Multi-layer varnished surface, method for producing a multi-layer varnished surface and furniture products comprising such a surface - Patents.com
A multilayer varnished surface using acrylate-based varnishes cured with electron beam radiation addresses formaldehyde release and resistance issues, achieving formaldehyde-free, mechanically resistant decorative surfaces for furniture.
Patent Information
- Application Number
- JP2024525022
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing decorative surfaces release formaldehyde due to the use of water-based varnishes containing melamine formaldehyde resins, which are harmful and irritating, and existing multilayer surfaces do not provide adequate chemical and mechanical resistance.
A multilayer varnished surface composed of a carrier layer and two varnish layers, where the varnish layers consist of acrylate compounds and reactive diluents, with the first layer containing a matting agent and dispersed pigment, and the second layer being transparent and electron beam-cured, eliminating formaldehyde sources and ensuring adequate resistance.
The solution achieves formaldehyde-free decorative surfaces with enhanced chemical and mechanical resistance, suitable for furniture applications, by using acrylate-based varnishes that are cured with electron beam radiation, providing uniform color and gloss without additional decorative layers.
Smart Images

Figure 2024540003000001_ABST
Abstract
Description
[Technical field]
[0001] The subject of the invention is a multi-varnished surface comprising a transparent varnish layer, which can be cured by means of electron beam or UV radiation, on a carrier such as paper or an artificial film, in particular biaxially oriented polypropylene BoPP, cast unoriented polypropylene cPP, PVC, PET, etc. The subject of the invention is also a method for producing such a multi-varnished surface and a furniture product comprising the multi-varnished surface. [Background technology]
[0002] Multi-coated surfaces for use as decorative materials and methods for producing such surfaces are known in the art.
[0003] Known coated surfaces are usually obtained from an aqueous varnish layer to which acid has been added before application to accelerate the curing process. This layer is then covered with a topcoat of varnish, which is then cured by electron beam or UV. However, aqueous varnishes to which acid has been added to accelerate the curing process of the solid particles of resin also contain melamine formaldehyde resins in amounts of 15 to 45%, which bind the varnish but at the same time cause formaldehyde emissions from such surfaces. Formaldehyde is a colorless gas, accompanied by a strong, characteristic odor, which can be found in our natural environment. Formaldehyde decomposes under the action of sunlight, metabolic processes and the action of bacteria present in soil or water. It can be released into the atmosphere by many materials, such as chipboards, fiberboards, wooden panels, sandwich panels, adhesives, paints and varnishes (mainly those used for wood). Depending on the concentration, formaldehyde can be a toxic, harmful, corrosive or irritating substance.
[0004] Invention US4942198A discloses such water-based varnishes, which contain blocked acid resin, polyacrylate and melamine resin or melamine urea resin. These varnishes are cured by heat treatment, while acid acts as a catalyst in the curing process. Although it is mentioned to keep the formaldehyde level low, the varnishes disclosed in invention US4942198A still emit formaldehyde, because its origin, melamine urea resin, still exists in the varnish composition, and formaldehyde is released during the heat treatment of the varnish.
[0005] Similarly, the invention US4940841A refers to a varnish that can be used on decorative surfaces, which contains polyacrylates, melamine resins, urea resins, polyols and amines. The varnishes used contain formaldehyde sources, melamine and urea resins, which is why the emission of formaldehyde is not prevented.
