This is done by using the same maximum internal pressure p=R p0.2、Al ·s Al / R i、Al =R p0.2、St ·s St / R i、St With the assumption of the same inner radius Ri of the cells, this means that R p0.2、Al ·s Al =R p0.2、St ·s Al Therefore, the wall thickness ratio δ can be calculated from the yield strength ratio given above: δ = s Al / s St =R p0.2、St / R p0.2、Al The wall thickness ratio δ to steel is a measure of the increase in the wall thickness of the battery cell housing when steel is replaced by aluminum and can in particular be used to compare various aluminum alloy strips or sheets with each other. A δ value according to the invention not greater than 1.6, preferably not greater than 1.4, has a positive effect on the volumetric energy density of the battery cell, since the volume of space occupied by the present aluminum alloy strip or sheet is thereby minimized with the same mechanical stability. Furthermore, the limited wall thickness ratio in combination with the low density of aluminum compared to steel maximizes the gravitational energy density.
[0035] In a further embodiment of the battery cell housing according to the invention, the aluminum alloy strip or sheet, prior to its processing to form the battery cell housing, has an average percentage ear height Z of not more than 4%, preferably not more than 3%, and a maximum percentage ear height Z of not more than 6%, preferably not more than 5.5%. max The earring parameters Z and Z max is determined in an earring test according to DIN EN 1669 using blanks with a diameter of 60 mm, a perforation diameter of 33 mm and the lubricant lanolin. The mean percentage ear height Z is not greater than 4%, preferably not greater than 3%, and the maximum achieved percentage ear height Z is not greater than 6%, preferably not greater than 5.5%. max This means that the aluminum alloy strip or sheet is highly suitable for deep drawing with minimal process scrap and thus for the efficient manufacture of battery cell housings according to the invention.
[0036] According to the second teaching of the present invention, the aforementioned object of the use of an aluminum alloy strip or sheet for manufacturing a battery cell housing is achieved in that the aluminum alloy strip or sheet is used to manufacture a battery cell housing according to the first teaching of the present invention. Thus, due to the aforementioned advantageous properties of the aluminum alloy strip or sheet, a battery cell housing that is improved compared to the prior art can be provided.
[0037] In one embodiment of the use according to the invention, the battery cell housing is a housing for a secondary battery, preferably a lithium-ion or sodium-ion secondary battery. Since secondary batteries, especially lithium-ion secondary batteries, are currently being increasingly used in the field of electric mobility and consumer electronics, the advantageous properties of the aluminum alloy strip or sheet used according to the invention can be used in particular for this type of battery cell. This also applies to sodium-ion secondary batteries, which are currently still the subject of research and may in the future replace lithium-ion secondary batteries in certain applications due to the better economics and good availability of sodium. The use of the battery cell housing according to the invention further includes the use of this housing for solid-state secondary batteries, especially with solid-state electrolyte.
[0038] In a further embodiment of the use according to the invention, the battery cell housing has a cylindrical, prismatic or pouch design. Thus, the advantageous properties of the aluminum alloy strip or sheet used according to the invention can be used in all currently common designs for battery cell housings.
[0039] In a further embodiment of the use according to the invention, the aluminium alloy strip or sheet has - casting a rolling ingot from the aluminium alloy; - homogenizing the rolled ingot; - hot rolling the rolled ingot to form a hot rolled strip; - cold rolling the hot rolled strip; The present invention is produced by a method comprising the steps of:
[0040] The aforementioned process steps are preferably carried out in the specified order, in which case homogenization of the rolled ingot can be carried out separately or integrated into the preheating of the rolled ingot for hot rolling. It has been found that using the method described above it is possible to produce an aluminum alloy strip or sheet which, when used according to the invention, is able to meet the requirements of the battery cell housing, especially with regard to strength, electrolyte stability and electrical and thermal conductivity, while at the same time achieving a high recycling rate. Moreover, this process allows for economical production of this aluminum alloy strip or sheet.
[0041] The casting of rolled ingots from the aluminum alloy is preferably carried out in direct chill continuous casting, also called DC continuous casting, so that the economic viability of the production process can be further increased.
