Process for preparing copolymers of (meth)acrylic acid and cyclic ketene acetals

A novel method for preparing biodegradable copolymers of cyclic ketene acetal and (meth)acrylic acid addresses the inefficacy of previous methods by ensuring biodegradability and functionality as dispersants and scale inhibitors through controlled polymerization and deprotection.

JP2024539926APending Publication Date: 2024-10-31ROHM & HAAS CO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024524395
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-04
Filing Date
2022-11-01
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for preparing biodegradable polyacrylic acid (PAA) copolymers, such as those disclosed by Bailey and Guo, fail to produce detectable amounts of biodegradable MDO-AA copolymers, rendering them ineffective as dispersants and scale inhibitors.

Method used

A method involving gradual addition of a cyclic ketene acetal monomer and t-butyl (meth)acrylate to a reaction vessel with an initiator in an organic solvent, followed by heating and deprotection to form a copolymer of cyclic ketene acetal monomer and (meth)acrylic acid, with a specific molar ratio and deprotection conditions, ensuring biodegradability and effectiveness.

Benefits of technology

The process yields copolymers that are biodegradable and function effectively as dispersants and scale inhibitors, confirmed by NMR spectroscopy and molecular weight analysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539926000001
    Figure 2024539926000001
  • Figure 2024539926000002
    Figure 2024539926000002
  • Figure 2024539926000003
    Figure 2024539926000003
Patent Text Reader

Abstract

The present invention relates to a method for preparing copolymers containing structural units of acrylic acid and cyclic ketene acetal monomers, which copolymers are useful as biodegradable dispersants.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION The present invention relates to a method for preparing copolymers of (meth)acrylic acid and cyclic ketene acetals, more specifically aqueous solutions of acrylic acid and 2-methylene-1,3-dioxepane (MDO). [Background technology]

[0002] Low molecular weight (MW) polyacrylic acid (PAA) is widely used as a dispersant and antiscalant in the home care and oil and gas industries. In these applications, PAA typically enters municipal wastewater treatment plants or is at least partially released into the environment after use. Increasing scrutiny from governments, regulatory agencies, companies, and consumers regarding the fate of polymers in the environment has created a need to find new biodegradable materials. Previous studies have established that PAA is difficult to biodegrade, due in part to the inert nature of its carbon-carbon backbone. On the other hand, PAA oligomers with molecular weights below 1000 g / mol are susceptible to biodegradation. (Kawai, F., Bacterial Degradation of Acrylic Oligomers and Polymers, Applied Microbiology and Biotechnology 1993, 39(3), 382-385; Hayashi, T.; Mukouyama, M.; Sakano, K.; Tani, Y., Degradation of a Sodium Acrylate Oligomer by an Arthrobacter sp. Appl Environ Microbiol 1993,59(5),1555-9;Larson,RJ;Bookland,EA;Williams,RT;Yocom,KM;Saucy,DA;Freeman,MB;Swift,G., Biodegradation of Acrylic Acid Polymers and Oligomers by Mixed Microbial Communities in Activated Sludge,Journal of environmental polymer degradation 1997, 5(1), 41-48). Nevertheless, these biodegradable oligomers are unsuitable as dispersants and scale inhibitors.Strategies for incorporating labile bonds into PAA polymers have been reported.For example, US Patent No. 4,923,941 (Bailey) discloses an aqueous preparation of biodegradable MDO-AA copolymer by reacting sodium acrylate with MDO in water containing tetrabutylammonium bromide. Similarly, Guo et al. (Guo) report the preparation of MDO-AA copolymer by reacting incompletely neutralized acrylic acid with MDO in water also containing tetrabutylammonium bromide (Acta Polymerica Sinica 2012, 12, 958-964). Bailey claims that evidence of copolymer formation can be confirmed by the "presence of ester bonds in the copolymer chain." Similarly, Guo assigns the triplet peak at δ=4.00 ppm in the disclosed proton NMR spectrum of the polymer product to the methylene protons associated with the MDO structural unit. However, despite the assertions of Bailey and Guo, the present inventors have confirmed that no detectable amount of MDO-AA copolymer can be formed by the similar methods disclosed by Bailey and Guo et al.