[0006] Document P.426181 discloses a multi-coated surface and a method for producing such a surface. The multi-layer surface in said document P.426181 comprises a carrier layer, a printed decoration layer, a primer layer and a varnish layer. However, the last varnish layer, which forms the structure, does not completely cover the surface, but rather copies the printed decoration. Moreover, document P.426181 discloses a method for producing said multi-layer decorated surface. The method consists in applying the decoration to the carrier layer, then applying a primer to it and then applying a varnish that can be cured with an electron beam. A matte surface is obtained by excimer irradiation. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] U.S. Pat. No. 4,942,198 [Patent Document 2] U.S. Pat. No. 4,940,841 [Patent Document 3] Polish Patent Application Publication No. 426181 Summary of the Invention [Problem to be solved by the invention]
[0008] Thus, the present invention aims to reduce or eliminate formaldehyde emissions from decorative surfaces by eliminating water-based varnishes to which acid is added before application, while ensuring the chemical and mechanical resistance of the new decorative surfaces. To achieve this goal, the multi-coat surface of the present invention uses formaldehyde-free coatings as varnishes. In the present invention, no formaldehyde sources are used, such as acid-cured varnishes and melamine-formaldehyde resins. [Means for solving the problem]
[0009] a) a carrier layer 1 made of a material based on paper or polymer film; b) a first varnish layer 2; c) a second varnish layer 3; A multi-layer varnished surface, comprising: a varnish in the first and second varnish layers comprising an acrylate compound and a reactive diluent monomer; The varnish in the first varnish layer 2 having a thickness in the range of 2 to 10 μm further comprises at least one matting agent and at least one dispersed pigment, the first varnish layer 2 is applied directly to the carrier layer 1 and covers the entire surface of the carrier layer 1, and the second varnish layer 3 having a thickness in the range of 2 to 10 μm is applied directly to the first varnish layer 2 and covers the entire surface of the first varnish layer 2, resulting in a multi-layer varnished surface. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 shows a cross section of a decorative product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] 1. A multi-layer varnished surface consisting of: a) a layer made of a material based on paper or polymer film; b) a first coat of varnish; c) a second layer of varnish; It consists of: The varnish in the first and second varnish layers comprises an acrylate compound and a reactive diluent monomer; It is characterized by the fact that the varnish in the first varnish layer having a thickness in the range of 2 to 10 μm comprises at least one matting agent and at least one dispersed pigment, the first varnish layer is applied directly to the carrier layer and covers the entire surface of the carrier layer, and the second varnish layer is applied directly to the first varnish layer and covers the entire surface of the first varnish layer.
[0012] Preferably, the polymer film is BoPP, cPP, PVC or PET and the paper is an impregnated paper.
[0013] It is also preferred that the second varnish layer comprises a matting agent.
[0014] The matting agent is titanium dioxide (TiO 2 It is also preferred that:
[0015] It is also preferred that the second varnish layer comprises an adhesion promoter.
[0016] The multi-layer surface is composed of a carrier layer 1, a first varnish layer 2 and a second varnish layer 3. The carrier layer 1 is made of a material based on paper or a polymer film. The polymer film is selected from the group consisting of BoPP, cPP, PVC and PET. If the carrier layer 1 is paper, the paper can be impregnated.
[0017] The first varnish layer 2 is applied directly to the surface of the carrier layer 1, covering the entire surface of the carrier layer 1. The first varnish layer 2 has a thickness ranging from 2 to 10 μm. This layer determines the final color appearance of the product and is also a key factor in obtaining chemical resistance on the decorative surface. However, a single varnish layer does not achieve the level of mechanical resistance expected in the furniture industry. It has been observed that if only one varnish layer is present on the decorative surface, the sensitivity to metal abrasion tests increases. For this reason, another coat of varnish should be applied to improve the abrasion resistance.
[0018] The second layer, applied directly to the entire surface of the first layer, is a coating of transparent electron beam cured varnish, the thickness of which ranges from 2 to 10 μm. The application system of this varnish layer used at present makes it possible to obtain optimal surface properties in terms of homogeneity and gloss, which are particularly important in the final visual evaluation of the product.
[0019] The varnish in the first varnish layer comprises an acrylate compound, a reactive diluent monomer, at least one matting agent and at least one pigment. The acrylic resin binds the solid substances (fillers, pigments), creates a uniform coating, is responsible for adhesion to the substrate and affects the gloss and transparency of the coating. The reactive diluent monomers have a low molecular weight and low viscosity. The monomers do not evaporate from the coating and are involved in the chemical reaction (i.e. they create the coating). Due to the pigments used in the varnish, the decorative surface has one uniform color and there is no need to apply additional decorative layers. Moreover, the resulting multi-layer surface is economically produced, since no additional decorative layers are required. The matting agent is TiO 2 It can also act as a white pigment if such a varnish does not contain formaldehyde and therefore does not emit formaldehyde.
