Composition for producing polycaprolactone shape memory material, polycaprolactone shape memory material, and method for producing and use thereof
The use of modified polyrotaxane polymer chains with reversible linking groups in polycaprolactone shape memory materials addresses issues of non-uniform stress distribution and limited reworkability, resulting in improved toughness and rapid shape recovery, suitable for complex designs and medical applications.
Patent Information
- Application Number
- JP2024525419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-28
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-10-28
AI Technical Summary
Conventional polycaprolactone shape memory materials suffer from non-uniform stress distribution due to non-uniform cross-linked networks, leading to poor shape recovery performance, low toughness, and limited reworkability, which restricts their application in fields requiring complex shape design and remoldability.
A composition comprising modified polyrotaxane polymer chains with reversible linking groups, such as photoreversible or thermoreversible groups, is used to create a polycaprolactone shape memory material through ring-opening polymerization and crosslinking, allowing for a slidable structure that adjusts polymer network topology and introduces dynamic covalent bonds for improved toughness and remoldability.
The resulting polycaprolactone shape memory material exhibits high tensile deformation, rapid shape recovery (within 5 seconds), and enhanced elongation (over 900%), enabling complex shape design and reworkability, suitable for applications like medical retrievable fixatives.
Smart Images

Figure 2024540110000001_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of Chinese patent application No. 202111266177.2, filed on October 28, 2021, the contents of which are incorporated herein by reference. [Technical field]
[0002] The present invention relates to the field of polycaprolactone shape memory materials, in particular to compositions for producing polycaprolactone shape memory materials, polycaprolactone shape memory materials, and methods of producing and using same. [Background technology]
[0003] Shape memory materials are materials that have a certain shape (initial state) under certain conditions, but when external conditions change, such as when they are stimulated by heat, light, electricity, chemical treatment, etc., they can change their shape and maintain this shape (temporary shape), and reversibly recover to their original state when the external environment changes again in a certain way and pattern. Shape memory polymer materials (SMPs) are a type of shape memory material, and compared to other shape memory materials (alloys, ceramics), they have advantages such as good shape change (up to 1000% deformation recovery possible), low density, low cost, structural designability, and controllability of deformation recovery behavior, and are widely used in fields such as biomedicine, aerospace industry, automotive and robotics industries.
[0004] Generally, in order to prevent the degradation of memory performance caused by the slippage of polymer molecular chains during shape memory cycles, it is necessary to crosslink the polymer to permanently fix its shape. However, the mixing of polymer network precursors, the linking of ends and the chain growth reaction continue until the polymer network is formed, which is a statistical process, which will cause defects in most polymer networks and limit the properties of the material. For example, the uneven distribution of network nodes will lead to uneven stress distribution in the material during stress-strain cycles, which will cause the shape recovery performance and toughness to not meet the preset requirements. In addition, since the crosslinked network of traditional polymers is generally an irreversible covalent bond, once a shape memory material is molded, it cannot change its permanent shape and cannot be reprocessed and molded, which limits the scope of application in various fields. Polycaprolactone shape memory materials are often used as biomedical materials due to their excellent biodegradability and biocompatibility. However, due to the uneven crosslinked network and lack of reprocessability, this material has a slow shape recovery rate and a low failure resistance rate when used in disposable medical supplies.
[0005] Therefore, there is a need for improved methods for producing polycaprolactone shape memory materials. Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a composition for producing a polycaprolactone shape memory material, a polycaprolactone shape memory material, and a method for producing and using the same, in order to solve the problems existing in the toughness, complex shape designability, and solid state reshapeability of conventional polycaprolactone shape memory materials. [Means for solving the problem]
[0007] In order to achieve the above object, the first aspect of the present invention comprises: Provided is a polycaprolactone shape-memory material comprising: a plurality of modified polyrotaxane polymer chains; and a plurality of composite polymer chains connecting different modified polyrotaxane polymer chains, each of the composite polymer chains comprising at least two polycaprolactone polymer chain segments, a reversible linking group between the different polycaprolactone polymer chains, and a linking modification group connecting the polycaprolactone polymer chain and a cyclic structure derived from cyclodextrin contained in the modified polyrotaxane polymer chain, wherein the reversible linking group is a photoreversible linking group or a thermoreversible linking group.
[0008] A second aspect of the present invention is The present invention provides a composition for producing a polycaprolactone shape-memory material, comprising a polyrotaxane-based initiator, an end-group modifier, ε-caprolactone, a catalyst, and a crosslinking agent, wherein the end-group modifier is selected from a nitrocinnamic acid-based compound and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid.
[0009] A third aspect of the present invention is (1) hydroxypropylating the polyrotaxane to obtain a hydroxypropylated polyrotaxane; (2) ring-opening polymerization of the hydroxypropylated polyrotaxane and ε-caprolactone in the presence of a catalyst to obtain a polycaprolactone-graft-polyrotaxane copolymer; (3) subjecting the polycaprolactone-graft-polyrotaxane copolymer to a modification reaction with the photoreversible group of the end group modifying agent to obtain a polymer network precursor in which the end group portion has been modified with the photoreversible group; and (4) reacting the photoreversible groups by the action of heating and ultraviolet light in the presence of a crosslinking agent to crosslink the polymer network precursor to obtain a polycaprolactone shape memory material.
[0010] A fourth aspect of the invention provides a polycaprolactone shape memory material produced by the method of the invention.
[0011] A fifth aspect of the invention provides the use of the polycaprolactone shape memory material of the invention in a medical retrievable fixation material. Effect of the Invention
[0012] According to the above technical solution, the present invention uses a polyrotaxane modifier as an initiator to prepare a slidable polycaprolactone polymer chain (PCL) by ring-opening polymerization, and then modifies a part of the end group of the PCL into a photoreversible group and crosslinks it to form a crosslinked structure to obtain the polycaprolactone shape memory material of the present application. By designing the crosslinked network of the polycaprolactone shape memory material as a slidable structure, the defects of the polymer network topology are adjusted to improve the toughness of the shape memory material. By changing the crosslinking method to a reversible bond connection, the dynamic covalent bond introduced realizes the designability of complex shapes of the shape memory material and the reshapeability of the solid state. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1(a) is a schematic structural diagram and H-NMR spectrum of α-cyclodextrin, FIG. 1(b) is a schematic structural diagram and H-NMR spectrum of polyethylene glycol diamine, and FIG. 1(c) is a schematic structural diagram and H-NMR spectrum of the polyrotaxane produced in Example 1. [Diagram 2] 1 is a GPC comparison chart of polyethylene glycol diamine and α-cyclodextrin in Example 1, and the produced polyrotaxane. [Diagram 3] 1 is a 1H-NMR chart of the hydroxypropylated polyrotaxane produced in Example 1. [Figure 4]1 is an infrared comparison chart of the polyrotaxane, hydroxypropylated polyrotaxane, and polycaprolactone-grafted polyrotaxane copolymer produced in Example 1. [Diagram 5] 1 is a 1H-NMR chart of the polycaprolactone graft polyrotaxane copolymer produced in Example 1. [Figure 6] FIG. 2 is a schematic diagram of a cross-linked network of polycaprolactone shape memory material. [Figure 7] FIG. 13 is a diagram demonstrating the shape reshaping process of polycaprolactone shape memory material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The range endpoints and any values disclosed herein are not intended to be limiting to the exact ranges or values, and these ranges or values should be understood to include values close to these ranges or values. In the case of numerical ranges, the individual range endpoints, the individual range endpoints and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0015] The first aspect of the present invention is Provided is a polycaprolactone shape-memory material comprising: a plurality of modified polyrotaxane polymer chains; and a plurality of composite polymer chains connecting different modified polyrotaxane polymer chains, each of the composite polymer chains comprising at least two polycaprolactone polymer chain segments, a reversible linking group between the different polycaprolactone polymer chains, and a linking modification group connecting the polycaprolactone polymer chain and a cyclic structure derived from cyclodextrin contained in the modified polyrotaxane polymer chain, wherein the reversible linking group is a photoreversible linking group or a thermoreversible linking group.