[0003] Thus, there remains a need in the art of biodegradable dispersants to find methods of preparing PAAs that are biodegradable yet remain effective as dispersants and scale inhibitors. Summary of the Invention

[0004] The present invention relates to a method for preparing a copolymer comprising structural units of a cyclic ketene monomer and (meth)acrylic acid, comprising the steps of: a) gradually adding a cyclic ketene acetal monomer and t-butyl (meth)acrylate to a reaction vessel in the presence of an organic solvent and simultaneously and separately gradually adding an initiator to the reaction vessel; heating the contents of the reaction vessel to a temperature sufficient to promote polymerization of the cyclic ketene acetal monomer and the t-butyl (meth)acrylate to provide a solution of a copolymer of the cyclic ketene acetal monomer and the t-butyl (meth)acrylate; and b) contacting the copolymer of the cyclic ketene acetal monomer and the t-butyl (meth)acrylate with a deprotecting agent to form a copolymer of the cyclic ketene acetal monomer and (meth)acrylic acid; Including, a molar:molar ratio of the t-butyl (meth)acrylate to the cyclic ketene acetal monomer in the first portion and the second portion ranges from 2:1 to 15:1; The cyclic ketene acetal monomer has the following structure:

[0005] [ka] (Wherein, n is 0, 1, or 2; R is H or C 1 -C 6 -alkyl, R 1 and R 2 are independently H, C 1 -C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 -C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently H or C 1 -C 12 -alkyl or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, if n is 1, R 3 and R 3’ are independently H, C 1 -C 12 -alkyl, phenyl, or R 3 and R 3’forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, if n is 2, Each R 3 are independently H, C 1 -C 12 -alkyl or, together with the carbon atom to which they are attached, an internal double bond, a fused benzene ring, or a fused C 3 -C 7 -Forms an alicyclic ring) The present invention addresses the need in the art by providing a method, comprising:

[0006] The process of the present invention provides copolymers of acrylic acid that are biodegradable yet effective as dispersing agents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention relates to a method for preparing a copolymer comprising structural units of a cyclic ketene monomer and (meth)acrylic acid, comprising the steps of: a) gradually adding a cyclic ketene acetal monomer and t-butyl (meth)acrylate to a reaction vessel in the presence of an organic solvent and simultaneously and separately gradually adding an initiator to the reaction vessel; heating the contents of the reaction vessel to a temperature sufficient to promote polymerization of the cyclic ketene acetal monomer and the t-(meth)butyl acrylate to provide a solution of a copolymer of the cyclic ketene acetal monomer and the t-(meth)butyl acrylate; and b) contacting the copolymer of the cyclic ketene acetal monomer and the t-(meth)butyl acrylate with a deprotecting agent to form a copolymer of the cyclic ketene acetal monomer and (meth)acrylic acid; Including, a molar:molar ratio of the t-butyl (meth)acrylate to the cyclic ketene acetal monomer in the first and second portions is in the range of 2:1 to 15:1; The cyclic ketene acetal monomer has the following structure:

[0008] [ka] (In the formula, n is 0, 1, or 2, R is H or C 1 -C 6 -alkyl, R 1 and R 2 are independently H, C 1 -C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 -C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently hydrogen or C 1 -C 12 -alkyl or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, if n is 1, R 3 and R 3’ are independently H, C 1 -C 12 -alkyl, phenyl, or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, if n is 2, Each R 3 are independently H, C1-C12-alkyl, or together with the carbon atom to which they are attached form an internal double bond, a fused benzene ring, or a fused C 3 -C 7 -Forms an alicyclic ring) The present invention addresses the need in the art by providing a method, comprising:

[0009] As used herein, the term "structural unit of (meth)acrylic acid" refers to the following repeating unit: 4 is H or CH 3 , preferably H)

[0010] [ka] or a salt thereof.

[0011] The term "cyclic ketene acetal monomer structural unit" refers to the following repeating unit:

[0012] [ka] Structural unit of cyclic ketene acetal monomer (In the formula, R, R 1 , R 2 , R 3 , R 1’ , R 2’ , R 3’ , and n is as previously defined).

[0013] Examples of cyclic ketene acetal monomers include:

[0014] [ka] A preferred cyclic ketene acetal monomer is 2-methylene-1,3-dioxepane (MDO).