[0020] The method for obtaining a multi-layer varnished surface comprises these steps: a) providing a carrier layer made of a paper or polymer film based material; b) coating the entire surface of the carrier layer with a first layer of varnish comprising a matting agent, c) exposing the applied first varnish layer to a dose of 2 to 6 kGy of electron beam radiation or to a sufficient dose of UV radiation; d) covering the entire surface with a second layer of varnish; e) exposing the applied second varnish layer to a dose of at least 35 kGy of electron beam radiation or to a sufficient dose of UV radiation.
[0021] Preferably, before curing in step e), the applied transparent varnish layer is subjected to excimer lamp irradiation at a wavelength of 172 nm.
[0022] The coating of steps b) and d) can be carried out by any method known in the art. 3WS and DKR coating methods and flexographic coating are preferred. It is advantageous if both methods are combined, i.e. the first varnish layer is applied using a 3WS coating system and the second varnish layer is applied using a flexographic coating system, or the first varnish layer is applied using a 3WS coating system and the second varnish layer 3 is applied using a DKR coating system.
[0023] With doses in the range of 2-6 kGy, the electron beam curing treatment carried out in step c) does not cause a complete polymerization of the applied first layer of varnish, but rather causes a prepolymerization, i.e. a gelation, allowing the application of the next layer and providing sufficient adhesion between the next layer and the first layer of applied varnish.
[0024] The electron beam curing carried out in step e) with a dose of 35 kGy leads to a complete polymerization of the surface. As a result of this treatment, the second varnish layer is completely cured.
[0025] The manufacturing process is based on a varnishing or print-varnishing machine. A blank roll is placed in the unwinding section. The web advances by a series of guide rollers to the first varnish layer coating section. Application takes place at the contact point of the substrate and the varnishing roller. A second coat of varnish is applied in the same way in the next varnishing system. After applying the two layers of varnish and allowing them to properly harden, the web advances to the winding section. The product is ready for further processing in the furniture system.
[0026] The essence of the solution is also a furniture product having the above-mentioned multi-layer varnished surface.
[0027] The subject of the invention is presented in more detail in FIG. 1, where item 1 is the carrier layer, 2 is the electron beam cured pigmented varnish layer, and 3 is the electron beam cured clear varnish layer. EXAMPLES
[0028] All Schattdecor varnishes used in the examples below contain a matting agent. 71-83.0 40%-TiO 2 71-83.4 40%-TiO 2 0.26%-Flame Silica (Pyro) 70-92.1 1.5% - amorphous, synthetic silica (3.4~4.0μm) 31%-PMMA 70-92.10 0.2%-furnaceous silica - used as an anti-delamination agent
[0029] On the other hand, Hesse varnish is available on the market and its composition is published by the manufacturer.
[0030] For the excimer lamps used, the standard neutralization level in the chamber containing these lamps during production is 50-200 ppm.
[0031] In empirical varnishing tests we were able to obtain coatings with thicknesses between 8 and 20 μm that resist mechanical and chemical tests.
[0032] Example 1: Two-layer online coating - two 3WS systems A base roller in the form of a smooth impregnated paper semi-finished product, the so-called vorimpregnate, is placed in the unwinding section of the machine.
[0033] A first varnish layer 2, which is an electron beam cured pigmented varnish, is applied to the carrier layer 1. At this stage of the process the coat has the following composition: · Schattdecor 71 Varnish - 83.4 - 0.5 parts · Schattdecor 71 Varnish - 83.0 - 0.5 parts
[0034] The coating takes place in a 3WS system. The substrate is uniformly coated on the entire surface with a 7 μm thick layer. The layer undergoes prepolymerization (gelation) in an electron beam generator. The generator parameter settings are as follows: ·Radiation dose-5kGy High voltage - 110kV
[0035] The applied layer has a surface gloss of 19° measured in 60° geometry.
[0036] The coated material then moves to a second 3WS coating station where a second coat of varnish 3 is applied. The composition of the second varnish layer 3 is as follows: · Schattdecor 70 Varnish - 92.10 - 0.8 parts · Schattdecor 70 Varnish - 92.1 - 0.2 parts
[0037] The resulting coating is fully electron beam cured in the generator. The equipment settings are as follows: ·Radiation dose-35kGy High voltage - 110kV
[0038] The finished surface has a gloss of 26° measured in 60° geometry and a total coating thickness of 15μm±1μm.