[0016] The structure of the polycaprolactone shape memory material according to the present invention is shown in FIG.
[0017] In some embodiments of the present invention, the photoreversible linking group is preferably derived from a compound having a photoreversible group, and preferably the compound is selected from a nitrocinnamic acid compound and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid. The nitrocinnamic acid compound may be a compound represented by the following formula:
[0018] [ka]
[0019] (wherein R′ represents a substituent that substitutes at least one position numbered 1 to 5 on the benzene ring, and R′ is a structure represented by the following formula:
[0020] [ka]
[0021] Here, R'''' and R''' are each independently selected from H or a C1-C6 linear or branched alkyl, * represents a connection point to the benzene ring, R'' is a substituent substituting at least one position on the benzene ring among the positions numbered 1 to 5 other than the R' substituted position, and R'' is H or a C1-C6 linear or branched alkyl.
[0022] Preferably, the nitrocinnamic acid compound is a compound represented by the following formula:
[0023] [ka]
[0024] (where R 1# , R 2# and R 3# are each independently selected from H or C1-C6 linear or branched alkyl; R 1#The substitution position of is at least one of the positions numbered 1' to 4' on the benzene ring, and most preferably 4-nitrocinnamic acid (R 1# , R 2# and R 3# is H.)
[0025] Taking 4-nitrocinnamic acid as an example, the photoreversible linking group formed may have the following schematic structure:
[0026] [ka]
[0027] The photoreversible process may be as follows.
[0028] [ka]
[0029] (where R 1 and R 2 represents each polycaprolactone polymer chain linked to a different modified polyrotaxane.) In some embodiments of the present invention, the thermally reversible linking group is preferably derived from a diisocyanate, and preferably the diisocyanate is at least one selected from hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate, and lysine diisocyanate. The reversible linking group formed may have the following schematic structure:
[0030] [ka]
[0031] Taking hexamethylene diisocyanate as an example, the thermally reversible process may be as follows:
[0032] [ka]
[0033] (Here, R1, R2, R3, and R4 represent polycaprolactone polymer chains linked to different modified polyrotaxanes, and R represents the main group of diisocyanate (the structure other than the two isocyanate groups).) In some embodiments of the present invention, the linking modification group is preferably derived from a compound for hydroxypropylation. For example, it may be a polycaprolactone polymer chain structure formed by ring-opening polymerization caused by a modified group formed by a hydroxypropylation reaction between a cyclic structure derived from cyclodextrin contained in a polyrotaxane polymer chain and propylene oxide. Preferably, it is a group represented by the structural formula -CH2-CH(CH3)-O-.
[0034] In some embodiments of the present invention, the total amount of the polycaprolactone polymer chains is preferably 80 to 100 wt %, and more preferably 95 to 99.9 wt %, based on the total amount of the modified polyrotaxane polymer chains.
[0035] In some embodiments of the present invention, the weight average molecular weight of the polycaprolactone polymer chain is preferably 5,000 to 100,000 kDa, preferably 10,000 to 80,000 kDa.
[0036] In some embodiments of the present invention, the weight average molecular weight of the modified polyrotaxane polymer chain is preferably 10 kDa to 100 kDa, and more preferably 30 kDa to 90 kDa.
[0037] In some embodiments of the present invention, the polycaprolactone shape memory material has improved toughness, large tensile deformation, good recovery performance, and shape reshaping. Preferably, the polycaprolactone shape memory material has a breaking elongation of more than 900%, a gel content of 37-78 wt%, and a time to recover to its original shape under 100% strain of 5 s or less.
[0038] In the present invention, the above structure of the polycaprolactone shape memory material can be determined by Raman spectroscopy, gel content measurement, GPC, Fourier transform infrared spectroscopy and 1 The physical and chemical properties of the polycaprolactone shape memory material can be determined by a combination of H NMR, ...
[0039] A second aspect of the present invention provides a composition for producing the polycaprolactone shape memory material of the present invention, the composition comprising a polyrotaxane-based initiator, an end group modifier, ε-caprolactone, a catalyst, and a crosslinking agent, the end group modifier being selected from a nitrocinnamic acid-based compound and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid.
[0040] The above composition according to the present invention contains polyrotaxane as an initiator to initiate ring-opening polymerization of ε-caprolactone into a slidable polycaprolactone molecular chain. The end group modifier modifies a part of the end group of polycaprolactone into a photoreversible group, changing the crosslinking method into a reversible bond linkage, and solving the problems of toughness, designability, and reshapeability that exist in conventional polycaprolactone shape memory materials.
[0041] In some embodiments of the present invention, the weight average molecular weight of the polyrotaxane-based initiator is preferably 10 kDa to 100 kDa, preferably 30 kDa to 90 kDa. The polyrotaxane-based initiator may be obtained as a commercial product or may be self-prepared. Any initiator may be used as long as it satisfies the above requirements.
[0042] In some embodiments of the present invention, the catalyst is preferably at least one selected from stannous octoate, lithium diisopropylamide, scandium(III) trifluoromethanesulfonate, and phosphazene base (BEMP).
[0043] In some embodiments of the present invention, the crosslinking agent is preferably selected from diisocyanates, preferably at least one selected from hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate, and lysine diisocyanate. Different polycaprolactone polymer chains formed by ring-opening polymerization of ε-caprolactone can be linked together.
[0044] In the present invention, the photoreversible group may be a cinnamic acid group or a coumarinyl group, for example, a nitrocinnamic acid compound may be a compound having the above structure, and although not described in detail here, it can provide a cinnamic acid group, and 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid can provide a coumarinyl group. The structural formula of 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid is shown below.
[0045] [ka]
[0046] The photoreversible group modifies one end of a polycaprolactone polymer chain formed by ring-opening polymerization of ε-caprolactone, and then bonding occurs between the photoreversible groups of different polycaprolactone polymer chains. The structure thus formed can have bonds broken or bonded by irradiation with ultraviolet light of various wavelengths, and the resulting polycaprolactone shape-memory material is endowed with designability and reshapeability in the solid state.
[0047] In some embodiments of the present invention, the composition preferably contains, based on the total amount of the composition, 0.01 to 0.1 wt % of the polyrotaxane initiator, 99.99 to 99 wt % of ε-caprolactone, 0.5 to 2 wt % of the catalyst, 0.02 to 0.05 wt % of the end group modifying agent, and 0.1 to 1 wt % of the crosslinking agent.
[0048] A third aspect of the present invention is (1) hydroxypropylating a polyrotaxane to obtain a hydroxypropylated polyrotaxane; (2) ring-opening polymerization of the hydroxypropylated polyrotaxane and ε-caprolactone in the presence of a catalyst to obtain a polycaprolactone-graft-polyrotaxane copolymer; (3) subjecting the polycaprolactone-graft-polyrotaxane copolymer to a modification reaction with the photoreversible groups of the end group modifying agent to obtain a polymer network precursor in which a portion of the end groups has been modified with the photoreversible groups; and (4) reacting the photoreversible groups by the action of heating and ultraviolet light in the presence of a crosslinking agent to crosslink the polymer network precursor to obtain a polycaprolactone shape memory material.
[0049] In some embodiments of the present invention, preferably, in step (1), the hydroxypropylation process includes dissolving the polyrotaxane in an alkaline solution, reacting with a hydroxylation reagent, and washing the resulting product. The hydroxylation reagent may be propylene oxide.
[0050] In some embodiments of the present invention, preferably in step (2), the catalyst is at least one selected from stannous octoate, lithium diisopropylamide, scandium(III) trifluoromethanesulfonate, and a phosphazene base.