[0042] By homogenizing the rolled ingot, an improvement in the microstructure of the aluminum alloy strip or sheet is achieved, which has a positive effect on the strength and formability. Preferably, homogenization is carried out at a temperature between 480°C and 620°C, in particular between 550°C and 610°C, for a duration of at least 0.5 hours, preferably at least 1 hour, in particular at least 2 hours.
[0043] Hot rolling of the rolled ingot to form the hot rolled strip is preferably carried out at a temperature between 280°C and 550°C, the hot strip temperature after the last hot rolling pass being between 280°C and 380°C, preferably between 310°C and 360°C. Hot rolling of the rolled ingot can be carried out either in reverse direction in one roll stand or in forward direction in tandem stands. In particular, hot rolling can be carried out in reverse direction up to a slab thickness between 20mm and 50mm and then the slab can be rolled up to the hot strip thickness in tandem stands. The hot strip thickness, i.e. the thickness of the hot rolled strip, is in one embodiment of the method between 1mm and 15mm, preferably between 2mm and 12mm, in particular between 2mm and 9mm. This ensures that a sufficiently high reduction ratio can be adjusted during the subsequent cold rolling, which determines both the strength and formability of the aluminium alloy strip or sheet as well as the crystallographic structure and thus the ear profile.
[0044] The cold rolling of the aluminum alloy strip or sheet may be carried out in one or more passes. In an embodiment of the method in which several cold rolling passes are carried out, at least one intermediate anneal is optionally carried out during cold rolling. In one embodiment of the method, the intermediate anneal is carried out in the temperature range between 150°C and 450°C, preferably between 200°C and 400°C, in particular between 300°C and 400°C. Preferably, the intermediate anneal is carried out as a recrystallization anneal, in which a recrystallized microstructure is provided for the subsequent cold rolling pass. This cold rolling pass may then be carried out at a higher reduction ratio, which has a strength-enhancing effect on the finished rolled aluminum alloy strip or sheet. However, as an alternative, a recovery anneal, which results in reduced hardening, may be carried out instead of the recrystallization anneal.
[0045] In one embodiment of the method, the reduction ratio during cold rolling at the final thickness is at least 20%, preferably at least 50%, in particular at least 70%. If the method is carried out with an intermediate anneal during cold rolling, the reduction ratio during cold rolling at the final thickness after the last intermediate anneal is at least 20%, preferably at least 50%, in particular at least 70%. Due to a reduction ratio during cold rolling at the final thickness of at least 20%, preferably at least 50%, in particular at least 70%, the strength of the produced aluminum alloy strip or sheet can be increased so as to be particularly suitable for use according to the invention. Due to the high reduction ratio, earrings occur at the 45° position. Nevertheless, earrings can be compensated for by choosing the hot rolling parameters such that a recrystallized hot strip is produced. In that case, the recrystallized hot strip has earrings at the 0° / 90° position, and thus the earrings at the 45° position can be compensated for. Thereby, the average percentage ear height Z and the maximum percentage ear height Z max may be limited, which has a positive effect on productivity in the deep drawing process and reduces the amount of scrap generated in the deep drawing process.
[0046] The invention is explained in more detail below using exemplary embodiments and reference is also made to the drawings. [Brief description of the drawings]
[0047] [Figure 1] FIG. 2 shows a schematic diagram of a cylindrical design battery cell having a battery cell housing according to the present invention. [Diagram 2] FIG. 2 shows a schematic diagram of a prismatic design battery cell having a battery cell housing according to the present invention. [Diagram 3] FIG. 1 shows a schematic diagram of a pouch design battery cell having a battery cell housing according to the present invention. [Figure 4] 1 shows a flow diagram of a method for producing an aluminium alloy strip or sheet for use according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0048] 1 shows in a schematic diagram a cylindrical design battery cell 10. The battery cell 10 includes a battery cell housing 11 according to the present invention and adjacent thereto an anode terminal 12 and a cathode terminal 13.
[0049] 2 shows in a schematic diagram a battery cell 20 of prismatic design. The battery cell 20 includes a battery cell housing 21 according to the present invention and adjacent thereto an anode terminal 22 and a cathode terminal 23.
[0050] 3 shows in a schematic diagram a pouch design battery cell 30. The battery cell 30 includes a battery cell housing 31 according to the present invention and adjacent thereto an anode terminal 32 and a cathode terminal 33.