[0039] The decorative surface obtained is characterized by a uniform color, guaranteed by the composition of the varnish from the first layer 2, as well as chemical and mechanical resistance adapted to the requirements of the furniture industry. Moreover, both varnish layers are formaldehyde-free, which makes the product even more attractive. A condition for good adhesion of both varnish layers is the initial gelation of the first varnish layer.
[0040] FIG. 1 shows a cross section of a substrate having a layer of varnish.
[0041] Example 2: Two on-line layers - first layer in 3WS system - second layer in flexographic printing system, coating refined by excimer lamp exposure The carrier layer 1, the first varnish layer 2 applied thereon and cured are the same as in Example 1. The gelled first varnish layer 2 evenly coats the entire web of impregnated paper and proceeds to the second flexographic coating station.
[0042] The system application roller applies a layer of transparent electron beam curable varnish consisting of: Hesse FL27692 varnish - 0.9 parts Hesse FL27800 Varnish - 0.08 parts ·Scuff resistance additive-Hesse FZ2711-0.05 part Varnish adhesion enhancing additive - Hesse FL2720 - 0.015 parts
[0043] The applied layers first go through a surface refinement chamber using excimer lamps, which allows to obtain a matte varnish coating, then the moving web passes through a chamber of an electron beam generator, where both layers of varnish are finally cured, creating a material ready for further furniture processing.
[0044] Parameters of the electron beam generator during the final curing of the varnish layer: ·Radiation dose-35kGy High voltage - 110kV
[0045] The product surface is characterized by a gloss in the range of 8°-10° when measured at a 60° geometry, and a coating having a thickness of 14 μm±1 μm.
[0046] The conditions for good adhesion of both layers of varnish are the initial gelation of the first varnish layer and the addition of an adhesion promoter in the second varnish layer.
[0047] The resulting film and its cross section are disclosed in FIG.
[0048] Example 3: Two On-line Layers - Two 3WS Systems - Second Layer Refined Using Excimer Lamp Exposure The method of applying and curing the carrier layer 1 and the first varnish layer 2 thereon is the same as in Example 1. The gelled first varnish layer 2 evenly coats the entire web of impregnated paper and proceeds to a second coating station with 3WS rollers.
[0049] At this stage the web is coated with a layer of a transparent electron beam cured varnish having the following composition: Hesse FL27692 varnish - 0.5 parts Hesse FL27800 Varnish - 0.48 parts ·Scuff resistance additive-Hesse FZ2711-0.05 part Varnish adhesion enhancing additive - Hesse FL2720 - 0.15 parts
[0050] The applied layers first go through a surface refinement chamber using excimer lamps, which allows to obtain a matte varnish coating, then the advancing web passes through a chamber of an electron beam generator, where both layers of varnish are finally cured, thus preparing the finished product for further processing in the furniture surface refining process.
[0051] Parameters of the electron beam generator during the final curing of the varnish layer: ·Radiation dose-35kGy High voltage - 110kV
[0052] The surface of the finished material is characterized by a coating having a 6° gloss and a thickness of 16 μm±1 μm when measured at a 60° geometry.
[0053] The decorative material thus obtained can be successfully used for veneer applications on kitchen fronts or other furniture surfaces. The matt finish produced in this example complements the range of standard monochromatic high gloss surfaces.
[0054] The conditions for good adhesion of both layers of varnish are initial gelation of the first varnish layer 2 and the addition of an adhesion promoter in the second varnish layer 3 .
[0055] The resulting film and its cross section are disclosed in FIG.
[0056] Example 4: Two online layers - two 3WS systems - synthetic film as carrier Unlike examples 1 and 2 or 3, the substrate coated on the two layers of varnish is a polypropylene or polyethylene synthetic film. Good properties for further processing in furniture applications are obtained by using polypropylene and polyethylene films.
[0057] All coating and refinement processes can be repeated in this embodiment based on the processes of Examples 1, 2 or 3.
[0058] The surfaces obtained are materials for furniture applications in various application areas, especially where it is appropriate to use monochromatic decorative effects and where the application of substrates in the form of synthetic films is required.
[0059] As in Examples 1, 2 or 3 above, the condition for adhesion of both layers of varnish is to first gel the first layer before applying the second layer.
[0060] FIG. 1 shows a cross section of a product according to the principles of the invention.