[0051] In some embodiments of the present invention, the amount of the catalyst used is preferably 0.5 to 2 wt %, and more preferably 0.8 to 1.2 wt %, of the total mass of the hydroxypropylated polyrotaxane and ε-caprolactone.
[0052] In some embodiments of the present invention, the molar ratio of the hydroxypropylated polyrotaxane to ε-caprolactone is preferably 1:50 to 600, and more preferably 1:50 to 1:200, calculated in terms of the number of active hydroxyl groups contained in the hydroxypropylated polyrotaxane. The number of active hydroxyl groups is determined from the ratio of the integrated area at a chemical shift of 1.1 ppm in a hydrogen nuclear magnetic spectrum to the integrated area of cyclodextrin.
[0053] In some embodiments of the present invention, the temperature of the ring-opening polymerization is preferably 100 to 140° C., preferably 110 to 130° C., and the time of the ring-opening polymerization is preferably 40 to 50 hours, preferably 45 to 50 hours.
[0054] In some embodiments of the present invention, the ring-opening polymerization process preferably includes: polymerizing a mixture of the hydroxypropylated polyrotaxane, ε-caprolactone, and the catalyst under nitrogen protection; dissolving the obtained primary product in tetrahydrofuran, followed by multiple precipitations in n-hexane; and drying the obtained solid-phase precipitate to obtain the polycaprolactone-graft-polyrotaxane copolymer.
[0055] In some embodiments of the present invention, preferably, in step (3), the molar ratio of the end group modifier to the polycaprolactone-graft-polyrotaxane copolymer is 100 to 400:1.
[0056] In some embodiments of the present invention, the end group modifying agent is preferably a compound having a photoreversible group, and is preferably selected from nitrocinnamic acid compounds and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid. Specific compounds are as described above.
[0057] In some embodiments of the present invention, preferably, the temperature of the terminal group modification reaction is 40 to 60° C., and the time of the terminal group modification reaction is 15 to 25 hours.
[0058] In some embodiments of the present invention, the process of the end group modification reaction preferably includes: mixing the solutions prepared by the end group modification agent and the polycaprolactone-graft-polyrotaxane copolymer in a first organic solvent, adding the water-absorbing agent-I and the esterification catalyst to the obtained mixed solution to carry out the end group modification reaction; precipitating the obtained primary product multiple times, and drying the obtained solid precipitate to obtain the polymer network precursor.
[0059] In some embodiments of the present invention, preferably, the first organic solvent is at least one selected from tetrahydrofuran, N,N-dimethylformamide, dichloromethane, and dioxane, the water absorbing agent-I is at least one selected from N,N-diisopropylcarbodiimide, dicyclohexylcarbodiimide, and concentrated sulfuric acid, and the esterification catalyst is at least one selected from 4-dimethylaminopyridine, p-toluenesulfonic acid, and thionyl chloride.
[0060] In some embodiments of the present invention, the amount of the first organic solvent used is preferably such that the concentration of the mixed solution is 1 to 10 g / mL, preferably 2 to 8 g / mL, i.e., the total content of the terminal group modifier and the polycaprolactone-graft-polyrotaxane copolymer contained in the mixed solution.
[0061] In some embodiments of the present invention, the amount of the water-absorbing agent-I used is preferably 1 to 5 wt %, preferably 1.5 to 4.5 wt %, of the total amount of the end group modifier and the polycaprolactone-graft-polyrotaxane copolymer.
[0062] In some embodiments of the present invention, preferably, the molar ratio of the esterification catalyst to the polycaprolactone-graft-polyrotaxane copolymer is 1:1.5-3.5, preferably 1:2-3.
[0063] In some embodiments of the present invention, the photoreversible group is derived from an end group modifier and may be a cinnamic acid group or a coumarinyl group. Preferably, the polymer network precursor has a plurality of slidable polycaprolactone molecular chains, and contains a photoreversible group derived from the end group modifier at some chain ends of the polycaprolactone molecular chains. For example, the polycaprolactone molecular chains contain a hydroxyl group and a cinnamic acid group at some chain ends.
[0064] In some embodiments of the present invention, preferably, in step (4), the crosslinking agent is at least one selected from diisocyanate, preferably hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate, and lysine diisocyanate. Since the modification reaction may not be completed in step (3), not all of the terminal groups of the polycaprolactone polymer chain in the polycaprolactone graft polyrotaxane copolymer are modified to photoreversible groups, that is, the polymer network precursor may contain unmodified hydroxyl terminal groups of the polycaprolactone polymer chain, which allows different polycaprolactone polymer chains to be thermally reversibly linked through diisocyanate by the crosslinking agent. In addition, relinking can be made possible through ester exchange, which corresponds to the same polycaprolactone polymer chain being linked to a different polycaprolactone polymer chain by exchange.
[0065] In some embodiments of the present invention, the amount of the crosslinking agent used is preferably 0.1 to 1 wt % of the polymer network precursor.
[0066] In some embodiments of the present invention, the heating temperature is preferably 70 to 90° C., and the heating time is preferably 45 to 60 hours.
[0067] In some embodiments of the present invention, the ultraviolet light preferably has a wavelength of 250 to 380 nm.
[0068] In some embodiments of the present invention, the crosslinking process preferably includes dissolving the polymer network precursor in a second organic solvent, then adding a butyl acetate solution of the crosslinker and crosslinking catalyst to obtain a liquid mixture, heating the liquid mixture to dryness, and irradiating with the ultraviolet light to obtain the polycaprolactone shape memory material.
[0069] In some embodiments of the present invention, preferably, the second organic solvent is at least one selected from tetrahydrofuran, N,N-dimethylformamide, dichloromethane, dioxane, and the crosslinking catalyst is at least one selected from dibutyltin dilaurate, an organobismuth catalyst, and N,N-dimethylcyclohexylamine.
[0070] In some embodiments of the present invention, the amount of the second organic solvent used is preferably such that the concentration of the liquid mixture is 1 to 10 g / mL, preferably 2 to 8 g / mL, i.e., the total content of the polymer network precursor, the crosslinking agent, and the crosslinking catalyst in the liquid mixture. The amount of the crosslinking catalyst used is 1 to 5 wt %, preferably 2 to 4 wt %, of the polymer network precursor.
[0071] In some embodiments of the present invention, the polyrotaxane may be self-made. Preferably, the polyrotaxane is prepared by reacting α-cyclodextrin with polyethylene glycol diamine in the presence of a large steric hindrance compound.
[0072] In some embodiments of the present invention, the large sterically hindered compound is preferably at least one selected from N-benzyloxycarbonyl-L-tyrosine, 1-adamantaneacetic acid, fluorescein isothiocyanate, and L-phenylalanine.
[0073] In some embodiments of the present invention, the weight average molecular weight of the polyethylene glycol diamine is preferably from 5 kDa to 40 kDa, and more preferably from 10 kDa to 35 kDa.
[0074] In some embodiments of the present invention, the molar ratio of α-cyclodextrin to the polyethylene glycol diamine is preferably 50-100:1, preferably 80-90:1.
[0075] In some embodiments of the present invention, preferably the molar ratio of the large sterically hindered compound to the polyethylene glycol diamine is 2-10:1, preferably 5-8:1.
[0076] In some embodiments of the present invention, preferably the reaction process comprises: (i) adding the polyethylene glycol diamine to a saturated aqueous solution of α-cyclodextrin, stirring the mixture at 20 to 35° C. for 20 to 40 hours, and drying the resulting white precipitate to obtain an inclusion compound; (ii) preparing a solution by dissolving the large steric hindrance compound, the amidation catalyst, and the water absorbent-II in a third organic solvent, then adding the inclusion compound to the solution to obtain a suspension, subjecting the suspension to an amidation reaction, causing precipitation, and washing and drying the obtained solid-phase precipitate to obtain the polyrotaxane.