[0051] 4 shows a flow diagram of a method 40 for producing an aluminum alloy strip or sheet for use in accordance with the present invention. The method 40 comprises the steps of: - step 42 of casting a rolling ingot from the aluminum alloy; - homogenizing the rolled ingot 44; - hot rolling 46 the rolled ingot to form a hot rolled strip; - cold rolling 48 the hot rolled strip; Includes.
[0052] Within the scope of the present invention, a total of seven aluminum alloy strips, hereinafter referred to as strips 1 to 7, were produced from various aluminum alloys. The alloy composition of each of strips 1 to 7 is summarized in table 1 below. The contents of the individual alloying elements are specified in weight percent. The remainder, i.e. the difference from 100 weight percent, consists of aluminum and unavoidable impurities, each of which amounts to at most 0.05 weight percent and in total to at most 0.15 weight percent. Strips 1, 2, 3, 7 are exemplary embodiments according to the invention with an alloy composition corresponding to the invention, which is identical for strip 1 and strip 2. Conversely, strips 4, 5, 6 are comparative examples with an aluminum alloy of type AA3003.
[0053] [Table 1]
[0054] Aluminum alloy strips 1 to 7 were inspected according to the method shown in FIG. 4. In particular, rolled ingots were cast from the respective aluminum alloys in a DC continuous caster. To produce the rolled ingots of strips 1, 2, 3, 7 according to the invention, a proportion of recycled material of at least 70% by weight was selected. A maximum recycling rate of 30% by weight was achieved in comparative examples 4, 5, 6. After casting, the rolled ingots were homogenized and then hot rolled to form hot rolled strips. The hot rolled strips were then strain rolled respectively to a final thickness between 0.5 mm and 1.0 mm. The following table 2 shows the various process parameters for the manufacture of strips 1 to 7. In particular, these are the hot strip thickness, i.e. the respective thickness of the hot rolled strip, the parameters of the optional intermediate annealing during cold rolling, temperature, duration and strip thickness, as well as the rolling ratio during cold rolling at the final thickness.
[0055] [Table 2]
[0056] As can be seen from table 2, strips 1 to 3 according to the invention were produced without an intermediate anneal, whereas strip 7 according to the invention as well as comparative strips 4 to 6 were produced with an intermediate anneal, in particular a recrystallization anneal. In the case of strip 2, a final anneal was carried out after cold rolling at a temperature of 250° C. with a holding time of 2 hours.
[0057] The aluminum alloy strips were then examined for various properties related to battery cell housings. The results of these examinations are summarized in Table 3 below. In detail, Table 3 shows the material state, thickness d as the final thickness after cold rolling, electrical conductivity σ, yield strength R of strips 1 to 7. p0.2 , tensile strength R m , wall thickness ratio δ to steel, average percentage ear height Z and maximum percentage ear height Z max The yield strength R p0.2 and tensile strength R m was determined in a tensile test according to DIN EN ISO 6892-1. The wall thickness ratio δ of the steel to the wall thickness is based on a yield strength R of 350 MPa, which is a typical value for nickel-plated steel strip of type AISI 1020. p0.2、St The yield strength R of each of the aluminum alloy strips 1 to 7 is p0.2、Al The mean percentile ear height Z and the maximum percentile ear height Z were determined by dividing by max was determined in an earring test according to DIN EN 1669 using a blank with a diameter of 60 mm, a perforation diameter of 33 mm and the lubricant lanolin.
[0058] [Table 3]
[0059] As table 3 shows, higher yield and tensile strengths can be achieved with strips 1, 2, 3, 7 according to the invention than with comparative strips 4, 5, 6 made of aluminium alloy AA3003. The strain hardening state of type H1X, in particular state H18 or H19, has a more positive effect on the strength as shown by the comparison between strips 1, 2, 3, 7 according to the invention. Thus, the yield and tensile strengths of strip 2, which has the same alloy composition as strip 1 (see table 1) but is strain hardened and annealed in state H24, are higher than those of comparative strips 3, 4, 5, but lower than strip 1 in only strain hardened state H18.
