METHOD FOR PRODUCING STEAM REFORMING CATALYST FOR SULFUR-CONTAINING METHANE GAS AND METHOD FOR PRODUCING HYDROGEN USING THE SAME

The triple metal catalyst on alumina support addresses sulfur and coke issues in steam reforming, maintaining high hydrogen production efficiency and durability by using a controlled manufacturing process.

JP2024540100AActive Publication Date: 2024-10-31HEESUNG CATALYSTS CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024525400
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-18
Filing Date
2022-11-14
Publication Date
2024-10-31
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

Existing nickel-based catalysts for steam reforming of methane are susceptible to sulfur poisoning, coke deposition, and sintering, leading to reduced activity and durability, making them less economical and less effective for long-term hydrogen production.

Method used

A triple metal catalyst is developed by supporting nickel, cerium, and barium on an alumina support with controlled pore characteristics, enhancing sulfur resistance and suppressing coke deposition and sintering, using a specific manufacturing process that includes heat treatment, metal precursor impregnation, and hydrogen reduction.

Benefits of technology

The catalyst maintains high conversion rates and selectivity for hydrogen production while resisting sulfur poisoning and coke formation, ensuring stable activity over an extended period.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540100000001_ABST
    Figure 2024540100000001_ABST
Patent Text Reader

Abstract

This relates to a method for manufacturing a nickel-auxiliary metal composite metal catalyst using an alumina carrier having a mixture of different crystal phases, and a method for manufacturing hydrogen by steam reforming of sulfur-containing methane gas using the same. The composite alumina carrier has acid sites removed by heat treatment, and is manufactured by compositely and sequentially incorporating nickel and auxiliary metals into the composite alumina carrier using a pressurized injection method. The alumina carrier has an α-alumina / θ-alumina ratio of 10 or more and a specific surface area of ​​5 to 20 m. 2 The present invention relates to a nickel-transition metal / mixed alumina catalyst, the catalyst being prepared and used with a pore size distribution in the range of 10-50 nm, the nickel loading amount in the catalyst being 5-15 wt%, the nickel dispersion degree being 2-15%, and the nickel / auxiliary metal weight ratio being in the range of 5-10, and a method for producing hydrogen by steam reforming of sulfur-containing methane gas using the catalyst. By using the catalyst prepared according to the present invention, the large pores in the catalyst maximize the gas permeability between the reactants and the catalyst, thereby increasing the reaction rate, and the problems of carbon deposition and particle sintering at high temperatures, which are problems with nickel catalysts, are suppressed by combining with cerium, and barium is added to increase resistance to sulfur poisoning, thereby improving the durability of the catalyst and enabling stable hydrogen production for a long period of time.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a nickel-based alumina catalyst used in a steam reforming process for producing hydrogen from methane, which is the main component of liquefied natural gas. More specifically, the present invention relates to a method for producing a macroporous nickel-auxiliary metal / alumina catalyst and a method for producing hydrogen by the steam reforming reaction of sulfur-containing methane gas using the same. [Background technology]

[0002] Recently, energy demand is increasing worldwide due to industrial development and population growth, but the fossil fuels used as energy sources are gradually becoming depleted, and in order to prepare for global warming caused by greenhouse gases, countries around the world are continuing to research clean energy sources that can replace fossil fuels. Among these, the substance that is being most actively researched as an environmentally friendly energy source is hydrogen. Hydrogen is said to be able to replace almost all of the energy used in existing sources, and since it does not contain carbon, the main component of carbon dioxide, it has been attracting attention as a clean energy source.

[0003] Hydrogen is also used as a raw material for fuel cells, which are classified as a new renewable energy source, and its demand is expected to explode in the future. The traditional methods for producing hydrogen are reforming fossil fuels and electrolysis of water using renewable energy. The electrolysis method currently produces hydrogen at a level of about 5-10% of the total hydrogen required, but due to its low economic efficiency, it is expected that full-scale mass production will be possible after 2030 or 2040. Therefore, to date, the most widely used method for producing hydrogen is to use natural gas or polyols such as glycerol, sorbitol, and xylitol, and biomass, and many researchers are focusing on improving the efficiency and reducing the cost of hydrogen production in this process. Representative methods for producing hydrogen using natural gas include auto-thermal reforming [Non-Patent Document 1: Jeongdong Kim et al., Ind. Eng. Chem. Res. 2021, 60, 19. 7257-7274], partial oxidation [Non-Patent Document 2: Anis Fakeeha et al., Processes 2020, 8, 499], carbon dioxide reforming [Non-Patent Document 3: Mun-Sing Fan et al., Int J Hydrogen Energy, 36, 8, 2011, 4875-4886], and steam reforming [Non-Patent Document 4: Kantilal Chouhan et al., Int J Hydrogen Energy, 46, 53, 2021, Among these, the steam reforming process is the most economical hydrogen production process when carbon dioxide separation and storage are not taken into consideration, and since the reaction products are simpler than other reactions and the selectivity for hydrogen is high, it is the process most commonly used commercially.