[0077] In some embodiments of the present invention, preferably, the amidation catalyst is at least one selected from Carter condensation reagent, zinc chloride, and iron chloride hexahydrate, the water absorbing agent-II is at least one selected from N,N-diisopropylethylamine, 1-hydroxybenzotriazole, and dicyclohexylcarbodiimide, and the third organic solvent is at least one selected from N,N-dimethylformamide, tetrahydrofuran, and dichloromethane.
[0078] In some embodiments of the present invention, the amount of the amidation catalyst is preferably 1-5wt%, preferably 2-4wt%, of the total amount of the polyethylene glycol diamine and α-cyclodextrin, the amount of the water absorbing agent-II is 1-5wt%, preferably 2-4wt%, of the total amount of the polyethylene glycol diamine and α-cyclodextrin, and the amount of the third organic solvent is such that the concentration of the solution is 1-10g / mL, preferably 2-8g / mL. That is, the total content of the large steric hindrance compound, the amidation catalyst, and the water absorbing agent-II in the solution.
[0079] In some embodiments of the present invention, the weight average molecular weight of the polyrotaxane is preferably 10 to 100 kDa, and more preferably 30 to 90 kDa.
[0080] A fourth aspect of the invention provides a polycaprolactone shape memory material produced by the method of the invention.
[0081] In some embodiments of the present invention, preferably, the polycaprolactone shape memory material has polycaprolactone molecular chains that can slide on polyethylene glycol molecular chains, can recover 95% or more of its original shape within 5s, has a crosslinked structure, and has a photoreversible dynamic covalent bond at the node portion of the crosslinked structure, so that the covalent bond is broken by irradiation with 256 nm ultraviolet light, giving the solid material the ability to reform its original shape. The process of reforming the shape of the polycaprolactone shape memory material is shown in FIG. 7. The polycaprolactone shape memory material has a breaking elongation of more than 900%, a gel content of 37 to 78 wt%, and a time to recover to its initial shape under 100% strain of 5 s or less.
[0082] A fifth aspect of the invention provides the use of the polycaprolactone shape memory material of the invention in a medical retrievable fixation material.
[0083] Preferably the use involves a shape memory medical fastening clip.
[0084] The present invention will now be described in detail with reference to examples. 1 H-NMR spectra are measured using a Bruker ARX-500 (Bruker, Switzerland) with a resolution of <0.2 Hz and sensitivity of >100. 1 H-NMR is used, deuterated chloroform or deuterated dimethylsulfoxide is the solvent, and the test is performed at an operating frequency of 500 MHz, a magnetic field strength of 7.05 T, and at room temperature.
[0085] GPC spectra were measured by triple detection-size exclusion chromatography (TD-SEC) from Waters, USA, to characterize the molecular weight and molecular weight distribution (PDI) of the polymer at 35 °C, with polystyrene as the standard sample, THF as the mobile phase, and the test flow rate of 1.0 mL / min.
[0086] The Fourier transform infrared spectrum was measured by Avatar 370 manufactured by Nicolet, USA. The test used KBr press samples in transmission mode, and the scanning range was 500-4000 cm. -1 , resolution is 2cm -1 Let us assume that.
[0087] The gel content is measured by the Soxhlet extraction method, which involves extraction with chloroform for 24 hours followed by weighing the mass of the sample before and after extraction to obtain the gel content.
[0088] The shape recovery speed and shape recovery rate are measured according to the plate heating tensile method using a Q800 universal testing machine manufactured by TA Instruments, USA.
[0089] The produced PCL samples are cut into dumbbell-shaped specimens using a standard 4×25 cutter, and mechanical property tests are performed using an electronic universal testing machine at a tensile speed of 20 mm / min and a preload of 0.5 N, and then the breaking elongation and tensile strength of each sample are calculated using the following formulas: Before testing, a mark is made with a marker at 2 centimeters in the center of the sample, and the thickness of the marked part is measured three times at equal intervals using a standard vernier caliper, and the average value is calculated and recorded as the average thickness of the sample.
[0090]
number
[0091] where L1 is the length of the sample at break, L0 is the initial length of the sample, F max is the maximum tensile force in the tensile process, and A is the initial cross-sectional area of the sample.
[0092] Example 1 The steps for producing the reshapeable polycaprolactone shape memory material are as follows.
[0093] Step 1: 5.3 x 10 polyethylene glycol diamine with a weight average molecular weight of 10 kDa -5 mol was weighed and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). After stirring at room temperature for 24 h to obtain a white precipitate, it was freeze-dried for 48 h in a freeze dryer to obtain an inclusion compound.
[0094] 2.6×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence. Then, the inclusion compound was added into the solution, and the suspension was subjected to amidation reaction at 25 °C for 24 h. After that, the suspension was put into excess ethyl ether to precipitate the primary product, which was centrifuged at 1800 rpm at room temperature for 20 min to collect the precipitate. The precipitate was then washed by stirring the precipitate three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane (PR).
[0095] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0096] Step 2: HP-PR and purified ε-caprolactone (ε-CL) were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR:ε-CL = 1:200), stannous octanoate was added at 1 wt% of the total mass (total mass of HP-PR and ε-caprolactone, same below), high-purity nitrogen gas was introduced and replaced, and the mixture was reacted at 120 °C for 48 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0097] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalents of 4-dimethylaminopyridine were added, and the mixture was reacted at 50 °C for 20 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0098] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and butyl acetate solution of dibutyltin dilaurate was added and stirred for 5 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 365 nm UV lamps with a power of 5 W for 12 h to obtain a polycaprolactone shape memory material.
[0099] Figure 1 shows the interaction of the produced PR with PEG (polyethylene glycol) and α-CD. 11H-NMR spectrum comparison chart. In (a), the peak at chemical shift 3.28 ppm is the proton peak on the carbon of mark 2, the peaks at chemical shifts 3.5 to 3.7 ppm correspond to the proton peaks on the carbon of marks 4, 5, and 6, the peak at chemical shift 3.76 ppm corresponds to the proton peak on the carbon of mark 3, the peak at chemical shift 4.51 ppm is the proton peak of the hydroxyl group on the carbon of mark 6, the peak at chemical shift 4.80 ppm is the proton peak of the carbon of mark 1, the peak at chemical shift 5.45 ppm is the proton peak of the hydroxyl group on the carbon of mark 3, and the peak at chemical shift 5.54 ppm is the proton peak of the hydroxyl group on the carbon of mark 2. In (b), the peak at chemical shift 2.04 ppm (mark j) is a proton peak on the amino groups at both ends of PEG-NH2, and the peak at chemical shift 3.58 ppm (mark i) is a proton peak on the methylene of PEG-NH2. In (c), the peak at chemical shift 3.51 ppm is a proton peak of the methylene of PEG, and the peak at chemical shift 4.4 to 5.7 ppm is a proton peak on α-CD. As can be seen from the nuclear magnetic spectrum, the nuclear magnetic spectrum of the synthesized PR contains a characteristic peak of the methylene at 3.5 ppm of PEG and a characteristic peak of the carbon of mark 1 at 4.8 ppm on α-CD, which proves that the PR molecule contains PEG and α-CD structural units. Integration of the characteristic peaks at 4.8 ppm and 3.5 ppm gave ∫4.8:∫3.5=1:4, indicating that one α-CD molecule exists on an average of approximately six PEG structural units.
[0100] Figure 2 shows the GPC comparison chart of the produced PR with PEG-NH2 and α-CD. As can be seen from the retention times, the molecular weight of PR is larger than that of PEG-NH2, and it is clear that there is no small molecular component. Also referring to the nuclear magnetic data in Figure 1, the α-CD found in the nuclear magnetic spectrum is attached to the PEG molecular chain, and the synthesis of PR was successful.