[0061] Example 5: Off-line coating of two layers - DKR+3WS On the carrier, a first layer of electron beam cured pigmented varnish is applied by a DKR roller coating station as in example 1. This process results in a coating varnish of the following composition: · Schattdecor 71 Varnish - 83.4 - 0.5 parts · Schattdecor 71 Varnish - 83.0 - 0.5 parts
[0062] The applied layer having a thickness of 8 μm is partially polymerized (gelled) by irradiation from an electron beam generator. The partial polymerization is described with the following equipment settings: ·Radiation dose-5kGy High voltage - 110kV
[0063] After this stage of the process, a varnish coated web is obtained with a uniform color visual effect with a gloss of 18° measured at a 60° geometry. The web is wound up on a roller, fixed and prepared for the next coating process on a different machine.
[0064] In order for the product to meet the chemical and mechanical resistance requirements, a second stage of varnish coating is necessary, which can occur on a different varnishing machine or at a different time on the same machine, but with a different configuration of the varnish coat application process. For this reason, this embodiment is called off-line coating, which means that the finished product is obtained by passing the substrate through the coater twice.
[0065] The second varnishing process is carried out using a 3WS coating station. At this stage a layer of transparent electron beam cured varnish is applied. The varnish has the following composition: · Schattdecor 70 Varnish - 92.10 - 0.8 parts · Schattdecor 70 Varnish - 92.1 - 0.2 parts
[0066] The resulting coating is fully cured with an electron beam in a generator.
[0067] The device settings are as follows: ·Radiation dose-35kGy High voltage - 110kV
[0068] The decorative surface has a gloss coating of 25° measured using a 60° geometry. The coated web is characterized by a total thickness of the varnish coat of approximately 17 μm±1 μm and a homogeneous monochromatic decorative effect.
[0069] A condition for good adhesion of both varnish layers is initial gelation of the first varnish layer.
[0070] FIG. 1 shows a cross section of a decorative product.
[0071] [Table 1]
Claims
1. a) a carrier layer 1 made of a material based on paper or polymer film; b) a first varnish layer 2; c) a second layer of varnish 3; A multi-layer varnished surface, comprising: a varnish in the first and second varnish layers comprising an acrylate compound and a reactive diluent monomer; A multi-layer varnish coated surface, characterized in that the varnish in the first varnish layer 2 having a thickness in the range of 2 to 10 μm further comprises at least one matting agent and at least one dispersed pigment, the first varnish layer 2 is applied directly to the carrier layer 1 and covers the entire surface of the carrier layer 1, and the second varnish layer 3 having a thickness in the range of 2 to 10 μm is applied directly to the first varnish layer 2 and covers the entire surface of the first varnish layer 2.
2. 2. A multi-layer varnished surface according to claim 1, characterized in that the polymer film is BoPP, cPP, PVC or PET.
3. 2. A multi-varnished surface according to claim 1, characterized in that the second varnish layer (3) comprises a matting agent.
4. The matting agent is titanium dioxide TiO 2 4. A multi-layer varnished surface according to claim 1 or 3, characterized in that:
5. 2. A multi-layer varnished surface according to claim 1, characterized in that the second varnish layer (3) comprises an adhesion-promoting additive.
6. a) providing a carrier layer 1 made of a paper or polymer film based material, b) coating the entire surface of the carrier layer 1 with a first varnish layer 2 comprising a matting agent, c) exposing the applied first varnish layer 2 to a dose of 2-6 kGy of electron beam radiation or to a sufficient dose of UV radiation, d) coating said entire surface with a second layer of varnish 3, e) exposing said applied second varnish layer 3 to a dose of at least 35 kGy of electron beam radiation or to a sufficient dose of UV radiation, 2. A method for obtaining a multi-layer varnished surface, comprising the steps of:
7. 7. A method according to claim 6, characterized in that before curing in step e), the applied transparent varnish layer 3 is subjected to an excimer lamp with a wavelength of 172 nm.
8. A furniture article comprising a multi-layer varnished surface according to claims 1 to 5.
Citation Information
Patent Citations
PL426181
Aqueous two-component paints for one-coating of high-resistant finishing sheeting and continuous edging
US4940841A
Aqueous pigmented two-component lacquers for single-layered coating of finish films and continuous edges
US4942198A