[0004] Generally, the conversion of natural gas (mainly methane) to hydrogen is an endothermic reaction, so it is carried out at high temperatures to maintain the reaction temperature, and excess steam is injected to reduce the rate of coke formation during the reaction.

[0005] Therefore, the currently commercialized methane steam reforming process (Reaction Scheme 1) produces synthesis gas of hydrogen and carbon monoxide at an operating temperature of 800°C to 1000°C by injecting steam and methane at a ratio of 2.0 to 3.0 in the presence of a reforming catalyst. In addition, the carbon monoxide produced after steam reforming is further converted into hydrogen through the water gas shift reaction (Reaction Scheme 2), thereby increasing the hydrogen yield. The theoretical reaction scheme for converting natural gas to hydrogen as described above is as follows:

[0006] Reaction formula 1 (methane steam reforming reaction): CH4 + H2O → CO + 3H2 Reaction 2 (Carbon monoxide water-gas shift reaction): CO+H2O→CO2+H2 Overall (Reaction 1 + Reaction 2) Reaction: CH4 + H2O → CO2 + 4H2

[0007] Meanwhile, catalysts for steam reforming reactions to produce hydrogen from natural gas must have high reaction activity, a certain period of life, high heat transfer, low pressure drop, high thermal durability and mechanical strength. For this purpose, catalysts are manufactured by incorporating active metals using a strong oxide-type support, and catalysts developed so far include precious metal catalysts (platinum, palladium, rhodium, ruthenium, iridium, etc.), non-precious metal catalysts (nickel, copper, etc.), or mixed catalysts of precious metals-non-precious metals and non-precious metals-non-precious metals (platinum-nickel, rhodium-nickel, ruthenium-nickel, nickel-copper, nickel-zinc, nickel-tin, etc.) (Non-Patent Document 5: Eugenio Meloni et al, Catalysts 2020, 10, 352). Precious metal catalysts have the advantage of a high hydrogen production rate due to a lower coke generation rate during the reaction compared to non-precious metal catalysts, but have the disadvantage that they are not economically viable for use in commercial processes due to the continued rise in precious metal prices worldwide. In the case of non-noble metal catalysts, nickel-containing catalysts are typically used in most reforming processes at present because they have reforming ability and are inexpensive.

[0008] However, nickel catalysts are more susceptible to sulfur poisoning than precious metal catalysts (sulfur compounds such as thiophenes and mercaptans are present in natural gas and are removed using an adsorbent before the reforming reaction, but depending on the reforming method, sulfur at a level of 0.1 to 5 ppm remains in the gas after desulfurization, and the residual sulfur is adsorbed by the catalyst during the reforming reaction, causing a decrease in activity), and as summarized in Table 1, various types of coke (whisker type coke or pyrolytic coke) are actively produced at high temperatures, which can lead to the destruction of the catalyst itself due to deposition on the surfaces of metals and catalysts and continuous accumulation within the catalyst, and therefore can be disadvantageous in long-term use (Non-Patent Document 6: Qimin Ming et al., Catalysis Today, Vol. 77, Issues 1×2, 2002, Pages 51-64).

[0009] [Table 1]

[0010] In addition, due to its low thermal durability, the nickel metal in the catalyst gradually aggregates and sinters during high-temperature reactions, increasing the particle size and gradually speeding up the deactivation rate over time. Regarding this technical matter, JR Rostrup-Nielsen et al. (Advances in Catalysis 2002, 47:65-139) conducted a study on the rate of coke formation depending on nickel particle size, and confirmed that the larger the nickel particle size, the more rapidly the initial stage of coke formation occurs.

[0011] For this reason, many researchers have been researching to find a method for manufacturing a catalyst that can improve coke resistance, sulfur resistance, and long-term durability at high temperatures even though it is a non-precious metal catalyst, and most of the research in the process has focused on research to improve catalytic activity by diversifying the type of catalyst support or adjusting the metal-support interaction. In addition, research has been continuing for a long time to improve activity by using composite metals other than nickel alone as the catalytically active metal. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Republic of Korea Patent No. 10-0781503 [Patent Document 2] Republic of Korea Patent No. 10-0962584 [Patent Document 3] Republic of Korea Patent No. 10-0980591 [Patent Document 4] Republic of Korea Patent No. 10-0394076 [Patent Document 5] Republic of Korea Patent No. 10-1625537 [Non-patent literature]

[0013]

Non-licensed literature 1

Non-licensed Document 2

Non-licensed Document 4

Non-licensed Document 5

Non-licensed Document 6

Non-licensed Document 7

Non-licensed Document 8

Non-licensed literature 9

Non-licensed literature 10

[0014] As a method for suppressing coke deposition and enhancing activity by changing the type of support for nickel catalysts, a catalyst in which nickel is supported on a silica-zirconia composite oxide support (Patent Document 1: Korean Patent No. 10-0781503), a mesoporous nickel-alumina hybrid catalyst using an anionic surfactant, sol-gel, and a templating method (Patent Documents 2-3: Korean Patent No. 10-0962584; Korean Patent No. 10-0980591), a catalyst in which nickel is supported on a cerium-zirconia support (Patent Document 4: Korean Patent No. 10-0394076; Non-Patent Document 8: Ignacio Iglesias et al., Int J Hydrogen Energy, Vol. 44. Issue 16, 2019, Pages 8121-8132), and a La catalyst using a template method have been reported. 1-x Ce x Catalysts using these supports have the advantage of being able to improve the durability of the catalyst, but they have the limitation of being less price-competitive because the manufacturing process is complicated and the manufacturing costs are high compared to commercially used alumina supports.