[0015] [ka]

[0016] The copolymer of cyclic ketene acetal monomer and acrylic acid is prepared in multiple steps. In a first step, a mixture of cyclic ketene acetal monomer and t-butyl (meth)acrylate, preferably t-butyl acrylate, is gradually added from a monomer container (monomer container) to a reaction vessel in the presence of an organic solvent. At the same time, an initiator, advantageously diluted with the same organic solvent as used for the monomer, is gradually added from an initiator container (initiator container) to the reaction vessel. It may be desirable to gradually add the monomer and initiator mixture to a reaction vessel containing a solvent and a small amount of monomer (typically on the order of 10-30 weight percent of the total monomer used to prepare the copolymer).

[0017] Suitable organic solvents include aliphatic esters such as ethyl acetate, ethers such as tetrahydrofuran and 1,4-dioxane, alkanes such as pentane, hexane, and isododecane, and aromatic solvents such as benzene, toluene, and xylene. Examples of suitable initiators include t-amyl peroxypivalate (commercially available as Trigonox 125-C75 initiator), t-butyl peroxypivalate (commercially available as Trigonox 25-C75), t-amyl peroxy-2-ethylhexanoate, 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate).

[0018] A chain transfer agent such as n-dodecyl mercaptan may also be added simultaneously with the monomers and initiator to control the molecular weight of the intermediate and final copolymers.

[0019] The contents of the reaction vessel are heated to a temperature sufficient to promote copolymerization of the cyclic ketene acetal monomer and t-butyl (meth)acrylate, generally in the range of from 40° C., or from 50° C. to 150° C., or to 100° C., or to 80° C., to provide a solution of an intermediate copolymer of the cyclic ketene acetal monomer and t-butyl (meth)acrylate.

[0020] In a second step, the intermediate copolymer is reacted under deprotection conditions to convert the t-butyl pendant groups of the copolymer to carboxylic acid groups or salts thereof, thereby forming a solution of a copolymer of cyclic ketene acetal monomer and (meth)acrylic acid, preferably acrylic acid or a salt thereof. The deprotection conditions preferably convert the intermediate copolymer to a pK ranging from -2 or -1 to 2 or 1. a The deprotection step includes contacting the cyclic ketene acetal monomer with an organic acid having a formula: embedded image Examples of suitable acids for deprotection include trifluoroacetic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, and methanesulfonic acid. The organic solution of the copolymer of the cyclic ketene acetal monomer and acrylic acid can then be converted to an aqueous solution of the copolymer of the cyclic ketene acetal monomer and acrylic acid by conventional means, such as removing the solvent in vacuum followed by dissolving in water, or removing the solvent in vacuum followed by dissolving in water, lyophilizing, and then redissolving in water.

[0021] When the cyclic ketene acetal monomer is MDO, the MDO-AA copolymer is found to contain two types of structural units of MDO, one of which is degradable by treatment with base and the other of which is not readily degradable by treatment with base, as described.

[0022] [ka]

[0023] For the copolymers to be useful for the purposes of this invention, they must contain degradable structural units, cyclic ketene acetal monomers; although the formation of non-degradable structural units is undesirable, it has proven difficult to prepare copolymers without some residual concentration of the non-degradable forms.

[0024] The molar to molar ratio of (meth)acrylic acid structural units to the total structural units of cyclic ketene acetal monomers (both degradable and non-degradable), preferably MDO, ranges from 2:1, or 3:1, or 4:1, to 15:1, or 10:1, or 8:1, or 7:1. Preferably, the M of the desired copolymer is n ranges from 1500 g / mole to 20000, or 15000, or 10,000 g / mole. Statistically, the polymer backbone is expected to contain 2 to 15 structural units of (meth)acrylic acid (preferably fragments of acrylic acid groups) anchored at each end by a single degradable structural unit of a cyclic ketene acetal monomer, as illustrated:

[0025] [ka] (In the formula, R 4 is H or CH 3 , preferably H, x ranges from 2, or 3, or 4 to 15, or 10, or 8, or 7, and the dotted line represents the attachment of a structural unit of MDO to another fragment of the acrylic acid group).

[0026] In accelerated aging studies, the ester groups are hydrolyzed with a strong base such as KOH to give a distribution of oligomers, including, in part, an oligomer predicted to have the following structure:

[0027] [ka]

[0028] The presence of non-degradable structural units of cyclic ketene acetal monomers is predicted to form copolymers that are hydrolyzable to the following oligomers:

[0029] [ka]

[0030] Although the exact structure of the oligomers can be deduced, the number average molecular weight (M) of the hydrolyzed copolymers as determined by gel permeation chromatography according to the method detailed in the Examples section. n ) can be identified with greater confidence as being in the range of 144, or 200, or 400, or 500 g / mol to 1000, or 800, or 750 g / mol.