[0060] As Table 3 further shows, strips 1, 2, 3, 7 according to the invention have a yield strength R of at least 180 MPa. p0.2 and a tensile strength R of at least 190 MPa m They are therefore particularly suitable for use in the manufacture of battery cell housings according to the invention. The yield strength and tensile strength values given in Table 3 apply to strips 1, 2, 3, 7 before processing to form a battery cell housing, but it can be assumed that battery cell housings manufactured from strips 1, 2, 3, 7 have at least equally high values in the finished state. This is due to the fact that processing, typically performed by cold forming, for example deep drawing, is generally accompanied by an increase in strength.
[0061] In addition to the yield strengths contained in table 3, which refer to room temperature, the yield strengths at 100 ° C and at 200 ° C were also determined according to DIN EN ISO 6892-2 for the strip 3 according to the invention as well as for the comparative strip 4. The strip 3 according to the invention reached a value of 270 MPa at 100 ° C and a value of 161 MPa at 200 ° C. The comparative strip 4 reached a value of 151 MPa at 100 ° C and a value of 92 MPa at 200 ° C. The strip 3 according to the invention is particularly suitable for use in the manufacture of battery cell housings according to the invention due to its significantly higher thermal stability compared to the comparative strip 4, since in the event of defects, damage or the effects of improper use, the battery cell heats up, sometimes to temperatures significantly higher than room temperature. The aforementioned values of the yield strengths at 100 ° C and 200 ° C apply to the strip 3 before it is processed to form the battery cell housing, but here too it can be assumed that the battery cell housing manufactured from the strip 3 has at least equally high values in the finished state.
[0062] As Table 3 further shows, the strips 1, 3, 7 according to the invention have a wall thickness ratio δ to steel not higher than 1.6. In the case of the inventive use of the aforementioned strips for manufacturing battery cell housings, this value has a positive effect on the volumetric and gravimetric energy density of the finished battery cell, since the volume of space occupied by the aluminum alloy strip and the weight of the battery cell are thereby minimized with the same mechanical stability. Thus, the strips 1, 3, 7 according to the invention are particularly suitable for use in the manufacture of battery cell housings according to the invention.
[0063] As Table 3 further shows, strips 1, 2, and 3 according to the invention have an average percentage ear height Z of not more than 4% and a maximum percentage ear height Z of not more than 6%. max For this reason, they are highly suitable for deep drawing and therefore for producing the battery cell housing according to the invention with minimal scrap generation. maxThe values are comparable or slightly better than those of comparative strips 4, 5 and 6.
[0064] As Table 3 further shows, the strips 1, 2, 3, 7 according to the invention have an electrical conductivity σ of at least 35% IACS. The electrical conductivity is therefore significantly increased in such a way that faster charging times, lower electrical losses and therefore less heat generation during the operation of the battery cell are achieved compared to the battery cell housings used up to now made of nickel-plated steel. Although the electrical conductivity σ of the strips 1, 2, 3, 7 according to the invention is slightly inferior to that of the comparative strips 4, 5, 6, it still easily meets the requirements of the battery cell housing. Similar considerations apply to the thermal conductivity, due to the Wiedemann-Franz law, which states that there is a direct relationship between electrical conductivity and thermal conductivity in metals. The improved thermal conductivity of the aluminum alloy strips according to the invention compared to nickel-plated steel allows a significantly more efficient cooling of the battery cell, especially at the high C-rates that occur during fast charging, as well as a more uniform temperature distribution on the package, which limits the aging of the battery cell.
[0065] As Table 3 further shows, the strips 1, 2, 3, 7 according to the invention have a thickness between 0.1 mm and 2.0 mm. Thus, a good compromise between mechanical stability and efficient use of the material is achieved when used to manufacture the battery cell housing according to the invention. Moreover, the weight and volumetric energy density of the corresponding battery cell or battery module or battery system are not significantly reduced.
[0066] The corrosion behavior of the strip 3 according to the invention and the comparative strip 4 was evaluated by cyclic polarization measurements according to DIN 50918:2018-09 with lithium hexafluorophosphate electrolyte. First the rest potential of the degreased strip in this electrolyte was measured and then the following polarization: 1. Polarization of the resting potential to 600 mV at 1 mV / s in the cathodic direction; 2. 1mA / cm at 1mV / s from the cathode region to the anode 2 Polarization to a potential corresponding to a corrosion current of 3. Reverse polarization at 1 mV / s back towards the cathode was carried out.