[0015] In addition to nickel alone, a method of binding different metals as promoters to an alumina support to increase activity has been used, such as Ni / Mg-Al2O3, Ni / Si-Al2O3, Ni / La-Al2O3, Ni / Ce-Al2O3, etc., which change the properties of the support, or adding Ru, Au, Ce, Ir, Nb, Pt, Co, Ag, etc. as auxiliary metals to increase activity (Non-Patent Document 9: Haotian Zhang et al., Renewable and Sustainable Energy Reviews, 149, 2021, 111330). Non-Patent Document 10: Juliana da S. Lisboa et al. (Catalysis Today 101, 2005, 15-21) and others showed the effect of suppressing the aggregation phenomenon of nickel particles by adding alkali metals or alkaline earth metals to nickel catalysts, but showed the disadvantage that the methane conversion rate was low and the overall reaction activity was low. [Means for solving the problem]

[0016] As mentioned above, nickel catalysts developed to date have been improved in activity and durability through various methods. As part of such manufacturing methods, the present invention aims to manufacture a triple metal catalyst by adding nickel and a different auxiliary metal to an alumina support with controlled pore characteristics, and to apply this to the steam reforming reaction of sulfur-containing methane gas to demonstrate stable catalytic activity for a long period of time.

[0017] Therefore, the technical object of the present invention is to provide a method for producing a catalyst used for producing hydrogen by steam reforming of sulfur-containing methane gas simulating natural gas, which has resistance to poisoning by trace amounts of sulfur components remaining in the reactants, minimizes deposition of coke generated during high-temperature reactions, and inhibits sintering of nickel metal, thereby maintaining stable reaction activity for a long period of time.

[0018] Another technical object of the present invention is to provide a method for stably producing hydrogen by steam reforming of sulfur-containing methane gas using the catalyst produced as described above.

[0019] In order to achieve the above technical objective, the inventors have manufactured a catalyst by changing the pore distribution of a highly cost-competitive alumina carrier so that the reactant natural gas can diffuse within the catalyst and the product can quickly move outside the catalyst. In addition, the inventors have manufactured a catalyst by positioning cerium, which can increase the dispersion of nickel, the main active site, and barium, which can suppress poisoning by sulfur, in a tri-metallic form on the manufactured carrier so that each metal can exhibit its own unique characteristics.

[0020] The alumina carrier used in the present invention is heat-treated to increase its strength so that it can withstand high temperatures during the reforming reaction, and the heat treatment temperature of the carrier is adjusted to support 10 wt% or more of nickel and auxiliary metals, so that the surface area is 5 to 20 m. 2 / g, and the average pore distribution was maintained in the range of 10 to 50 nm. The crystal phase of the support was initially γ-alumina, which was calcined at 1100 to 1150 °C, and then it was manufactured to have a mixed crystal phase of α-alumina and θ-alumina.

[0021] In the present invention, the catalyst is prepared by mixing 80-90 wt % of alumina carrier, 10-15 wt % of nickel metal, a weight ratio of nickel / cerium of 5-10, and a weight ratio of nickel / barium of 15-100, and the nickel metal is mixed in the carrier at a concentration of 0.5-1.5 wt % / m 2 / g (weight% / specific surface area of ​​carrier 10-20m 2 / g basis), and the auxiliary metal cerium is present in the carrier at an active metal density of 0.05 to 0.2 wt% / m 2 / g, and another auxiliary metal, barium, is added to the support at 0.005 to 0.03 wt% / m 2 The active metal density was uniformly increased by 100%.

[0022] The present invention also relates to a method for preparing a carrier having a weight ratio of α-alumina / θ-alumina of 10 or more (α 91%-theta 9%) to (α 100%-theta 0%) by heat treating spherical γ-alumina at 1100-1150°C, b) supporting an alloy solution, in which nickel and cerium precursors are mixed and dissolved in a solvent, on the prepared hybrid alumina carrier by pressurized spraying at room temperature, and c) drying the supported carrier at 100-120°C in an air atmosphere and calcining the supported carrier at 700-850°C. d) supporting the prepared nickel-cerium / mixed alumina material with a solution of a barium precursor by a pressurized spray method at room temperature; e) drying the supported material at 100-120°C in an air atmosphere and calcining the material at 500-600°C; and f) rapidly reducing the prepared nickel-cerium-barium / mixed alumina oxidation catalyst with hydrogen gas at a temperature in the range of 550-700°C to prepare a final catalyst.