[0101] Figure 3 shows the nuclear magnetic spectrum of the HP-PR after the hydroxypropyl modification. Compared to the nuclear magnetic spectrum of PR, the positions above 2.0 ppm are almost the same, but in HP-PR, there is one more methyl proton peak at the chemical shift of 1.0 ppm (mark k), which indicates that the hydroxypropyl modification of α-CD on PR was successful. The peaks at 4.2-6.0 ppm and 1.0 ppm were integrated, and the hydroxypropyl modification rate DS of PR was calculated from the area integral ratio of the peaks at 4.2-6.0 ppm and 1.0 ppm, and the hydroxypropyl modification rate DS of PR was 6.
[0102] FIG. 4 is an infrared comparison chart of the produced PR, HP-PR, and PCL-g-PR. In the figure, -1 Absorption peaks at 3400 cm for PR and HP-PR -1 The absorption peak at 2946 cm for PCL-g-PR is due to the stretching vibration of -OH on -OH and -NH on -NH-. -1 The absorption peaks at 2923 cm for PR and HP-PR -1 The absorption peak at 2866 cm for PCL-g-PR is due to the asymmetric stretching vibration of -CH on -CH-. -1 The absorption peak at 1725 cm for PCL-g-PR is due to the symmetric stretching vibration of -CH on -CH-. -1 The absorption peak at 1640 cm is due to the stretching vibration of the carbonyl (C=O) on the side chain of polycaprolactone, and the peak at 1640 cm is due to the stretching vibration of the carbonyl (C=O) on the side chain of polycaprolactone. -1 The absorption peak at (C=O) is due to the stretching vibration of the carbonyl on the amide bond. -1 is due to bending vibration in the CH plane, and is in the range of 1000 to 1300 cm -1 The absorption peaks at 650–1000 cm are due to the CC skeletal vibration and the CC skeletal vibration. -1The absorption peaks in the IR spectrum are due to bending vibrations out of the CH plane. The carbonyl peaks found in PR and HP-PR are due to amide bonds, while the carbonyl peak found in PCL-g-PR is obviously higher in frequency and corresponds to ester bonds. This proves that HP-PR was used as an initiator to initiate the ring-opening polymerization of ε-caprolactone to form large molecular ester bonds. The infrared characteristic peaks of PR and HP-PR are almost similar, but the intensity of the characteristic peak of HP-PR is higher, which may be due to the weakening of the hydrogen bonds between α-cyclodextrins after hydroxypropylation of α-cyclodextrin on PR, leading to a larger vibration frequency between atoms.
[0103] FIG. 5 shows the nuclear magnetic spectrum of the produced PCL-g-PR. The peak at chemical shift 1.32 ppm (mark d) corresponds to the proton peak on the central methylene of the caprolactone segment, the peak at chemical shift 1.58 ppm (mark c) corresponds to the proton peak on the methylene adjacent to the central carbon atom of the caprolactone segment, the peak at chemical shift 2.24 ppm (mark b) corresponds to the proton peak on the carbon at the ortho position of the carbonyl of the caprolactone segment, the peak at chemical shift 3.99 ppm (mark a) corresponds to the proton peak on the carbon at the ortho position of the oxygen atom of the caprolactone segment, and at chemical shift 3.58 ppm, there is a very weak characteristic peak that is thought to be the PEG methylene. This is thought to be because the peak signal of the methylene proton on the PEG chain is shielded by the growth of the PCL segment of the PCL-g-PR side chain.
[0104] FIG. 6 illustrates the crosslinked network structure of the polycaprolactone shape memory material obtained in Example 1. In the figure, the polyethylene glycol polymer chain has a large steric hindrance group (derived from N-benzyloxycarbonyl-L-tyrosine) shown as a dot, which penetrates α-cyclodextrin shown as a ring on the polycaprolactone polymer chain, forming a crosslinked network structure between the polyethylene glycol polymer chain and the polycaprolactone polymer chain, and the ring structure by α-cyclodextrin allows the polycaprolactone polymer chain to slide on the polyethylene glycol polymer chain. The polycaprolactone polymer chain also has a reversible linking group represented by a square that provides a reversible covalent bond, and this reversible linking group is formed by a photoreversible group provided by an end group modifier or a thermoreversible group provided by a crosslinking agent, which introduces a dynamic covalent bond into the polycaprolactone shape memory material, enabling linkage by reversible bonds, and realizing the designability of complex shapes of shape memory materials and reshapeability in the solid state.
[0105] Example 2 The steps for producing the reshapeable polycaprolactone shape memory material are as follows.
[0106] Step 1: 6.4 x 10 polyethylene glycol diamine with a weight average molecular weight of 15 kDa -5 mol was weighed and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). After stirring at 30°C for 30 h to obtain a white precipitate, it was freeze-dried in a freeze dryer for 48 h to obtain an inclusion compound.
[0107] 3.4×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, then the inclusion compound was added to the solution, and the suspension was subjected to amidation reaction at 25 °C for 26 h. The suspension was then placed in excess ethyl ether to precipitate the primary product, and centrifuged at room temperature at 1800 rpm for 25 min to collect the precipitate. The precipitate was then washed by stirring it three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane.
[0108] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 55 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0109] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:400), stannous octanoate of 1 wt% of the total mass (total mass of HP-PR and ε-caprolactone) was added, high-purity nitrogen gas was introduced and replaced, and the mixture was reacted at 130 °C for 50 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0110] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 40 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalents of 4-dimethylaminopyridine were added, and the mixture was reacted at 55 °C for 22 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0111] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and butyl acetate solution of dibutyltin dilaurate was added and stirred for 5 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 370 nm UV lamps with a power of 5 W for 14 h to obtain a polycaprolactone shape memory material.
[0112] Example 3 The steps for producing the reshapeable polycaprolactone shape memory material are as follows.
[0113] Step 1: 8.0 x 10 polyethylene glycol diamine with a weight average molecular weight of 20 kDa -5 mol was weighed and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). After stirring at room temperature for 24 h to obtain a white precipitate, it was freeze-dried for 48 h in a freeze dryer to obtain an inclusion compound.
[0114] 4.2×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, then the inclusion compound was added to the solution, and the suspension was subjected to an amidation reaction at 30 °C for 25 h, after which the suspension was placed in excess ethyl ether to precipitate the primary product, and the precipitate was collected by centrifugation at room temperature and 2000 rpm for 15 min. The precipitate was then washed by stirring it three times in large amounts of acetone, methanol, and water, and then freeze-dried to obtain polyrotaxane.
[0115] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0116] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:600), stannous octanoate of 1 wt% of the total mass (total mass of HP-PR and ε-caprolactone) was added, high-purity nitrogen gas was introduced and replaced, and the mixture was reacted at 130 °C for 55 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0117] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalent of 4-dimethylaminopyridine were added, and the mixture was reacted at 45 °C for 15 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0118] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and butyl acetate solution of dibutyltin dilaurate was added and stirred for 5 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 380 nm UV lamps with a power of 5 W for 10 h to obtain a polycaprolactone shape memory material.
[0119] Example 4 The steps for producing the polycaprolactone shape memory material are as follows.
[0120] Step 1: 5.3 x 10 polyethylene glycol diamine with a weight average molecular weight of 20 kDa -5 mol was weighed and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). After stirring at room temperature for 24 h to obtain a white precipitate, it was freeze-dried for 48 h in a freeze dryer to obtain an inclusion compound.
[0121] 2.6×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, then the inclusion compound was added to the solution, and the suspension was subjected to amidation reaction at 25 °C for 30 h. The suspension was then placed in excess ethyl ether to precipitate the primary product, and centrifuged at room temperature at 2000 rpm for 25 min to collect the precipitate. The precipitate was then washed by stirring the precipitate three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane.