[0067] From the evaluation of these measurements the parameters shown in Table 4 below were obtained for the characterization of the corrosion behavior. In particular, Table 4 shows the cathodic current density, exchange current density and polarization resistance. As the table shows, the strip 3 according to the invention and the comparative strip 4 have practically the same cathodic current density, exchange current density and polarization resistance, so that the strip 3 according to the invention meets the requirements for electrolyte stability in the same way as the reference strip 4, which has an alloy-state combination typical of prior art prismatic battery cell housings.
[0068] [Table 4]
[0069] Since the electrolyte stability is essentially determined by the chemical composition, which is very similar for the strips 1, 2, 3, 7 according to the invention on the one hand and the comparative strips 4, 5, 6 on the other hand, the cyclic polarization measurements according to DIN 50918:2018-09 show that, overall, the electrolyte stability for the strips 1, 2, 3, 7 according to the invention is essentially the same as that for the comparative strips 4, 5, 6 made of aluminium alloy AA3003. The strips according to the invention therefore fulfill the requirements for electrolyte stability in the same way and are therefore suitable for use in the manufacture of battery cell housings according to the invention.
[0070] Due to the advantageous properties of the strips 1, 2, 3, 7 according to the invention, which have just been described in detail, in particular the strips 1, 3, they are particularly suitable for the use according to the invention for producing a battery cell housing. In this way it is possible to produce the battery cell housing according to the invention shown by way of example in figures 1 to 3.
[0071] The battery cells (10, 20, 30) shown in Figures 1 to 3 may be secondary batteries, in particular lithium-ion secondary batteries or sodium-ion secondary batteries, and therefore the battery cell housings (11, 21, 31) according to the present invention are housings for secondary batteries, in particular lithium-ion secondary batteries or sodium-ion secondary batteries, respectively. Therefore, the advantageous properties of the aluminum alloy strip used according to the present invention may be used in particular for these types of battery cells.
[0072] Furthermore, the battery cell housing (11, 21, 31) according to the invention shown in Figures 1 to 3 may in particular have a cylindrical, prismatic or pouch design. Figure 1 shows the battery cell housing (11) according to the invention in a cylindrical design, Figure 2 shows the battery cell housing (21) according to the invention in a prismatic design and Figure 3 shows the battery cell housing (31) according to the invention in a pouch design. Thus, the advantageous properties of the aluminum alloy strip used according to the invention can be used in all currently typical designs of battery cell housings.
[0073] Furthermore, the aluminum alloy on which the battery cell casing (11, 21, 31) according to the invention shown in Figures 1 to 3 is based preferably has a proportion of recycled material of at least 50% by weight, preferably at least 70% by weight. This recycling rate is preferably achieved by using post-consumer scrap. The associated energy savings allow the production of the battery cell casing with the lowest possible CO2 footprint, increasing the sustainability of the battery cell casing. This is possible since the battery cell casings (11, 21, 31) according to the invention are highly suitable for achieving high recycling rates due to their alloy composition. Additionally or alternatively, this recycling rate can also be achieved by using internal or external process scrap, with a corresponding reduction in the CO2 footprint being achieved compared to production relying on primary aluminum.
Claims
1. A battery cell housing (11, 21, 31) having an aluminum alloy strip or sheet, The aluminum alloy strip or sheet has the following components in weight percent: 0.1%≦Si≦0.5%, 0.25%≦Fe≦0.8%, Cu≦0.6%, 0.6%≦Mn≦1.4%, 0.5%≦Mg≦1.5%, Cr≦0.25%, Zn≦0.4%, Ti≦0.2%, the balance being Al, and alloying components being at most 0.05% individually and at most 0.15% in total of unavoidable impurities; A battery cell housing (11, 21, 31).
2. The aluminum alloy strip or sheet has the following components in weight percent: 0.2%≦Si≦0.4%, preferably 0.2%≦Si≦0.35%, 0.3%≦Fe≦0.7%, preferably 0.4%≦Fe≦0.7%, Cu≦0.3%, preferably 0.1%≦Cu≦0.2%, 0.8%≦Mn≦1.1%, 0.8%≦Mg≦1.5%, preferably 0.8%≦Mg≦1.2%, Cr≦0.1%, preferably Cr≦0.05%, 0.02%≦Zn≦0.25%, preferably 0.04%≦Zn≦0.25%, 0.005%≦Ti≦0.1%, preferably 0.005%≦Ti≦0.05%, the balance being Al, and alloying components being at most 0.05% individually and at most 0.15% in total of unavoidable impurities; The battery cell housing of claim 1 .