[0023] In the presence of the catalyst produced in the present invention, a steam reforming reaction of sulfur-containing methane gas simulating liquefied natural gas is carried out. The steam / methane gas volume ratio is in the range of 2.5 to 3.5 at a reaction temperature of 700 to 850°C and a gas hourly space velocity (GHSV) of 500 to 30,000 h -1 The present invention provides a method for producing hydrogen, comprising the steps of: Effect of the Invention

[0024] The nickel-cerium-barium / alumina triple catalyst with controlled pore size and surface area prepared according to the present invention and the hydrogen production method using the same are applied to the steam reforming reaction of sulfur-containing methane gas, and are intended to exhibit resistance to sulfur poisoning, catalyst sintering, and coke deposition, which are causes of catalyst deactivation, even under high temperature reaction conditions. As a result, the agglomeration phenomenon of nickel metals is suppressed, significantly reducing the rate of deactivation, and nickel metal is no longer poisoned by coke and sulfur, so that the conversion rate and selectivity to hydrogen are maintained at a high level stably for a long period of time during the steam reforming reaction. [Brief description of the drawings]

[0025] [Figure 1] 1 is a flow chart illustrating steps of a manufacturing method according to a first embodiment of the present invention. [Diagram 2] 1 is an electron microscope (video microscope) and electron probe X-ray microanalyzer (EPMA) photographs of the catalyst prepared in Example 1 of the present invention. [Diagram 3] 1 shows the results of a long-term reforming reaction using the catalysts produced in Example 1 and Comparative Examples 4, 5, and 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention relates to a method for producing a catalyst used in the steam reforming reaction of sulfur-containing methane gas, and is characterized in that a support having an adjusted acid site and pore size is produced, nickel is used as an active metal, and cerium and barium are supported as auxiliary metals to enhance sulfur resistance and coke resistance to produce a catalyst.

[0027] The composite metal catalyst of the present invention, in which nickel-auxiliary metal is supported on an alumina support having controlled crystal phase and pore characteristics, is a) heat-treating spherical γ-alumina at 1100-1150°C to produce a carrier having an α-alumina / θ-alumina weight ratio of 10 or more, preferably 91% by weight or more of α-alumina and 9% by weight or less of θ-alumina; b) supporting an alloy solution in which nickel and cerium precursors are mixed and dissolved in a solvent on the prepared hybrid alumina support by a pressurized spray method at room temperature; c) drying the supported catalyst at 100 to 120° C. in an air atmosphere and calcining the supported catalyst at 700 to 850° C.; d) supporting a solution of a barium precursor dissolved in a solvent on the prepared nickel-cerium / mixed alumina by pressurized spraying at room temperature; e) drying the supported catalyst at 100 to 120° C. in an air atmosphere and calcining the supported catalyst at 500 to 600° C.; f) rapidly reducing the prepared nickel-cerium-barium / mixed alumina oxidation catalyst at a high temperature in the range of 550 to 700° C. using hydrogen gas to prepare a catalyst.

[0028] Each step will be described in detail below. The temperature unit indicated in this specification is Celsius.

[0029] In step a), the alumina support may be prepared by using boehmite, pseudoboehmite or γ-alumina as a starting material, and by heat-treating the support at a temperature of 1100-1150°C for 1-5 hours in a heat treatment furnace in order to remove the acid sites and adjust the pore size, thereby changing the crystal phase to α-alumina containing 1-10 wt% of θ-alumina. The heat treatment temperature is closely related to the crystal phase and pore structure of the support. When the heat treatment temperature is less than 1100°C, the crystal phase of alumina may be in a mixed state of θ-alumina phase and γ-alumina phase, and acid sites may still exist in the support, and the pore size of the support is small, so the diffusion rate of reactants in the support may be low. When the heat treatment temperature is more than 1150°C, the pore size becomes large, and the crystal phase of alumina becomes an alpha phase and exists as a single crystal phase, so all the acid sites in the support can be removed, but the specific surface area is 3m 2 The alumina carrier thus produced has an average pore distribution in the range of 20 to 50 nm, an α-alumina / θ-alumina ratio of 10 or more, and a specific surface area of ​​5 to 20 m 2 The carrier may have a shape of sphere, cylinder, pellet, or tube, and these shapes can be produced by oil-drop, tablet, or extrusion methods.

[0030] In step b), the nickel precursor may be any one of nickel nitrate hydrate, nickel chloride hydrate, nickel acetate hydrate, and nickel sulfate hydrate, and the cerium precursor may be any one of cerium nitrate hydrate, cerium chloride hydrate, cerium acetate hydrate, cerium sulfate hydrate, and cerium oxalate hydrate. Preferably, compounds having the same anion form may be sequentially supported or mixed to prepare a support solution. The active metal precursor may be prepared by dissolving the active metal precursor in ion water or a dihydric alcohol (ethanol, ethylene glycol, etc.) solvent in an amount equal to the pore volume of the support, and supporting the active metal precursor on the support using a pressurized spray method.