[0031] The compositions of the present invention are ostensibly disclosed in U.S. Pat. No. 4,923,941 (Bailey), however, repeating the procedure and proton NMR spectroscopy of Bailey's only example demonstrates that Bailey's interpretation of the data is incorrect and, in fact, the disclosed example does not permit the preparation of copolymers of MDO and AA.

[0032] Bailey's example was repeated as described and the proton NMR spectrum of the reaction mixture of sodium acrylate and MDO was recorded after 30 minutes of reaction at 90° C. Triplets were observed at 4.02 ppm and 3.52 ppm, consistent with 4-hydroxybutyl acetate, the hydrolysis product of MDO.

[0033] [ka]

[0034] A small triplet at the same resonance was also observed in the proton NMR spectrum of the isolated product. Diffusion-edited proton NMR spectroscopy, which suppresses the chemical shifts of small molecules and reveals only those associated with the polymer, confirmed that these residual peaks could not be attributed to ester formation of the copolymer. Importantly, no chemical shifts were observed near 4 ppm, confirming that Bailey was unable to form detectable levels of copolymers of AA and MDO by the method disclosed. Moreover, proton NMR spectroscopy further confirmed that MDO was hydrolyzed to 4-hydroxybutyl acetate (among other by-products) under the initial reaction conditions reported by Bailey at room temperature.

[0035] Similarly, in Acta Polymerica Sinica 2012,12,958-964, Guo claims to have prepared MDO-AA copolymers by reacting incompletely neutralized acrylic acid with MDO in water containing tetrabutylammonium bromide. Guo's method was repeated as described, and additional experiments were performed using acrylic acid at various degrees of neutralization. The method described by Guo could not be reproduced to obtain proton NMR spectroscopy patterns consistent with those reported by Guo. In contrast, NMR spectroscopy did not show detectable amounts of MDO-AA copolymers. Proton NMR and diffusion NMR spectroscopy did not indicate the formation of structural units of MDO (as concluded by Guo), but rather revealed a small, sharp triplet resonance at 4.0 ppm characteristic of MDO hydrolysis products such as 4-hydroxybutyl acetate.

[0036] In contrast, copolymers prepared by the process of the present invention and analyzed by diffusion-edited proton NMR spectroscopy reveal a strong and broad chemical shift near 4 ppm, consistent with the expected profile for copolymers containing structural units of cyclic ketene acetal monomers. The compositions prepared by the process of the present invention are useful as biodegradable dispersants and scale inhibitors. EXAMPLES

[0037] M n Decision Aqueous samples for gel permeation chromatography (GPC) were prepared at a concentration of approximately 2 mg / mL in aqueous 20 mM phosphate buffer at pH 7. Separation was performed on a Waters UPLC system equipped with a refractive index detector, using the same phosphate buffer as the mobile phase. An APC column set consisting of a TOSOH Bioscience TSKgel G2500PWxl 7.8 mm ID x 30 cm, 7 μm column and a TOSOH Bioscience TSKgel GMPWxl 7.8 mm ID x 30 cm, 13 μm column was used. The flow rate was maintained at 1.0 mL / min and the column temperature was maintained at 35 °C. Peak molecular weights (M) of 216 g / mol to 1,100,000 g / mol were obtained. p The results were calibrated using narrow pAA standards and fitted to a quadratic calibration curve. Standards 1–15 were obtained from American Polymer Standards, and standard 16 (M p The peak molecular weights (M = 216 AA trimer) were prepared in-house. The flow rate was 1.0 mL / min and the column temperature was maintained at 35 °C. p The results were calibrated using narrow pAA standards of 0.01 and fitted to a quadratic calibration curve. The M of the copolymers in the examples was calculated using Empower Version 3 software (Waters Corporation). n was calculated.

[0038] A GPC calibration table showing the retention times of the 16 standards is shown in Table 1.