[0122] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0123] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR:ε-CL = 1:200), stannous octanoate of 1 wt% of the total mass (total mass of HP-PR and ε-caprolactone) was added, high-purity nitrogen gas was introduced and replaced, and the mixture was reacted at 120 °C for 48 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0124] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalents of 4-dimethylaminopyridine were added, and the mixture was reacted at 60 °C for 15 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0125] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and dibutyltin dilaurate in butyl acetate was added and stirred for 5 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 375 nm UV lamps with a power of 5 W for 13 h to obtain a polycaprolactone shape memory material.
[0126] Example 5 The steps for producing the polycaprolactone shape memory material are as follows.
[0127] Step 1: 5.7 x 10 polyethylene glycol diamine with a weight average molecular weight of 20 kDa -5 The mixture was weighed out in moles and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). The mixture was stirred at 30°C for 24 hours to obtain a white precipitate, which was then freeze-dried for 50 hours in a freeze dryer to obtain an inclusion compound.
[0128] 2.7×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, then the inclusion compound was added to the solution, and the suspension was subjected to amidation reaction at 25 °C for 28 h. The suspension was then placed in excess ethyl ether to precipitate the primary product, and centrifuged at room temperature at 1800 rpm for 30 min to collect the precipitate. The precipitate was then washed by stirring it three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane.
[0129] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0130] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:400), stannous octanoate of 1 wt% of the total mass was added, high-purity nitrogen gas was introduced and substituted, and the mixture was reacted at 125 °C for 50 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0131] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalents of 4-dimethylaminopyridine were added, and the mixture was reacted at 40 °C for 25 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0132] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and dibutyltin dilaurate in butyl acetate was added and stirred for 5 minutes. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48h, then vacuum dried overnight at 80°C, and finally irradiated for 15h with four 365nm UV lamps with a power of 5W in an ultraviolet box to obtain a polycaprolactone shape memory material.
[0133] Example 6 The steps for producing the reshapeable polycaprolactone shape memory material are as follows.
[0134] Step 1: 7.4 x 10 polyethylene glycol diamine with a weight average molecular weight of 30 kDa -5 mol was weighed and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). After stirring at room temperature for 24 h to obtain a white precipitate, it was freeze-dried for 48 h in a freeze dryer to obtain an inclusion compound.
[0135] 3.5×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, then the inclusion compound was added into the solution, and the suspension was reacted at 25 °C for 24 h. The suspension was poured into excess ethyl ether to precipitate the primary product, and centrifuged at 1800 rpm at room temperature for 30 min to collect the precipitate. The precipitate was then washed by stirring the precipitate three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane.
[0136] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0137] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:600), stannous octanoate of 1 wt% of the total mass was added, high-purity nitrogen gas was introduced and replaced, and the mixture was reacted at 110 °C for 50 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0138] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 40 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalent of 4-dimethylaminopyridine were added, and the mixture was reacted at 60 °C for 20 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0139] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and dibutyltin dilaurate in butyl acetate was added and stirred for 10 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated with four 380 nm UV lamps with a power of 5 W in a UV box for 12 h to obtain a polycaprolactone shape memory material.
[0140] Example 7 The steps for producing the polycaprolactone shape memory material are as follows.
[0141] Step 1: 5.3 x 10 polyethylene glycol diamine with a weight average molecular weight of 35 kDa -5 mol was weighed and added to a saturated aqueous solution of α-CD (7.25 g / 50 mL, double distilled H2O). The mixture was stirred at 30°C for 26 h to obtain a white precipitate, which was then freeze-dried for 48 h in a freeze dryer to obtain the inclusion compound.
[0142] 2.6×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, and then the inclusion compound was added to the solution, and the suspension was subjected to amidation reaction at 25 °C for 24 h. The suspension was placed in excess ethyl ether to precipitate the primary product, and centrifuged at room temperature at 2000 rpm for 20 min to collect the precipitate. The precipitate was then washed by stirring the precipitate three times in large amounts of acetone, methanol, and water, and lyophilized to obtain polyrotaxane.
[0143] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0144] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:200), stannous octanoate of 1 wt% of the total mass was added, high-purity nitrogen gas was introduced and replaced, and the mixture was reacted at 130 °C for 45 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0145] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalents of 4-dimethylaminopyridine were added, and the mixture was reacted at 50 °C for 20 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0146] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and dibutyltin dilaurate in butyl acetate was added and stirred for 5 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 370 nm UV lamps with a power of 5 W for 15 h to obtain a polycaprolactone shape memory material.
[0147] Example 8 The steps for producing the polycaprolactone shape memory material are as follows.
[0148] Step 1: 6.9 x 10 polyethylene glycol diamine with a weight average molecular weight of 35 kDa -5 mol was weighed and added to a saturated aqueous solution of α-CD (7.25 g / 50 mL, double-distilled H2O). After stirring at room temperature for 24 h to obtain a white precipitate, it was freeze-dried for 48 h in a freeze dryer to obtain the inclusion compound.
[0149] 3.5×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, and then the inclusion compound was added to the solution, and the suspension was subjected to amidation reaction at 25 °C for 26 h. The suspension was placed in excess ethyl ether to precipitate the primary product, and centrifuged at room temperature at 1800 rpm for 30 min to collect the precipitate. The precipitate was then washed by stirring the precipitate three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane.
[0150] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0151] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:400), stannous octanoate of 1 wt% of the total mass was added, high-purity nitrogen gas was introduced and substituted, and the mixture was reacted at 110 °C for 50 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum-dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0152] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalent of 4-dimethylaminopyridine were added, and the mixture was reacted at 60 °C for 20 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0153] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and butyl acetate solution of dibutyltin dilaurate was added and stirred for 10 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 365 nm UV lamps with a power of 5 W for 15 h to obtain a polycaprolactone shape memory material.
[0154] Example 9 The steps for producing the polycaprolactone shape memory material are as follows.
[0155] Step 1: 5.8 x 10 polyethylene glycol diamine with a weight average molecular weight of 35 kDa -5 mol was weighed and added to a saturated aqueous solution of α-cyclodextrin (7.25 g / 50 mL, double-distilled H2O). After stirring at room temperature for 24 h to obtain a white precipitate, it was freeze-dried for 48 h in a freeze dryer to obtain an inclusion compound.
[0156] 2.7×10 -3mol of N-benzyloxycarbonyl-L-tyrosine (ZL-Tyr), Carter condensation reagent (BOP), 1-hydroxybenzotriazole (HOBt), and N,N-diisopropylethylamine (DIEA) were dissolved in a small amount of N,N-dimethylformamide (DMF) in sequence, and then the inclusion compound was added to the solution, and the suspension was subjected to amidation reaction at 20 °C for 30 h. The suspension was precipitated in excess ethyl ether, centrifuged at room temperature at 2000 g for 20 min, and the precipitate was collected. The precipitate was then washed by stirring the precipitate three times in large amounts of acetone, methanol, and water, and freeze-dried to obtain polyrotaxane.
[0157] An appropriate amount of polyrotaxane was weighed and dissolved in 50 mL of 1 mol / L NaOH solution, and an appropriate amount of propylene oxide was added drop by drop under ice bath conditions, and the mixture was stirred overnight. As the ice in the solution melted, the reaction temperature gradually rose to room temperature. The sample was purified by dialysis against deionized water for one week and freeze-dried. The freeze-dried sample was added to 100 mL of dichloromethane and stirred overnight to filter out the free polyethylene glycol generated by decomposition during hydroxypropylation, which was then washed with a large amount of acetone, centrifuged to collect the precipitate, and vacuum dried at 60 °C to obtain hydroxypropylated polyrotaxane (HP-PR).