[0031] The nickel precursor may be supported at 10-15 wt% based on the final catalyst. If supported at 10 wt% or less, catalytic performance is difficult to achieve, and if supported at 15 wt% or more, the nickel precursor is not drawn into the support and accumulates on the surface of the support, resulting in poor nickel dispersibility and reduced durability. The cerium precursor may be supported at a nickel / cerium weight ratio of 5-10, preferably 5-7.

[0032] In step c), the nickel-cerium / mixed alumina precursor produced in step b) may be dried and then heat-treated at a temperature in the range of 700 to 800° C. to remove moisture and anions derived from the metal precursor. The heat treatment temperature is common knowledge and may be within an appropriate range, so further detailed description will be omitted. However, it is preferable to carry out the heat treatment at a temperature equal to or higher than the reforming reaction temperature so that deformation of the metal in the catalyst does not progress during the steam reforming reaction.

[0033] In step d), the barium precursor may be any one of barium nitrate hydrate, barium chloride hydrate, barium acetate hydrate, and barium hydroxide hydrate, and the active metal precursor may be dissolved in ion water or a dihydric alcohol (ethanol, ethylene glycol, etc.) solvent in an amount equal to the pore volume of the support, and then supported on the support using a pressurized spray method. The barium precursor may be supported at a nickel / barium weight ratio of 15 to 100, and preferably at a nickel / barium weight ratio of 80 to 100. If the weight ratio is 15 or less, barium is excessively supported in the catalyst, resulting in a low reaction conversion rate, and if the weight ratio is 100 or more, the sulfur resistance effect of barium may not be exhibited.

[0034] In step e), the nickel-cerium-barium / mixed alumina precursor prepared in step d) may be dried and then heat-treated in an air atmosphere at a temperature ranging from 500 to 600° C. in order to remove moisture and anions derived from the metal precursor. The heat treatment temperature is within a suitable range according to common knowledge, and therefore further detailed description will be omitted.

[0035] In step f), in order to express catalytic activity from the nickel-cerium-barium / mixed alumina oxide prepared in step e), a rapid reduction process is performed using hydrogen gas at a temperature range of 550 to 700°C to obtain a final catalyst. If the reduction temperature is below 400°C, the metal oxide species may not be completely reduced, and if the reduction temperature is higher than 700°C, the metal particles may aggregate and sinter, resulting in a decrease in active sites. In the reduction process, the catalyst was heated to 600°C in a nitrogen atmosphere in a stepwise manner, and then hydrogen gas was introduced to produce the catalyst. If the catalyst contains two or more active metal species, the active metal species can be instantly produced in the form of an alloy by immediately exposing the catalyst to hydrogen gas at a high temperature as in the reduction method, but if the catalyst is gradually heated from room temperature to a hydrogen atmosphere and reduced, each metal is reduced according to its own oxygen desorption temperature, making it difficult to produce an alloy.

[0036] In addition, the catalyst prepared in the present invention can be used for the steam reforming reaction of sulfur-containing methane gas after being introduced into a reactor, and can be used for the steam reforming reaction of sulfur-containing methane gas at a reaction temperature of 700 to 850°C and a gas hourly velocity (GHSV) of 500 to 30,000 h -1 Hydrogen can be produced by a gas phase reaction under the above conditions. The higher the gas space velocity, the greater the amount of hydrogen produced. Therefore, the gas space velocity can be adjusted to an optimal value according to the volume of the reactor and the amount of catalyst, and is not limited to a specific value within the range.

[0037] The reactor for producing hydrogen by the reforming reaction is not particularly limited, and may be a fixed-bed catalytic reactor in which a catalyst is packed in the reactor. In addition, since the dehydrogenation reaction is an endothermic reaction, it is important that the catalytic reactor always maintains adiabatic conditions. It is important that the reforming reaction process of the present invention is carried out while maintaining the reaction conditions of reaction temperature, pressure, and gas space velocity within appropriate ranges. If the reaction temperature is less than 700°C, the reforming reaction does not proceed sufficiently and a very low amount of hydrogen is obtained, and if the reaction temperature is 850°C or higher, side reactions such as agglomeration of the active metal of the catalyst introduced into the reactor, sintering phenomenon, coke generation, and cracking reactions may occur, resulting in problems with the durability of the catalyst.

[0038] The technical configuration of the present invention will be described in detail below with reference to the drawings, examples, and comparative examples.