[0039] [Table 1]

[0040] Proton NMR spectrum analysis Proton NMR spectra were obtained using a Bruker NEO 600 MHz spectrometer equipped with a 5 mm BBO CryoProbe using a Bruker zg30 pulse sequence. The relaxation delay was 12 seconds. Pulsed-field gradient NMR spectroscopy experiments were performed using a Bruker ledbpgp2s1d pulse sequence with a gradient pulse length of 2 ms and a delay time of 20 ms.

[0041] Example 1 - Preparation of MDO-AA Copolymer The following procedure was used to prepare copolymers of MDO and acrylic acid with approximately a 1:4 mole:mol ratio of MDO:AA building blocks.

[0042] A. Preparation of MDO-t-butyl acrylate copolymer (1:4 molar ratio of MDO:t-butyl acrylate) A 250 mL three-neck round-bottom flask equipped with a condenser, stir bar, thermocouple, and a Y-shaped glass adapter for two polyethylene feed tubes was charged with ethyl acetate (18.0 g) and placed on an Opti-chem hotplate stirrer heated to 75 °C. 2A blanket of 100 g was applied to remove entrained air and the agitation was set to 300 rpm. The monomer vessel was charged with t-butyl acrylate (24.55 g), MDO (5.45 g), and n-dodecyl mercaptan (0.90 g), and the initiator vessel was charged with Trigonox 125-C75 initiator (0.40 g, 75% active in mineral spirits) in 7.50 g of ethyl acetate (7.50 g). A portion of the contents of the monomer vessel (6.18 g) was added to the reaction flask over 2 minutes. After several minutes, the remainder of the contents of the monomer vessel and the contents of the initiator vessel were metered into the reaction flask at rates of 0.275 g / min and 0.088 g / min, respectively, such that the addition of the contents of the initiator vessel and the remainder of the monomer vessel was completed in 90 minutes. The monomer vessel was rinsed with ethyl acetate (4.50 g), which was added to the reaction flask. After 15 minutes, a portion of Trigonox 125-C75 initiator (0.60 g) in ethyl acetate (2.25 g) was metered into the reaction flask over 30 minutes, followed by a 15 minute hold, followed by a second addition of the same amount of initiator also metered into the reaction flask over 30 minutes. Heating and stirring of the contents of the reaction flask was continued for an additional 30 minutes, after which the reaction was cooled to room temperature. The resulting copolymer was transferred to a glass container for storage without further purification. The solids content was found to be 41.42 wt.%. The conversions of both t-butyl acrylate and MDO were determined to be quantitative by proton NMR spectroscopy.

[0043] B. Deprotection of MDO-t-butyl acrylate copolymer A portion (5.0 g) of the copolymer prepared from Part A was transferred to a 1 oz. glass vial equipped with a stir bar. The volatiles were removed by vacuum distillation, and then the dried polymer was dissolved in methylene chloride (CH 2 Cl 2 -, 8.0 g). Trifluoroacetic acid (TFA, 4.4 g) was added dropwise to the stirred contents of the vial. After the addition was complete, the vial was capped and the reaction mixture was stirred at ambient temperature for 18 hours. A slightly yellow opaque mixture was obtained.

[0044] The volatiles were removed in vacuum, and then anhydrous tetrahydrofuran (THF, 5.0 g) was added to redissolve the reaction mixture. The volatiles were once again removed in vacuum, and the resulting crude product (2.68 g) was dissolved in deionized water (10.26 g) and neutralized with 1N NaOH solution (5.73 g) to obtain a clear solution with a pH of 5.86. The neutralized polymer was dialyzed against deionized water in dialysis tubing with a molecular weight cut-off (MWCO) of 100-500 g / mol to remove low molecular weight impurities. The dialyzed solution was lyophilized to obtain a fluffy white polymer as the final product. The M of the product by GPC as described above was n was 2060 g / mol (polydispersity 4.66). Using proton NMR spectroscopy, the ester content was found to be 18 wt%, the ester retention in the polymer backbone was found to be 80 wt%, and the residual t-butyl groups in the backbone were found to be 3 wt%.

[0045] Example 2 - Preparation of MDO-AA Copolymer The procedure used to prepare the MDO-AA copolymer of Example 2 varied the amounts of t-butyl acrylate (26.62 g), MDO (3.38 g), and n-dodecyl mercaptan (0.34 g) for Part A to give a final molar ratio of MDO:AA of about 1:7, with M n The procedure was essentially the same as that described for the preparation of the MDO-AA copolymer in Example 1, except that the copolymer produced an MDO-AA copolymer with a molecular weight of 4080 g / mol (polydispersity 4.61).