3. 3. A battery cell housing according to claim 1 or 2, characterized in that the aluminium alloy has a proportion of recycled material of at least 50% by weight, preferably at least 70% by weight.
4. 4. The battery cell housing according to claim 1, wherein the aluminum alloy strip or sheet has a strain hardening condition of type H1X, preferably a strain hardening condition H18 or H19.
5. 5. The battery cell housing according to claim 1 , wherein the aluminum alloy strip or sheet has a thickness between 0.1 mm and 2.0 mm, preferably between 0.2 mm and 1.5 mm, particularly preferably between 0.35 mm and 1.2 mm.
6. 6. The battery cell housing according to claim 1, wherein the aluminum alloy strip or sheet has an electrical conductivity σ of at least 35% IACS.
7. The aluminum alloy strip or sheet preferably has a yield strength R of at least 180 MPa, preferably at least 220 MPa, particularly preferably at least 250 MPa, prior to its treatment to form the battery cell housing. p0.2 The battery cell housing according to any one of claims 1 to 6, characterized in that it comprises:
8. The aluminum alloy strip or sheet has a yield strength R of at least 200 MPa at a temperature of 100° C. p0.2 and / or a yield strength R of at least 150 MPa at a temperature of 200° C. p0.2 The battery cell housing according to any one of claims 1 to 7, characterized in that it comprises:
9. 9. The battery cell housing according to claim 1 , characterized in that the aluminum alloy strip or sheet has a wall thickness ratio δ to steel, prior to its treatment to form the battery cell housing, of not more than 1.6, preferably not more than 1.
4.
10. The aluminum alloy strip or sheet, prior to its processing to form the battery cell housing, has an average percentage ear height Z of not more than 4%, preferably not more than 3%, and preferably a maximum percentage ear height Z of not more than 6%, preferably not more than 5.5%, in an earring test according to DIN EN 1669. max The battery cell housing according to any one of claims 1 to 9, characterized in that it comprises:
11. Use of an aluminium alloy strip or sheet for manufacturing a battery cell housing according to any one of claims 1 to 10.
12. 12. Use according to claim 11, characterised in that the battery cell housing is the housing of a secondary battery, preferably a lithium-ion secondary battery, a sodium-ion secondary battery or a solid-state secondary battery.
13. 13. Use according to claim 11 or 12, characterized in that the battery cell housing has a cylindrical, prismatic or pouch design.
14. The aluminum alloy strip or sheet has the following properties: - casting (42) a rolling ingot from the aluminium alloy; - homogenizing the rolled ingot (44); - hot rolling (46) said rolled ingot to form a hot rolled strip; - cold rolling (48) said hot rolled strip, Use according to any one of claims 11 to 13, characterized in that it is produced by a process (40) comprising:
15. Use according to claim 14, characterised in that the thickness of the hot-rolled strip is between 1 mm and 15 mm, preferably between 2 mm and 12 mm, particularly preferably between 2 mm and 9 mm.
16. 16. Use according to claim 14 or 15, characterised in that during the cold rolling at least one intermediate annealing is carried out.
17. Use according to any one of claims 14 to 16, characterised in that the reduction ratio during the cold rolling to final gauge, preferably after the last intermediate annealing, is at least 20%, preferably at least 50%, particularly preferably at least 70%.
Citation Information
Patent Citations
Secondary battery having aluminum external can
JP1996329908A
Al-Mn-Mg ALLOY PLATE FOR FORMING CASE, AND ITS MANUFACTURING METHOD
JP2001131666A
Aluminum alloy plate for battery case and manufacturing method therefor
JP2002157978A
Aluminum alloy plate for rectangular cross-section battery container and aluminum alloy plate rectangular cross-section battery container
JP2007305597A
Aluminum alloy sheet superior in heat resistance, manufacturing method therefor, aluminum alloy sheet superior in heat resistance and deep drawability, and manufacturing method therefor
JP2009019223A