[0158] Step 2: HP-PR and purified ε-caprolactone were added to a silanized dry round-bottom flask in a molar ratio (number of active hydroxyl groups on HP-PR: ε-CL = 1:600), stannous octanoate of 1 wt% of the total mass was added, high-purity nitrogen gas was introduced and substituted, and the mixture was reacted at 130 °C for 48 h. After that, the primary product was dissolved in a small amount of tetrahydrofuran and precipitated in excess n-hexane three times, and the precipitate was vacuum dried at 60 °C for 48 h to obtain polycaprolactone-grafted polyrotaxane copolymer (PCL-g-PR).
[0159] Step 3: 0.5 molar equivalents of 4-nitrocinnamic acid with active hydroxyl groups in HP-PR were weighed and dissolved in 25 mL of DMF at 50 °C. Then, the DMF solution of PCL-g-PR was added to the DMF solution of 4-nitrocinnamic acid and stirred for 30 min. Then, 1 molar equivalent of N,N-diisopropylcarbodiimide and 0.5 molar equivalents of 4-dimethylaminopyridine were added, and the mixture was reacted at 40 °C for 25 h. The primary product was precipitated in excess ethyl ether and centrifuged to collect the solid. The solid product was dissolved in a small amount of toluene, precipitated in ethyl ether three more times, and dried in vacuum at 60 °C overnight to obtain a polymer network precursor in which some of the end groups were modified to cinnamic acid groups.
[0160] Step 4: The polymer network precursor was dissolved in N,N-dimethylformamide at 80°C, then an appropriate amount of hexamethylene diisocyanate and butyl acetate solution of dibutyltin dilaurate was added and stirred for 10 min. The liquid mixture was placed between two glass plates separated by a silicone rubber gasket and placed in an oven at 80°C for 48 h, then vacuum dried at 80°C overnight, and finally irradiated in a UV box with four 380 nm UV lamps with a power of 5 W for 12 h to obtain a polycaprolactone shape memory material.
[0161] Comparative Example 1 The thermally crosslinked polycaprolactone shape memory plate material was produced using 90 parts by weight of polycaprolactone as ingredients, 5 parts by weight of benzoyl peroxide as a crosslinking agent, 80 parts by weight of dichloromethane as a solvent, and 1 part by weight of a mold release agent.
[0162] The manufacturing method of the above thermally crosslinked polycaprolactone shape memory plate includes the following manufacturing steps:
[0163] Step 1: Polycaprolactone, benzoyl peroxide as a crosslinker, and dichloromethane as a solvent were placed in a round-bottom flask to perform solution blending, and then ultrasonicated for 30 min. The mixture was then transferred to a mechanical mixer and stirred for 1 h to obtain a mixture.
[0164] Step 2: The solvent was evaporated from the obtained mixture at room temperature for 1-2 h, and then the mixture was vacuum dried at 50-70°C for 24 h to obtain a PCL / BPO solid mixture.
[0165] Step 3: The solid mixture obtained in step 2 was placed into a customized iron mold, sprayed with a release agent, and the thermal crosslinking process of polycaprolactone was started with peroxide at 140-160°C by a flat vulcanizer, for 5-15 min, and at a maximum pressure of 10 MPa, to obtain a thermally crosslinked polycaprolactone shape memory plate material.
[0166] For the products obtained in Examples 1 to 9 and Comparative Example 1, the gel content, shape recovery speed, shape recovery rate, breaking elongation, and tensile strength were measured. The results are shown in Table 1.
[0167] [Table 1]
[0168] From the results in Table 1, it is clear that the polycaprolactone shape memory materials of Examples 1 to 9 obtained by the method according to the present invention have a faster shape recovery speed and a higher shape recovery rate than the products produced in the comparative examples, and can recover 95% or more of the original shape within 5 seconds. In addition, the results of measuring the breaking elongation and tensile strength of the products obtained in the examples show that the breaking elongation is clearly improved compared to Comparative Example 1. For example, in Example 9, the breaking elongation is improved by 1 times, which proves that the toughness of the shape memory material can be improved.
[0169] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited thereto. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solutions of the present invention, including combining each technical feature in another suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed in the present invention, and all fall within the protection scope of the present invention.
Claims
1. 1. A polycaprolactone shape-memory material comprising: a plurality of modified polyrotaxane polymer chains; and a plurality of composite polymer chains connecting different modified polyrotaxane polymer chains, each of the composite polymer chains comprising at least two polycaprolactone polymer chain segments, a reversible linking group between the different polycaprolactone polymer chains, and a linking modification group connecting the polycaprolactone polymer chain and a cyclic structure derived from cyclodextrin contained in the modified polyrotaxane polymer chain, wherein the reversible linking group is a photoreversible linking group or a thermoreversible linking group.
2. The photoreversible linking group is derived from a compound having a photoreversible group, and preferably, the compound is selected from a nitrocinnamic acid compound and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid; The polycaprolactone shape memory material according to claim 1, wherein the thermally reversible linking group is derived from a diisocyanate, and the diisocyanate is preferably at least one selected from hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate, and lysine diisocyanate.
3. The linkage modifying group is derived from a compound for hydroxypropylation and preferably has the structural formula -CH 2 -CH(CH 3 3. The polycaprolactone shape-memory material according to claim 1 or 2, wherein the group is represented by the formula:
4. the total amount of the polycaprolactone polymer chains is 80 to 100 wt %, preferably 95 to 99.9 wt %, based on the total amount of the modified polyrotaxane polymer chains; Preferably, the weight average molecular weight of the polycaprolactone polymer chain is 5000 to 100000 kDa, preferably 10000 to 80000 kDa; The polycaprolactone shape memory material according to any one of claims 1 to 3, wherein the weight average molecular weight of the modified polyrotaxane polymer chain is preferably 10 kDa to 100 kDa, preferably 30 kDa to 90 kDa.
5. The polycaprolactone shape memory material according to any one of claims 1 to 4, wherein the polycaprolactone shape memory material has an elongation at break of more than 900%, a gel content of the polycaprolactone shape memory material is 37 to 78 wt %, and the time for the polycaprolactone shape memory material to recover to its initial shape under 100% strain is 5 s or less.
6. The composition for producing the polycaprolactone shape-memory material according to any one of claims 1 to 5, comprising a polyrotaxane-based initiator, a terminal group modifier, ε-caprolactone, a catalyst, and a crosslinking agent, wherein the terminal group modifier is selected from a nitrocinnamic acid-based compound and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid.
7. The weight average molecular weight of the polyrotaxane initiator is 10 kDa to 100 kDa, preferably 30 kDa to 90 kDa; Preferably, the catalyst is at least one selected from stannous octanoate, lithium diisopropylamide, scandium(III) trifluoromethanesulfonate, and a phosphazene base; 7. The composition according to claim 6, wherein the crosslinking agent is a diisocyanate, preferably at least one selected from hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate, lysine diisocyanate.
8. 8. The composition according to claim 6, comprising, based on a total amount of the composition, 0.01 to 0.1 wt % of the polyrotaxane initiator, 99.99 to 99 wt % of ε-caprolactone, 0.5 to 2 wt % of the catalyst, 0.02 to 0.05 wt % of the terminal group modifying agent, and 0.1 to 1 wt % of the crosslinking agent.
9. (1) a step of hydroxypropylating a polyrotaxane to obtain a hydroxypropylated polyrotaxane; (2) ring-opening polymerization of the hydroxypropylated polyrotaxane and ε-caprolactone in the presence of a catalyst to obtain a polycaprolactone-graft-polyrotaxane copolymer; (3) subjecting the polycaprolactone-graft-polyrotaxane copolymer to a modification reaction with a photoreversible group possessed by an end group modifying agent to obtain a polymer network precursor in which the end group portion is modified to a photoreversible group; and (4) reacting the photoreversible groups by the action of heating and ultraviolet light in the presence of a crosslinking agent to crosslink the polymer network precursor to obtain a polycaprolactone shape memory material.