[0039] <Example 1> The carrier used in Example 1 was a γ-alumina carrier (manufactured by BASF in Germany, specific surface area: 210 m 2 The carrier was used after undergoing a phase transformation by calcining at 1100°C for 5 hours. The phase-transformed carrier had a structure in which the θ-alumina crystal phase and the α-alumina crystal phase were mixed in a ratio of 1:9, and had a specific surface area of ​​19 m. 2It has physical properties of 0.1 g / g and pore size of 32 nm. To support the metals first, nickel was used as a precursor for nickel (Ni(NO3)2·6H2O), and cerium, used as an auxiliary metal, was used as a precursor for cerium (Ce(NO3)3·6H2O). The nickel and cerium precursors were dissolved in water and impregnated into the phase-transformed theta-alpha hybrid alumina support using the spray-support method. After impregnation, the catalyst was aged for about 1 hour to ensure that the metal solution was sufficiently distributed inside the support, and then dried at 120°C for 12 hours to completely remove moisture from the catalyst. The metal was then immobilized through a heat treatment process at 700°C for 6 hours in an air atmosphere. Thereafter, in order to load metal again, barium acetate (Ba(C2H3O2)2 was loaded into the internal pores of the alumina containing nickel and cerium by the spray loading method, and the metal-loaded composition was heat-treated in an air atmosphere at 550°C for 4 hours to prepare a metal-loaded catalyst. The heat-treated catalyst was heated to 600°C in an air atmosphere, purged with nitrogen for 5 minutes, and then subjected to rapid reduction while flowing hydrogen gas to prepare a catalyst. It was confirmed that the catalyst prepared in Example 1 contained 10.0 wt% nickel, 1.5 wt% cerium, and 0.12 wt% barium. In addition, nickel-cerium-barium was uniformly distributed inside the carrier.

[0040] <Example 2> In Example 2, a catalyst was produced in the same manner as in Example 1, except that the final catalyst contained 5.0 wt % nickel, 0.75 wt % cerium, and 0.06 wt % barium as metals.

[0041] <Example 3> In Example 3, a catalyst was produced in the same manner as in Example 1, except that the final catalyst contained 15.0 wt % nickel, 2.25 wt % cerium, and 0.18 wt % barium as metals.

[0042] <Comparative Example 1> In Comparative Example 1, a catalyst was produced in the same manner as in Example 1, except that the support used in Example 1 was heat-treated at a temperature of 900° C. during the preparation of the carrier. The carrier crystal phase of the catalyst was a mixture of γ and θ phases, and the specific surface area was 121 m 2 / g and the pore size was 10 nm.

[0043] <Comparative Example 2> In Comparative Example 2, a catalyst was produced in the same manner as in Example 1, except that the support used in Example 1 was heat-treated at a temperature of 1000°C during the preparation of the carrier. The carrier crystal phase of the catalyst was a mixture of γ and θ phases, and the specific surface area was 84 m 2 / g and the pore size was 14 nm.

[0044] <Comparative Example 3> In Comparative Example 3, a catalyst was produced in the same manner as in Example 1, except that the carrier used in Example 1 was heat-treated at a temperature of 1200° C. during the preparation of the carrier. The carrier crystal phase of the catalyst was the alpha phase, and the specific surface area was 3 m 2 / g and the pore size was 45 nm.

[0045] <Comparative Example 4> Comparative Example 4 was produced in the same manner as in Example 1, except that only nickel was used as the metal, and the final catalyst contained only 10.0 wt % nickel as the metal.

[0046] <Comparative Example 5> Comparative Example 5 was produced in the same manner as in Example 1, except that only nickel and cerium were used as metals, and the final catalyst contained 10.0 wt % nickel and 1.5 wt % cerium as metals.

[0047] <Comparative Example 6> Comparative Example 6 was produced in the same manner as in Example 1, except that only nickel and barium were used as metals, and the final catalyst contained 10.0 wt % nickel and 0.12 wt % barium as metals.

[0048] <Comparative Example 7> Comparative Example 7 was produced in the same manner as in Example 1, except that the production temperature of the reduction catalyst was 650°C.

[0049] <Comparative Example 8> Comparative Example 8 was produced in the same manner as in Example 1, except that the production temperature of the reduction catalyst was 700°C.

[0050] <Comparative Example 9> Comparative Example 9 was produced in the same manner as in Example 1, except that the temperature was increased in a hydrogen atmosphere during production of the reduction catalyst.

[0051] <Comparative Example 10> Comparative Example 10 was produced in the same manner as in Example 1, except that nickel, cerium, and barium were separately supported.

[0052] <Comparative Example 11> Comparative Example 11 was produced in the same manner as Comparative Example 10, except that the temperature was raised in a hydrogen atmosphere during production of the reduction catalyst.

[0053] <Reaction example> The catalysts prepared in the examples and comparative examples were evaluated for their performance as follows. To measure catalytic activity, a reforming reaction was carried out using a mixed gas of methane and hydrogen. The reactor was evaluated using a fixed bed reaction system. 1.57 g of the catalyst was packed into a tubular reactor, and hydrogen gas was constantly flowed at 30 cc / min to remove oxygen species on the catalyst surface before the reaction, and the catalyst was reduced at 800°C for 1 hour. Then, the temperature of the reactor was kept constant at 800°C, and a mixed gas of methane gas and hydrogen, which are the raw materials used in the reaction, was continuously fed to the reactor at a constant volume ratio of 1:1, and the gas space velocity was 2000 h. -1The reaction pressure was fixed at a constant value of 1.0 atm. Also, in order to suppress the generation of coke during the catalytic reaction, steam and carbon were injected together at a ratio of 0.85:1. The reaction pressure was maintained at a constant value of 1.0 atm using a pressure regulator. The substances produced after the reaction were transferred to a GC (Gas Chromatography) through an injection line wrapped with a hot wire, and quantitative analysis was performed using a FID (Flame Ionization Detector) and a TCD (Thermal Conductivity Detector).