[0046] Biodegradation Simulation The MDO-t-butyl acrylate copolymer of Example 1A was subjected to exhaustive hydrolysis to simulate the biodegradable potential of the MDO-AA copolymer as follows: A general-purpose acid digestion Parr bomb with a 23 mL PTFE cup was charged with 4-5 KOH pellets, approximately the polymer solution (1 g, approximately 40 wt % solids), and ethanol (10 g). The bomb was tightly sealed and transferred to a 150° C. oven and equilibrated for 3 days. The bomb was removed from the oven and cooled to ambient temperature. Disassembly of the bomb revealed the presence of liquid and solid portions. The liquid portion was separated and discarded, and the solid portion was diluted with approximately 5 g of water. The resulting polymer solution was analyzed by GPC as described above, revealing the M of the hydrolyzed polymer. n was found to be 677 g / mol. Hydrolysis studies predict a dramatic reduction in molecular weight from the useful MDO-AA copolymer to biodegradable oligomers.

Claims

1. 1. A process for preparing a copolymer comprising structural units of a cyclic ketene acetal monomer and (meth)acrylic acid, comprising the steps of: a) gradually adding a cyclic ketene acetal monomer and t-butyl (meth)acrylate to a reaction vessel in the presence of an organic solvent and simultaneously and separately gradually adding an initiator to the reaction vessel; heating the contents of the reaction vessel to a temperature sufficient to promote polymerization of the cyclic ketene acetal monomer and the t-butyl (meth)acrylate to provide a solution of a copolymer of the cyclic ketene acetal monomer and the t-butyl (meth)acrylate; and b) contacting the copolymer of the cyclic ketene acetal monomer and the t-butyl (meth)acrylate with a deprotecting agent to form a copolymer of the cyclic ketene acetal monomer and (meth)acrylic acid; Including, a molar:molar ratio of the t-butyl (meth)acrylate to the cyclic ketene acetal monomer in the first portion and the second portion ranges from 2:1 to 15:1; The cyclic ketene acetal monomer has the following structure: 【Chemistry 1】 (wherein n is 0, 1, or 2; R is H or C 1 -C 6 - alkyl, R 1 and R 2 are each independently H, C 1 -C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 -C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently hydrogen or C 1 -C 12 - alkyl or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, when n is 1, R 3 and R 3’ are each independently H, C 1 -C 12 - alkyl, phenyl or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, when n is 2, Each R 3 are independently H, C1-C12-alkyl, or together with the carbon atom to which they are attached form an internal double bond, a fused benzene ring, or a fused C 3 -C 7 - Forms an alicyclic ring) The method comprising:

2. 2. The method of claim 1, wherein the cyclic ketene acetal monomer is selected from the group consisting of: 【Chemistry 2】

3. 3. The method of claim 2, wherein the cyclic ketene acetal monomer is 2-methylene-1,3-dioxepane (MDO) and the t-butyl (meth)acrylate is t-butyl acrylate, and the molar to molar ratio of t-butyl acrylate to MDO ranges from 3:1 to 8:

1.

4. 4. The method of claim 3, wherein in step (a) a chain transfer agent is added slowly to the reaction vessel along with the second portion of the monomer.

5. 4. The method of claim 3, wherein the chain transfer agent is n-dodecyl mercaptan and the temperature of the contents of the vessel in step (a) ranges from 40° C. to 150° C.

6. 6. The method of claim 5, wherein the organic solvent is ethyl acetate and the temperature of the contents of the vessel in step (a) is in the range of 50° C. to 80° C.

7. 2. The method of claim 1, wherein the t-butyl (meth)acrylate is t-butyl acrylate, and after step (b), the organic solvent is removed and the copolymer of cyclic ketene acetal monomer and acrylic acid is dissolved in water.

8. The cyclic ketene acetal monomer is MDO and the MDO-AA copolymer has the following structure: 【Chemistry 3】 The method of claim 7, wherein the aryl group is hydrolyzable to an oligomer having the formula:

9. 4. The method of claim 3, wherein the reaction vessel initially contains a first portion of MDO and t-butyl acrylate in an amount of 10 to 30 weight percent of the combined MDO and t-butyl acrylate used in the reaction.