10. In step (2), the catalyst is at least one selected from stannous octanoate, lithium diisopropylamide, scandium(III) trifluoromethanesulfonate, and a phosphazene base; Preferably, the amount of the catalyst used is 0.5 to 2 wt %, preferably 0.8 to 1.2 wt %, of the total mass of the hydroxypropylated polyrotaxane and ε-caprolactone; Preferably, the molar ratio of the hydroxypropylated polyrotaxane to ε-caprolactone is 1:50 to 600, preferably 1:50 to 1:200, calculated in terms of the number of active hydroxyl groups contained in the hydroxypropylated polyrotaxane; Preferably, the ring-opening polymerization temperature is 100 to 140° C., preferably 110 to 130° C., and the ring-opening polymerization time is 40 to 50 h, preferably 45 to 50 h; The method according to claim 9, wherein the ring-opening polymerization process comprises: polymerizing a mixture of the hydroxypropylated polyrotaxane, ε-caprolactone, and the catalyst under nitrogen protection; dissolving the obtained primary product in tetrahydrofuran, followed by multiple precipitations in n-hexane; and drying the obtained solid-phase precipitate to obtain the polycaprolactone-graft-polyrotaxane copolymer.
11. In step (3), the molar ratio of the end group modifying agent to the polycaprolactone-graft-polyrotaxane copolymer is 100 to 400:1; Preferably, the end group modifying agent is selected from a compound having a photoreversible group, preferably a nitrocinnamic acid compound and / or 4-((4-methyl-2-oxo-2H-chromen-7-yl)oxy)butyric acid; Preferably, the temperature of the terminal group modification reaction is 40 to 60° C., and the time of the terminal group modification reaction is 15 to 25 h; Preferably, the process of the end group modification reaction includes: mixing solutions prepared by using the end group modifying agent and the polycaprolactone-graft-polyrotaxane copolymer in a first organic solvent, adding the water-absorbing agent-I and an esterification catalyst to the obtained mixed solution to carry out the end group modification reaction; precipitating the obtained primary product multiple times, and drying the obtained solid precipitate to obtain the polymer network precursor; Preferably, the first organic solvent is at least one selected from tetrahydrofuran, N,N-dimethylformamide, dichloromethane, and dioxane, the water absorbing agent-I is at least one selected from N,N-diisopropylcarbodiimide, dicyclohexylcarbodiimide, and concentrated sulfuric acid, and the esterification catalyst is at least one selected from 4-dimethylaminopyridine, p-toluenesulfonic acid, and thionyl chloride, Preferably, the amount of the first organic solvent used is such that the concentration of the mixed solution is 1 to 10 g / mL, preferably 2 to 8 g / mL, the amount of the water-absorbing agent-I used is 1 to 5 wt %, preferably 1.5 to 4.5 wt %, of the total amount of the end group modifying agent and the polycaprolactone-graft-polyrotaxane copolymer, and the molar ratio of the esterification catalyst to the polycaprolactone-graft-polyrotaxane copolymer is 1:1.5 to 3.5, preferably 1:2 to 3, The method according to claim 9 or 10, wherein the polymer network precursor has a plurality of slidable polycaprolactone molecular chains and contains a photoreversible group derived from the end group modifier at a part of the chain ends of the polycaprolactone molecular chains, and the photoreversible group is preferably a coumarinyl group or a cinnamic acid group.
12. In step (4), the crosslinking agent is a diisocyanate, preferably at least one selected from hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate, and lysine diisocyanate; Preferably, the amount of the crosslinking agent used is 0.1 to 1 wt % of the polymer network precursor; Preferably, the heating temperature is 70 to 90° C., and the heating time is 45 to 60 h. Preferably, the wavelength of the ultraviolet light is 250 to 380 nm; Preferably, the crosslinking process includes dissolving the polymer network precursor in a second organic solvent, then adding a butyl acetate solution of the crosslinking agent and the crosslinking catalyst to obtain a liquid mixture, heating the liquid mixture to dry it, and irradiating it with ultraviolet light to obtain the polycaprolactone shape memory material; Preferably, the second organic solvent is at least one selected from tetrahydrofuran, N,N-dimethylformamide, dichloromethane, and dioxane, and the crosslinking catalyst is at least one selected from dibutyltin dilaurate, an organic bismuth catalyst, and N,N-dimethylcyclohexylamine, 12. The method according to any one of claims 9 to 11, wherein the amount of the second organic solvent used is preferably such that the concentration of the liquid mixture is 1-10 g / mL, preferably 2-8 g / mL, and the amount of the crosslinking catalyst used is 1-5 wt %, preferably 2-4 wt %, of the polymer network precursor.
13. The polyrotaxane is produced by reacting α-cyclodextrin with polyethylene glycol diamine in the presence of a large steric hindrance compound; Preferably, the large steric hindrance compound is at least one selected from N-benzyloxycarbonyl-L-tyrosine, 1-adamantaneacetic acid, fluorescein isothiocyanate, and L-phenylalanine; Preferably, the weight average molecular weight of the polyethylene glycol diamine is from 5 kDa to 40 kDa, preferably from 10 kDa to 35 kDa; Preferably, the molar ratio of α-cyclodextrin to said polyethylene glycol diamine is 50-100:1, preferably 80-90:1; Preferably, the molar ratio of the large sterically hindered compound to the polyethylene glycol diamine is 2 to 10:1, preferably 5 to 8:1; Preferably, the reaction process comprises: (i) adding the polyethylene glycol diamine to a saturated aqueous solution of α-cyclodextrin, stirring at 20 to 35° C. for 20 to 40 hours, and drying the resulting white precipitate to obtain an inclusion compound; (ii) dissolving the large steric hindrance compound, the amidation catalyst, and the water absorbent-II in a third organic solvent to prepare a solution, then adding the inclusion compound to the solution to obtain a suspension, causing an amidation reaction and precipitation, and washing and drying the obtained solid-phase precipitate to obtain the polyrotaxane; Preferably, the amidation catalyst is at least one selected from Carter condensation reagent, zinc chloride, and iron chloride hexahydrate, the water absorbing agent-II is at least one selected from N,N-diisopropylethylamine, 1-hydroxybenzotriazole, and dicyclohexylcarbodiimide, and the third organic solvent is at least one selected from N,N-dimethylformamide, tetrahydrofuran, and dichloromethane, Preferably, the amount of the amidation catalyst used is 1 to 5 wt %, preferably 2 to 4 wt %, of the total amount of the polyethylene glycol diamine and the α-cyclodextrin, the amount of the water-absorbing agent-II used is 1 to 5 wt %, preferably 2 to 4 wt %, of the total amount of the polyethylene glycol diamine and the α-cyclodextrin, and the amount of the third organic solvent used is such that the concentration of the solution is 1 to 10 g / mL, preferably 2 to 8 g / mL, The method according to any one of claims 9 to 12, wherein the weight average molecular weight of the polyrotaxane is preferably from 10 to 100 kDa, preferably from 30 to 90 kDa.
14. A polycaprolactone shape memory material produced by the method according to any one of claims 9 to 13.
15. Use of the polycaprolactone shape memory material according to any one of claims 1 to 5 and 14 in a medical retrievable fixation material, preferably said use comprising a shape memory medical fixation clip.
Citation Information
Patent Citations
Preparation method of shape-restorable polyurethane material
CN111848899A
Flexible polyurethane foam
JP2021161288A
Composition for polyurethane foam containing polyrotaxane, polyurethane foam derived from composition, and method for producing polyurethane foam
WO2017130998A1
Spherical powder containing crosslinked body formed having polyrotaxane, and method for producing same
WO2018074404A1