[0054] In the sulfur tolerance experiment, hydrogen sulfide was continuously injected at 5~15ppm per minute together with methane / hydrogen mixed gas to simulate the sulfur components present in natural gas, and activity was compared.

[0055] The conversion rate of methane to the reactants was calculated according to the following criteria to compare the activity of the catalysts.

[0056] Methane conversion rate (%) = [number of moles of methane before reaction - number of moles of methane after reaction] / [number of moles of methane before reaction] x 100

[0057] Table 2 shows the manufacturing methods of the examples and comparative examples, and Table 3 shows the activity evaluation results for the catalysts manufactured by the examples and comparative examples in the absence of sulfur injection.

[0058] [Table 2]

[0059] [Table 3]

[0060] <Evaluation> Examples 2 and 3 and Comparative Examples 1 to 11 were compared with Example 1. The nickel dispersion and particle size were analyzed by carbon monoxide chemisorption, and the conversion rate and coke were analyzed by performing a methane reforming reaction without injecting sulfur.

[0061] In Examples 1 to 3, the ratios of nickel, cerium, and barium are the same, but the total content ratio of metals in the catalyst is adjusted to produce catalysts. Example 2 shows that the methane conversion rate is significantly low due to the low nickel content, and Example 3 shows that the nickel dispersion is low due to the excessive inclusion of nickel and cerium in the catalyst, and thus the performance is lower than that of Example 1, even though the nickel content is 15 wt. As a result, it is shown that an appropriate amount of active metal is supported for the methane reforming reaction.

[0062] In Example 1 and Comparative Examples 1 to 3, catalysts were produced by varying the carrier calcination temperature. In Comparative Examples 1 and 2, when the calcination temperature was 1000°C or less, the γ-alumina crystal phase and the θ-alumina crystal phase were mixed before calcination, and the specific surface area was 100 m 2 / g or more, and there are a considerable amount of micropores inside the carrier, and the nickel dispersion is high. As a result of the methane reforming reaction, in the cases of Comparative Examples 1 and 2 in which the γ-alumina crystal phase exists, a high amount of coke is generated, which is believed to be due to the acid sites on the surface of the γ-alumina generating a large amount of coke during the reforming reaction. In contrast, in the case of Comparative Example 3, where the calcination temperature is 1200°C, a pure α-alumina crystal phase is displayed, and it is found that the nickel dispersion is very low due to the low specific surface area. In the case of the α-alumina single crystal phase, the amount of coke generated during the reforming reaction is small, but the methane conversion rate is low. This shows that the nickel metal aggregates due to the low specific surface area of ​​α-alumina, resulting in a low specific surface area and therefore low activity. This shows that the crystal phase must be transformed to θ-alumina or higher before the reforming reaction, and that the surface area in the carrier must be present in an appropriate amount.

[0063] Example 1 and Comparative Examples 4 to 6 are comparisons of catalysts prepared by individually supporting active metals in the catalyst, and Comparative Examples 4 and 6, which are catalysts not supporting cerium, were analyzed to have slightly lower nickel dispersion than Example 1, and the amount of coke after the reaction was also higher in Comparative Examples 4 and 6. This shows that there is an effect of supporting cerium in Example 1, and Comparative Example 5 shows a similar value to Example 1, indicating that barium is not involved in activity and coke formation.

[0064] In Example 1 and Comparative Examples 7 and 8, catalysts were prepared by adjusting the temperature of hydrogen reduction, which is the metal activation step of the prepared catalyst. In Comparative Examples 7 and 8, it was found that the nickel dispersion was reduced due to the high reduction temperature, which resulted in a low methane conversion rate during the reforming reaction.

[0065] Example 1 and Comparative Example 9 are catalysts manufactured according to different reduction methods during hydrogen reduction, which is the metal activation step of the manufactured catalyst, and in Comparative Example 9, the temperature was raised to 600°C, which is the reduction temperature, in a hydrogen atmosphere, and as a result, the nickel dispersion and methane conversion rate were similar to those of Comparative Example 4, which is a catalyst supported solely on nickel. This indicates that when reduction is performed while raising the temperature, alloying with cerium does not occur, and the effect of adding cerium is not expressed.

[0066] Example 1 and Comparative Examples 10 and 11 compare the effect of sequential metal loading and the effect of temperature-rising reduction after sequential metal loading during active metal loading, and both Comparative Examples 10 and 11 show the same nickel dispersion as Comparative Example 4, and the reactivity is lower than that of Example 1. This is believed to be because cerium and barium do not form an alloy with nickel, but rather block the surface of the nickel metal in the catalyst and the surface area in the support, causing a decrease in activity.

[0067] As a result, as in Example 1, the crystal phase of the support is a mixture of θ-alumina and α-alumina, and the specific surface area of ​​the support is approximately 20 m 2 / g, nickel content was about 10wt%, nickel / cerium was 6.7 by weight, nickel / barium was 83 by weight, metal loading was performed in the order of primary nickel-cerium and barium, and the reduction step was treated at 600°C by rapid reduction, making it possible to produce a catalyst that showed high methane conversion and low coke formation.

[0068] Meanwhile, Table 4 and FIG. 3 show the results of evaluation of the deactivation degree after catalytic reaction and the long-term durability with respect to the sulfur content for the catalysts prepared in Example 1 and Comparative Examples 4 to 6.

[0069] [Table 4]

[0070] <Evaluation> In Table 4 and FIG. 3, a reforming reaction of methane gas containing sulfur was carried out for Example 1 and Comparative Examples 4 to 6.

[0071] From Table 3, it can be seen that, for all of the catalysts of Example 1 and Comparative Examples 4 to 6, as the sulfur content increases, deactivation clearly occurs 24 hours after the start of the reaction. However, the catalyst of Example 1 shows the lowest deactivation degree at the same sulfur injection amount, and Comparative Examples 4 and 5, which do not contain barium, show high deactivation degrees, indicating that barium is useful for suppressing catalyst deactivation. In terms of methane conversion, Example 1 and Comparative Example 5, which support cerium to promote nickel dispersion, show higher values ​​than the catalysts not supporting cerium.

[0072] Next, a long-term activity evaluation was carried out for Example 1 and Comparative Examples 4 to 6 at the same sulfur injection amount, and the results are shown in FIG.

[0073] In both Example 1 and Comparative Examples 4 to 6, rapid deactivation occurred during the first 24 hours of the reaction, but the activity gradually decreased thereafter. In particular, Example 1 showed a performance decrease of about 7% from 24 hours to 100 hours, while the catalysts of Comparative Examples 4 to 6 showed a performance decrease rate of about 10%.

[0074] As a result, Example 1, which contained cerium to increase nickel dispersion and barium to increase sulfur resistance, not only showed the highest activity and the lowest deactivation degree, but also showed high durability in long-term evaluation.

Claims

1. A method for producing a catalyst for steam reforming of sulfur-containing methane gas, comprising the steps of: a) heat-treating γ-alumina at 1100-1150° C. to prepare a hybrid alumina carrier having an α-alumina / θ-alumina ratio of 10 or more; b) supporting an alloy solution in which a nickel precursor and a cerium precursor are mixed and dissolved in a solvent on the prepared hybrid alumina support; c) supporting the nickel-cerium / mixed alumina prepared by drying and calcining the support with a solution containing a barium precursor; d) drying and calcining the support to produce a nickel-cerium-barium / mixed alumina catalyst, and rapidly reducing the catalyst at a temperature in the range of 550 to 700° C. A method comprising:

2. The mixed alumina is 91% by weight or more of α-alumina and 9% by weight or less of θ-alumina. The method of claim 1.

3. The loading steps b) and c) are carried out at room temperature by pressurized injection. The method of claim 1.

4. The drying and calcination in step c) is carried out in an air atmosphere at 100 to 120° C. and calcination at 700 to 850° C. The method of claim 1.

5. The drying and calcination step d) is carried out in an air atmosphere at 100 to 120° C. and calcination at 500 to 600° C. The method of claim 1.

6. Rapid reduction is carried out using hydrogen gas The method of claim 1.

7. A method for producing hydrogen by steam reforming of sulfur-sulfate methane gas in a reactor containing a catalyst, comprising: At a reaction temperature of 700 to 850°C, a mixture of steam and methane gas with a volume ratio of 2.5 to 3.5 is used at a gas hourly space velocity of 500 to 30,000 h -1 A gas phase reaction is carried out under the conditions of The catalyst is produced by the method of claim 1. A method comprising:

8. The reactor is a fixed-bed catalytic reactor in which a catalyst is packed. The method according to claim 7.

9. The catalytic reactor is kept adiabatic. The method according to claim 8.

Citation Information

Patent Citations

  • Catalyst for catalytic partial oxidation of hydrocarbon and manufacturing method of synthetic gas

    JP2007069151A

  • Method for producing 4-nitrodiphenylamine

    JP2012006909A

  • Catalyst for producing hydrogen, method for manufacturing the catalyst, and method for producing hydrogen by using the catalyst

    JP2012061398A

  • Fischer-tropsch catalyst with low surface area alumina, its preparation and use thereof

    US20040077737A1

  • Catalyst for reforming hydrocarbon and method for preparation thereof, and process for reforming hydrocarbon using said catalyst

    WO2002078840A1